Devulcanized rubber, rubber composition, rubber composition for tires, tires, hoses, belts, crawlers

By producing desulfurized rubber with controlled thermal decomposition and specific component ratios, the mechanical strength of crosslinked rubber products is improved, addressing the limitations of existing methods and enabling eco-friendly production of tires, hoses, and crawlers.

JP7553324B2Active Publication Date: 2024-09-18BRIDGESTONE CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020183040
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-15
Filing Date
2020-10-30
Publication Date
2024-09-18
Estimated Expiration
2040-10-30

AI Technical Summary

Technical Problem

Existing desulfurization methods for recycled rubber result in low molecular weight hydrocarbons, limiting the mechanical strength of crosslinked rubber products.

Method used

The production of desulfurized rubber with a weight average molecular weight of 260,000 to 600,000, comprising soluble and insoluble rubber components in specific ratios, using controlled thermal decomposition in solvents with aldehydes or compounds with aliphatic carbon-carbon double bonds, to maintain high molecular weight and improve mechanical strength.

Benefits of technology

This approach enables the creation of crosslinked rubbers with enhanced mechanical strength, suitable for tires, hoses, belts, and crawlers, while reducing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553324000003
    Figure 0007553324000003
  • Figure 0007553324000005
    Figure 0007553324000005
  • Figure 0007553324000006
    Figure 0007553324000006
Patent Text Reader

Abstract

To provide a desulfurized rubber and rubber composition with which it is possible to manufacture cross-linked rubber having excellent mechanical strength, a rubber composition for a tire with which it is possible to manufacture a tire having excellent mechanical strength, and a tire, hose, belt, and crawler having excellent mechanical strength.SOLUTION: The desulfurized rubber has a weight-average molecular weight greater than 260,000 and less than 600,000, and includes a solvent-soluble rubber component A and a solvent-insoluble rubber component B, wherein the content ratio of the rubber component B is less than 45 mass% of the total mass of content a of the rubber component A and content b of the rubber component B.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a devulcanized rubber, a rubber composition, a rubber composition for tires, a tire, a hose, a belt, and a crawler. [Background technology]

[0002] From the viewpoints of the environment and resource conservation, the regeneration of crosslinked rubber and its reuse as new crosslinked rubber have been considered. For example, Patent Document 1 discloses that in reclaimed rubber obtained by devulcanizing vulcanized rubber, the ratio of sol to gel is 10 to 80%, the weight average molecular weight (Mw) of the sol measured by gel permeation chromatography (GPC) is within the range of 20,000 to 300,000, and the swelling degree of the gel is 3.0 to 20.0. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2000-128901 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the devulcanization method described in Patent Document 1, the weight-average molecular weight of the devulcanized rubber that was actually produced in the examples was only 258,000, and further investigation is required to obtain liquid hydrocarbons with high molecular weights.

[0005] The present invention aims to provide a devulcanized rubber and rubber composition from which crosslinked rubber having excellent mechanical strength can be produced, a rubber composition for tires from which tires having excellent mechanical strength can be produced, and tires, hoses, belts, and crawlers having excellent mechanical strength, and an object of the present invention is to achieve this aim. [Means for solving the problem]

[0006] <1> A devulcanized rubber having a weight average molecular weight of more than 260,000 and less than 600,000, comprising a rubber component A soluble in a solvent and a rubber component B insoluble in a solvent, wherein the content of the rubber component B is less than 45% by mass of the total mass of a content a of the rubber component A and a content b of the rubber component B.

[0007] <2> The weight average molecular weight of the rubber component A is more than 300,000 and less than 600,000. <1> The devulcanized rubber described in <3> The rubber component A and the rubber component B each contain at least one selected from the group consisting of an isoprene skeleton, a butadiene skeleton, and a styrene-butadiene skeleton. <1> or <2> The devulcanized rubber described in <4> The rubber component A and the rubber component B each contain an isoprene skeleton. <1> ~ <3> 13. The devulcanized rubber according to any one of the preceding claims.

[0008] <5> Contains rubber components, <1> ~ <4> 2. A rubber composition comprising the devulcanized rubber according to claim 1 in an amount of more than 10 mass % in the rubber component. <6> Further, the rubber composition contains 20 to 120 parts by mass of a filler based on 100 parts by mass of the rubber component. <5> The rubber composition according to claim 1. <7> <5> or <6> A rubber composition for tires comprising the rubber composition according to claim 1.

[0009] <8> <7> A tire using the rubber composition for tires according to claim 1.

[0010] <9> <5> or <6> A hose using the rubber composition according to claim 1. <10> <5> or <6> A belt using the rubber composition described in . <11> <5> or <6> A crawler using the rubber composition described above. Effect of the Invention

[0011] According to the present invention, it is possible to provide a devulcanized rubber and a rubber composition from which crosslinked rubber having excellent mechanical strength can be produced, a rubber composition for tires from which tires having excellent mechanical strength can be produced, and tires, hoses, belts, and crawlers having excellent mechanical strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] <Devulcanized rubber> The devulcanized rubber of the present invention has a weight average molecular weight of more than 260,000 and less than 600,000, and contains a rubber component A that is soluble in a solvent and a rubber component B that is insoluble in a solvent, and the content of the rubber component B is less than 45 mass% of the total mass of the content a of the rubber component A and the content b of the rubber component B. The devulcanized rubber of the present invention is a rubber component that has been devulcanized by breaking down the sulfur crosslinks in vulcanized rubber, and is a recycled rubber that can be used to regenerate vulcanized rubber. However, it does not include powdered rubber that has been obtained by pulverizing vulcanized rubber into powder form.

[0013] Devulcanized rubber obtained by devulcanization treatment such as thermal decomposition of vulcanized rubber generally contains solids that remain undecomposed in addition to liquid products. When waste tires are used as the vulcanized rubber, the solids also contain fillers because tires usually contain fillers. In the case of isoprene rubber (IR), raw rubber before vulcanization generally has a weight average molecular weight (Mw) of about 1.2 million and a number average molecular weight (Mn) of about 400,000, and in the case of styrene-butadiene copolymer rubber (SBR), generally, the weight average molecular weight (Mw) is about 400,000 and the number average molecular weight (Mn) is about 100,000. The closer the Mw and Mn of the liquid hydrocarbons contained in the liquid component are to these values, the closer the molecular chain of the rubber obtained is to the raw rubber.

