Infrared light emitting device

The infrared light emitting element with a dislocation filter layer and controlled layer composition enhances emission intensity, addressing the insufficient signal intensity issue in existing LEDs for analytical instruments.

JP7554176B2Active Publication Date: 2024-09-19ASAHI KASEI MICRODEVICES CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021202790
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-12-21
Filing Date
2021-12-14
Publication Date
2024-09-19
Estimated Expiration
2038-08-30

AI Technical Summary

Technical Problem

Existing infrared LEDs do not provide sufficient emission intensity, limiting their application in analytical instruments due to insufficient signal intensity (S/N ratio).

Method used

The infrared light emitting element is designed with a specific layered structure that includes a dislocation filter layer to reduce defect density, comprising a semiconductor substrate, a first layer with a first conductivity type, a light emitting layer, and a second layer with a second conductivity type, where the layers are composed of AlInSb or AlGaInSb materials with controlled thickness and composition to bend dislocations laterally, reducing non-radiative recombination.

Benefits of technology

The design achieves a significant increase in emission intensity, enabling infrared LEDs to be used effectively in analytical instruments by improving the S/N ratio.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554176000008
    Figure 0007554176000008
  • Figure 0007554176000009
    Figure 0007554176000009
  • Figure 0007554176000010
    Figure 0007554176000010
Patent Text Reader

Abstract

Provided is an infrared light emitting element with high luminous intensity. The infrared light emitting device (100) comprises a semiconductor substrate (10), a first layer (20) formed on the semiconductor substrate and having a first conductivity type, a light emitting layer (30) formed on the first layer, and a second layer (40) formed on the light emitting layer and having a second conductivity type, the first layer being made of Al x(1) In 1-x(1) The layer containing Sb and the layer with a thickness of t y(1) [nm] and Al y(1) In 1-y(1) Sb-containing layer and Al x(2) In 1-x(2) a layer containing Sb, and y(1) , x(1), x(2) and y(1) are j=1, 2, 0 <t y(1) ≦2360×(y(1)-x(j))-240 (0.11≦y(1)-x(j)≦0.19), 0 <t y(1) ≦-1215×(y(1)-x(j))+427 (0.19
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to infrared light emitting devices. [Background technology]

[0002] In general, infrared rays in the long wavelength band of 2 μm or more are used in motion sensors that detect the human body, non-contact temperature sensors, gas sensors, etc., due to their thermal effect and the effect of infrared absorption by gas. For example, gas sensors can be used for monitoring and protecting the atmospheric environment, and even for early detection of fires, and have been attracting attention in recent years. In particular, in the wavelength range from 2.5 μm to 10.0 μm, there are many absorption bands specific to various gases, making this wavelength range suitable for use in gas sensors.

[0003] The principle of the gas sensor using infrared rays is as follows. For example, when a gas is injected into the space between the infrared light source and the light receiving element, a specific gas absorbs infrared rays of a specific wavelength, so the type and concentration of the gas can be measured by analyzing the wavelength spectrum before and after the gas is injected. Here, an incandescent bulb, for example, is used as the infrared light source, and the infrared rays emitted from the incandescent bulb are white light. Therefore, in order to separate a specific wavelength, a filter must be provided on the light receiving element side. Such filters are expensive and weaken the intensity of the infrared rays, reducing the sensitivity of the gas sensor. Furthermore, the life of an incandescent bulb is short, so the light source must be replaced frequently.

[0004] In order to solve the above problems, it is effective to use a semiconductor light-emitting element (LED: Light Emitting Diode) that emits infrared rays of a specific wavelength as a light source. Analytical equipment using infrared LEDs can be made smaller, lighter, and consume less power than analytical equipment using other light sources (e.g., light bulbs, etc.). Infrared LEDs are an effective light source for portable, space-saving, and low-power analytical equipment.

[0005] However, currently, analytical instruments that use LEDs as light sources, especially in the infrared region, have not yet come into widespread use. One of the reasons for this is that known infrared LEDs do not provide sufficient emission intensity, so the analytical instrument as a whole does not provide sufficient signal strength (S / N ratio). Since the S / N ratio improves as the emission intensity increases, sufficient infrared LED emission intensity must be obtained for widespread application.

[0006] Infrared LEDs have a so-called pn junction diode structure in which an emitting layer having a band gap capable of emitting infrared light with a wavelength of 2 μm or more is sandwiched between an n-layer and a p-layer, and emit infrared light by passing a forward current through the pn junction diode and recombining electrons and holes in the emitting layer. For infrared LEDs, AlInSb is preferably used, which can produce relatively good quality crystals. For example, an infrared LED using AlInSb has a structure as shown in Non-Patent Document 1. However, even with this structure, it is difficult to obtain a sufficiently high emission intensity. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2015-90901 A [Non-patent literature]

[0008] [Non-Patent Document 1] MK Haigh et al., “Mid-Infrared AlxIn1-xSb light-emitting diodes” Applied Physics Letters, 90(23), 23116(2007) Summary of the Invention [Problem to be solved by the invention]

[0009] In order to commercialize infrared light-emitting diodes (LEDs), further improvements in the emission intensity are required.

[0010] The present invention has been made in consideration of the above circumstances, and has an object to provide an infrared light emitting device having high emission intensity. [Means for solving the problem]

[0011] The infrared light emitting device of the present invention comprises a semiconductor substrate, a first layer formed on the semiconductor substrate and having a first conductivity type, a light emitting layer formed on the first layer, and a second layer formed on the light emitting layer and having a second conductivity type, the first layer being made of Al x(1) In 1-x(1) The layer containing Sb and the layer with a thickness of t y(1) [nm] and Al y(1) In 1-y(1) Sb-containing layer and Al x(2) In 1-x(2) A layer containing Sb, y(1) , the x(1), the x(2) and the y(1) are 0 <t y(1) ≦2360×(y(1)-x(1))-240 (0.11≦y(1)-x(1)≦0.19), 0 <t y(1) ≦-1215×(y(1)-x(1))+427 (0.19 <y(1)-x(1)≦0.33)、 0 <t y(1) ≦2360×(y(1)-x(2))-240 (0.11≦y(1)-x(2)≦0.19), 0 <t y(1) ≦-1215×(y(1)-x(2))+427 (0.19 <y(1)-x(2)≦0.33)、 0 <x(1)<0.18、および、 0 <x(2)<0.18 It satisfies the following.

[0012] The present invention also provides an infrared light emitting device comprising: a semiconductor substrate; a first layer formed on the semiconductor substrate and having a first conductivity type; a light emitting layer formed on the first layer; and a second layer formed on the light emitting layer and having a second conductivity type, the first layer being made of Al x(1) Ga p(1) In 1-x(1)-p(1) The layer containing Sb and the layer with a thickness of t y(1) [nm] and Al y(1) Ga q(1) In 1-y(1)-q(1) Sb-containing layer and Al x(2) Ga p(2) In 1-x(2)-p(2) A layer containing Sb, y(1) , the x(1), the x(2), the y(1), the p(1), the p(2), and the q(1) are 0 <t y(1) ≦2360×(y(1)+q(1)-x(1)-p(1))-240 (0.11≦y(1)+q(1)-x(1)-p(1)≦0.19), 0 <t y(1) ≦-1215×(y(1)+q(1)-x(1)-p(1))+427 (0.19 <y(1)+q(1)-x(1)-p(1)≦0.33)、 0 <t y(1) ≦2360×(y(1)+q(1)-x(2)-p(2))-240 (0.11≦y(1)+q(1)-x(2)-p(2)≦0.19), 0 <t y(1) ≦-1215×(y(1)+q(1)-x(2)-p(2))+427 (0.19 <y(1)+q(1)-x(2)-p(2)≦0.33)、 0 <x(1)+p(1)<0.18、 0 <x(2)+p(2)<0.18、および 0 <q(1) / (y(1)+q(1))≦1 It satisfies the following. Effect of the Invention

[0013] According to the present invention, it is possible to provide an infrared light emitting element with high emission intensity. [Brief description of the drawings]

[0014] [Figure 1] FIG. 13 is a diagram showing the relationship between composition difference and film thickness. [Diagram 2] 1 is a cross-sectional view showing a configuration of an infrared light emitting element according to a first embodiment. [Diagram 3] FIG. 4 is a cross-sectional view showing a configuration of an infrared light-emitting element according to a second embodiment. [Figure 4] FIG. 11 is a cross-sectional view showing a configuration of an infrared light-emitting element according to a third embodiment. [Diagram 5] FIG. 1 is a correlation diagram between Al composition and critical film thickness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] In the following detailed description, many specific configurations are described to provide a complete understanding of the embodiments of the present invention. However, it is clear that other embodiments can be implemented without being limited to such specific configurations. In addition, the following embodiments do not limit the invention according to the claims, and include all combinations of the characteristic configurations described in the embodiments.

[0016] <Infrared light emitting element> The infrared light emitting device according to this embodiment includes a semiconductor substrate, a first layer formed on the semiconductor substrate and having a first conductivity type, a light emitting layer formed on the first layer, and a second layer formed on the light emitting layer and having a second conductivity type. The first layer is made of Al x(1) In 1-x(1) The layer containing Sb and the layer with a thickness of t y(1) [nm] and Al y(1) In 1-y(1) Sb-containing layer and Al x(2) In 1-x(2) A layer containing Sb, in this order, and t y(1) , x(1), x(2) and y(1) are 0 <t y(1) ≦2360×(y(1)-x(1))-240 (0.11≦y(1)-x(1)≦0.19), 0 <t y(1)≦-1215×(y(1)-x(1))+427 (0.19 <y(1)-x(1)≦0.33)、 0 <t y(1) ≦2360×(y(1)-x(2))-240 (0.11≦y(1)-x(2)≦0.19), 0 <t y(1) ≦-1215×(y(1)-x(2))+427 (0.19 <y(1)-x(2)≦0.33)、 0 <x(1)<0.18、および、 0 <x(2)<0.18 It satisfies the following.

[0017] One of the reasons why infrared light emitting devices cannot obtain sufficient emission intensity is that the density of defects in the light emitting layer is high, causing electrons and holes to be deactivated through non-radiative recombination.

