Manufacturing method of laminated pulp container and manufacturing device of laminated pulp container

The method and apparatus ensure laminate films are adhered to both sides of pulp containers using molds and gas pressure, addressing contamination issues and enhancing resistance, even in stacked configurations.

JP7553071B2Active Publication Date: 2024-09-18KP PLATEC CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020035811
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-03
Publication Date
2024-09-18
Estimated Expiration
2040-03-03

AI Technical Summary

Technical Problem

Existing laminated pulp containers lack a laminate film on the outer surface, leading to potential contamination of the inner surface of stacked containers due to pulp fiber transfer and difficulty in attaching a laminate film to both sides of the container.

Method used

A method and apparatus that utilize a pair of molds to extrude and adhere laminate films to both the inner and outer surfaces of a pulp container body, using gas pressure and elastic members to ensure proper attachment without evacuating the container.

Benefits of technology

The laminate films are effectively attached to both sides of the container, preventing pulp fiber transfer and ensuring cleanliness and moisture/oil resistance, even when stacked.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553071000007
    Figure 0007553071000007
  • Figure 0007553071000002
    Figure 0007553071000002
  • Figure 0007553071000003
    Figure 0007553071000003
Patent Text Reader

Abstract

To provide a manufacturing method of a laminate pulp container which can attach a laminate film on both surfaces of a container.SOLUTION: A manufacturing method of a laminate pulp container includes: first steps ST1-ST7 of attaching a first laminate film 12 to any one surface out of an inside surface and an outside surface of a concave container body 10 made by papermaking by pulp fiber; and second steps ST11-ST16 of attaching a second laminate film 14 on the other surface out of the inside surface and the outside surface. The second steps include: support step ST12 of allowing one mold body out of a pair of mold bodies corresponding to the container body to support the container body on which the first laminate film is attached; arrangement step ST13 of arranging the other of the mold bodies so as to face the other surface of the container body via the second laminate film; and attachment step ST14 of attaching the second laminate film closely on the container body by the other of the mold bodies.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and an apparatus for manufacturing laminated pulp containers used for storing food, etc. [Background technology]

[0002] There is a known method for manufacturing a laminated pulp container made of a laminate in which a pulp layer and a plastic layer are laminated (for example, Patent Document 1). In the manufacturing method of Patent Document 1, first, a pulp layer is paper-formed from a raw material liquid containing pulp fibers into a shape with a recess capable of accommodating contents. Then, a laminate film is arranged along the inner surface of the recess, and the pulp layer is vented from the outer surface to bring the laminate film into close contact with the pulp layer. The laminated pulp container is completed by further adhering the film to the pulp layer. By providing a plastic layer on the inner surface of the recess, it is possible to impart water resistance and oil resistance to the inner surface of the recess, making it possible to accommodate food, etc., in the recess. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2007-30925 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the laminated pulp container manufactured by the method described in Patent Document 1, since no laminate film is provided on the outer surface, the pulp layer is exposed on the outer surface. Therefore, when two laminated pulp containers are stacked one on top of the other, there is a risk that the pulp fibers contained in the pulp layer of the upper container will transfer to the surface of the plastic layer provided in the recess of the lower container. Since such transfer of pulp fibers reduces the cleanliness of the plastic layer surface, it is desirable to adhere a laminate film to the outer surface of the pulp layer as well.

[0005] Therefore, it is conceivable to attach a laminate film to the inner surface of the recessed portion according to the method described in Patent Document 1, and then arrange a new laminate film along the outer surface of the pulp layer, vent the pulp layer from the inner surface of the recessed portion, and adhere the laminate film to the outer surface of the pulp layer. However, because the laminate film has poor breathability, it is difficult to vent the pulp layer from the inner surface of the recessed portion after attaching the laminate film to the inner surface of the recessed portion, and it is not easy to attach the laminate film to the outer surface of the pulp layer.

[0006] The problem to be solved by the present invention is to provide a method and an apparatus for manufacturing a laminated pulp container that enables a laminate film to be bonded to both sides of the container. [Means for solving the problem]

[0007] A manufacturing method for a laminated pulp container (1) according to the present invention includes a first step (ST1 to ST7) of attaching a first laminate film (12) to one of the inner and outer surfaces of a concave container body (10) made from pulp fibers, and a second step (ST11 to ST16) of attaching a second laminate film (14) to the other of the inner and outer surfaces. The second step includes a supporting step (ST12) of supporting the container body to which the first laminate film has been attached, on one of a pair of mold bodies corresponding to the container body, an arrangement step (ST13) of arranging the other of the mold bodies so as to face the other surface of the container body via the second laminate film, and a bonding step (ST14) of tightly adhering the second laminate film to the container body by the other of the mold bodies.

[0008] According to this configuration, the second laminate film is pushed out onto the container body by the mold, and the second laminate film is adhered to the container body. Therefore, since the container body does not need to be evacuated to attach the laminate film, it is possible to adhere the laminate film to both sides of the container.

[0009] In the above embodiment, more preferably, in the bonding step, gas is blown in a direction in which the second laminate film faces the other surface of the container body.

[0010] According to this configuration, the second laminate film moves toward the container body when the gas is blown thereto, which makes it easier for the second laminate film to come into close contact with the container body.

[0011] In the above embodiment, it is more preferable that in the first step, the first laminate film is attached to the inner surface, and the other side of the mold body is a female mold having a recess and an introduction hole that connects from the outside to the inside of the recess and opens at the bottom surface of the recess, and in the bonding step, the gas is blown onto the second laminate film by introducing the gas from the introduction hole between the other side of the mold body and the second laminate film.

