Cladding and its manufacturing method

A cladding method using explosive crimping and heat treatment creates a strong bond between alloys with differing hardnesses, addressing cracking and peeling issues, enhancing wear resistance and workability in manufacturing equipment.

JP7554270B2Active Publication Date: 2024-09-19ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022542611
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-14
Filing Date
2021-07-21
Publication Date
2024-09-19
Estimated Expiration
2041-07-21

AI Technical Summary

Technical Problem

Existing cladding technologies fail to provide a strong bond between alloys with significantly different hardness levels, leading to issues such as cracking, peeling, and reduced wear resistance and workability in manufacturing equipment.

Method used

A cladding method involving a first alloy with low hardness and high workability, bonded to a second alloy with higher hardness through explosive crimping, followed by quenching and tempering to achieve a hardness difference of HRC44 or more, ensuring a defect-free and strong interface.

Benefits of technology

The resulting cladding exhibits high wear resistance and workability, with a strong bonding interface that withstands harsh environments, reducing cracking and peeling, and is suitable for heavy machinery and construction equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554270000002
    Figure 0007554270000002
  • Figure 0007554270000004
    Figure 0007554270000004
  • Figure 0007554270000003
    Figure 0007554270000003
Patent Text Reader

Abstract

The present disclosure provides cladding in which at least two layers of alloys are joined, the cladding having high wear resistance, high workability, and excellent strength at the joining interface of the alloys. The cladding is composed of two or more layers including a first alloy and a second alloy joined to the first alloy. The hardness of the second alloy of the cladding is greater than that of the first alloy, and the difference in hardness between the first alloy and the second alloy is at least HRC 44. When a shearing test based on JIS G 0601 is performed on the cladding, the breakage is on the first alloy side.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a clad having first and second alloys joined together and a method for making the same. [Background technology]

[0002] In manufacturing equipment for resin and rubber products, various additives are added to mix and knead raw materials uniformly, so raw materials and parts of the equipment are always in contact with each other. In crushers used in fields such as recycling waste wood, waste plastic, and tires, the materials to be crushed and the equipment are always in contact with each other. In these manufacturing equipment and crushers, alloys with excellent wear resistance are required to extend the life of the equipment.

[0003] In manufacturing equipment and crushers, it is effective to increase the surface hardness of the alloy in order to improve wear resistance. Generally, high-hardness steel obtained by adding specific chemical components or alloys to carbon steel and then subjecting the steel to heat treatment such as quenching has been widely used as wear-resistant steel.

[0004] On the other hand, if the hardness of the alloy is increased to improve the wear resistance, problems arise such as the need for man-hours for drilling screw holes and cutting for attachment to the device body, and poor dimensional accuracy. In addition, when screwing is used for attachment to the device body, stress is concentrated at the screw fastening portion, which causes the high hardness alloy to crack. In addition, when alloys that have been heat-treated such as quenching are metallurgically fastened by welding instead of screwing, the alloy is re-quenched in the part that is locally heated by the welding heat, and the hardness increases significantly, which may lead to cracking. On the other hand, in the part where heat below the quenching temperature is transferred due to the welding heat, the alloy is annealed, which causes problems such as a decrease in hardness, making it difficult to apply it as a product.

[0005] For example, in manufacturing equipment such as kneaders and crushers, as shown in FIG. 1, the inner member (2) that pushes out raw materials and waste materials comes into violent contact with the wall surface of the extruder (3) and is exposed to a significant abrasion and sliding environment, so thick, high-hardness steel is required that can be used for a long time even if it wears out to a certain extent. On the other hand, the outer member (1) that fastens these does not require abrasion resistance and sliding resistance, and a soft alloy with good workability is required for mechanical fastening or metallurgical fastening. In other words, in manufacturing equipment such as the above, a clad in which alloys with extremely different hardnesses are firmly bonded together is required.

[0006] Therefore, there are some prior arts that attempt to solve the above problem by joining an alloy having high hardness and abrasion resistance to one side of an alloy having softness and high workability. For example, in Non-Patent Documents 1 and 2, an alloy having wear resistance is overlaid on one side of a general-purpose soft carbon steel. Therefore, although it is considered that these alloys are easy to process, cracks and defects occur during overlaid welding, and when used in manufacturing equipment, crushers, etc., the cracks may progress due to strong impact and sliding, and the cracked overlaid member may be mixed into the manufacturing equipment as an impurity. In addition, peeling may occur from the joint interface starting from the welding defect.

[0007] The clads disclosed in Patent Documents 1 and 2 are clads of a steel material having high hardness and wear resistance and a steel material having relatively low hardness, and mention imparting impact resistance. However, there is no description of the strength of the joint surface, and since the difference in hardness between the steel materials is small, the workability is poor. Furthermore, Patent Document 3 describes a clad of stainless steel having wear resistance and carbon steel. However, the hardness of stainless steel is low, and it is considered that the wear resistance is insufficient and it cannot withstand use in harsh environments where devices come into intense contact with each other.