[0018] The main defects contained in the light-emitting layer are line defects, or dislocations, that occur due to the difference in lattice constant between the semiconductor substrate and the compound semiconductor material laminated on the substrate. It is known that the thicker the compound semiconductor material laminated here, the lower the dislocation density. This is mainly because dislocations collide with each other and disappear. However, making the film thicker is undesirable because it increases the film formation time and increases the difficulty of the device formation process.

[0019] As an effective method for reducing the defect density, a dislocation filter layer (for example, in the first embodiment, the thickness is t y(1) And Al y(1) In 1-y(1)Examples of effective methods include the introduction of a layer containing Sb. A dislocation filter layer is a thin layer with a lattice constant significantly different from that of the base material that is introduced into the base material in order to reduce the density of line defects, i.e. dislocations. Misfit stress caused by the difference in lattice constant between the base material and the dislocation filter layer is concentrated in the thin dislocation filter layer, causing the dislocations to bend laterally. Multiple bent dislocations collide with each other and disappear, suppressing the propagation of dislocations to upper layers. Dislocation filter layers are preferred because they can reduce dislocations despite their comparatively thin thickness, and there is a comparatively small increase in the film formation time and difficulty of the device formation process.

[0020] Important design elements for the dislocation filter layer are the lattice constant difference with the base material, the thickness of the dislocation filter layer, and elastic constants such as Poisson's ratio. The greater the lattice constant difference with the base material and the thicker the dislocation filter layer, the greater the misfit stress, making it easier for dislocations to bend. However, if the misfit stress becomes greater than a certain level, the crystal cannot withstand the stress and dislocations will be generated instead. The thickness at this time is called the critical film thickness. Although there is a theoretical formula for the critical film thickness, there have been reported cases where dislocations were reduced without generating new dislocations even in the case of a film thickness thicker than the theoretical value (Patent Document 1), and the thickness required for dislocation bending and the thickness at which dislocations are generated depend greatly on the material system. Therefore, in reality, consideration based on experiments, etc. is required. At this time, if new dislocations are not generated in a study under certain conditions, it is common to consider making the dislocation filter layer thicker in the next study. This is because, as described above, the thicker the dislocation filter layer, the easier it is for dislocations to bend.

[0021] As the material for the infrared light emitting device, it is possible to use InSb, AlInSb, InGaSb, InAsSb, etc., which can provide crystals of relatively good quality. For example, when introducing a dislocation filter layer into a base material made of AlInSb, it is preferable to introduce a dislocation filter layer containing AlInSb, which is the same element type, from the viewpoint of easiness of the device formation process.

[0022] Also, Ga can be used instead of Al, and GaInSb and AlGaInSb can be preferably used as the base material and the dislocation filter layer. Since the lattice constants and elastic constants of the binary crystals AlSb and GaSb are close to each other, the lattice constants and elastic constants of the AlInSb mixed crystal and GaInSb mixed crystal, which are mixed crystals of these and InSb, are also close to each other when the Al composition and Ga composition are the same. Therefore, by replacing the value of the "Al composition" of AlInSb with the "Ga composition" in GaInSb or the "sum of the Al composition and Ga composition" in AlGaInSb, it is possible to design a layer whose lattice constant and elastic constant are very close to that of the desired AlInSb.

[0023] When both the base material and the dislocation filter layer are AlInSb, by introducing an AlInSb layer having a different Al composition from that of the base material AlInSb layer as the dislocation filter layer, a lattice constant difference and misfit stress are generated, making it possible to bend dislocations.

[0024] In this specification, the "Al composition" of each layer refers to the ratio of the number of Al elements to all group III elements contained in the layer. Similarly, the "Ga composition" and "In composition" of each layer refer to the ratio of the number of Ga elements and In elements to all group III elements contained in the layer.

[0025] In the infrared light emitting device of this embodiment, dislocations, i.e., line defects, are bent laterally in the first layer, thereby reducing the line defect density in the active layer located above the first layer, and non-radiative recombination via dislocations in the active layer is suppressed, thereby enabling the emission intensity to be improved.

[0026] In addition, the term "on" in the expression "a first layer formed on a semiconductor substrate and having a first conductivity type" means that the first layer is formed on the semiconductor substrate, but also includes the case where another layer exists between the semiconductor substrate and the first layer. The same meaning is also applicable when the term "on" is used to express the relationship between other layers.

[0027] Also here, "Al x(1) In 1-x(1) The word "containing" in the expression "layer containing Sb" means that the layer mainly contains Al, In, and Sb, but this expression also includes cases where other elements are contained. Specifically, this expression naturally also includes cases where the composition of this layer is slightly changed by adding small amounts of other elements (for example, elements such as As, P, Ga, N, etc., a few percent or less). The same meaning is intended when the word "containing" is used to describe the composition of other layers.

[0028] Hereinafter, each component of the infrared light emitting device according to this embodiment will be described with reference to an example.

[0029] <Semiconductor substrate> The semiconductor substrate in the infrared light emitting device according to this embodiment is not particularly limited as long as the first layer described below can be laminated on the semiconductor substrate. Examples of the semiconductor substrate include, but are not limited to, GaAs substrates, Si substrates, InP substrates, and InSb substrates. From the viewpoint of easy crystal growth of compound semiconductors, GaAs substrates are preferred.

[0030] There are no restrictions on doping the semiconductor substrate with donor impurities or acceptor impurities, but from the viewpoint of enabling a plurality of independent infrared light-emitting elements formed on the conductive substrate to be connected in series or in parallel, it is desirable for the semiconductor substrate to be semi-insulating or capable of being insulated and separated from the compound semiconductor layer.

[0031] In addition, the semiconductor substrate is preferably a single crystal substrate from the viewpoint of laminating compound semiconductor single crystals. The surface orientation of the semiconductor substrate is not particularly limited, but (001), (111), (101), etc. are preferable. It is also preferable to use a surface orientation tilted by about 1° to 5° from these surface orientations.

[0032] The surface of the semiconductor substrate may be heated in a vacuum to remove any oxide film, or may be subjected to a cleaning treatment using an acid or alkali after removing contaminants such as organic matter and metals.

[0033] <First layer> The first layer in the infrared light-emitting element according to this embodiment is formed on a semiconductor substrate and has a first conductivity type (either n-type or p-type). Further, the first layer has a layer containing Al x(1) In 1-x(1) Sb (0 < x(1) < 1), a layer with a film thickness of t y(1) and Al y(1) In 1-y(1) Sb (0 < y(1) < 1), and a layer containing Al x(2) In 1-x(2) Sb (0 < x(2) < 1) in this order, 0 < t y(1) ≤ 2360×(y(1) - x(1)) - 240 (0.11 ≤ y(1) - x(1) ≤ 0.19), 0 < t y(1) ≤ -1215×(y(1) - x(1)) + 427 (0.19 < y(1) - x(1) ≤ 0.33), 0 < t y(1) ≤ 2360×(y(1) - x(2)) - 240 (0.11 ≤ y(1) - x(2) ≤ 0.19), 0 < t y(1) ≤ -1215×(y(1) - x(2)) + 427 (0.19 < y(1) - x(2) ≤ 0.33) satisfies the above conditions.

[0034] (Measurement method of Al composition of each layer) The Al composition of each layer of the first layer was determined as follows by secondary ion mass spectrometry (SIMS). A magnetic field type SIMS device IMS 7f manufactured by CAMECA was used for the measurement. This method is a method of performing composition analysis by irradiating a beam-shaped primary ion species on the solid surface, detecting the secondary ions generated simultaneously while digging in the depth direction by the sputtering phenomenon. Here, the Al composition refers to the ratio of the Al element to all group 13 elements contained in each layer.

[0035] Specifically, the primary ion species was cesium ion (Cs+), the primary ion energy was 2.5 keV, the beam incidence angle was 67.2°, and MCs+ (where M is Al, Ga, In, As, Sb, etc.), which has a small matrix effect, was detected as the secondary ion species.

[0036] In this case, sputtering was performed under the above-mentioned constant conditions, and the composition of the target layer was analyzed by continuing sputtering for a specified time until the target layer depth was reached. The target layer depth can be determined from the thickness of each layer by cross-sectional TEM measurement, which will be described later. The conversion of sputtering time to depth in SIMS analysis was performed by measuring the sputtering depth for a certain period of time under the same conditions as the analysis, for example using a stylus-type step gauge, to determine the sputtering rate, and then using this to convert the sputtering time during sample measurement into depth.

[0037] The Al composition was calculated from the signal intensity of MCs+ in each layer. For example, in the case of an AlInSb layer, the Al composition was calculated by (signal intensity of AlCs+)÷((signal intensity of AlCs+)+(signal intensity of InCs+)).

[0038] Even if each layer has a uniform composition in the depth direction, the signal intensity may be distributed in the depth direction due to the influence of sputtering. In this case, the maximum signal intensity is taken as the representative value of the signal intensity of each layer.

[0039] The quantitative value of the Al composition obtained by the analysis may deviate from the true value. In order to correct this deviation from the true value, a separate sample was prepared by determining the lattice constant value obtained by X-ray diffraction (XRD) and used as a standard sample with a known Al composition value. SIMS analysis was performed using the measurement conditions for the Al composition of each layer in the first layer to determine the sensitivity coefficient of the Al composition to the signal intensity. The Al composition of each layer in the first layer was determined by multiplying the SIMS signal intensity in each layer in the first layer by the above sensitivity coefficient.

[0040] Here, another sample is an Al layer with a thickness of 800 nm laminated on a GaAs substrate.x In 1-x Sb was used. For this sample, the lattice constant was determined as follows by X-ray diffraction (XRD) method using an X-ray diffractometer X’Pert MPD manufactured by Spectris Co., Ltd., and the Al composition x as a standard sample was determined.

[0041] By performing a 2θ-ω scan by X-ray diffraction, from the peak position in the 2θ-ω scan of the plane index of the plane corresponding to the plane orientation of the substrate surface, Al x In 1-x the lattice constant in the normal direction to the substrate surface of the layer containing Sb was determined, and the Al composition x was determined using Vegard's law from the lattice constant in the normal direction. Here, it was assumed that there was no anisotropic strain in the Al x In 1-x Sb layer. Specifically, Vegard's law is expressed by the following formula (1).