[0012] According to this configuration, by introducing gas from the bottom surface of the recess of the mold body, a gas flow can be generated so as to flow out of the recess, whereby the second laminate film can be blown toward the container body, and the second laminate film can be moved toward the container body.

[0013] In the above embodiment, more preferably, in the bonding step, the other side of the mold body is brought into contact with the second laminate film to form an airtight space between the other side of the mold body and the second laminate film, and the gas is introduced into the airtight space through the introduction hole to increase the internal pressure of the airtight space.

[0014] According to this configuration, when the container body and the second laminate film come into contact with each other, the second laminate film is pressed against the container body by the gas trapped in the sealed space, so that the second laminate film is pressed more strongly against the container body, thereby improving the adhesion between the second laminate film and the container body.

[0015] In the above embodiment, it is more preferable that the method further includes a heating step of heating the second laminate film before the positioning step, and the gas is heated before being blown onto the second laminate film in the bonding step.

[0016] According to this configuration, the second laminate film is easily deformed by heating, so that the adhesion between the second laminate film and the container body is improved. Furthermore, since the gas is heated before being blown onto the second laminate film, the second laminate film is less likely to be cooled by the blowing of the gas.

[0017] In the above embodiment, more preferably, an elastic member capable of elastic deformation is provided on the other side of the mold body, and the elastic member is pressed against the container body in the bonding step.

[0018] According to this configuration, when the mold body is pressed against the container body from the other side, the elastic member elastically deforms to match the shape of the container body, thereby improving the adhesion between the second laminate film and the container body.

[0019] In the above embodiment, more preferably, in the bonding step, when the elastic member is pressed against the container body, air is evacuated between the other of the mold bodies and the second laminate film.

[0020] This configuration can prevent gas from remaining between the second laminate film and the elastic member, which makes it easier for the elastic member to elastically deform to match the shape of the container body, improving the adhesion between the second laminate film and the container body.

[0021] The laminated pulp container manufacturing apparatus (1) according to the present invention is an apparatus for manufacturing a laminated pulp container in which laminate films (12, 14) are attached to both sides of a container body (10) made of paper made of pulp fibers, and includes a pair of mold bodies including a female mold (38) having a recess (38A) and an introduction hole (38E) opening into the bottom surface of the recess, and a male mold (39) having a protrusion (39A) that fits into the recess, and a press machine that fits the female mold and the male mold together. The apparatus includes a drive unit (40), a gas supply unit (41) connected to the inlet hole, and a control unit (43) capable of controlling the gas supply unit and the drive unit, and the control unit drives the drive unit to engage the female mold and the male mold, while driving the gas supply unit to introduce gas from the inlet hole between the mold body and the laminate film, thereby blowing the gas onto the laminate film and adhering the laminate film to the container body.

[0022] According to this configuration, the laminate film is pushed out to the container body by the gas between the laminate film and the mold body, and the laminate film is adhered to the container body. Therefore, since it is not necessary to evacuate the container body to attach the laminate film, it is possible to adhere the laminate film to both sides of the container.

[0023] In the above embodiment, preferably, the device further includes an exhaust device (42) connected to the introduction hole.

[0024] According to this configuration, it is possible to prevent gas from remaining between the laminate film and the female mold, and therefore the laminate film can be more reliably pressed against the container body by the female mold.

[0025] In the above embodiment, the female mold is preferably provided with an elastic member that is elastically deformable.

[0026] According to this configuration, when the male mold and female mold are fitted together to bond the laminate film to the container body, the elastic member undergoes elastic deformation, so that the laminate film can be more closely attached to the container body.

[0027] In the above embodiment, preferably, the apparatus further includes a film heating device that heats the laminate film, and a gas heating device (45) that is provided in a gas inlet path (41B) that leads from the gas supply device to the inlet hole and heats the gas passing through the gas inlet path.

[0028] According to this configuration, the laminate film is easily deformed by heating, so that the adhesion between the laminate film and the container body is improved. Furthermore, since the gas is blown onto the laminate film after being heated, the laminate film is less likely to be cooled by the blowing of the gas. Effect of the Invention

[0029] According to the present invention, it is possible to provide a method and an apparatus for manufacturing a laminated pulp container that enable a laminate film to be bonded to both sides of a container. [Brief description of the drawings]

[0030] [Figure 1] FIG. 1A is a perspective view of a laminated pulp container manufactured according to the manufacturing method of the present invention, and FIG. 1B is a cross-sectional view taken along the line IB-IB. [Diagram 2] Schematic diagram showing a production unit for carrying out the production method of the present invention. [Diagram 3] FIG. 1 is a schematic diagram for explaining a manufacturing process based on the manufacturing method of the first embodiment; [Figure 4] Enlarged view of IV in Fig. 3 [Diagram 5] 1 is a flow chart showing an inner lamination process according to the manufacturing method of the present invention. [Figure 6] A flow chart showing the outer surface lamination process of the manufacturing method according to the present invention. [Figure 7]FIG. 11 is a schematic diagram for explaining a manufacturing process based on the manufacturing method of the second embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] Hereinafter, an embodiment of a method for producing a laminated pulp container according to the present invention will be described with reference to FIGS.

[0032] <<First embodiment>> As shown in Fig. 1(A), a laminated pulp container 1 manufactured by the manufacturing method of the present invention is in the form of a tray having a storage recess 2 for storing food or other contents and a flange 3 on the edge of the opening. As shown in Fig. 1(B), the laminated pulp container 1 is composed of a multilayer structure 5 made of a plurality of layers. More specifically, the laminated pulp container 1 includes a pulp layer 6 made of pulp fibers and having a recess formed on one surface (hereinafter, the inner surface) for defining the storage recess 2, an inner surface laminate layer 7 bonded to the inner surface of the pulp layer 6, and an outer surface laminate layer 8 bonded to the other surface (hereinafter, the outer surface) of the pulp layer 6.

