Water and oil repellent
A polysaccharide-based water and oil repellent with controlled viscosity and a sizing agent provides stable, effective water and oil repellency on paper surfaces, addressing the challenges of viscosity and resistance in existing agents.
Patent Information
- Application Number
- JP2022164285
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-10-12
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2042-10-12
AI Technical Summary
Existing oil-resistant agents for paper struggle to achieve both high water and oil repellency without increasing viscosity, making stable application difficult, and low concentrations compromise oil resistance.
A water and oil repellent formulation containing a polysaccharide with a viscosity of 60 cps or less at 50°C and a sizing agent, such as alkyl ketene dimer, applied at specific concentrations to form a stable coating on paper.
The formulation enables excellent water and oil repellency on paper surfaces, facilitating easy application and maintaining high resistance properties.
Smart Images

Figure 0007553835000003 
Figure 0007553835000002 
Figure 0007553835000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a water and oil repellent. [Background technology]
[0002] Food packaging materials and food containers made of paper are required to prevent the penetration of moisture and oil from food. Therefore, oil-resistant agents are applied to paper to impart oil repellency to the paper (Patent Documents 1 to 4). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2006-307363 A [Patent Document 2] JP 2002-69889 A [Patent Document 3] International Publication No. 2022 / 080464 [Patent Document 4] JP 2022-103182 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present disclosure is to provide a water- and oil-repellent agent that can impart excellent water- and oil-repellency to paper. [Means for solving the problem]
[0005] The present disclosure includes the following aspects. <1> A water and oil repellent agent comprising a polysaccharide and a sizing agent, The polysaccharide is a water / oil repellent having a viscosity of 60 cps or less at 50° C. in a 20% by mass aqueous solution. <2> The polysaccharide is starch. <1> The water and oil repellent according to claim 1. <3> The starch is a hydrophobically modified starch. <2> The water and oil repellent according to claim 1. <4> The hydrophobically modified starch is an alkenyl succinate starch. <3> The water and oil repellent according to claim 1. <5> The sizing agent is an alkyl ketene dimer. <1> ~ <4> 13. The water / oil repellent according to any one of claims 1 to 12. <6> The viscosity at 50°C is 300 cps or less. <1> ~ <5> 13. The water / oil repellent according to any one of claims 1 to 12. <7> The content of the polysaccharide in the water / oil repellent is 40% by mass or less. <1> ~ <6> 13. The water / oil repellent according to any one of claims 1 to 12. <8> The content of the sizing agent in the water / oil repellent is 5% by mass or less. <1> ~ <7> 13. The water / oil repellent according to any one of claims 1 to 12. <9> The content of the sizing agent in the water / oil repellent is 10% by mass or less based on the total amount of the polysaccharide and the sizing agent. <1> ~ <8> 13. The water / oil repellent according to any one of claims 1 to 12. <10> The above further contains additives. <1> ~ <9> 13. The water / oil repellent according to any one of claims 1 to 12. <11> For treating the surface of paper, <1> ~ <10> 13. The water / oil repellent according to any one of claims 1 to 12. <12> the above <1> ~ <11> 2. A water- and oil-repellent paper having a water- and oil-repellent layer formed on a surface of the paper from the water- and oil-repellent agent according to any one of claims 1 to 11. <13> The solid content of the water- and oil-repellent agent in the water- and oil-repellent layer is 6.0 g / m 2 The above is <12> The water- and oil-repellent paper described in 1. <14> the above <1> ~ <11> 2. A method for treating paper, comprising treating the paper by externally adding the water / oil repellent according to any one of claims 1 to 11. Effect of the Invention
[0006] According to the present disclosure, it is possible to provide a water- and oil-repellent agent that can impart excellent water- and oil-repellency to paper. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] <Water and oil repellent> The water / oil repellent of the present disclosure is a water / oil repellent comprising a polysaccharide and a sizing agent, wherein the polysaccharide exhibits a viscosity of 60 cps or less at 50° C. in a 20% by mass aqueous solution.
[0008] Conventionally, when an greaseproofing agent contains a polysaccharide at a high concentration, the viscosity of the greaseproofing agent increases, making it difficult to stably apply the greaseproofing agent to paper. On the other hand, when an greaseproofing agent contains a polysaccharide at a low concentration, the greaseproofing agent may have a low oil resistance.