[0008] In addition, in the clad embodiment disclosed in Patent Document 1, a metal powder having wear resistance is placed on a metal molded body and is integrated by hot pressing. However, it is considered that there are restrictions on the shape and size, and it is difficult to firmly bond metals having different mechanical properties by hot pressing. On the other hand, in the clad embodiment disclosed in Patent Documents 2 and 3, the clad is manufactured by hot rolling or cold rolling. However, it is considered that the heat input during hot rolling makes the steel material reach a state in which it has been subjected to quenching heat treatment, and if a temperature gradient occurs during this hot rolling and the hardness becomes insufficient, it is necessary to anneal once to restore the hardness, and then to perform quenching heat treatment again, which requires manufacturing man-hours and increases costs. In addition, even in the case of cold rolling, a high temperature is applied to the joining surface, but the steel material is not heated uniformly throughout, so that the above-mentioned reheating process may be required. Furthermore, since cold rolling is limited to the production of thin plates, it is impossible to manufacture relatively thick plates such as those used in kneading and crushing equipment. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2000-108246 A [Patent Document 2] JP 2003-301237 A [Patent Document 3] Japanese Patent Application Publication No. 4-182081 [Non-patent literature]

[0010] [Non-Patent Document 1] Tokuden Co., Ltd. product catalog "Tokuden TOP PLATE", [online], [searched on July 22, 2020], Internet <http: / / www.tokuden.co.jp / product / top_plate / index.html> [Non-Patent Document 2] Nikko Yozai Kogyo Co., Ltd. Product Catalog "Nichia Welding Rod Wear-Resistant Overlay Clad SUPER PLATE", [online], December 5, 2019, [Retrieved July 22, 2020], Internet <https: / / www.nikko-yozai.co.jp / pamhlet / > Summary of the Invention [Problem to be solved by the invention]

[0011] An object of the present disclosure is to provide a clad formed by bonding at least two alloy layers, which has high wear resistance and high workability, and has excellent strength at the alloy bonding interface. [Means for solving the problem]

[0012] As a result of intensive research aimed at solving the above problems, the inventors have newly discovered that it is possible to achieve both high levels of wear resistance and workability by joining an alloy (1) having low hardness and excellent workability to an alloy (2) having high hardness, as shown diagrammatically in FIG. 2. [1] A clad having two or more layers, comprising a first alloy and a second alloy joined to the first alloy, wherein the hardness of the second alloy is higher than that of the first alloy, the difference in hardness between the first alloy and the second alloy is HRC44 or more, and when a shear test of JIS G 0601 is performed on the clad, the clad breaks on the side of the first alloy. [2] 2. The clad according to item 1, wherein the clad has no defects at the bonding interface between the first alloy and the second alloy when inspected by the back echo method of ultrasonic inspection according to JIS G 0601. [3] 3. The cladding according to claim 1 or 2, wherein when subjected to a penetrant test in accordance with ASME BPVC-VIII, the surface of the cladding is free of indications, the cross section of the cladding is free of indications whose length exceeds three times its width, free of circular or elliptical indications whose size exceeds 5 mm, and free of four or more indications spaced 1.5 mm or less from end to end in a substantially straight line. [4] 4. The clad according to any one of items 1 to 3, wherein the hardness of the first alloy is HRC5 or less. [5] 5. The clad according to any one of items 1 to 4, wherein the first alloy and the second alloy are directly bonded to each other. [6] 6. The clad according to any one of items 1 to 5, wherein a wave height at a bonding interface between the first alloy and the second alloy is 30 μm or more and 100 μm or less. [7] Joining the first alloy and the second alloy by explosive bonding; hardening the second alloy by subjecting the joined second alloy to quenching and tempering heat treatment, so that the hardness of the second alloy is higher than that of the first alloy and the hardness difference between the first alloy and the second alloy is HRC44 or more; A method for manufacturing a cladding comprising: [8] Joining the first alloy and the second alloy by explosive bonding; A method for manufacturing a clad, comprising: subjecting the joined second alloy to heat treatment, i.e., solution treatment and aging treatment, to harden the second alloy, so that the hardness of the second alloy is higher than that of the first alloy, and the hardness difference between the first alloy and the second alloy is HRC44 or more. [9] A method for using a clad according to any one of items 1 to 6, comprising mechanically or metallurgically fastening the first alloy of the clad to an apparatus and exposing the second alloy to an environment in which it is subjected to an abrasive load. Effect of the Invention

