Inorganic insulation material and method for forming inorganic insulation layer
A nonflammable inorganic heat insulating material with specific cement and rock wool ratios is sprayed to form a low thermal conductivity and high adhesive strength layer, addressing the flammability and efficiency issues of existing materials, enhancing safety and energy efficiency in structures.
Patent Information
- Application Number
- JP2020160460
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-25
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-09-25
AI Technical Summary
Existing heat insulating materials used in architectural and civil engineering structures are either highly flammable or have high thermal conductivity, leading to poor heating and cooling efficiency, and existing fire-resistant coatings are bulky and use harmful CFCs.
An inorganic heat insulating material composed of cement slurry and rock wool, with specific water-to-cement-to-rock wool ratios of 0.7 to 3.0 and 0.05 to 0.3, respectively, is sprayed onto structures using a specialized gun to form a nonflammable, low thermal conductivity, and high adhesive strength layer.
The material achieves low thermal conductivity, low bulk density, and high adhesion strength, making it an effective and safe substitute for conventional insulating materials, reducing fire risk and improving energy efficiency.
Smart Images

Figure 0007553301000003 
Figure 0007553301000004 
Figure 0007553301000005
Abstract
Description
[Technical field]
[0001] The present invention relates to an inorganic thermal insulation material and a method for forming an inorganic thermal insulation layer, and more particularly to an inorganic thermal insulation material composed of a substantially non-combustible inorganic material and a method for forming an inorganic thermal insulation layer by spraying the inorganic thermal insulation material. [Background technology]
[0002] Architectural and civil engineering structures are constructed from materials such as steel, concrete, mortar, stone, brick, wood, tile, plaster, glass, and earth. However, structures constructed solely from these materials have high thermal conductivity and allow heat to escape easily, resulting in poor heating and cooling efficiency. For this reason, foamed resin insulating materials such as bead-method polystyrene foam, extruded polystyrene foam, and rigid urethane foam are widely used as insulating materials. However, many of these are flammable, and fires have occurred both in Japan and overseas due to the ignition of foamed resin insulation materials.
[0003] On the other hand, in order to impart fire resistance, a rock wool spraying method is being used in which a fireproof coating material made of rock wool, cement, and water is sprayed onto structural components. This fireproof coating material has excellent performance in that it can protect the coated components for a certain period of time even when exposed to flames of 1000°C or higher, but it has a high bulk density and its insulating properties are less than half that of urethane foam using fluorocarbons, making it difficult to use as a substitute for foamed resin insulating materials. In addition, a non-combustible spray insulation material made by binding rock wool with synthetic resin has been proposed (for example, see Patent Document 1), but since this non-combustible spray insulation material contains synthetic resin as a binder, it is not essentially composed of a non-combustible inorganic material. Therefore, an insulation material composed of a substantially non-combustible inorganic material has been desired. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-087479 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention relates to providing an inorganic insulation material which is substantially composed of a non-flammable inorganic material, has low thermal conductivity and bulk density when dry, and has high adhesion strength, as well as a method for forming an inorganic insulation layer by spraying the same. [Means for solving the problem]
[0006] As a result of extensive research, the inventors have discovered that an inorganic insulating material in which the ratio of the mass of water to the sum of the mass of cement and the mass of rock wool is 0.7 to 3.0, and the ratio of the mass of cement to the sum of the mass of cement and the mass of rock wool is 0.05 to 0.3, has low thermal conductivity and bulk density when dry and high adhesion strength, and have completed the present invention.