[0009] The water- and oil-repellent agent of the present disclosure has the above-mentioned characteristics and can impart excellent water- and oil-repellency to paper. In particular, even when the polysaccharide concentration is high, the agent can treat paper well and impart excellent water- and oil-repellency to paper.
[0010] The water- and oil-repellent agent of the present disclosure may include a medium (for example, a liquid medium such as water and an organic solvent). The water- and oil-repellent agent of the present disclosure may preferably be an aqueous dispersion.
[0011] The water / oil repellent of the present disclosure contains a polysaccharide. The polysaccharide may consist of one type of polysaccharide, or may consist of two or more types of polysaccharides. The polysaccharide contained in the water / oil repellent can provide water and oil repellency to paper.
[0012] Conventionally, when an greaseproofing agent contains a polysaccharide at a high concentration, the viscosity of the greaseproofing agent increases, making it difficult to stably apply the greaseproofing agent to paper. On the other hand, when an greaseproofing agent contains a polysaccharide at a low concentration, the greaseproofing agent may have a low oil resistance.
[0013] The polysaccharide contained in the water- and oil-repellent agent of the present disclosure may be a water-soluble polysaccharide or a hydrophobic polysaccharide. The polysaccharide may be dissolved or partially dissolved in water to form an aqueous solution of the polysaccharide or a dispersion containing the polysaccharide. The aqueous solution or dispersion of the polysaccharide has a predetermined viscosity according to the amount of the polysaccharide contained in the aqueous solution or dispersion.
[0014] Hereinafter, in this specification, the term "aqueous solution" is not limited to a form in which the polysaccharide is completely dissolved in a liquid, but may also include a form in which the polysaccharide is partially dissolved in a liquid. For example, the term "aqueous solution" in this specification also includes a form such as a dispersion in which the polysaccharide is dispersed in a liquid, or a suspension in which the polysaccharide is suspended in a liquid.
[0015] The polysaccharides contained in the water / oil repellent of the present disclosure exhibit a viscosity of 60 cps or less at 50° C. in a 20% by mass aqueous solution. By exhibiting such a viscosity, even if the water / oil repellent contains a high concentration of polysaccharides, the viscosity of the water / oil repellent is unlikely to increase. Therefore, the water / oil repellent containing a high concentration of polysaccharides can be easily applied to paper, and the water and oil repellency of the paper can be improved.
[0016] From the viewpoint of facilitating application of the water / oil repellent of the present disclosure to paper, the polysaccharide, in a 20% by mass aqueous solution, may preferably exhibit a viscosity of 55 cps or less at 50°C, more preferably a viscosity of 50 cps or less, even more preferably a viscosity of 45 cps or less, particularly preferably 40 cps, and especially preferably 30 cps.
[0017] From the viewpoint of improving water repellency and oil repellency, the polysaccharide may exhibit a viscosity of 1 cps or more, preferably 5 cps or more, and more preferably 10 cps or more, in a 20% by mass aqueous solution at 50°C.
[0018] From the viewpoint of facilitating application of the water / oil repellent of the present disclosure to paper, the polysaccharide, in a 20% by mass aqueous solution, may exhibit a viscosity of 200 cps or less at 30° C. From the viewpoint of further improving water and oil repellency, the polysaccharide, in a 20% by mass aqueous solution, may exhibit a viscosity of preferably 150 cps or less at 30° C., more preferably 130 cps or less, and even more preferably 120 cps or less.
[0019] From the viewpoint of improving water repellency and oil repellency, the polysaccharide may exhibit a viscosity of 1 cps or more, preferably 10 cps or more, and more preferably 30 cps or more, in a 20% by mass aqueous solution at 30°C.
[0020] The viscosity of the aqueous solution of the polysaccharide is measured using a B-type rotational viscometer. For example, a No. 2 rotor may be used for the measurement using a B-type rotational viscometer. The rotation speed of the rotor may be 60 rpm.
[0021] The viscosity in a 20% by mass aqueous solution at 50°C can be adjusted, for example, by adjusting the molecular weight of the polysaccharide. Specifically, the viscosity in a 20% by mass aqueous solution at 50°C may be adjusted by cleaving the glucosidic bonds of the polysaccharide. The cleavage of the glucosidic bonds of the polysaccharide may be carried out, for example, by using a wet acid treatment, a dry acid treatment, a heat treatment, an amylolytic enzyme, or an oxidizing agent. By cleaving the glucosidic bonds of the polysaccharide, the molecular weight of the polysaccharide is reduced, and the viscosity in a 20% by mass aqueous solution at 50°C can be reduced. In other words, a polysaccharide with a reduced viscosity can be obtained. The reduction in the viscosity of the polysaccharide may be carried out after processing (or modification) of the polysaccharide, or may be carried out before processing (or modification).
