Wiring board, light emitting device, and manufacturing method thereof
By embedding a conductive paste of metal nanoparticles and particles in the insulating base material, the method enhances adhesion and reduces lateral spread, facilitating closer wiring layer spacing and preventing short circuits in wiring boards and light emitting devices.
Patent Information
- Application Number
- JP2023030068
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-06-27
- Filing Date
- 2023-02-28
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2043-02-28
Smart Images

Figure 0007553846000024 
Figure 0007553846000011 
Figure 0007553846000025
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a conductive paste, a wiring board, a light emitting device, and methods for manufacturing the same. [Background technology]
[0002] Conventionally, a wiring board having a wiring layer in which copper fine particles are sintered on a substrate is known. For example, Patent Document 1 discloses a method for producing a copper film, which includes a step of applying a composition containing copper fine particles onto a substrate to form a coating film, and a step of arranging a shape-conforming shield above the coating film and hot-pressing the coating film to sinter the copper fine particles. The copper fine particles contain copper nanoparticles having a number-average particle diameter of 1 nm or more and 200 nm or less. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2010-146734 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present disclosure is to provide a wiring board and a light emitting device that facilitate narrowing the gap between adjacent wiring layers, as well as methods for manufacturing the same, and a conductive paste for use therein. [Means for solving the problem]
[0005] A method for manufacturing a wiring board according to an embodiment of the present disclosure includes preparing a conductive paste containing metal nanoparticles having a median diameter of 10 nm or more and 500 nm or less, metal particles having a median diameter of 1 μm or more and 10 μm or less, and a resin; arranging the conductive paste on at least the first surface of an insulating base material having a first surface and a second surface opposite to the first surface; and heating and pressing the conductive paste using a roll press or a hard SUS plate to form a wiring layer, wherein in preparing the conductive paste, the mass of the metal nanoparticles is a compounding ratio of 5 mass% or more and 95 mass% or less with respect to the total mass of the metal nanoparticles and the metal particles, and in forming the wiring layer, the conductive paste is heated and pressed so that a portion of the wiring layer in the thickness direction is embedded in at least the first surface of the insulating base material.
[0006] A method for manufacturing a light emitting device according to an embodiment of the present disclosure includes manufacturing a wiring board by the method for manufacturing a wiring board disclosed in the embodiment, and placing a light emitting component on the wiring board.
[0007] A wiring board according to an embodiment of the present disclosure comprises an insulating substrate having a first surface and a second surface opposite to the first surface, and a wiring layer which is a conductive member including a sintered body of a mixture of metal nanoparticles and metal particles having a particle size larger than that of the metal nanoparticles and is arranged on at least the first surface of the insulating substrate, wherein the upper surface of the wiring layer is flat, the arithmetic mean roughness Ra indicating the flatness is 10 nm or more and 100 nm or less, and a portion of the wiring layer in the thickness direction is embedded in the insulating substrate.
[0008] A light emitting device according to an embodiment of the present disclosure includes a wiring board disclosed in the embodiment, and a light emitting component placed on the wiring board.
[0009] The conductive paste according to an embodiment of the present disclosure includes metal nanoparticles having a median diameter of 10 nm or more and 500 nm or less, metal particles having a median diameter of 1 μm or more and 10 μm or less, and a resin, in which the mass of the metal nanoparticles is mixed in a ratio of 5 mass% to 95 mass% relative to the total mass of the metal nanoparticles and the metal particles. Effect of the Invention
[0010] According to the embodiments of the present disclosure, it is possible to provide a wiring board and a light emitting device that facilitate narrowing the gap between adjacent wiring layers, as well as methods for manufacturing the same and a conductive paste used therefor. [Brief description of the drawings]
[0011] [Figure 1A] FIG. 1 is a schematic plan view illustrating an example of a light emitting device according to an embodiment. [Figure 1B] FIG. 1B is a schematic plan view showing an example of a part of FIG. 1A. [Figure 1C] FIG. 2 is a schematic plan view illustrating an example of a portion of a wiring board according to an embodiment. [Figure 1D] FIG. 2 is a schematic bottom view illustrating an example of a portion of a wiring board according to an embodiment. [Figure 2A] FIG. 2 is a schematic cross-sectional end view taken along line IIA-IIA in FIG. 1B. [Figure 2B] FIG. 2 is a schematic cross-sectional end view taken along line IIB-IIB in FIG. 1B. [Figure 2C] 4 is a schematic cut end view showing an example of a portion of an interlayer connection portion of a wiring board according to an embodiment. FIG. [Figure 3A] 4 is a flowchart showing a method for manufacturing a wiring board according to the embodiment. [Figure 3B] 4 is a flowchart showing a method for manufacturing a light emitting device according to an embodiment. [Figure 4A] 5A to 5C are schematic end views of a cut portion illustrating an example of a method for manufacturing a wiring board according to an embodiment. [Figure 4B] 5A to 5C are schematic end views of a cut portion illustrating an example of a method for manufacturing a wiring board according to an embodiment. [Figure 4C]5A to 5C are schematic end views of a cut portion illustrating an example of a method for manufacturing a wiring board according to an embodiment. [Figure 4D] 5A to 5C are schematic cross-sectional views illustrating an example of a method for manufacturing a light emitting device according to an embodiment. [Figure 4E] 5A to 5C are schematic cross-sectional views illustrating an example of a method for manufacturing a light emitting device according to an embodiment. [Figure 5A] 5A to 5C are schematic end views of a cut portion illustrating an example of a method for manufacturing a wiring board according to an embodiment. [Figure 5B] 5A to 5C are schematic end views of a cut portion illustrating an example of a method for manufacturing a wiring board according to an embodiment. [Figure 5C] 5A to 5C are schematic end views of a cut portion illustrating an example of a method for manufacturing a wiring board according to an embodiment. [Figure 5D] 5A to 5C are schematic end views of a cut portion illustrating an example of a method for manufacturing a wiring board according to an embodiment. [Figure 5E] 5A to 5C are schematic end views of a cut portion illustrating an example of a method for manufacturing a wiring board according to an embodiment. [Figure 5F] 5A to 5C are schematic end views of a cut portion illustrating an example of a method for manufacturing a wiring board according to an embodiment. [Figure 5G] 5A to 5C are schematic cross-sectional views illustrating an example of a method for manufacturing a light emitting device according to an embodiment. [Figure 6A] 1 is an image of a cross section of a wiring board in Example 1. [Figure 6B] 2 is a plan view image of a wiring board in Example 1. [Figure 6C] FIG. 1 is a plan view showing a sample when a chip share test is performed. [Figure 7A] 13 is an image of a cross section of a wiring board in Example 2. [Figure 7B] 13 is a plan view image of a wiring board in Example 2. [Figure 8A] 1 is an image of a cross section of a wiring board in Comparative Example 1. [Figure 8B] 1 is a plan view image of a wiring board in Comparative Example 1. [Figure 9] 13 is an image of a cross section of a wiring board in Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] <<Embodiment>> The embodiments will be described below with reference to the drawings. However, the embodiments shown below are illustrative of the conductive paste, wiring board, light-emitting device, and their manufacturing methods for embodying the technical idea of the present embodiment, and are not limited to the following. Furthermore, the dimensions, materials, shapes, and relative positions of the components described in the embodiments are merely illustrative, and are not intended to limit the scope of the present invention, unless otherwise specified. The sizes and positional relationships of the components shown in each drawing may be exaggerated or simplified to clarify the explanation. Furthermore, in the embodiments, "covering" is not limited to direct contact, but also includes indirect covering, for example, through other members. Furthermore, "disposing" is not limited to direct contact, but also includes indirect disposing, for example, through other members. Furthermore, "mounting" is not limited to direct contact, but also includes indirect mounting, for example, through other members.
[0013] <Wiring board and light emitting device> First, an example of a wiring substrate in a light emitting device according to an embodiment will be described, and then an example of a light emitting device according to an embodiment will be described.
[0014] FIG. 1A is a schematic plan view showing an example of a light emitting device according to an embodiment. FIG. 1B is a schematic plan view showing an example of a portion of FIG. 1A. FIG. 1C is a schematic plan view showing an example of a portion of a wiring board according to an embodiment. FIG. 1D is a schematic bottom view showing an example of a portion of a wiring board according to an embodiment. FIG. 2A is a schematic end view of a cut portion taken along line IIA-IIA in FIG. 1B. FIG. 2B is a schematic end view of a cut portion taken along line IIB-IIB in FIG. 1B. FIG. 2C is a schematic end view of a cut portion showing an example of a portion of an interlayer connection portion of a wiring board according to an embodiment.
[0015] 1B to 1D are schematic diagrams showing a portion A in FIG. 1A, and FIGS. 1C and 1D show the wiring board from which the light emitting component and covering member have been removed.
[0016] [Wiring board] The wiring board 100 includes an insulating base material 10 having a first surface 10a and a second surface 10b opposite to the first surface 10a, and a wiring layer 20 which is a conductive member. The wiring layer 20 includes a sintered body of a mixture of metal nanoparticles and metal particles having a particle size larger than that of the metal nanoparticles, which is disposed on at least the first surface 10a of the insulating base material 10. The upper surface of the wiring layer 20 is flat, and the arithmetic mean roughness Ra indicating the flatness is 10 nm or more and 100 nm or less. In the wiring board 100, a part of the wiring layer 20 in the thickness direction is embedded in the insulating base material 10.