[0033] The pulp layer 6 is a sheet member formed into a tray shape, is made of pulp fibers, and has air permeability. The pulp layer 6 is produced from a raw material liquid containing pulp fibers by a known method. For ease of explanation, the structure consisting of only the pulp layer 6 will be referred to as the container body 10, and the recess formed in the pulp layer 6 will be referred to as the main body recess 11.

[0034] The inner laminate layer 7 is formed by attaching an inner laminate film 12 (first laminate film; see FIG. 3), which is a plastic film, to the surface of the container body 10 on which the body recess 11 is formed, i.e., the inner surface. The inner laminate layer 7 covers the entire wall surface of the body recess 11. The body recess 11 is provided on the outer surface of the container body 10, so that a body protrusion 13 is provided which is pushed outward and protrudes outward. The outer laminate layer 8 is formed by attaching an outer laminate film 14 (second laminate film; see FIG. 3), which is a plastic film, to the outer surface of the container body 10 including the body protrusion 13. The outer laminate layer 8 covers the entire outer surface of the container body 10.

[0035] Next, a manufacturing unit 20 used in manufacturing the laminated pulp container 1 will be described. As shown in Fig. 2, the manufacturing unit 20 has a known paper-making device (not shown) for paper-making the container body 10 from the raw material liquid, an inner laminating device 21 that attaches the inner laminating film 12 to the inner side of the container body 10, and an outer laminating device 22 that attaches the outer laminating film 14 to the outer side. Below, the inner laminating device 21 and the outer laminating device 22 will be described in detail with reference to Fig. 2.

[0036] 2, the inner laminating device 21 has a pair of reels 23 supporting the inner laminating film 12 wound in a roll, a first transport device 24 transporting the inner laminating film 12, a first heating device 25, a first bonding device 26, and a first cutting device (not shown). The reels 23 are each provided on a horizontal plane so as to face each other with the first heating device 25, the first bonding device 26, and the first cutting device in between.

[0037] The first transport device 24 transports the inner laminate film 12 while keeping it taut by unwinding it from a reel 23 (hereinafter, referred to as the delivery reel 23A) located on the side of the first heating device 25 and winding it onto a reel 23 (hereinafter, referred to as the take-up reel 23B) located on the side of the first bonding device 26.

[0038] The first heating device 25 includes two heaters 25A for heating both sides of the inner laminating film 12, and a roller 25B for transporting the inner laminating film 12.

[0039] 2, the first bonding device 26 includes a pair of a first female die 28 and a first male die 29, a first drive device 30 for relatively moving the first female die 28 and the first male die 29, a first exhaust device 31, and a first control device 32 for receiving input from an operator and controlling the first drive device 30 and the first exhaust device 31. The first female die 28 is a stainless steel mold, and includes a first cavity 28A recessed in a shape corresponding to the main body recess 11. The first female die 28 is provided with a first vent hole 28B that extends from the outer surface to a wall surface (hereinafter, the inner surface) that defines the first cavity 28A and opens on the inner surface.

[0040] The first male die 29 has a first pressing portion 29A having an outer surface shape similar to the inner surface shape of the first cavity 28A. In this embodiment, an elastic member 29B that can be elastically deformed by pressing the first pressing portion 29A against the inner surface of the first cavity 28A is provided on the outer surface of the first pressing portion 29A. The elastic member 29B is, for example, a rubber-like member, and more preferably made of silicone rubber. This makes it possible to prevent the elastic member 29B from being deformed or altered by heat from the inner surface laminate film 12.

[0041] Based on a signal from the first control device 32, the first drive device 30 moves the first male die 29 between a position where the first pressing portion 29A is separated from the first cavity 28A (separation position) and a position where the first pressing portion 29A is inserted into the first cavity 28A and they fit together (insertion position). In this embodiment, the first male die 29 is disposed above the first female die 28, and the first drive device 30 moves the first female die 28 and the first male die 29 in the vertical direction to move them between the separation position and the insertion position.

[0042] The first exhaust device 31 is connected to the first ventilation hole 28B via a predetermined pipe 28C. The first exhaust device 31 is driven based on a signal from the first control device 32, and exhausts air from the first ventilation hole 28B.

[0043] The first control device 32 is a computer equipped with a central processing unit (CPU) and storage devices such as a memory and a HDD, and has a first input unit 32A that accepts input from an operator. The first input unit 32A is, for example, a touch panel. The first control device 32 drives the first transport device 24 to transport the inner laminating film 12 based on the input to the first input unit 32A. The first control device 32 also drives the first drive device 30 based on the input to the first input unit 32A to move the first female die 28 and the first male die 29 between the separation position and the insertion position. The first control device 32 also drives the first exhaust device 31 based on the input to the first input unit 32A to exhaust air from the first ventilation hole 28B.

[0044] The first cutting device cuts the inner surface laminate film 12 attached to the inner surface of the container body 10. By cutting the inner surface laminate film 12 by the first cutting device, the container body 10 can be separated from the inner surface laminate film 12 wound in a roll.

[0045] The outer laminating device 22 has a pair of reels 33 that support the outer laminating film 14 wound in a roll, a second transport device 34 that transports the outer laminating film 14, a second heating device 35 (film heating device), a second bonding device 36, and a second cutting device (not shown). The reels 33 are each provided on a horizontal plane so as to face each other with the second heating device 35, the second bonding device 36, and the second cutting device in between.

[0046] The second transport device 34 transports the outer surface side laminate film 14 while keeping it taut by pulling it out from the reel 33 (hereinafter, the delivery reel 33A) located on the side of the second heating device 35 and winding it up onto the reel 33 (hereinafter, the take-up reel 33B) located on the side of the second bonding device 36.