[0022] The polysaccharide may be a compound in which a plurality of monosaccharides (three or more, for example, three or more and two thousand or less) such as glucose, galactose, fructose, etc. are bonded together. The polysaccharide may be an oligosaccharide in which three or more and ten or less monosaccharides are bonded together.
[0023] The polysaccharides may be acidic polysaccharides, neutral polysaccharides, or basic polysaccharides. Acidic polysaccharides are generally polysaccharides having carboxyl groups (-COOH) and the like. Specific examples of acidic polysaccharides are carrageenan, pectin, gum arabic, xanthan gum, gellan gum, agar, and tragacanth gum. Neutral polysaccharides are polysaccharides that are electrically neutral. Specific examples of neutral polysaccharides are tamarind seed gum, guar gum, locust bean gum, starch, and pullulan. Basic polysaccharides are polysaccharides having amino groups (-NH2) and the like. Specific example of basic polysaccharides is chitosan.
[0024] Specific examples of polysaccharides include xanthan gum, karaya gum, welan gum, guar gum, pectin, tamarind gum, carrageenan, chitosan, gum arabic, locust bean gum, cellulose, cellulose derivatives such as carboxymethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, hydroxypropylmethylcellulose, alginic acid, starch (in other words, starch), agar, dextran, pullulan, etc. The polysaccharide may be a substituted polysaccharide, in particular a polysaccharide in which the hydroxyl groups are substituted.
[0025] From the viewpoint of improving water repellency and oil repellency, the polysaccharide may be starch. The starch may be vegetable starch. For example, the starch may be rice starch, wheat starch, corn starch, potato starch, tapioca starch, sweet potato starch, adzuki bean starch, mung bean starch, kudzu starch, or potato chestnut starch.
[0026] The starch may be an unmodified starch or a modified starch. In other words, the starch may be an unmodified starch or a modified starch. The starch may be a modified starch that has been subjected to at least one modification such as esterification modification, etherification modification, oxidation modification, alkali modification, enzyme modification, and bleaching modification.
[0027] Examples of modified starches include acetylated adipic acid cross-linked starch, acetylated oxidized starch, acetylated phosphate cross-linked starch, alkenyl succinate esterified starch, starch acetate, oxidized starch, hydroxyalkylated starch, hydroxyalkylated phosphate cross-linked starch (e.g., alkyl group having 2 to 40 carbon atoms or 2 to 10 carbon atoms, particularly 2 or 3), phosphate cross-linked starch, phosphorylated starch, phosphate monoesterified phosphate cross-linked starch, acid modified starch, alkali treated starch, enzyme treated starch, bleached starch, cationic starch (e.g., quaternary ammonium starch), and pregelatinized starch. Also included is dextrin obtained by lowering the molecular weight of starch by a chemical or enzymatic method.
[0028] From the viewpoint of improving water repellency and oil repellency, the starch may be a hydrophobically modified starch. The hydrophobically modified starch is starch that has been modified (hydrophobized) to have a hydrophobic group (e.g., a hydrocarbon group having 1 to 40, 2 to 40, 3 to 30, or 4 to 20 carbon atoms). Examples of the hydrophobically modified starch include alkenyl succinate esterified starch, acetate esterified starch, polyacrylonitrile grafted starch, (meth)acrylic acid or (meth)acrylic acid ester grafted starch, and crosslinked starch. Examples of (meth)acrylic acid esters are methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate. In the crosslinked starch, a polyfunctional (divalent to pentavalent) agent is used, and examples of the polyfunctional agent include phosphorus oxychloride and epichlorohydrin.
