Porous bricks for porous plugs and porous plugs
A porous brick using spherical alumina, mullite, and spinel achieves high air permeability and strength without chromium or zirconium, addressing environmental concerns and material safety in molten metal containers.
Patent Information
- Application Number
- JP2020174292
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-16
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-10-16
AI Technical Summary
Existing porous bricks used in molten metal containers face challenges in achieving sufficient air permeability, permeation resistance, and strength while avoiding the use of chromium and zirconium-containing raw materials, which are environmentally harmful and potentially radioactive.
A porous brick composed of spherical alumina particles, mullite particles, and fine powder with a specific composition, including 10-20% by mass of mullite, 1-15% by mass of spinel, and the remainder mainly alumina, without chromium and zirconium, ensuring optimal porosity and particle sizes for high air permeability and strength.
The solution provides a porous brick with excellent air permeability, permeation resistance, and strength, suitable for use in porous plugs, without the use of environmentally harmful or radioactive materials.
Smart Images

Figure 0007554627000005 
Figure 0007554627000003 
Figure 0007554627000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a porous brick suitable for use as a porous plug that is held via a tuyere refractory on the bottom wall of a molten metal container such as a ladle and is used to inject gas into molten metal, and relates to a porous brick for porous plug and a porous plug in which chromium oxide and zircon / zirconia are not added as raw materials. [Background technology]
[0002] A porous plug is a porous refractory material that is attached to the tuyere refractory material on the bottom wall of a molten metal container such as a ladle or tundish and has good air permeability to allow gas to be injected into the molten metal. It is used for the purposes of stirring the molten steel, floating inclusions in the molten steel, and promoting metallurgical reactions.
[0003] The porous plug comprises a shell that forms the outer peripheral surface of the porous plug, a castable refractory material that fills the shell and holds the porous bricks within the shell, and a porous brick that is arranged so that its upper end surface is exposed to the molten metal side and acts as a gas inlet, and a gas supply pipe is connected to the lower end.
[0004] As the porous brick, alumina porous bricks having air permeability, for example, high alumina, alumina-chrome, alumina-magnesia, and other porous bricks, are widely used.
[0005] The properties required for a porous brick are air permeability, strength, resistance to penetration and resistance to corrosion.
[0006] In order to allow a sufficient amount of gas to be blown into the molten metal, it is necessary to have sufficient gas permeability.
[0007] Porous bricks are in contact with high-temperature molten metal such as molten steel, and wear occurs due to the agitation of the molten metal caused by gas injection. To minimize this wear, porous bricks must be strong. It also needs to be resistant to corrosion by molten metal and slag.
[0008] When gas is injected into molten steel, it is important that the molten steel and slag have a high resistance to penetration into the pores. While gas injection is stopped, molten steel and slag penetrate into the porous bricks and solidify, forming a penetration layer. When a penetration layer is formed, the gas permeability decreases, so oxygen cleaning is performed to restore gas permeability. Oxygen cleaning is performed by blowing oxygen into the porous bricks from the vessel side after the molten steel is discharged, and removing the molten steel and slag that have penetrated and solidified while oxidizing and burning the penetrated steel. At this time, removal of the penetration layer causes wear of the porous bricks, so in order to reduce the amount of wear, the porous bricks need to be resistant to penetration by molten steel and slag.
[0009] In order to ensure sufficient gas permeability, it is effective to increase the pore size and porosity, but when the pore size and porosity are increased, molten steel and slag are more likely to permeate, and the permeation resistance decreases and the strength also decreases. In other words, it has been difficult to simultaneously obtain sufficient gas permeability, permeation resistance, and strength by controlling the pores alone.
[0010] Therefore, various methods have been studied to ensure strength and permeation resistance. Methods in which zircon or zirconia is added to improve strength and permeation resistance (e.g., Patent Documents 1 and 2) and methods in which chromium oxide is added to improve permeation resistance (e.g., Patent Documents 1, 2, and 3) have been disclosed. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Japanese Patent Application Publication No. 9-52168 [Patent Document 2] Japanese Patent Application Publication No. 60-65778 [Patent Document 3] Japanese Patent Application Publication No. 8-309515 Summary of the Invention [Problem to be solved by the invention]
[0012] However, due to increasing concern for the global environment, there is a demand for the development of alumina porous bricks that do not use chromium oxide. In addition, it is known that zircon and zirconia raw materials contain relatively large amounts of radioactive materials, and refractories that use these raw materials also emit small amounts of radiation. Therefore, the development of alumina porous bricks that do not use zircon or zirconia raw materials is important, but there have been few reports of research on porous bricks that do not contain zirconium.