[0047] The second heating device 35 is similar to the first heating device 25, and includes two heaters 35A for heating both sides of the outer laminating film 14, and a roller 35B for transporting the outer laminating film 14.

[0048] The second bonding device 36 includes a pair of a second female die 38 (mold body) and a second male die 39 (mold body), a second drive device 40 for relatively moving the second female die 38 and the second male die 39, a compressed air supply device 41, a second exhaust device 42, and a second control device 43 for receiving input from an operator and controlling the second drive device 40, the compressed air supply device 41 (gas supply device), and the second exhaust device 42. In this embodiment, the second bonding device 36 further includes a compressed air heater 45 (gas heating device) for heating the compressed air supplied from the compressed air supply device 41.

[0049] The second female die 38 is a mold body having a second cavity 38A, which is a recess recessed upward and has a shape corresponding to the main body protrusion 13. More specifically, the second female die 38 has a metal base 38B and an elastic member 38C similar to that of the first male die 29. The base 38B has a base recess 38D recessed upward to form the second cavity 38A, and the elastic member 38C covers the wall surface defining the base recess 38D and the peripheral portion of the opening of the base recess 38D. Thus, at least the wall surface of the second cavity 38A is covered by the elastic member 38C. The elastic member 38C provided in the second female die 38 may be the same as the elastic member 29B provided in the first male die 29, and is preferably made of silicone rubber. The second female die 38 is provided with a plurality of second vent holes 38E that communicate from the outside to the inside of the second cavity 38A and open at the bottom surface of the second cavity 38A (the surface that defines the upper boundary of the second cavity 38A).

[0050] In this embodiment, the second cavity 38A is recessed into a substantially rectangular parallelepiped shape. At least one of the second air holes 38E opens in the substantially central portion of the bottom surface of the second cavity 38A.

[0051] The second male die 39 is a stainless steel die having a second pressing portion 39A at its lower portion. The second pressing portion 39A has an outer surface shape that matches the inner surface shape of the main body recess 11, and as shown in FIG. 2, has an outer surface shape similar to the inner surface shape of the second cavity 38A.

[0052] Based on a signal from the second control device 43, the second drive device 40 moves the second female die 38 between a position (separation position) where the second cavity 38A is separated from the second pressing part 39A and a position (insertion position) where the second pressing part 39A is inserted into the second cavity 38A and they fit together. In this embodiment, the second female die 38 is disposed above the second male die 39, and the second drive device 40 moves the second female die 38 and the second male die 39 in the vertical direction to move them between the separation position and the insertion position.

[0053] The compressed air supply device 41 is connected to the second vent hole 38E by a pipe 41A. The compressed air supply device 41 is driven based on a signal from the second control device 43 to supply compressed air into the pipe 41A and release the compressed air from the second vent hole 38E. That is, the pipe 41A defines a compressed air introduction path 41B (gas introduction path) from the compressed air supply device 41 to the inside of the second cavity 38A, and the second vent hole 38E functions as an introduction hole for introducing the compressed air into the inside of the second cavity 38A. However, in this embodiment, the compressed air supply device 41 supplies compressed air into the pipe 41A, but it may be any other device that supplies compressed gas to the pipe 41A, for example, compressed nitrogen gas may be supplied into the pipe 41A.

[0054] The second exhaust device 42 is connected to the pipe 41A via a predetermined pipe 42A. The second exhaust device 42 is driven based on a signal from the second control device 43 to reduce the pressure in the pipe 41A to atmospheric pressure. The second exhaust device 42 may be a device that releases the pipe 41A to the atmosphere to reduce the internal pressure of the pipe 41A to atmospheric pressure, or may be a pump that forcibly reduces the pressure in the pipe 41A.

[0055] The second control device 43, like the first control device 32, is a computer equipped with a central processing unit (CPU) and storage devices such as a memory and a HDD, and has a second input unit 43A that accepts input from an operator. The second input unit 43A is, for example, a touch panel. The second control device 43 drives the second transport device 34 based on the input to the second input unit 43A to transport the outer surface side laminating film 14. The second control device 43 also drives the second drive device 40 based on the input to the second input unit 43A to move the second female die 38 and the second male die 39 between the separation position and the insertion position. The second control device 43 also drives the second exhaust device 42 based on the input to the second input unit 43A to exhaust air from the second ventilation hole 38E. The second control device 43 also drives the compressed air supply device 41 based on the input to the second input unit 43A to release compressed air from the second ventilation hole 38E.

[0056] The compressed air heater 45 is a device for heating the compressed air that is supplied from the compressed air supply device 41 and passes through the compressed air introduction path 41B, and is provided in the pipe 41A.

[0057] The second cutting device cuts the outer laminate film 14 attached to the outer surface of the container body 10. By cutting the outer laminate film 14 by the second cutting device, the container body 10 can be separated from the outer laminate film 14 wound in a roll.

[0058] Next, the manufacturing process of the laminated pulp container 1 will be described with reference to Figs. 3 to 6. The manufacturing process includes a papermaking process, an inner lamination process (first process, ST1 to ST7 in Fig. 5), and an outer lamination process (second process, ST11 to ST16 in Fig. 6) in the order described. The papermaking process is a process of papermaking the container body 10 from a raw material liquid containing pulp fibers, and may be based on a known method. The inner lamination process is a process of attaching an inner lamination film 12 to the inner side of the container body 10 after papermaking, and the outer lamination process is a process of attaching an outer lamination film 14 to the outer side of the container body 10 after the inner lamination process is completed. First, the inner lamination process will be described below with reference to Figs. 3 and 5.

