Solder composition and electronic substrate
A solder composition with defined amide compounds and flux components balances printability and sag resistance, addressing the challenge of simultaneous improvement in both properties.
Patent Information
- Application Number
- JP2022031866
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-03-02
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2042-03-02
AI Technical Summary
Existing solder compositions struggle to balance printability and sag resistance during heating, with improvements in sag resistance often leading to decreased printability.
A solder composition comprising a flux composition with specific amide compounds having defined molecular weights and Mw/Mn ratios, along with rosin resin, activators, and thixotropic agents, to maintain thixotropy and improve sag resistance while preserving printability.
The composition achieves excellent printability and sag resistance during heating, enabling effective soldering on micro lands without defects.
Smart Images

Figure 0007554218000003 
Figure 0007554218000002 
Figure 0007554218000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a solder composition and an electronic substrate. [Background technology]
[0002] The solder composition is a mixture of solder powder and flux composition (rosin resin, activator, solvent, etc.) kneaded into a paste (see Patent Document 1). In addition to printability and solderability, this solder composition is required to have a property (resistance to sagging when heated) that suppresses sagging (deformation of the coated film of the solder composition during preheating) during preheating in the reflow process. In addition, since mounting on micro lands has progressed in recent years, further improvement in sagging when heated is required. However, if the viscosity or thixotropy of the solder composition is increased in order to improve the sagging when heated, the printability of the solder composition tends to decrease. In this way, it is difficult to achieve both printability and sagging when heated. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5887330 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a solder composition that is excellent in both printability and sagging resistance when heated, and an electronic board using the same. [Means for solving the problem]
[0005] According to one aspect of the present invention, there is provided a solder composition comprising: a flux composition containing (A) a rosin-based resin, (B) an activator, and (C) a thixotropic agent; and (D) a solder powder, wherein the component (C) contains (C1) an amide compound having a weight average molecular weight Mw of 500 or more and 2500 or less, a number average molecular weight Mn of 500 or more and 1500 or less, and an Mw / Mn value of 1.2 or more and 2.5 or less.
[0006] According to one aspect of the present invention, there is provided an electronic substrate having a portion soldered using the solder composition according to the above aspect of the present invention. Effect of the Invention
[0007] According to the present invention, it is possible to provide a solder composition that is excellent in both printability and sagging resistance when heated, and an electronic substrate using the same. [Brief description of the drawings]
[0008] [Figure 1] 2 is a graph showing the results of measuring the molecular weight of the amide compound obtained in Preparation Example 1. [Diagram 2] 2 shows a graph showing the results of measuring the molecular weight of the amide compound obtained in Preparation Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The solder composition of the present embodiment contains a flux composition containing (A) a rosin-based resin, (B) an activator, and (C) a thixotropic agent, and (D) a solder powder.
[0010] The reason why a solder composition having both excellent printability and excellent sagging properties when heated can be obtained according to this embodiment is not entirely clear, but the present inventors speculate as follows. In other words, the present inventors surmise that the mechanism by which the amide compound (C1) having a weight average molecular weight Mw of 500 or more and 2500 or less, a number average molecular weight Mn of 500 or more and 1500 or less, and a Mw / Mn value of 1.2 or more and 2.5 or less can improve sagging resistance when heated while maintaining printability is as follows. First, the (C1) amide compound contributes to the thixotropy of the solder composition, but the degree of contribution to the thixotropy varies depending on the molecular weight of the amide compound. The degree of contribution to the thixotropy also varies depending on the temperature of the solder composition. The (C1) component of this embodiment has an Mw / Mn value of 1.2 or more and 2.5 or less, and contains a predetermined amount or more of a relatively high molecular weight component. The relatively high molecular weight component and the average molecular weight component change their degree of contribution to the thixotropy depending on the temperature of the solder composition. The (C1) component of this embodiment can adjust the thixotropy ratio to a range that provides excellent printability during printing, and can adjust the thixotropy ratio to a range that provides excellent heat sagging during heating. The inventors speculate that the effects of the present invention are achieved in the above manner.