[0013] In view of the above, an object of the present invention is to provide a porous brick for a porous plug, which does not use a raw material containing chromium and zirconium and has excellent air permeability, penetration resistance and strength, and to provide a porous plug using the porous brick. [Means for solving the problem]
[0014] In the invention described in claim 1, the porous brick for a porous plug is mainly composed of spherical alumina particles. 10 to 20 mass% of mullite particles and fine powder as a binder, The aggregate and the fine powder do not contain chromium and zirconium, The fine powder is 10 to 20 mass %, with 1 to 15 mass % of spinel, and the remainder being composed mainly of alumina, containing sintering aid components and unavoidable components.
[0016] Claim 2 In the invention described in claim 1 to In the porous brick for a porous plug described in the above, the particle size of the aggregate is 0.2 to 1.5 mm.
[0017] Claim 3 In the invention described in claim 1 Or claim 2 In the porous brick for a porous plug described in the above, the particle size of the fine powder is 150 μm or less.
[0018] Claim4 In the invention described in claim 1 or claims 3 In the porous brick for porous plug described in any one of the above, the aggregate contains 15 to 20% by weight of mullite particles, 10 to 15% by mass of the fine powder, 2 to 6% by mass of spinel, and the remainder mainly composed of alumina.
[0019] Claim 5 In the invention described in claim 1, the porous plug is 4 The present invention uses a porous brick for a porous plug according to any one of the above technical means. Effect of the Invention
[0020] According to the porous brick for porous plug of the present invention, it is possible to provide a porous brick for porous plug, which has excellent air permeability, penetration resistance and strength, without using raw materials containing chromium and zirconium. In addition, the porous brick can be used to provide a porous plug. [Brief description of the drawings]
[0021] [Figure 1] FIG. 2 is a diagram showing the observation results of the microstructure and element distribution in Reference Example 1, Comparative Example 1, and Examples 2 and 3. [Diagram 2] FIG. 13 is a diagram showing the results of observation of the microstructure and element distribution of Example 2 after a crucible test. [Diagram 3] FIG. 13 is a diagram showing the results of observation of the microstructure and element distribution of Example 3 after a crucible test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The present inventors have conducted extensive research to solve the above-mentioned problems and have discovered a porous brick that has properties equivalent to those of existing porous bricks, without using raw materials containing chromium and zirconium. The technical concept of the material design is as follows:
[0023] In conventional porous bricks, chromium oxide (Cr2O3) mainly contributes to improving corrosion resistance against slag, while zirconia (ZrO2) and zircon (ZrSiO4) mainly contribute to improving strength.
[0024] In order to achieve the above effects, an attempt was made to use fine powders of spinel (MgAl2O4) and alumina (Al2O3) instead of chromium oxide (Cr2O3), zirconia (ZrO2) and zircon (ZrSiO4), and a porous brick with properties equivalent to those of existing porous bricks was obtained.
[0025] The structure of the porous brick of the present invention will be described below.
[0026] The porous brick for porous plug of the present invention (hereinafter referred to as the porous brick) does not contain particles mainly composed of zirconium or chromium, and comprises aggregate mainly composed of spherical alumina particles and fine powder as a binder, the fine powder being 10 to 20 mass %, 1 to 15 mass % of spinel, and the remainder being composed mainly of alumina, sintering aid components and unavoidable components.
[0027] The porosity of the porous brick is preferably 20 to 35%. If the porosity is less than 20%, the porous brick becomes dense and the air permeability decreases. If the porosity is more than 35%, both the strength and the penetration resistance decrease.
[0028] The aggregate contains spherical alumina particles as a main component, and may additionally contain 10 to 20 mass % of mullite particles.
[0029] As the spherical alumina particles, spherical alumina particles having a particle diameter of 0.2 to 1.5 mm can be suitably used. By using spherical alumina particles as the alumina aggregate, the contact area between particles is reduced, and high breathability can be obtained without increasing the porosity or pore size.