[0014] The liquid hydrocarbons contained in conventional devulcanized rubber are prone to having their rubber molecules broken down into smaller pieces during the devulcanization process, which tends to reduce their weight-average molecular weight. Therefore, even if the rubber is crosslinked again to obtain a crosslinked rubber, it is difficult to improve its mechanical strength. In contrast, the devulcanized rubber of the present invention has the above-mentioned structure, and therefore a crosslinked rubber having excellent mechanical strength can be produced.

[0015] Rubber component A is a component obtained as a liquid hydrocarbon by devulcanization treatment, and is a component that contributes to the re-crosslinking reaction and can re-crosslink when the devulcanized rubber is re-crosslinked. When the weight average molecular weight of rubber component A is greater than 260,000, the mechanical strength of the crosslinked rubber obtained by re-crosslinking the devulcanized rubber can be improved. Rubber component B is a solid component that remains without decomposition, and is unlikely to contribute to the re-crosslinking reaction even if the devulcanized rubber is re-crosslinked. By making the content of rubber component B in the devulcanized rubber less than 45% by mass of the total mass of rubber components A and B, the proportion of rubber component A, which is an effective component, increases, and it is believed that a crosslinked rubber having excellent mechanical strength can be produced. The devulcanized rubber of the present invention will be described in detail below.

[0016] (Rubber component A) Rubber component A is a rubber component soluble in a solvent among rubber components obtained by devulcanizing vulcanized rubber, and has a weight average molecular weight of more than 260,000 and less than 600,000. With respect to the rubber component A, being soluble in a solvent means that the solubility in 100 g of solvent is 10 g or more when left to stand at 25° C. under atmospheric pressure (0.1 MPa) for 20 hours.

[0017] Here, the solvent may be any known solvent, such as water; alcohol solvents such as methanol, ethanol, and 2-propanol; aliphatic or alicyclic hydrocarbon solvents such as hexane, cyclohexane, and heptane; aromatic hydrocarbon solvents such as benzene, chlorobenzene, toluene, and xylene; halogenated hydrocarbon solvents such as methylene chloride, 1,2-dichloroethane, chloroform, and carbon tetrachloride; ether solvents such as diethyl ether, tetrahydrofuran, and 1,4-dioxane; ester solvents such as methyl acetate and ethyl acetate; ketone solvents such as acetone and methyl ethyl ketone; amide solvents such as N,N-dimethylformamide; nitrile solvents such as acetonitrile and propionitrile; and aprotic polar solvents such as dimethyl sulfoxide, N-methylpyrrolidone, and N,N'-dimethylimidazolinone. These solvents may be used alone or in combination of two or more as necessary. Among the above, the solvent preferably includes an alcohol-based solvent and an ether-based solvent, and more preferably includes an ether-based solvent.

[0018] The solubility of rubber component A in an ether-based solvent when left overnight at 25°C under atmospheric pressure is preferably 3 g / 100 g or more, more preferably 4 g / 100 g or more, more preferably 10 g / 100 g or more, even more preferably 20 g / 100 g or more, still more preferably 55 g / 100 g or more, and even more preferably 65 g / 100 g or more.

[0019] The rubber component A is a liquid hydrocarbon. "Liquid" means that the substance is in a liquid state at room temperature (25°C) and atmospheric pressure (0.1 MPa) or is easily soluble in petroleum components (alcohol, diethyl ether, tetrahydrofuran, etc.) and becomes liquid.

[0020] The weight average molecular weight of the rubber component A is greater than 260,000 and less than 600,000. If the weight average molecular weight of rubber component A is 260,000 or less, the re-crosslinked rubber obtained by re-crosslinking the devulcanized rubber will not have excellent mechanical strength, and it will be difficult to obtain a rubber component that is a soluble component of the devulcanized rubber and has a weight average molecular weight of 600,000 or more. The weight average molecular weight of the rubber component A is preferably more than 300,000 and less than 600,000, more preferably 320,000 or more, and further preferably 350,000 or more. The weight average molecular weight of the rubber component A can be measured, for example, by gel permeation chromatography (GPC).

[0021] (Rubber component B) Rubber component B is a rubber component that is insoluble in a solvent among rubber components obtained by devulcanizing a vulcanized rubber, and is unlikely to contribute to the crosslinking reaction when the devulcanized rubber is re-crosslinked. With respect to the rubber component B, being insoluble in a solvent means that the solubility in 100 g of the solvent is less than 3 g. The type of the solvent is not particularly limited, and one or more of the above-mentioned types of solvents can be used. Among them, the solvent preferably includes an alcohol-based solvent and an ether-based solvent, and more preferably includes an ether-based solvent. The solubility of rubber component B in an ether solvent is preferably 3 g / 100 g or less, more preferably 2 g / 100 g or less, and even more preferably 1 g / 100 g or less.

[0022] The content of rubber component B in the devulcanized rubber is less than 45% by mass of the total mass of the content a of rubber component A and the content b of rubber component B. If the content of rubber component B in the devulcanized rubber is 45% by mass or more, the content of rubber component A, which is a cross-linking component when the devulcanized rubber is re-cross-linked, decreases, and the mechanical strength of the re-cross-linked rubber decreases. The content of rubber component B in the devulcanized rubber is preferably 40% by mass or less, more preferably 38% by mass or less, and even more preferably 35% by mass or less of the total mass of the content a of rubber component A and the content b of rubber component B. There is no particular lower limit for the content of rubber component B in the devulcanized rubber, but it is usually 15% by mass or more of the total mass of the content a of rubber component A and the content b of rubber component B.

[0023] The devulcanized rubber of the present invention may be a mixture of a soluble component (rubber component A) and an insoluble component (rubber component B) obtained by devulcanizing the same vulcanized rubber, although the devulcanized rubber may be a mixture of different soluble components (rubber component A) and insoluble components (rubber component B). Therefore, both rubber component A and rubber component B preferably contain at least one selected from the group consisting of an isoprene skeleton, a butadiene skeleton, and a styrene-butadiene skeleton, and preferably contain an isoprene skeleton.

