Semiconductor light emitting device and its manufacturing method
The semiconductor light emitting device with an airtight substrate and cap structure using a gold network structure addresses the degradation issue by replacing internal gases without ports, ensuring high airtightness and improved reliability.
Patent Information
- Application Number
- JP2021022564
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-16
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2041-02-16
AI Technical Summary
Semiconductor light emitting devices, particularly those emitting ultraviolet light, are susceptible to degradation by environmental gases, necessitating a package with high airtightness and a gas atmosphere that prevents deterioration.
A semiconductor light emitting device with an airtight substrate and cap structure, utilizing a gold network structure impregnated with AuSn alloy for bonding, allows gas replacement without a port, ensuring high airtightness and protection from environmental gases.
The device achieves high airtightness and prevents semiconductor element deterioration by replacing the internal gas atmosphere effectively, enhancing reliability and longevity.
Smart Images

Figure 0007554685000006 
Figure 0007554685000001 
Figure 0007554685000010
Abstract
Description
[Technical field]
[0001] The present invention relates to a semiconductor light emitting device and a manufacturing method thereof, and more particularly to a semiconductor light emitting device in which a semiconductor light emitting element that emits ultraviolet light is enclosed, and a manufacturing method thereof. [Background technology]
[0002] Conventionally, there has been known a semiconductor device in which a semiconductor element is enclosed inside a semiconductor package. In the case of a semiconductor light emitting module, a transparent window member such as glass that transmits light from the light emitting element is bonded to a support on which the semiconductor light emitting element is mounted, thereby hermetically sealing the semiconductor light emitting element.
[0003] For example, Patent Document 1 discloses a light-emitting element in which a light-emitting chip is placed in a cavity having a ventilation through-hole, and after the gas in the cavity is evacuated through the ventilation through-hole, the ventilation through-hole is sealed to prevent the light-emitting chip from coming into contact with external water vapor and oxygen.
[0004] Patent Document 2 discloses a semiconductor light emitting element package that emits short wavelength light such as ultraviolet light. The package has a through hole sealed with a hot melt material, and the inside is filled with an inert gas.
[0005] Patent Document 3 discloses a package for housing an optical element, in which a through hole is provided and sealed with a sealing material.
[0006] Moreover, Patent Document 4 discloses an electronic component device in which the inside of a package is evacuated through an exhaust port provided in the package, and then the exhaust port is sealed. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2018-142690 A [Patent Document 2] JP 2006-93372 A [Patent Document 3] JP 2007-123444 A [Patent Document 4] JP 2007-287967 A [Non-patent literature]
[0008] [Non-Patent Document 1] Nagase & Co., Ltd. https: / / www.nagase-pactech.jp / solder / spec / [Non-Patent Document 2] Tanaka Precious Metals Co., Ltd. https: / / tanaka-preciousmetals.com / jp / products / detail / aurofuse / ?nav=use Summary of the Invention [Problem to be solved by the invention]
[0009] However, there is a demand for even higher reliability for semiconductor light emitting devices. In particular, semiconductor light emitting elements that emit ultraviolet light, particularly AlGaN-based semiconductor light emitting elements, are easily degraded by environmental gases. Therefore, there is a demand for packages with a highly airtight sealing structure that replaces the inside of the package with an environment that prevents the degradation of the semiconductor light emitting elements.
[0010] The present invention has been made in consideration of the above-mentioned points, and aims to provide a semiconductor light-emitting device and a manufacturing method thereof that have high airtightness and can replace the inside of the package with an environment (gas atmosphere) that is less likely to deteriorate the semiconductor light-emitting element, without providing a gas replacement port in the package. [Means for solving the problem]
[0011] A semiconductor light emitting device according to one embodiment of the present invention comprises: A semiconductor light emitting element; an airtight substrate having a substrate bonding surface to which a wiring connected to the semiconductor light emitting device and a ring-shaped substrate metal layer surrounding the semiconductor light emitting device are fixed; a window portion that transmits the emitted light of the semiconductor light emitting element, and a flange portion to which a ring-shaped cap metal layer corresponding to the substrate metal layer is fixed, the cap metal layer being bonded to the substrate metal layer by a bonding layer, the cap metal layer having an internal space for accommodating the semiconductor light emitting element, and an airtight light-transmitting cap that is airtightly bonded to the substrate, The bonding layer is an impregnated bonded body in which a gold (Au) mesh structure is impregnated with a bonding metal.