[0013] According to the present disclosure, it is possible to provide a clad having high wear resistance, high workability, and excellent strength of the alloy bonding interface. Therefore, the wear-resistant clad according to the present disclosure can be used in vehicles such as heavy machinery, construction equipment, and structures that require high wear resistance and workability at the same time, for example, in applications that require one side to have high wear resistance and the other side to have high workability and weldability for fastening equipment, such as the wall surface of a manufacturing device or crusher shown in FIG. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a schematic diagram showing an example of using the clad according to the present disclosure in a manufacturing device such as an extrusion / kneading device. [Diagram 2] FIG. 2 is a schematic diagram showing the appearance of a cladding according to the present disclosure. [Diagram 3] 1 is a photograph for explaining the definition of wave height at a joint interface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Clad <Hardness difference> Hereinafter, an embodiment of the present disclosure (hereinafter, referred to as "the present embodiment") will be described in detail. The clad of this embodiment includes a first alloy and a second alloy bonded to the first alloy, and the hardness of the second alloy is higher than that of the first alloy, that is, the second alloy is an alloy having wear resistance, and the first alloy is an alloy having excellent workability and weldability. It is essential that the hardness difference between the first alloy and the second alloy is HRC (Rockwell hardness) 44 or more. In general kneaders and crushers, alloys with high hardness and wear resistance are used for components subjected to wear and sliding load. In order to prevent deterioration and wear due to wear and the resulting inclusion of impurities, it is preferable to use an alloy of HRC44 or more for the alloy (second alloy) subjected to wear and sliding load, because it can withstand long-term use even in a severe wear-resistant environment. On the other hand, if the hardness is less than HRC44, although it can withstand use for a certain period of time as an equipment component, its life is significantly reduced in a severe environment where high wear resistance is required. In addition, it is important that the other alloy (first alloy) of the clad has a sufficiently lower hardness than the second alloy in order to improve workability and weldability. Therefore, in order to achieve both high wear resistance and workability, the hardness difference between the first alloy and the second alloy is HRC44 or more.

[0016] For high workability, the hardness of the first alloy is preferably HRC 0 to 5, more preferably HRC 0 to 4, and even more preferably HRC 0 to 3. For improved wear resistance and crack prevention, the hardness of the second alloy is preferably HRC 44 to 75, more preferably HRC 48 to 70, and even more preferably HRC 50 to 65.

[0017] In order to achieve both high wear resistance and processability, the lower limit of the hardness difference between the first alloy and the second alloy may be preferably HRC45 or more, HRC46 or more, HRC47 or more, HRC48 or more, HRC49 or more, HRC50 or more, HRC51 or more, HRC52 or more, HRC53 or more, or HRC54 or more.

[0018] In this specification, the term "wear" is defined as a gradual weight loss phenomenon of a solid surface due to friction, and is a phenomenon in which surface material is removed by friction. Mechanically, wear occurs due to a combination of mechanical contact and metallic adhesion between metal surfaces moving relative to one another, and an alloy that can withstand this is defined as a "wear-resistant alloy." In general terms, it is known that the wear resistance of alloys that have been quenched and tempered, or solution-treated and aged is proportional to their hardness. The alloys used as the second alloy (wear-resistant alloy) are preferably carbon tool steels as specified in JIS G 4401, high-speed tool steels as specified in JIS G 4403, alloy tool steels as specified in JIS G 4404, corrosion-resistant and heat-resistant superalloys as specified in JIS G 4902, rolled materials of nickel and nickel alloys, and hot-rolled stainless steel plates as specified in JIS G 4304, such as SKD61. Examples of alloys that can be made wear-resistant by solution treatment and aging treatment include nickel alloys, preferably nickel alloys mainly containing nickel and containing chromium, iron, and carbon. "Mainly containing" means that it accounts for 50 mass% or more of the alloy composition. In addition, alloys that can be age-hardened (precipitation hardened) by hardening intermetallic compounds by precipitating from the structure are known as wear-resistant alloys, and these may also be used as wear-resistant alloys.

[0019] The alloy used as the first alloy is preferably a carbon steel or a low hardness alloy, more preferably a low carbon steel. The term "low carbon steel" refers to an alloy with a low carbon content among carbon steels, and is generally defined as an alloy with a carbon content (weight percent concentration) of 0.25% by weight or less. It is known that low carbon steel has a low carbon content, and therefore its properties do not change significantly with heat treatment. For example, when the entire clad is hardened by heat treatment such as quenching and tempering, or solution and aging treatment in order to impart wear resistance to the second alloy of the clad, if a steel material with a high carbon content is used for the first alloy, the first alloy may also be hardened by the heat treatment, and the workability may decrease. When low carbon steel with a low carbon content is used as the first alloy, it is difficult to harden even when heat treatment is performed, and therefore high workability can be maintained. As an example of low carbon steel, it is preferable to use one having a low carbon content among general structural rolled steel materials specified in JIS G 3101, such as SS400, rolled steel plate for welded structure specified in JIS G 3106, and carbon steel materials for mechanical structure specified in JIS G 4051. However, other alloys may be used as long as they have a low carbon content and are excellent in workability and weldability.

[0020] As a combination of the first alloy and the second alloy, in order to manufacture a clad that can achieve both wear resistance and workability at a higher level, it is effective to use a hardened steel that increases in hardness by quenching as the second alloy, preferably a hardened steel that is quenched from the austenite single phase region to obtain a martensite structure, and to use a low-carbon steel that is not easily altered by heat treatment, i.e., that increases in hardness only slightly, as the first alloy. It can be said that manufacturing a clad using a low-carbon steel as the first alloy has a large advantage in terms of reducing costs and processing man-hours, compared to constructing an apparatus using a single material of a wear-resistant alloy.