[0030] If the particle size of the spherical alumina particles is smaller than 0.2 mm, the pore size becomes small and sufficient breathability cannot be ensured. If the particle size is larger than 1.5 mm, the pore size becomes too large, making it easier for molten steel to penetrate into the pores and reducing the penetration resistance. For this reason, it is preferable to set the particle size to 0.2 to 1.5 mm. In particular, when the penetration resistance is important, it is preferable to set the particle size to 0.2 to 1.0 mm.
[0031] Mullite (3Al2O3·2SiO2) particles react with the spherical alumina particles to strengthen the bonds between the aggregates, resulting in high strength.
[0032] As with the spherical alumina particles, mullite particles having a particle diameter of 0.2 to 1.5 mm can be suitably used. In particular, when emphasis is placed on ensuring sufficient breathability, the particle diameter is preferably 0.5 to 1.5 mm. The content of mullite is preferably 10 to 20 mass%. If the content is less than 10 mass%, the bonding force between aggregates cannot be sufficiently increased, and strength cannot be improved. Furthermore, if the content exceeds 20 mass%, the porosity decreases and sufficient breathability cannot be ensured. Furthermore, the SiO2 component increases, resulting in a decrease in corrosion resistance.
[0033] The fine powder is 10 to 20 mass%, with 1 to 15 mass% spinel and the remainder being mainly alumina. In the present invention, the fine powder refers to a powder having a particle diameter of 150 μm or less. If the particle diameter is larger than 150 μm, the binding property decreases and the strength decreases, so the above range is preferable.
[0034] If the fine powder content is less than 10% by mass, the neck growth is insufficient, the binding force of the aggregate cannot be increased sufficiently, and strength cannot be improved.On the other hand, if the fine powder content exceeds 20% by mass, sintering proceeds too much, the porosity decreases, and sufficient breathability cannot be secured.
[0035] If the fine powder is only alumina, sufficient penetration resistance and strength cannot be obtained. Therefore, in order to develop penetration resistance and strength, a specified amount (1 to 15 mass%) of spinel is contained in the fine powder. Here, if the fine powder is entirely made of spinel, sintering proceeds too much and the desired characteristics cannot be obtained.
[0036] The strength-enhancing effect of spinel can be explained as follows. As shown in the examples, Mg in the spinel is diffused throughout the particles. Therefore, it is believed that recombination occurs between the aggregate and the spinel, resulting in densification and increased bonding strength.
[0037] The effect of spinel in improving penetration resistance can be explained as follows. It is believed that the spinel dissolves the FeO component in the molten steel, increasing the viscosity of the molten steel and suppressing penetration. This makes it possible to prevent initial penetration, so even a small amount of spinel, 1 mass% or more, can be effective.
[0038] Here, the ratio of Al2O3 and MgO in the spinel is not limited to the theoretical composition (MgAl2O4).
[0039] The method for producing the porous brick of the present invention is as follows: The raw materials and sintering aids are weighed and mixed, kneaded, and then molded into a predetermined shape. The molded body is fired in air at a firing temperature of 1500°C or higher to obtain a porous brick.
[0040] The porous brick thus obtained is formed into a predetermined shape, supported by an iron shell and a castable refractory material, and a gas supply pipe is connected to obtain a porous plug.
[0041] As fine powder, SiO2, TiO2, etc. may be contained within the range that does not impair the effects of the present invention.
[0042] (Effects of the embodiment) According to the porous brick of the present invention, it is possible to provide a porous brick having excellent air permeability, penetration resistance and strength without using raw materials containing chromium and zirconium. Furthermore, the porous brick of the present invention has sufficient air permeability, corrosion resistance and strength, and can be suitably used for a porous plug. EXAMPLES
[0043] The present invention will be described below with reference to examples. However, the present invention is not limited to these examples. Table 1 shows the blending ratios of raw materials in Reference Examples 1 and 2 which are conventional porous bricks, Examples 1 to 6 which are porous bricks of the present invention, and Comparative Examples 1 and 2. Here, the Reference Examples are conventional products containing zircon and chromium, and Reference Example 1 has a total of 12 mass% fine powder, and Reference Example 2 has a total of 20 mass% fine powder. In addition, in Examples 1 to 4, the total of the fine powder is 12 mass%, in Examples 5 and 6, the total of the fine powder is 20 mass%, in Comparative Example 1, the fine powder is only alumina at 12 mass%, and in Comparative Example 2, the fine powder is only spinel at 20 mass%.