[0024] <Manufacturing method of devulcanized rubber> In a first aspect, the method for producing devulcanized rubber of the present invention preferably includes a step of heating vulcanized rubber at 300°C or less in a reaction solvent containing an aldehyde having a hydrocarbon group having two or more carbon atoms to obtain devulcanized rubber. In addition, as a second aspect, it is preferable to have a step of heating the vulcanized rubber at 150° C. or more and 300° C. or less in a reaction solvent containing a compound which contains at least one aliphatic carbon-carbon double bond and in which the number of hydroxyl groups and the number of aldehyde groups are each zero, to obtain a devulcanized rubber. The step of obtaining the devulcanized rubber in the first and second embodiments described above may hereinafter be referred to as a "decomposition step". The method for producing devulcanized rubber of the present invention may include, in addition to the decomposition step, a drying step of drying the reaction product obtained in the decomposition step.

[0025] When the manufacturing method for devulcanized rubber includes the above steps, it is easy to obtain a liquid rubber component A having a weight average molecular weight of more than 260,000, and the content of rubber component B that is insoluble in a solvent is easy to be less than 45 mass% of the total mass of the content a of rubber component A and the content b of rubber component B.

[0026] The method for producing devulcanized rubber of the present invention is also effective for regenerating crosslinked rubber that has been crosslinked with a crosslinking agent other than a vulcanizing agent. A rubber composition containing liquid hydrocarbons corresponding to rubber component A can be obtained by heating the crosslinked rubber at 300°C or less in a reaction solvent containing an aldehyde having a hydrocarbon group with two or more carbon atoms, or by heating the vulcanized rubber at 150°C or more and 300°C or less in a reaction solvent containing a compound that has at least one aliphatic carbon-carbon double bond and has zero hydroxyl groups and zero aldehyde groups. The rubber composition or devulcanized rubber obtained by breaking down the crosslinked structure of the crosslinked rubber (including vulcanized rubber) in the above-mentioned decomposition step is sometimes referred to as "decomposition-produced organic matter".

[0027] It is believed that the method for producing devulcanized rubber of the present invention breaks bonds (carbon-carbon bonds) between carbon atoms derived from the rubber molecules that make up the vulcanized rubber, and bonds (e.g., carbon-sulfur bonds) between such carbon atoms and heteroatoms (oxygen atoms, sulfur atoms, etc.) derived from the crosslinking agent, due to the effects of heat and solvent, generating radicals and / or new bonds. It is believed that hydrogen atoms released from aldehydes having a hydrocarbon group with two or more carbon atoms are attracted to the highly reactive radical species generated by these scission, terminating the radical reaction. It is believed that aldehydes having a hydrocarbon group with two or more carbon atoms are more likely to donate hydrogen than alcohols, and are more likely to terminate the radical reaction. In addition, the primary aldehyde is oxidized to a primary carboxylic acid, which is oxygen required to scission the main chain of the rubber molecule, and this consumes the oxygen in the autoclave. As a result, it is believed that scission of the main chain is suppressed, and it is possible to obtain a larger amount of rubber component A, which is a liquid hydrocarbon with a higher molecular weight than conventional methods.

[0028] [Vulcanized rubber] Vulcanized rubber is a vulcanized product of a rubber component, and the rubber component (pure rubber component) that is the raw material of the vulcanized rubber may be either a diene rubber or a non-diene rubber. The diene rubber may be at least one selected from the group consisting of natural rubber (NR) and synthetic diene rubber. Examples of synthetic diene rubbers include polyisoprene rubber (IR), styrene-butadiene copolymer rubber (SBR), polybutadiene rubber (BR), ethylene-propylene-diene rubber (EPDM), chloroprene rubber (CR), halogenated butyl rubber, and acrylonitrile-butadiene rubber (NBR). Examples of non-diene rubbers include butyl rubber, ethylene propylene rubber, urethane rubber, silicone rubber, and acrylic rubber. These rubber components may be used alone or in combination of two or more.

[0029] Among the above, since rubber products such as tires generally use diene rubber, it is preferable that the rubber component contains 50% by mass or more of diene rubber. In other words, it is preferable that the crosslinked rubber is a crosslinked product of a rubber component containing 50 to 100% by mass of diene rubber. It is more preferable that the rubber component contains 70% by mass or more of diene rubber, and even more preferable that the rubber component contains 90% by mass or more of diene rubber. In addition, it is preferable that the diene rubber is at least one selected from the group consisting of natural rubber, polyisoprene rubber, polybutadiene, and styrene-butadiene copolymer rubber.

[0030] When vulcanized rubber is heated at 300°C or less in a reaction solvent containing an aldehyde with a hydrocarbon group having two or more carbon atoms, the carbon-sulfur bonds that mainly constitute the molecular structure of the vulcanized rubber undergo exchange reactions due to bond scission caused by heat and solvent effects, etc., and it is thought that the hydrogen atoms released from the aldehyde with a hydrocarbon group having two or more carbon atoms are attracted to the highly reactive radical species generated by the scission, thereby terminating the radical reaction. When the above-mentioned method for producing devulcanized rubber is applied to a crosslinked rubber obtained by using a crosslinking agent other than a vulcanizing agent, examples of the crosslinking agent for the rubber component include an organic peroxide-based crosslinking agent, an acid crosslinking agent, a polyamine crosslinking agent, a resin crosslinking agent, and an oxime-nitrosamine-based crosslinking agent.

[0031] (Filler) The vulcanized rubber may contain a filler. Tires generally contain reinforcing fillers such as carbon black and silica in order to improve various functions of the tire, such as durability and abrasion resistance. On the other hand, in a vulcanized rubber that does not contain a filler, the decomposition rate of rubber component A can be increased and the content of rubber component B can be reduced. As the filler, either silica or carbon black may be used alone, or both silica and carbon black may be used.

[0032] The silica is not particularly limited, and may be any type depending on the application, such as general-grade silica, special silica that has been surface-treated with a silane coupling agent, etc. As the silica, it is preferable to use, for example, wet silica. The carbon black is not particularly limited and can be appropriately selected depending on the purpose. For example, FEF, SRF, HAF, ISAF, and SAF grade carbon black are preferable. The content of the filler in the vulcanized rubber is preferably from 20 to 100 parts by mass, and more preferably from 30 to 90 parts by mass, per 100 parts by mass of the rubber component.

[0033] The vulcanized rubber may be a crosslinked product obtained by crosslinking a rubber composition containing, in addition to the rubber component and the above-mentioned filler, compounding agents commonly used in the rubber industry, such as softeners, stearic acid, antioxidants, zinc oxide, vulcanization accelerators, etc. Tires generally contain vulcanized rubber obtained by vulcanizing rubber compositions containing these compounding agents.