[0017] In addition, the insulating substrate 10 has a through hole 15, a wiring layer 20 is arranged on the first surface 10a of the insulating substrate 10 and the second surface 10b of the insulating substrate 10, and a conductive member 23 is arranged in the through hole 15, so that a portion of the thickness direction of each of the wiring layer 20 on the first surface 10a and the wiring layer 20 on the second surface 10b is embedded in the insulating substrate 10. Hereinafter, the wiring layer 20 on the first surface 10a of the insulating base material 10 will be referred to as a first wiring layer 21 as appropriate, and the wiring layer 20 on the second surface 10b of the insulating base material 10 will be referred to as a second wiring layer 22 as appropriate.
[0018] The insulating base material 10 is preferably glass epoxy, bismaleimide triazine resin, or liquid crystal polymer. If the insulating base material 10 is glass epoxy, bismaleimide triazine resin, or liquid crystal polymer, the insulating base material 10 is likely to soften by heating in the manufacturing process of the wiring board 100, and the wiring layer 20 is easily embedded in the insulating base material 10. As the glass epoxy, a plate-shaped glass epoxy obtained by impregnating one or more sheets of glass cloth with an insulating resin such as epoxy resin and hardening the same can be used. As the glass epoxy, for example, FR-4 can be mentioned.
[0019] The through hole 15 is formed penetrating the insulating base material 10. The through hole 15 is provided at a location in the insulating base material 10 where the first wiring layer 21 of the insulating base material 10 and the second wiring layer 22 of the insulating base material 10 are electrically connected. The shape of the through hole 15 in plan view is preferably a circle, but it may also be an ellipse or a polygon such as a rectangle. When the shape of the through hole 15 in plan view is a circle, it is preferable that the diameter is, for example, 100 μm or more and 400 μm or less. By setting the diameter of the through hole 15 within this range, it becomes easier to arrange the conductive member 23.
[0020] The insulating base material 10 has a first recess 11 on the first surface 10a side and a second recess 12 on the second surface 10b side. The first recess 11 and the second recess 12 are formed by embedding the wiring layer 20. The thickness T1 of the insulating base material 10 in the area where the first recess 11 and the second recess 12 are not formed is preferably 40 μm or more and 1 mm or less. If the thickness T1 of the insulating base material 10 is 40 μm or more, the strength of the wiring board 100 can be improved. On the other hand, if the thickness T1 of the insulating base material 10 is 1 mm or less, the wiring board 100 can be made thinner. The first surface 10a of the insulating base material 10 includes the bottom surface of the first recess 11. The second surface 10b of the insulating base material 10 includes the bottom surface of the second recess 12. The thickness T1 is the maximum thickness in the direction perpendicular to the second surface 10b of the insulating base material 10.
[0021] The first surface 10a and the second surface 10b of the insulating base material 10 are preferably roughened. The roughened surface improves the adhesion between the insulating base material 10 and the wiring layer 20 and the covering member 30. The roughening can be performed, for example, by etching, polishing, a method using a mold, or the like. The roughening can be performed, for example, so that the surface roughness Ra (arithmetic mean roughness) is 1 μm or more and 7 μm or less. The surface roughness Ra can be a value measured by using, for example, a stylus-type step thickness gauge (Alpha-Step-IQ manufactured by KLA Tencor) to measure 2000 μm at a speed of 200 μm / s.
[0022] The first wiring layer 21 is disposed on the first surface 10a of the insulating base material 10. The second wiring layer 22 is disposed on the second surface 10b of the insulating base material 10. The first wiring layer 21 and the second wiring layer 22 are formed by heating and pressurizing a conductive paste containing a mixture of metal nanoparticles and metal particles to sinter the mixture, as described later. Therefore, the first wiring layer 21 and the second wiring layer 22 are conductive members containing a sintered body of the mixture. Here, the sintered body may be in a state in which unsintered metal particles are contained in a sintered body of metal nanoparticles, or in a state in which sintered metal particles are contained. That is, the metal particles may be in a state of unsintered particles, or in a state in which metal particles are sintered with each other, or in a state in which metal particles are sintered with metal nanoparticles.
[0023] The first surface 21a of the first wiring layer 21 is flat. Therefore, it is easy to place the light emitting component 50 thereon. In addition, the first surface 22a of the second wiring layer 22 is flat. Note that, "flat" refers to, for example, a difference in thickness between the thinnest part and the thickest part of the wiring layer 20 being 3 μm or less, preferably 0.3 μm or less, and more preferably 0.03 μm or less. In forming the wiring layer 20, it is preferable that the upper surface, i.e., the first surface 21a, of the formed first wiring layer 21 is flat, and the thickness difference between the thinnest and thickest parts of the first wiring layer 21 is 3 μm or less. Similarly, in forming the wiring layer 20, it is preferable that the upper surface, i.e., the first surface 22a, of the formed second wiring layer 22 is flat, and the thickness difference between the thinnest and thickest parts of the second wiring layer 22 is 3 μm or less. The arithmetic mean roughness Ra indicating the flatness of the first surface 21a of the first wiring layer 21 and the first surface 22a of the second wiring layer 22 is preferably 10 nm or more and 100 nm or less. The arithmetic mean roughness Ra indicating the flatness is based on JIS B 0601:2013.
[0024] Moreover, the end 21ae of the first surface 21a of the first wiring layer 21 is preferably rounded. According to such a configuration, when the first wiring layer 21 is covered with the first covering member 31, the thickness of the first covering member 31 at the end 21ae becomes thick. Therefore, the color of the end 21ae is less likely to be transparent, and the reflectance can be increased. In the vicinity of the light-emitting component 50, the higher the reflectance, the brighter the surface light-emitting body can be. Furthermore, the roundness makes the first covering member 31 less likely to be damaged. Similarly, the end 22ae of the first surface 22a of the second wiring layer 22 is preferably rounded. According to such a configuration, the second covering member 32 is less likely to be damaged.
[0025] A part of the first wiring layer 21 in the thickness direction is embedded in the insulating base material 10. That is, a part of the first wiring layer 21 in the thickness direction is disposed in the first recess 11 of the insulating base material 10. This improves the adhesion between the first wiring layer 21 and the insulating base material 10. In addition, the thickness of the first wiring layer 21 exposed from the insulating base material 10 is reduced, and the thickness of the wiring board 100 can be reduced. The first wiring layer 21 is embedded in the insulating base material 10 over the entire second surface 21b, which is the surface opposite to the first surface 21a of the first wiring layer 21, and a predetermined length from the second surface 21b of the first wiring layer 21 in the thickness direction is embedded in the insulating base material 10. Furthermore, when a part of the first wiring layer 21 in the thickness direction is embedded by heating and pressurization, the outer periphery of the wiring where pressure is concentrated is deformed and embedded in a rounded shape.
[0026] Similarly, it is preferable that a part of the second wiring layer 22 in the thickness direction is embedded in the insulating base material 10. That is, it is preferable that a part of the second wiring layer 22 in the thickness direction is disposed in the second recess 12 of the insulating base material 10. This improves the adhesion between the second wiring layer 22 and the insulating base material 10. In addition, the thickness of the second wiring layer 22 exposed from the insulating base material 10 is reduced, and the thickness of the wiring board 100 can be reduced. The second wiring layer 22 is embedded in the insulating base material 10 over the entire second surface 22b, which is the surface of the second wiring layer 22 opposite to the first surface 22a, and a predetermined length in the thickness direction from the second surface 22b of the second wiring layer 22 is embedded in the insulating base material 10. Furthermore, when a part of the second wiring layer 22 in the thickness direction is embedded by applying heat and pressure, the outer periphery of the wiring where pressure is concentrated is deformed and embedded in a rounded shape.
[0027] The thickness t1 of the first wiring layer 21 is preferably 10 μm or more and 35 μm or less, and the first wiring layer 21 is preferably embedded in the insulating base material 10 to a depth of 5 μm or more and 25 μm or less. If the thickness t1 of the first wiring layer 21 is 10 μm or more, the first wiring layer 21 is easily formed, and a part of the first wiring layer 21 in the thickness direction is easily disposed within the insulating base material 10. The thickness t1 of the first wiring layer 21 is more preferably 13 μm or more, and further preferably 15 μm or more. On the other hand, if the thickness t1 of the first wiring layer 21 is 35 μm or less, the wiring board 100 can be made thinner. The thickness t1 of the first wiring layer 21 is more preferably 30 μm or less, and further preferably 20 μm or less.
[0028] Furthermore, if the thickness t3 of the first wiring layer 21 embedded in the insulating base material 10 is 5 μm or more, the adhesion between the first wiring layer 21 and the insulating base material 10 is further improved. The thickness t3 of the first wiring layer 21 is more preferably 7 μm or more, and even more preferably 10 μm or more. On the other hand, if the thickness t3 of the first wiring layer 21 embedded in the insulating base material 10 is 25 μm or less, the first wiring layer 21 is easily formed, and a part of the first wiring layer 21 in the thickness direction is easily disposed in the insulating base material 10. The thickness t3 of the first wiring layer 21 is more preferably 20 μm or less, and even more preferably 15 μm or less. Note that the thicknesses t1 and t3 are the maximum thicknesses of the first wiring layer 21 in the direction perpendicular to the second surface 21b.