[0007] That is, the present invention provides the following: <1> ~ <3> This provides: <1> An inorganic insulating material comprising (A) a cement slurry containing cement and water as main components, and (B) rock wool, wherein a ratio (W / (C+RW)) of the mass of the water (W) to the sum of the mass of the cement (C) and the mass of the rock wool (RW) is 0.7 to 3.0, and a ratio (C / (C+RW)) of the mass of the cement (C) to the sum of the mass of the cement (C) and the mass of the rock wool (RW) is 0.05 to 0.3. <2> The cement concentration of the cement slurry is 3 to 30% by mass. <1> 2. The inorganic heat insulating material according to claim 1 . <3> The rock wool and the cement slurry are separately sent to a spray gun having a rock wool pipeline with a rock wool nozzle at the tip and one or more cement slurry nozzles arranged on the outer periphery of the rock wool nozzle and / or in the rock wool pipeline, and the rock wool supplied to the rock wool pipeline is sprayed from the rock wool nozzle, and the cement slurry is sent to the cement slurry nozzle and sprayed from the cement slurry nozzle, thereby A method for forming an inorganic insulation layer, comprising mixing rock wool with the cement slurry and spraying the resulting mixture onto an object to be coated to form an inorganic insulation layer made of a rock wool composition, wherein the ratio (W / (C+RW)) of the mass of water (W) to the sum of the mass of cement (C) and the mass of rock wool (RW) is 0.7 to 3.0, and the ratio (C / (C+RW)) of the mass of cement (C) to the sum of the mass of cement (C) and the mass of rock wool (RW) is 0.05 to 0.3. Effect of the Invention
[0008] The inorganic heat insulating material of the present invention has a low thermal conductivity and a low bulk density when dried, and has a high adhesive strength. Therefore, according to the method for forming an inorganic heat insulating material layer of the present invention, an inorganic heat insulating material layer having a low thermal conductivity, a low bulk density, and a high adhesive strength can be formed. [Brief description of the drawings]
[0009] [Figure 1] 1 is a schematic diagram of an example of a spraying device used in the method for forming an inorganic insulation layer (spraying method) of the present invention. [Diagram 2] FIG. 2 is a conceptual cross-sectional view of an example of a spray gun (center gun) used in the present invention. [Diagram 3] 1 is a photograph showing the rock wool granular cotton used in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Inorganic insulation material] The inorganic heat insulating material of the present invention contains (A) a cement slurry mainly composed of cement and water, and (B) rock wool, and is characterized in that the ratio (W / (C+RW)) of the mass of the water (W) to the sum of the mass of the cement (C) and the mass of the rock wool (RW) is 0.7 to 3.0, and the ratio (C / (C+RW)) of the mass of the cement (C) to the sum of the mass of the cement (C) and the mass of the rock wool (RW) is 0.05 to 0.3.
[0011] The inorganic heat insulating material of the present invention has a ratio (W / (C+RW)) of 0.7 to 3.0. If the ratio (W / (C+RW)) is less than 0.7, spraying failure is likely to occur when forming the inorganic heat insulating material layer. If the ratio (W / (C+RW)) is more than 3.0, the cement slurry pressure increases, making it unsafe to form the inorganic heat insulating material layer. The ratio (W / (C+RW)) is preferably 0.8 to 2.7, more preferably 0.82 to 2.64, still more preferably 1.1 to 1.4, still more preferably 1.17 to 1.36, and particularly preferably 1.17 to 1.32, from the viewpoints of bone dry bulk density, thermal conductivity, and adhesive strength.
[0012] In addition, the inorganic heat insulating material of the present invention has a ratio (C / (C+RW)) of 0.05 to 0.3. If the ratio (C / (C+RW)) is less than 0.05, the adhesive strength is insufficient. If the ratio (C / (C+RW)) is more than 0.3, the thermal conductivity is high. The ratio (C / (C+RW)) is preferably 0.06 to 0.27, more preferably 0.08 to 0.27, further preferably 0.08 to 0.15, and particularly preferably 0.1 to 0.15, from the viewpoints of the bone dry bulk density, the thermal conductivity, and the adhesive strength.