[0012] A method for manufacturing a semiconductor light emitting device according to another embodiment of the present invention is a method for manufacturing the above-mentioned semiconductor light emitting device, A plurality of bonding material bumps are arranged on the substrate metal layer along an extending direction of the substrate metal layer of the airtight substrate; Applying nano Au paste so as to embed the plurality of bonding material bumps; The flange portion is pressed while the cap metal layer is placed on the nano Au paste. Sintering the nano Au paste at a first heat treatment temperature to form an Au network structure and bond the substrate and the airtight transparent cap; placing the assembly of the substrate and the light-transmitting cap under a reduced pressure environment to evacuate the internal space; After the evacuation, the assembly is placed in an environment of a predetermined gas and a pressure higher than the reduced pressure environment, and the interior space is replaced with the predetermined gas; After the replacement with the predetermined gas, the Au network structure is impregnated with the bonding material of the bonding material bump at a second heat treatment temperature higher than the first heat treatment temperature. [Brief description of the drawings]
[0013] [Figure 1A] 1 is a plan view diagrammatically illustrating the upper surface of a semiconductor light emitting device 10 according to a first embodiment of the present invention. [Figure 1B] 1 is a diagram illustrating a schematic side view of a semiconductor light emitting device 10. FIG. [Figure 1C] 2 is a plan view showing a schematic view of the back surface of the semiconductor light emitting device 10. FIG. [Figure 1D]1 is a diagram illustrating an internal structure of a semiconductor light emitting device 10. FIG. [Figure 2A] 1B is a cross-sectional view that illustrates a schematic cross section of the semiconductor light-emitting device 10 taken along line AA in FIG. 1A. [Figure 2B] 2 is a partially enlarged cross-sectional view showing an enlarged portion W where the substrate 11 and the light-transmitting cap 13 are joined together. FIG. [Figure 3A] 1 is a diagram showing a schematic view of a bonded portion between a cap metal layer 21 and a substrate metal layer 12 in manufacturing steps STEP 1 to STEP 3. A cross-sectional view in each step is shown on the upper side, and a plan view in a plane parallel to line AA of the cross-sectional view is shown on the lower side. [Figure 3B] 1A to 1C are diagrams illustrating the bonded portion between the cap metal layer 21 and the substrate metal layer 12 in STEP 4 to STEP 6 of the manufacturing process. [Figure 4A] 1 is a cross-sectional view that typically illustrates a cross section of a semiconductor light-emitting device 50 according to a second embodiment of the present invention. [Figure 4B] 2 is a partially enlarged cross-sectional view showing an enlarged portion W where the substrate 11 and the light-transmitting cap 13 are joined together. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] In the following, preferred embodiments of the present invention will be described, which may be modified and combined as appropriate. In the following description and accompanying drawings, substantially the same or equivalent parts are designated by the same reference numerals. [First embodiment] Fig. 1A is a plan view typically showing the top surface of a semiconductor light emitting device 10 according to a first embodiment of the present invention. Fig. 1B is a diagram typically showing a side surface of the semiconductor light emitting device 10. Fig. 1C is a plan view typically showing the back surface of the semiconductor light emitting device 10. Fig. 1D is a diagram typically showing the internal structure of the semiconductor light emitting device 10.
[0015] Fig. 2A is a cross-sectional view showing a schematic cross section of the semiconductor light emitting device 10 taken along the line AA in Fig. 1A. Fig. 2B is a partially enlarged cross-sectional view showing an enlarged portion W where the substrate 11 and the light-transmitting cap 13 are joined.