[0029] In addition, the first wiring layer 21 is preferably embedded in the insulating base material 10 at a thickness of 1 / 100 or more and 6 / 100 or less of the thickness T1. If the first wiring layer 21 embedded in the insulating base material 10 is 1 / 100 or more of the thickness T1 of the insulating base material 10, the adhesion between the first wiring layer 21 and the insulating base material 10 is further improved. The first wiring layer 21 embedded in the insulating base material 10 is more preferably 2 / 100 or more of the thickness T1 of the insulating base material 10. On the other hand, if the first wiring layer 21 embedded in the insulating base material 10 is 6 / 100 or less of the thickness T1 of the insulating base material 10, the first wiring layer 21 is easily formed, and a part of the first wiring layer 21 in the thickness direction is easily disposed within the insulating base material 10. The first wiring layer 21 embedded in the insulating base material 10 is more preferably 4 / 100 or less of the thickness T1 of the insulating base material 10.
[0030] Moreover, for the same reason as for the first wiring layer 21, it is preferable that the second wiring layer 22 has the following configuration. The thickness t2 of the second wiring layer 22 is preferably 10 μm or more and 35 μm or less, and the second wiring layer 22 is preferably embedded in the insulating base material 10 to a depth of 5 μm or more and 25 μm or less. The thickness t2 of the second wiring layer 22 is more preferably 13 μm or more, and even more preferably 15 μm or more. The thickness t2 of the second wiring layer 22 is more preferably 30 μm or less, and even more preferably 20 μm or less. The thickness t4 of the second wiring layer 22 embedded in the insulating base material 10 is more preferably 7 μm or more, and even more preferably 10 μm or more. The thickness t4 of the second wiring layer 22 embedded in the insulating base material 10 is more preferably 20 μm or less, and even more preferably 15 μm or less. The thicknesses t2 and t4 are the maximum thicknesses in the direction perpendicular to the second surface 22b of the second wiring layer 22.
[0031] The second wiring layer 22 is preferably embedded in a thickness ranging from 1 / 100 to 6 / 100 of the thickness T1 of the insulating base material 10. The second wiring layer 22 embedded in the insulating base material 10 is more preferably embedded in a thickness ranging from 2 / 100 to 4 / 100 of the thickness T1 of the insulating base material 10. Note that the preferred ratio between the thickness of the insulating base material 10 and the thickness of the first wiring layer 21 embedded in the insulating base material 10 or the thickness of the second wiring layer 22 embedded in the insulating base material 10, and the preferred numerical values of the thickness of the insulating base material 10, the thickness of the first wiring layer 21, the thickness of the second wiring layer 22, and the thicknesses of the first wiring layer 21 and the second wiring layer 22 embedded in the insulating base material 10 vary depending on the thickness, hardness, etc. of the members used. Therefore, these actual ratios and thicknesses do not necessarily match the preferred values explained above.
[0032] The conductive member 23 is disposed in the through hole 15, and is electrically connected to the first wiring layer 21 and the second wiring layer 22. The conductive member 23 disposed in the through hole 15 serves as an interlayer connection portion. The conductive member 23 in the through hole 15 is made of the same material as the first wiring layer 21 and the second wiring layer 22, and is a conductive member including a sintered body of a mixture of metal nanoparticles and metal particles.
[0033] In the wiring board 100, in a plan view of the portion where the through hole 15 is formed, the diameter R1 of the center in the thickness direction is larger than the diameter R2 of the portion formed on the first surface 10a of the insulating base material 10 and the diameter R3 of the portion formed on the second surface 10b of the insulating base material 10. That is, the diameter R1 of the center of the through hole 15 in the thickness direction is larger than the diameter R2 of one hole opening portion and the diameter R3 of the other hole opening portion. The diameter R1 of the center of the through hole 15 is larger than the diameters R2 and R3 of the hole opening portion, so that the conductive member 23 arranged in the through hole 15 is formed into a barrel shape. For convenience, the diameters R1, R2, and R3 are illustrated in a cross-sectional view in FIG. 2C. Thus, in a cross-sectional view, the width of the center of the through hole 15 (corresponding to R1) is larger than the width of one hole opening portion (corresponding to R2) and the width of the other hole opening portion (corresponding to R3).
[0034] The barrel shape is formed such that the conductive member 23 arranged in the through hole 15 is compressed more densely, so that the diameter R1 of the hole center and the diameters R2 and R3 of the hole opening are different. By forming such a shape, the adhesion between the insulating base material 10 and the conductive member 23 in the through hole 15 is improved, and the conductive member 23 is less likely to come out of the through hole 15. This further improves the adhesion between the wiring layer 20 and the insulating base material 10. In addition, by forming such a shape, the density of, for example, Cu is higher in the center of the through hole 15, so that the thermal resistance and electrical resistance of the interlayer connection are lowered. In addition, voids are crushed and disappear during compression, so that voids are less likely to occur in the interlayer connection.
[0035] It is preferable that the through hole 15 formed in the wiring board 100 has a diameter R1 at the center of the hole in the thickness direction that is 3% or more larger than the diameter R2 of one hole opening portion and the diameter R3 of the other hole opening portion. With this configuration, the density of Cu is higher in the center of the through hole 15, so that the thermal resistance and electrical resistance of the interlayer connection are lowered. Also, voids are less likely to occur in the interlayer connection. The upper limit of the diameter R1 of the hole center relative to the diameters R2 and R3 of the hole opening portions may be, for example, about 7.5%.
[0036] The diameters R2 and R3 of the hole openings may be the same as the diameter R1 of the hole center. Even with this configuration, if the conductive member 23 in the through hole 15 is compressed, the density of the conductive member 23 increases, so that the thermal resistance and electrical resistance of the interlayer connection are reduced. Also, voids are crushed and eliminated during compression, so that voids are less likely to occur in the interlayer connection.
[0037] The volume resistivity of the conductive member is preferably 10 μΩ·cm or less. That is, the volume resistivity of the wiring layer 20 (i.e., the first wiring layer 21 and the second wiring layer 22) and the conductive member 23 is preferably 10 μΩ·cm or less. If the volume resistivity of the conductive member is 10 μΩ·cm or less, the electrical resistance of the wiring layer 20 and the conductive member 23 can be further reduced. The volume resistivity of the conductive member is more preferably 8 μΩ·cm or less, and further preferably 6 μΩ·cm or less. The lower limit of the volume resistivity of the conductive member is not particularly limited, but is, for example, 2 μΩ·cm or more. The volume resistivity of the conductive member can be measured, for example, using Loresta GP MCP-T610 (manufactured by Mitsubishi Chemical Analytech Co., Ltd.).
[0038] The specific gravity of the conductive member is preferably 7.0 or more. That is, the specific gravity of the wiring layer 20 (i.e., the first wiring layer 21 and the second wiring layer 22) and the conductive member 23 is preferably 7.0 or more. If the specific gravity of the conductive member is 7.0 or more, the adhesion between the wiring layer 20 and the conductive member 23 and the insulating substrate 10 is further improved. The specific gravity of the conductive member is more preferably 7.5 or more, and further preferably 8.0 or more. The upper limit of the specific gravity of the conductive member is not particularly limited, but is, for example, 8.8 or less. The specific gravity of the conductive member can be measured, for example, using the method described in JIS Z 8807:2012 "Method of measuring density and specific gravity of solids" (for example, a method using a pycnometer).
[0039] [Light emitting device] Next, an example of a light emitting device according to an embodiment will be described. The light emitting device 200 includes a wiring board 100 and a light emitting component 50 mounted on the wiring board 100. It is preferable that the light emitting device 200 further includes a covering member 30. The wiring board 100 is as described above.
[0040] The covering member 30 includes a first covering member 31 and a second covering member 32. The first covering member 31 is disposed, for example, on the wiring board 100 at a location other than the location where the light emitting component 50 is disposed. Specifically, on the first surface 10a side of the insulating base material 10, an opening 35 is formed at the location where the light emitting component 50 is disposed, and the first covering member 31 is disposed so as to cover the first surface 10a and the first wiring layer 21 of the insulating base material 10. Moreover, the second covering member 32 is disposed on the second surface 10b side of the insulating base material 10 so as to cover the second surface 10b and the second wiring layer 22 of the insulating base material 10.
[0041] The covering member 30 is insulating, and may be, for example, a solder resist, a polyimide resin, a phenyl silicone resin, a dimethyl silicone resin, or the like. As the solder resist, for example, a general one in which a solvent, a defoaming agent, or the like is mixed with a copolymer resin such as epoxy, or a one whitened by adding a filler such as titanium oxide, may be used. The thickness of the first covering member 31 and the second covering member 32 is, for example, 10 μm or more and 50 μm or less.