[0044] The spherical alumina particles and mullite used as aggregates had particle sizes of 0.2 to 1.5 mm (specifically, alumina particles of 0.2 to 1.0 mm, mullite particles of 0.5 to 1.5 mm), and the fine powder used had a size of 150 μm or less.
[0045] [Table 1]
[0046] The various raw materials listed in Table 1 were mixed with water and additives in a wet pan and pressed into a truncated cone shape (φ80 × φ140 × h300mm) using a 300t friction press to achieve the same bulk density. The resulting molded body was dried at 150°C for 24 hours and then fired at 1500°C for 10 hours to produce a porous brick, which was then processed into the specified sample shape to be used in the evaluation.
[0047] The evaluation items were the air permeability index T, the penetration resistance index S, and the compressive strength σ, and the comparison was made with the reference example as the standard. The porosity and average porosity are also shown.
[0048] (Breathability Index T) The prepared sample was fitted with an iron shell and the amount of air permeability was measured. The amount of air permeability was measured by blowing air at a predetermined pressure in a space kept at a constant temperature, and measuring the flow rate of air blown out from the tip of the porous plug. Then, the air permeability index T was calculated and evaluated by standardizing the amount of air permeability of Reference Example 1 to 100. The larger the air permeability index T, the higher the air permeability. Using this air permeability index T, the material was evaluated as 100≧T>80 (◎), 80≧T>60 (○), and 60≧T>50 (△). When the air permeability index T was 50 or less, it was marked as (×). Here, the evaluations ◎, ○, and △ indicate that the material can be fully used in the same manner as Reference Example 1 when applied to an actual machine.
[0049] (Permeability index S) The permeation resistance was evaluated by a crucible erosion test. In the crucible erosion test, 5 g of synthetic slag mixed to have a C / S ratio of 2.0 and 10 g of steel were placed in the recess of a crucible (φ30 mm, depth 25 mm) and held at 1500°C for 3 hours. After the test, the sample was cut in the center in the longitudinal direction to measure the amount of corrosion, and the permeation resistance index S was calculated by dividing the permeation amount (permeation depth) of the slag in Reference Example 1 by the permeation amount (permeation depth) of the slag in the comparative sample. The permeation resistance index S is higher, indicating higher permeation resistance. Using this permeation resistance index S, the evaluation was made as 100≧S>90 (◎), 90≧S>80 (○), and 80≧S>70 (△). When the permeation resistance index S was 70 or less, it was marked (×). Here, the evaluations of ◎, ◯, and △ indicate that the material in question is sufficiently durable for use in an actual device, similar to Reference Example 1.
[0050] (Compressive strength σ) The compressive strength σ (MPa) was measured in accordance with JIS R 2206. The compressive strength σ was evaluated as σ>60 (◎), 60≧σ>40 (◯), and 40≧σ (×). The evaluations ◎ and ◯ indicate that the material can be sufficiently used in an actual machine, similar to Reference Example 1.
[0051] The porosity was measured in accordance with Japanese Industrial Standard JIS R 2205. The average pore diameter was the median diameter measured using a mercury porosimeter.
[0052] The evaluation results are shown in Table 2.
[0053] [Table 2]
[0054] Examples 1 to 4 are materials with a total fine powder content of 12% by mass. All of the materials showed good values for the air permeability index, penetration resistance index, and compressive strength. The penetration resistance index showed a good value even when the amount of spinel was as small as 1% by mass. In particular, Examples 2 and 3 showed excellent values for the air permeability index and penetration resistance index, which are important for porous bricks.
[0055] Examples 5 and 6 are materials with a total fine powder content of 20 mass%. Although the air permeability index of each material tended to decrease compared to Examples 1 to 4, they still showed good values. The compressive strength was higher, which is believed to be due to the fact that sintering proceeded with the increase in the amount of fine powder, resulting in a decrease in porosity. The penetration resistance index showed good values similar to Examples 1 to 4.
[0056] Comparative Example 1 is a material containing 12 mass% of fine powder, similar to Examples 1 to 4. In Comparative Example 1, the air permeability index showed a good value, but the penetration resistance index and compressive strength showed values that were not suitable for use. The decrease in the penetration resistance index is believed to be due to the absence of spinel, which contributes to the improvement of penetration resistance. The decrease in compressive strength is believed to be due to the absence of spinel or zircon, which contributes to the improvement of bonding strength.