[0034] [Reaction Solvent] One example of the reaction solvent includes an aldehyde having a hydrocarbon group with two or more carbon atoms (compound 1 in the present invention). As another example, there may be mentioned an embodiment including a compound (compound 2 in the present invention) which contains at least one aliphatic carbon-carbon double bond and has zero hydroxyl groups and zero aldehyde groups. By selecting as the reaction solvent an aldehyde having a hydrocarbon group with two or more carbon atoms, or a compound containing at least one aliphatic carbon-carbon double bond and with zero hydroxyl and aldehyde groups, the crosslinking points of the vulcanized rubber are decomposed, but scission of the main chain of the rubber molecules is suppressed, and the molecular weight of the recovered rubber component A can be maintained high. This is thought to be because oxidative deterioration occurs when alcohol is used as the reaction solvent, but oxidative deterioration is less likely to occur with aldehydes.

[0035] (Aldehyde having a hydrocarbon group having two or more carbon atoms; Compound 1 in the present invention) If the number of carbon atoms in the hydrocarbon group of the aldehyde is less than 2, the molecular weight of the recovered rubber component A cannot be maintained high. The hydrocarbon group preferably has 3 to 12 carbon atoms, and more preferably has 6 to 10 carbon atoms, from the viewpoint of maintaining a high molecular weight of the recovered rubber component A.

[0036] The hydrocarbon group of the aldehyde is not particularly limited as long as it has two or more carbon atoms, and examples thereof include an aliphatic group and an aromatic group. The aliphatic group may be linear or branched, and may be a saturated or unsaturated aliphatic group. Examples of the aliphatic group include an ethyl group, a 1-propyl group, a 1-butyl group, a 2-butyl group, a tert-butyl group, a 1-pentyl group, a 2-methyl-1-pentyl group, a 1-hexyl group, a 1-heptyl group, a 1-octyl group, a 1-nonyl group, a 1-decyl group, a 1-dodecyl group, a vinyl group, and a propenyl group. Examples of the aromatic group include a phenyl group and a naphthyl group. The aldehyde having a hydrocarbon group having two or more carbon atoms may be used alone or in combination of two or more. In addition, there is no particular limitation other than that it has the above-mentioned hydrocarbon group, and for example, it may further have a substituent such as a halogen atom.

[0037] Specific examples of aldehydes having a hydrocarbon group having two or more carbon atoms include aldehydes having a propyl group (propanal), aldehydes having a butyl group (butanal), aldehydes having a pentyl group (pentanal), aldehydes having a hexyl group (hexanal), aldehydes having a heptyl group (heptanal), aldehydes having an octyl group (octanal), aldehydes having a nonyl group (nonanal), aldehydes having a decyl group (decanal), aldehydes having an unsaturated carbon chain (cinnamaldehyde), and aldehydes having a phenyl group (benzaldehyde).

[0038] Of the above, from the viewpoint of maintaining a high molecular weight of the recovered rubber component A, the hydrocarbon group is preferably an aliphatic group, more preferably a saturated aliphatic group, and even more preferably a linear saturated aliphatic group. Specifically, the aldehyde having a hydrocarbon group having two or more carbon atoms is preferably at least one selected from the group consisting of an aldehyde having a hexyl group (hexanal), an aldehyde having a heptyl group (heptanal), an aldehyde having an octyl group (octanal), and an aldehyde having a nonyl group (nonanal), and more preferably an aldehyde having a nonyl group (nonanal).

[0039] (Compound containing at least one aliphatic carbon-carbon double bond and having zero hydroxyl groups and zero aldehyde groups; Compound 2 in the present invention) From the viewpoints of maintaining a high molecular weight of the recovered liquid hydrocarbons and producing liquid hydrocarbons at a high cracking rate, the compound containing at least one aliphatic carbon-carbon double bond and having zero hydroxyl group and zero aldehyde group preferably has a carbon number of 4 to 18, more preferably 4 to 16, even more preferably 5 to 14, even more preferably 5 to 12, and even more preferably 5 to 10. Specifically, examples include anethole (carbon number 10), pinene (carbon number 10), estragole (carbon number 10), limonene (carbon number 10), carene (carbon number 10), camphene (carbon number 10), and derivatives thereof. If there are isomers, they are included.

[0040] The derivatives of compounds 1 and 2 of the present invention may be used as reaction solvents. Derivatives include structures in which one or more hydrogen atoms are substituted with a substituent such as an alkyl group, etc. Examples of the alkyl group include a methyl group, an amyl group (propyl group), a butyl group, and a hexyl group. Specifically, for example, derivatives of cinnamaldehyde include alkyl aldehydes, and amyl cinnamaldehyde (having 14 carbon atoms) is particularly preferred. Compounds other than cinnamaldehyde, such as derivatives of heptanal and anethole, can also be used.

[0041] The reaction solvent may consist of a compound which contains at least one aldehyde or an aliphatic carbon-carbon double bond having a hydrocarbon group with a carbon number of two or more and in which the number of hydroxyl groups and the number of aldehyde groups are each zero, or it may contain other solvents in addition to a compound which contains at least one aldehyde or an aliphatic carbon-carbon double bond having a hydrocarbon group with a carbon number of two or more and in which the number of hydroxyl groups and the number of aldehyde groups are each zero. However, from the viewpoint of increasing the decomposition rate of rubber component A, it is preferable that the main component of the reaction solvent is either one of the compounds which contain at least one aldehyde or an aliphatic carbon-carbon double bond having a hydrocarbon group with a carbon number of two or more and in which the number of hydroxyl groups and the number of aldehyde groups are each zero. Here, the term "main component" refers to a content of an aldehyde having a hydrocarbon group with two or more carbon atoms or a compound containing at least one aliphatic carbon-carbon double bond and having zero hydroxyl group and zero aldehyde group in the reaction solvent exceeding 50% by volume, and the content of the aldehyde having a hydrocarbon group with two or more carbon atoms in the reaction solvent is preferably 70% by volume or more, more preferably 90% by volume or more, and may be 100% by volume or more.

[0042] In the decomposition step, it is preferable to use a reaction solvent such that the ratio (Vs / Wg) of the volume [mL] (Vs) of the reaction solvent to the mass [mg] (Wg) of the vulcanized rubber is preferably in the range of 0.001 / 1 to 1 / 1, more preferably 0.005 / 1 to 0.1 / 1. By using the reaction solvent within the above range, the solvolysis reaction is further promoted, sufficient hydrogen atoms are supplied to the vulcanized rubber, recombination of radicals generated by thermal decomposition is suppressed, and the vulcanized rubber can be efficiently decomposed.