[0029] Examples of the hydrophobic modification method include a method of esterifying raw starch with an alkenyl succinic acid (e.g., an alkenyl succinic anhydride having 3 to 40 carbon atoms, e.g., 5 to 30 or 6 to 24 carbon atoms in the alkenyl group) derivative (e.g., an alkenyl succinic anhydride such as octenylsuccinic anhydride or dodecenylsuccinic anhydride) to obtain an alkenylsuccinic acid esterified starch (or an alkenylsuccinic acid modified starch), a method of grafting a hydrophobic monomer (e.g., an unsaturated nitrile such as acrylonitrile, an acrylic monomer such as an alkyl (meth)acrylate (e.g., an alkyl group having 1 to 30 carbon atoms)) onto raw starch, a method of reacting raw starch with an organosilane, and a method of imparting a hydrophobic group containing a hydrocarbon group (e.g., 1 to 30 carbon atoms) to starch by etherification or esterification, etc. When raw starch is esterified to obtain alkenyl succinate-esterified starch, the raw starch may be reacted with an alkenyl derivative of succinic acid in a weakly basic environment (e.g., pH 7.5 to 8.0). Examples of raw starch include natural starches such as corn starch, rice starch, wheat starch, corn starch, potato starch, tapioca starch, and sweet potato starch.
[0030] From the viewpoint of improving water repellency and oil repellency, the polysaccharide may be an alkenyl succinate starch (for example, octenyl succinate starch or octenyl succinic acid modified starch). In the alkenyl succinate starch, the carbon number of the alkenyl group may be 3 to 40, for example, 5 to 30 or 6 to 24. Specific examples of the alkenyl succinate starch include octenyl succinate starch, decenyl succinate starch, dodecenyl succinate starch, tetradecenyl succinate starch, hexadecenyl succinate starch, and octadecenyl succinate starch. Octenyl succinate starch is preferred. The degree of esterification of the esterified starch is expressed as the degree of substitution (moles of substituents DS per mole of anhydroglucose residues) and may be DS between 0.005 and 0.3 or between 0.01 and 0.2.
[0031] The hydrophobically modified starch has a hydrophobic group (e.g., a hydrocarbon group having 1 to 40, 2 to 40, or 3 to 30 carbon atoms), but preferably also has a hydrophilic group (e.g., a hydroxyl group, an amino group, a carboxyl group, or an oxyalkylene group (alkylene having 1 to 3 carbon atoms, particularly 1 or 2)). The presence of the hydrophobic group and the hydrophilic group can enhance water and oil repellency.
[0032] The polysaccharide content in the water / oil repellent of the present disclosure may be 40% by mass or less, preferably 35% by mass or less, more preferably 30% by mass or less, even more preferably 25% by mass or less, and even more preferably 20% by mass or less.
[0033] The polysaccharide content in the water / oil repellent of the present disclosure may be 1% by mass or more, preferably 3% by mass or more, more preferably 5% by mass or more, even more preferably 7% by mass or more, even more preferably 10% by mass or more, and particularly preferably 15% by mass or more.
[0034] The water- and oil-repellent agent of the present disclosure includes a sizing agent. By including a sizing agent in the water- and oil-repellent agent, the water- and oil-repellent properties of the water- and oil-repellent agent can be improved. The sizing agent used in the water- and oil-repellent agent of the present disclosure may be a commercially available sizing agent.
[0035] Examples of the sizing agent include olefin-based sizing agents, rosin-based sizing agents, acrylic-based sizing agents, polyacrylamide-based sizing agents, styrene-maleic acid-based sizing agents, acrylic copolymer-based sizing agents, acrylic emulsion-based sizing agents, olefin-maleic acid resin-based sizing agents, urethane-based sizing agents, AKD (alkyl ketene dimer)-based sizing agents, ASA (alkenyl succinic anhydride)-based sizing agents, and petroleum resin-based sizing agents. The ionic nature of the sizing agent may be cationic, anionic, or nonionic. From the viewpoint of further improving water repellency and oil repellency, the sizing agent may be an alkyl ketene dimer.
[0036] The alkyl ketene dimer is, for example, represented by the following formula: [ka] [In formula: R 1 is an alkyl or alkenyl group R 2 is an alkyl or alkenyl group] The compound may be represented by the formula:
[0037] In order to further improve water and oil repellency, R 1 and R 2 may each independently be an alkyl group or alkenyl group having 4 to 32 carbon atoms, preferably an alkyl group or alkenyl group having 8 to 28 carbon atoms, more preferably an alkyl group or alkenyl group having 12 to 24 carbon atoms, and even more preferably an alkyl group or alkenyl group having 14 to 24 carbon atoms.
[0038] The content of the sizing agent in the water / oil repellent of the present disclosure may be 5% by mass or less, preferably 0.1 to 5% by mass, more preferably 0.3 to 3% by mass, and even more preferably 0.5 to 1% by mass.