[0057] Comparative Example 2 is a material containing 20 mass% of fine powder, similar to Examples 5 and 6. In Comparative Example 2, the compressive strength and the penetration resistance index showed good values, but the air permeability index did not show a value that could withstand use. The reason for the decrease in the air permeability index is thought to be that the fine powder was all spinel, and sintering proceeded too far, resulting in a decrease in porosity.
[0058] From the above, it was confirmed that the porous plugs that do not use raw materials mainly composed of chromium and zirconium and that satisfy the conditions set forth in the present invention are excellent in air permeability, permeation resistance, and strength. In particular, Examples 2 and 3 showed excellent values in the air permeability index and permeation resistance index, which are important for porous bricks. In other words, it is preferable that the porous brick has a composition similar to that of Examples 2 and 3, and that the aggregate contains 15 to 20 weight % mullite particles, 10 to 15 mass % fine powder, 2 to 6 mass % spinel, and the remainder is mainly composed of alumina.
[0059] (Microstructure observation) The observation results of the microstructure and element distribution of Reference Example 1, Comparative Example 1, and Examples 2 and 3 are shown in FIG. 1. In Reference Example 1, Cr and Al exist in the same position, and it is considered that Cr is solid-dissolved in Al. In addition, Zr exists in the grain boundaries of Al, and it is considered that it is vitrified and strengthens the bond. It is considered that this shows a higher strength than Comparative Example 1, which is bonded only by Al. In Example 2, Mg is diffused throughout the particles, and it is considered that the bonded part is densified by being turned into a spinel, and the bond strength is increased.
[0060] The microstructure of Example 2 after the crucible test was observed and the results are shown in Figure 2. The slag components Si and Ca had infiltrated into the grain boundaries. On the other hand, Fe was present in the same position as Mg and was considered to have dissolved in the spinel as FeO. This is thought to have suppressed the infiltration of FeO.
[0061] The observation results of the microstructure and element distribution of Example 2 and Example 3 are shown in Figure 1. In Example 3, which has a larger amount of spinel than Example 2, Mg diffused throughout the particles and Mg colonies were observed, similar to Example 2. This is thought to be because the amount of Mg added exceeded the amount of Mg required to form spinel at the joints, and the excess Mg did not diffuse.
[0062] The microstructure of Example 3 after the crucible test was observed and the results are shown in Figure 3. As in Example 2, the slag components Si and Ca penetrated into the grain boundaries and were present in the same position as Mg. The reason why the penetration resistance index did not change even when the amount of spinel added was changed is thought to be because the pore diameter of Example 3 was larger, which made it easier for Fe to penetrate, and this was offset.
[0063] From the above results, it was confirmed that by satisfying the requirements of the present invention, a porous brick excellent in air permeability, penetration resistance and strength can be obtained.
Claims
1. The aggregate is composed of spherical alumina particles as a main component and contains 10 to 20 mass% of mullite particles, and fine powder as a binder. The aggregate and the fine powder do not contain chromium and zirconium, The fine powder is 10 to 20% by mass, spinel is 1 to 15% by mass, and the remainder is mainly composed of alumina, A porous brick for a porous plug, comprising: a sintering aid component; and an unavoidable component.
2. 2. The porous brick for a porous plug according to claim 1, characterized in that the particle size of the aggregate is 0.2 to 1.5 mm.
3. 3. The porous brick for a porous plug according to claim 1 or 2, characterized in that the fine powder has a particle size of 150 μm or less.
4. The aggregate contains 15 to 20 weight percent mullite particles; 4. The porous brick for a porous plug according to claim 1, wherein the fine powder is 10 to 15 mass %, the spinel is 2 to 6 mass %, and the remainder is mainly composed of alumina.
5. A porous plug using the porous brick for porous plug according to any one of claims 1 to 4.
Citation Information
Patent Citations
Porous slag
JP1985065778A
Refractory for gas blowing
JP1990307863A
Production of porous refractories for gas blowing porous plug and gas blowing porous plug formed by using these porous refractories
JP1996309515A
Porous plug
JP1997052168A
Porous plug for gas blowing
JP1998251739A