[0042]

Equation

[0043] Here, a AlSb is the lattice constant of AlSb, a InSb is the lattice constant of InSb, and a AlInSb is the lattice constant of Al x In 1-x Sb obtained by the above X-ray diffraction. 6.1355 Å was used for a AlSb , and 6.4794 Å was used for a InSb . As a standard sample for SIMS measurement, those with 0.10 < x < 0.15 were used.

[0044] Regarding the composition of elements other than Al in each layer of the first layer, it can be measured by using the same method as above.

[0045] For example, regarding the Ga composition when Ga is included, it can be measured by using the same method as above.

[0046] At this time, as a separate sample, Ga with a film thickness of 800 nm laminated on a GaAs substrateg Use 1-g Sb. For Ga g Use 1-g Sb, Vegard's law is specifically expressed by the following formula (2).

[0047] [Number]

[0048] Here, a GaSb is the lattice constant of GaSb, a InSb is the lattice constant of InSb, and a GaInSb is the lattice constant of Al g In 1-g Sb obtained by the above X-ray diffraction. For a GaSb , 6.0959 Å was used, and for a InSb , 6.4794 Å was used. As the standard sample for SIMS measurement, those with 0.10 < g < 0.15 were used.

[0049] (Measurement method for the film thickness of each layer) The film thickness of each layer of the first layer can be measured by the cross-sectional TEM (TEM: Transmission Electron Spectroscopy) method. Specifically, a sample with a thickness of approximately 500 nm or less was prepared by the FIB method using a FIB device (FB-2100) manufactured by Hitachi High-Technologies Corporation, and cross-sectional observation was performed in a transmission image at an acceleration voltage of 200 kV using a Hitachi STEM device (HD-2300A) to measure the thickness of each layer. The film thickness of the layers other than the first layer can also be measured by using the same measurement method.

[0050] From the viewpoint of introducing the stress necessary for the bending of line defects, the lower limit of the film thickness t y(1) of the layer containing Al 1-y(1) In y(1) [nm] is preferably 2 nm or more, and more preferably 5 nm or more.

[0051] In view of the fact that in mixed crystals with more than a ternary system, crystals of better quality can be obtained as the mixed crystal ratio is smaller, from the viewpoint of obtaining crystals of relatively good quality and from the viewpoint of the ease of the element formation process, 0 < x(1) < 0.25 is preferable, and 0 < x(1) < 0.18 is more preferable. More preferably, 0 < x(1) < 0.09 is desirable, and the same range is preferable for x(2).

[0052] Also, the first layer may contain As as a Group V element. However, since it is necessary to irradiate an excessive amount of As element during crystal growth, which inhibits the diffusion of surface atoms during crystal growth and leads to deterioration of crystallinity, the ratio of As atoms to all Group V elements is preferably 3% or less.

[0053] Also, Al y(1) In 1-y(1) From the viewpoint of uniformly applying stress to the layer containing Sb, |x(1) - x(2)| < 0.10 is preferable, and |x(1) - x(2)| < 0.03 is more preferable.

[0054] Also, Al x(1) In 1-x(1) Regarding the film thickness t of the layer containing Sb x(1) From the viewpoint of absorbing misfit stress, t x(1) ≧200 nm is preferable, and t x(1) ≧300 nm is more preferable. For the film thickness t of the layer containing Al x(2) In 1-x(2) Sb, the same range is preferable. x(2)

[0055] Also, from the viewpoint of increasing the film formation time and the ease of the element formation process, t x(1) ≦700 nm is preferable, and more preferably t x(1) ≦600 nm is particularly preferable. The same range is preferable for t x(2)

[0056] As described above, the thicker the dislocation filter layer Al y(1) In 1-y(1) Sb becomes, and also the thicker the dislocation filter layer Al y(1)In 1-y(1) Sb and Al in the base layer x(1) In 1-x(1) The greater the difference in lattice constant with Sb, the easier it is for dislocations to bend. However, the dislocation filter layer Al is used in infrared light emitting devices. y(1) In 1-y(1) It is not preferable for Sb to be thick, because this leads to an increase in the deposition time and an increase in the difficulty of the infrared light emitting device formation process. From the above viewpoints, it is preferable for the dislocation filter layer used in the infrared light emitting device to have a large difference in lattice constant with the base material and a thin film thickness.

[0057] For example, film thickness t y(1) [nm] is preferably 200 nm or less, and more preferably 100 nm or less. y(1) [nm] The thickness is preferably 6 times or less, and more preferably 4 times or less, of the critical film thickness (FIG. 5 described later).

[0058] Here, the critical thickness is a function of y(1)-x(1) and is given by the following formulas (3) to (5). A method for determining the critical thickness hc will be described below.

[0059] Equation (3) shows the Matthews equation regarding the critical film thickness of the intermediate layer in a double heterostructure (Patent Document 1).

[0060] In formula (3), hc is the Al corresponding to the intermediate layer. y(1) In 1-y(1) is the critical thickness of Sb, f is the degree of lattice mismatch, ν is the Poisson's ratio, b is the magnitude of the Burgers vector, α is the angle between the direction of the dislocation line and the Burgers vector, and λ is the angle between the interface between the dislocation filter layer and the buffer layer and the slip plane.

[0061] These parameters vary depending on the type of dislocation being considered, but here we consider a 60° dislocation that is common in zinc blende structures containing AlInSb, and use b=a / √2, cosα=1 / 2, and cosλ=1 / 2. Substituting these into equation (3) and rearranging, we obtain equation (4). The Poisson's ratio used is 0.35. The lattice constant a is the Al y(1) In 1-y(1) The lattice constant of Sb was used.

[0062] Al equivalent to the dislocation filter layer y(1) In 1-y(1) Sb composition y(1), Al corresponding to the buffer layer x(1) In 1-x(1) Using the Sb composition x(1), the lattice constant of each layer can be calculated using Vegard's law (equation (1)), and the lattice mismatch f can be calculated (equation (5)). These equations allow the critical thickness hc to be calculated. The relationship between the Al composition difference and the critical thickness hc at this time is shown in Figure 5.

[0063]

number

[0064]

number

[0065]

number

[0066] As will be shown in the examples below, t y(1) , x(1), x(2) and y(1) are 0 <t y(1) ≦6901×(y(1)-x(1))-1087 (0.16≦y(1)-x(1)≦0.19), 0 <t y(1) ≦-2673×(y(1)-x(1))+699 (0.19 <y(1)-x(1)≦0.25)、 0 <ty(1) ≦6901×(y(1)-x(2))-1087 (0.16≦y(1)-x(2)≦0.19), and 0 < t y(1) ≦-2673×(y(1)-x(2))+699 (0.19 < y(1)-x(2)≦0.25) preferably satisfies more preferably 0 < t y(1) ≦1993×(y(1)-x(1))-242 (0.13≦y(1)-x(1)≦0.19), 0 < t y(1) ≦-1040×(y(1)-x(1))+324 (0.19 < y(1)-x(1)≦0.29), 0 < t y(1) ≦1993×(y(1)-x(2))-242 (0.13≦y(1)-x(2)≦0.19), and 0 < t y(1) ≦-1040×(y(1)-x(2))+324 (0.19 < y(1)-x(2)≦0.29) preferably satisfies even more preferably 0 < t y(1) ≦3067×(y(1)-x(1))-472 (0.16≦y(1)-x(1)≦0.19), 0 < t y(1) ≦-1188×(y(1)-x(1))+322 (0.19 < y(1)-x(1)≦0.25), 0 < t y(1) ≦3067×(y(1)-x(2))-472 (0.16≦y(1)-x(2)≦0.19), and 0 < t y(1) ≦-1188×(y(1)-x(2))+322 (0.19 < y(1)-x(2)≦0.25) more preferably satisfies.

[0067] Also, the first layer is a layer containing Al x(i) In 1-x(i) Sb(0 < x(i) < 1), and the film thickness is t y(i) [nm] and is Al y(i) In 1-y(i)It is preferable to have a stacked structure in which layers containing Sb (0 < y(i) < 1) are sequentially stacked n layers at a time in this order.

[0068] Here, regarding the number of repetitions n, from the viewpoint of reducing the line defect density, it is preferably n ≥ 2, and more preferably n ≥ 3.

[0069] Also, from the viewpoints of increasing the film formation time and the ease of the device formation process, it is preferably n ≤ 6, and more preferably n ≤ 5.

[0070] Also, as shown in the examples described later, the first layer is, for an integer i from 1 to n (2 ≤ n ≤ 6), a layer containing Al x(i) In 1-x(i) Sb, and a layer containing Al y(i) [nm] and having a stacked structure in which layers containing Al y(i) In 1-y(i) Sb are sequentially stacked n layers at a time in this order, and a layer containing Al y(n) [nm] and a layer containing Al y(n) In 1-y(n) Sb directly above the layer containing Al x(n+1) In 1-x(n+1) Sb, and t y(i) , x(i), x(i + 1) and y(i) are 0 < t y(i) ≤ 2360×(y(i) - x(i)) - 240 (0.11 ≤ y(i) - x(i) ≤ 0.19), 0 < t y(i) ≤ -1215×(y(i) - x(i)) + 427 (0.19 < y(i) - x(i) ≤ 0.33), 0 < t y(i) ≤ 2360×(y(i) - x(i + 1)) - 240 (0.11 ≤ y(i) - x(i + 1) ≤ 0.19), 0 < t y(i) ≤ -1215×(y(i) - x(i + 1)) + 427 (0.19 < y(i) - x(i + 1) ≤ 0.33), 0 < x(i) < 0.18, and 0 < x(i + 1) < 0.18 It is preferable to satisfy.

[0071] where t y(i) Regarding t y(1) As for x(i) and x(i+1), the same range as that of the above-mentioned x(1) is preferable.