[0011] [Flux composition] First, the flux composition used in this embodiment will be described. The flux composition used in this embodiment is a component other than the solder powder in the solder composition, and contains (A) a rosin resin, (B) an activator, and (C) a thixotropic agent, which will be described below.
[0012] [Component (A)] The rosin-based resin (A) used in this embodiment includes rosins and rosin-modified resins. Examples of rosins include gum rosin, wood rosin, and tall oil rosin. Examples of rosin-modified resins include disproportionated rosin, polymerized rosin, hydrogenated rosin, and derivatives thereof. Examples of hydrogenated rosin include fully hydrogenated rosin, partially hydrogenated rosin, and hydrogenated products of unsaturated organic acid-modified rosins (also called "hydrogenated acid-modified rosin"), which are modified rosins of unsaturated organic acids (aliphatic unsaturated monobasic acids such as (meth)acrylic acid, aliphatic unsaturated dibasic acids such as α,β-unsaturated carboxylic acids such as fumaric acid and maleic acid, unsaturated carboxylic acids having aromatic rings such as cinnamic acid, etc.). These rosin-based resins may be used alone or in combination of two or more.
[0013] The amount of the (A) component is preferably 20% by mass or more and 70% by mass or less, and more preferably 30% by mass or more and 60% by mass or less, based on 100% by mass of the flux composition. If the amount of the (A) component is more than the lower limit, the oxidation of the copper foil surface of the soldering land is prevented, making the surface more easily wetted with molten solder, so that the so-called solderability can be improved and solder balls can be sufficiently suppressed. Also, if the amount of the (A) component is less than the upper limit, the amount of flux residue can be sufficiently suppressed.
[0014] [(B) Component] The (B) activator used in this embodiment includes organic acids, non-dissociative activators (halogen-based activators) made of non-dissociative halogenated compounds, and amine-based activators. These may be used alone or in combination of two or more. Among these, it is preferable to contain (B1) an organic acid. It is also preferable that the (B) component further contains (B2) an amine-based activator. Examples of the component (B1) include other organic acids in addition to monocarboxylic acids and dicarboxylic acids, etc. These may be used alone or in combination of two or more. Monocarboxylic acids include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, enanthic acid, capric acid, lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, tuberculostearic acid, arachidic acid, behenic acid, lignoceric acid, and glycolic acid. Examples of dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, fumaric acid, maleic acid, tartaric acid, and diglycolic acid. Among these, succinic acid, glutaric acid, and dodecanedioic acid are preferred from the viewpoint of activity. Other organic acids include 3-hydroxy-2-naphthoic acid, dimer acid, trimer acid, levulinic acid, lactic acid, acrylic acid, benzoic acid, salicylic acid, anisic acid, citric acid, picolinic acid, etc. Among these, it is more preferable to use 3-hydroxy-2-naphthoic acid from the viewpoint of activity. From the viewpoint of improving the solder melting property on the minute land, it is preferable to use a plurality of organic acids in combination, and it is particularly preferable to use succinic acid, glutaric acid, dodecanedioic acid, and 3-hydroxy-2-naphthoic acid in combination.
[0015] The blending amount of the (B1) component is preferably 1% by mass or more and 12% by mass or less, more preferably 2% by mass or more and 10% by mass or less, and particularly preferably 3% by mass or more and 7% by mass or less, based on 100% by mass of the flux composition. If the blending amount of the (B1) component is equal to or more than the lower limit, the activation action tends to be improved, whereas if it is equal to or less than the upper limit, the insulating properties of the flux composition tend to be maintained.
[0016] Examples of the (B2) component include imidazolines (such as 2-phenylimidazoline), amines (such as polyamines such as ethylenediamine), amine salts (organic acid salts or inorganic acid salts (such as hydrochloric acid, sulfuric acid, hydrobromic acid, etc.) of amines and aminoalcohols such as trimethylolamine, cyclohexylamine, and diethylamine), amino acids (glycine, alanine, aspartic acid, glutamic acid, valine, etc.), and amide compounds. Specific examples include diphenylguanidine hydrobromide, cyclohexylamine hydrobromide, diethylamine salts (such as hydrochloride, succinate, adipate, and sebacate), triethanolamine, monoethanolamine, and hydrobromides of these amines. Among these, imidazolines are preferred from the viewpoint of activity, and 2-phenylimidazoline is particularly preferred. From the viewpoint of improving the solder melting properties on a minute land, it is preferable to use the component (B1) in combination with the component (B2), and it is particularly preferable to use the component (B1) in combination with 2-phenylimidazoline.
