Ceramic composite and manufacturing method thereof
The ceramic composite addresses the issue of light spread and brightness by utilizing controlled particle sizes and heat treatments to create voids and distinct crystal phases, achieving focused and bright light emission.
Patent Information
- Application Number
- JP2020133773
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-06
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2040-08-06
AI Technical Summary
Ceramic composites used as wavelength conversion members in light emitting devices require improvements to reduce the spread of emitted light and enhance brightness.
A ceramic composite is manufactured with specific particle size distributions and heat treatment processes to create voids and different crystal phases, including a first rare earth aluminate phosphor crystal phase with voids, a second rare earth aluminate phosphor crystal phase without voids, and a rare earth aluminate crystal phase, which controls light diffusion and refraction to reduce light spread while maintaining high brightness.
The ceramic composite effectively reduces light spread and enhances brightness by diffusing incident light through voids and controlling refraction, allowing focused light emission with high luminance and reduced chromaticity deviations.
Smart Images

Figure 0007553780000007 
Figure 0007553780000009 
Figure 0007553780000015
Abstract
Description
[Technical field]
[0001] The present disclosure relates to ceramic composites and methods for making the same. [Background technology]
[0002] Light emitting devices that include a light emitting diode (LED) or a laser diode (LD) and a wavelength conversion member that includes a phosphor are known. Such light emitting devices are used as light sources for, for example, in-vehicle lighting, general lighting, backlights for liquid crystal display devices, projectors, etc.
[0003] As an example of a wavelength conversion member provided in a light emitting device, Patent Document 1 discloses a ceramic composite containing a Ce-activated yttrium-aluminum-garnet phosphor and an inorganic material made of aluminum oxide present between phosphor particles. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2010-514189 Summary of the Invention [Problem to be solved by the invention]
[0005] However, for ceramic composites used as wavelength conversion members, there is a demand for them to emit light with higher brightness by further reducing the divergence of the emitted light. An object of the present disclosure is to provide a ceramic composite capable of emitting light with high brightness by reducing the divergence of the emitted light, and a method for producing the same. [Means for solving the problem]
[0006] The first aspect is a first particle size Dm that corresponds to a cumulative frequency of 50% in a first particle size distribution on a volume basis measured by a laser diffraction scattering method. 1 is in the range of 0.1 μm or more and 2.0 μm or less, and the first standard deviation Sd 1 A first rare earth aluminate phosphor having a second particle size Dm that is 50% of the cumulative frequency in a second particle size distribution on a volume basis determined by a laser diffraction scattering method. 2 is in the range of 2.1 μm or more and 20 μm or less, and the second standard deviation Sd 2 the content of the first rare earth aluminate phosphor is within the range of 69 mass% or more and 95.8 mass% or less, the content of the second rare earth aluminate phosphor is within the range of 4 mass% or more and 30 mass% or less, and the content of the rare earth oxide particles is within the range of 0.2 mass% or more and 10 mass% or less, where the total amount of the first rare earth aluminate phosphor, the second rare earth aluminate phosphor, and the rare earth oxide particles is taken as 100 mass%, the method comprising: preparing a raw material mixture, molding the raw material mixture to prepare a molded body, and heat-treating the molded body at a temperature range of 1200° C. or more and 1800° C. or less to obtain a first sintered body.
[0007] The second embodiment is a ceramic composite including a first rare earth aluminate phosphor crystal phase containing voids, a second rare earth aluminate phosphor crystal phase not containing voids, and a rare earth aluminate crystal phase. Effect of the Invention
[0008] According to the present disclosure, it is possible to provide a ceramic composite capable of reducing the divergence of emitted light and emitting light with high brightness, and a method for manufacturing the same. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a flow chart showing a method for manufacturing a ceramic composite. [Diagram 2] FIG. 2 is a flowchart showing a method for manufacturing a ceramic composite. [Diagram 3] FIG. 3 is a flowchart showing a method for manufacturing a ceramic composite. [Figure 4] FIG. 4 is a graph showing the relationship between particle diameter in particle size distribution and cumulative frequency (cumulative volume (%)) of particles on a volume basis. [Diagram 5] FIG. 5 is a graph showing the relationship between particle diameter in particle size distribution and cumulative frequency (cumulative volume (%)) of particles on a volume basis. [Figure 6A] FIG. 6A is a schematic plan view of a light emitting device. [Figure 6B] FIG. 6B is a schematic cross-sectional view of a light emitting device. [Figure 7] FIG. 7 is a schematic diagram showing the directions in which the chromaticity coordinates (x, y) of light emitted from a ceramic composite are measured. [Figure 8] FIG. 8 is a SEM photograph of the surface of the ceramic composite according to Example 1. [Figure 9] FIG. 9 is an SEM photograph of the surface of the ceramic composite according to Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The method for producing a ceramic composite will be described below based on the embodiments. However, the embodiments shown below are merely examples for embodying the technical concept of the present invention, and the present invention is not limited to the method for producing a ceramic composite. The relationship between the color name and the chromaticity coordinates, and the relationship between the wavelength range of light and the color name of monochromatic light, are in accordance with JIS Z8110. In this specification, ceramics refers to any inorganic nonmetallic material at a temperature of 1000°C or less.
[0011] Manufacturing method of ceramic composite 1 The method for producing the ceramic composite includes preparing a molded body by molding a raw material mixture containing a first rare earth aluminate phosphor with a content of 69% by mass to 95.8% by mass, a second rare earth aluminate phosphor with a content of 4% by mass to 30% by mass, and rare earth oxide particles with a content of 0.2% by mass to 10% by mass, with the total amount being 100% by mass, and heat-treating the molded body at a temperature range of 1200°C to 1800°C to obtain a first sintered body. However, for convenience of explanation, the step of preparing the molded body may be described separately as preparing a raw material mixture and molding the raw material mixture to prepare a molded body. In addition, the first rare earth aluminate phosphor has a first particle size Dm that is 50% of the cumulative frequency in a first particle size distribution on a volume basis by a laser diffraction scattering method. 1 is in the range of 0.1 μm or more and 2.0 μm or less, and the first standard deviation Sd 1 The second rare earth aluminate phosphor has a second particle size Dm at which the cumulative frequency of 50% in a second volumetric particle size distribution determined by a laser diffraction scattering method is reached. 2 is in the range of 2.1 μm or more and 20 μm or less, and the second standard deviation Sd 2 is in the range of 0.2 to 0.7.
[0012] Since the first rare earth aluminate phosphor and the second rare earth aluminate phosphor have different particle size ranges and the same or similar composition, at least two crystal growth patterns are presumed, as explained below. (A) Particles of the first rare earth aluminate phosphor, which has a smaller particle size than the second rare earth aluminate phosphor, gather together and integrate with each other to form a single rare earth aluminate phosphor crystal phase. (B) The first rare earth aluminate phosphor, which has a smaller particle size than the second rare earth aluminate phosphor, gathers around the particles of the second rare earth aluminate phosphor, and the particles of the first rare earth aluminate phosphor and the second rare earth aluminate phosphor are integrated to form a single rare earth aluminate phosphor crystal phase. The first rare earth aluminate phosphor and the second rare earth aluminate phosphor have different crystal growth rates due to the difference in particle size, and voids are formed during any of the steps included in the method for producing the ceramic composite described above when the rare earth aluminate phosphor crystal phase is formed. It is presumed that the tendency for such voids to be formed is due to the difference in crystal growth rate, since the crystal growth rate of the particles of the first rare earth aluminate phosphor (A) integrated with each other is faster than the crystal growth rate of the particles of the first rare earth aluminate phosphor (B) integrated with the particles of the second rare earth aluminate phosphor (B) integrated with each other due to the difference in particle size. The crystal phase in which the particles of the first rare earth aluminate phosphor (A) are integrated with each other may contain voids, and the crystal phase in which the particles of the first rare earth aluminate phosphor (B) are integrated with the particles of the second rare earth aluminate phosphor may also contain voids. The voids formed in the ceramic composite diffuse the incident light, and the rare earth aluminate phosphor crystal phase efficiently converts the wavelength of the light, allowing the ceramic composite to emit light with high brightness. In addition, by setting the void content within a specific range and including a rare earth aluminate phosphor crystal phase containing voids, the light emitted from the ceramic composite is less spread and is focused at a desired position. In this specification, the rare earth aluminate phosphor crystal phase containing voids is also referred to as a "first rare earth aluminate phosphor crystal phase containing voids". The rare earth aluminate phosphor crystal phase that does not contain voids is also referred to as a "second rare earth aluminate phosphor crystal phase that does not contain voids".
[0013] The rare earth oxide particles react with aluminum contained in the first rare earth aluminate phosphor or the second rare earth aluminate phosphor, and a rare earth aluminate crystal phase is formed in the ceramic composite. By containing the rare earth aluminate crystal phase in the ceramic composite, light incident on the ceramic composite hits the rare earth aluminate crystal phase, and the light is refracted in the ceramic composite, suppressing the spread in the lateral direction. Therefore, when light is emitted from the ceramic composite, the spread of the emitted light is reduced, and light that can be focused at a target position can be emitted from the ceramic composite. Since the refractive index of the rare earth aluminate crystal phase formed in the ceramic composite is small compared to the refractive index of the rare earth aluminate phosphor crystal phase, the decrease in the luminous flux of the light emitted from the ceramic composite can be suppressed compared to voids.