[0059] In the first step of the inner lamination process (step ST1, see FIG. 5), the worker drives the first transport device 24 to transport the inner lamination film 12 between the heaters 25A of the first heating device 25, and heats both sides of the film (see FIG. 3(A)). An adhesive is applied to the back side of the heated inner lamination film 12 (the side to be attached to the container body 10).

[0060] Next, the worker places the container body 10 so that the body protrusion 13 of the container body 10 protrudes downward, and inserts the body protrusion 13 into the first cavity 28A of the first female die 28, thereby setting the container body 10 in the first female die 28 (step ST2). After that, the worker performs a predetermined input to the first input unit 32A to drive the first transfer device 24. As a result, the heated inner lamination film 12 is transferred between the container body 10 and the first male die 29, and the heated inner lamination film 12 is placed between the container body 10 and the first male die 29 (see FIG. 3(B) . Step ST3). At this time, the inner lamination film 12 is held by the pair of reels 23 in a stretched state.

[0061] Thereafter, when the worker performs a predetermined input to the first input unit 32A, the first control device 32 causes the first driving device 30 to raise the first female die 28 so that the container body 10 approaches the inner surface side laminate film 12. Thereafter, the first control device 32 lowers the first male die 29, inserts the first pressing unit 29A into the body recess 11, and engages the first female die 28 with the first male die 29 (see FIG. 3(C), step ST4).

[0062] Thereafter, the first driving device 30 further lowers the first male mold 29, and the back surface of the inner laminate film 12 contacts the surface (inner surface) of the container body 10 on which the main body recess 11 is provided (see FIG. 3(C)). Furthermore, the first control device 32 drives the first driving device 30 to lower the first male mold 29, and presses the elastic member 29B against the container body 10 with a predetermined load (see FIG. 3(D); step ST5). At this time, the inner laminate film 12 is pressed against the surface (inner surface) of the container body 10 on which the main body recess 11 is provided by the elastic member 29B, and the inner laminate film 12 is pressure-bonded to the container body 10. As a result, the inner laminate film 12 is adhered to the container body 10.

[0063] After the back surface of the inner laminate film 12 comes into contact with the inner surface of the container body 10, until the bonding of the inner laminate film 12 is completed, the first control device 32 drives the first exhaust device 31 to exhaust air from the first ventilation hole 28B between the inner laminate film 12 and the container body 10. This reduces the pressure between the inner laminate film 12 and the container body 10. Therefore, the inner laminate film 12 and the container body 10 can be tightly attached to each other without air remaining between them and generating air bubbles.

[0064] When a predetermined time has elapsed after the first male die 29 is pressed against the inner surface of the container body 10 by the elastic member 29B, the first control device 32 raises the first male die 29 away from the first female die 28 and pulls out the first pressing part 29A from the first cavity 28A (step ST6). Then, the first control device 32 controls the first cutting device to cut the inner surface laminate film 12 (step ST7). Then, the first control device 32 stops driving the first exhaust device 31 and ends exhausting from the first ventilation hole 28B. This completes the inner surface lamination process.

[0065] Thereafter, the worker takes out the container body 10 with the inner laminating film 12 attached to the inner surface from the inner laminating device 21.

[0066] Next, the worker performs the outer lamination process shown in Figures 3, 4, and 6. In the first step of the outer lamination process (step ST11 in Figure 6), the worker drives the second transport device 34, transports the outer lamination film 14 between the heaters 35A of the second heating device 35, and heats both sides of the outer lamination film 14 (see Figure 3(E) (hereinafter, heating step)). An adhesive is applied to the back surface (adhesive surface) of the outer lamination film 14 to be heated.

[0067] When the heating step is completed, the worker places the container body 10 with the inner laminate film 12 attached to the inner surface so that the body recess 11 faces downward, and places the container body 10 over the second pressing portion 39A of the second male mold 39. As a result, the second pressing portion 39A is inserted into the body recess 11, and the container body 10 that has undergone the inner lamination step is set in the second male mold 39. At this time, the container body 10 with the inner laminate film 12 already attached to the inner surface is supported by the second male mold 39 (step ST12, hereinafter referred to as the supporting step).

[0068] When the supporting step is completed, the worker performs a predetermined input to the second input section 43A to drive the second transfer device 34. As a result, the heated outer laminate film 14 is transferred between the container body 10 and the second female die 38, and the heated outer laminate film 14 is placed between the container body 10 and the second female die 38 (step ST13, hereinafter, the placing step). At this time, the outer laminate film 14 is held by the pair of reels 33 in a pulled state. At this time, the second female die 38 is located on the side of the surface (the surface on which the adhesive surface is not provided) of the outer laminate film 14, and is placed in a position facing the outer surface of the container body 10 via the outer laminate film 14 and aligned.

[0069] Furthermore, when the operator inputs to the second input unit 43A, the second control device 43 controls the second drive device 40, the compressed air supply device 41, the second exhaust device 42, and the compressed air heater 45 to perform a bonding step of fitting the second female die 38 and the second male die 39 together to bond the outer laminate film 14 to the container body 10. The bonding step (step ST14) will be described in detail below.

[0070] In the bonding step, the second control device 43 first drives the second drive device 40 to lower the second female die 38 so that it approaches the surface of the outer laminate film 14. As a result, a space S is formed between the second female die 38 and the outer laminate film 14. The space S communicates with the outside via a gap P between the second female die 38 and the outer laminate film 14.

[0071] Thereafter, the second control device 43 raises the second male die 39 and inserts the second pressing portion 39A of the second male die 39 into the second cavity 38A. As a result, the outer laminating film 14 is pushed upward by the upper surface (protruding end surface) of the second pressing portion 39A.