[0017] The blending amount of the (B2) component is preferably 1% by mass or more and 12% by mass or less, more preferably 2% by mass or more and 10% by mass or less, and particularly preferably 3% by mass or more and 7% by mass or less, based on 100% by mass of the flux composition. If the blending amount of the (B2) component is equal to or more than the lower limit, the activation action tends to be improved, whereas if it is equal to or less than the upper limit, the insulating properties of the flux composition tend to be maintained.
[0018] The blending amount of the (B) component is preferably 3% by mass or more and 25% by mass or less, more preferably 5% by mass or more and 20% by mass or less, and particularly preferably 8% by mass or more and 15% by mass or less, based on 100% by mass of the flux composition. If the blending amount of the (B) component is equal to or more than the lower limit, the activation action tends to be improved, whereas if it is equal to or less than the upper limit, the insulating property of the flux composition tends to be maintained.
[0019] [(C) component] The (C) thixotropic agent used in this embodiment must contain (C1) an amide compound having a weight average molecular weight Mw of 500 or more and 2500 or less, a number average molecular weight Mn of 500 or more and 1500 or less, and an Mw / Mn value of 1.2 or more and 2.5 or less. With such a (C1) component, sagging properties when heated can be improved while maintaining printability.
[0020] If the weight average molecular weight Mw of the component (C1) is less than 500, sagging during heating cannot be suppressed. On the other hand, if the weight average molecular weight Mw of the component (C1) is more than 2500, sagging during printing cannot be suppressed. From the same viewpoint, the weight average molecular weight Mw of the component (C1) is preferably 700 or more and 2400 or less, more preferably 1000 or more and 2350 or less, and particularly preferably 1500 or more and 2300 or less.
[0021] If the number average molecular weight Mn of the component (C1) is less than 500, sagging during heating cannot be suppressed. On the other hand, if the number average molecular weight Mn of the component (C1) is more than 1500, sagging during printing cannot be suppressed. From the same viewpoint, the number average molecular weight Mn of the component (C1) is preferably 550 or more and 1,400 or less, more preferably 600 or more and 1,350 or less, and particularly preferably 700 or more and 1,300 or less.
[0022] If the Mw / Mn value of the component (C1) is less than 1.2 or exceeds 2.5, at least one of sagging during heating and sagging during printing cannot be suppressed. From the same viewpoint, the Mw / Mn value of the component (C1) is preferably 1.3 or more and 2.2 or less, and particularly preferably 1.35 or more and 2 or less.
[0023] In this embodiment, it is preferable to use two or more types of component (C1) in combination, which can further improve the properties of the solder composition.
[0024] This component (C1) can be prepared, for example, by condensing an aliphatic monocarboxylic acid having 2 to 22 carbon atoms, including a hydroxyaliphatic monocarboxylic acid, an aliphatic dicarboxylic acid having 2 to 12 carbon atoms, and a diamine having 2 to 16 carbon atoms. Among aliphatic monocarboxylic acids having 2 to 22 carbon atoms, the number average molecular weight Mn of the component (C1) tends to decrease as the carbon number decreases. Among aliphatic dicarboxylic acids having 2 to 12 carbon atoms, the number average molecular weight Mn of the component (C1) tends to decrease as the number of carbon atoms decreases. Among diamines having 2 to 16 carbon atoms, the number average molecular weight Mn of component (C1) tends to decrease as the number of carbon atoms decreases.
