Electromagnetic wave shielding moldings
A composite plastic material using carbon fibers within a specific length range addresses the reuse challenges of ASR, providing enhanced electromagnetic shielding and antistatic properties for electronic device applications.
Patent Information
- Application Number
- JP2020175915
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-20
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-10-20
AI Technical Summary
Plastic components from automobile shredder residue (ASR) are difficult to reuse due to their complex composition and lack of electrical conductivity and antistatic properties, limiting their application in electromagnetic shielding and antistatic functions, while carbon fiber reinforced resins face challenges in recycling and maintaining strength.
A composite plastic material is developed using plastic materials from automobile parts, incorporating carbon fibers with a specific length range (105 μm to 20 mm) and optionally carbon black and talc, enhancing electromagnetic shielding and antistatic properties.
The composite plastic material achieves excellent electromagnetic shielding and antistatic properties, with improved mechanical strength and conductivity, suitable for various electronic device housings and components.
Smart Images

Figure 0007554463000012 
Figure 0007554463000005 
Figure 0007554463000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite plastic material that can be produced by reusing plastic materials derived from automobile parts, such as plastic components contained in automobile shredder residue (ASR), which is generated in large quantities when automobiles are discarded. [Background technology]
[0002] Traditionally, used automobiles are pressed and shredded after valuable parts such as batteries, engines, and tires are removed, and are reused as scrap iron. During this shredding process, shredder dust containing a mixture of plastics, rubber, iron, aluminum, copper, etc. is generated. About 200 kg of shredder dust is generated when shredding one used automobile weighing about 1 ton, and about 1 million tons of shredder dust is generated from used automobiles every year in Japan. This shredder dust is separated according to the Automobile Recycling Law, and metals and glass are being reused. However, plastics and rubber are difficult to reuse, so they are either disposed of in landfills or burned and melted in waste incinerators.
[0003] Since the plastic components in ASR have a complex composition and are black, gravity separation and optical separation are difficult, and most of them have been incinerated. However, in recent years, ASR separation technology has improved, and not only is it possible to separate foreign matter such as rubber and wood chips, but a grade separation technology according to the amount of inorganic filler components such as talc has also been disclosed (see Non-Patent Document 1). However, since the separated ASR has inferior mechanical properties compared to virgin resin, its reuse is currently not widespread. Therefore, the recovered, separated, and grade-separated ASR is required to have added-value performance and / or functions similar to virgin resin. In addition, many plastic parts used in automotive parts contain carbon black as a filler, but when reused as a plastic material, it hardly exhibits the necessary conductivity or antistatic properties as it is. Therefore, some kind of treatment is required to impart functions such as electromagnetic shielding performance and antistatic properties required for various applications.
[0004] On the other hand, resin materials reinforced with carbon fibers are currently used in aircraft fuselages, etc., but are expected to be used in various structural material fields in the future. To reduce the weight of automobiles, carbon fiber reinforced resins are predicted to be widely used as exterior panel materials for automobiles (see Non-Patent Document 2).
[0005] However, since it is not always possible to guarantee that used carbon fiber reinforced resin will retain its strength, it is difficult to reuse it as a structural material, and it is also difficult to crush it for recycling. For these reasons, material recycling of carbon fiber reinforced resin materials has not progressed very much at present. [Prior art documents] [Non-patent literature]
[0006] [Non-Patent Document 1] FY2015 Low Carbon 3R Technology and System Demonstration Project (Creating a mechanism for recycling materials from ASR) Report (February 29, 2016, Toyota Tsusho Corporation, https: / / www.env.go.jp / recycle / car / pdfs / h27_report01_mat05.pdf) [Non-Patent Document 2] Journal of the Japan Society for Precision Engineering, Vol. 81, No. 6, pp. 489-493, 2015. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a new composite plastic material using a plastic material derived from an automobile part. [Means for solving the problem]
[0008] The present inventors have proposed a method for producing a composite plastic material having high strength, electromagnetic shielding performance, and antistatic properties using plastic materials derived from automotive parts (Patent Application No. 2020-072374).