[0043] [Reaction conditions for the decomposition process] (temperature) In the decomposition step, in a first embodiment, the vulcanized rubber and the reaction solvent are heated at 300° C. or less. In a second embodiment, the vulcanized rubber and the reaction solvent are heated at 150° C. or more and 300° C. or less. By setting the heating temperature at 300°C or less, energy saving is excellent, and a decrease in the decomposition rate due to side reactions and the like can be suppressed. The heating temperature in the decomposition process is sometimes called the decomposition temperature. By heating the vulcanized rubber at a lower temperature, the vulcanized rubber can be decomposed by prioritizing the reaction involving the solvent. The heating temperature is preferably 150°C or more, more preferably 155°C or more, and even more preferably 160°C or more, and is preferably 250°C or less, more preferably 240°C or less, even more preferably 230°C or less, even more preferably 220°C or less, and even more preferably 210°C or less.

[0044] (Decomposition time) In the decomposition step, the time for heating the vulcanized rubber (decomposition time) is preferably 30 minutes to 20 hours, and more preferably 60 minutes to 180 minutes, from the viewpoint of sufficiently advancing the decomposition reaction of the vulcanized rubber.

[0045] (pressure) In the decomposition step, the pressure applied to the vulcanized rubber and the reaction solvent is not particularly limited. From the viewpoints of the reaction rate of the decomposition reaction of the vulcanized rubber and of saving resources and energy, the pressure is preferably 0.1 to 2.0 MPa (G), and more preferably 0.1 to 1.5 MPa (G). The unit "MPa (G)" means that the pressure is a gauge pressure. When the pressure is 2.0 MPa (G) or less, the molecular weight of the rubber component A is less likely to decrease, and when the pressure is 0.1 MPa (G) or more, the reaction solvent can easily penetrate into the vulcanized rubber, making it easier to increase the reaction rate.

[0046] (atmosphere) The reaction atmosphere in the decomposition step at 300° C. or less is not particularly limited, and the reaction may be carried out in a gas atmosphere consisting of an inert gas such as argon gas or nitrogen gas (hereinafter simply referred to as an inert gas atmosphere), a gas atmosphere consisting of air (hereinafter simply referred to as an air atmosphere), or a mixed gas atmosphere of air and an inert gas. When an inert gas is used, two or more kinds of inert gases may be mixed and used. From the viewpoint of performing the decomposition of the vulcanized rubber using lighter equipment and promoting energy saving, the vulcanized rubber is preferably heated in an aerobic environment, i.e., in an oxygen-containing atmosphere, more preferably in an atmosphere of a gas containing air, and even more preferably in an air atmosphere.

[0047] [Drying process] The method for producing devulcanized rubber of the present invention preferably includes a drying step of drying the reaction product (devulcanized rubber of the present invention) obtained in the decomposition step. The reactants may be subjected to blowing of hot air at, for example, 100 to 150° C. The hot air may be air or an inert gas such as nitrogen gas.

[0048] <Rubber composition> The rubber composition of the present invention contains a rubber component, and contains the devulcanized rubber of the present invention in an amount of more than 10% by mass in the rubber component. When the rubber composition of the present invention contains a rubber component containing the devulcanized rubber of the present invention in an amount of more than 10 mass % in the rubber component, a recrosslinked rubber having excellent mechanical strength can be produced while reducing the environmental burden. The rubber component may consist solely of the devulcanized rubber of the present invention, or may contain a rubber component (pure rubber component) that is usually used as a raw material for vulcanized rubber. The rubber composition of the present invention may also contain various additives that are usually contained in rubber compositions, such as a filler and a crosslinking agent.

[0049] From the viewpoint of reducing the environmental burden, the content of the devulcanized rubber of the present invention in the rubber component is preferably as high as possible, and may be 100% by mass. From the viewpoint of not impairing the mechanical strength of the re-crosslinked rubber obtained by re-crosslinking the rubber composition, the content of the devulcanized rubber of the present invention in the rubber component is preferably 70 mass % or less. From the viewpoints of reducing the environmental burden and the mechanical strength of the re-crosslinked rubber, the content of the devulcanized rubber of the present invention in the rubber component is preferably 10 to 70 mass%, more preferably 11 to 68 mass%, even more preferably 12 to 65 mass%, even more preferably 13 to 62 mass%, even more preferably 15 to 60 mass%, even more preferably 17 to 58 mass%, even more preferably 19 to 54 mass%, and even more preferably 20 to 52 mass%.

[0050] Other rubber components that can be used together with the devulcanized rubber of the present invention include rubber components (pure rubber components) that are usually used as raw materials for vulcanized rubber. The pure rubber component is the rubber component already mentioned as the raw material for the crosslinked rubber. Among them, at least one selected from the group consisting of natural rubber (NR) and synthetic diene rubber is preferable, and at least one selected from the group consisting of natural rubber, polyisoprene rubber, polybutadiene rubber, and styrene-butadiene copolymer rubber is more preferable.

[0051] The rubber composition of the present invention may contain a filler. When the rubber composition of the present invention contains a filler, the re-crosslinked rubber can have improved properties such as durability and abrasion resistance. Examples of the filler include reinforcing fillers such as carbon black and silica. Either silica or carbon black may be used alone, or both silica and carbon black may be used.

[0052] The silica is not particularly limited, and may be any type depending on the application, such as general-grade silica, special silica that has been surface-treated with a silane coupling agent, etc. As the silica, it is preferable to use, for example, wet silica. The carbon black is not particularly limited and can be appropriately selected depending on the purpose. For example, FEF, SRF, HAF, ISAF, and SAF grade carbon black are preferable. The content of the filler in the vulcanized rubber is preferably 20 to 120 parts by mass, more preferably 30 to 100 parts by mass, and further preferably 40 to 80 parts by mass, based on 100 parts by mass of the rubber component.

[0053] The rubber composition of the present invention may contain a crosslinking agent, a crosslinking accelerator, a softener, stearic acid, an antioxidant, zinc oxide, etc., in addition to the rubber component containing the devulcanized rubber of the present invention and a filler. The conditions for recrosslinking the rubber composition of the present invention are not particularly limited. As the crosslinking agent, a vulcanizing agent such as sulfur may be used, or an organic peroxide-based crosslinking agent, an acid crosslinking agent, a polyamine crosslinking agent, a resin crosslinking agent, an oxime-nitrosamine-based crosslinking agent, or the like may be used. When a vulcanizing agent is used as the crosslinking agent, one or more of various vulcanization accelerators such as sulfenamide-based, thiazole-based, and guanidine-based accelerators may be used as the crosslinking accelerator.