[0025] The greater the amount of the aliphatic dicarboxylic acid having 2 to 12 carbon atoms relative to the aliphatic monocarboxylic acid having 2 to 22 carbon atoms, the greater the number average molecular weight Mn of the component (C1). It is preferable that the total amount of carboxyl groups in the aliphatic monocarboxylic acid having 2 to 22 carbon atoms and the aliphatic dicarboxylic acid having 2 to 12 carbon atoms is equal to the amount of amino groups in the diamine having 2 to 16 carbon atoms. When these amounts are equal, the condensation reaction easily proceeds.
[0026] The temperature during the condensation reaction is preferably from 100° C. to 250° C., more preferably from 120° C. to 210° C., and particularly preferably from 150° C. to 190° C. The higher the temperature, the larger the weight average molecular weight Mw of the (C1) component tends to be. The time for the condensation reaction is preferably from 1 to 15 hours, more preferably from 3 to 11 hours, and particularly preferably from 5 to 8 hours. The longer this time is, the larger the weight average molecular weight Mw of the (C1) component tends to be. In other words, the weight-average molecular weight Mw, number-average molecular weight Mn, and Mw / Mn value of the component (C1) can be appropriately adjusted by, for example, (i) adjusting the types and amounts of the raw materials of the component (C1), (ii) adjusting the temperature during the condensation reaction, and (iii) adjusting the time spent on the condensation reaction.
[0027] The blending amount of the (C1) component is preferably 0.1% by mass or more and 25% by mass or less, more preferably 1% by mass or more and 20% by mass or less, even more preferably 2% by mass or more and 16% by mass or less, and particularly preferably 3% by mass or more and 10% by mass or less, based on 100% by mass of the flux composition. If the blending amount of the (C) component is equal to or more than the lower limit, sagging during printing and sagging during heating can be suppressed. If the blending amount of the (C) component is equal to or less than the upper limit, the thixotropy is not too high, and printing defects can be suppressed.
[0028] Component (C) may contain a thixotropic agent other than component (C1) (hereinafter, component (C2)). Examples of component (C2) include hydrogenated castor oil, amides other than component (C1), kaolin, colloidal silica, organic bentonite, and glass frit. These may be used alone or in combination of two or more.
[0029] The blending amount of the (C) component is preferably 1% by mass or more and 25% by mass or less, more preferably 3% by mass or more and 20% by mass or less, even more preferably 5% by mass or more and 16% by mass or less, and particularly preferably 6% by mass or more and 10% by mass or less, based on 100% by mass of the flux composition. If the blending amount of the (C) component is equal to or more than the lower limit, thixotropy is obtained and sagging during printing can be suppressed. If the blending amount of the (C) component is equal to or less than the upper limit, thixotropy is not too high and printing defects can be suppressed.
[0030] [solvent] In the flux composition of the present embodiment, it is preferable to further contain a solvent from the viewpoint of printability, etc. As the solvent used here, a known solvent can be appropriately used. As such a solvent, it is preferable to use a solvent having a boiling point of 170° C. or more. In addition, a glycol-based solvent is preferable. Examples of such solvents include diethylene glycol, dipropylene glycol, triethylene glycol, hexylene glycol, hexyl diglycol, 1,5-pentanediol, methyl carbitol, butyl carbitol, 2-ethylhexyl diglycol (EHDG), octanediol, phenyl glycol, diethylene glycol monohexyl ether, tetraethylene glycol dimethyl ether, dibutyl maleic acid, etc. These solvents may be used alone or in combination of two or more.
[0031] When a solvent is used, the blending amount is preferably 10% by mass or more and 60% by mass or less, and more preferably 20% by mass or more and 40% by mass or less, based on 100% by mass of the flux composition. When the blending amount of the solvent is within the above range, the viscosity of the obtained solder composition can be appropriately adjusted to an appropriate range.
[0032] [Antioxidants] In the flux composition of the present embodiment, it is preferable to further contain an antioxidant from the viewpoint of solder melting property, etc. As the antioxidant used here, a known antioxidant can be appropriately used. Examples of the antioxidant include sulfur compounds, hindered phenol compounds, and phosphite compounds. Among these, hindered phenol compounds are preferable.
[0033] Examples of the hindered phenol compound include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionic acid][ethylene bis(oxyethylene)], N,N'-bis[2-[2-(3,5-di-tert-butyl-4-hydroxyphenyl)ethylcarbonyloxy]ethyl]oxamide, and N,N'-bis{3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl}hydrazine.