[0009] The inventors, in the course of further intensive research into composite plastic materials using plastic materials derived from automobile parts, discovered that the carbon fiber length changes during processing from the raw materials to the actual final product, and that this change in carbon fiber length significantly affects the electromagnetic shielding properties. As a result of further intensive research, the inventors discovered that by setting the carbon fiber length within a specific range, excellent electromagnetic shielding properties can be reliably obtained, and thus completed the present invention.
[0010] That is, the present invention is as follows. [1] A composite plastic material comprising: (a) a plastic material derived from an automobile part; and (b) one or both of carbon fiber and a carbon fiber-containing resin material containing carbon fiber and a resin component, A composite plastic material characterized in that the volume average fiber length of the carbon fibers is 105 μm or more and 20 mm or less.
[0011] [2] The composite plastic material according to [1] above, characterized in that the number average fiber length of the carbon fibers is 80 μm or more and 15 mm or less. [3] The composite plastic material according to the above [1] or [2], characterized in that a mass ratio of the resin component of the composite plastic material to the carbon fiber is 99:1 to 60:40. [4] The composite plastic material according to any one of the above [1] to [3], characterized in that the plastic material derived from automobile parts (a) is a plastic material derived from automobile shredder residue. [5] The composite plastic material according to any one of the above [1] to [4], characterized in that the carbon fiber-containing resin material (b) is derived from a waste resin material containing carbon fibers.
[0012] [6] The composite plastic material according to any one of the above [1] to [5], further comprising a compatibilizer. [7] The composite plastic material according to any one of the above [1] to [6], characterized in that it contains carbon black. [8] The composite plastic material according to any one of the above [1] to [7], further comprising talc.
[0013] [9] An electromagnetic wave shielding molded article comprising the composite plastic material according to any one of the above [1] to [8]. Effect of the Invention
[0014] The composite plastic material of the present invention has excellent electromagnetic wave shielding properties. [Brief description of the drawings]
[0015] [Figure 1] This is an electron microscope image of carbon fibers (mixed once) contained in a composite plastic material. [Diagram 2] This is an electron microscope image of carbon fibers (mixed twice) contained in a composite plastic material. [Diagram 3] This is an electron microscope image of carbon fibers (kneaded three times) contained in a composite plastic material. [Figure 4] This is an electron microscope image of carbon fibers (kneaded four times) contained in a composite plastic material. [Diagram 5] 1 is a graph showing the electromagnetic wave shielding performance of a composite plastic material (mixed once). [Figure 6] 1 is a graph showing the electromagnetic wave shielding performance of a composite plastic material (mixed twice). [Figure 7] 1 is a graph showing the electromagnetic wave shielding performance of a composite plastic material (mixed three times). [Figure 8] 1 is a graph showing the electromagnetic wave shielding performance of a composite plastic material (mixed four times). [Figure 9] 1 is a graph showing the electromagnetic wave shielding performance of only plastic material derived from automobile parts that does not contain carbon fiber (mixed once). [Figure 10] 1 is a graph showing the volume resistivity and surface resistivity of composite plastic materials (mixed 1 to 4 times). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The composite plastic material of the present invention is characterized in that it contains (a) a plastic material derived from an automobile part, and (b) one or both of carbon fibers and a carbon fiber-containing resin material containing carbon fibers and a resin component, and the volume average fiber length of the carbon fibers is 105 μm or more and 20 mm or less.
[0017] That is, the plastic material of the present invention may include an embodiment comprising (a) a plastic material derived from automobile parts and (b) carbon fiber, an embodiment comprising (a) a plastic material derived from automobile parts and (b) a carbon fiber-containing resin material containing carbon fiber and a resin component, and an embodiment comprising (a) a plastic material derived from automobile parts and (b) carbon fiber, as well as a carbon fiber-containing resin material containing carbon fiber and a resin component.
[0018] Here, "plastic material" means a material that contains a thermoplastic resin as a main component, melts or softens when heated, and can easily flow or plastically deform when stress is applied. "Composite" means a mixture of a heat-meltable plastic material and an infusible or insoluble component, such as an inorganic filler component such as talc contained in plastics derived from automobile parts, an organic filler component such as carbon black, or a carbon fiber component or a thermosetting resin component in a carbon fiber-containing resin material. "Resin" includes thermoplastic resins and thermosetting resins.