[0042] The light emitting component 50 is placed on the first wiring layer 21 at the position of the opening 35 of the first covering member 31 via the adhesive member 40. The adhesive member 40 may be, for example, solder paste. The light emitting component 50 may be, for example, a light emitting element. The light emitting element may be, for example, a semiconductor laser element, an LED (Light Emitting Diode), an organic electroluminescence element, or the like. The light emitting component 50 may be a known light emitting element itself, or may be a light emitting component in which a known light emitting element is mounted on a board, a package, or the like. That is, the light emitting device 200 may be one in which a light emitting element is directly mounted on the wiring board 100, or one in which a light emitting component including at least a light emitting element is mounted on the wiring board 100.
[0043] <Conductive paste> Next, an example of a conductive paste used in manufacturing the wiring board according to the embodiment will be described. The conductive paste contains, for example, metal nanoparticles with a median diameter of 10 nm to 500 nm, metal particles with a median diameter of 1 μm to 10 μm, and a resin. The compounding ratio of the metal nanoparticles and the metal particles, [metal nanoparticles:metal particles], is preferably from [95:5] to [5:95]. This indicates that the mass of the metal nanoparticles is from 5 mass% to 95 mass% with respect to the total mass of the metal nanoparticles and the metal particles. In other words, the compounding ratio of the metal nanoparticles (%) = (mass of the metal nanoparticles / (mass of the metal nanoparticles+mass of the metal particles)) x 100 (%), and the compounding ratio of the metal particles (%) = (mass of the metal particles / (mass of the metal nanoparticles+mass of the metal particles)) x 100 (%).
[0044] The metal nanoparticles are, for example, nano-copper powder. The metal nanoparticles are, for example, metal nanoparticles that are sintered at 300°C or less. The metal nanoparticles are preferably sintered at 150°C or less, more preferably 120°C or less, and even more preferably 100°C or less. The lower limit of the temperature is not particularly limited as long as sintering is possible using the metal nanoparticles, but is, for example, 90°C or more. However, the lower limit of the temperature is preferably as low as possible.
[0045] The metal nanoparticles preferably have a median diameter of 10 nm to 500 nm, inclusive. Such metal nanoparticles are easily available commercially and are easy to prepare. The metal nanoparticles may be spherical, flat, or have another shape. The term "flat" refers to a flat shape, for example, a shape whose thickness is smaller than the maximum length in the planar direction.
[0046] The metal particles are, for example, copper powder having a particle size larger than that of the metal nanoparticles. The metal particles preferably have a median diameter of 1 μm or more and 10 μm or less. Such metal particles are easy to obtain commercially and are easy to prepare. By mixing the metal particles with the metal nanoparticles, the lateral spread of the particles is suppressed, making it easier to narrow the gap between adjacent wiring layers 20.
[0047] Here, the median diameter is the 50% particle diameter (D50) in the volume-based particle size distribution, specifically, the particle diameter (volume median diameter) at which the volume cumulative frequency from the small diameter side in the volume-based particle size distribution measured by the laser diffraction scattering particle size distribution measurement method reaches 50%. For the laser diffraction scattering particle size distribution measurement method, for example, a laser diffraction particle size distribution measurement device (product name: MASTER SIZER3000, manufactured by MALVERN) can be used for the measurement.
[0048] The metal particles may be spherical, flat, or of other shapes. However, the metal particles are preferably flat. If the metal particles are flat, the voids in the wiring layer 20 tend to be reduced after a part of the wiring layer 20 is embedded in the insulating substrate 10, and the wiring layer 20 is less likely to break. Furthermore, the metal particles preferably have a flat shape, and the ratio of the thickness to the maximum length in the surface direction is in the range of 5 to 20. That is, when the maximum length in the surface direction is 100, the thickness is preferably in the range of 5 to 20. With such a flat shape, the voids in the wiring layer 20 tend to be reduced, and the wiring layer 20 is less likely to break. The thickness means the maximum thickness in the direction perpendicular to the surface direction.
[0049] The metal nanoparticles and metal particles may be commercially available. As the metal nanoparticles, for example, CH-0200L1 (spherical) and CH-0200DP (flat) manufactured by Mitsui Mining & Smelting Co., Ltd. may be used. As the metal particles, for example, 1200Y (spherical) and 1200YP (flat) manufactured by Mitsui Mining & Smelting Co., Ltd. may be used. It is preferable that the surface of the metal particles is not covered with aliphatic carboxylic acid molecules. This makes it easier to prepare the conductive paste.
[0050] The compounding ratio of the metal nanoparticles and the metal particles, [metal nanoparticles:metal particles], is preferably from [95:5] to [5:95]. That is, when the total mass of the metal nanoparticles and the metal particles is 100 mass%, the metal nanoparticles are preferably from 5 mass% to 95 mass% and the metal particles are preferably from 5 mass% to 95 mass%. If the metal nanoparticles are 5 mass% or more, the mixture of the metal nanoparticles and the metal particles is easily sintered. The metal nanoparticles are more preferably 25 mass% or more. Moreover, the metal nanoparticles are more preferably 60 mass% or more, and even more preferably 70 mass% or more. By making the metal nanoparticles 60 mass% or more, the metal nanoparticles can be densely packed between the metal particles, and the resistance can be reduced by sintering. On the other hand, if the metal nanoparticles are 95 mass% or less, the spread of the particles in the lateral direction is further suppressed, and the interval between the adjacent wiring layers 20 can be made narrower. The metal nanoparticles are more preferably 87 mass% or less, and even more preferably 85 mass% or less. Moreover, if the metal particles are 5% by mass or more, the spread of the particles in the lateral direction is further suppressed, and the interval between adjacent wiring layers 20 can be made narrower. On the other hand, if the metal particles are 95% by mass or less, the mixture is more easily sintered. The metal particles are more preferably 75% by mass or less. The ratio of [metal nanoparticles:metal particles] is preferably from [85:15] to [25:75], more preferably from [83:17] to [77:23], and even more preferably from [80:20]. In other words, the ratio of the mass of the metal nanoparticles to the total mass of the metal nanoparticles and the metal particles is preferably from 25% by mass to 85% by mass, more preferably from 77% by mass to 83% by mass, and even more preferably 80% by mass.
[0051] The resin is preferably contained in an amount of 0.2% by mass or more and 30% by mass or less with respect to the total mass of the conductive paste. If the resin content is 0.2% by mass or more, the viscosity of the conductive paste is increased, the wiring layer 20 is easily formed, and the adhesion between the wiring layer 20 and the insulating base material 10 is further improved. On the other hand, if the resin content is 30% by mass or less, the mixture is more easily sintered. Examples of the resin include thermosetting resins such as epoxy resin, silicone resin, phenol resin, polyimide resin, polyurethane resin, melamine resin, and urea resin, and thermoplastic resins such as polyvinylpyrrolidone resin, polyvinyl alcohol resin, polyethylene glycol resin, and polyamide resin, and specifically, for example, S-LEC (registered trademark) SV-26 manufactured by Sekisui Chemical Co., Ltd. The resin may be the same type as that of the insulating base material 10.
[0052] The conductive paste preferably contains a solvent. The conductive paste preferably contains 2% by mass or more and 50% by mass or less of the solvent with respect to the total mass of the conductive paste. If the content of the solvent is 2% by mass or more, the resin is easily dissolved. On the other hand, if the content of the solvent is 50% by mass or less, the viscosity of the conductive paste is high, and the wiring layer 20 is easily formed. In addition, the solvent preferably has a boiling point of 300° C. or less. If the boiling point is 300° C. or less, the solvent is easily volatilized when the conductive paste is heated and pressurized. The boiling point of the solvent is more preferably 280° C. or less, even more preferably 260° C. or less, and even more preferably 250° C. or less. The lower limit of the boiling point is not particularly limited, but is, for example, 80° C. or more, preferably 150° C. or more, and even more preferably 200° C. or more. If the boiling point is 150° C. or more, the solvent is easily decomposed and easily imparts reducing properties when the conductive paste is sintered.
[0053] The solvent is preferably a reducing solvent. By using a reducing solvent, the mixture of metal nanoparticles and metal particles can be sintered while being reduced. This makes it easier to promote sintering of the mixture even in an air atmosphere. The reducing solvent preferably includes at least one of alcohol-based, ether-based, ester-based, and acrylic-based solvents having at least a hydrocarbon group having 3 or more carbon atoms. Specific examples of the reducing solvent include butyl carbitol, 2-ethyl-1,3-hexanediol, 1,5-pentanediol, 1,2-hexanediol, and α-terpineol. Other examples include methanol, ethanol, propyl alcohol, butanol, hexanol, octanol, decanol, oleyl alcohol, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, glycerin, methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, oleylamine, α-terpineol, tetrahydronaphthalene, tetrahydroquinoline, tetralin, tetrahydrofuran, toluene, hexane, octane, hydrogenated pyrene, hydrogenated phenanthrene, hydrogenated wash oil, hydrogenated anthracene oil, and insulating oils such as silicon oil, aldehydes, and ketones.
[0054] <Method of Manufacturing Wiring Board and Light Emitting Device> Next, an example of a method for manufacturing a wiring board and a method for manufacturing a light emitting device according to the embodiment will be described. First, an example of a method for manufacturing a wiring board will be described, and then an example of a method for manufacturing a light emitting device will be described.