[0072] As shown in the examples below, the t y(i) , x(i), x(i+1) and y(i) are 0 <t y(i) ≦6901×(y(i)-x(i))-1087 (0.16≦y(i)-x(i)≦0.19), 0 <t y(i) ≦-2673×(y(i)-x(i))+699 (0.19 <y(i)-x(i)≦0.25)、 0 <t y(i) ≦6901×(y(i)-x(i+1))-1087 (0.16≦y(i)-x(i+1)≦0.19), and 0 <t y(i) ≦-2673×(y(i)-x(i+1))+699 (0.19 <y(i)-x(i+1)≦0.25) It is preferable that More preferably, 0 <t y(i) ≦1993×(y(i)-x(i))-242 (0.13≦y(i)-x(i)≦0.19), 0 <t y(i) ≦-1040×(y(i)-x(i))+324 (0.19 <y(i)-x(i)≦0.29)、 0 <t y(i) ≦1993×(y(i)-x(i+1))-242 (0.13≦y(i)-x(i+1)≦0.19), and 0 <t y(i) ≦-1040×(y(i)-x(i+1))+324 (0.19 <y(i)-x(i+1)≦0.29) It is more preferable that More preferably 0 <t y(i) ≦3067×(y(i)-x(i))-472 (0.16≦y(i)-x(i)≦0.19), 0 <t y(i)≦-1188×(y(i)-x(i))+322 (0.19 <y(i)-x(i)≦0.25)、 0 <t y(i) ≦3067×(y(i)-x(i+1))-472 (0.16≦y(i)-x(i+1)≦0.19), and 0 <t y(i) ≦-1188×(y(i)-x(i+1))+322 (0.19 <y(i)-x(i+1)≦0.25) In this case, it is more preferable that the Al of the different layers is satisfied. y(i) In 1-y(i) For Sb, the value of the Al composition y(i) can be the same or different.

[0073] The material for the first layer is the above-mentioned Al. x(1) In 1-x(1) The layer containing Sb and the layer with a thickness of t y(1) And Al y(1) In 1-y(1) Sb-containing layer and Al x(2) In 1-x(2) In addition to the laminated structure having a layer containing Sb and a layer containing Sb in this order, a single layer or laminated structure of a single crystal or a mixed crystal of AlAs, GaAs, InAs, AlSb, GaSb, InSb, or InP may be used.

[0074] Furthermore, when the aforementioned semiconductor substrate is a GaAs substrate, the layer in the first layer that is in contact with the GaAs substrate is preferably a layer made of InSb in order to ensure good crystallinity.

[0075] The first layer is preferably doped with a donor impurity or an acceptor impurity to be n-type or p-type, but does not necessarily have to be doped as long as it has the first conductivity type. If the first layer is doped, the doping concentration is preferably 1×10 18 [cm -3 ] or more is preferable, and from the viewpoint of ensuring crystallinity, it is preferably 1×10 19 [cm -3 ] or less.

[0076] The first conductivity type is preferably an n-type conductivity type from the viewpoint of current diffusion in the infrared light emitting element and from the viewpoint of improving infrared transmittance due to the Burstein-Moss effect.

[0077] When the first layer and the light-emitting layer are in direct contact with each other, from the viewpoint of improving the carrier confinement effect in the light-emitting layer, it is preferable that the material of the first layer in contact with the light-emitting layer has a larger band gap than that of the light-emitting layer.

[0078] <Light-emitting layer> The light-emitting layer in the infrared light-emitting device according to this embodiment is a layer formed on the first layer. The material of the light-emitting layer is not particularly limited as long as it is a compound semiconductor having a band gap corresponding to infrared rays having a wavelength of 2 μm or more. For example, a single layer of a single crystal or a mixed crystal of AlAs, GaAs, InAs, AlSb, GaSb, InSb, or InP, or a laminate structure thereof may be used.

[0079] In particular, from the viewpoint of obtaining crystals of relatively good quality, Al is used as the material for the light-emitting layer. z In 1-z Sb is preferable. In this case, the Al composition z is preferably smaller than 0.25, more preferably smaller than 0.18, from the viewpoint of ensuring good crystallinity. It is further preferable that it is smaller than 0.09. Also, from the viewpoint of increasing the band gap and improving the energy per unit photon, it is preferably larger than 0.01, more preferably larger than 0.02. Also, from the viewpoint of obtaining good quality crystals, the Al composition z of the first layer is preferably larger than 0.01, more preferably larger than 0.02. x(1) In 1-x(1) It is preferable that the lattice constant is close to that of the layer containing Sb.

[0080] The conductivity type of the light-emitting layer may be either n-type or p-type. The light-emitting layer may be non-doped (doped with no impurities) or may be doped with a donor impurity or an acceptor impurity to be n-type or p-type.

[0081] In order to suppress non-radiative recombination due to defects, the linear defect density in the light-emitting layer must be 3.0×10 8 [book / cm2 The line defect density of the light-emitting layer can be measured by observing it with a planar TEM. Specifically, a sample is prepared by processing it with a FIB method using a Hitachi FIB device (FB-2100), and a planar TEM image is observed using a Hitachi STEM device (HD-2300A). 2 The number of line defects in a continuous field of view having the above area is counted, and the number of line defects per unit area is calculated, thereby making it possible to calculate the line defect density.

[0082] From the viewpoint of preventing the overflow of electrons and holes when a voltage is applied, the lower limit of the thickness [nm] of the light-emitting layer is preferably 10 nm or more, and more preferably 20 nm or more. From the viewpoint of increasing the film formation time and facilitating the device formation process, the upper limit of the thickness of the light-emitting layer is preferably 4000 nm or less, and more preferably 3000 nm or less.

[0083] <2nd layer> The second layer in the infrared light emitting device according to this embodiment is formed on the light emitting layer and is a layer having a second conductivity type (either n-type or p-type).

[0084] The second layer is preferably of a conductivity type opposite to the first conductivity type of the first layer, for example, if the first layer is n-type, the second layer is preferably p-type, and vice versa.

[0085] As described above, the first layer is preferably n-type, and therefore the second layer is preferably p-type.

[0086] The second layer is preferably doped with a donor impurity or an acceptor impurity to be n-type or p-type, but does not necessarily have to be doped as long as it has the second conductivity type.

[0087] If the second layer is doped, the doping concentration should be less than 1×10 18 [cm -3] or more is preferable, and from the viewpoint of ensuring crystallinity, it is preferably 1×10 19 [cm -3 ] or less.

[0088] The material for the second layer is not particularly limited as long as it is a compound semiconductor, and examples thereof include a single layer or a multilayer structure of a single crystal or a mixed crystal of AlAs, GaAs, InAs, AlSb, GaSb, InSb, or InP.

[0089] When the second layer and the light-emitting layer are in direct contact with each other, from the viewpoint of improving the carrier confinement effect in the light-emitting layer, it is preferable that the material of the second layer in contact with the light-emitting layer has a larger band gap than that of the light-emitting layer.

[0090] In the embodiment of the present invention, each compound semiconductor layer (first layer, light emitting layer, second layer, etc.) can be formed using various film formation methods. For example, molecular beam epitaxy (MBE) method and metalorganic vapor phase epitaxy (MOVPE) method are preferable. Each compound semiconductor layer can be formed on a semiconductor substrate using these methods. In the process of forming each compound semiconductor layer, the semiconductor substrate may be temporarily removed from the film formation device into the atmosphere during the formation of each layer constituting each compound semiconductor layer.

[0091] From the viewpoint of preventing damage during the device formation process, the lower limit of the thickness [nm] of the second layer is preferably 30 nm or more, and more preferably 50 nm or more. From the viewpoint of increasing the film formation time and facilitating the device formation process, the upper limit of the thickness [nm] of the second layer is preferably 2000 nm or less, and more preferably 1000 nm or less.

[0092] <Laminated structure> In an embodiment of the present invention, the infrared light emitting device has the following layered structure.

[0093] The first layer 20 has a thickness t x(i) And Al x(i) In 1-x(i) A buffer layer X(i) containing Sb and a thickness ty(i) And Al y(i) In 1-y(i) The dislocation filter layer Y(i) containing Sb is laminated in this order in layers of n each, and a layer of thickness t x(n+1) And Al x(n+1) In 1-x(n+1) The term "sequentially laminated" as used herein means that "a Y(i) layer is laminated directly on an X(i) layer, and an X(i+1) layer is laminated directly on an Y(i) layer."

[0094] Here, the Y(i) layer functions as a dislocation filter layer, and the X(i) layer functions as a buffer layer that absorbs misfit stress. By applying misfit stress to the Y(i) layer, dislocations are bent at the interface between the X(i) and Y(i) layers and at the interface between the Y(i) and X(i+1) layers.

[0095] Therefore, the greater the difference in composition between the Y(i) layer and the X(i) and X(i+1) layers, the greater the misfit stress, making it easier for dislocations to bend. On the other hand, if the difference in composition between the Y(i) layer and the X(i) and X(i+1) layers becomes too large, the crystal cannot withstand the excessive misfit stress, and dislocations instead occur.

[0096] Also, the thickness of the Y(i) layer is t y(i) The thicker the Y(i) layer, the greater the misfit stress, making it easier for the dislocation to bend. y(i) If the thickness becomes too thick, the crystal will not be able to withstand the misfit stress and dislocations will occur. y(i) are not independent of each other, and there are suitable ranges as described above.

[0097] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. However, in each of the drawings described below, the same reference numerals are used to designate corresponding parts, and the description of overlapping parts will be omitted as appropriate. In addition, the embodiment of the present invention is an example of a configuration for embodying the technical idea of ​​the present invention, and the material, shape, structure, arrangement, dimensions, etc. of each part are not specified as described below. In addition, the embodiment of the present invention includes all combinations of the characteristic configurations described below. The technical idea of ​​the present invention can be modified in various ways within the technical scope defined by the claims described in the claims.

[0098] 2 is a cross-sectional view showing the configuration of a first embodiment of an infrared light emitting device 100 according to the present invention. The infrared light emitting device 100 has a structure in which a compound semiconductor layer 50 is laminated on a semiconductor substrate 10. The compound semiconductor layer 50 has a structure in which a first layer 20, a light emitting layer 30, and a second layer 40 are laminated in this order. In the first embodiment, the first layer 20 has a thickness t x(1) And Al x(1) In 1-x(1) The first layer 20 has a thickness t y(1) And Al y(1) In 1-y(1) The first layer 20 has a thickness t x(2) And Al x(2) In 1-x(2) The first layer 20 has a buffer layer 25 that is a layer X(2) containing Sb. In the first embodiment, the first layer 20 has a structure in which a buffer layer 23 and a dislocation filter layer 24 are laminated in this order as one layer (one set), and the buffer layer 25 is laminated directly thereon.

[0099] Here, the first layer 20 further includes a buffer layer (InSb layer 21) containing InSb, and a barrier layer 22. As shown in Fig. 2, the first layer 20 has a structure in which a buffer layer 23 is laminated directly on the InSb layer 21. The first layer 20 also has a structure in which a barrier layer 22 is laminated directly on the buffer layer 25.