[0021] In this embodiment, when the second alloy and the first alloy are simply "joined", it includes both a structure in which the second alloy is directly joined to the surface of the first alloy, and a structure in which the second alloy is indirectly joined via one or more intermediate materials other than the first alloy and the second alloy. The material of the intermediate material is not limited to steel materials, and examples thereof include titanium and its alloys, nickel and its alloys, other metal materials and their alloys, and non-ferrous metal materials. When low carbon steel is used as the first alloy and hardened steel, which is hardened by quenching, is used as the second alloy, a material with high strength at high temperatures, such as nickel or a nickel alloy, can be used, and from the viewpoint of the mechanical strength of the bonding interface, it is more preferable that the second alloy is directly bonded to the surface of the first alloy. In the technical field of the clad, among the alloys to be bonded, a relatively thick alloy is sometimes called a "base material" and a relatively thin alloy is sometimes called a "clad material". In this disclosure, the first alloy may be the base material and the second alloy may be the clad material, or the second alloy may be the base material and the first alloy may be the clad material.

[0022] <Joining interface> The clad of this embodiment breaks on the first alloy side when a shear test according to JIS G 0601 is carried out. That is, it is preferable that the first alloy, which has a relatively low hardness, breaks in the shear test before peeling occurs at the bonding interface between the first alloy and the second alloy. When an intermediate material is interposed between the first alloy and the second alloy, "breaks on the first alloy side" means that the first alloy or the intermediate material, which has a relatively low hardness, breaks before peeling occurs at the bonding interface between the second alloy and the intermediate material, or the bonding interface between the intermediate material and the first alloy. In other words, the mechanical strength of the bonding interface in the shear test according to JIS G 0601 is higher than the mechanical strength of the intermediate material and the first alloy. This feature makes the bonding between the first alloy and the second alloy stronger, and can withstand long-term use even in a severe wear-resistant environment. The "shear strength" is a value obtained from the results of a shear strength test performed according to the shear strength test specified in the test method for clads in JIS G 0601. The shear strength of the clad of this embodiment, when a low carbon steel such as SS400 is used as the first alloy, is higher than 230 MPa, preferably higher than 400 MPa, more preferably 410 MPa or more, and even more preferably 420 MPa or more.

[0023] In a shear test, a method for configuring the cladding to break on the first alloy side rather than peeling at the bonding interface includes adjusting the wave height at the bonding interface between the first alloy and the second alloy to preferably 30 μm to 1000 μm (1 mm), more preferably 40 μm to 800 μm, and even more preferably 50 μm to 600 μm. When the wave height is greater than 30 μm, the bonding area becomes large, resulting in a strong bonding interface. In addition, when the wave height is 1000 μm or less, it is possible to suppress the occurrence of microcracks due to the formation of an alloy layer at the bonding interface caused by plastic deformation or thermal effects during bonding, which makes the bonded portion hard and brittle. In addition, in the case where an intermediate material is interposed between the first alloy and the second alloy, it is preferable to adjust the wave height at the bonding interface between the first alloy and the intermediate material and the bonding interface between the intermediate material and the second alloy to preferably 30 μm to 1000 μm (1 mm), more preferably 40 μm to 800 μm, and even more preferably 50 μm to 600 μm. In this specification, the "wave height" at the bonding interface indicates the difference in height from the top to the bottom of the waveform at the bonding interface, as shown in FIG. 3. The waveform at the bonding interface can be formed by bonding the first alloy and the second alloy by explosive bonding. In this embodiment, the wave height is measured by processing the explosively bonded clad into a required shape and measuring the cross section including the bonding part using an electron microscope. The measurement is performed by measuring about 10 arbitrary points at the bonding interface and calculating the average value.

[0024] <Defects / Indications> The clad of this embodiment preferably has no defects at the bonding interface between the first alloy and the second alloy when inspected by the bottom echo method of ultrasonic inspection according to JIS G 0601. The absence of defects at the bonding interface between the first alloy and the second alloy makes the bonding between the first alloy and the second alloy stronger, and the clad can withstand long-term use even in a severe wear-resistant environment.

[0025] The clad of this embodiment preferably has no indications on the surface of the clad when the ASME BPVC-VIII penetrant test is performed. In addition, it is preferable that the cross section of the clad has no indications whose length exceeds three times the width, no circular or elliptical indications whose length exceeds 5 mm, and no four or more indications arranged in a substantially straight line with an interval of 1.5 mm or less from end to end. An indication means a pattern in which the penetrant used in the penetrant test penetrates into scratches present on the observation surface and becomes visible. The penetrant is typically red. The absence of indications means that these scratches are not visible. The size of the circular or elliptical indication means the maximum dimension (i.e., the diameter of the circle or the major axis of the ellipse) when the indication is assumed to be a circle or an ellipse. It is preferable that the clad has no continuous indications, but if there are indications, it is preferable that there are no more than four continuous indications arranged in a substantially straight line with an interval of 1.5 mm or less. This allows the clad to withstand long-term use even in a severe wear-resistant environment.