[0072] During this time, the second drive device 40 drives the compressed air supply device 41 and the compressed air heater 45. This introduces heated compressed air into the space S between the outer laminate film 14 and the second female die 38. The introduced compressed air is discharged into the space S from the second air hole 38E of the second female die 38. The compressed air discharged into the space S flows toward the gap P (see the arrow in FIG. 3(G)). At this time, the compressed air is blown onto the outer laminate film 14 so that the outer laminate film 14 moves toward the outer surface of the container body 10. This causes the outer laminate film 14 to be pushed toward the outer surface of the container body 10, and the outer laminate film 14 moves toward the outer surface of the container body 10 (see the dashed arrow in FIG. 4).

[0073] In this embodiment, the second vent hole 38E is opened at approximately the center of the bottom surface of the second cavity 38A, so the compressed air discharged from the second vent hole 38E flows from top to bottom. This flow of compressed air causes the outer surface laminate film 14 to move from top to bottom toward the outer surface of the container body 10. This prevents air from being trapped between the outer surface laminate film 14 and the outer surface of the container body 10, which would otherwise cause air bubbles to form.

[0074] The second drive device 40 further raises the second male die 39, inserts the second pressing portion 39A of the second male die 39 into the second cavity 38A of the second female die 38, and engages the second female die 38 with the second male die 39. Until the second female die 38 and the second male die 39 are engaged with each other, air present between the outer laminate film 14 and the container body 10 passes through the inside of the container body 10 and is released to the outside from the edge of the container body 10 (see the dashed arrow in FIG. 3(G)).

[0075] Thereafter, the second control device 43 controls the second drive device 40 to move the second female die 38 downward, and press the elastic member 38C of the second female die 38 against the container body 10 with a predetermined load (see FIG. 3(H)). At this time, the elastic member 38C of the second female die 38 comes into contact with the outer laminate film 14, and the outer laminate film 14 is pressed against the outer surface of the container body 10 by the elastic member 38C. This makes the outer laminate film 14 more closely adhere to the container body 10. Air located between the outer laminate film 14 and the container body 10 is released to the outside from the edge of the container body 10, preventing air from remaining between the outer laminate film 14 and the outer surface of the container body 10.

[0076] When the elastic member 38C of the second female die 38 is pressed against the container body 10 with a predetermined load, the second control device 43 stops the compressed air supply device 41 and drives the second exhaust device 42 to exhaust air. This more reliably prevents air from remaining in the space S, making it easier for the elastic member 38C to deform along the outer surface of the container body 10. This makes it easier for the outer laminate film 14 to be in close contact with the outer surface of the container body 10.

[0077] 3(H), in this embodiment, the second female die 38 contacts the outer laminate film 14 only at the elastic member 38C. That is, the portion of the second female die 38 that contacts the outer laminate film 14 is formed by the elastic member 38C.

[0078] Next, the second control device 43 maintains the state in which the elastic member 38C of the second female die 38 is pressed against the container body 10 with a predetermined load for a predetermined time, and then moves the second female die 38 upward to separate the second pressing part 39A from the second cavity 38A (step ST15). When the separation is complete, the second control device 43 stops the second exhaust device 42. Thereafter, the lamination process on both the front and back sides is completed, and the excess outer laminate film 14 is cut by the second cutting device (step ST16), completing the laminated pulp container 1.

[0079] The effects of the manufacturing method of the laminated pulp container 1 configured as follows will be described. By providing the inner laminate layer 7 on the inner surface of the container body 10, it is possible to impart water resistance and oil resistance to the inner surface of the container body 10. This makes it possible to prevent water and oil from leaking out of the laminated pulp container 1 when food or the like is stored in the storage recess 2.

[0080] During shipping or reuse, laminated pulp containers 1 may be stacked on top of each other. At this time, the outer surface of the laminated pulp container 1 comes into contact with the inner surface of another laminated pulp container 1. In the laminated pulp container 1 according to the present invention, an outer laminate layer 8 is provided on the outer surface. This prevents pulp fibers from adhering to the inner surface of another laminated pulp container 1 that contacts the outer surface of the laminated pulp container 1 when the laminated pulp containers 1 are stacked. This prevents the cleanliness of the wall surface of the storage recess 2 from decreasing when the laminated pulp containers 1 are stacked. In addition, it is possible to prevent moisture and oil adhering to the wall surface of the storage recess 2 from adhering to the outer surface of another laminated pulp container 1 stacked and seeping into the inside of the container body 10.

[0081] Since the laminate film is made of plastic, it has poor breathability. Therefore, it is difficult to ventilate from the inner side of the container body 10 with only the inner laminate film 12 attached, and it is difficult to attach the outer laminate film 14 to the outer surface of the container body 10. In this embodiment, the outer laminate film 14 is pressed against the outer surface of the container body 10 by the second female die 38 and adhered to the container body 10. Therefore, since it is not necessary to vent the container body 10 to attach the outer laminate film 14, it is possible to adhere the laminate film to both sides of the container body 10.

[0082] In this embodiment, compressed air is introduced into the space S between the outer laminate film 14 and the second female die 38, and the outer laminate film 14 is blown thereto, so that the outer laminate film 14 moves to the outer surface of the container body 10. This makes it easier for the outer laminate film 14 to fit the outer surface of the container body 10, and makes it easier for the outer laminate film 14 to be tightly attached to the outer surface of the container body 10.