[0039] The amount of the sizing agent in the water / oil repellent of the present disclosure may be 10% by mass or less, preferably 1% by mass to 10% by mass, more preferably 1% by mass to 8% by mass, and even more preferably 2% by mass to 5% by mass, based on the total content of the polysaccharide and the sizing agent contained in the disclosed water / oil repellent.
[0040] The water / oil repellent may have a viscosity of 300 cps or less at 50° C. When the water / oil repellent of the present disclosure has such a viscosity, the water / oil repellent of the present disclosure is easily applied to paper. From the viewpoint of making it easier to apply the water / oil repellent of the present disclosure to paper, the viscosity of the water / oil repellent of the present disclosure at 50° C. may be preferably 1 to 300 cps, more preferably 30 cps to 250 cps, and even more preferably 50 cps to 200 cps.
[0041] The water / oil repellent of the present disclosure may further contain additives such as a pH adjuster, a paper strength enhancer, a retention improver, a colorant (dye or pigment), a fluorescent colorant, a slime control agent, an anti-slip agent, and an antifoaming agent.
[0042] <Application> The water- and oil-repellent agent according to the present disclosure can be used as an external treatment agent (surface treatment agent) or an internal treatment agent. Products obtained by treatment with the water- and oil-repellent agent have high water and / or oil repellency. Therefore, the water- and oil-repellent agent is used as a water repellent and / or oil repellent. Furthermore, the water- and oil-repellent agent can be used as an antifouling agent, an oil-resistant agent, an oil-resistant agent, a dirt release agent, a release agent, or a component thereof.
[0043] <Water- and oil-repellent paper> The water- and oil-repellent agent of the present disclosure can be used to treat (for example, surface treat) paper. That is, the water- and oil-repellent agent of the present disclosure can be a water- and oil-repellent agent for treating the surface of paper. By treating paper with the water- and oil-repellent agent of the present disclosure, water- and oil-repellent paper can be obtained.
[0044] The water- and oil-repellent agent can be applied to paper by a conventionally known method, for example, an internal addition treatment method in which the water- and oil-repellent agent of the present disclosure is added to a pulp slurry before papermaking, or an external addition treatment method in which the water- and oil-repellent agent of the present disclosure is applied to paper after papermaking can be used.
[0045] The treatment method of the water- and oil-repellent agent of the present disclosure is preferably an external addition treatment method. As the external addition treatment method, size press, coating (for example, gate roll coater, bill blade coater, bar coater, etc.), spray device, etc. may be adopted. The water- and oil-repellent agent may be dispersed and diluted in an organic solvent or water, and applied to the surface of the object to be treated by a known method such as dip coating, spray coating, foam coating, etc., and then dried.
[0046] The size press of the external additive treatment method can be divided as follows according to the coating method. One coating method is a so-called pond type two-roll size press, in which a coating liquid (i.e., sizing liquid) is supplied to a nip formed by passing paper between two rubber rolls, a coating liquid pool called a pond is created, and the paper is passed through this coating liquid pool to apply the sizing liquid to both sides of the paper. Other coating methods are a gate roll type in which the sizing liquid is applied by a surface transfer type, and a rod metering size press. In the pond type two-roll size press, the sizing liquid is likely to penetrate into the inside of the paper, and in the surface transfer type, the sizing liquid components are likely to remain on the surface of the paper. In the surface transfer type, the coating layer is more likely to remain on the surface of the paper than in the pond type two-roll size press, and the water-repellent and oil-repellent layer formed on the surface is larger than in the pond type two-roll size press. In the present disclosure, water repellency and oil repellency can be imparted to paper even when the former pond type two-roll size press is used. The paper thus treated exhibits excellent water and oil repellency, after simple drying at room or elevated temperature, optionally followed by a heat treatment which, depending on the nature of the paper, may range from up to 300°C, for example up to 200°C, in particular from 80°C to 180°C.
[0047] The paper processing method of the present disclosure may be a method in which the water- and oil-repellent agent of the present disclosure is externally added to paper on-machine. In other words, it may be a processing method in which the paper manufacturing process and the coating process are integrated (in other words, continuous). For example, the paper processing method of the present disclosure may be a method in which a paper raw material slurry is supplied to the wire part of a papermaking machine to be dehydrated, and then water is squeezed out in a press part, and then the paper is passed through a dryer part to be dried to obtain a base paper for coating, and the base paper for coating is passed through a coater head to be coated with a water- and oil-repellent agent, and then the base paper is passed through a dryer part to be dried.