[0014] 1 to 3 are flow charts showing an example of a method for producing a ceramic composite. The steps of the method for producing a ceramic composite according to the first embodiment will be described with reference to FIG. 1 to FIG. 3. As shown in FIG. 1, the method for producing a ceramic composite includes a step S101 of preparing a molded body by molding a raw material mixture containing a first rare earth aluminate phosphor, a second rare earth aluminate phosphor, and rare earth oxide particles, and a step S102 of heat-treating the molded body to obtain a first sintered body. As shown in FIG. 2, the method for producing a ceramic composite may include a step S103 of obtaining a second sintered body by performing a second heat treatment by hot isostatic pressing (HIP) treatment after obtaining the first sintered body. The method for producing a ceramic composite may also include a step S104 of annealing the first sintered body or the second sintered body. As shown in FIG. 3, the method for manufacturing a ceramic composite may include a step S105 of cutting and processing the first sintered body, the second sintered body, or the annealed second sintered body to a desired size or thickness, and may further include a step S106 of performing surface treatment.
[0015] A method for producing a ceramic composite will now be described.
[0016] The particle size distribution of each particle of the first rare earth aluminate phosphor, the second rare earth aluminate phosphor, and the rare earth oxide particles measured by the laser diffraction scattering method is integrated from the smaller particle size on a volume basis to the larger particle size, and the particle size assumed to be a spherical equivalent diameter is set on the horizontal axis (logarithmic axis) and the integrated value (cumulative volume (%)) is set on the vertical axis and plotted. The particle size assumed to be a spherical equivalent diameter of the particle can be obtained from the angular distribution of the scattered light intensity of the diffraction by the laser light. Figure 4 is a graph showing the relationship between the particle size in the particle size distribution and the cumulative frequency (cumulative volume (%)) of the particle on a volume basis. The horizontal axis of the graph is the particle size (X), and the vertical axis is the cumulative volume (Q) (%). The integrated value Q a The particle size of the arbitrary cumulative value (cumulative volume (%)) in D a And this D a Two particle sizes on either side of X j and X j+1 Accumulated value (cumulative volume (%)) Q j and Q j+1 When is known, the integrated value Q a Any integral value of particle diameter D a can be calculated from the following formulas (1) and (2). In this specification, the median diameters at a cumulative frequency of 50% in the first particle size distribution, the second particle size distribution, and the third particle size distribution are referred to as the first particle size Dm 1 , second particle size Dm 2 , 3rd grain size Dm 3 It was decided.
[0017]
number
[0018]
number
[0019] In the particle size distribution of each particle of the first rare earth aluminate phosphor, the second rare earth aluminate phosphor, and the rare earth oxide particles measured by the laser diffraction scattering method, the particle size is integrated from the smaller particle size on a volume basis to the larger particle size, and the integrated value (cumulative volume (%)) is set on the horizontal axis and the vertical axis, and plotted as shown in FIG. 5. FIG. 5 is a graph showing the relationship between the particle size in the particle size distribution and the volume-based cumulative frequency (cumulative volume (%)) of the particles. The horizontal axis of the graph is the particle size (X or D), and the vertical axis is the cumulative volume (%). At a particle size Dm where the cumulative volume (%) at +1σ from the particle size Dm at 50% cumulative frequency is 84.135, the particle size Dm is 84.135. 84.135 and the cumulative volume (%) of -1σ from the particle size Dm with a cumulative frequency of 50 volume% is 15.865. 15.865 The standard deviation (σlog) can be calculated from the following formula (3). In this specification, the standard deviations (σlog) in the first particle size distribution, the second particle size distribution, and the third particle size distribution are respectively defined as the first standard deviation Sd 1 , second standard deviation Sd 2 , third standard deviation Sd 3 It was decided.
[0020]
number
[0021] First rare earth aluminate phosphor The first rare earth aluminate phosphor has a first particle size Dm that is 50% of the cumulative frequency in a first particle size distribution based on volume as determined by a laser diffraction scattering method. 1 is in the range of 0.1 μm or more and 2.0 μm or less, and the first standard deviation Sd 1 The first particle size Dm of the first rare earth aluminate phosphor is within a range of 0.2 or more and 2.0 or less. 1 may be in the range of 0.2 μm to 1.8 μm, or in the range of 0.3 μm to 1.5 μm. 1is in the range of 0.2 to 2.0, and by using a first rare earth aluminate phosphor having a particle size distribution with a moderate degree of variation, a first sintered body can be obtained that includes a first rare earth aluminate phosphor crystal phase that contains voids to such an extent that the density of the first sintered body obtained is not reduced. 1 may be in the range of 0.3 or more and 1.8 or less, may be in the range of 0.4 or more and 1.5 or less, or may be in the range of 0.5 or more and 1.2 or less.
[0022] The first rare earth aluminate phosphor is preferably obtained by a coprecipitation method. 1 The first particle size distribution has a relatively small particle size in the range of 0.1 μm or more and 2.0 μm or less, and a first standard deviation Sd 1 It is easy to obtain a first rare earth aluminate phosphor in which the value of the rare earth aluminate phosphor satisfies the range of 0.2 or more and 2.0 or less.
[0023] The method of forming the first rare earth aluminate phosphor by the coprecipitation method includes, for example, preparing an oxide containing a constituent element contained in the composition of the first rare earth aluminate phosphor, or a compound that easily becomes an oxide at high temperature, as a raw material, and weighing each compound so as to obtain the composition of the first rare earth aluminate phosphor while considering the stoichiometric ratio. Each compound weighed to obtain the composition of the first rare earth aluminate phosphor is dissolved in a liquid, and a precipitant is added to the solution to cause coprecipitating, thereby obtaining a coprecipitate. The oxide obtained by firing the coprecipitate and other raw materials as necessary, for example, oxides contained in the composition of the first rare earth aluminate phosphor, are weighed, and these raw materials are mixed in a wet or dry manner. A flux may be added to the raw materials. The first rare earth aluminate phosphor formed by the coprecipitation method can be obtained by firing a mixture containing the oxide obtained by coprecipitating, other raw materials, and, as necessary, flux. Examples of compounds that easily turn into oxides at high temperatures include hydroxides, oxalates, carbonates, chlorides, nitrates, sulfates, etc., containing elements that constitute the composition of the first rare earth aluminate phosphor. Examples of compounds that easily turn into oxides at high temperatures include oxides containing metals, such as aluminum metal, that are made of elements that constitute the composition of the first rare earth aluminate phosphor. Examples of liquids that dissolve metals or compounds include deionized water, etc. Examples of precipitants include oxalic acid or oxalates, carbonates, ammonium hydrogen carbonate, etc. Examples of oxalates include ammonium oxalate, etc., and examples of carbonates include ammonium carbonate, etc.
[0024] Rare Earth Aluminate Phosphors The second rare earth aluminate phosphor has a second particle size Dm that is the cumulative frequency of 50% in the second particle size distribution based on volume measured by the laser diffraction scattering method. 2 is in the range of 2.1 μm or more and 20 μm or less, and the second standard deviation Sd 2 The second particle size Dm of the second rare earth aluminate phosphor is within a range of 0.2 to 0.7. 2The second standard deviation Sd in the second particle size distribution of the second rare earth aluminate phosphor may be in the range of 2.5 μm or more and 18 μm or less, in the range of 3.0 μm or more and 15 μm or less, or in the range of 4.0 μm or more and 12 μm or less. 2 is in the range of 0.2 to 0.7, and it is preferable that the variation in particle size is small. 2 The larger second particle size Dm may be in the range of 0.2 to 0.5. 2 A small first particle size Dm is disposed around the second rare earth aluminate phosphor having the 1 It is presumed that the rare earth aluminate phosphor crystal phase is formed by the first rare earth aluminate phosphor and / or rare earth oxide particles gathering together. 2 The smaller the variation in the particle size distribution, the more likely it is that a relatively large rare earth aluminate phosphor crystal phase is formed in a state in which it is substantially uniformly dispersed in the ceramic composite. When a relatively large rare earth aluminate phosphor crystal phase is substantially uniformly dispersed in the ceramic composite, the incident light is diffused by the voids in the void-containing rare earth aluminate phosphor crystal phase, and the wavelength is efficiently converted by the rare earth aluminate phosphor crystal phase, resulting in less spreading of the emitted light, and allowing light with high brightness to be emitted from the ceramic composite.
[0025] The second rare earth aluminate phosphor has a second particle size Dm 2 is within the above range, and the second standard deviation Sd 2 The manufacturing method is not limited as long as it is within the above range. The second rare earth aluminate phosphor may be manufactured by the above-mentioned coprecipitation method or by other methods.