[0054] The rubber composition of the present invention can produce a recrosslinked rubber having excellent mechanical strength while reducing the environmental burden, and is therefore suitable for producing industrial products such as automobile parts other than tires, hose tubes, anti-vibration rubbers, conveyor belts, crawlers, cables, sealing materials, ship parts, and building materials.

[0055] <Rubber composition for tires> The rubber composition for a tire of the present invention comprises the rubber composition of the present invention. The rubber composition for tires of the present invention comprises the rubber composition of the present invention, so that tires excellent in mechanical strength can be produced while reducing the environmental burden.

[0056] <Tires> The tire of the present invention is produced using the rubber composition for tires of the present invention. By producing a tire using the rubber composition of the present invention containing the devulcanized rubber of the present invention, a tire with a small environmental impact and excellent mechanical strength can be obtained. Depending on the type and components of the tire to be applied, the tire may be obtained by molding an uncrosslinked rubber composition and then crosslinking it, or by first obtaining a semi-crosslinked rubber from an uncrosslinked rubber composition through a preliminary crosslinking step or the like, and then molding the rubber using the semi-crosslinked rubber and then further performing full crosslinking. As the gas to be filled into the tire, in addition to normal air or air with an adjusted oxygen partial pressure, inert gases such as nitrogen, argon, and helium can be used.

[0057] <Hoses, belts, crawlers> The hose of the present invention is made using the rubber composition of the present invention. The belt of the present invention is made using the rubber composition of the present invention. The crawler of the present invention is made using the rubber composition of the present invention. By producing hoses, belts, and crawlers using the rubber composition of the present invention, it is possible to obtain products that have a small environmental impact and excellent mechanical strength. EXAMPLES

[0058] The present invention will be described in more detail below by way of examples. However, these examples are intended to illustrate the present invention and are not intended to limit the present invention in any way.

[0059] <Preparing vulcanized rubber> As the vulcanized rubber, the following vulcanized rubber was prepared. Vulcanized rubber (IR): Vulcanized rubber obtained by vulcanizing polyisoprene rubber. Vulcanized rubber (a1): Vulcanized rubber obtained by vulcanizing a rubber composition containing at least natural rubber and carbon black. Vulcanized rubber (a2): A vulcanized rubber obtained by vulcanizing a rubber composition containing at least natural rubber, polybutadiene rubber, and carbon black.

[0060] <Devulcanized rubber production A> Example 1 (decomposition process) 0.4 g of vulcanized rubber (IR) cut into small pieces of about 1 mm and 5 mL of 1-heptanal were placed in an autoclave (EYELA pressure vessel, product name "HIP-30L"). The autoclave was sealed and placed in a heating vessel (EYELA personal organic synthesis apparatus ChemStation, product name "PPV-CTRL1"), and the contents were heated at 200°C for 2 hours in an air atmosphere. After heating, the heating vessel was returned to room temperature (25°C) with cooling water, and the reactants were allowed to reach room temperature.

[0061] (drying process) The reaction product obtained in the decomposition step was dried using a spray-type test tube concentrator (manufactured by EYELA, product name "MGS-3100") under nitrogen flow conditions at 130°C to obtain the decomposition product organic matter of Example 1 (devulcanized rubber).

[0062] [Examples 2 to 5, Comparative Examples 1 to 2] The decomposition step and drying step were carried out in the same manner as in Example 1 except that the reaction solvent was changed to the solvent shown in Table 1, and decomposition product organic substances (devulcanized rubber) of Examples 2 to 5 and Comparative Examples 1 and 2 were obtained.

[0063] <Analysis of decomposition-produced organic matter (devulcanized rubber)> Of the devulcanized rubbers obtained in the Examples and Comparative Examples, the liquid product (rubber component A) was dissolved in tetrahydrofuran and analyzed by gel permeation chromatography (GPC). From the analysis results, the proportion of solids (rubber component B) in the devulcanized rubber and the weight average molecular weight (Mw) of the liquid product (rubber component A) were measured. A calibration curve was created using tetrahydrofuran solutions of pure rubber component (IR) with different concentrations. The calibration curve was used to quantify the liquid product (rubber component A) in tetrahydrofuran, and the decomposition rate of the liquid product (rubber component A) was calculated. The proportion of solids (rubber component B) in the devulcanized rubber was calculated by "100% - decomposition rate of liquid product (rubber component A)". The results are shown in Table 1. The significant figures in Table 1 are three digits. The molecular weight shown in Table 1 is, for example, 389×10 in the case of Example 1. 3 , that is, 389,000.

[0064] The conditions for the GPC measurement are as follows: Column: Tosoh Corporation, manufactured by TSKgel GMHXL Eluent: Tetrahydrofuran ·Flow rate: 1mL / min ·Temperature: 40℃ Detector: RI

[0065] [Table 1]

[0066] <Production of devulcanized rubber B and production of regulcanized rubber> Example 6 The decomposition process was carried out in the same manner as in Example 3, except that the vulcanized rubber (IR) was changed to the vulcanized rubber (a1) and the heating time (decomposition time) of the input material was changed from 2 hours to the time shown in Table 2. Thereafter, purification was carried out to remove the solvent, and a drying process was carried out to obtain the decomposition product organic matter of Example 6 (devulcanized rubber A). Using the produced devulcanized rubber A, the components were blended according to the composition shown in Table 3 to prepare the rubber compositions of Examples 7 and 8. Two types of rubber compositions were prepared, in which the content of devulcanized rubber A in the rubber component was 30 parts by mass and 70 parts by mass per 100 parts by mass of polyisoprene rubber, which is the pure rubber component. The obtained rubber compositions were each vulcanized to obtain revulcanized rubber.

[0067] Comparative Example 3 The decomposition process was carried out in the same manner as in Example 3, except that the vulcanized rubber (IR) was changed to the vulcanized rubber (a1) and the heating time (decomposition time) of the input material was changed from 2 hours to the time shown in Table 2. Thereafter, purification was carried out to remove the solvent, and a drying process was carried out to obtain the decomposition product organic matter (devulcanized rubber B) of Comparative Example 3. Using the produced devulcanized rubber B, the components were blended according to the composition shown in Table 3 to prepare rubber compositions of Comparative Examples 6 and 7. Two types of rubber compositions were prepared, in which the content of devulcanized rubber B in the rubber component was 30 parts by mass and 70 parts by mass per 100 parts by mass of polyisoprene rubber, which is the pure rubber component. The obtained rubber compositions were each vulcanized to obtain revulcanized rubber.