[0034] [Other ingredients] In addition to the (A) component, the (B) component, the (C) component, the solvent, and the antioxidant, other additives and even other resins can be added to the flux composition used in this embodiment as necessary. Examples of the other additives include antifoaming agents, modifiers, matting agents, and foaming agents. The blending amount of these additives is preferably 0.01% by mass or more and 5% by mass or less with respect to 100% by mass of the flux composition. Examples of the other resins include acrylic resins.
[0035] [Solder composition] Next, the solder composition of the present embodiment will be described. The solder composition of the present embodiment contains the flux composition of the present embodiment described above and the solder powder (D) described below. The amount of the flux composition is preferably 5% by mass or more and 35% by mass or less, more preferably 7% by mass or more and 15% by mass or less, and particularly preferably 8% by mass or more and 12% by mass or less, relative to 100% by mass of the solder composition. When the amount of the flux composition is less than 5% by mass (when the amount of the solder powder exceeds 95% by mass), the flux composition as a binder is insufficient, so that it tends to be difficult to mix the flux composition and the solder powder. On the other hand, when the amount of the flux composition is more than 35% by mass (when the amount of the solder powder is less than 65% by mass), when the obtained solder composition is used, it tends to be difficult to form a sufficient solder joint.
[0036] [(D) component] The solder powder (D) used in this embodiment is preferably made of only lead-free solder powder, but may be lead-containing solder powder. The solder alloy in this solder powder preferably contains at least one selected from the group consisting of tin (Sn), copper (Cu), zinc (Zn), silver (Ag), antimony (Sb), lead (Pb), indium (In), bismuth (Bi), nickel (Ni), cobalt (Co) and germanium (Ge). The solder alloy in the solder powder is preferably an alloy mainly composed of tin. More preferably, the solder alloy contains tin, silver, and copper. Furthermore, the solder alloy may contain at least one of antimony, bismuth, and nickel as an additive element. According to the flux composition of the present embodiment, even when a solder alloy containing an additive element that is easily oxidized, such as antimony, bismuth, and nickel, is used, the generation of voids can be suppressed. Here, lead-free solder powder refers to a powder of solder metal or alloy to which no lead is added. However, the presence of lead as an unavoidable impurity in the lead-free solder powder is permitted, but in this case, the amount of lead is preferably 300 ppm by mass or less.
[0037] Specific examples of alloy systems for lead-free solder powder include Sn-Ag-Cu systems, Sn-Cu systems, Sn-Ag systems, Sn-Bi systems, Sn-Ag-Bi systems, Sn-Ag-Cu-Bi systems, Sn-Ag-Cu-Ni systems, Sn-Ag-Cu-Bi-Sb systems, Sn-Ag-Bi-In systems, and Sn-Ag-Cu-Bi-In-Sb systems.
[0038] The average particle size of component (D) is usually 1 μm or more and 40 μm or less, but from the viewpoint of compatibility with electronic boards having narrow pitches of solder pads, it is more preferably 1 μm or more and 35 μm or less, even more preferably 2 μm or more and 35 μm or less, and particularly preferably 3 μm or more and 32 μm or less. The average particle size can be measured by a dynamic light scattering type particle size measuring device.
[0039] [Method of manufacturing solder composition] The solder composition of this embodiment can be produced by blending the above-described flux composition and the above-described (D) solder powder in the above-described predetermined ratio, and stirring and mixing them.
[0040] [Electronic board] Next, the electronic board of this embodiment will be described. The electronic board of this embodiment is characterized by having a soldered portion using the solder composition described above. The electronic board of the present invention can be manufactured by mounting electronic components on an electronic board (such as a printed wiring board) using the solder composition. Examples of the coating device used here include a screen printer, a metal mask printer, a dispenser, and a jet dispenser. In addition, an electronic component can be mounted on an electronic board by a reflow process in which an electronic component is placed on the solder composition applied by the application device and heated under specified conditions in a reflow furnace to mount the electronic component on a printed wiring board.