[0055] Fig. 3A is a flowchart showing a method for manufacturing a wiring board according to an embodiment. Fig. 3B is a flowchart showing a method for manufacturing a light emitting device according to an embodiment. Figs. 4A to 4C and Figs. 5A to 5F are schematic cross-sectional end views showing an example of a method for manufacturing a wiring board according to an embodiment. Figs. 4D, 4E, and 5G are schematic cross-sectional end views showing an example of a method for manufacturing a light emitting device according to an embodiment.
[0056] [Method of manufacturing wiring board] A method for manufacturing the wiring board 100 includes preparing a conductive paste 220 containing metal nanoparticles having a median diameter of 10 nm or more and 500 nm or less, metal particles having a median diameter of 1 μm or more and 10 μm or less, and a resin, arranging the conductive paste 220 on at least the first surface 10a of an insulating base material 10 having a first surface 10a and a second surface 10b opposite to the first surface 10a, and heating and pressing the conductive paste 220 using a roll press or a hard SUS plate to form a wiring layer 20, wherein in preparing the conductive paste 220, the mass of the metal nanoparticles is a compounding ratio of 5 mass% or more and 95 mass% or less with respect to the total mass of the metal nanoparticles and the metal particles, and in forming the wiring layer 20, the heating and pressing of the conductive paste 220 is performed so that a portion of the wiring layer 20 in the thickness direction is embedded in at least the first surface 10a of the insulating base material 10.
[0057] In addition, in the manufacturing method of the wiring board 100, in arranging the conductive paste 220, the insulating base material 10 has a through hole 15, and further, in arranging the conductive paste 220 on the second surface 10b of the insulating base material 10 and in the through hole 15, and forming a wiring layer, it is preferable that the heating and pressurization of the conductive paste 220 is performed so that a portion of the thickness direction of the wiring layer 20 is embedded in the second surface 10b of the insulating base material 10.
[0058] Specifically, the method for manufacturing the wiring substrate 100 includes steps S101 of preparing a conductive paste, S102 of arranging the conductive paste, and S103 of forming a wiring layer. The materials and arrangement of each member are the same as those described above in connection with wiring board 100, and therefore will not be described here as appropriate.
[0059] (Prepare the conductive paste) In step S101 of preparing a conductive paste, a conductive paste 220 is prepared, which contains metal nanoparticles having a median diameter of 10 nm or more and 500 nm or less, metal particles having a median diameter of 1 μm or more and 10 μm or less, and a resin. In S101 of preparing the conductive paste, the mass of the metal nanoparticles is set to a compounding ratio of 5 mass % to 95 mass % with respect to the total mass of the metal nanoparticles and the metal particles. The conductive paste 220 is as described above in relation to the example of the conductive paste.
[0060] (Place conductive paste) In S102 of disposing the conductive paste, the conductive paste 220 is disposed on the first surface 10a of the insulating base material 10. In this embodiment, the conductive paste 220 is also disposed on the second surface 10b of the insulating base material 10 and in the through holes 15 (see FIG. 4A and FIG. 5A to FIG. 5D). In S102 of disposing the conductive paste, for example, first, a film mask 60 such as a screen mask is attached to the insulating substrate, and then, for example, a through hole 15 is formed by drilling or punching to prepare the insulating substrate 10. Then, the through hole 15 of the insulating substrate 10 is filled with the conductive paste 220, and the conductive paste 220 is dried. Next, after the film mask 60 is peeled off, the conductive paste 220 is compressed by a roll press to dispose the conductive paste 220 in the through hole 15. Next, the conductive paste 220 is disposed on the first surface 10a of the insulating substrate 10, and then the conductive paste 220 is dried. Next, the conductive paste 220 is disposed on the second surface 10b of the insulating substrate 10, and then the conductive paste 220 is dried. By drying the conductive paste 220 disposed on the first surface 10a and the second surface 10b of the insulating substrate 10, the conductive paste 220 can be made to have a desired hardness, which makes it easier to apply pressure thereafter. The drying temperature is preferably, for example, from 60° C. to 100° C. The drying time is preferably, for example, from 3 minutes to 15 minutes.
[0061] The conductive paste 220 can be disposed by, for example, a screen printing method using a screen mask, or may be disposed by metal mask printing or by injection from the nozzle of a dispenser.
[0062] (Forming the wiring layer) In S103 for forming the wiring layer, the conductive paste 220 is heated and pressurized using a roll press or a hard SUS plate to form the wiring layer 20 (see Figs. 4B, 4C, 5E, and 5F). In S103 for forming the wiring layer 20, a mixture of metal nanoparticles and metal particles is sintered to form a sintered body. In S103 for forming the wiring layer 20, the resin in the conductive paste 220 is cured. In the method for manufacturing the wiring board 100, the conductive paste 220 is compressed and the mixture is sintered simultaneously, which further improves the adhesion between the wiring layer 20 and the insulating base material 10. In addition, the number of manufacturing steps can be reduced.
[0063] In S103 for forming the wiring layer, the conductive paste 220 is heated and pressed using a roll press or a hard SUS plate. In this way, the conductive paste 220 is less likely to adhere to the roll press or the hard SUS plate, and the surface condition of the wiring layer 20 can be improved.
[0064] In S103 of forming the wiring layer, the conductive paste 220 is heated and pressurized so that a part of the first wiring layer 21 in the thickness direction is embedded in the first surface 10a of the insulating base material 10. As a result, a first recess 11 is formed in the insulating base material 10. It is preferable that the conductive paste 220 is further heated and pressurized so that a part of the second wiring layer 22 in the thickness direction is embedded in the second surface 10b of the insulating base material 10. As a result, a second recess 12 is formed in the insulating base material 10. Note that by heating and pressing the conductive paste 220, a part of the wiring layer 20 in the thickness direction is embedded in at least the first surface 10a of the insulating base material 10 while the mixture is sintered.
[0065] In S103 for forming the wiring layers, the conductive paste 220 is preferably heated and pressurized so that the end 21ae of the first surface 21a of the first wiring layer 21 and the end 22ae of the first surface 22a of the second wiring layer 22 are rounded. When the conductive paste 220 is pressed, the conductive paste 220 is pressed with a flat member, so that pressure is concentrated on the end, and the end 21ae and the end 22ae are rounded.
[0066] In addition, in S103 for forming the wiring layers, it is preferable to heat and pressurize the conductive paste 220 so that the first wiring layer 21 and the second wiring layer 22 are embedded in the insulating base material 10 to a depth of 5 μm or more and 25 μm or less. In addition, in S103 for forming the wiring layers, it is preferable to heat and pressurize the conductive paste 220 so that the first wiring layer 21 and the second wiring layer 22 are embedded in the insulating base material 10 to a depth of 1 / 100 or more and 6 / 100 or less of the thickness of the insulating base material 10.
[0067] In S103 for forming the wiring layer, the conductive paste 220 is preferably heated and pressurized also for the conductive paste 220 disposed in the through hole 15. The conductive paste 220 is preferably heated and pressurized such that the diameter of the central portion in the thickness direction is larger than the diameter of the portions formed on the first surface 10a of the insulating base material 10 and the second surface 10b of the insulating base material 10 in a plan view in the portion where the through hole 15 is formed.
[0068] In S103, where the wiring layer is formed, it is preferable that the upper surface of the formed wiring layer 20 is flat, and the thickness difference between the thinnest part and the thickest part of the wiring layer 20 is 3 μm or less. In S103, where the wiring layer is formed, it is preferable that the upper surface of the formed wiring layer 20 is flat, and the arithmetic mean roughness Ra indicating flatness is 10 nm or more and 100 nm or less. In S103, where the wiring layer is formed, it is preferable that the interval between adjacent wiring layers 20 is 30 μm or more and 5 cm or less.
[0069] The conductive paste 220 is preferably heated and pressurized at, for example, 190°C or higher and 300°C or lower and 2MPa or higher and 20MPa or lower. If the heating temperature is 190°C or higher, the insulating base material 10 is likely to become soft, and the first wiring layer 21 and the second wiring layer 22 are likely to be embedded in the insulating base material 10. Also, the mixture is likely to be sintered. The heating temperature is more preferably 230°C or higher, and even more preferably 250°C or higher. On the other hand, if the heating temperature is 300°C or lower, the energy required during heating can be reduced, which is economical. The heating temperature is more preferably 280°C or lower, and even more preferably 270°C or lower.
[0070] Furthermore, if the pressure during pressurization is 2 MPa or more, the first wiring layer 21 and the second wiring layer 22 are easily embedded in the insulating base material 10. The pressure during pressurization is more preferably 5 MPa or more, and even more preferably 7 MPa or more. On the other hand, if the pressure during pressurization is 20 MPa or less, the energy required during pressurization can be reduced, which is economical. The pressure during pressurization is more preferably 15 MPa or less, and even more preferably 10 MPa or less.