[0026] Compositions of the first rare earth aluminate phosphor and the second rare earth aluminate phosphor The first rare earth aluminate phosphor and the second rare earth aluminate phosphor each contain at least one rare earth element selected from the group consisting of Y, La, Lu, Gd, and Tb. 1and at least one element M selected from the group consisting of Ga and Sc, and at least a part of Al is optionally replaced by M. 1 may be substituted with rare earth elements Ln 1 The total molar ratio of Al and Ce is 3, and the total molar ratio of Al and element M 1 It is preferable that the first composition has a molar ratio of the total of the elements k and 5, which is 0.95 or more and 1.05 or less, and a molar ratio of Ce, which is 0.003 or more and 0.030 or less, which is the product of variables n and 3. When the first rare earth aluminate phosphor and the second rare earth aluminate phosphor are both rare earth aluminate phosphors having a rare earth aluminate composition containing at least Ce as an activator element, a first sintered body with high brightness can be obtained.
[0027] The first rare earth aluminate phosphor and the second rare earth aluminate phosphor preferably have a first composition represented by the following formula (I). (Ln 1 1-n Ce n )3(Al 1-m M 1 m ) 5k O 12 (I) (In formula (I), Ln 1 is at least one rare earth element selected from the group consisting of Y, La, Lu, Gd and Tb, M 1 is at least one element selected from Ga and Sc, and m, n, and k are numbers that satisfy 0≦m≦0.1, 0.003≦n≦0.030, and 0.95≦k≦1.05, respectively.
[0028] The first rare earth aluminate phosphor and the second rare earth aluminate phosphor may have the same composition or different compositions.
[0029] Rare Earth Oxide Particles The rare earth oxide particles are classified into the third particle size distribution Dm, which is the volume-based third particle size distribution determined by the laser diffraction scattering method and has a cumulative frequency of 50%. 3 is within the range of 0.5 μm to 5 μm, and the third standard deviation Sd3 It is preferable that the third particle diameter Dm of the rare earth oxide particles is in the range of 0.2 or more and 1.0 or less. 3 is within the range of 0.5 μm to 5 μm, and the third standard deviation Sd 3 is within the range of 0.2 to 1.0, in the heat treatment step described below, the rare earth aluminate crystal phase is integrated with the first rare earth aluminate phosphor or the second rare earth aluminate phosphor, or forms a rare earth aluminate crystal phase separate from the first rare earth aluminate phosphor and the second rare earth aluminate phosphor. The ceramic composite contains a rare earth aluminate crystal phase having a different composition from the first rare earth aluminate phosphor crystal phase containing voids and the second rare earth aluminate phosphor not containing voids, so that scattering of light within the ceramic composite is controlled, the spread of emitted light is reduced, and light that can be focused at a desired position can be emitted from the ceramic composite. Since the difference between the refractive index of the rare earth aluminate crystal phase within the ceramic composite and the refractive index of the rare earth aluminate phosphor crystal phase is small, the decrease in the luminous flux of the light emitted from the ceramic composite can be suppressed compared to the case of voids. The third particle diameter Dm of the rare earth oxide particles 3 The third standard deviation Sd in the third particle size distribution of the rare earth oxide particles may be in the range of 1.0 μm to 4.0 μm, or in the range of 1.2 μm to 3.5 μm. 3 is in the range of 0.2 to 1.0, and it is preferable that the variation in particle size is small. 3 may be in the range of 0.3 to 0.8.
[0030] The rare earth oxide particles contain at least one rare earth element selected from the group consisting of Y, La, Lu, Gd, Tb and Ce. 2It is preferable that the rare earth oxide particles contain Y2O3, La2O3, Lu2O3, Gd2O3, Tb2O3, and CeO2. The rare earth oxide particles react with the first rare earth aluminate phosphor or the second rare earth aluminate phosphor to form a rare earth aluminate crystal phase having a crystal structure different from that of the first rare earth aluminate phosphor crystal phase and the second rare earth aluminate phosphor crystal phase.
[0031] Preparing a raw material mixture In a method for manufacturing a ceramic composite, a raw material mixture is prepared that contains a first rare earth aluminate phosphor, a second rare earth aluminate phosphor, and rare earth oxide particles. In the raw material mixture, the content of the first rare earth aluminate phosphor is within a range of 69% by mass to 95.8% by mass, the content of the second rare earth aluminate phosphor is within a range of 4% by mass to 30% by mass, and the content of the rare earth oxide particles is within a range of 0.2% by mass to 10% by mass, where the total amount of the first rare earth aluminate phosphor, the second rare earth aluminate phosphor, and the rare earth oxide particles is taken as 100% by mass. The raw material mixture may have a first rare earth aluminate phosphor content of 70% by mass or more and 91.7% by mass or less, a second rare earth aluminate phosphor content of 8% by mass or more and 28% by mass or less, and rare earth oxide particles content of 0.3% by mass or more and 8% by mass or less, where the total amount of the first rare earth aluminate phosphor, the second rare earth aluminate phosphor, and the rare earth oxide particles is taken as 100% by mass. The raw material mixture may have a first rare earth aluminate phosphor content of 72% by mass or more and 90.6% by mass or less, a second rare earth aluminate phosphor content of 9% by mass or more and 25% by mass or less, and rare earth oxide particles content of 0.4% by mass or more and 7% by mass or less, where the total amount of the first rare earth aluminate phosphor, the second rare earth aluminate phosphor, and the rare earth oxide particles is taken as 100% by mass. When the contents of the components in the raw material mixture are within the aforementioned ranges, a ceramic composite can be obtained that includes a first rare earth aluminate phosphor crystal phase containing voids, large and small second rare earth aluminate phosphor crystal phases that do not contain voids, and a rare earth aluminate crystal phase that does not contain voids, due to differences in the crystal growth rate caused by differences in particle size or crystal structure.
[0032] The raw material mixture may be mixed using a mortar and pestle, or may be mixed using a mixing medium such as a ball mill. In addition, a mixing medium such as water or ethanol may be used to facilitate uniform mixing of the powder. In addition, a dispersant may be used to increase the dispersibility of the powder. The mixing medium is preferably one that is easily volatilized in order to form a powder raw material mixture during molding. The mixing medium is preferably in the range of 10 parts by mass to 200 parts by mass, and may be in the range of 50 parts by mass to 150 parts by mass, relative to 100 parts by mass of the raw material mixture. For example, a water-based dispersant may be used, and a cationic dispersant, an anionic dispersant, a nonionic dispersant, or the like may be used as the dispersant. When a dispersant is added to the raw material mixture, it is preferable that the amount of the dispersant is an amount that can be volatilized in the subsequent heat treatment step relative to 100% by mass of the raw material mixture, and may be 5% by mass or less, 3% by mass or less, or 1% by mass or less.
[0033] Preparing a molded body The raw material mixture can be molded by adopting a known method such as a press molding method. Examples of the press molding method include a die press molding method, a molding method in which compression is performed in a uniaxial direction by a roller bench method, and a cold isostatic pressing (CIP) method, the term of which is defined in JIS Z2500:2000, No. 2109. The molding method may adopt two types of methods to adjust the shape of the molded body, for example, a mold press molding may be followed by CIP, or a uniaxially pressurized compression molding may be performed by a roller bench method, and then CIP may be performed. It is preferable that a liquid such as water is used as a medium for CIP. It is preferable that the raw material mixture is formed into a molded body by CIP. The raw material mixture is put into a packaging container and isotropically pressed by CIP to produce a small first particle size Dm 1 and a second rare earth aluminate phosphor having a large particle size Dm 2 Since the adhesion of the second rare earth aluminate phosphor having the above structure is enhanced, the heat treatment described below can cause crystal growth while forming voids to a degree that allows the incident light to be scattered without reducing the density.
[0034] The pressure during die press molding or uniaxial compression molding is preferably 5 MPa to 50 MPa, more preferably 5 MPa to 30 MPa. If the pressure during die press molding or uniaxial compression molding is within the above range, the molded body can be shaped into a desired shape.
[0035] The pressure in the CIP is preferably 50 MPa or more and 200 MPa or less, more preferably 50 MPa or more and 180 MPa or less. When the pressure in the CIP is within the range of 50 MPa or more and 200 MPa or less, the raw material mixture is isotropically pressed to increase the density of the molded body, and a molded body can be formed from which a first sintered body having a relative density of 90% or more and a porosity of 1% or more and 10% or less can be obtained by the first heat treatment.
[0036] A step of obtaining a first sintered body by performing a first heat treatment The temperature of the first heat treatment is preferably in the range of 1200°C to 1800°C, more preferably in the range of 1400°C to 1790°C, and even more preferably in the range of 1600°C to 1780°C. If the temperature of the first heat treatment of the molded body is 1200°C or higher, the rate of crystal growth will differ due to differences in the particle size or crystal structure of each component, and a first sintered body containing a first rare earth aluminate phosphor crystal phase containing voids, a second rare earth aluminate phosphor crystal phase not containing voids, and a rare earth aluminate crystal phase can be obtained. If the temperature of the first heat treatment of the molded body is 1800°C or lower, a first sintered body containing a first rare earth aluminate phosphor crystal phase containing voids, a second rare earth aluminate phosphor crystal phase not containing voids, and a rare earth aluminate crystal phase can be obtained without dissolving the molded body so that the grain boundaries of each crystal phase disappear. The atmosphere for the first heat treatment may be an air atmosphere, an oxygen-containing atmosphere, an inert atmosphere, or a reducing atmosphere.