[0013] The ratio (RW / C) of the mass of rock wool (RW) to the mass of cement (C) is preferably 1 to 20, more preferably 2 to 17, further preferably 2 to 13, and particularly preferably 5 to 13, from the viewpoints of bone dry bulk density, thermal conductivity, and adhesive strength. The ratio (W / RW) of the mass of water (W) to the mass of rock wool (RW) is preferably 0.5 to 3.5, more preferably 1 to 3, still more preferably 1 to 1.43, and particularly preferably 1.3 to 1.43, from the viewpoints of bone dry bulk density, thermal conductivity, and adhesive strength. The ratio (C / RW) of the mass (C) of cement to the mass (RW) of rock wool is preferably 0.01 to 0.4, more preferably 0.05 to 0.4, still more preferably 0.08 to 0.4, and particularly preferably 0.08 to 0.2, from the viewpoints of bone dry bulk density, thermal conductivity, and adhesive strength.
[0014] In this specification, the term "inorganic insulation material" refers to an insulation material that is substantially composed of an inorganic material. The term "non-flammable inorganic material" encompasses cement, rock wool, and water. The term "inorganic insulation layer" refers to an insulation layer formed by spraying the inorganic insulation material. The total content of cement, water and rock wool is preferably 97.5 to 100 mass%, more preferably 98 to 100 mass%, still more preferably 99 to 100 mass%, and particularly preferably 99.9 to 100 mass%, based on the total mass of the inorganic thermal insulation material.
[0015] The cement used in the present invention may be any hydraulic cement, including, for example, various Portland cements such as ordinary, early strength, extra early strength, low heat, and moderate heat, special cements such as white cement, ecocement, and alumina cement, and various mixed cements obtained by mixing fly ash, blast furnace slag, silica fume, or limestone powder with these Portland cements or special cements. One of these may be used alone, or two or more may be used in combination.
[0016] The above cement is mixed with water and used as a cement slurry (cement paste). The cement concentration of the cement slurry, i.e., the cement slurry concentration, is preferably 3 to 30 mass%, more preferably 4 to 25 mass%. The water content is preferably 70 to 97 mass%, more preferably 75 to 96 mass%, based on the total mass of the cement slurry. The cement slurry may be any as long as it contains cement and water as the main components, and the total content of cement and water is preferably 98 to 100 mass%, more preferably 98.5 to 100 mass%, even more preferably 99 to 100 mass%, and particularly preferably 99.9 to 100 mass%, based on the total mass of the cement slurry.
[0017] The cement slurry may contain one or more admixtures as long as the effects of the present invention are not impaired. Examples of the admixtures include cement dispersants, expansion agents, waterproofing agents, rust inhibitors, shrinkage reducing agents, thickeners, water retention agents, pigments, fibers, water repellents, efflorescence inhibitors, quick-setting agents (materials), quick-hardening agents (materials), setting retarders, foaming agents, defoamers, gypsum, ground granulated blast furnace slag, pozzolanic substances, water repellents, polymers for cement, and surface hardeners. The admixtures are preferably inorganic admixtures, but organic admixtures can also be used in amounts of about 5 parts by mass or less per 100 parts by mass of cement.
[0018] The rock wool used in the present invention may be any material (mineral fiber) produced by quenching a material mainly composed of rocks or blast furnace slag melted in a melting furnace and then fibrousizing it, and includes, for example, slag wool produced from a material mainly composed of blast furnace slag. The rock wool used in the present invention is preferably granular rock wool (granular cotton). Granular rock wool can be prepared by pulverizing raw cotton, which is a collection of fiberized mineral fibers, with a cotton-opening machine, etc. Specifically, the raw rock wool can be prepared by subjecting it to one or more treatments selected from crushing, cotton-opening, cutting, classification (e.g., sieving), and granulation. In the present invention, when raw cotton is used as the rock wool, it is preferable to break it into small pieces using a cotton opener or the like before pumping. Also, when granular rock wool (granular cotton) is used as the rock wool, it is preferable to break it into small pieces using a cotton opener or the like before pumping, since this increases the contact surface area with the cement slurry. The content of rock wool is preferably 15 to 55 mass %, more preferably 20 to 50 mass %, still more preferably 24 to 45 mass %, and particularly preferably 24.5 to 43 mass %, based on the total mass of the inorganic thermal insulation material.