[0041] In the reflow process, the electronic component is placed on the solder composition and heated in a reflow furnace under predetermined conditions. This reflow process allows sufficient solder bonding between the electronic component and the printed wiring board. As a result, the electronic component can be mounted on the printed wiring board. The reflow conditions may be appropriately set according to the melting point of the solder. For example, the preheat temperature is preferably 140°C or higher and 200°C or lower, and more preferably 150°C or higher and 160°C or lower. The preheat time is preferably 60 seconds or higher and 120 seconds or lower. The peak temperature is preferably 230°C or higher and 270°C or lower, and more preferably 240°C or higher and 255°C or lower. The holding time at a temperature of 220°C or higher is preferably 20 seconds or higher and 60 seconds or lower.
[0042] Furthermore, the solder composition and electronic substrate of the present embodiment are not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. For example, in the electronic substrate, the printed wiring board and the electronic component are bonded by a reflow process, but the present invention is not limited thereto. For example, instead of the reflow process, the printed wiring board and the electronic component may be bonded by a process (laser heating process) of heating the solder composition using laser light. In this case, the laser light source is not particularly limited and can be appropriately adopted according to the wavelength that matches the absorption band of the metal. Examples of the laser light source include solid lasers (ruby, glass, YAG, etc.), semiconductor lasers (GaAs, InGaAsP, etc.), liquid lasers (dye, etc.), and gas lasers (He-Ne, Ar, CO2, excimer, etc.). EXAMPLES
[0043] The present invention will now be described in more detail with reference to examples and comparative examples, but the present invention is not limited to these examples. The materials used in the examples and comparative examples are shown below. (Component (A)) Rosin resin A: Hydrogenated acid-modified rosin (softening point: 124 to 134°C, acid value: 230 to 245 mgKOH / g), product name "Pine Crystal KE-604", manufactured by Arakawa Chemical Industries Co., Ltd. Rosin resin B: Fully hydrogenated rosin (softening point: 79-88°C, acid value: 158-173mgKOH / g), product name "Foral AX", manufactured by Rika Finetech Co., Ltd. ((B1) component) Organic acid A: Succinic acid Organic acid B: Glutaric acid Organic acid C: Dodecanedioic acid Organic acid D: 3-hydroxy-2-naphthoic acid ((B2) component) Amine surfactant: 2-phenylimidazoline ((C1) component) Amide compound A: An amide compound obtained in Preparation Example 1 below (weight average molecular weight Mw is 2000, number average molecular weight Mn is 1139, Mw / Mn is 1.755) Amide compound B: An amide compound obtained in Preparation Example 2 below (weight average molecular weight Mw is 1030, number average molecular weight Mn is 746, Mw / Mn is 1.381) ((C2) component) Thixotropic agent A: hexamethylene hydroxystearic acid amide, trade name "Slipax ZHH", manufactured by Mitsubishi Chemical Corporation, Mw / Mn is less than 1.2 Thixotropic agent B: Ethylene bis hydroxystearic acid amide, trade name "Slipax H", manufactured by Mitsubishi Chemical Corporation, Mw / Mn is less than 1.2 Thixotropic agent C: Trade name "Himako", manufactured by KF Trading Co., Ltd. (Other ingredients) Amine Compounds: 2-Phenylimidazoline Antioxidant: Trade name "Irganox 245", manufactured by BASF Solvent: Diethylene glycol mono-2-ethylhexyl ether (2-ethylhexyl diglycol (EHDG), boiling point: 272°C), manufactured by Nippon Nyukazai Co., Ltd. ((D) component) Solder powder: alloy composition is Sn-3.0Ag-0.5Cu, particle size distribution is 15-25μm (equivalent to type 5 of IPC-J-STD-005A), solder melting point is 217-220℃
[0044] [Preparation Example 1] In a reaction apparatus equipped with a stirrer, a thermometer, and a water divider, a predetermined amount of 12-hydroxystearic acid derived from hydrogenated castor oil fatty acid and an aliphatic dicarboxylic acid having 2 to 12 carbon atoms were added, and the mixture was melted by heating to 80 to 100° C. Then, a predetermined amount of hexamethylenediamine was added, and a condensation reaction was carried out while dehydrating in a nitrogen atmosphere at a temperature of 150° C. to 190° C. for 5 to 8 hours to obtain an amide compound A having an acid value of 5 mgKOH / g or less.