[0048] The water and oil repellent agent of the present disclosure can be used in gypsum board base paper, coated base paper, medium-quality paper, general liners and cores, neutral pure white roll paper, neutral liners, rust-proof liners and metal interleaving paper, kraft paper, etc. It can also be used in neutral printing and writing paper, neutral coated base paper, neutral PPC paper, neutral thermal paper, neutral pressure-sensitive base paper, neutral inkjet paper, and neutral information paper.
[0049] The paper to be treated with the water / oil repellent of the present disclosure may be a paper container, a paper molded product (e.g., a pulp mold), etc. For example, food packaging materials and food containers are preferred. The paper can be produced by a conventionally known papermaking method.
[0050] As the pulp raw material for paper, any of bleached or unbleached chemical pulps such as kraft pulp or sulfite pulp, bleached or unbleached high-yield pulps such as groundwood pulp, mechanical pulp or thermomechanical pulp, and waste paper pulp such as recycled newspapers, recycled magazines, recycled corrugated cardboard, deinked recycled paper, etc. Also usable are mixtures of the above pulp raw materials with synthetic fibers such as asbestos, polyamide, polyimide, polyester, polyolefin, polyvinyl alcohol, etc.
[0051] A sizing agent may be added to improve the water resistance of the paper. Examples of the sizing agent include cationic sizing agents, anionic sizing agents, and rosin-based sizing agents (e.g., acidic rosin-based sizing agents and neutral rosin-based sizing agents). The amount of the sizing agent may be 0.01% by mass or more and 5% by mass or less based on the pulp.
[0052] If necessary, additives used in the manufacture of paper, such as paper strength enhancers such as carboxymethyl cellulose and polyamide polyamine-epichlorohydrin resin, flocculants, fixing agents, retention improvers, dyes, fluorescent dyes, slime control agents, and defoamers, can be used as papermaking chemicals to the extent that they are normally used. If necessary, a water- and oil-repellent agent can be applied to the paper by a size press, a gate roll coater, a bill blade coater, a calendar, or the like, using polyvinyl alcohol, glucose, dyes, coating colors, and anti-slip agents. It is preferable to use polyvinyl alcohol or glucose as an additive. By using polyvinyl alcohol or glucose together with polysaccharides, high water- and oil-repellency can be obtained. The amount of polyvinyl alcohol as a papermaking chemical may be 1 part by mass or more and 1000 parts by mass or less, 2 parts by mass or more and 200 parts by mass or less, 3 parts by mass or more and 100 parts by mass or less, or 5 parts by mass or more and 50 parts by mass or less, particularly 10 parts by mass or more and 40 parts by mass or less, relative to 100 parts by mass of polysaccharides.
[0053] The water- and oil-repellent paper of the present disclosure has a water- and oil-repellent layer formed on the surface of the paper from the water- and oil-repellent agent of the present disclosure. The polysaccharide content in the water- and oil-repellent layer is 6.0 g / m 2 or less, preferably 0.02 g / m 2 More than 6.0g / m 2 Less than or equal to 0.2 g / m 2 More than 5.0g / m 2 Less than 0.5 g / m, more preferably 0.5 g / m 2 More than 4.0g / m 2 Less than 1.0 g / m 2 More than 3.0g / m 2 The content of the water / oil repellent agent in the water / oil repellent layer may be the amount of solids contained in the water / oil repellent agent.
[0054] In the external addition, the sizing agent contained in the water- and oil-repellent layer is 0.01 g / m 2 More than 2.0g / m 2 or less, preferably 0.01 g / m 2 More than 1.5g / m 2 Less than or equal to 0.03 g / m2 More than 1.3g / m 2 Less than 0.05 g / m 2 More than 1.0g / m 2 It may be the following:
[0055] The water- and oil-repellent paper of the present disclosure may have an air permeability of, for example, 1000 seconds or more, 2000 seconds or more, and particularly 3000 seconds or more. The air permeability is measured in accordance with JIS P8117 (2009). The higher the air permeability, the higher the gas barrier property, and the more difficult it is for not only gases such as oxygen but also moisture (including water vapor) to pass through. EXAMPLES
[0056] The water and oil repellent of the present disclosure will be described below with reference to examples, but the present disclosure is not limited to the following examples.