[0019] The inorganic insulating material of the present invention can be produced, for example, by pumping (A) a cement slurry containing cement and water as its main components, and (B) rock wool to a spray gun via separate routes, and then spraying (A) the cement slurry and (B) the rock wool from the respective nozzles of the spray gun and allowing them to merge and mix.
[0020] The inorganic heat insulating material of the present invention is composed of a substantially non-combustible inorganic material, and has low thermal conductivity, low bulk density when dried, and high adhesive strength. Therefore, the inorganic insulating material of the present invention can be used, for example, as a substitute for foamed resin-based insulating materials in walls, floors, ceilings, etc., and since it is composed of a substantially non-flammable inorganic material, it is difficult to burn and is unlikely to cause a fire due to ignition, making it extremely useful as an insulating material for structures, etc.
[0021] [Method of forming inorganic heat insulating layer] The method for forming an inorganic heat insulating layer of the present invention comprises: feeding rock wool and cement slurry separately to a spray gun having a rock wool pipe with a rock wool nozzle at its tip, and one or more cement slurry nozzles arranged on the outer periphery of the rock wool nozzle and / or within the rock wool pipe; spraying the rock wool supplied to the rock wool pipe from the rock wool nozzle; and feeding the cement slurry to the cement slurry nozzle and spraying the cement slurry from the cement slurry nozzle. The method for forming an inorganic insulation layer comprises mixing the rock wool and the cement slurry together and spraying the resulting mixture onto an object to be coated to form an inorganic insulation layer made of a rock wool composition, wherein the ratio (W / (C+RW)) of the mass of the water (W) to the sum of the mass of the cement (C) and the mass of the rock wool (RW) is 0.7 to 3.0, and the ratio (C / (C+RW)) of the mass of the cement (C) to the sum of the mass of the cement (C) and the mass of the rock wool (RW) is 0.05 to 0.3.
[0022] The inorganic heat insulating material layer is preferably formed using a spraying device used in a semi-dry rock wool spraying method used to form a fire-resistant coating material consisting of cement slurry and rock wool. Fig. 1 is a schematic diagram of an example of a spraying device used in the method for forming an inorganic heat insulating layer (spraying method) of the present invention, and this device is used in a semi-dry rock wool spraying method. Fig. 2 is a conceptual cross-sectional view of an example of a spray gun (center gun) used in the present invention. Here, a method of forming an inorganic thermal insulation layer using the spraying device shown in Fig. 1 will be described. As shown in Fig. 1, the spraying device 10 includes a spray gun 1, a rock wool pressure-feeding hose 9, a cotton-opening machine 20, a blower 14, a cement slurry pressure-feeding hose 6, a cement slurry pressure-feeding pump 7, a cement slurry storage tank 8, and a cement slurry suction hose 15. The cotton-opening machine 20 includes a first cotton-opening section 21, a second cotton-opening section 22, a screw feeder 24, a hopper 23, a rock wool pressure-feeding pipe 26, and a rotary feeder (fixed-volume supply device) 25.