[0045] [Preparation Example 2] Amide compound B having an acid value of 5 mgKOH / g or less was obtained in the same manner as in Preparation Example 1, except that the type and amount of the aliphatic dicarboxylic acid having 2 to 12 carbon atoms used and the temperature and time during the condensation reaction were changed.
[0046] [Molecular weight measurement of amide compounds] The molecular weights (weight average molecular weight Mw, number average molecular weight Mn) of the amide compounds obtained in Preparation Examples 1 and 2 were measured by gel permeation chromatography (GPC) analysis. The analysis conditions were as follows. The results are shown in Figures 1 and 2. GPC equipment: HLC-8420GPC (Tosoh Corporation) Column: TSKgel Super AWM-H (6.0 mm I.D. x 15 cm) x 2 (Tosoh Corporation) Detector: Differential refractometer (RI detector), polarity=(+) Eluent: HFIP (1,1,1,3,3,3-hexafluoro-2-propanol) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) + 10 mM-CF3COONa (Fujifilm Wako Pure Chemical Industries, Ltd. Grade 1) ·Flow rate: 0.3mL / min Column temperature: 40℃ Sample concentration: 1mg / mL Sample injection volume: 20μL Sample pretreatment: The sample was weighed, a specified amount of eluent was added, and the sample was left to dissolve overnight at room temperature. After gentle shaking, the sample was filtered through a 0.45 μm PTFE cartridge filter. When the sample solution was visually observed, no insoluble matter was found in the sample. Calibration curve: A cubic approximation curve was made using standard polymethyl methacrylate (PMMA) (Agilent Technologies). In other words, the obtained value is the molecular weight converted into PMMA.
[0047] [Example 1] 31 mass% rosin-based resin A, 9 mass% rosin-based resin B, 0.5 mass% organic acid A, 0.5 mass% organic acid B, 1 mass% organic acid C, 2.5 mass% organic acid D, 5 mass% amine-based activator, 32.5 mass% solvent, 2 mass% antioxidant, and 16 mass% amide compound A were charged into a container and mixed using a planetary mixer to obtain a flux composition. Thereafter, 11 mass % of the obtained flux composition, 1.2 mass % of the solvent, and 87.8 mass % of the solder powder (total 100 mass %) were charged into a container and mixed with a planetary mixer to prepare a solder composition.
[0048] [Examples 2 to 9] A solder composition was obtained in the same manner as in Example 1, except that the materials were mixed according to the composition shown in Table 1. [Comparative Examples 1 to 3] A solder composition was obtained in the same manner as in Example 1, except that the materials were mixed according to the composition shown in Table 1.
[0049] <Evaluation of solder composition> The solder compositions were evaluated (for properties, heat sagging, and printability) by the following methods. The results are shown in Table 1. (1) Properties The solder composition was visually checked for gloss. Then, the solder composition was stirred at the center and sides of the container with a spatula to check for smoothness. The properties were then evaluated according to the following criteria. : No problems with gloss or smoothness. Good: No problem with gloss, but some problem with smoothness. Δ: There is a problem with at least one of the gloss and smoothness. ×: Problems with both gloss and smoothness. (2) Heated sauce A solder composition was printed on a test board (double-sided copper-clad laminate) using a metal mask having pattern holes arranged at 0.1 mm pitch from 0.1 mm to 1.2 mm, and heated at a temperature of 150°C for 1 minute. After heating, the test board was observed and the minimum spacing of the pattern holes at which the printed solder composition did not become integrated was measured. This measurement was performed on multiple pattern holes and the average was taken. Heat sagging was then evaluated according to the following criteria. ⊚: The average minimum spacing is 0.2 mm or less. ◯: The average minimum spacing is greater than 0.2 mm and not greater than 0.3 mm. △: The average minimum spacing is greater than 0.3 mm and equal to or less than 0.4 mm. ×: The average minimum spacing is 0.4 mm or more. (3) Printability A test board (FR4 substrate, solder resist opening diameter 75 μm) and a metal mask (thickness 30 μm, metal mask opening diameter 95 μm, pitch size 130 μm) having a pattern corresponding to this test board were used. The solder composition was printed on the test board with a urethane squeegee with a metal hardness of 90 and a printing angle of 60° using a printing device (product name: SP-0601, manufactured by Panasonic Factory Solutions Co., Ltd.). The test substrate after printing was observed using a metallurgical microscope to observe the proportion of the solder composition that was not transferred onto the Cu lands (9,800 locations) (non-transfer rate) and whether or not any areas of the Cu lands were visible. The printability was then evaluated according to the following criteria. A: 100% of the solder composition was transferred. ◯: The non-transfer rate is less than 0.1%. △: The non-transfer rate is 0.1% or more and less than 0.5%. ×: The non-transfer rate is 0.5% or more, or the solder composition is not transferred onto the board and there are some areas where the Cu land is visible.