[0057] The test methods used below are as follows:
[0058] Viscosity measurement The viscosity was measured using a Brookfield digital viscometer. The viscosity was measured at a rotation speed of 60 rpm and a temperature of 50° C., using a rotor No. 2. The Brookfield digital viscometer was used.
[0059] Oil resistance test (practical oil test) Approximately 0.1 g of commercially available olive oil was dropped onto water- and oil-repellent paper and placed in a 70°C oven, then removed after 7 minutes and the degree of absorption was observed. The following evaluation values were set according to the degree of penetration on the reverse side. 5:0-5% 4:6-20% 3:21-50% 2:51-75% 1:76-100%
[0060] <Water absorption (Cobb value) evaluation> The water absorbency (Cobb value) was measured in accordance with JIS P 8140:1998. The paper substrate was placed on the surface of a hard base plate with one side finished smoothly, and a metal cylinder with an inner diameter of 112.8 mm was clamped to the surface. Water was then poured into the cylinder so that the water depth was 10 mm. The weight of water absorbed in one minute after the water started to come into contact with the paper substrate was calculated. The obtained value was converted to weight per square meter (gsm) to calculate the water absorbency (Cobb value).
[0061] Air permeability The air permeability (air resistance) of the bottom of the paper container formed into a container shape was measured in accordance with JISP8117 (2009) using an automatic Gurley-type DENSO meter (product No. 323-AUTO, air hole diameter 28.6 ± 0.1 mm) manufactured by Yasuda Seiki Seisakusho Co., Ltd.
[0062] Viscosity measurement of 20% polysaccharide aqueous solution A predetermined amount of octenylsuccinic acid modified starch-1 was dissolved in water to prepare an aqueous solution with a concentration of 20% by mass of octenylsuccinic acid modified starch. The viscosity of the aqueous solution was measured. Aqueous solutions of 20% by mass of octenylsuccinic acid modified starch-2 and octenylsuccinic acid modified starch-3 were also prepared and their viscosities were measured. The measurement results of these viscosities are shown in Table 1.
[0063] [Table 1]
[0064] [Example 1] (Preparation of base paper) A pulp slurry was prepared with a mass ratio of 60% LBKP (broadleaf bleached kraft pulp) and 40% NBKP (softleaf bleached kraft pulp) as wood pulp, and a pulp freeness of 400 ml (Canadian Standard Freeness). A wet strength agent was added to this pulp slurry at a solid content concentration of 0.5% by mass relative to the dry pulp, and the slurry was spun on a Fourdrinier papermaking machine to produce a paper with a density of 0.58 g / cm3 and a basis weight of 48 g / m. 2The paper was used as the base paper for external treatment (size press treatment). The oil resistance (practical oil test) of the base paper was 1. The water absorption (Cobb value) of the base paper was 65. The air permeability of the base paper was 250 seconds. (Production of octenylsuccinic acid modified starch) To a flask containing 400 parts of water, 20 parts of corn starch was added in small portions at 25° C. with strong stirring, and then dilute hydrochloric acid was added and stirred until the pH became 4 or less. This aqueous solution was dried at about 70 to 90°C until the moisture content was 7% or less, and then roasted at 160°C until a predetermined viscosity was reached, to obtain low-viscosity corn starch. 100 parts of the obtained low-viscosity corn starch was added little by little to a flask containing 120 parts of water with stirring, and then the pH was neutralized with a 2% aqueous sodium hydroxide solution. Next, 4 parts of octenylsuccinic anhydride was added while maintaining the pH at 7.5 to 8.0, and the mixture was reacted at about 30 to 40° C. for 5 hours. After the reaction, the reaction mixture was neutralized with dilute sulfuric acid and then washed several times with 300 parts of water. The obtained solid was dried and then crushed to obtain starch sodium octenyl succinate. By adjusting the roasting time at 160°C, starch sodium octenyl succinate 1 to 3 having different desired viscosities were obtained.