[0037] A step of obtaining a second sintered body by performing a second heat treatment. The obtained first sintered body may be subjected to a second heat treatment to obtain a second sintered body. The second heat treatment is preferably performed by hot isostatic pressing (HIP) treatment, the term of which is defined in JIS Z2500:2000, No. 2112, at a temperature range of 1500°C to 1800°C to obtain a second sintered body. By performing the second heat treatment while isostatically pressing by HIP, the voids (open pores) formed on the surface of the first sintered body are crushed without crushing the voids (closed pores) incorporated in the first rare earth aluminate phosphor crystal phase, and the density of the obtained second sintered body can be increased. The temperature of the second heat treatment is more preferably in the range of 1550°C to 1790°C, and even more preferably in the range of 1600°C to 1780°C.
[0038] The second heat treatment is preferably performed under an inert gas atmosphere. The inert gas atmosphere means an atmosphere containing argon, helium, nitrogen, etc. as the main component of the atmosphere. Here, the atmosphere containing argon, helium, nitrogen, etc. as the main component means that the atmosphere contains at least one gas selected from the group consisting of argon, helium, and nitrogen at 50% by volume or more. When the atmosphere of the secondary firing is an inert gas atmosphere, the deterioration of the crystal structure of each crystal phase is suppressed by the second heat treatment, and a second sintered body with a high relative density can be obtained.
[0039] The pressure in the HIP treatment is preferably in the range of 50 MPa to 300 MPa, more preferably in the range of 80 MPa to 200 MPa. When the pressure in the HIP treatment is in the range of 50 MPa to 300 MPa, a second sintered body having a higher density can be obtained without deteriorating the crystal structure of each crystal phase.
[0040] The time for the HIP treatment is, for example, from 0.5 hours to 20 hours, and preferably from 1 hour to 10 hours.
[0041] Annealing step The obtained second sintered body is preferably annealed under an oxygen-containing atmosphere. By annealing the obtained second sintered body in an oxygen-containing atmosphere, the dull body color of the first rare earth aluminate phosphor crystal phase and the second rare earth aluminate phosphor crystal phase contained in the first sintered body or the second sintered body by the first heat treatment or the second heat treatment can be restored to the original body color, and the decrease in wavelength conversion efficiency caused by the dull body color can be suppressed. The oxygen-containing atmosphere is preferably the same as the oxygen-containing atmosphere during the first heat treatment. The oxygen content in the atmosphere in the annealing step is preferably 5% by volume or more, more preferably 10% by volume or more, and even more preferably 15% by volume or more, and may be an air atmosphere (oxygen content of 20% by volume or more). The amount of oxygen in the atmosphere may be measured, for example, by the amount of oxygen flowing into a firing device, and may be measured at a temperature of 20°C and atmospheric pressure (101.325 kPa). The atmospheric pressure for annealing may be atmospheric pressure (101.325 kPa).
[0042] The annealing temperature is lower than that of the first heat treatment or the second heat treatment, and is preferably within the range of 1000° C. to 1600° C. The annealing temperature is more preferably within the range of 1000° C. to 1600° C., and even more preferably within the range of 1100° C. to 1400° C. If the annealing temperature is lower than that of the first heat treatment or the second heat treatment, and within the range of 1000° C. to 1600° C., it is possible to obtain a ceramic composite that can emit light with high brightness without reducing the voids in the sintered body and without dulling the body color.
[0043] Processing process The first sintered body or the second sintered body obtained may be cut to a desired size or thickness. The cutting method may be a known method, such as a blade dicing, a laser dicing, or a cutting method using a wire saw. Among these, a wire saw is preferred from the viewpoint of suppressing the formation of unevenness on the cut surface.
[0044] Surface treatment process Further, a surface treatment step described below may be added. The surface treatment step is a step of surface-treating the surface of the cut product obtained by cutting the first sintered body or the second sintered body obtained. This surface treatment step not only makes it possible to make the surface of the first sintered body or the second sintered body into an appropriate state in order to improve the luminescence characteristics of the first sintered body or the second sintered body, but also, in combination with the above-mentioned processing step or alone, makes it possible to obtain a ceramic composite in which the first sintered body or the second sintered body has a desired shape, size, or thickness. The surface treatment step may be performed before or after the processing step in which the first sintered body or the second sintered body is cut and processed to a desired size or thickness. Examples of methods for surface treatment include a method using sandblasting, a method using mechanical grinding, a method using dicing, and a method using chemical etching.
[0045] Ceramic Composites The ceramic composite includes a first rare earth aluminate phosphor crystalline phase containing voids, a second rare earth aluminate phosphor crystalline phase not containing voids, and a rare earth aluminate crystalline phase.
[0046] In the ceramic composite, the first rare earth aluminate phosphor crystal phase containing voids (hereinafter also referred to as "first rare earth aluminate phosphor crystal phase C1") and the second rare earth aluminate phosphor crystal phase not containing voids (hereinafter also referred to as "second rare earth aluminate phosphor crystal phase C2") have almost the same composition as the first rare earth aluminate phosphor or the second rare earth aluminate phosphor, and contain at least one rare earth element Ln selected from the group consisting of Y, La, Lu, Gd, and Tb. 1 and Ce and Al, and at least a part of the Al is optionally replaced with at least one element M selected from Ga and Sc. 1 The rare earth element Ln 1 and Ce have a total molar ratio of 3; and Al and the element M 1and a molar ratio of Ce is the product of the variable n of 0.003 to 0.030 and 3. In the ceramic composite, the first rare earth aluminate phosphor crystalline phase C1 and the second rare earth aluminate phosphor crystalline phase C2 preferably have the first composition represented by the above formula (I).
[0047] The ceramic composite includes a rare earth aluminate crystal phase (hereinafter also referred to as "rare earth aluminate crystal phase C3") formed by a reaction between rare earth oxide particles and aluminum contained in the first rare earth aluminate phosphor or the second rare earth aluminate phosphor. The rare earth aluminate crystal phase C3 has a crystal structure different from that of the first rare earth aluminate phosphor crystal phase C1 and the second rare earth aluminate phosphor crystal phase C2. Since the rare earth aluminate crystal phase C3 has a crystal structure different from that of the first rare earth aluminate phosphor or the second rare earth aluminate phosphor, it does not absorb light that becomes excitation light and emit light even if the rare earth oxide particles contain an element that can become an activator element, such as CeO2. For example, when the first rare earth aluminate phosphor crystal phase C1 and the second rare earth aluminate phosphor crystal phase C2 have a cubic garnet structure containing Ce as an activator element, the rare earth oxide particles and the rare earth aluminate crystal phase C3 may have an orthorhombic perovskite structure, such as YAP (yttrium aluminum perovskite, YAlO3). The rare earth aluminate crystal phase C3 may have a monoclinic structure, such as YAM (yttrium aluminum monoclinic, Y4Al2O9). The third rare earth aluminate crystal phase C3 preferably has an orthorhombic perovskite structure. When the rare earth aluminate crystal phase C3 has an orthorhombic perovskite structure, its crystal structure is different from the cubic garnet structure of the first rare earth aluminate phosphor crystal phase C1 containing voids or the second rare earth aluminate phosphor crystal phase C2 containing no voids. As a result, scattering of light wavelength-converted in the first rare earth aluminate phosphor crystal phase C1 and the second rare earth aluminate phosphor crystal phase C2 is suppressed, and light that can be focused at a desired position with reduced spread can be emitted from the ceramic composite.
[0048] In the ceramic composite, the rare earth aluminate crystal phase contains the rare earth element contained in the rare earth oxide particles. The rare earth element contained in the rare earth aluminate crystal phase is at least one rare earth element selected from the group consisting of Y, La, Lu, Gd, Tb, and Ce. 2The rare earth aluminate crystal phase preferably contains at least one rare earth element selected from the group consisting of Y, La, Lu, Gd, Tb and Ce. 2 and Al, and if necessary, at least a part of Al is at least one element M selected from the group consisting of Ga and Sc. 2 may be substituted with rare earth elements Ln 2 The molar ratio of Al or Al and element M is 1. 2 It is preferred that the second composition has a molar ratio of the sum of:
[0049] The rare earth aluminate crystal phase preferably has a second composition represented by the following formula (II). Ln 2 Al 1-p M 2 p O3(II) (In formula (II), Ln 2 is at least one rare earth element selected from the group consisting of Y, La, Lu, Gd, Tb and Ce, and M 2 is at least one element selected from the group consisting of Ga and Sc, and p is a number satisfying 0≦p≦0.8.
[0050] In ceramic composites, the relatively small primary grain size Dm 1 The crystal phase formed by crystal growth in which the particles of the first rare earth aluminate phosphor having a relatively small first particle size Dm 1 This is believed to be because the crystal growth rate of the first rare earth aluminate phosphor particles having a relatively small first particle size Dm 1 and a relatively large second particle size Dm 2The crystal phase in which the particles of the second rare earth aluminate phosphor having the first particle diameter Dm are integrated may also contain voids, and a void-containing first rare earth aluminate phosphor crystal phase may be formed. 1 The first rare earth aluminate phosphor particles having a relatively small first particle size Dm 1 and a relatively large second particle size Dm 2 It is not possible to determine whether the particles of the second rare earth aluminate phosphor having the above formula (I) are formed by integral crystal growth.