[0019] The composite plastic material of the present invention has excellent electromagnetic shielding properties. In other words, if processing is performed without taking into consideration the carbon fiber length, there may be cases where sufficient electromagnetic shielding properties cannot be obtained, but the composite plastic material of the present invention containing carbon fibers having a fiber length within the specified range certainly exhibits excellent electromagnetic shielding properties. In addition, the composite plastic material of the present invention also has excellent antistatic properties. In addition, it also has excellent electrical conductivity and mechanical strength. Therefore, the composite plastic material of the present invention is useful as a material for an electromagnetic shielding molded product.
[0020] Here, "electromagnetic shielding performance" refers to the ability of a partition to limit the flow of electromagnetic fields between two locations separated by the partition. Electromagnetic shielding performance for blocking radio frequency electromagnetic waves is also known as RF shielding.
[0021] Additionally, "antistatic" refers to preventing static electricity from building up. Generally, plastics are prone to static electricity (static charge), and static electricity on plastic films can easily cause problems at each stage of the manufacturing process, secondary processing, and final product. For example, it is known that if a plastic film becomes statically charged while in a bag, it will attract surrounding dust and foreign matter, making the bag more susceptible to contamination.
[0022] Examples of the "molded product" include pellets obtained by extruding a molten material through a die, cooling the resulting strand-like material, and cutting the strand-like material into short pieces; three-dimensional products obtained by injecting a molten material into a pre-designed mold and cooling it; sheet- or film-like products obtained by extruding a molten material through a T-die or by reheating and melting pellets and pressing them; and roll- or strip-like products obtained by melting a heated and molten roll into a sheet and stretching the sheet.
[0023] In addition, the "plastic material derived from automobile parts" in the present invention refers to non-standard parts produced during the manufacture of automobile parts, waste products generated during repairs, etc., and plastic components derived from scrapped automobiles which automobile manufacturers are obligated to take back and recycle under the Automobile Recycling Law that came into effect in 2005. Specifically, the plastic material derived from automobile parts is a plastic component obtained by separating the residue remaining after useful metals and glass are recovered from ASR obtained by removing airbags, fluorocarbons, doors, engines, etc. from used automobiles and shredding them, from which rubber, fabric, etc. are separated. Most of the plastic materials used in automotive parts are thermoplastic resins, specifically, polyolefins such as polyethylene and polypropylene; styrene-based resins such as polystyrene, acrylonitrile-butadiene-styrene (ABS) resin, acrylonitrile-styrene (AS) resin, and methyl methacrylate-butadiene-styrene (MBS) resin; aromatic polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN); aromatic polycarbonates such as bisphenol A polycarbonate; and aliphatic polyesters such as polylactic acid, polycaprolactone, poly(3-hydroxybutyric acid), polytetramethylglycolide, and polyglycolic acid. Currently, about 80% (by mass) of the resources are recovered at the dismantling and crushing stage, but by properly treating the slightly less than 20% of the residue remaining after resource recovery, more than 90% of the entire vehicle can be recycled.
[0024] These plastics derived from automobile parts often contain carbon black as a filler. Carbon black is an important component for improving the rigidity and weather resistance of plastics, and is contained in the plastics derived from automobile parts at 10% by mass or less, and in many cases at about 0.1 to 2.0% by mass.
[0025] In addition, plastics derived from automobile parts often contain talc as a filler. This talc is an important component for improving the rigidity of plastics, like carbon black, but the performance and function of the composite plastic of the present invention may change depending on the content of talc in the ASR. Therefore, by producing the composite plastic of the present invention using ASR with a talc content limited within a certain range, more stable performance and function can be imparted. As a method for keeping the talc content within a certain range, a fractionation technique using Raman spectroscopy has been disclosed, and for example, fractionation is possible within the range of talc content of 5% or less, 5% to 15%, 15% to 28%, and 28% or more. It is a preferred embodiment to apply the manufacturing method of the composite plastic of the present invention to each talc-containing ASR, since it is possible to produce a composite plastic with stably controlled rigidity.