[0065] (Preparation of water- and oil-repellent paper) The water- and oil-repellent agent was adjusted to have 20% by mass of octenylsuccinic acid modified starch-1 and 0.5% by mass of alkyl ketene dimer, processed with a size press machine, and then dried with a drum dryer to obtain water- and oil-repellent paper (processed paper). The viscosity of the water- and oil-repellent agent was 80 cps. The total coating weight of the solids of the octenylsuccinic acid modified starch-1 and alkyl ketene dimer of the obtained water- and oil-repellent paper was 3.2 g / m 2The obtained water- and oil-repellent paper was used as a test paper to carry out an oil resistance test (practical oil test), an evaluation of water absorbency (Cobb value), and an evaluation of air permeability. The evaluation results are shown in Table 2. The size press treatment (using a size press machine manufactured by Mathis) described here refers to a so-called pound-type two-roll size press treatment in which a water- and oil-repellent agent is stored between rolls and the base paper is passed through the water- and oil-repellent agent between the rolls at any roll speed and nip pressure.
[0066] [Example 2] The same treatment as in Example 1 was carried out except that the alkyl ketene dimer was adjusted to 1.0 mass %. The total solid coating amount of the octenylsuccinic acid modified starch-1 and the alkyl ketene dimer of the obtained water- and oil-repellent paper was 3.5 g / m 2 The viscosity of the water / oil repellent was 108 cps. The evaluation results are shown in Table 2.
[0067] [Example 3] Except for using octenylsuccinic acid modified starch-2, the same treatment as in Example 1 was carried out. The coating amount of the solid content of octenylsuccinic acid modified starch-2 on the obtained water- and oil-repellent paper was 3.2 g / m 2 The viscosity of the water / oil repellent was 58 cps. The evaluation results are shown in Table 2.
[0068] [Example 4] The same treatment as in Example 1 was carried out except that the amount of octenylsuccinic acid modified starch-2 was adjusted to 20% by mass and the amount of alkyl ketene dimer was adjusted to 1.0% by mass. The total coating amount of the solid content of the octenylsuccinic acid modified starch-2 and the alkyl ketene dimer of the obtained water- and oil-repellent paper was 3.4 g / m 2 The viscosity of the water / oil repellent was 91 cps. The evaluation results are shown in Table 2.
[0069] [Comparative Example 1] The same treatment as in Example 1 was carried out except that octenyl succinic acid modified starch-3 was used. The viscosity of the water- and oil-repellent agent was 390 cps. Because the viscosity of the water- and oil-repellent agent was too high, the water- and oil-repellent agent could not be used to treat the paper. The evaluation results are shown in Table 2.
[0071] [Table 2]
[0072] From the above results, it was found that the water- and oil-repellent agent of the present disclosure can impart excellent water- and oil-repellency to paper. [Industrial Applicability]
[0073] The water and oil repellent of the present disclosure can be applied to paper used for food containers and food packaging materials.
Claims
1. A water and oil repellent agent comprising a polysaccharide and a sizing agent, The polysaccharide has a viscosity of 60 cps or less at 50° C. in a 20% by mass aqueous solution.
2. The water / oil repellent according to claim 1 , wherein the polysaccharide is starch.
3. The water / oil repellent according to claim 2 , wherein the starch is a hydrophobically modified starch.
4. The water / oil repellent according to claim 3 , wherein the hydrophobically modified starch is an alkenyl succinate-modified starch.
5. The water / oil repellent according to claim 1 , wherein the sizing agent is an alkyl ketene dimer.
6. The water / oil repellent according to claim 1, which has a viscosity at 50° C. of 300 cps or less.
7. The water / oil repellent according to claim 1 , wherein the content of the polysaccharide in the water / oil repellent is 40 mass % or less.
8. The water / oil repellent according to claim 1 , wherein the content of the sizing agent in the water / oil repellent is 5% by mass or less.
9. The water / oil repellent according to claim 1 , wherein the content of the sizing agent in the water / oil repellent is 10 mass % or less with respect to a total content of the polysaccharide and the sizing agent.
10. The water / oil repellent according to claim 1 , further comprising an additive.
11. The water- and oil-repellent agent according to claim 1 for treating the surface of paper.
12. A water- and oil-repellent paper having a water- and oil-repellent layer formed on a surface of the paper from the water- and oil-repellent agent according to claim 1.
13. The solid content of the water / oil repellent agent in the water / oil repellent layer is 6.0 g / m 2 The water- and oil-repellent paper according to claim 12, wherein:
14. A method for treating paper, comprising treating the paper with the water / oil repellent according to claim 1 by externally adding the same to the paper.
Citation Information
Patent Citations
Oil-proof treatment method of paper
CN105421144A
Coating agent for paper product
JP2002069889A
Surface treatment for paper
JP2005029940A
Oilproof sheetlike material