[0051] In the ceramic composite, the first rare earth aluminate phosphor crystal phase C1 containing voids and the second rare earth aluminate phosphor crystal phase C2 not containing voids may have a circle-equivalent crystal diameter in the range of 0.2 μm to 30 μm, or in the range of 1 μm to 25 μm. The circle-equivalent crystal diameter of the first rare earth aluminate phosphor crystal phase C1 containing voids tends to be larger than the circle-equivalent crystal diameter of the second rare earth aluminate phosphor crystal phase C2 not containing voids.
[0052] In the ceramic composite, the rare earth aluminate crystal phase C3 produced by the reaction of the rare earth oxide particles with aluminum contained in the first rare earth aluminate phosphor or the second rare earth aluminate phosphor does not contain voids. The rare earth aluminate crystal phase C3 does not contain voids because the rare earth oxide particles have a relatively small particle size and good reactivity, and the rare earth oxide particles do not contain a part of the components of the first rare earth aluminate phosphor or the second rare earth aluminate phosphor (e.g., Al or element M). 1 ), it is considered that voids are unlikely to be formed in the rare earth aluminate crystal phase C3. The crystal grain size of the rare earth aluminate crystal phase C3 may be 0.5 μm or more, or 1.0 μm or more, or 10 μm or less, or 8 μm or less.
[0053] The circle-equivalent crystal grain size of each crystal phase contained in the ceramic composite can be measured as follows. A scanning electron microscope (SEM) is used to observe an SEM image of the surface or cross section of the ceramic composite, and the maximum and minimum diameters of one crystal phase separated by each crystal phase boundary in the SEM image are measured, or the diameters of two or more points of one crystal phase are measured, and the average of the maximum and minimum values, or the average of the diameters of two or more points, can be regarded as the circle-equivalent crystal grain size of the crystal phase. For example, the circle-equivalent crystal grain size of a plurality of, for example, 20, crystal phases in an SEM image of the surface or cross section of a rare earth aluminate sintered body is measured, and the arithmetic average value obtained by dividing the total value of the circle-equivalent crystal grain size of each crystal phase by the number of crystal phases measured can be regarded as the circle-equivalent average crystal grain size of each crystal phase.
[0054] The relative density of the ceramic composite is preferably in the range of 97% to 99.98%, more preferably 97.5% or more, even more preferably 98% or more, more preferably 99.95% or less, and even more preferably 99.90% or less. When the relative density of the ceramic composite is in the range of 97% to 99.98%, the excitation light incident on the ceramic composite is diffused in the voids, and the wavelength is efficiently converted in the first rare earth aluminate phosphor crystal phase and the second rare earth aluminate phosphor crystal phase, so that light with high brightness can be emitted from the ceramic composite. In addition, since the ceramic composite contains a rare earth aluminate crystal phase, the spread of light in the ceramic composite is reduced, and light that can be focused at a desired position can be emitted.
[0055] The porosity of the ceramic composite is preferably in the range of 0.01% to 1%, more preferably in the range of 0.05% to 0.80%, even more preferably in the range of 0.10% to 0.50%, even more preferably in the range of 0.12% to 0.40%, and particularly preferably in the range of 0.15% to 0.30%. The content of voids in the first rare earth aluminate phosphor crystal phase of the ceramic composite is defined as the porosity of the ceramic composite. If the porosity of the ceramic composite is within the above range, the incident light is diffused in the voids in the ceramic composite, and the wavelength is efficiently converted in the first rare earth aluminate phosphor crystal phase and the second rare earth aluminate phosphor crystal phase, so that light with high brightness can be emitted from the ceramic composite. In addition, the spread of the emitted light is reduced, and light that can be focused at a desired position is emitted from the ceramic composite.
[0056] The porosity of a ceramic composite is measured from an SEM image of the surface or cross section of the ceramic composite obtained using an SEM. The porosity of a ceramic composite is the ratio of the total area of voids (nm 2 The porosity of a ceramic composite is specifically determined by analyzing the surface or cross-section of a ceramic composite taken using an SEM using image analysis software (e.g., ImageJ) and binarizing the SEM image so that the outline of the voids can be confirmed in the phosphor crystal phase. The binarized measurement object is then measured by dividing the total area (nm 2 ) versus the total area (nm2) of voids in the first rare earth aluminate phosphor crystal phase obtained freshly after binarization 2 ) is expressed as a percentage. The image analysis software "ImageJ" is an open source, public domain image analysis and processing software developed by the National Institutes of Health in the United States.
[0057] The ceramic composite can be used as a transmissive wavelength conversion member in which an incident surface (first main surface) into which excitation light is incident and an exit surface (second main surface) from which wavelength-changed light is emitted are opposed surfaces. When the ceramic composite is used as a transmissive wavelength conversion member in which an incident surface of excitation light and an exit surface of light are opposed surfaces, there are no limitations on the thickness of the ceramic composite, and when the ceramic composite is a plate-shaped body, the plate thickness is preferably within a range of 90 μm or more and 250 μm or less, more preferably within a range of 100 μm or more and 240 μm or less.
[0058] The resulting ceramic composite can be used as a wavelength conversion member in a light emitting device by combining it with a light source.
[0059] Light-emitting device The light emitting device includes the above-mentioned ceramic composite and an excitation light source. The above-mentioned ceramic composite may be used as a wavelength conversion member as it is, or may be included in a wavelength conversion member together with other members.
[0060] FIG. 6A shows an example of a light emitting device, and is a schematic plan view of the light emitting device 100, and FIG. 6B is a schematic cross-sectional view of the light emitting device 100 shown in FIG. 6A along the VIB-VIB' line. The light emitting device 100 includes a light emitting element 20 and a wavelength conversion member 30 made of a ceramic composite that emits light when excited by light from the light emitting element 20. The light emitting element 20 is flip-chip mounted on the substrate 10 via bumps that are conductive members 60. The wavelength conversion member 30 is provided on the light emitting surface of the light emitting element 2 via an adhesive layer 40. The light emitting element 20 and the wavelength conversion member 30 have their sides covered by a covering member 50 that reflects light. The light emitting element 20 can emit light by receiving power from outside the light emitting device 100 via wiring and the conductive member 60 formed on the substrate 10. The light emitting device 100 may include a semiconductor element 70 in addition to the light emitting element 20. The covering member 50 is provided so as to cover the semiconductor element 70, for example. The covering member 50 may contain a resin 51 and at least one additive 52 selected from the group consisting of a colorant, a phosphor, and a filler. Each member used in the light emitting device will be described below. For details, the disclosure of JP2014-112635A can be referred to, for example.
[0061] Excitation Light Source The excitation light source is preferably a semiconductor light-emitting element made of an LED chip or an LD chip. The semiconductor light-emitting element can be a nitride-based semiconductor. By using a semiconductor light-emitting element as the excitation light source, a stable light-emitting device can be obtained that is highly efficient, has a high linearity of output relative to input, and is resistant to mechanical shock. The ceramic composite can convert the wavelength of light emitted from the nitride-based semiconductor light-emitting element, and can form a light-emitting device that emits wavelength-converted mixed color light. The nitride-based semiconductor light-emitting element is preferably one that emits light in a wavelength range of, for example, 350 nm or more and 500 nm or less. The ceramic composite is preferably one that converts the wavelength of the excitation light from the nitride-based semiconductor light-emitting element, and emits output light having an emission peak wavelength in the range of 500 nm or more and less than 650 nm.
[0062] The semiconductor light emitting element preferably has an emission peak wavelength in the range of 380 nm to 500 nm, more preferably has an emission peak wavelength in the range of 390 nm to 495 nm, further preferably has an emission peak wavelength in the range of 400 nm to 490 nm, and particularly preferably has an emission peak wavelength in the range of 420 nm to 490 nm. The semiconductor light emitting element is provided with a p-electrode and an n-electrode. The p-electrode and the n-electrode of the semiconductor light emitting element may be formed on the same side of the semiconductor light emitting element or may be provided on different sides. The semiconductor light emitting element may be flip-chip mounted.
[0063] Wavelength conversion material The wavelength conversion member may be the ceramic composite described above. The thickness of the ceramic composite used as the wavelength conversion member may be in the range of 50 μm to 500 μm, 60 μm to 450 μm, or 70 μm to 400 μm. The size of the ceramic composite used as the wavelength conversion member may be a size that covers the entire light extraction surface of the light emitting element. An adhesive layer may be interposed between the light emitting element and the wavelength conversion member, and the light emitting element and the wavelength conversion member may be fixed by the adhesive layer. The adhesive constituting the adhesive layer is preferably made of a material that can optically connect the light emitting element and the wavelength conversion member. The material constituting the adhesive layer is preferably at least one resin selected from the group consisting of epoxy resin, silicone resin, phenol resin, and polyimide resin.