[0026] The "carbon fiber-containing resin material" may be any resin material (including both thermoplastic resin and thermosetting resin) containing carbon fiber, but is preferably a crushed product of carbon fiber reinforced plastic (CFRP) that is rapidly becoming more widely used as a composite material that is lighter and stronger than steel as a material for aircraft and automobiles, or a carbon fiber reinforced thermoplastic resin (CFTRP) containing carbon fiber in a thermoplastic resin. Conventional CFRP prioritizes high strength, so a thermosetting resin such as an epoxy resin is used as a resin component. However, as CFRP is used for automobile parts, the importance of moldability has increased, and thermoplastic resins have come to be used as matrix resins. As the carbon fiber-containing resin material used in the manufacturing method for the composite plastic material of the present invention, CFTRP using a thermoplastic resin as a matrix resin has excellent melt processability and is more preferably used. In actual manufacturing sites, a required portion is cut from a sheet of CFRP, and the remaining 40 to 50% is discarded, resulting in a large amount of CFRP waste. Here, CFRP has a great advantage in that it is difficult to burn, but on the other hand, its incineration requires a huge fuel cost. Therefore, most of the waste is actually disposed of in landfills.
[0027] In the composite plastic material of the present invention, as described above, it is important that the volume average fiber length of the carbon fibers contained therein is 105 μm or more and 20 mm or less. If the volume average fiber length is less than 105 μm, the generally required performance of −30 dB / mm -1 The following electromagnetic shielding properties cannot be obtained: Furthermore, if the volume average fiber length exceeds 20 mm, moldability deteriorates.
[0028] The volume average fiber length (Lv) of the carbon fibers contained in the composite plastic material of the present invention is preferably 120 μm or more, more preferably 140 μm or more, even more preferably 200 μm or more, and particularly preferably 250 μm or more. The upper limit is preferably 15 mm, more preferably 10 mm, and even more preferably 5 mm.
[0029] Here, the volume average fiber length Lv is the average fiber length defined by the following formula based on the fiber volume for 100 or more fibers randomly observed under an electron microscope. Lv = Σ(L × v) / Σv Σ means the set, L means the length of each fiber, and v means the volume of each fiber.
[0030] The volume is calculated assuming that each carbon fiber has a cylindrical shape with the same diameter at each point. As shown in the above formula, the volume average fiber length is an index weighted by the volume of each fiber, and generally reflects the performance and function of a composite more accurately than the number average fiber length. It is also an effective index when carbon fibers with different diameters are mixed.
[0031] The diameter of the carbon fibers is not particularly limited, but is, for example, 5 μm to 20 μm.
[0032] Furthermore, in the composite plastic material of the present invention, the number average fiber length (Ln) of the carbon fibers contained therein is preferably 80 μm or more, more preferably 100 μm or more, and even more preferably 150 μm or more. The upper limit is preferably 15 mm, more preferably 10 mm, and even more preferably 5 mm. This makes it possible to more reliably obtain sufficient electromagnetic shielding properties.
[0033] Here, the number average fiber length Ln is the average fiber length defined by the following formula based on the number of fibers (number) for 100 or more fibers randomly observed under an electron microscope. Ln=ΣL / Σn Σ means a set, L means the length of each fiber, and n means the number of fibers. The method using the number average fiber length (Ln) as an index can be used as a simpler method.
[0034] Furthermore, the value D obtained by dividing the volume average fiber length by the number average fiber length is used as an index representing the variation in length and thickness of carbon fibers. D=Lv / Ln The larger the D value, the greater the variation in length and thickness of the carbon fibers, which is likely to affect the performance and function of the composite. In order to improve electromagnetic shielding, antistatic properties, and mechanical strength, it is preferable for the D value to be 1.4 or more.
[0035] The amount of carbon fiber in the plastic material of the present invention can be appropriately determined within a range in which the desired effect is exhibited, but the mass ratio of the resin component of the composite plastic material to the carbon fiber is preferably 99:1 to 60:40, more preferably 95:5 to 65:35, and even more preferably 90:10 to 70:30. A larger amount of carbon fiber is more effective in expressing mechanical and electrical properties, but a smaller amount is more effective in terms of moldability. The resin component of the composite plastic material refers to the resin component contained in the plastic material derived from the automobile parts of the component (a) and the resin component contained in the carbon fiber-containing resin material of the component (b).