[0068] Comparative Example 4 The decomposition process was carried out in the same manner as in Example 3, except that the vulcanized rubber (IR) was changed to the vulcanized rubber (a1) and the heating time (decomposition time) of the input material was changed from 2 hours to the time shown in Table 2. Thereafter, purification was carried out to remove the solvent, and a drying process was carried out to obtain the decomposition product organic matter (devulcanized rubber C) of Comparative Example 4. Using the produced devulcanized rubber C, the components were blended according to the composition shown in Table 3 to prepare rubber compositions of Comparative Examples 8 and 9. Two types of rubber compositions were prepared, in which the content of devulcanized rubber C in the rubber component was 30 parts by mass and 70 parts by mass per 100 parts by mass of polyisoprene rubber, which is the pure rubber component. The obtained rubber compositions were each vulcanized to obtain revulcanized rubber.

[0069] Comparative Example 5 The revulcanized rubber of Comparative Example 5 (reference revulcanized rubber) was produced in the same manner as in the production of the vulcanized rubber of Example 6, except that 100 mass % of polyisoprene rubber (IR), which is a pure rubber component, was used as the rubber component.

[0070] The details of the components shown in Table 3 are as follows. Devulcanized rubbers A to C: Devulcanized rubbers produced in Example 6, Comparative Example 3, and Comparative Example 4 IR: Polyisoprene rubber, manufactured by JSR Corporation, product name "IR2200" Carbon black: SAF grade 6C: Antioxidant, N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Nocrac 6C" DM: Vulcanization accelerator, di-2-benzothiazolyl disulfide, manufactured by Sanshin Chemical Industry Co., Ltd., product name "Suncerer DM" NS: Vulcanization accelerator, Nt-butyl-2-benzothiazylsulfenamide, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Noccela NS" DPG: Vulcanization accelerator, 1,3-diphenylguanidine, Sanshin Chemical Industry Co., Ltd., product name "Suncerer D"

[0071] <Analysis of devulcanized rubber> The produced devulcanized rubbers A to C were analyzed in the same manner as in the analysis of the devulcanized rubber in Example 1 to measure the weight average molecular weight (Mw) of the liquid product (rubber component A) and the proportion of solid content (rubber component B) in the devulcanized rubber, and the results are shown in Table 2. The significant figures for the molecular weight and the proportion of rubber component B in Table 2 are three digits. As in Table 1, the molecular weight shown in Table 2 is, for example, 271 × 103 , that is, 271,000.

[0072] [Table 2]

[0073] <Evaluation of vulcanized rubber properties> The mechanical strength and loss tangent (tan δ) of each revulcanized rubber were evaluated using the revulcanized rubbers of Examples 7 to 8, the reference revulcanized rubber (the revulcanized rubber of Comparative Example 5), and the revulcanized rubbers of Comparative Examples 6 to 9. The results are shown in Table 3.

[0074] 1. Mechanical strength The mechanical strength of each re-vulcanized rubber was evaluated in terms of tensile strength at break (TB), which was measured based on JIS K 6251 (2017) as the maximum tensile force required to break the vulcanized rubber when it was stretched 100% at room temperature (23°C). The obtained breaking strength value was expressed as an index, with the breaking strength value of the reference vulcanized rubber being set at 100. A larger index value means that the revulcanized rubber has a higher breaking strength.

[0075] 2.Loss tangent (tanδ) The loss tangent (tan δ) of each revulcanized rubber was measured using a viscoelasticity measuring device (ARES-G2 manufactured by TA Instruments) under the conditions of a temperature of 50°C, a strain of 10%, and a frequency of 15Hz. The obtained tan δ values ​​were expressed as an index, with the reciprocal of tan δ of the reference revulcanized rubber taken as 100. The larger the index value, the better the low heat build-up properties of the revulcanized rubber.

[0076] [Table 3]

[0077] <Devulcanized rubber production C> Example 9 0.4 g of vulcanized rubber (IR) cut into small pieces of about 1 mm and 5 mL of anethole were placed in an autoclave (EYELA pressure vessel, product name "HIP-30L"). The autoclave was sealed and placed in a heating vessel (EYELA personal organic synthesis apparatus ChemStation, product name "PPV-CTRL1"), and the contents were heated at 200°C for 2 hours in an air atmosphere. After heating, the heating vessel was returned to room temperature (25°C) with cooling water, and the reactants were allowed to reach room temperature.

[0078] (drying process) The reaction product obtained in the decomposition step was dried using a spray-type test tube concentrator (manufactured by EYELA, product name "MGS-3100") under nitrogen flow conditions at 130°C to obtain the decomposition product organic matter of Example 9 (devulcanized rubber D).

[0079] [Examples 10 and 11] Except for changing the reaction solvent to the solvent shown in Table 4, the decomposition process and drying process were carried out in the same manner as in Example 9, and the decomposition product organic matter of Example 10 (devulcanized rubber E) and the decomposition product organic matter of Example 11 (devulcanized rubber F) were obtained.

[0080] <Analysis of organic matter produced by decomposition> The decomposition organic matter obtained in Examples 9 to 11 was dissolved in tetrahydrofuran and analyzed by gel permeation chromatography (GPC). From the analysis results, the solubilization rate and weight average molecular weight (Mw) of the decomposition organic matter were measured. In addition, a calibration curve was created using tetrahydrofuran solutions of pure rubber components with different concentrations. Using the calibration curve, the liquid product (rubber component A) in tetrahydrofuran was quantified, and the decomposition rate of the liquid product (rubber component A) was calculated. The proportion of solids (rubber component B) in the devulcanized rubber was calculated by "100% - decomposition rate of liquid product (rubber component A)". The molecular weight shown in Table 4 is, for example, 430 × 10 in the case of Example 9 (decomposition temperature 200 ° C.). 3 , that is, 430,000.