[0064] substrate The substrate is preferably made of an insulating material that is difficult to transmit light from the light emitting element or external light. Examples of the substrate material include ceramics such as aluminum oxide and aluminum nitride, and resins such as phenol resin, epoxy resin, polyimide resin, bismaleimide triazine resin (BT resin), and polyphthalamide (PPA) resin. Ceramics are preferred as a substrate material because of their high heat resistance.
[0065] adhesive layer An adhesive layer is interposed between the light emitting element and the wavelength conversion member, and fixes the light emitting element and the wavelength conversion member. The adhesive constituting the adhesive layer is preferably made of a material that can optically connect the light emitting element and the wavelength conversion member. The material constituting the adhesive layer is preferably at least one resin selected from the group consisting of epoxy resin, silicone resin, phenol resin, and polyimide resin.
[0066] Semiconductor Device Examples of semiconductor elements that are provided in a light-emitting device as needed include transistors for controlling light-emitting elements, and protective elements for preventing the light-emitting elements from being destroyed or their performance from deteriorating due to application of excessive voltage. Examples of protective elements include Zener diodes and capacitors.
[0067] Covering material The material of the covering member is preferably an insulating material. More specifically, it may be a phenol resin, an epoxy resin, a bismaleimide triazine resin (BT resin), a polyphthalamide (PPA) resin, or a silicone resin. The covering member may contain at least one additive selected from the group consisting of a colorant, a phosphor, and a filler, if necessary.
[0068] Conductive material The conductive member may be a bump, and the material of the bump may be Au or an alloy thereof, and other conductive members may be eutectic solder (Au-Sn), Pb-Sn, lead-free solder, or the like.
[0069] Method for manufacturing a light emitting device An example of a method for manufacturing a light emitting device will be described. For details, refer to, for example, the disclosures of JP 2014-112635 A or JP 2017-117912 A. The method for manufacturing a light emitting device preferably includes a step of arranging a light emitting element, a step of arranging a semiconductor element as necessary, a step of forming a wavelength conversion member including a ceramic composite, a step of bonding the light emitting element and the wavelength conversion member, and a step of forming a coating member.
[0070] Light emitting element arrangement process In the step of arranging the light emitting element, the light emitting element is arranged on a substrate and mounted thereon. The light emitting element and the semiconductor element are mounted on the substrate by, for example, flip chip mounting.
[0071] Bonding process between light emitting element and wavelength conversion material In the step of adhering the light emitting element and the wavelength conversion member, the wavelength conversion member is opposed to the light emitting surface of the light emitting element, and the wavelength conversion member is bonded onto the light emitting element by an adhesive layer.
[0072] Forming process of the covering member In the step of forming the covering member, the side surfaces of the light emitting element and the wavelength conversion member except for the light emitting surface are covered with the composition for covering member, and a covering member is formed on the side surfaces of the light emitting element and the wavelength conversion member except for the light emitting surface. This covering member is for reflecting light emitted from the light emitting element, and is formed so as to cover the side surfaces without covering the light emitting surface of the wavelength conversion member and to embed the semiconductor element.
[0073] In this manner, the light emitting device shown in FIGS. 6A and 6B can be manufactured. EXAMPLES
[0074] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0075] First rare earth aluminate phosphor Yttrium chloride (YCl3), cerium chloride (CeCl3), aluminum chloride (AlCl3), and gadolinium chloride (GdCl3) are 2.44 Gd 0.55 Ce 0.003 The mixture was weighed out so that the composition was expressed as (Y)3Al5, and dissolved in deionized water to prepare a mixed solution. This mixed solution was poured into a (NH3)2CO3 solution, and the mixture was precipitated by coprecipitation. 2.44 Gd 0.55 Ce 0.003 )3Al 5· We obtained carbonate represented by xCO3. The x in the composition is (Y 2.44 Gd 0.55Ce 0.003 )3Al5 ion's absolute charge to carbonate ion (CO3 2- The carbonate was placed in an alumina crucible and fired for 10 hours at 1200 to 1600°C in an air atmosphere (101.3 kPa) to obtain a fired product. The fired product was passed through a dry sieve to be classified, and the electric charge (Y 2.44 Gd 0.55 Ce 0.003 )3AlO 12 A first rare earth aluminate phosphor (coprecipitation YAG phosphor) having a composition represented by the following formula was prepared by coprecipitation. The first particle diameter Dm of the first rare earth aluminate phosphor was measured by the measuring method described later. 1 is 0.201μm, and the first standard deviation Sd 1 was 1.08.
[0076] Rare Earth Aluminate Phosphors Yttrium oxide (Y2O3), cerium oxide (CeO2), aluminum oxide (Al2O3), gadolinium oxide (Gd2O3), (Y 2.40 Gd 0.60 Ce 0.003 )3AlO 12 The ingredients were weighed and mixed to obtain a composition represented by the formula: and aluminum fluoride (AlF3) was added as a flux and mixed in a ball mill. This mixture was placed in an alumina crucible and fired in a reducing atmosphere at a temperature range of 1400°C to 1600°C for 10 hours to obtain a fired product. The fired product was dispersed in deionized water, passed through a sieve while applying various vibrations, passed through a wet sieve, dehydrated, dried, and passed through a dry sieve to classify, and the resulting powder was classified into (Y 2.40 Gd 0.60 Ce 0.003 )3AlO 12 A second rare earth aluminate phosphor having a composition represented by the following formula was prepared. The second particle diameter Dm of the second rare earth aluminate phosphor was measured by the measuring method described later. 2 is 5.22μm, and the second standard deviation Sd 2 was 0.417.
[0077] Rare Earth Oxide Particles 3rd particle size Dm 3 is 0.923μm, and the third standard deviation Sd 3 Yttrium oxide particles (composition formula: Y2O3, purity of yttrium oxide: 99.9 mass%) with a .DELTA. of 0.205 were used.
[0078] Particle size and standard deviation The first particle size distribution, the second particle size distribution, and the third particle size distribution of the first rare earth aluminate phosphor, the second rare earth aluminate phosphor, and the rare earth oxide particles are measured by a laser diffraction scattering method using a laser diffraction particle size distribution measuring device (MASTER SIZER 3000, manufactured by MALVERN), and the first particle size Dm 1 , second particle size Dm 2 , 3rd grain size Dm 3 , first standard deviation Sd 1 , second standard deviation Sd 2 , and the third standard deviation Sd 3 was calculated based on the above formulas (1) to (3).
[0079] Example 1 Preparing a raw material mixture 25.1 g of the first rare earth aluminate phosphor, 2.80 g of the second rare earth aluminate phosphor, and 0.112 g of the rare earth oxide particles were each weighed out, and a dispersant (Floren G-700, Kyoeisha Chemical Co., Ltd.) was added at 1 mass% when the total amount of the first rare earth aluminate phosphor, the second rare earth aluminate phosphor, and the rare earth oxide particles was taken as 100 mass%, and 42 g of ethanol was further added, and mixed in a wet ball mill. After removing the balls as a mixing medium from the mixture, the ethanol was separated using an evaporator, and the resulting mixture was dried as described above to prepare a raw material mixture powder for a compact. The contents of the first rare earth aluminate phosphor, the second rare earth aluminate phosphor, and the rare earth oxide particles are shown in Table 1, where the total amount of the first rare earth aluminate phosphor, the second rare earth aluminate phosphor, and the rare earth oxide particles is taken as 100 mass%.
[0080] Preparing a molded body The prepared raw material powder mixture was filled into a mold and subjected to a pressure of 19.6 MPa (200 kgf / cm 2 The molded body was then uniaxially pressed at a pressure of 176 MPa to obtain a cylindrical molded body with a diameter of 20 mm and a thickness of 20 mm. The obtained molded body was placed in a packaging container and vacuum-packed, and further subjected to CIP treatment at 176 MPa using water as the pressure medium in a cold isostatic pressing device (manufactured by Kobe Steel, Ltd. (KOBELCO)) to prepare a molded body.
[0081] A step of obtaining a first sintered body by performing a first heat treatment The prepared compact was subjected to a first heat treatment in a sintering furnace (manufactured by Marusho Denki Co., Ltd.) by holding it in an air atmosphere (101.3 kPa, 20% oxygen by volume) at a temperature of 1700° C. for 6 hours to obtain a first sintered body.
[0082] A step of obtaining a second sintered body by performing a second heat treatment. The obtained sintered body was subjected to HIP treatment using a hot isostatic pressing apparatus (manufactured by Kobe Steel, Ltd. (KOBELCO)) with nitrogen gas as the pressure medium in a nitrogen gas atmosphere (nitrogen 99% or more by volume) at 1700°C, 198 MPa, and for 2 hours to obtain a second sintered body.
[0083] Annealing step The obtained second sintered body was annealed in a sintering furnace (manufactured by Marusho Denki Co., Ltd.) by holding it in an air atmosphere (101.3 kPa, 20% by volume of oxygen) at a temperature of 1400° C. for 6 hours to obtain a second sintered body.
[0084] Machining and surface treatment The annealed second sintered body was cut into an appropriate shape and size using a wire saw, and the surfaces of the cut pieces were polished using a surface grinder to obtain a ceramic composite with a thickness of 180 μm.