[0023] The spray gun 1 used in the spraying device shown in Figure 1 is a center gun in which a cement slurry nozzle 3 is arranged near the center of a rock wool nozzle 2, but a gun in which one or more cement slurry nozzles are arranged on the outer periphery of the rock wool nozzle 2 (for example, a ring gun) can also be used in the method of forming an inorganic insulation layer of the present invention. In the center gun shown in FIG. 2, the cement slurry injection port 3 is located on the central axis 33 of the rock wool pipe 32. In the center gun shown in FIG. 2, the cement slurry injection port 3 is accommodated in a recessed state in the rock wool pipe 32 so as not to protrude from the tip of the rock wool pipe 32, but may protrude from the rock wool injection port 2 or may be located at the same position as the rock wool injection port 2. In addition, the rock wool pipe 32 is a straight pipe, and the cement slurry pipe 31 is a curved pipe, but both are preferably cylindrical. A part of the cement slurry pipe 31 (an area including the end opposite to the cement slurry injection port 3) protrudes to the outside from a pipe through hole provided in the wall surface of the rock wool pipe 32. Representative examples of center guns include the spray gun shown in Figures 1 and 2 of Japanese Utility Model Publication No. 55-054755 or a spray gun having no air pipe, or the inorganic fiber spray gun shown in Figure 2 of Japanese Utility Model Publication No. 59-024384.
[0024] The rock wool 11 is fed into a hopper 23 of a defibrillator 20. The fed rock wool 11 is defibrated in a first defibrillation section 21 provided at the bottom of the hopper 23, then sent to a second defibrillation section 22 by a screw feeder 24, and after being further finely defibrated in this second defibrillation section 22, it falls by its own weight into a rotary feeder 25 provided at the bottom of the second defibrillation section 22, and is supplied in a fixed amount to a rock wool pressure feed pipe 26 as a partition inside the rotary feeder 25 rotates.
[0025] The rock wool supplied in a fixed amount to the rock wool pressure pipe 26 is passed through the rock wool pressure hose 9 connected to the rock wool pressure pipe 26 by the air flow sent from the blower 14, and is supplied to the rock wool pipe 32 of the spray gun 1, and is sprayed (discharged) from the rock wool nozzle 2 toward the substrate 13.
[0026] The cement slurry 4 is stored in a cement slurry storage tank 8. The tip of a cement slurry suction hose 15 connected to the suction port of the cement slurry pressure pump 7 is inserted into the cement slurry 4 stored in the cement slurry storage tank 8. When the cement slurry pressure pump 7 is operated, the cement slurry 4 is sucked from the tip of the cement slurry suction hose 15, passes through the cement slurry pressure delivery hose 6, and passes through the cement slurry pipe 31 of the spray gun 1 connected to the hose 6, and is sprayed (discharged) from the cement slurry nozzle 3 at the tip towards the base 13.
[0027] The sprayed cement slurry 4 is atomized and mixed with the rock wool 5 sprayed from the rock wool nozzle 2 to become an inorganic insulation material, which is then sprayed onto the base 13 to form an inorganic insulation layer 12 consisting of the combined mixture of rock wool and cement slurry.
[0028] The components contained in the inorganic insulation layer made of a rock wool composition thus formed by the method for forming an inorganic insulation layer of the present invention (the inorganic insulation layer made of a confluent mixture of rock wool and cement slurry) and the content ratio and amount of each component are the same as the components contained in the inorganic insulation of the present invention and the content ratio and amount of each component. Here, the content ratio and amount of each component contained in the inorganic insulation layer refers to the value when sprayed onto the object to be coated. EXAMPLES
[0029] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.
[0030] [Test No. 1-11] <Formation of inorganic heat insulating layer> A cement paste was made using ordinary Portland cement (manufactured by Taiheiyo Cement Corporation) and water (waterworks in Sakura City, Chiba Prefecture), and together with rock wool (granular rock wool cotton (manufactured by Taiheiyo Materials Corporation) shown in Figure 3), it was sprayed onto the steel substrate (steel plate) of the wall surface using a device equipped with a center gun used in the semi-dry rock wool spraying method to form an inorganic insulation layer. The amount of rock wool sprayed at this time was 4.0 kg / min. The mixing ratio of each material and the composition ratio of the inorganic insulation (W / (C+RW), C / (C+RW)) are shown in Table 1. <Composition ratio of inorganic insulation material> ·W / (C+RW): Ratio of the mass of water (W) to the sum of the mass of cement (C) and the mass of rock wool (RW) C / (C+RW): Ratio of the mass of cement (C) to the sum of the mass of cement (C) and the mass of rock wool (RW)
[0031] The evaluation results of the spray application and the inorganic heat insulating materials produced are shown in Table 2. The evaluation methods of the spray application and the inorganic heat insulating materials are as follows. <Evaluation method for spray application> ·Safety The pressure of the cement slurry (slurry pressure) during spraying was measured. Slurry pressures of 1.0 MPa or less were evaluated as safe (symbol: ○), and those exceeding 1.0 MPa were evaluated as unsafe (symbol: ×). If the slurry pressure exceeds 1.0 MPa, there is a risk that the cement slurry pressure-transfer hose will burst and that the cement slurry pressure-transfer hose will come off the cement slurry pressure-transfer pump and / or the cement slurry pipe of the spray gun.