[0071] The heating and pressurizing time is preferably, for example, 10 minutes or more and 1 hour or less. If the heating and pressurizing time is 10 minutes or more, the first wiring layer 21 and the second wiring layer 22 are easily embedded in the insulating base material 10. In addition, the mixture is easily sintered. The heating and pressurizing time is more preferably 20 minutes or more, and even more preferably 30 minutes or more. On the other hand, if the heating and pressurizing time is 1 hour or less, the energy required for heating and pressurizing can be reduced, which is economical. The heating and pressurizing time is more preferably 45 minutes or less, and even more preferably 40 minutes or less. It is preferable to perform the heating and pressurizing in an air atmosphere. By performing the heating and pressurizing in an air atmosphere, it is not necessary to block the outside air, and the wiring layer 20 can be easily formed. In addition, the conductive paste 220 preferably contains a reducing solvent, and the mixture of the metal nanoparticles and the metal particles is preferably sintered while being reduced with the reducing solvent. This makes it easier to sinter the mixture of the metal nanoparticles and the metal particles in the air atmosphere.
[0072] The conditions for heating and pressing may be appropriately adjusted depending on the thicknesses of the first wiring layer 21 and the second wiring layer 22 to be embedded in the insulating base material 10.
[0073] In S103, where the wiring layer is formed, it is preferable that at least the surface of the insulating base material 10 is deformed at a temperature of 190° C. or more and 300° C. or less. This makes it easier to embed the first wiring layer 21 and the second wiring layer 22 in the insulating base material 10. Also, it makes it easier to improve the adhesion between the insulating base material 10 and the wiring layer 20. Note that the deformation here refers to the occurrence of distortion, unevenness, etc. on the surface as the surface of the insulating base material 10 becomes soft. Also, the surface specifically refers to the first surface 10a and the second surface 10b of the insulating base material 10.
[0074] After disposing the conductive paste 220, and before forming the wiring layer 20, it is preferable to cover the conductive paste 220 with a polyimide sheet or a hard SUS plate as the peeling member 70. Then, in S103 where the wiring layer is formed, it is preferable to pressurize the conductive paste 220 via the peeling member 70. By doing so, the conductive paste 220 is less likely to adhere to the peeling member 70, and the peeling member 70 can be easily peeled off from the wiring layer 20 after heating and pressurization. This makes it possible to improve the surface condition of the wiring layer 20. Note that a metal plate that has been subjected to a release treatment such as Caniflon plating can also be used as the peeling member 70.
[0075] In this embodiment, the conductive paste 220 is made of a mixture of metal nanoparticles and metal particles, which suppresses the lateral spread of the particles. Therefore, the interval between adjacent wiring layers 20 may be 30 μm or more and 5 cm or less, and is easily set to, for example, 90 μm or more and 200 μm or less.
[0076] [Manufacturing method of light emitting device] The method for manufacturing the light emitting device 200 includes manufacturing the wiring board 100 by the method for manufacturing the wiring board 100, and placing the light emitting component 50 on the wiring board 100. Furthermore, a covering member 30 may be disposed.
[0077] Specifically, the method for manufacturing the light emitting device 200 includes S11 of manufacturing a wiring board, S12 of arranging a covering member, and S13 of mounting a light emitting component. The materials and arrangement of each member are the same as those described above in connection with the light emitting device 200, and therefore will not be described here as appropriate.
[0078] (Manufactures wiring boards) In step S11 for manufacturing the wiring board, the wiring board 100 is manufactured by the above-described method for manufacturing the wiring board 100. In S11 for manufacturing the wiring board, the wiring board 100 is manufactured by carrying out the above-mentioned S101 to S103.
[0079] (Placing covering materials) In S12 of disposing the covering member, the covering member 30 is disposed on the upper and lower surfaces of the wiring board 100 in areas other than the areas where the light emitting components 50 are disposed (see FIGS. 4D and 5G). The covering member 30 can be disposed by, for example, a screen printing method using a screen mask. Furthermore, when greater precision is required, the covering member 30 can be disposed by exposing and developing a photosensitive resist material.
[0080] In the wiring board 100, a part of the wiring layer 20 in the thickness direction is embedded in the insulating base material 10, so that the thickness of the wiring layer 20 exposed from the insulating base material 10 can be made thin. Therefore, when forming the covering member 30, the covering member 30 is less likely to sag in the portion covering the wiring layer 20, and the covering member 30 is more likely to be applied thickly with a predetermined thickness. This allows the light emitting device 200 to have an improved reflectance.
[0081] (Place the light-emitting parts) In step S13 of placing the light emitting component, the light emitting component 50 is placed on the wiring board 100 (see FIG. 4E). In S13 of placing the light emitting component, the light emitting component 50 is placed on the first wiring layer 21 at the position of the opening 35 of the first covering member 31 using an adhesive member 40 such as solder paste.
[0082] The wiring board and light emitting device of the present embodiment have the following advantageous effects compared to the conventional technology. For example, in a wiring board having a wiring layer in which copper nanoparticles are sintered on a substrate as in the conventional technology, it is not possible to improve the adhesion between the wiring layer and the substrate. In addition, when only nanoparticles are used, the nanoparticles tend to spread laterally. When the nanoparticles spread laterally, bleeding occurs in the wiring layer, which makes it easy for short circuits to occur with adjacent wiring. Therefore, it is difficult to narrow the distance between the wirings in the conventional technology.
[0083] In contrast, in the wiring board and light emitting device according to the present embodiment, a part of the wiring layer in the thickness direction is embedded in at least the first surface of the insulating base material, and therefore the adhesion between the wiring layer and the insulating base material is excellent. In addition, the manufacturing method of the wiring board and light emitting device according to the present embodiment uses a mixture of metal nanoparticles and metal particles, so that the particles are suppressed from spreading laterally, and the particles are less likely to spread laterally. This suppresses bleeding of the wiring layer, and makes it difficult for adjacent wirings to short out. Therefore, the wiring board and light emitting device according to the present embodiment make it easier to narrow the distance between the wirings. Furthermore, in the wiring board and light emitting device according to the present embodiment, the conductive paste is pressurized and the mixture is sintered simultaneously, so that the adhesion between the wiring layer and the insulating base material is improved.
[0084] Although the embodiments of the invention have been described above in detail, the gist of the present invention is not limited to these descriptions and should be broadly interpreted based on the claims. In addition, various changes and modifications based on these descriptions are also included in the gist of the present invention.
[0085] For example, the wiring board and the light emitting device may have no interlayer connection. Alternatively, the wiring board and the light emitting device may have a wiring layer only on the first surface of the insulating base material. Furthermore, the light emitting device may include electronic components such as chip resistors and capacitors in addition to or instead of the light emitting components.
[0086] Furthermore, the method for manufacturing the wiring board and the light emitting device may include other steps between, before, or after each of the steps (S101 to S103, S11 to S13) as long as they do not adversely affect the steps. For example, the method may include removing foreign matter that has been mixed in during the manufacturing process. EXAMPLES
[0087] Next, examples and comparative examples will be described. FIG. 6A is an image of a cross section of the wiring board in Example 1. FIG. 6B is an image of a plan view of the wiring board in Example 1. FIG. 6C is a plan view showing a sample when performing a chip share test. FIG. 7A is an image of a cross section of the wiring board in Example 2. FIG. 7B is an image of a plan view of the wiring board in Example 2. FIG. 8A is an image of a cross section of the wiring board in Comparative Example 1. FIG. 8B is an image of a plan view of the wiring board in Comparative Example 1. FIG. 9 is an image of a cross section of the wiring board in Example 3.
[0088] The wiring board was made using the following materials. Insulating substrate: FR-4 (substrate thickness: 400 μm) Insulating substrate: FR-4 (substrate thickness: 200 μm) Metal nanoparticles: CH-0200L1 (Mitsui Mining & Smelting Co., Ltd., median diameter: 210 nm, spherical) Metal particles: 1200YP (Mitsui Mining & Smelting Co., Ltd., median diameter: 2.98 μm, flat shape) Metal particles: 1200Y (Mitsui Mining & Smelting Co., Ltd., median diameter: 1.91 μm, spherical) Solvent: Butyl carbitol (boiling point: 230°C) Resin: S-LEC SV-26 (manufactured by Sekisui Chemical Co., Ltd.) Film mask: HITALEX (registered trademark) (manufactured by Showa Denko Materials Co., Ltd., film thickness: 40 μm)
[0089] [Example 1] The compounding ratio of the metal nanoparticles and the metal particles (1200YP) [metal nanoparticles:metal particles] is set to [50:50]. A conductive paste was prepared by mixing 13 parts by mass of the solvent and 1 part by mass of the resin when the mixture of the metal nanoparticles and the metal particles (1200YP) was set to 100 parts by mass. Next, the conductive paste was screen-printed on the upper surface of the insulating substrate (substrate thickness: 400 μm) using a screen mask with a line (i.e., the width of the wiring, here the width of the conductive paste) of 0.2 mm and a space (i.e., the interval between adjacent wiring, here the interval between the conductive paste) of 0.2 mm, and dried at 80 ° C. Next, the conductive paste was covered with a polyimide sheet and hot-pressed in the air at 260 ° C., 9 MPa, and 30 minutes to prepare a wiring board in which a part of the thickness direction of the wiring layer was embedded in the insulating substrate.