[0026] <Method of manufacturing cladding> Explosive bonding In the manufacturing method of the clad of this embodiment, it is important to perform a heat treatment after joining the second alloy to the first alloy to harden the second alloy. Since the hardening heat treatment is performed after joining, the joining method is preferably cold joining without heat load, and more preferably, joining by explosive bonding. When the second alloy is hardened and then joined to the first alloy in cold, there is a risk that the wear-resistant alloy of the second alloy may crack. However, by joining the second alloy to the first alloy in cold before hardening heat treatment and then hardening heat treatment, high hardness can be imparted to the second alloy and a strong bond can be obtained without cracking. For example, the clad manufactured by explosive bonding may be subjected to non-heated cold rolling after explosive bonding to produce a clad with a predetermined thickness, and then heat treatment may be performed. When joining alloys that are difficult to join directly, or for cladding that will be subject to a large thermal load when used as a product, an intermediate material may be used between the alloys. This is not limited to steel materials, but examples include titanium and its alloys, nickel and its alloys, other metal materials and their alloys, and non-ferrous metal materials.

[0027] When one or more intermediate materials are present between the first alloy and the second alloy, the respective materials may be joined simultaneously in a single explosive bonding operation, or the intermediate material may be explosively bonded to the first alloy, and then the second alloy may be explosively bonded onto the intermediate material. Alternatively, the intermediate material may be explosively bonded to the second alloy, and then the second alloy may be explosively bonded to the first alloy. Alternatively, the first alloy, the intermediate material, and the second alloy may be explosively bonded simultaneously.

[0028] Explosive bonding is a metal joining method that uses the high pressure of explosives, and is a technology that can firmly join dissimilar metals. The main features of this technology are that it can join relatively thick materials over 10 mm without applying almost any heat to the metal materials, and can firmly join metals with combinations and thicknesses that cannot be joined by normal methods. As a mechanism for strong joining, it is known that the joint interface of metals joined by explosive bonding exhibits a unique wavy shape, which is said to be due to the fact that the joint area is larger than that of a straight joint interface. The height of the waves (wave height) is as described above.

[0029] The explosive used in explosive bonding is a type of explosive that generates a detonation wave. In order to firmly bond metal plates, it is preferable to use an explosive with an explosion speed of 1000 m / s or more, and it is more preferable to use an explosive with an explosion speed of 1,500 m to 3,000 m / s, which is 1 / 3 to 1 / 2 the sound speed of metal, in order to obtain a more optimal bonding force. Specific examples of explosives include ammonium nitrate, nitrate esters such as PETN (pentaerythritol tetranitrate) and nitroglycerin, nitro compounds such as TNT (trinitrotoluene), and nitramines such as cyclotrimethylenetrinitramine and cyclotetramethylenetetranitramine. These may be used alone or in combination with other explosive components or other components other than explosives.

[0030] <Heat Treatment> The heat treatment in this embodiment refers to a hardening heat treatment of the second alloy performed after explosive bonding. The heat treatment may be performed on the joined second alloy side to mainly harden only the second alloy and adjust the hardness difference to HRC44 or more. Preferably, a material such as low carbon steel that is difficult to harden by heat treatment is used as the first alloy, and while the first alloy and the second alloy are entirely heat treated, mainly the second alloy is hardened and the hardness difference is adjusted to HRC44 or more. The heat treatment method generally includes a method of performing a quench hardening treatment by cooling under conditions such that the alloy is transformed into martensite or bainite after austenitization; a method of performing a tempering treatment in which the alloy is soaked at a specific temperature one or more times after the above quench hardening or heat treatment to obtain the required properties, and then cooled at an appropriate rate; and a method of performing an age hardening treatment in which the properties of the alloy (e.g., hardness, etc.) change over time after quenching, cold working, etc. The method of heat treatment and its temperature and time are specified by JIS standards, etc. For example, in the case of SKD61, an alloy tool steel material specified in JIS G 4404, a steel material of HRC50 or more can be obtained by quenching at a temperature of 1030°C, air cooling, and air-cooled tempering at 550°C. In this embodiment, heat treatment is performed after explosive bonding, but as long as the hardness of the second alloy is higher than that of the first alloy after heat treatment and the hardness difference between the first alloy and the second alloy is HRC44 or more, other alloys than SKD61 may be used. In the case of imparting a higher hardness to the second alloy, for example, surface treatments such as carburizing quenching, flame quenching, high-frequency quenching, nitriding, and salt bath soft nitriding treatment specified in JIS G 0201 may be combined. In one embodiment, the hardened layer is obtained from the surface by several mm or more compared to the above-mentioned carburizing quenching, flame quenching, high-frequency quenching, and nitriding, so that the life of the manufacturing equipment can be extended. Taking into consideration the service life during use, the thickness of the hardened layer is desirably 3 mm or more from the surface, more desirably 5 mm or more from the surface, and further desirably the second alloy is hardened throughout the entirety. EXAMPLES

[0031] Examples and comparative examples of the present disclosure are shown below, but the present disclosure is not limited to these examples and comparative examples.

[0032] Measurement and evaluation methods <Hardness and hardness difference> The HRC (Rockwell hardness) was measured in accordance with the Rockwell hardness test of JIS Z 2245.