[0050] [Table 1]
[0051] As is clear from the results shown in Table 1, it was confirmed that the solder compositions of the present invention (Examples 1 to 9) were good in all respects, including wetting of the QFN end face and viscosity stability during storage. Note that the solder compositions of Examples 1 to 4 do not contain a halogen-based activator, and are therefore non-halogen type solder compositions. Therefore, it was confirmed that the solder composition of the present invention, although being a halogen-free or non-halogen type, is excellent in both wettability and viscosity stability during storage. [Industrial Applicability]
[0052] The solder composition of the present invention can be suitably used in a technique for mounting electronic components on electronic substrates such as printed wiring boards of electronic devices.
Claims
1. A solder composition comprising: a flux composition including (A) a rosin-based resin, (B) an activator, and (C) a thixotropic agent; and (D) a solder powder, the component (C) contains (C1) an amide compound having a weight average molecular weight Mw of 500 or more and 2,500 or less, a number average molecular weight Mn of 500 or more and 1,500 or less, and a value of Mw / Mn of 1.2 or more and 2.5 or less, the component (C1) is an amide compound obtained by condensing an aliphatic monocarboxylic acid having 2 to 22 carbon atoms, including a hydroxyaliphatic monocarboxylic acid, an aliphatic dicarboxylic acid having 2 to 12 carbon atoms, and a diamine having 2 to 16 carbon atoms, The blending amount of the (A) component is 20% by mass or more and 70% by mass or less with respect to 100% by mass of the flux composition, The blending amount of the (B) component is 3 mass% or more and 25 mass% or less with respect to 100 mass% of the flux composition, The blending amount of the (C) component is 1 mass % or more and 25 mass % or less with respect to 100 mass % of the flux composition, The blending amount of the (C1) component is 0.1 mass % or more and 25 mass % or less with respect to 100 mass % of the flux composition, The blending amount of the (D) component is 65% by mass or more and 95% by mass or less with respect to 100% by mass of the solder composition. Solder composition.
2. The solder composition according to claim 1, The weight average molecular weight Mw of the (C1) component is 1,500 or more and 2,300 or less, the number average molecular weight Mn is 700 or more and 1,300 or less, and the Mw / Mn value is 1.35 or more and 2 or less. Solder composition.
3. The solder composition according to claim 1 or claim 2, The component (C1) is an amide compound obtained by condensing hydroxystearic acid, an aliphatic dicarboxylic acid having 2 to 12 carbon atoms, and hexamethylenediamine. Solder composition.
4. The solder composition according to any one of claims 1 to 3, Two or more of the (C1) components are used in combination. Solder composition.
5. A soldered portion comprising the solder composition according to any one of claims 1 to 4. Electronic board.
Citation Information
Patent Citations
Preparation of entangled cocoon filament
JP1983087330A
Solder composition for laser soldering and electronic substrate
JP2020044562A
Flux and solder paste
JP2020142271A
Flux and solder paste
JP2022080811A
Soldering flux and solder composition
WO2013191121A1