[0090] 6A and 6B, the thickness of the wiring layer 20A was 18 μm, of which 5 μm was embedded in the insulating base material 10 A in the thickness direction. The distance between the wiring layers 20A was in the range of 90 μm to 120 μm. As shown in FIG. 6C, a wiring board was fabricated by forming wiring layers 20A1 and 20A2 on the insulating base material 10A under the above conditions. A 1 mm×1 mm LED chip 50A having a terminal 51 was solder-mounted on the wiring layer 20A1, and a chip shear test was performed on three of them. The adhesion between the wiring layer 20A1 arranged under the LED chip 50A and the insulating base material 10A was examined. The average adhesion was 3.1 kgf. In addition, when the wiring layers 20A2 at the four corners were inspected by X-ray inspection, voids were found to occur in all three of them at a rate of about 10% or less.
[0091] [Example 2] A wiring board was produced under the same conditions as in Example 1, except that 1200Y was used as the metal particles.
[0092] 7A and 7B, the thickness of the wiring layer 20B was 29 μm, of which 9 μm was embedded in the insulating base material 10A in the thickness direction. The distance between the wiring layers 20B was in the range of 150 μm to 180 μm. As in Example 1, a chip share test was performed, and the average value was 2.3 kgf.
[0093] [Comparative Example 1] A wiring board was produced under the same conditions as in Example 1, except that a conductive paste was prepared in which no metal particles were used and the metal nanoparticles were set to 100.
[0094] As shown in FIG. 8A and FIG. 8B, the thickness of the wiring layer 201 was 17 μm, of which 11 μm was embedded in the insulating base material 10A in the thickness direction. In addition, since only metal nanoparticles were used, bleeding occurred in the wiring layer 201, and adjacent wiring layers 201 came into contact with each other in some places. In addition, as in Examples 1 and 2, a chip share test was performed, and the average result was 3.8 kgf. In addition, when the wiring layers at the four corners were checked by X-ray inspection, voids were generated at a rate of about 10% or more in all three.
[0095] [Example 3] A conductive paste similar to that of Example 1 was prepared. After a film mask was attached to an insulating substrate (substrate thickness: 200 μm), a through hole with a diameter of 150 μm was formed. Then, the through hole of the insulating substrate was filled with a conductive paste, and the conductive paste was dried. Next, after removing the film mask, the conductive paste was compressed by a roll press to arrange the conductive paste in the through hole. Next, the conductive paste was screen-printed on the first surface of the insulating substrate, and dried at 80° C. Next, the conductive paste was screen-printed on the second surface of the insulating substrate, and dried at 80° C. Next, the conductive paste on the first surface and the second surface of the insulating substrate was covered with a polyimide sheet, and hot pressing was performed in the atmosphere under conditions of 260° C., 9 MPa, and 30 minutes. In this way, as shown in FIG. 9, a wiring board was produced in which a conductive member 23C was arranged in the through hole 15 and a part of the wiring layer 20C in the thickness direction was embedded in the first surface and the second surface of the insulating substrate 10B. The first wiring layer 21C on the first surface side and the second wiring layer 22C on the second surface side each had a thickness of 35 μm, of which 10 μm was embedded in the insulating base material 10B in the thickness direction. In addition, the interlayer connection formed by disposing the conductive member 23C in the through hole 15 had a barrel shape.
[0096] The conductive paste, wiring board, and light emitting device according to the embodiments of the present disclosure, and the methods for manufacturing the same, are, for example, as follows. [Section 1] Preparing a conductive paste containing metal nanoparticles having a median diameter of 10 nm to 500 nm, metal particles having a median diameter of 1 μm to 10 μm, and a resin; disposing the conductive paste on at least the first surface of an insulating substrate having a first surface and a second surface opposite the first surface; The conductive paste is heated and pressed using a roll press or a hard SUS plate to form a wiring layer; In preparing the conductive paste, the mass of the metal nanoparticles is 5 mass% or more and 95 mass% or less with respect to the total mass of the metal nanoparticles and the metal particles; A method for manufacturing a wiring board, in which, in forming the wiring layer, the conductive paste is heated and pressurized such that a portion of the wiring layer in a thickness direction is embedded in at least the first surface of the insulating base material.
[0097] [Section 2] Item 2. The method for manufacturing a wiring board according to item 1, wherein in preparing the conductive paste, the metal particles have a flat shape and a ratio of thickness to maximum length in a surface direction is in the range of 5 to 20.
[0098] [Section 3] 3. The method for producing a wiring board according to item 1 or 2, wherein in preparing the conductive paste, the surfaces of the metal particles are not covered with aliphatic carboxylic acid molecules.
[0099] [Section 4] 4. The method for manufacturing a wiring board according to any one of items 1 to 3, wherein in forming the wiring layer, the conductive paste is heated and pressurized at a temperature of 190° C. to 300° C. and at a pressure of 2 MPa to 20 MPa.
[0100] [Section 5] 5. The method for manufacturing a wiring board according to any one of items 1 to 4, wherein in disposing the conductive paste, the insulating base material is glass epoxy, bismaleimide triazine resin, or liquid crystal polymer.
[0101] [Section 6] 6. The method for manufacturing a wiring board according to any one of items 1 to 5, wherein in forming the wiring layer, at least a surface of the insulating base material is deformed at a temperature of 190° C. or more and 300° C. or less.
[0102] [Section 7] Item 7. The method for manufacturing a wiring board according to any one of items 1 to 6, wherein after the conductive paste is placed, the conductive paste is covered with a polyimide sheet or a hard SUS plate before the wiring layer is formed.
[0103] [Section 8] 8. The method for manufacturing a wiring board according to any one of items 1 to 7, wherein in preparing the conductive paste, the conductive paste contains a solvent having a boiling point of 300° C. or less.
[0104] [Section 9] 9. The method for manufacturing a wiring board according to item 8, wherein in preparing the conductive paste, the solvent includes at least one of an alcohol-based, an ether-based, an ester-based, and an acrylic-based solvent having a hydrocarbon having at least 3 carbon atoms.
[0105] [Section 10] 10. The method for manufacturing a wiring board according to item 8 or 9, wherein in preparing the conductive paste, the solvent has a boiling point of 150° C. or higher and 300° C. or lower.
[0106] [Section 11] In disposing the conductive paste, the insulating base material has a through hole, and the conductive paste is disposed on the second surface of the insulating base material and in the through hole; Item 11. The method for manufacturing a wiring board according to any one of items 1 to 10, wherein in forming the wiring layer, the conductive paste is heated and pressurized so that a part of the wiring layer in a thickness direction is embedded in the second surface of the insulating base material.
[0107] [Section 12] Item 12. The method for manufacturing a wiring board according to item 11, wherein in forming the wiring layer, the heating and pressurization of the conductive paste is also performed on the conductive paste disposed in the through hole.
[0108] [Section 13] Item 13. The method for manufacturing a wiring board according to item 11 or 12, wherein in forming the wiring layer, the conductive paste is heated and pressurized such that, in a plan view in the portion where the through hole is formed, the diameter of a center portion in a thickness direction is larger than the diameter of the portion formed on the first surface of the insulating base material and the second surface of the insulating base material.
[0109] [Section 14] Item 14. The method for manufacturing a wiring board according to any one of items 1 to 13, wherein, in forming the wiring layer, the conductive paste is heated and pressurized so that the wiring layer is embedded in the insulating base material to a depth of 5 μm to 25 μm.
[0110] [Section 15] Item 15. The method for manufacturing a wiring board according to any one of items 1 to 14, wherein, in forming the wiring layer, the conductive paste is heated and pressurized so that the wiring layer is embedded in the insulating base material by 1 / 100 or more and 6 / 100 or less of a thickness of the insulating base material.
[0111] [Section 16] Item 16. The method for manufacturing a wiring board according to any one of items 1 to 15, wherein, in forming the wiring layer, an upper surface of the formed wiring layer is flat, and a thickness difference between the thinnest part and the thickest part of the wiring layer is 3 μm or less.
[0112] [Section 17] Item 17. The method for manufacturing a wiring board according to any one of items 1 to 16, wherein, in forming the wiring layer, an upper surface of the formed wiring layer is flat, and an arithmetic mean roughness Ra indicating the flatness is 10 nm or more and 100 nm or less.
[0113] [Section 18] Item 18. The method for manufacturing a wiring board according to any one of items 1 to 17, wherein, in forming the wiring layers, a distance between adjacent wiring layers is 30 μm or more and 5 cm or less.
[0114] [Section 19] Manufacturing a wiring board by the method for manufacturing a wiring board according to any one of items 1 to 18; and placing a light emitting component on the wiring board.
[0115] [Section 20] an insulating substrate having a first surface and a second surface opposite to the first surface; a wiring layer that is a conductive member including a sintered body of a mixture of metal nanoparticles and metal particles having a particle size larger than that of the metal nanoparticles, the wiring layer being disposed on at least a first surface of the insulating base material; The upper surface of the wiring layer is flat, and the arithmetic mean roughness Ra indicating the flatness is 10 nm or more and 100 nm or less; A wiring board in which a part of the wiring layer in a thickness direction is embedded in the insulating base material.