[0033] <Shear test> The test was specified in accordance with the test method for clads in JIS G 0601. After the shear test, the test piece was observed, and if the first alloy was attached to the second alloy, it was judged that the fracture occurred on the first alloy side. If the first alloy was not attached to the second alloy and the bonding surface was exposed, it was judged that the fracture occurred at the bonding interface. In addition, in the case of clads having an intermediate material, if the intermediate material was attached to the second alloy or if the first alloy was attached to the intermediate material, it can be judged that the fracture occurred on the first alloy side. Also, if the intermediate material was not attached to the second alloy and the bonding surface between the two was exposed, or if the first alloy was not attached to the intermediate material and the bonding surface between the two was exposed, it can be judged that the fracture occurred at the bonding interface.

[0034] Wave height The explosively bonded clad was processed into a 20x20x20 block shape including the bonded interface, and the cross section including the bonded part was measured using an electron microscope. Measurements were taken at about 10 random points on the bonded interface, and the average value was calculated.

[0035] <Ultrasonic testing> The ultrasonic testing was carried out in accordance with the ultrasonic testing method stipulated in the test method for clad steel in JIS G 0601. When the horizontal axis shows the propagation time and the vertical axis shows the sound pressure, and the bottom echo height is set to 80%, if no defect echo is detected with an interface echo height of 40% or more, it is determined that there is no defect.

[0036] <Penetrant testing> The surface and cross-section of the cladding were subjected to penetrant testing in accordance with ASME BPVC-VIII-1 or equivalent standards. The cross-section of the cladding was milled or polished and the observation surface was cleaned before testing. The size and number of red indications detected were measured using calipers and other measuring instruments.

[0037] Example 1 As the first alloy, which has excellent workability and weldability, SS400, a 100mm thick general structural rolled steel material specified in JIS G 3101, was used, and as the second alloy, SKD61, an 8mm thick alloy tool steel material specified in JIS G 4404, was used as an abrasion-resistant alloy. A specified gap was provided between the second alloy and the first alloy, and a powdered explosive mainly composed of ammonium nitrate was placed at a specified thickness, and the explosive was detonated with a 6mm diameter detonator to perform explosive bonding. As a result, the second alloy and the first alloy were joined, and the ultrasonic flaw detection test (JIS G 0601, bottom echo method) determined that the entire surface was joined without any defects.

[0038] Next, the clad produced by explosive bonding was quenched at 1,030°C and then tempered twice at 550°C. The surface hardness of the second alloy (SKD61) became HRC50 or higher, while the first alloy (SS400) maintained its initial hardness of HRC0-1.

[0039] Next, ultrasonic testing (JIS G 0601, bottom echo method) was conducted on the cladding after the above heat treatment, and it was determined to be a defect-free full-surface bond. In addition, a penetrant test (ASME BPVC-VIII-1) was conducted on the cross-section of the joint surface of the cladding after the heat treatment, and no indications were detected on the surface or cross-section of the cladding, and the entire surface was maintained as a bond without any defects or peeling. The wave height at the joint interface was 450μm.

[0040] Next, a total of four test samples were cut out from the clad and subjected to shear testing (JIS G 0601). As a result, as shown in Table 1, the average shear strength was about 420 MPa, and all of the fracture occurred on the first alloy side of SS400, indicating that the bonded interface had sufficient strength.

[0041] In order to install the clad in the manufacturing equipment, cutting was performed on the outer circumference and in the thickness direction of the clad, and screw holes and welding were performed on the SS400 side. It was found that the clad could be easily cut and welded into the desired shape, and there was no problem in using it as a product. From the above results, it was confirmed that the clad of Example 1 has wear resistance and high workability.

[0042] Example 2 As the first alloy, which has excellent workability and weldability, SM490A with a thickness of 20 mm, which is a rolled steel plate for welding structure specified in JIS G 3106, was used, and as the second alloy, SKD1 with a thickness of 6 mm, which is an alloy tool steel material specified in JIS G 4404 for wear-resistant alloys, was used. A specified gap was provided between the second alloy and the first alloy, and a powdered explosive mainly composed of ammonium nitrate was placed at a specified thickness, and the explosive was detonated with a 6 mm diameter detonator to perform explosive bonding. As a result, the second alloy and the first alloy could be joined, and the result of ultrasonic testing (JIS G 0601, bottom echo method) determined that the entire surface was joined without any defects.

[0043] Next, the clad produced by explosive bonding was quenched at 970°C and then subjected to a single tempering heat treatment at 180°C. The surface hardness of the second alloy (SKD1) became HRC63 or higher, while the first alloy (SM490A) maintained its initial hardness of HRC0-1.

[0044] Next, ultrasonic testing (JIS G 0601, bottom echo method) was conducted on the cladding after the above heat treatment, and it was determined to be a defect-free full-surface bond. In addition, a penetrant test (ASME BPVC-VIII-1) was conducted on the cross-section of the joint surface of the cladding after the heat treatment, and no indications were detected on the surface or cross-section of the cladding, and the entire surface was maintained as a bond without any defects or peeling. The wave height at the joint interface was 620 μm.