[0016] 1A and 1B, in the semiconductor light emitting device 10, a rectangular plate-shaped substrate 11 and a light-transmitting cap 13 are joined to form a light emitting element package 10A. A light emitting element 15 is accommodated in the light emitting element package 10A. Note that the side surfaces of the substrate 11 are parallel to the x and y directions, and the top surface of the substrate 11 is parallel to the xy plane. (Light-transmitting cap 13 and cap metal layer 21) 1A, 1B, and 2A, the light-transmitting cap 13 is made of a window portion 13A, which is a light-transmitting window made of semispherical glass, and a flange 13B (cap joint portion) extending from the end of the bottom of the window portion 13A. That is, the light-transmitting cap 13 is airtight, and is configured, for example, by airtightly connecting the window portion 13A and the flange 13B.
[0017] The light-transmitting cap 13 is made of light-transmitting glass that transmits the light emitted from the light-emitting element 15 disposed in the semiconductor light-emitting device 10. For example, quartz glass or borosilicate glass can be suitably used.
[0018] The flange 13B has a circular plate shape. More specifically, the bottom surface of the flange 13B has a circular shape (center: C) that is concentric with the center of the window portion 13A. That is, the outer edge (outer periphery) of the flange 13B is concentric with the inner edge (inner periphery) of the flange 13B.
[0019] The flange 13B has a cap metal layer 21 which is a metal layer fixed to a bottom surface (cap joint surface) 13S of the flange 13B and has a circular plate shape concentric with the flange 13B.
[0020] The cap metal layer 21 may be, for example, a chromium / nickel / gold (Cr / Ni / Au) layer or a titanium / palladium / copper / nickel / gold (Ti / Pd / Cu / Ni / Au) layer (with the Au layer being the outermost layer). (Substrate metal layer 12, light-transmitting cap 13, and bonding layer 24) 2A, a ring-shaped metal layer 12 (hereinafter also referred to as substrate metal layer 12) is formed on the upper surface of substrate 11, which is concentric with flange 13B and cap metal layer 21. Cap metal layer 21 is bonded to substrate metal layer 12 by bonding layer 22 to form bonding portion 24, and airtightness between substrate 11 and light-transmitting cap 13 is maintained.
[0021] That is, the cap metal layer 21 has a shape and size corresponding to the substrate metal layer 12 , and the cap metal layer 21 and the substrate metal layer 12 are bonded to each other by the bonding layer 22 .
[0022] The substrate metal layer 12 has a structure (W / Ni / Au) in which tungsten, nickel, and gold are laminated in this order on the substrate 11. Alternatively, a structure (NiCr / Au / Ni / Au) in which nickel chromium, gold, nickel, and gold are laminated can be used. Note that by selecting a metal that is easily nitrided (or oxidized in the case of oxide ceramic) as the metal in contact with the base ceramic of the substrate 11, high adhesion to the substrate 11 can be obtained.
[0023] It is preferable that the surface (substrate bonding surface) 11S of the substrate 11 to which the substrate metal layer 12 is fixed and the cap bonding surface 13S to which the cap metal layer 21 is fixed are flat surfaces.
[0024] The bonding layer 22 has a structure in which a network structure in which nano-sized Au particles are connected in a network shape is impregnated with an AuSn alloy and includes cavities therein. The detailed structure of the bonding layer 22 will be described later. (Substrate, Wiring Electrode, and Light Emitting Device) The substrate 11 is a ceramic substrate that is impermeable to gases and has excellent airtightness. For example, aluminum nitride (AlN), which has high thermal conductivity and excellent airtightness against gases, is used. The thermal conductivity of AlN ceramic is 150 to 170 (W / m K), and the thermal expansion coefficient is 4.5 to 4.6 (10 -6 ·K -1 ).
[0025] The base material of the substrate 11 may be silicon carbide (SiC), which has high thermal conductivity, or white alumina (Al2O3), which has high reflectivity. The thermal conductivity of SiC is 200 (W / m K) and the thermal expansion coefficient is 4.4 (10 -6 ·K -1 ), and the thermal conductivity of Al2O3 is 29~32 (W / m K) and the thermal expansion coefficient is 7.7~8 (10 -6 ·K -1 ).