[0100] Fig. 3 is a cross-sectional view showing a configuration of a second embodiment of the infrared light emitting device 100 according to the present invention. In the second embodiment, the first layer 20 has a structure in which the number of repetitions n of the above-mentioned laminated structure is set to 2. In Fig. 3, the same elements as those in the infrared light emitting device 100 of the first embodiment are denoted by the same reference numerals, and description thereof will be omitted.

[0101] In the second embodiment, the first layer 20 has a thickness t y(2) And Al y(2) In 1-y(2) The first layer 20 has a thickness t x(3) And Al x(3) In 1-x(3) The first layer 20 has a buffer layer 27 which is a layer X(3) containing Sb. The first layer 20 has a structure in which a buffer layer 23 and a dislocation filter layer 24, and a buffer layer 25 and a dislocation filter layer 26 are laminated in this order in two layers (two sets), and the buffer layer 27 is laminated directly thereon. In the second embodiment, the first layer 20 has a structure in which a barrier layer 22 is laminated directly on the buffer layer 27.

[0102] Fig. 4 is a cross-sectional view showing a configuration of a third embodiment of the infrared light emitting device 100 according to the present invention. In the third embodiment, the first layer 20 has a structure in which the number of repetitions n of the above-mentioned laminated structure is set to 3. In Fig. 4, the same elements as those in the infrared light emitting device 100 of the second embodiment are denoted by the same reference numerals, and description thereof will be omitted.

[0103] In the third embodiment, the first layer 20 has a thickness t y(3) And Al y(3) In 1-y(3) The first layer 20 has a thickness t x(4) And Al x(4) In 1-x(4)The first layer 20 has a buffer layer 29 which is a layer X(4) containing Sb. The first layer 20 has a structure in which a buffer layer 23 and a dislocation filter layer 24, a buffer layer 25 and a dislocation filter layer 26, and a buffer layer 27 and a dislocation filter layer 28 are laminated in this order in three layers (three sets), with the buffer layer 29 laminated directly thereon. In the third embodiment, the first layer 20 has a structure in which a barrier layer 22 is laminated directly on the buffer layer 29.

[0104] Although the first, second and third embodiments of the present invention have been described above, the technical scope of the present invention is not limited to the scope described in the above embodiments. For example, the number of repetitions n of the laminated structure is not limited to 2 or 3, and may be selected in the range of 4 to 6. In addition, it is clear to those skilled in the art that various modifications or improvements can be made to the above embodiments. It is clear from the claims that such modifications or improvements can also be included in the technical scope of the present invention.

[0105] Also, even if Ga is used instead of Al, as mentioned above, it is possible to form GaSb, which has a lattice constant close to that of AlSb, and stress can be generated within the layer. As another embodiment of the infrared light emitting device according to the present invention, A semiconductor substrate; a first layer formed on a semiconductor substrate and having a first conductivity type; a light-emitting layer formed on the first layer; a second layer formed on the light emitting layer and having a second conductivity type; The first layer is Al x(1) Ga p(1) In 1-x(1)-p(1) The layer containing Sb and the layer with a thickness of t y(1) [nm] and Al y(1) Ga q(1) In 1-y(1)-q(1) Sb-containing layer and Al x(2) Ga p(2) In 1-x(2)-p(2) a layer containing Sb, t y(1) , x(1), x(2), y(1) p(1), p(2), and q(1) are 0 <t y(1) ≦2360×(y(1)+q(1)-x(1)-p(1))-240 (0.11≦y(1)+q(1)-x(1)-p(1)≦0.19), 0 <t y(1) ≦-1215×(y(1)+q(1)-x(1)-p(1))+427 (0.19 <y(1)+q(1)-x(1)-p(1)≦0.33)、 0 <t y(1) ≦2360×(y(1)+q(1)-x(2)-p(2))-240 (0.11≦y(1)+q(1)-x(2)-p(2)≦0.19), 0 <t y(1) ≦-1215×(y(1)+q(1)-x(2)-p(2))+427 (0.19 <y(1)+q(1)-x(2)-p(2)≦0.33)、 0 <x(1)+p(1)<0.18、 0 <x(2)+p(2)<0.18、および 0<q(1) / (y(1)+q(1))≦1 The present invention can take a form including a layer satisfying the above.

[0106] In the infrared light emitting device according to this embodiment, dislocations, i.e., linear defects, are bent laterally in the first layer, so that the linear defect density in the active layer located above the first layer is reduced. Then, non-radiative recombination via dislocations in the active layer is suppressed, so that the emission intensity can be improved. This effect can be confirmed in Examples 21 and 22 described later, and the emission intensity is similar to that of the embodiment in which the base material and the dislocation filter layer contain AlInSb. Note that the various preferred embodiments described above regarding the embodiment in which the base material and the dislocation filter layer contain AlInSb can also be applied to the infrared light emitting device of this embodiment by replacing "Al composition" with "the sum of the Al composition and the Ga composition." EXAMPLES

[0107] The present invention will be described in detail below based on examples. However, the present invention is not limited to the following examples, and it goes without saying that various modifications can be made without departing from the spirit of the invention.

[0108] <Example 1> For example, as shown in FIG. 3, a semiconductor substrate 10 is grown on a semi-insulating GaAs substrate using an MBE apparatus. Sn = 7 × 10 18 [cm -3 ] doped n-type InSb layer 21 is 0.5 μm, Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.08 In 0.92 The Sb layer is 0.5 μm thick (buffer layer 23). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.27 In 0.73 The Sb layer is 0.02 μm thick (dislocation filter layer 24). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.08 In 0.92 The Sb layer is 0.5 μm thick (buffer layer 25). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.27 In 0.73 The Sb layer is 0.02 μm thick (dislocation filter layer 26). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.08 In 0.92 The Sb layer is 0.5 μm thick (buffer layer 27). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.27 In 0.73 The Sb layer is 0.02 μm thick (barrier layer 22). Non-doped Al 0.08 In 0.92 The Sb layer (light-emitting layer 30) is 1 μm thick. Zn 3×10 18 [cm -3 ] doped p-type l 0.27 In 0.73The Sb layer is 0.02 μm thick (a barrier layer constituting the second layer 40). Zn 3×10 18 [cm -3 ] doped p-type Al 0.08 In 0.92 The Sb layer is 0.5 μm thick (the p layer constituting the second layer 40). were laminated in this order from the semi-insulating GaAs substrate (semiconductor substrate 10 ) side to form a compound semiconductor layer 50 .

[0109] Next, a resist pattern was formed on the compound semiconductor layer 50, and a mesa structure was fabricated by etching. Furthermore, in order to electrically isolate each light-emitting element, insulating grooves made of silicon oxide were formed between the mesa structures, and silicon nitride was formed as an insulating layer on the entire surface of the compound semiconductor layer 50 including the mesa structures and the insulating grooves. A contact hole was formed in a part of this insulating layer, and titanium (Ti), platinum (Pt), and gold (Au) were deposited in this order to cover the contact hole, forming an electrode portion, and a plurality of infrared LED elements connected in series were obtained.

[0110] A measurement sample was prepared from within 0.3 μm of the light-emitting layer 30 close to the p-layer constituting the second layer 40, and line defect density was observed by planar TEM. The line defect density was found to be 1.1×10 8 [book / cm 2 It can be seen that the defect density is reduced compared to the comparative example described later.

[0111] <Examples 2 to 12, 18 to 20> According to Tables 1 and 2, the Al composition y(i) of the dislocation filter layer 24 (Y(1) layer) and the dislocation filter layer 26 (Y(2) layer) were changed.

[0112] <Examples 13 and 14> The Al composition z of the light emitting layer 30 and the Al compositions of the buffer layers 23 (X(1) layer), 25 (X(2) layer), and 27 (X(3) layer) were changed according to Table 2. The Al composition of the barrier layer was set to 0.26.

[0113] <Example 15> The Al composition z of the light emitting layer 30 and the Al compositions of the buffer layers 23 (X(1) layer), 25 (X(2) layer), and 27 (X(3) layer) were changed according to Table 2. The Al composition of the barrier layer was set to 0.33.

[0114] <Example 16> For example, as shown in FIG. 2, a semiconductor substrate 10 is grown on a semi-insulating GaAs substrate using an MBE apparatus. Sn = 7 × 10 18 [cm -3 ] doped n-type InSb layer 21 is 0.5 μm, Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.08 In 0.92 The Sb layer is 0.75 μm thick (buffer layer 23). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.27 In 0.73 The Sb layer is 0.02 μm thick (dislocation filter layer 24). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.08 In 0.92 The Sb layer is 0.75 μm thick (buffer layer 25). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.27 In 0.73 The Sb layer is 0.02 μm thick (barrier layer 22). Non-doped Al 0.08 In 0.92 The Sb layer (light-emitting layer 30) is 1 μm thick. Zn 3×10 18 [cm -3 ] doped p-type l 0.27 In 0.73 The Sb layer is 0.02 μm thick (a barrier layer constituting the second layer 40). Zn 3×10 18 [cm -3 ] doped p-type Al 0.08 In 0.92 The Sb layer is 0.5 μm thick (the p layer constituting the second layer 40). They were laminated in this order from the semi-insulating GaAs substrate (semiconductor substrate 10) side to form a compound semiconductor layer 50.

[0115] At this time, Al x(i) In 1-x(i) The number of repetitions n of the laminated structure of the layer containing Sb (0 < x(i) < 1) and the layer containing Al y(i) [nm] and Al y(i) In 1-y(i) The number of repetitions n of the laminated structure of the layer containing Sb (0 < y(i) < 1) corresponds to 1.

[0116] Next, a resist pattern was formed on the compound semiconductor layer 50, and etching was performed to fabricate a mesa structure. Further, an insulating groove made of silicon oxide was formed between the mesa structures so that each light-emitting element was electrically independent, and silicon nitride was formed as an insulating layer on the entire surface of the compound semiconductor layer 50 including the mesa structure and the insulating groove. A contact hole was formed in a part of this insulating layer, and titanium (Ti), platinum (Pt), and gold (Au) were deposited in this order so as to cover the contact hole to form an electrode portion, and a plurality of infrared LED elements connected in series were obtained.