[0036] In addition, the composite plastic material of the present invention usually contains carbon black derived from plastic materials derived from automobile parts, but when it is not contained or the amount is small, it is preferable to separately mix carbon black. The mass ratio of carbon black to carbon fiber is preferably 4.5:1 to 1:500, more preferably 1:1 to 1:100, and further preferably 1:5 to 1:50.
[0037] When using the plastic material derived from automobile parts as component (a) and the carbon fiber-containing resin material as component (b), they are mixed by heating and melting. In this case, it is preferable that the resin components of both raw materials are the same type. However, even if the resin components of both raw materials are different, they can be mixed at the molecular level without any problems as long as the two resins are compatible. When the two resins are incompatible, they can be mixed uniformly by adding an appropriate compatibilizer. As such a compatibilizer, for example, in the case of polyethylene and polypropylene, a block copolymer or graft copolymer having a polyethylene chain block and a polypropylene chain block is preferably used.
[0038] In addition, carbon fibers are often made polar by surface oxidation treatment or the like in order to enhance adhesion to the matrix resin. In this case, any commonly available compatibilizer can be used without any restrictions, but it is preferable that the compatibilizer has a polar group in its molecule. Examples of suitable compatibilizers include maleic anhydride-modified polypropylene and maleic anhydride-modified polyethylene. Furthermore, the surface of the carbon fiber is coated with a sizing agent in order to enhance adhesion to the resin. The sizing agent is often prepared according to the chemical properties and composition of the resin, but its affinity with the resin is improved more than that of the carbon fiber itself, and in the present invention, it is also a suitable embodiment to use the carbon fiber coated with the sizing agent and the resin composition containing it as they are.
[0039] The mass ratio of the resin component and the compatibilizer in the composite plastic material is preferably, for example, 99.8:0.2 to 95:5.
[0040] In the present invention, it has been surprisingly found that by melt-mixing component (a) plastic material derived from automobile parts with component (b) carbon fiber-containing plastic material, the resulting mixture exhibits electromagnetic wave shielding performance and antistatic properties far superior to those obtained when either component is used alone, as shown in the examples below. This performance and function is only achieved when the components in the ASR come into contact with the carbon fiber through melt-mixing. The mechanical strength and electrical conductivity were also superior to those obtained when either component was used alone.
[0041] The method for melt molding the composite plastic material according to the present invention can be any known method without any restrictions, as long as it can uniformly disperse the carbon fibers in the resin component. Suitable melt kneading methods include injection molding using an injection molding machine, extrusion molding using an extrusion molding machine, blow molding using a blow molding machine, etc. Furthermore, deep drawing molding using a vacuum molding machine or compression molding using a compression molding machine is preferably used with a pellet-shaped or sheet-shaped molded body produced by extrusion molding as a raw material. Among these molding methods, injection molding and extrusion molding are more preferably used in terms of versatility and scalability.
[0042] Injection molding is a method to obtain a molded product by injecting the material melted and mixed by screw rotation in the heated cylinder of an injection molding machine into the mold cavity and cooling and solidifying it, and the molten composite plastic is filled into the mold cavity of the molded body through parts called sprues and runners. Here, since carbon fiber and carbon fiber-containing thermosetting resins do not melt, when performing injection molding that requires melt fluidity, a thermoplastic resin with excellent fluidity is selected.
[0043] The extrusion molding method is a molding method in which the material melted and mixed in the heated cylinder of the extruder is extruded at a constant speed from the extrusion opening of the die by the shear stress caused by the rotation of the screw, cooled and solidified in the form of strands, and then pelletized by a pelletizer or the like. Since high fluidity like that of injection molding is not required, a high molecular weight thermoplastic resin with high melt viscosity that does not drip after being extruded from the extrusion opening is selected. Furthermore, in the extrusion molding method, there are various screw shapes and rotation directions for kneading with the screw, and they can be selected according to the purpose of use. In the production of the composite plastic material of the present invention, kneading with twin co-rotating screws is a more suitable method in order to increase the degree of kneading.