[0116] [Section 21] The insulating substrate has a through hole, the wiring layer is disposed on a first surface and a second surface of the insulating base material, and the conductive member is disposed in the through hole; 21. The wiring board according to item 20, wherein a part of the thickness direction of each of the wiring layer on the first surface and the wiring layer on the second surface is embedded in the insulating base material.
[0117] [Section 22] Item 22. The wiring board according to item 21, wherein in a plan view in the portion where the through hole is formed, the diameter of the center in the thickness direction is larger than the diameter of the portion formed on the first surface of the insulating substrate and the second surface of the insulating substrate.
[0118] [Section 23] The thickness of the wiring layer is 10 μm or more and 35 μm or less, 23. The wiring board according to any one of items 20 to 22, wherein the wiring layer is embedded in the insulating base material to a depth of 5 μm to 25 μm.
[0119] [Section 24] Item 24. The wiring board according to any one of items 20 to 23, wherein the conductive member has a volume resistivity of 10 μΩ·cm or less.
[0120] [Section 25] Item 25. The wiring board according to any one of items 20 to 24, wherein the conductive member has a specific gravity of 7.0 or more.
[0121] [Section 26] 26. A light emitting device comprising: the wiring board according to any one of claims 20 to 25; and a light emitting component mounted on the wiring board.
[0122] [Section 27] Metal nanoparticles having a median diameter of 10 nm or more and 500 nm or less; Metal particles having a median diameter of 1 μm or more and 10 μm or less; A resin, The conductive paste has a compounding ratio of the mass of the metal nanoparticles to the total mass of the metal nanoparticles and the metal particles of 5 mass % or more and 95 mass % or less. [Industrial Applicability]
[0123] The wiring board and the light emitting device according to the embodiments of the present disclosure can be used in various electronic devices. [Explanation of symbols]
[0124] 10, 10A, 10B Insulating substrate 10a 1st page 10b 2nd side 11 First recess 12 Second recess 15 Through Hole 20, 20A, 20B, 20C, 20A1, 20A2 wiring layer 21, 21C 1st wiring layer 21a 1st page 21ae end 22, 22C 2nd wiring layer 21b 2nd side 22ae end 23, 23C Conductive materials 220 Conductive Paste 30 Covering material 31 First covering member 32 Second covering member 35 Opening 40 Adhesive material 50 Light emitting parts 50A LED Chip 51 Terminal 60 Film Mask 70 Peeling member 100 Wiring board 200 Light emitting device
Claims
1. Preparing a conductive paste containing metal nanoparticles having a median diameter of 10 nm to 500 nm, metal particles having a median diameter of 1 μm to 10 μm, and a resin; disposing the conductive paste on at least the first surface of an insulating substrate having a first surface and a second surface opposite the first surface; The conductive paste is heated and pressed using a roll press or a hard SUS plate to form a wiring layer; In preparing the conductive paste, a mass of the metal nanoparticles is 5 mass% or more and 95 mass% or less with respect to a total mass of the metal nanoparticles and the metal particles; In preparing the conductive paste, the metal particles have a flat shape and a ratio of a thickness to a maximum length in a surface direction is in a range of 5 to 20, The method for manufacturing a wiring board, in which the conductive paste is heated and pressurized in forming the wiring layer, such that a portion of the wiring layer in a thickness direction is embedded in at least the first surface of the insulating base material.
2. Preparing a conductive paste containing metal nanoparticles having a median diameter of 10 nm to 500 nm, metal particles having a median diameter of 1 μm to 10 μm, and a resin; disposing the conductive paste on at least the first surface of an insulating substrate having a first surface and a second surface opposite the first surface; The conductive paste is heated and pressed using a roll press or a hard SUS plate to form a wiring layer; In preparing the conductive paste, a mass of the metal nanoparticles is 5 mass% or more and 95 mass% or less with respect to a total mass of the metal nanoparticles and the metal particles; In disposing the conductive paste, the insulating base material has a through hole, and the conductive paste is disposed on the second surface of the insulating base material and in the through hole; A method for manufacturing a wiring board, in which, in forming the wiring layer, the conductive paste is heated and pressurized so that a portion of the wiring layer in the thickness direction is embedded in the first surface and the second surface of the insulating base material.
3. 3. The method for manufacturing a wiring board according to claim 1, wherein in preparing the conductive paste, the surfaces of the metal particles are not covered with aliphatic carboxylic acid molecules.
4. 3. The method for manufacturing a wiring board according to claim 1, wherein in forming the wiring layer, the conductive paste is heated and pressurized at a temperature of 190° C. to 300° C. and at a pressure of 2 MPa to 20 MPa.
5. 3. The method for manufacturing a wiring board according to claim 1, wherein the insulating base material is glass epoxy, bismaleimide triazine resin, or liquid crystal polymer in disposing the conductive paste.
6. 3. The method for manufacturing a wiring board according to claim 1, wherein in forming the wiring layer, at least a surface of the insulating base material is deformed at a temperature of 190° C. or more and 300° C. or less.
7. 3. The method for manufacturing a wiring board according to claim 1, wherein after the conductive paste is placed, the conductive paste is covered with a polyimide sheet or a hard SUS plate before the wiring layer is formed.
8. 3. The method for manufacturing a wiring board according to claim 1, wherein in preparing the conductive paste, the conductive paste contains a solvent having a boiling point of 300[deg.] C. or less.
9. 9. The method for manufacturing a wiring board according to claim 8, wherein in preparing the conductive paste, the solvent includes at least one of an alcohol-based, an ether-based, an ester-based, and an acrylic-based solvent having a hydrocarbon group having at least three carbon atoms.
10. 9. The method for manufacturing a wiring board according to claim 8, wherein in preparing the conductive paste, the solvent has a boiling point of 150° C. or more and 300° C. or less.
11. 3. The method for manufacturing a wiring board according to claim 2, wherein in forming the wiring layer, the conductive paste disposed in the through hole is also heated and pressurized.
12. 3. The method for manufacturing a wiring board as described in claim 2, wherein in forming the wiring layer, the conductive paste is heated and pressurized so that, in a planar view in the portion where the through hole is formed, the diameter of the center in the thickness direction is larger than the diameter of the portion formed on the first surface of the insulating base material and the second surface of the insulating base material.
13. 3. The method for manufacturing a wiring board according to claim 1, wherein in forming the wiring layer, the conductive paste is heated and pressurized so that the wiring layer is embedded in the insulating base material to a depth of 5 μm to 25 μm.
14. 3. The method for manufacturing a wiring board according to claim 1, wherein in forming the wiring layer, the conductive paste is heated and pressurized so that the wiring layer is embedded in the insulating base material by 1 / 100 or more and 6 / 100 or less of a thickness of the insulating base material.
15. 3. The method for manufacturing a wiring board according to claim 1, wherein, in forming the wiring layer, an upper surface of the formed wiring layer is flat, and a difference in thickness between the thinnest part and the thickest part of the wiring layer is 3 [mu]m or less.
16. 3. The method for manufacturing a wiring board according to claim 1, wherein, in forming the wiring layer, an upper surface of the formed wiring layer is flat, and an arithmetic mean roughness Ra indicating the flatness is 10 nm or more and 100 nm or less.
17. 3. The method for manufacturing a wiring board according to claim 1, wherein, in forming the wiring layers, a distance between adjacent wiring layers is 30 [mu]m or more and 5 cm or less.
18. Manufacturing a wiring board by the method for manufacturing a wiring board according to claim 1 or 2; and placing a light emitting component on the wiring board.
19. an insulating substrate having a first surface and a second surface opposite to the first surface; a wiring layer that is a conductive member including a sintered body of a mixture of metal nanoparticles and metal particles having a particle size larger than that of the metal nanoparticles, the wiring layer being disposed on at least a first surface of the insulating base material; The insulating substrate has a through hole, the wiring layer is disposed on a first surface and a second surface of the insulating base material, and the conductive member is disposed in the through hole; the upper surface of the wiring layer is flat, and the arithmetic mean roughness Ra indicating the flatness is 10 nm or more and 100 nm or less; A wiring board in which a portion of each of the wiring layer on the first surface and the wiring layer on the second surface in a thickness direction is embedded in the insulating base material.
20. The wiring board according to claim 19 , wherein in a planar view of the portion where the through hole is formed, the diameter of the center in the thickness direction is larger than the diameter of the portion formed on the first surface of the insulating substrate and the second surface of the insulating substrate.
21. The thickness of the wiring layer is 10 μm or more and 35 μm or less, 20. The wiring board according to claim 19, wherein the wiring layer is embedded in the insulating base material to a depth of 5 μm to 25 μm.
22. 20. The wiring board according to claim 19, wherein the conductive member has a volume resistivity of 10 μΩ·cm or less.
23. 20. The wiring board according to claim 19, wherein the conductive member has a specific gravity of 7.0 or more.
24. A light emitting device comprising: the wiring board according to claim 19; and a light emitting component mounted on the wiring board.
Citation Information
Patent Citations
Manufacture of wiring board
JP1997293952A
Method of manufacturing copper film
JP2010146734A
Copper paste and conductive film formation method
JP2020009554A
Circuit board and component mounting board, and manufacturing method thereof
JP2020053524A