[0117] <Example 17> For example, as shown in FIG. 4, on a semi-insulating GaAs substrate (semiconductor substrate 10), using an MBE apparatus An n-type InSb layer 21 doped with Sn at 7×10 18 [cm -3 with a thickness of 0.5 μm, and An n-type Al 18 [cm -3 doped with Sn at 7×10 0.08 In 0.92 Sb layer with a thickness of 0.5 μm (buffer layer 23), An n-type Al 18 [cm -3 doped with Sn at 7×10 0.27 In 0.73 Sb layer with a thickness of 0.02 μm (dislocation filter layer 24), An n-type Al 18 [cm -3 doped with Sn at 7×10 0.08 In 0.92The Sb layer is 0.333 μm thick (buffer layer 25). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.27 In 0.73 The Sb layer is 0.02 μm thick (dislocation filter layer 26). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.08 In 0.92 The Sb layer is 0.333 μm thick (buffer layer 27). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.27 In 0.73 The Sb layer is 0.02 μm thick (dislocation filter layer 28). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.08 In 0.92 The Sb layer is 0.333 μm thick (buffer layer 29). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.27 In 0.73 The Sb layer is 0.02 μm thick (barrier layer 22). Non-doped Al 0.08 In 0.92 The Sb layer (light-emitting layer 30) is 1 μm thick. Zn 3×10 18 [cm -3 ] doped p-type l 0.27 In 0.73 The Sb layer is 0.02 μm thick (a barrier layer constituting the second layer 40). Zn 3×10 18 [cm -3 ] doped p-type Al 0.08 In 0.92 The Sb layer is 0.5 μm thick (the p layer constituting the second layer 40). were laminated in this order from the semi-insulating GaAs substrate (semiconductor substrate 10 ) side to form a compound semiconductor layer 50 .

[0118] At this time, Al x(i) In1-x(i) A layer containing Sb(0 < x(i) < 1) and a layer with a thickness of t y(i) [nm] and Al y(i) In 1-y(i) The number of repetitions n of the laminated structure with a layer containing Sb(0 < y(i) < 1) corresponds to 3.

[0119] Next, a resist pattern was formed on the compound semiconductor layer 50 and etched to fabricate a mesa structure. Further, an insulating groove made of silicon oxide was formed between the mesa structures so that each light-emitting element was electrically independent, and silicon nitride was formed as an insulating layer on the entire surface of the compound semiconductor layer 50 including the mesa structure and the insulating groove. A contact hole was formed in a part of this insulating layer, and titanium (Ti), platinum (Pt), and gold (Au) were deposited in this order so as to cover the contact hole to form an electrode portion, and an infrared LED element in which a plurality of elements were connected in series was obtained.

[0120] <Example 21> For example, as shown in FIG. 3, on a semi-insulating GaAs substrate (semiconductor substrate 10), using an MBE apparatus Sn was doped at 7×10 18 [cm -3 to form an n-type InSb layer 21 with a thickness of 0.5 μm, and Sn was doped at 7×10 18 [cm -3 to form an n-type Al 0.08 In 0.92 Sb layer with a thickness of 0.5 μm (buffer layer 23), Sn was doped at 7×10 18 [cm -3 to form an n-type Ga 0.27 In 0.73 Sb layer with a thickness of 0.02 μm (dislocation filter layer 24), Sn was doped at 7×10 18 [cm -3 to form an n-type Al 0.08 In 0.92 Sb layer with a thickness of 0.5 μm (buffer layer 25), Sn was doped at 7×10 18 [cm -3 to form an n-type Ga 0.27 In 0.73The Sb layer is 0.02 μm thick (dislocation filter layer 26). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.08 In 0.92 The Sb layer is 0.5 μm thick (buffer layer 27). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.27 In 0.73 The Sb layer is 0.02 μm thick (barrier layer 22). Non-doped Al 0.08 In 0.92 The Sb layer (light-emitting layer 30) is 1 μm thick. Zn 3×10 18 [cm -3 ] doped p-type l 0.27 In 0.73 The Sb layer is 0.02 μm thick (a barrier layer constituting the second layer 40). Zn 3×10 18 [cm -3 ] doped p-type Al 0.08 In 0.92 The Sb layer is 0.5 μm thick (the p layer constituting the second layer 40). were laminated in this order from the semi-insulating GaAs substrate (semiconductor substrate 10 ) side to form a compound semiconductor layer 50 .

[0121] Next, a resist pattern was formed on the compound semiconductor layer 50, and a mesa structure was fabricated by etching. Furthermore, in order to electrically isolate each light-emitting element, insulating grooves made of silicon oxide were formed between the mesa structures, and silicon nitride was formed as an insulating layer on the entire surface of the compound semiconductor layer 50 including the mesa structures and the insulating grooves. A contact hole was formed in a part of this insulating layer, and titanium (Ti), platinum (Pt), and gold (Au) were deposited in this order to cover the contact hole, forming an electrode portion, and a plurality of infrared LED elements connected in series were obtained.

[0122] <Example 22> For example, as shown in FIG. 3, a semiconductor substrate 10 is grown on a semi-insulating GaAs substrate using an MBE apparatus. Sn = 7 × 1018 [cm -3 ] doped n-type InSb layer 21 is 0.5 μm, Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.08 In 0.92 The Sb layer is 0.5 μm thick (buffer layer 23). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.13 Ga 0.14 In 0.73 The Sb layer is 0.02 μm thick (dislocation filter layer 24). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.08 In 0.92 The Sb layer is 0.5 μm thick (buffer layer 25). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.13 Ga 0.14 In 0.73 The Sb layer is 0.02 μm thick (dislocation filter layer 26). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.08 In 0.92 The Sb layer is 0.5 μm thick (buffer layer 27). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.27 In 0.73 The Sb layer is 0.02 μm thick (barrier layer 22). Non-doped Al 0.08 In 0.92 The Sb layer (light-emitting layer 30) is 1 μm thick. Zn 3×10 18 [cm -3 ] doped p-type l 0.27 In 0.73 The Sb layer is 0.02 μm thick (a barrier layer constituting the second layer 40). Zn 3×10 18 [cm -3 ] doped p-type Al 0.08 In0.92 The Sb layer is 0.5 μm thick (the p layer constituting the second layer 40). were laminated in this order from the semi-insulating GaAs substrate (semiconductor substrate 10 ) side to form a compound semiconductor layer 50 .

[0123] Next, a resist pattern was formed on the compound semiconductor layer 50, and a mesa structure was fabricated by etching. Furthermore, in order to electrically isolate each light-emitting element, insulating grooves made of silicon oxide were formed between the mesa structures, and silicon nitride was formed as an insulating layer on the entire surface of the compound semiconductor layer 50 including the mesa structures and the insulating grooves. A contact hole was formed in a part of this insulating layer, and titanium (Ti), platinum (Pt), and gold (Au) were deposited in this order to cover the contact hole, forming an electrode portion, and a plurality of infrared LED elements connected in series were obtained.

[0124] [Table 1]

[0125] [Table 2]

[0126] <Comparative Example 1> The comparative example has a double barrier structure. Sn = 7 × 10 18 [cm -3 ] doped n-type InSb layer 21 is 0.5 μm, Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.08 In 0.92 The Sb layer is 0.5 μm thick (corresponding to buffer layer 23). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.27 In 0.73 The Sb layer is 0.02 μm (equivalent to barrier layer 22), Non-doped Al 0.08 In 0.92Sb layer (equivalent to light-emitting layer 30) is 2 μm, Zn 3×10 18 [cm -3 ] doped p-type l 0.27 In 0.73 The Sb layer is 0.02 μm thick (corresponding to the barrier layer constituting the second layer 40). Zn 3×10 18 [cm -3 ] doped p-type Al 0.08 In 0.92 The Sb layer is 0.5 μm thick (corresponding to the p layer constituting the second layer 40), were laminated in this order from the semi-insulating GaAs substrate (semiconductor substrate 10 ) side to form a structure corresponding to the compound semiconductor layer 50 .

[0127] <Comparative Example 2> The comparative example has a double barrier structure. Sn = 7 × 10 18 [cm -3 ] doped n-type InSb layer 21 is 0.5 μm, Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.04 In 0.96 The Sb layer is 0.5 μm thick (corresponding to buffer layer 23). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.26 In 0.74 The Sb layer is 0.02 μm (equivalent to barrier layer 22), Non-doped Al 0.04 In 0.96 Sb layer (equivalent to light-emitting layer 30) is 2 μm, Zn 3×10 18 [cm -3 ] doped p-type l 0.26 In 0.74 The Sb layer is 0.02 μm thick (corresponding to the barrier layer constituting the second layer 40). Zn 3×10 18 [cm -3 ] doped p-type Al 0.04 In 0.96 The Sb layer is 0.5 μm thick (corresponding to the p layer constituting the second layer 40), were laminated in this order from the semi-insulating GaAs substrate (semiconductor substrate 10 ) side to form a structure corresponding to the compound semiconductor layer 50 .

[0128] <Comparative Example 3> The comparative example has a double barrier structure. Sn = 7 × 10 18 [cm -3 ] doped n-type InSb layer 21 is 0.5 μm, Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.13 In 0.87 The Sb layer is 0.5 μm thick (corresponding to buffer layer 23). Sn = 7 × 10 18 [cm -3 ] doped n-type Al 0.33 In 0.67 The Sb layer is 0.02 μm (equivalent to barrier layer 22), Non-doped Al 0.13 In 0.87 Sb layer (equivalent to light-emitting layer 30) is 2 μm, Zn 3×10 18 [cm -3 ] doped p-type l 0.33 In 0.67 The Sb layer is 0.02 μm thick (corresponding to the barrier layer constituting the second layer 40). Zn 3×10 18 [cm -3 ] doped p-type Al 0.13 In 0.87 The Sb layer is 0.5 μm thick (corresponding to the p layer constituting the second layer 40), were laminated in this order from the semi-insulating GaAs substrate (semiconductor substrate 10 ) side to form a structure corresponding to the compound semiconductor layer 50 .

[0129] In Comparative Example 1, a measurement sample was prepared from within the 0.3 μm area of ​​the light-emitting layer close to the p-layer, and line defect density was observed using a planar TEM. The line defect density was found to be 3.5 × 10 8 [book / cm 2 ] was the case.