[0044] When a composite plastic material is molded using a melt molding machine, large unmelted materials are filtered out through a screen installed near the tip of the molding machine, so it is effective for moldability if the carbon fibers are distributed more on the side with a relatively small long axis diameter. In particular, in the case of injection molding, high melt fluidity is required to fill the mold, so a short average chain length of the carbon fibers is advantageous for moldability. On the other hand, in the case of an extrusion molding machine, carbon fibers containing long fibrous components flow in the molten thermoplastic resin while being oriented in the flow direction relatively slowly. Therefore, a composite containing oriented carbon fibers is obtained as a result, and this is a preferred embodiment of the manufacturing method in which the improvement of mechanical properties due to fiber reinforcement is easily realized.
[0045] The composite plastic material of the present invention described above can be suitably used for a variety of applications, such as housings, parts, and components for various in-vehicle electronic devices, various IT devices, IoT home appliances, and even various medical devices, by utilizing its electromagnetic wave shielding performance and antistatic properties. EXAMPLES
[0046] The present invention will now be described in more detail with reference to examples, but these examples are not intended to limit the scope of the present invention.
[0047] (1) Preparation of composite plastic materials The plastic material derived from automobile parts was ASR pellets mainly made of polypropylene with a talc content of less than 5% by mass and a carbon black content of 1.0% by mass, which were graded by gravity fractionation and Raman spectroscopy of ASR provided by Kyushu Metal Industries Co., Ltd. The carbon fibers were cut into pieces with a fiber length of about 1 mm provided by Yoshino Co., Ltd. Furthermore, maleic anhydride-modified polypropylene was used as a compatibilizer. The composite plastic material consisting of these plastic materials derived from automobile parts, carbon fiber, and maleic anhydride-modified polypropylene was produced by melt mixing using a twin-screw extruder. The melt mixing conditions were hopper temperature: 120°C, screw upstream temperature: 200°C, screw downstream temperature: 200°C, and die (outlet) temperature: 200°C. A dry blend of pellets of plastic material derived from automotive parts, carbon fiber, and maleic anhydride-modified polypropylene (70:30:1 (mass ratio)) was added from a hopper and melt-kneaded for approximately 3 minutes at a screw rotation speed of 30 rpm, and finally the composite plastic was extruded into strands from the die. In addition, samples were also produced by performing melt kneading and extrusion 2 to 4 times under the same conditions.
[0048] Each composite plastic material melt-kneaded in a twin-screw extruder was compression molded using a heat press. The strand-like composite obtained from the extruder was chopped into pellets, then placed in an iron mold that also served as a spacer, sandwiched between polyethylene terephthalate (PET) sheets from above and below, and then between iron plates from the outside, and compression molded using an ASONE heat press model HC300-15. The molding conditions were a molding temperature of 180°C, melting time of 1 minute 30 seconds, pressing time of 1 minute 30 seconds, and pressing pressure of 20 MPa. This was used as the sample for measurement.
[0049] The amount of carbon fiber contained in each sample was measured by thermogravimetric differential thermal analysis (TG-DTA), and the results are shown in Table 1. The sample names are indicated by the number of melt-kneading cycles.
[0050] [Table 1]
[0051] Strictly speaking, the amount of carbon fiber shown here includes the amount of carbon black; however, since the amount of carbon black is very small at 1.0 mass %, it can be considered as essentially the amount of carbon fiber.
[0052] The carbon fibers were also observed under an electron microscope (150x) (Figs. 1 to 4), and the average carbon fiber length was determined from 100 randomly selected and observed carbon fibers. The fiber diameter was calculated based on the electron microscope photographs as 8.2 µm. The results are shown in Table 2. The composite plastic material that was melt-kneaded one to three times is the composite plastic material of the present invention, and the composite plastic material that was melt-kneaded four times is outside the scope of the present invention.
[0053] [Table 2]
[0054] In addition, only the ASR pellets mainly made of polypropylene with a talc content of less than 5% by mass and a carbon black content of 1.0% by mass, provided by Kyushu Metal Industries Co., Ltd., were extruded into a strand shape in the same manner as shown in "(1) Preparation of composite plastic material" above, and this was compression molded using a hot press device to prepare a comparative sample.
[0055] The above four samples and one comparative sample were measured for electromagnetic wave shielding performance and antistatic performance. The specific measurement methods are as follows.