[0081] The conditions for the GPC measurement are as follows: Column: Tosoh Corporation, manufactured by TSKgel GMHXL Eluent: Tetrahydrofuran ·Flow rate: 1mL / min ·Temperature: 40℃ Detector: RI

[0082] [Table 4]

[0083] <Manufacture of devulcanized rubber and manufacture of regulcanized rubber> [Example 12, Comparative Example 10] The decomposition step was carried out in the same manner as in Example 9, except that the vulcanized rubber (IR) was changed to the vulcanized rubber (a2), the anethole was changed to the solvent shown in Table 5, and the heating time (decomposition time) of the vulcanized rubber and the solvent was changed to the time shown in Table 5. Thereafter, purification was carried out to remove the solvent, and a drying step was carried out to obtain the decomposition product organic matter of Example 12 (devulcanized rubber G) and the decomposition product organic matter of Comparative Example 10 (devulcanized rubber H).

[0084] <Analysis of organic matter produced by decomposition> The produced decomposition product organic matter was analyzed in the same manner as the decomposition product organic matter of Example 1 to measure the weight average molecular weight (Mw) and decomposition rate of rubber component A, and the proportion of rubber component B was calculated from the decomposition rate of rubber component A. The weight average molecular weight of rubber component A and the proportion of rubber component B are shown in Table 5 with three significant digits. The molecular weight shown in Table 5 is, for example, 300×10 in the case of Example 11. 3 , that is, 300,000.

[0085] [Table 5]

[0086] In the devulcanized rubbers A to H obtained in the examples and comparative examples, the solubility of each of the rubber components A in 100 g of diethyl ether when left for 20 hours at 25°C and atmospheric pressure (0.1 MPa) was 3 g or more, and the solubility of each of the rubber components B in 100 g of diethyl ether when left for 20 hours at 25°C and atmospheric pressure (0.1 MPa) was less than 0.1 g.

[0087] Using the produced devulcanized rubbers G and H, the components were blended according to the compositions shown in Table 6 to prepare rubber compositions of Comparative Examples 11 to 12 and Examples 13 to 15. The obtained rubber compositions were each vulcanized to obtain revulcanized rubber.

[0088] The details of the components shown in Table 6 are as follows. NR: Natural rubber BR: High cis polybutadiene, manufactured by Ube Industries, product name "UBEPOL BR150L" Carbon black: SAF grade Anti-aging agents: Anti-aging agents including "Nocrac 6C" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization package: Contains sulfur. In addition to the components shown in Table 6, the rubber compositions of Comparative Examples 11 to 12 and Examples 13 to 15 contain 7.9 parts by mass of other chemicals in total.

[0089] <Evaluation of vulcanized rubber properties> The mechanical strength of each revulcanized rubber was evaluated using the revulcanized rubbers of Comparative Examples 11 and 12 and Examples 13 to 15. The results are shown in the table.

[0090] 1. Mechanical strength The mechanical strength of each re-vulcanized rubber was evaluated in terms of tensile strength at break (TB), which was measured based on JIS K 6251 (2017) as the maximum tensile force required to break the vulcanized rubber when it was stretched 100% at room temperature (23°C). The obtained breaking strength value was expressed as an index, with the breaking strength value of the reference vulcanized rubber being set at 100. A larger index value means that the revulcanized rubber has a higher breaking strength.

[0091] [Table 6]

[0092] As can be seen from Table 1, in Examples 1 to 5, the content of rubber component B as a solid content is lower, and devulcanized rubber containing liquid hydrocarbons (rubber component A) with a higher molecular weight can be produced, compared to Comparative Examples 1 and 2. Similarly, in Examples 9 to 11 shown in Table 4, it can be seen that the content of rubber component B as a solid content is lower, and devulcanized rubber containing liquid hydrocarbons (rubber component A) with a higher molecular weight can be produced. Also, as can be seen from Tables 2 and 3, the revulcanized rubber produced from the rubber composition containing the devulcanized rubber A of Example 6 has a higher mechanical strength and a lower heat buildup than the revulcanized rubber produced from the rubber composition containing the devulcanized rubber B and C of Comparative Examples 3 and 4. Also, it can be seen that the revulcanized rubber produced from the rubber composition containing the devulcanized rubber A of Example 6 has the same mechanical strength and low heat buildup as the standard revulcanized rubber composed of a pure rubber component as the rubber component. Similarly, in Tables 5 and 6, when comparing Example 15 with Comparative Example 12, it can be seen that the mechanical strength of the revulcanized rubber produced from the rubber composition containing the devulcanized rubber G of Example 12 is higher.

Claims

1. The rubber composition includes a rubber component A having a weight average molecular weight of more than 260,000 and less than 600,000, which is soluble in a solvent, and a rubber component B which is insoluble in a solvent, A devulcanized rubber having a content ratio of the rubber component B of less than 45% by mass of a total content a of the rubber component A and a content b of the rubber component B, The solvent-soluble rubber component A is a component dissolved in tetrahydrofuran using tetrahydrofuran as a solvent, The solvent-insoluble rubber component B is a component that is not dissolved in tetrahydrofuran when tetrahydrofuran is used as a solvent.

2. 2. The devulcanized rubber according to claim 1, wherein the weight average molecular weight of the rubber component A is more than 300,000 and less than 600,000.

3. 3. The devulcanized rubber according to claim 1, wherein the rubber component A and the rubber component B each contain at least one selected from the group consisting of an isoprene skeleton, a butadiene skeleton, and a styrene-butadiene skeleton.

4. The devulcanized rubber according to any one of claims 1 to 3, wherein the rubber component A and the rubber component B contain an isoprene skeleton.

5. Contains rubber components, A rubber composition comprising the devulcanized rubber according to any one of claims 1 to 4 in an amount of more than 10 mass% in the rubber component.

6. The rubber composition according to claim 5, further comprising 20 to 120 parts by mass of a filler per 100 parts by mass of the rubber component.

7. A rubber composition for tires comprising the rubber composition according to claim 5 or 6.

8. A tire using the rubber composition for tires according to claim 7.

9. A hose using the rubber composition according to claim 5 or 6.

10. A belt using the rubber composition according to claim 5 or 6.

11. A crawler using the rubber composition according to claim 5 or 6.

Citation Information

Patent Citations

  • Contracting agent for polystyrene foam and process and system for recovering polystyrene foam therewith

    JP1993263065A

  • Food packaging material suitable for recycle

    JP2000007019A

  • Reclaimed rubber

    JP2000128901A

  • Coat rubber composition for conveyor belt

    JP2009040815A

  • Desulfurized rubber and method

    JP2010512446A