[0085] Example 2 A ceramic composite was obtained in the same manner as in Example 1, except that in the step of preparing the raw material mixture, 24.8 g of the first rare earth aluminate phosphor, 2.77 g of the second rare earth aluminate phosphor, and 0.395 g of rare earth oxide particles (Y2O3) were weighed out to prepare the raw material mixture powder.
[0086] Comparative Example 1 A ceramic composite was obtained in the same manner as in Example 1, except that in the step of preparing the raw material mixture, 27.7 g of the first rare earth aluminate phosphor and 0.336 g of rare earth oxide particles (Y2O3) were weighed out, and the raw material mixture powder was prepared without using the second rare earth aluminate phosphor.
[0087] porosity The porosity of the ceramic composite was measured by performing image analysis using image analysis software (ImageJ) on the SEM image of the surface of the ceramic composite obtained using SEM, and binarizing the SEM image in which the outline of the voids in the first rare earth aluminate phosphor crystal phase could be confirmed. The binarized measurement object was then measured by dividing the area (nm 2 ) and the total area (nm 2 ) is expressed as a percentage. For example, when the resolution of an SEM image is 640 × 449, the total surface area of the ceramic composite is 2.8 × 10 9 nm 2 The porosity of the ceramic composites of the examples and comparative examples is 2.8×10 9 nm 2 The measurements were performed at a resolution of
[0088] For each of the obtained ceramic composites of the examples and comparative examples, the light emitting device 100 shown in Fig. 6A and Fig. 6B was fabricated as follows. The light emitting element 20 and the semiconductor element 70 were placed on the mounting substrate 10. Specifically, the light emitting element 20, which is formed by stacking semiconductor layers on a sapphire substrate, has a thickness of about 0.11 mm, a planar shape of a substantially square of about 1.0 mm square, and a dominant wavelength of 450 nm, was arranged in a line with the light emitting element 2 and the semiconductor element 7 so that the sapphire substrate side, which is a semiconductor growth substrate, serves as a light emitting surface, and was flip-chip mounted on the conductive pattern of the mounting substrate 10 using a conductive member 60 made of Au. Next, silicone resin was placed as adhesive 40 on the upper surface of the light-emitting element 20 to bond the wavelength conversion member 30 formed from each of the ceramic composites of the examples and comparative examples into a plate shape to the upper surface of the sapphire substrate of the light-emitting element 20. Next, the covering member 50 was disposed around the light emitting element 20, the wavelength conversion member 30, and the semiconductor element 70. The covering member 50 was disposed along the side surfaces of the light emitting element 20 and the wavelength conversion member 30, and the semiconductor element 70 was completely buried in the covering member 50. Dimethyl silicone resin was used as the resin 51 of the covering member 50, and titanium oxide particles with an average particle size of 0.28 μm were used as the light reflective material 52. The titanium oxide particles were contained in the resin 51 at 60 mass %. By these steps, the light emitting device 100 shown in FIGS. 6A and 6B was produced. The light emitting devices using the ceramic composites of the examples and comparative examples were evaluated as follows. The results are shown in Table 1.
[0089] Chromaticity coordinates (x, y), relative luminous flux (%), relative luminance (%), luminance / luminous flux ratio (L / F) For each light-emitting device using each ceramic composite of the Examples and Comparative Examples, the luminous flux and the chromaticity coordinates (x, y) in the chromaticity coordinate system of the CIE (Commission Internationale de l'Eclairage) 1931 chromaticity diagram were obtained using a light measurement system combining a spectrophotometer (PMA-11, Hamamatsu Photonics Co., Ltd.) and an integrating sphere. The luminance was obtained using an imaging colorimeter (ProMetric I8, manufactured by Radiant Vision Systems). The relative luminous flux and relative luminance were calculated using a reference line to calculate the luminous flux and luminance of each light-emitting device using each ceramic composite at a chromaticity coordinate x of 0.323 (x = 0.323), and the luminous flux and luminance of the light-emitting device using the ceramic composite of Comparative Example 1 were set as 100%, and the relative values of the luminous flux and luminance of the light-emitting device using each ceramic composite of the Examples were obtained. The reference line is a regression line derived from the correlation between the chromaticity coordinate x value of the light-emitting color emitted from each light-emitting device using each ceramic composite and the luminous flux or luminance. In addition, the ratio of relative luminance to relative luminous flux (L / F) of light-emitting devices using each ceramic composite was calculated. The higher the ratio of relative luminance to relative luminous flux (L / F), the stronger the light extracted in the direction perpendicular to the light-emitting surface of the ceramic composite is, indicating that the ceramic composite can emit light with high luminance and reduced spread.
[0090] Light distribution half-value angle (°) The half-value of the light distribution of the emitted light of each ceramic composite of the examples and comparative examples was measured. Specifically, a current of 1 A was applied to each ceramic composite of the examples and comparative examples to emit light, and the ceramic composite was rotated using a goniometer to change the directional angle, while the luminous intensity of the emitted light of each ceramic composite was measured using a spectrophotometer (PMA-11, manufactured by Hamamatsu Photonics K.K.) under the condition of Condition B, which is the average LED luminous intensity measurement recommended by CIE. The directional angle was set to 0° on the plane including the optical axis C, and the directional angle (°) was set to a range of ±90° from the optical axis C. In the emission spectrum of each ceramic composite described later, the angle range (light distribution half-value angle (°)) in which the light intensity of the emitted light emitted from the ceramic composite was 1 / 2 or more of the peak intensity was measured. The smaller the value of the light distribution half-value angle, the more the spread of light is suppressed when the wavelength-converted light is emitted from the same surface as the incident surface of the excitation light.
[0091] Light distribution chromaticity difference (Δx) The directional chromaticity coordinates of the emitted light of each ceramic composite of the examples and comparative examples were measured. Specifically, for each ceramic composite of the examples and comparative examples, a current of 1 A was applied to emit light, and the ceramic composite was rotated using a goniometer to change the directional angle, while the directional chromaticity coordinates (x, y) of the emitted color of the emitted light of each ceramic composite were measured using a spectrophotometer (PMA-11, manufactured by Hamamatsu Photonics K.K.) under the condition of Condition B, which is the average LED luminous intensity measurement recommended by CIE. FIG. 7 is a schematic diagram showing the direction in which the luminous intensity coordinates (x, y) of the emitted light of the ceramic composite were measured. The angle of inclination from the optical axis C of the ceramic composite to the light-emitting surface that emits the emitted light of the ceramic composite in the horizontal direction was measured as the light distribution angle θ. The optical axis C of the ceramic composite is parallel to the z-axis in the normal direction to the light-emitting surface of the ceramic composite, refers to an axis that passes through the center point of the ceramic composite, and has a light distribution angle of 0°. Specifically, in the xz plane shown in Fig. 7, the z axis relative to the xy plane is set as a light distribution angle of 0°, and the angle θ inclined from the z axis to the xy plane direction on the xz plane is set as a light distribution angle θ. In the chromaticity coordinates of the CIE chromaticity diagram, the chromaticity coordinates (x0, y0) of a light distribution angle of 0° and the chromaticity coordinates (x θ , y θ ) was measured. The x-coordinate x0 of the light distribution angle 0° and the x-coordinate x of the light distribution angle 60° 60 The difference Δx in the x-coordinate of these values was defined as the light distribution chromaticity difference. The smaller the light distribution chromaticity difference Δx, the smaller the deviation in chromaticity between the light emitted from the ceramic composite viewed at a light distribution angle of 0° and the light emitted from the ceramic composite viewed at a light distribution angle of 60°, indicating that color unevenness due to changes in the light distribution angle is reduced.
[0092] SEM images Using an SEM, SEM photographs of the ceramic composites of the examples and comparative examples were obtained. Fig. 8 is an SEM photograph of the ceramic composite of Example 1, and Fig. 9 is an SEM photograph of the ceramic composite of Comparative Example 1.
[0093] [Table 1]
[0094] The ceramic composites according to Examples 1 and 2 had a lower relative luminous flux than the ceramic composite according to Comparative Example 1, but the luminance was higher than that of the ceramic composite according to Comparative Example 1 because the first rare earth aluminate crystal phase C1 containing voids diffused the incident light in the voids. The voids contained in the ceramic composite tend to suppress the spread of light while decreasing the luminous flux of light emitted from the ceramic composite. The ceramic composites according to Examples 1 and 2 contain a rare earth aluminate crystal phase C3 as well as voids. The rare earth aluminate crystal phase contained in the ceramic composites according to Examples 1 and 2 has a different crystal structure from the first rare earth aluminate phosphor crystal phase C1 and the second rare earth aluminate phosphor crystal phase C2, and therefore suppresses the spread of light. In addition, the refractive index of the rare earth aluminate crystal phase C3 contained in the ceramic composites according to Examples 1 and 2 is small compared to the refractive index of the first rare earth aluminate phosphor crystal phase C1 and the second rare earth aluminate phosphor crystal phase C2, so the luminous flux of the light emitted from the ceramic composites is not reduced. The ceramic composites according to Examples 1 and 2 contain the rare earth aluminate crystal phase C3 together with the voids 4, so that the spread of light can be suppressed while the decrease in luminous flux can be suppressed. Therefore, the ceramic composites according to Examples 1 and 2 have a higher value of the ratio L / F of the relative luminance to the relative luminous flux than Comparative Example 1. From this result, it was confirmed that the ceramic composites according to Examples 1 and 2 have stronger light extracted in a direction perpendicular to the light exit surface of the ceramic composite than Comparative Example 1, and can emit light with high luminance with suppressed spread from the ceramic composites.