[0045] Next, a total of four test samples were cut out from the clad and subjected to a shear test (JIS G 0601). As a result, as shown in Table 1, the average shear strength was about 455 MPa, and all of the fracture occurred on the first alloy side of SM490A, indicating that the bonded interface had sufficient strength.

[0046] In order to install the clad in the manufacturing equipment, cutting was performed on the outer circumference and in the thickness direction of the clad, and screw holes and welding were performed on the SM490A side. It was found that the clad could be easily cut and welded into the desired shape, and there was no problem in using it as a product. From the above results, it was confirmed that the clad of Example 2 has wear resistance and high workability.

[0047] Example 3 As the first alloy, which has excellent workability and weldability, SS400, a 55mm thick general structural rolled steel specified in JIS G 3101, was used, and as the second alloy, SUS420J2, a 10mm thick hot-rolled stainless steel plate specified in JIS G 4304, was used as an abrasion-resistant alloy. A specified gap was provided between the second alloy and the first alloy, and a powdered explosive mainly composed of ammonium nitrate was placed at a specified thickness, and the explosive was detonated with a 6mm diameter detonator to perform explosive bonding. As a result, the second alloy and the first alloy could be joined, and the ultrasonic flaw detection test (JIS G 0601, bottom echo method) determined that the entire surface was joined without any defects.

[0048] Next, the clad produced by explosive bonding was quenched at 1030°C and then subjected to a single tempering heat treatment at 300°C. As a result, the surface hardness of the second alloy (SUS420J2) became HRC44 or higher, while the first alloy (SS400) maintained its initial hardness of HRC0-1.

[0049] Next, ultrasonic testing (JIS G 0601, bottom echo method) was conducted on the cladding after the above heat treatment, and it was determined to be a defect-free full-surface bond. In addition, a penetrant test (ASME BPVC-VIII-1) was conducted on the cross-section of the joint surface of the cladding after the heat treatment, and no indications were detected on the surface or cross-section of the cladding, and the entire surface was maintained as a bond without any defects or peeling. The wave height at the joint interface was 250 μm.

[0050] Next, a total of four test samples were cut out from the clad and subjected to shear testing (JIS G 0601). As a result, as shown in Table 1, the average shear strength was about 445 MPa, and all of the fracture occurred on the first alloy side of SS400, indicating that the bonded interface had sufficient strength.

[0051] In order to install the clad in the manufacturing equipment, cutting was performed on the outer circumference and in the thickness direction of the clad, and screw holes and welding were performed on the SS400 side. It was found that the clad could be easily cut and welded into the desired shape, and there was no problem in using it as a product. From the above results, it was confirmed that the clad of Example 3 has wear resistance and high workability.

[0052] Example 4 As the first alloy, which has excellent workability and weldability, SM490A, 30 mm thick, which is a rolled steel plate for welded structures specified in JIS G 3106, was used, and as the second alloy, NCF718, 10 mm thick, which is a corrosion-resistant and heat-resistant superalloy, nickel and nickel alloy rolled material specified in JIS G 4902, was used as an abrasion-resistant alloy. A specified gap was provided between the second alloy and the first alloy, and a powdered explosive mainly composed of ammonium nitrate was placed at a specified thickness, and the explosive was detonated with a 6 mm diameter detonator to perform explosive bonding. As a result, the second alloy and the first alloy could be joined, and the result of ultrasonic testing (JIS G 0601, bottom echo method) determined that the entire surface was joined without any defects.

[0053] Next, the clad produced by explosive bonding was solutionized at 1000°C, and then heat-treated by aging at 718°C and 620°C. The surface hardness of the second alloy (NCF718) became HRC47 or higher, while the first alloy (SM490A) maintained its initial hardness of HRC0-1.

[0054] Next, ultrasonic testing (JIS G 0601, bottom echo method) was conducted on the cladding after the above heat treatment, and it was determined to be a defect-free full-surface bond. In addition, a penetrant test (ASME BPVC-VIII-1) was conducted on the cross-section of the joint surface of the cladding after the heat treatment, and no indications were detected on the surface or cross-section of the cladding, and the entire surface was maintained as a bond without any defects or peeling. The wave height at the joint interface was 130 μm.

[0055] Next, a total of four test samples were cut out from the clad and subjected to shear testing (JIS G 0601). As a result, as shown in Table 1, the average shear strength was about 510 MPa, and all of the fracture occurred on the side of the first alloy material, SA490A, indicating that the bond interface had sufficient strength.

[0056] In order to install the clad in the manufacturing equipment, cutting was performed on the outer circumference and thickness direction of the clad material, and screw holes and welding were performed on the SM490A side. It was found that the clad could be easily cut and welded into the desired shape, and there was no problem in using it as a product. From the above results, it was confirmed that the clad of Example 4 has wear resistance and high workability.

[0057] Comparative Example 1 The basic conditions, explosive bonding conditions, and heat treatment conditions were the same as those in Example 1, but the manufacturing process of Example 1 was reversed. That is, when explosive bonding was performed after quenching and tempering heat treatment, although bonding between the second alloy and the first alloy was achieved, numerous cracks were observed on the surface of the wear-resistant alloy, which was the second alloy, and it was not usable as a product.