[0130] <Comparison of Luminescence Intensity> For the infrared LED elements formed according to the above Examples 1 to 22 and Comparative Examples 1 to 3, the luminescence intensity was measured. Specifically, for the elements obtained in the above examples, a current of 100 mA was passed in the forward direction at a frequency of 200 Hz and a Duty of 1%. Using HgCdTe (MCT) for the light receiver, signal amplification and noise removal were performed using an IV conversion amplifier and a lock-in amplifier, and then the output was obtained. The obtained luminescence intensities are as shown in Tables 1 and 2. Here, the luminescence intensity of the infrared LED element formed according to Comparative Example 1 is set to 1.

[0131] Including the dislocation filter layer t y(i) In the structures of Examples 1 to 12 and 18 to 20 where y(i), x(i), and x(i + 1) satisfy the following relational expressions (A) to (D), it was confirmed that a luminescence intensity of 1.2 times or more can be obtained compared to the structure of Comparative Example 1. 0 < t y(1) ≦2360×(y(i) - x(i)) - 240 (0.11 ≦ y(i) - x(i) ≦ 0.19) … Equation (A) 0 < t y(1) ≦ - 1215×(y(i) - x(i)) + 427 (0.19 < y(i) - x(i) ≦ 0.33) … Equation (B) 0 < t y(1) ≦2360×(y(i) - x(i + 1)) - 240 (0.11 ≦ y(i) - x(i + 1) ≦ 0.19) … Equation (C) 0 < t y(1) ≦ - 1215×(y(i) - x(i + 1)) + 427 (0.19 < y(i) - x(i + 1) ≦ 0.33) … Equation (D)

[0132] Here, FIG. 1 shows the relationship between the compositions and film thicknesses of Examples 1 to 9 and 18 to 20. The horizontal axis of FIG. 1 indicates the difference between y(i) and x(i). Here, x(i) and x(i + 1) in Examples 1 to 9 and 18 to 20 have the same composition. Therefore, the horizontal axis of FIG. 1 is also the difference between y(i) and x(i + 1). Further, the vertical axis of FIG. 1 indicates the film thickness of the dislocation filter layer Y(i). Some of Examples 1 to 9 and 18 to 20 are plotted in FIG. 1 as black squares. The above formulas (A) to (D) are calculated from the relationships shown in FIG. 1. The above formulas (A) and (C) correspond to the straight line 1001 in FIG. 1. Also, the above formulas (B) and (D) correspond to the straight line 1002 in FIG. 1.

[0133] Note that, as described above, it is known that the higher the thickness of the compound semiconductor material to be laminated, the lower the dislocation density. Therefore, for Examples 10, 11, and 12 with different thicknesses of the laminated compound semiconductor layers, a simple comparison of the emission intensities with other Examples 1 to 9 and 18 to 20 cannot be made.

[0134] Here, in Examples 1, 3, 4, 5, 7, 8, 9, 18, 19, and 20, emission intensities greater than 2.0 times that of Comparative Example 1 can be obtained. At this time, the following relational expressions (I) to (L) are satisfied. 0 < t y(1) ≦ 6901×(y(i) - x(i)) - 1087 (0.16 ≦ y(i) - x(i) ≦ 0.19) … Formula (I) 0 < t y(1) ≦ -2673×(y(i) - x(i)) + 699 (0.19 < y(i) - x(i) ≦ 0.25) … Formula (J) 0 < t y(1) ≦ 6901×(y(i) - x(i + 1)) - 1087 (0.16 ≦ y(i) - x(i + 1) ≦ 0.19) … Formula (K) 0 < t y(1) ≦ -2673×(y(i) - x(i + 1)) + 699 (0.19 < y(i) - x(i + 1) ≦ 0.25) … Formula (L)

[0135] The above formulas (I) to (L) are calculated from the relationships shown in FIG. 1. The above formulas (I) and (K) correspond to the straight line 1021 in FIG. 1. Also, the above formulas (J) and (L) correspond to the straight line 1022 in FIG. 1.

[0136] Regarding Examples 1, 3, 4, 5, 7, 8, 18, 19, and 20 that satisfy the following relational expressions (M) to (P), it was confirmed that a luminescence intensity 2.2 times or more greater than that of Comparative Example 1 can be obtained. 0 < t y(1) ≦1993×(y(i) - x(i)) - 242 (0.13 ≦ y(i) - x(i) ≦ 0.19) … Formula (M) 0 < t y(1) ≦ - 1040×(y(i) - x(i)) + 324 (0.19 < y(i) - x(i) ≦ 0.29) … Formula (N) 0 < t y(1) ≦1993×(y(i) - x(i + 1)) - 242 (0.13 ≦ y(i) - x(i + 1) ≦ 0.19) … Formula (O) 0 < t y(1) ≦ - 1040×(y(i) - x(i + 1)) + 324 (0.19 < y(i) - x(i + 1) ≦ 0.29) … Formula (P)

[0137] The above formulas (M) to (P) are calculated from the relationships shown in FIG. 1. The above formulas (M) and (O) correspond to the straight line 1031 in FIG. 1. Also, the above formulas (N) and (P) correspond to the straight line 1032 in FIG. 1.

[0138] Regarding Examples 1, 3, 4, 5, 7, and 8 that satisfy the following relational expressions (E) to (H), it was confirmed that a luminescence intensity 2.4 times or more greater than that of Comparative Example 1 can be obtained. 0 < t y(1) ≦3067×(y(i) - x(i)) - 472 (0.16 ≦ y(i) - x(i) ≦ 0.19) … Formula (E) 0 < t y(1) ≦ - 1188×(y(i) - x(i)) + 322 (0.19 < y(i) - x(i) ≦ 0.25) … Formula (F) 0 < t y(1)≦3067×(y(i) - x(i + 1)) - 472 (0.16 ≦ y(i) - x(i + 1) ≦ 0.19) … Equation (G) 0 < t y(1) ≦ - 1188×(y(i) - x(i + 1)) + 322 (0.19 < y(i) - x(i + 1) ≦ 0.25) … Equation (H)

[0139] The above equations (E) to (H) are calculated from the relationships shown in FIG. 1. The above equations (E) and (G) correspond to the straight line 1011 in FIG. 1. Also, the above equations (F) and (H) correspond to the straight line 1012 in FIG. 1.

[0140] Examples 1, 16, and 17 have the same thickness of the first layer and only differ in the number of repetitions of the dislocation filter structure. At this time, it can be seen that the emission intensity increases as the number of repetitions increases.

[0141] Examples 21 and 22 are examples in which Ga is included in the dislocation filter layer, and it can also be seen that emission intensities 2.7 times greater than that of Comparative Example 1 are obtained in these cases.

[0142] <Comparison of Emission Intensity> Regarding the infrared LED elements formed by the above Examples 13 and 14 and Comparative Example 2, the emission intensity was measured. Specifically, for the elements obtained in the above examples, a current of 30 mA was passed in the forward direction at a frequency of 200 Hz and a Duty of 1%. Using HgCdTe (MCT) for the light receiver, signal amplification and noise removal were performed using an IV conversion amplifier and a lock-in amplifier, and then the output was obtained. The obtained emission intensities are as shown in Table 2. Here, the emission intensity of the infrared LED element formed by Comparative Example 2 is set to 1.

[0143] Here, between Examples 1 to 12, 18 to 20 and Comparative Example 1, and between Examples 13 and 14 and Comparative Example 2, the Al composition of the light-emitting layer, that is, the bandgap of the light-emitting layer, is different, and the energy per photon of the generated light is different, so they cannot be simply compared. Therefore, for Examples 13 and 14, Comparative Example 2 is used as the object for comparison of the emission intensity.

[0144] Similarly, the emission intensity was measured for the infrared LED elements formed in Example 15 and Comparative Example 3. Specifically, the emission intensity was measured by passing a forward current of 100 mA at a frequency of 200 Hz and a duty of 1% through the elements obtained in the above examples, using HgCdTe (MCT) as the receiver, and performing signal amplification and noise removal using an IV conversion amplifier and a lock-in amplifier to obtain an output. The obtained emission intensities are shown in Table 2. Here, the emission intensity of the infrared LED element formed in Comparative Example 3 is set to 1.

[0145] In Examples 13 and 14, the emission intensity is 1.7 times as high as that of Comparative Example 2. Similarly, in Example 15, the emission intensity is 4.0 times as high as that of Comparative Example 3. Examples 13 and 14 do not include a dislocation filter layer. y(i) , y(i), x(i), and x(i+1) satisfy the above relational expressions (A) to (P), and it was shown that the luminescence intensity increases even if the Al composition z of the luminescent layer changes. [Explanation of symbols]

[0146] 10. Semiconductor Substrate 20 1st layer 21 InSb layer 22 Barrier Layer 23 Buffer layer (X(1) layer) 24 Transposition filter layer (Y(1) layer) 25 Buffer layer (X(2) layer) 26 Transposition filter layer (Y(2) layer) 27 Buffer layer (X(3) layer) 30 Light-emitting layer 40 2nd layer 50 Compound semiconductor layer 100 Infrared light emitting element

Claims

1. A semiconductor substrate; a first layer formed on the semiconductor substrate and having a first conductivity type; a light-emitting layer formed on the first layer; a second layer formed on the light emitting layer and having a second conductivity type; The first layer has a thickness of t x(1) [nm] and Al x(1) In 1-x(1) A layer containing Sb and a layer having a thickness of t y(1) [nm] and Al y(1) In 1-y(1) A layer containing Sb and a layer having a thickness of t x(2) [nm] and Al x(2) In 1-x(2) a layer containing Sb, Said t y(1) , the x(1), the x(2) and the y(1) are 0<t y(1) ≦2360×(y(1)-x(1))-240 (0.11≦y(1)-x(1)≦0.19)、 0<t y(1) ≦-1215×(y(1)-x(1))+427 (0.19<y(1)-x(1)≦0.33)、 0<t y(1) ≦2360×(y(1)-x(2))-240 (0.11≦y(1)-x(2)≦0.19)、 0<t y(1) ≦-1215×(y(1)-x(2))+427 (0.19<y(1)-x(2)≦0.33)、 0<x(1)<0.18, 0<x(2)<0.18, t x(1) ≧200, and t x(2) ≧200 Fulfilling the first layer further includes a barrier layer in contact with the light emitting layer and having a band gap larger than that of the light emitting layer, the second layer further includes a barrier layer in contact with the light emitting layer and having a band gap larger than that of the light emitting layer, The first layer has a thickness of t for an integer i ranging from 1 to n (2≦n≦6). x(i) [nm] and Al x(i) In 1-x(i) A layer containing Sb and a layer having a thickness of t y(i) [nm] and Al y(i) In 1-y(i) A layer including Sb is laminated in this order in units of n layers, and the thickness of the layer is t y(n) [nm] and Al y(n) In 1-y(n) A layer having a thickness of t x(n+1) [nm] and Al x(n+1) In 1-x(n+1) and a layer containing Sb, Said t y(i) , the x(i), x(i+1) and the y(i) are 0<t y(i) ≦2360×(y(i)-x(i))-240 (0.11≦y(i)-x(i)≦0.19)、 0<t y(i) ≦-1215×(y(i)-x(i))+427 (0.19<y(i)-x(i)≦0.33)、 0<t y(i) ≦2360×(y(i)-x(i+1))-240 (0.11≦y(i)-x(i+1)≦0.19)、 0<t y(i) ≦-1215×(y(i)-x(i+1))+427 (0.19<y(i)-x(i+1)≦0.33)、 0<x(i)<0.18, 0<x(i+1)<0.18, t x(i) ≧200, and t x(i+1) ≧200 Fulfilling Said t y(i) The infrared light emitting element has a wavelength of 100 nm or less.