[0032] ·Dust amount The amount of dust generated during spray application was visually confirmed and compared with the amount of dust generated by the semi-dry rock wool spraying method used to form fire-resistant coating material (with the same composition as Test No. 1). If the amount of dust generated was about the same, it was rated as "good" (symbol: ○); if the amount of dust generated was clearly less, it was rated as "best" (symbol: ◎); and if the amount of dust generated was clearly more, it was rated as "poor" (symbol: ×).
[0033] <Evaluation method for inorganic insulation materials> Thermal conductivity In accordance with JIS A 1412-2 "Methods for measuring thermal resistance and thermal conductivity of thermal insulation materials - Part 2: Heat flow meter method (HFM method)", measurements were taken using an Eiko Seiki Co., Ltd. thermal conductivity measuring device "FOX200" at an average temperature of 20°C and a sample size of 200 x 200 x 30 mm. In addition, thermal conductivity was rated as “good” (symbol: ○) for 0.045 W / (m·K) or more and less than 0.050 W / (m·K), “best” (symbol: ◎) for less than 0.045 W / (m·K), and “poor” (symbol: ×) for 0.050 W / (m·K) or more.
[0034] ·Absolutely dry bulk density The volume (V) of the specimen was calculated from the outer dimensions of the specimen after the thermal conductivity measurement, and the bulk density (ρ) was calculated from this value and the mass (M) of the specimen at that time using the following formula (1). ρ=M / V (1) The dry bulk density is rated at 0.21 g / cm 3 More than 0.30g / cm 3 Below "good" (symbol: ○), 0.20g / cm 3The following are "best" (symbol: ◎), 0.31g / cm 3 The above was categorized as "fail" (symbol: x).
[0035] Adhesion strength A frame 10 mm wide and 40 mm high was attached to each side of the flat surface (350 x 350 mm) of a steel plate (350 x 350 x 40 mm) to create a formwork with an inner shape of 330 x 330 x 40 mm. After spraying inorganic insulation material to a thickness of 40 mm into the formwork, the surface was flattened with a trowel. After attaching a 100 x 100 x 0.8 mm iron plate to the surface of the inorganic insulation material with adhesive, cuts were made along each side of the iron plate down to the underlying steel plate. The maximum tensile stress of the iron plate attached to the surface of the inorganic insulation material was measured using a push-pull gauge to determine the adhesive strength. The adhesion strength was evaluated as "good" (symbol: ○) if it was between 1000 Pa and 2000 Pa, "excellent" (symbol: ◎) if it was between 2000 Pa and 3500 Pa, "best" (symbol: ◎◎) if it was 3500 Pa or more, and "poor" (symbol: ×) if it was less than 1000 Pa.
[0036] ·comprehensive evaluation The evaluation criteria for the overall evaluation are as follows: "Best" (symbol: ◎): When the thermal conductivity is rated "best" (symbol: ◎) and the adhesion strength is rated "excellent" (symbol: ◎) or "best" (symbol: ◎◎) "Good" (symbol: ○): At least one of the evaluation of thermal conductivity and the evaluation of adhesive strength is "good" (symbol: ○) and there is no "bad" (symbol: ×) in these two evaluations. "Poor" (symbol: ×): When at least one of the evaluation of thermal conductivity and the evaluation of adhesion strength is "poor" (symbol: ×).