[0095] The ceramic composites according to Examples 1 and 2 had a smaller light distribution half-value angle and suppressed light spread of the emitted light than the ceramic composite according to Comparative Example 1. The ceramic composites according to Examples 1 and 2 had a smaller light distribution chromaticity difference Δx and less deviation in chromaticity of the emitted light than the ceramic composite according to Comparative Example 1, and color unevenness due to changes in light distribution angle was reduced.
[0096] 8 is an SEM photograph of the ceramic composite according to Example 1. In the ceramic composite according to Example 1, when the particles of the first rare earth aluminate phosphor or the particles of the first rare earth aluminate phosphor and the particles of the second rare earth aluminate phosphor are integrated to form the first rare earth aluminate phosphor crystal phase C1, the first particle size Dm 1 and the second particle size Dm 2 The difference in grain size caused a difference in the crystal growth rate, resulting in the formation of voids 4. The ceramic composite according to Example 1 also contained a second rare earth aluminate phosphor crystal phase C2 that did not contain voids. The ceramic composite according to Example 1 also contained a rare earth aluminate crystal phase C3.
[0097] 9 is an SEM photograph of the ceramic composite according to Comparative Example 1. Since the ceramic composite according to Comparative Example 1 does not contain a second rare earth aluminate phosphor, there is no difference in the crystal growth rate, and the first rare earth aluminate phosphor crystal phase C1 containing voids was not formed. The ceramic composite according to Comparative Example 1 was composed of a second rare earth aluminate phosphor crystal phase C2 and a rare earth aluminate crystal phase C3 that did not contain voids. [Industrial Applicability]
[0098] The ceramic composite obtained by the manufacturing method according to the present disclosure can be used in combination with an excitation light source as a wavelength conversion member for lighting devices for vehicles or general lighting, or backlights for liquid crystal display devices. [Explanation of symbols]
[0099] C1: first rare earth aluminate phosphor crystal phase, C2: second rare earth aluminate phosphor crystal phase, C3: rare earth aluminate crystal phase, 4: gap, 10: substrate, 20: light emitting element, 30: wavelength conversion member, 40: adhesive layer, 50: covering member, 60: conductive member, 70: semiconductor element, 100: light emitting device.
Claims
1. The first particle size Dm at which the cumulative frequency becomes 50% in the first particle size distribution on a volume basis by the laser diffraction scattering method 1 is in the range of 0.1 μm or more and 2.0 μm or less, and a first standard deviation Sd 1 A first rare earth aluminate phosphor having a second particle size Dm that is a cumulative frequency of 50% in a second particle size distribution on a volume basis measured by a laser diffraction scattering method. 2 is in the range of 2.1 μm or more and 20 μm or less, and the second standard deviation Sd 2 preparing a molded body by molding a raw material mixture, the molded body including a second rare earth aluminate phosphor having a R_2 content in the range of 69% by mass or more and 95.8% by mass or less, a content of the second rare earth aluminate phosphor in the range of 4% by mass or more and 30% by mass or less, and a content of the rare earth oxide particles in the range of 0.2% by mass or more and 10% by mass or less, where the total amount of the first rare earth aluminate phosphor, the second rare earth aluminate phosphor, and the rare earth oxide particles is taken as 100% by mass; and subjecting the molded body to a first heat treatment at a temperature of 1200° C. or more and 1800° C. or less to obtain a first sintered body. The porosity is in the range of 0.01% or more and 1% or less, The method for producing a ceramic composite, wherein the first standard deviation Sd 1 and the second standard deviation Sd 2 are standard deviations (σ log ) measured using the following formula (3): (In formula (3), D 50 is the particle size at 50% cumulative frequency on a volume basis in the particle size distribution, D 15.865 is the particle size at -1σ cumulative volume (%) of 15.865 from particle size D 50 at 50% cumulative frequency, and D 84.135 is the particle size at +1σ cumulative volume (%) of 84.135 from particle size D 50 at 50% cumulative frequency.)
2. In the step of preparing the molded body, the rare earth oxide particles are formed into a third particle size Dm at which a cumulative frequency of 50% is obtained in a volume-based particle size distribution measured by a laser diffraction scattering method. 3is in the range of 0.5 μm or more and 5 μm or less, and the third standard deviation Sd 3 is in the range of 0.2 or more and 1.0 or less, The method for producing a ceramic composite according to claim 1 , wherein the third standard deviation Sd 3 is calculated by measuring a standard deviation (σ log ) from the following formula (3): (In formula (3), D 50 is the particle size at 50% cumulative frequency on a volume basis in the particle size distribution, D 15.865 is the particle size at -1σ cumulative volume (%) of 15.865 from particle size D 50 at 50% cumulative frequency, and D 84.135 is the particle size at +1σ cumulative volume (%) of 84.135 from particle size D 50 at 50% cumulative frequency.)
3. 3. The method for producing a ceramic composite according to claim 1, wherein in the step of preparing the compact, the first rare earth aluminate phosphor is obtained by a coprecipitation method.
4. 4. The method for producing a ceramic composite according to claim 1, further comprising, after the step of obtaining the first sintered body, subjecting the first sintered body to a second heat treatment at a temperature of 1500° C. or more and 1800° C. or less by hot isostatic pressing (HIP) treatment to obtain a second sintered body.
5. The method for producing a ceramic composite according to claim 4 , wherein the step of obtaining the second sintered body includes annealing the second sintered body in an oxygen-containing atmosphere.
6. In the step of preparing the molded body, the first rare earth aluminate phosphor and the second rare earth aluminate phosphor each contain at least one rare earth element selected from the group consisting of Y, La, Lu, Gd, and Tb. 1 and at least one element M selected from Ga and Sc, where necessary, at least a part of the Al is selected from Ga and Sc. 1 The rare earth element Ln 1 and Ce have a molar ratio of 3; and 1and a molar ratio of Ce is the product of a variable n and 3 in a range of 0.003 to 0.
030.
7. In the step of preparing the molded body, the rare earth element Ln is added to the first rare earth aluminate phosphor and the second rare earth aluminate phosphor. 1 , Ce, Al and element M 1 The method for producing a ceramic composite according to claim 1 , wherein the composition formula represented by the following formula (I) is satisfied: (Ln 1 1-n C n ) 3 (Al 1-m M 1 m ) 5k O 12 (I) (In the formula (I), m, n, and k satisfy 0≦m≦0.1, 0.003≦n≦0.030, and 0.95≦k≦1.05, respectively.)
8. In the step of preparing the molded body, the rare earth oxide particles contain at least one rare earth element selected from the group consisting of Y, La, Lu, Gd, Tb and Ce. 2 The method for producing a ceramic composite according to claim 1 , comprising:
9. A rare earth aluminate phosphor comprising a first rare earth aluminate phosphor crystal phase containing voids which are closed pores, a second rare earth aluminate phosphor crystal phase not containing voids, and a rare earth aluminate crystal phase; The porosity is in the range of 0.01% or more and 1% or less, A ceramic composite, wherein a grain boundary exists between the first rare earth aluminate phosphor crystal phase and the second rare earth aluminate phosphor crystal phase.
10. The ceramic composite according to claim 9 , wherein the first rare earth aluminate phosphor crystal phase or the second rare earth aluminate phosphor crystal phase has a first composition represented by the following formula (I): (Ln 1 1-n C.E. n ) 3 (Al 1-m M 1 m ) 5k O 12 (I) (In the above formula (I), Ln 1 is at least one rare earth element selected from the group consisting of Y, La, Lu, Gd and Tb, M 1 is at least one element selected from Ga and Sc, and m, n, and k satisfy 0≦m≦0.1, 0.003≦n≦0.030, and 0.95≦k≦1.05, respectively.
11. The ceramic composite according to claim 9 or 10, wherein the rare earth aluminate crystal phase has a second composition represented by the following formula (II): Ln 2 A 1-p M 2 p O 3 (II) (In the above formula (II), Ln 2 is at least one rare earth element selected from the group consisting of Y, La, Lu, Gd, Tb and Ce, M 2 is at least one element selected from the group consisting of Ga and Sc, and p satisfies 0≦p≦0.8.
Citation Information
Patent Citations
Multi-particle light-emitting ceramics for light-emitting devices
JP2010514189A
Wavelength conversion member, light-emitting device, and method of manufacturing wavelength conversion member
JP2011256371A
Fluorescent member, manufacturing method therefor and light emitting device
JP2016204561A
Wavelength conversion member and wavelength conversion element, and light emitting device using the same
JP2017107072A
Manufacturing method of ceramic composite, ceramic composite and light-emitting device
JP2019182731A