2. Said t y(i) , the x(i), the x(i+1) and the y(i) are 0<t y(i) ≦6901×(y(i)-x(i))-1087 (0.16≦y(i)-x(i)≦0.19)、 0<t y(i) ≦-2673×(y(i)-x(i))+699 (0.19<y(i)-x(i)≦0.25)、 0<t y(i) ≦6901×(y(i)−x(i+1))−1087 (0.16≦y(i)−x(i+1)≦0.19), and 0<t y(i) ≦-2673×(y(i)-x(i+1))+699 (0.19<y(i)-x(i+1)≦0.25) The infrared light emitting device according to claim 1 , which satisfies the above.

3. Said t y(i) , the x(i), the x(i+1) and the y(i) are 0<t y(i) ≦1993×(y(i)-x(i))-242 (0.13≦y(i)-x(i)≦0.19)、 0<t y(i) ≦-1040×(y(i)-x(i))+324 (0.19<y(i)-x(i)≦0.29)、 0<t y(i) ≦1993×(y(i)−x(i+1))−242 (0.13≦y(i)−x(i+1)≦0.19), and 0<t y(i) ≦-1040×(y(i)-x(i+1))+324 (0.19<y(i)-x(i+1)≦0.29) The infrared light emitting device according to claim 1 or 2, which satisfies the above.

4. Said t y(i) , the x(i), the x(i+1) and the y(i) are 0<t y(i) ≦3067×(y(i)-x(i))-472 (0.16≦y(i)-x(i)≦0.19)、 0<t y(i) ≦-1188×(y(i)-x(i))+322 (0.19<y(i)-x(i)≦0.25)、 0<t y(i) ≦3067×(y(i)−x(i+1))−472 (0.16≦y(i)−x(i+1)≦0.19), and 0<t y(i) ≦-1188×(y(i)-x(i+1))+322 (0.19<y(i)-x(i+1)≦0.25) The infrared light emitting device according to claim 1 , which satisfies the above condition.

5. The first conductivity type is n-type, and the second conductivity type is p-type. The infrared light emitting device according to claim 1 .

6. the semiconductor substrate is a GaAs substrate, 6. The infrared light emitting device according to claim 1, wherein the first layer, which is in contact with the GaAs substrate, is a layer made of InSb.

7. The light-emitting layer is Al z In 1-z Sb (0<z<0.18) included The infrared light emitting device according to claim 1 .

8. The x(1) and x(2) are 0<x(1)<0.09, and 0<x(2)<0.09 The infrared light emitting device according to claim 1 , which satisfies the following:

9. The light-emitting layer is Al z In 1-z Sb (0<z<0.09) included The infrared light emitting device according to claim 1 .

10. The Al x(1) In 1-x(1) The layer containing Sb, y(1) In 1-y(1) The Sb-containing layer and the Al x(2) In 1-x(2) At least one of the layers containing Sb further contains As in an amount of 3% or less with respect to the total group V elements. The infrared light emitting device according to claim 1 .

11. Said t y(1) The infrared light emitting device according to claim 1 , wherein the thickness is 6 times or less of the critical thickness.

12. The light-emitting layer has a linear defect density of 3.0×10 8 [book / cm 2 ]or less The infrared light emitting element according to claim 1 .

13. A semiconductor substrate; a first layer formed on the semiconductor substrate and having a first conductivity type; a light-emitting layer formed on the first layer; a second layer formed on the light emitting layer and having a second conductivity type; The first layer has a thickness of t x(1) [nm] and Al x(1) G p(1) In 1-x(1)-p(1) A layer containing Sb and a layer having a thickness of t y(1) [nm] and Al y(1) G q(1) In 1-y(1)-q(1) A layer containing Sb and a layer having a thickness of t x(2) [nm] and Al x(2) G p(2) In 1-x(2)-p(2) a layer containing Sb, Said t y(1) , the x(1), the x(2), the y(1), the p(1), the p(2), and the q(1) are 0<t y(1) ≦2360×(y(1)+q(1)-x(1)-p(1))-240 (0.11≦y(1)+q(1)-x(1)-p(1)≦0.19)、 0<t y(1) ≦-1215×(y(1)+q(1)-x(1)-p(1))+427 (0.19<y(1)+q(1)-x(1)-p(1)≦0.33)、 0<t y(1) ≦2360×(y(1)+q(1)-x(2)-p(2))-240 (0.11≦y(1)+q(1)-x(2)-p(2)≦0.19)、 0<t y(1) ≦-1215×(y(1)+q(1)-x(2)-p(2))+427 (0.19<y(1)+q(1)-x(2)-p(2)≦0.33)、 0<x(1)+p(1)<0.18, 0<x(2)+p(2)<0.18, 0<q(1) / (y(1)+q(1))≦1, t x(1) ≧200, and t x(2) ≧200 Fulfilling the first layer further includes a barrier layer in contact with the light emitting layer and having a band gap larger than that of the light emitting layer, the second layer further includes a barrier layer in contact with the light emitting layer and having a band gap larger than that of the light emitting layer, The first layer has a thickness of t for an integer i ranging from 1 to n (2≦n≦6). x(i) [nm] and Al x(i) G p(i) In 1-x(i)-p(i) A layer containing Sb and a layer having a thickness of t y(i) [nm] and Al y(i) G q(i) In 1-y(i)-q(i) A layer including Sb is laminated in this order in units of n layers, and the thickness of the layer is t y(n) [nm] and Al y(n) G q(n) In 1-y(n)-q(n) A layer having a thickness of t x(n+1) [nm] and Al x(n+1) G p(n+1) In 1-x(n+1)-p(n+1) and a layer containing Sb, Said t y(i) , the x(i), x(i+1), y(i), p(i), p(i+1), and q(i) are 0<t y(i) ≦2360×(y(i)+q(i)-x(i)-p(i))-240 (0.11≦y(i)+q(i)-x(i)-p(i)≦0.19)、 0<t y(i) ≦-1215×(y(i)+q(i)-x(i)-p(i))+427 (0.19<y(i)+q(i)-x(i)-p(i)≦0.33)、 0<t y(i) ≦2360×(y(i)+q(i)-x(i+1)-p(i+1))-240 (0.11≦y(i)+q(i)-x(i+1)-p(i+1)≦0.19)、 0<t y(i) ≦-1215×(y(i)+q(i)-x(i+1)-p(i+1))+427 (0.19<y(i)+q(i)-x(i+1)-p(i+1)≦0.33)、 0<x(i)+p(i)<0.18, 0<x(i+1)+p(i+1)<0.18, 0<q(i) / (y(i)+q(i))≦1, t x(i) ≧200, and t x(i+1) ≧200 Fulfilling Said t y(i) The infrared light emitting element has a wavelength of 100 nm or less.

14. Said t y(i) , the x(i), the x(i+1), the y(i), the p(i), the p(i+1), and the q(i) are 0<t y(i) ≦1993×(y(i)+q(i)-x(i)-p(i))-242 (0.13≦y(i)+q(i)-x(i)-p(i)≦0.19)、 0<t y(i) ≦-1040×(y(i)+q(i)-x(i)-p(i))+324 (0.19<y(i)+q(i)-x(i)-p(i)≦0.29)、 0<t y(i) ≦1993×(y(i)+q(i)-x(i+1)-p(i+1))-242 (0.13≦y(i)+q(i)-x(i+1)-p(i+1)≦0.19)、 0<t y(i) ≦-1040×(y(i)+q(i)-x(i+1)-p(i+1))+324 (0.19<y(i)+q(i)-x(i+1)-p(i+1)≦0.29)、 The infrared light emitting device according to claim 13 , which satisfies the above.

15. Said t y(i) , the x(i), the x(i+1), the y(i), the p(i), the p(i+1), and the q(i) are 0<t y(i) ≦3067×(y(i)+q(i)-x(i)-p(i))-472 (0.16≦y(i)+q(i)-x(i)-p(i)≦0.19)、 0<t y(i) ≦-1188×(y(i)+q(i)-x(i)-p(i))+322 (0.19<y(i)+q(i)-x(i)-p(i)≦0.25)、 0<t y(i) ≦3067×(y(i)+q(i)-x(i+1)-p(i+1))-472 (0.16≦y(i)+q(i)-x(i+1)-p(i+1)≦0.19)、 0<t y(i) ≦-1188×(y(i)+q(i)-x(i+1)-p(i+1))+322 (0.19<y(i)+q(i)-x(i+1)-p(i+1)≦0.25)、 The infrared light emitting device according to claim 13 or 14, which satisfies the above.

Citation Information

Patent Citations

  • Method for manufacturing semiconductor device for mid-infrared light

    JP2008254966A

  • Group iii-v nitride layer and method for producing the same

    JP2008266113A

  • Nitride semiconductor light-emitting element

    JP2014143338A

  • Infrared detector

    JP2015090901A

  • Gas sensor

    JP2017015568A