[0056] (2) Measurement of the electromagnetic shielding performance of composite plastic materials The electromagnetic wave shielding performance was measured using a network analyzer model MS202C (Anritsu Corporation, Kanagawa Prefecture, Japan) by the coaxial method (manufactured by Keycom Corporation) in the range of 0.45 to 15 GHz at 23±2° C. The results are shown in Figures 5 to 8.
[0057] As shown in FIG. 5, the sample of the present invention having a volume average fiber length of 289.41 μm (number average fiber length of 195.18 μm) and melt kneaded once was confirmed to exhibit extremely excellent shielding properties against electromagnetic waves of all frequencies from 0 to 14 GHz. Also, as shown in FIG. 6, the sample of the present invention having a volume average fiber length of 140.69 μm (number average fiber length of 109.36 μm) and melt kneaded twice was also confirmed to exhibit excellent shielding properties against electromagnetic waves of all frequencies from 0 to 14 GHz, showing -30 dB or less, which is normally required. Furthermore, as shown in FIG. 7, the sample of the present invention having a volume average fiber length of 106.10 μm (number average fiber length of 83.18 μm) and melt kneaded three times was confirmed to exhibit excellent shielding properties against electromagnetic waves of frequencies of about 8 GHz or more, showing -30 dB or less, which is normally required.
[0058] On the other hand, as shown in Figures 8 and 9, the comparative example sample with a volume average fiber length of 103.13 μm (number average fiber length 75.45 μm) that was melt-kneaded four times and the comparative example sample that did not contain carbon fiber did not satisfy the normally required level of -30 dB or less for electromagnetic waves of any frequency between 0 and 14 GHz, and it was confirmed that they did not function sufficiently as electromagnetic wave shielding materials.
[0059] (3) Measurement of antistatic performance of composite plastic materials The antistatic performance test was carried out by evaluating the volume and surface electrical resistance. The composite pellets and the pellets of the comparative example were sandwiched between iron plates and pressed at 160°C and 5 MPa using a mini test press MP-SCH (Toyo Seiki Seisakusho). The obtained disk-shaped film was used as the measurement sample. The volume and surface electrical resistance were measured using a surface resistivity meter Loresta AP (Mitsubishi Yuka) by placing a terminal (terminal distance 1.5 mm) in the center of the disk-shaped film. The results are shown in Figure 10.
[0060] The sample of the present invention, which was melt-kneaded 1-2 times, showed extremely low resistance values for both volume resistance and surface resistance, and extremely high antistatic properties were observed. The sample of the present invention, which was melt-kneaded 3 times, and the comparative sample, which was melt-kneaded 4 times, showed higher resistance values than the sample, which was melt-kneaded 1-2 times, but showed antistatic properties that are generally considered to be high. On the other hand, the comparative sample, which did not contain carbon fiber, showed volume resistance and surface resistance values almost equal to those of the comparative sample, which was melt-kneaded 4 times.
Claims
1. (a) a plastic material derived from automobile shredder residue; (b) one or both of carbon fibers and carbon fiber-containing resin materials containing carbon fibers and resin components (excluding the plastic materials derived from automobile shredder residue); A molded article for an electromagnetic wave shielding material comprising a composite plastic material comprising: The carbon fibers have a volume average fiber length of 105 μm or more and 20 mm or less.
2. 2. The molded article for an electromagnetic shielding material according to claim 1, wherein the number average fiber length of the carbon fibers is 80 μm or more and 15 mm or less.
3. 3. The molded article for an electromagnetic wave shielding material according to claim 1, wherein a mass ratio of a resin component of the composite plastic material to the carbon fibers is 99:1 to 60:
40.
4. 4. The molded article for an electromagnetic shielding material according to claim 1, wherein the carbon fiber-containing resin material (b) is derived from a waste resin material containing carbon fibers.
5. The molded article for an electromagnetic wave shielding material according to any one of claims 1 to 4, further comprising a compatibilizer.
6. 6. The molded article for an electromagnetic wave shielding material according to claim 1, further comprising carbon black.
7. The molded article for an electromagnetic shielding material according to any one of claims 1 to 6, characterized in that it contains talc.
Citation Information
Patent Citations
Recycled resin composition, method for molding recycled resin composition, and molded article
JP2001113528A
Thermoplastic resin composition and molded product
JP2005048074A