[0083] The second female die 38 is provided with a second vent hole 38E that opens on the bottom surface of the second cavity 38A. This makes it easy to introduce compressed air into the space S between the outer laminate film 14 and the second female die 38. In addition, in this embodiment, the second vent hole 38E is provided on the bottom surface (more preferably, approximately the center) of the second cavity 38A, so that a flow of compressed air from the top to the bottom, that is, a flow of compressed air in the direction flowing out from the second cavity 38A (see the solid arrow in FIG. 4), is generated. This flow of compressed air can blow the outer laminate film 14 toward the container body 10, and the outer laminate film 14 can be moved toward the container body 10. This makes it easier for the outer laminate film 14 to be in close contact with the outer surface of the container body 10. In addition, since the flow of compressed air is directed from the top to the bottom, the outer laminating film 14 is easily adhered from the top, preventing the occurrence of wrinkles, air bubbles, and the like.

[0084] The outer laminate film 14 is heated in step ST11. This makes the outer laminate film 14 more easily deformable, and therefore the outer laminate film 14 is more easily attached to the container body 10. Furthermore, in this embodiment, the compressed air is blown onto the outer laminate film 14 after being heated. Therefore, the outer laminate film 14 is less likely to be cooled by blowing the compressed air, and therefore the adhesion between the outer laminate film 14 and the container body 10 can be improved compared to when the compressed air is not heated.

[0085] In this embodiment, in step ST14, the outer laminate film 14 is pressed against the outer surface of the container body 10 by the elastic member 38C of the second female die 38. This makes it possible to more reliably exhaust air between the back surface of the outer laminate film 14 and the outer surface of the container body 10, and to more reliably bond the outer laminate film 14 to the entire outer surface of the container body 10.

[0086] As shown in Fig. 3(H), the portion of the second female die 38 that comes into contact with the outer laminate film 14 is composed of an elastic member 38C. The elastic member 38C of the second female die 38 is made of silicone rubber and is elastically deformable, so that when the elastic member 38C is pressed against the container body 10, it deforms to match the shape of the container body 10. This makes it difficult for a gap to form between the outer laminate film 14 and the container body 10, thereby improving the adhesion of the outer laminate film 14 to the container body 10.

[0087] <<Second embodiment>> The method for manufacturing the laminated pulp container 1 according to the second embodiment differs from the first embodiment only in the bonding step of the outer laminate film 14, and other parts are the same as those of the first embodiment, so a description thereof will be omitted.

[0088] In the bonding step, the second control device 43 first drives the second drive device 40 to lower the second female die 38 and bring it into contact with the surface of the outer laminate film 14 (see FIG. 7(A)). This forms a space S between the second female die 38 and the outer laminate film 14, and further, the space S is effectively sealed. As a result, the space S is effectively sealed and becomes a sealed space. Here, being effectively sealed means that the internal pressure of the space S becomes higher than the outside air by supplying compressed air to the space S, and does not require that the air flow between the space S and the outside air be completely blocked.

[0089] After the second female die 38 is lowered and brought into contact with the surface of the outer laminate film 14, the second control device 43 drives the compressed air supply device 41 and the compressed air heater 45 to supply heated compressed air to the space S between the second female die 38 and the outer laminate film 14. This causes the internal pressure of the space S between the second female die 38 and the outer laminate film 14 to rise and become higher than atmospheric pressure.

[0090] Next, the second control device 43 drives the second drive device 40 to lower the second female die 38 and push the outer laminate film 14 downward (see FIG. 7(B)). Thereafter, the second control device 43 raises the second male die 39 to engage with the second female die 38 (see FIG. 7(C)). Thereafter, the elastic member 38C is pressed against the outer surface of the container body 10, thereby completing the bonding step. However, similarly to the first embodiment, while the elastic member 38C is being pressed against the outer surface of the container body 10, the second control device 43 may drive the second exhaust device 42 to make the internal pressure of the space S atmospheric pressure.

[0091] Next, the effect of the manufacturing method of the laminated pulp container 1 thus configured will be described. After the second female die 38 contacts the surface of the outer laminate film 14, while it is descending, the space S is maintained at a higher temperature than the outside air. At this time, as shown by the dashed arrow in FIG. 7(B), a load is applied to the outer laminate film 14 from the air trapped in the space S so as to expand the space S. This load presses the outer laminate film 14 more strongly against the outer surface of the container body 10. This allows the outer laminate film 14 to be pressed more strongly against the outer surface of the container body 10. Therefore, the outer laminate film 14 can be attached to the outer surface of the container body 10 with better adhesion.

[0092] The present invention has been described above with reference to its preferred embodiments. However, as will be easily understood by those skilled in the art, the present invention is not limited to such embodiments, and can be modified as appropriate without departing from the spirit of the present invention.

[0093] In the above embodiment, a step of attaching the inner laminate film 12 to the inner surface of the container body 10 is followed by a step of attaching the outer laminate film 14 to the outer surface of the container body 10, but this is not limited to the embodiment. A step of attaching the inner laminate film 12 to the inner surface of the container body 10 may be provided after the step of attaching the outer laminate film 14 to the outer surface of the container body 10.

[0094] Furthermore, not all of the components shown in the above embodiment are necessarily essential, and they can be appropriately selected without departing from the spirit of the present invention. [Explanation of symbols]