[0058] Comparative Example 2 The first alloy was SUS304, a hot-rolled stainless steel plate with a thickness of 10 mm, as specified in JIS G 4304, and the second alloy was SKD11, a wear-resistant alloy with a thickness of 5 mm, as specified in JIS G 4404. A specified gap was provided between the second alloy and the first alloy, and a powdered explosive mainly composed of ammonium nitrate was placed at a specified thickness, and the explosive was detonated with a 6 mm diameter detonator to perform explosive bonding. As a result, the second alloy and the first alloy were bonded, and an ultrasonic flaw detection test (JIS G 0601, bottom echo method) determined that the bond was complete and free of defects.

[0059] Next, the clad produced by explosive bonding was quenched at 1030°C and then subjected to a single tempering heat treatment at 180°C. The surface hardness of the second alloy (SKD11) became HRC59 or higher, and the surface hardness of the first alloy (SUS304) increased from the initial hardness to HRC26.

[0060] Next, ultrasonic testing (JIS G 0601, bottom echo method) was conducted on the cladding after the above heat treatment, and it was determined to be a defect-free full-surface bond. In addition, a penetrant test (ASME BPVC-VIII-1) was conducted on the cross-section of the joint surface of the cladding after the heat treatment, and no indications were detected on the surface or cross-section of the cladding, and the entire surface was maintained as a bond without any defects or peeling. The wave height at the joint interface was 100 μm.

[0061] Next, a total of four test samples were cut out from the clad and subjected to shear testing (JIS G 0601). As a result, as shown in Table 1, the average shear strength was about 550 MPa, and all of the fracture occurred on the first alloy side of SUS304, indicating that the bonded interface had sufficient strength.

[0062] In order to install the clad in the manufacturing equipment, cutting was carried out on the outer periphery of the clad and in the plate thickness direction, and screw holes and welding were carried out on the SUS304 side. However, because the SUS304 itself is very hard, it was difficult to process it into the specified shape, which resulted in increased processing time and weld cracks, making it unusable as a product.

[0063] [Table 1] [Industrial Applicability]

[0064] The clad of the present disclosure can be used as a component for kneaders for manufacturing equipment, extrusion components for crushers and the like, components that come into contact with other equipment, components that reciprocate with pistons, and other heavy machinery and industrial equipment components that crush and transport high-hardness components and materials. [Explanation of symbols]

[0065] 1. Soft steel 2. High-hardness steel 3. Extruder

Claims

1. A clad having two or more layers, comprising a first alloy and a second alloy bonded to the first alloy, wherein the hardness of the second alloy is higher than that of the first alloy, and the difference in hardness between the first alloy and the second alloy is HRC44 or more, and when a shear test of JIS G 0601 is performed on the clad, the clad breaks on the first alloy side, and the second alloy is thinner than the first alloy.

2. The clad according to claim 1 , wherein the clad is free of defects at a bonding interface between the first alloy and the second alloy when inspected by a back echo method of ultrasonic inspection according to JIS G 0601.

3. 3. The clad according to claim 1 or 2, wherein, when subjected to ASME BPVC-VIII penetrant testing, the clad has no indications on its surface, no indications in its cross section whose length exceeds three times its width, no circular or elliptical indications whose size exceeds 5 mm, and no indications that are spaced 1.5 mm or less apart from end to end in a substantially straight line.

4. The clad according to any one of claims 1 to 3, wherein the hardness of the first alloy is HRC 5 or less.

5. The clad according to any one of claims 1 to 4, wherein the first alloy and the second alloy are directly bonded.

6. The clad according to any one of claims 1 to 5, wherein a wave height at a bonding interface between the first alloy and the second alloy is 30 µm or more and 1000 µm or less.

7. Joining a first alloy and a second alloy thinner than the first alloy by explosive bonding; hardening the second alloy by subjecting the joined second alloy to quenching and tempering heat treatment, thereby making the hardness of the second alloy higher than that of the first alloy and making the hardness difference between the first alloy and the second alloy HRC 44 or more; A method for manufacturing a cladding comprising:

8. A method for manufacturing a clad, comprising: joining a first alloy and a second alloy that is thinner than the first alloy by explosive bonding; and performing heat treatment, including solution treatment and aging treatment, on the joined second alloy to harden the second alloy, so that the hardness of the second alloy is higher than that of the first alloy and the hardness difference between the first alloy and the second alloy is HRC 44 or more.

9. A method of using the clad according to any one of claims 1 to 6, comprising mechanically or metallurgically fastening the first alloy to a device and exposing the second alloy to an environment subject to abrasive loads.

Citation Information

Patent Citations

  • JP1971004060Y1

  • Manufacture of wear resistant member

    JP1992182081A

  • Explosive welded clad material and its production

    JP1995185840A

  • Clad material having high shock resistant property even after heat treatment, and worked member thereof

    JP2000108246A

  • Clad material and bending mold using the same

    JP2003301237A