[0037] [Table 1]
[0038] [Table 2]
[0039] The inorganic heat insulating materials of Test Nos. 2 to 8 (Examples) had low bulk density when dried, low thermal conductivity, excellent heat insulating properties, and high adhesive strength, and therefore excellent performance as a heat insulating material. Among these, the inorganic heat insulating materials of Test Nos. 5 to 7 were particularly excellent in heat insulating properties. The inorganic heat insulating materials of Test Nos. 5 to 6 were particularly excellent in heat insulating properties and adhesive strength. [Explanation of symbols]
[0040] 1 Spray gun (center gun) 2 Rock wool nozzle 3 Cement slurry nozzle 4. Cement Slurry 5. Unraveled rock wool 6. Cement slurry pressure transfer hose 7 Cement slurry pump 8. Cement slurry storage tank 9 Rock wool pressure transfer hose 10 Spraying equipment (spraying system) 11 Rockwool 12 Inorganic insulation layer consisting of a mixture of rock wool and cement slurry 13 Base (wall) 14 Blower 15 Cement slurry suction hose 20 Cotton opening machine 21 First Cotton Decomposition Department 22 Second cotton opening section 23 Hopper 24 Screw feeder 25 Rotary feeder (fixed quantity supply device) 26 Rock wool pressure pipe 31 Cement slurry pipeline 32 Rock wool pipe 33 Central axis of rock wool pipe
Claims
1. (A) a cement slurry containing cement and water as main components, and (B) rock wool; The total content of the cement, the water and the rock wool is 99 to 100% by mass based on the total mass of the inorganic insulation material, The ratio (W / (C + RW)) of the mass of the water (W) to the sum of the mass of the cement (C) and the mass of the rock wool (RW) is 0.7 to 3.0; An inorganic insulating material in which the ratio (C / (C+RW)) of the mass of the cement (C) to the sum of the mass of the cement (C) and the mass of the rock wool (RW) is 0.05 to 0.3 (excluding the case where the cement slurry contains a synthetic resin).
2. The inorganic heat insulating material according to claim 1, wherein the cement concentration of the cement slurry is 3 to 30 mass%.
3. A method for forming an inorganic insulation layer, comprising: feeding rock wool and cement slurry separately to a spray gun having a rock wool pipeline with a rock wool nozzle at its tip, and one or more cement slurry nozzles arranged on the outer periphery of the rock wool nozzle and / or within the rock wool pipeline; spraying the rock wool supplied to the rock wool pipeline from the rock wool nozzle, and feeding the cement slurry to the cement slurry nozzle and spraying the cement slurry from the cement slurry nozzle, thereby mixing the rock wool and the cement slurry and spraying the mixture onto an object to be coated, thereby forming an inorganic insulation layer made of a rock wool composition, The cement slurry is mainly composed of cement and water, The total content of the cement, the water and the rock wool is 99 to 100% by mass based on the total mass of the inorganic insulation material, The ratio (W / (C + RW)) of the mass of the water (W) to the sum of the mass of the cement (C) and the mass of the rock wool (RW) is 0.7 to 3.0; and a ratio (C / (C+RW)) of the mass of the cement (C) to the sum of the mass of the cement (C) and the mass of the rock wool (RW) is 0.05 to 0.3 (excluding the case where the cement slurry contains a synthetic resin).
Citation Information
Patent Citations
Composition containing granular inorganic fiber
JP1981140054A
Construction refractory material
JP1983069757A
Air-borne noncombustible insulation and construction method thereof
JP2012087479A
Fire-proof mortar
JP2014152101A
Granular fiber spray nozzle, granular fiber spray device and granular fiber spray method