[0095] 1: Laminated pulp container 2: Storage recess 3: Flange 5:Multilayer structure 6: Pulp layer 7: Inner laminate layer 8: Outer laminate layer 10: Container body 11: Main body recess 12: Inner lamination film (first lamination film) 13: Main body protrusion 14: Outer lamination film (second lamination film) 20: Manufacturing unit 21: Inner surface laminating device 22: Outer lamination device 23: Reel 23A: Delivery reel 23B: Take-up reel 24: 1st transfer device 25: 1st heating device 25A: Heater 25B: Lola 26: 1st adhesive device 28: First female type 28A: First cavity 28B: First ventilation hole 28C: Piping 29: 1st male type 29A: First pressing part 29B: Elastic member 30: First drive unit 31: First exhaust device 32: First control device 32A: First input section 33: Reel 33A: Delivery reel 33B: Take-up reel 34:Second transfer device 35: Second heating device (film heating device) 35A: Heater 35B: Lola 36:Second adhesive device 38: Second female mold (the other side of the mold body) 38A: Second cavity (recess) 38B:Base 38C: Elastic material 38D: Base recess 38E: Second ventilation hole (introduction hole) 39: Second male mold (one of the mold bodies) 39A: Second pressing part 40: Second drive unit 41: Compressed air supply device (gas supply device) 41A: Piping 41B: Compressed air introduction path (gas supply path) 42: Second exhaust system 42A: Piping 43: Second control device 43A: Second input section 45: Compressed air heater (gas heating device) P: Gap S: Space ST1: Step ST2: Step ST3: Step ST4: Step ST5: Step ST6: Step ST7: Step ST11: Step (heating step) ST12: Step (support step) ST13: Step (placement step) ST14: Step (adhesive step) ST15: Step ST16: Step

Claims

1. The method includes a first step of attaching a first laminate film to an inner surface of a concave container body made of pulp fibers, and a second step of attaching a second laminate film to an outer surface of the container body, The second step comprises: a supporting step of supporting the container body to which the first laminate film is attached on a male mold corresponding to the container body; a positioning step of positioning a female mold that fits into the male mold so as to face the outer surface of the container body via the second laminate film; and a bonding step of fitting the male mold and the female mold together to bond the second laminate film to the container body, In the first step, the first laminate film is attached to the inner surface, the female mold has a recess and an introduction hole that communicates from the outside to the inside of the recess and opens at the center of a bottom surface of the recess, In the supporting step, the second laminate film is placed between the female mold and the container body in a stretched state, In the bonding step, gas is introduced between the female mold and the second laminate film from the introduction hole, thereby blowing the gas onto the portion of the second laminate film that is to be bonded to the center of the outer surface of the bottom wall of the container body, and pushing the portion of the second laminate film that is to be bonded to the center of the outer surface of the bottom wall of the container body toward the center of the outer surface of the bottom wall of the container body, while moving the male mold toward the female mold to insert it into the recess of the female mold, thereby adhering the second laminate film to the outer surface of the bottom wall of the container body, and then, while introducing the gas from the introduction hole into the gap between the female mold and the container body, passing through the outer surface of the bottom wall of the container body and the outer surface of the side wall of the container body, and leading to the outside, the male mold is fitted into the female mold, thereby bonding the second laminate film to the container body.

2. 2. A method for manufacturing a laminated pulp container as described in claim 1, wherein in the bonding step, the female mold is brought into contact with the second laminate film to form an airtight space between the female mold and the second laminate film, and the gas is introduced into the airtight space through the introduction hole to increase the internal pressure of the airtight space.

3. A heating step of heating the second laminating film is included before the placing step, 3. The method for producing a laminated pulp container according to claim 1, wherein the gas is heated before being blown onto the second laminate film in the bonding step.

4. The female mold is provided with an elastic member capable of elastic deformation, 4. The method for manufacturing a laminated pulp container according to claim 1, wherein the elastic member is pressed against the container body in the bonding step.

5. 5. The method for producing a laminated pulp container according to claim 4, wherein in the bonding step, when the elastic member is pressed against the container body, air is evacuated between the female mold and the second laminate film.

6. A laminated pulp container manufacturing apparatus for manufacturing a laminated pulp container in which a laminate film is attached to both sides of a container body made of pulp fibers, comprising: A pair of mold bodies including a female mold having a recess and an introduction hole that opens to a bottom surface of the recess, and a male mold having a protrusion that fits into the recess; a drive device for fitting the female mold and the male mold together; A gas supply device connected to the inlet; a control device capable of controlling the gas supply device and the drive device, The introduction hole is provided at the center of the bottom surface of the female mold, The container body is supported by the male mold, and the laminate film is arranged in a stretched state between the female mold and the container body, The control device includes: The driving device is driven to bring the female mold close to the lamination film; the gas supply device is driven to introduce gas from the inlet between the female mold and the laminate film, thereby blowing the gas onto the portion of the laminate film that is to be bonded to the center of the outer surface of the bottom wall of the container body, and pushing the portion of the laminate film that is to be bonded to the center of the outer surface of the bottom wall of the container body toward the center of the outer surface of the bottom wall of the container body; while driving the drive device, the male mold is moved toward the female mold to insert the male mold into the recess of the female mold, thereby adhering the laminate film to the outer surface of the bottom wall of the container body; Then, the gas supply device is driven to introduce the gas from the inlet hole into the gap between the female mold and the container body, passing through the outer surface of the bottom wall of the container body and the outer surface of the side wall of the container body to the outside, while the driving device engages the male mold with the female mold to bond the laminate film to the container body.This is a laminated pulp container manufacturing device.

7. 7. The apparatus for producing a laminated pulp container according to claim 6, further comprising an exhaust device connected to the inlet.

8. 8. The laminated pulp container manufacturing apparatus according to claim 6, wherein the female mold is provided with an elastic member capable of being elastically deformed.

9. a film heating device for heating the laminate film; The laminated pulp container manufacturing apparatus according to any one of claims 6 to 8, further comprising a gas heating device provided in a gas inlet path leading from the gas supply device to the inlet hole, for heating the gas passing through the gas inlet path.

Citation Information

Patent Citations

  • Water-resistant pulp mold container

    JP2000309322A

  • Pulp mold tray and its producing method

    JP2002002655A

  • Laminated pulp container, and its manufacturing method

    JP2007030925A

  • Molding apparatus of paper-made sealed container

    JP2012076306A

  • Molded article coated with film

    WO2013008318A1