[0026] 1D and 2A, a first wiring electrode (e.g., an anode electrode) 14A and a second wiring electrode (e.g., a cathode electrode) 14B, which are wiring electrodes in the semiconductor light emitting device 10, are provided on the substrate 11 (hereinafter, when no particular distinction is made, they will be referred to as wiring electrodes 14). A semiconductor light emitting element 15, such as a light emitting diode (LED) or a semiconductor laser, is bonded onto the first wiring electrode 14A by a metal bonding layer 15A, and a bonding pad 15B on the light emitting element 15 is electrically connected to the second wiring electrode 14B via a bonding wire 18C.
[0027] The light emitting element 15 is an aluminum gallium nitride (AlGaN)-based semiconductor light emitting element (LED) in which a semiconductor structure layer including an n-type semiconductor layer, a light emitting layer, and a p-type semiconductor layer is formed. In the light emitting element 15, the semiconductor structure layer is formed (bonded) on a conductive support substrate (silicon: Si) via a reflective layer.
[0028] The light emitting element 15 has an anode electrode (not shown) on a surface of the support substrate opposite to the surface to which the semiconductor structure layer is bonded (also referred to as the back surface of the light emitting element 15), and is electrically connected to the first wiring electrode 14A on the substrate 11. The light emitting element 15 also has a cathode electrode (pad 15B) on a surface of the light emitting element 15 opposite to the surface to which the semiconductor structure layer is bonded (also referred to as the front surface of the light emitting element 15), and is electrically connected to the second wiring electrode 14B via a bonding wire.
[0029] The light emitting element 15 is preferably an aluminum nitride type light emitting element that emits ultraviolet light with a wavelength of 265 to 415 nm. Specifically, a light emitting element with a central emission wavelength of 265 nm, 275 nm, 355 nm, 365 nm, 385 nm, 405 nm, or 415 nm is used.
[0030] The aluminum composition of the semiconductor crystal constituting an aluminum nitride-based ultraviolet light-emitting element (UV-LED element) is high, and it is easily oxidized and deteriorated by moisture (H2O) and excess oxygen (O2). As the gas filled in the semiconductor light-emitting device 10, a mixed gas containing dry nitrogen gas (or inert gas) and dry oxygen gas in the range of 3 to 20% is preferably used.
[0031] When a bonding material containing an organic substance such as flux is used to bond the light emitting element 15 to the first wiring electrode 14A, the residual flux (organic substance) of the bonding material causes the deposition of carbonized material on the surface of the light emitting element, but this can be prevented by mixing a small amount of O2 into the sealed gas. In this case, O2 is inactivated before it can deteriorate the light emitting element 15, so there is no problem.
[0032] Further, on the substrate 11, a protection element 16 which is a Zener diode (ZD) connected to the first wiring electrode 14A and the second wiring electrode 14B is provided to prevent the light emitting element 15 from being damaged by electrostatic discharge.
[0033] The substrate metal layer 12 is electrically insulated from the first wiring electrode 14A, the second wiring electrode 14B, the light emitting element 15, and the protective element 16, and is formed so as to surround these.
[0034] 1C, a first mounting electrode 17A and a second mounting electrode 17B (hereinafter, referred to as mounting electrodes 17 unless otherwise specified) connected to the first wiring electrode 14A and the second wiring electrode 14B, respectively, are provided on the back surface of the substrate 11. Specifically, the first wiring electrode 14A and the second wiring electrode 14B are each connected to the first mounting electrode 17A and the second mounting electrode 17B via metal vias 18A and 18B (hereinafter, referred to as metal vias 18 unless otherwise specified).
[0035] The wiring electrodes 14, the mounting electrodes 17, and the metal vias 18 are made of, for example, tungsten / nickel / gold (W / Ni / Au) or nickel chromium / gold / nickel / gold (NiCr / Au / Ni / Au). That is, the substrate 11 is an airtight substrate in which the vias are filled with metal to maintain airtightness.
[0036] Referring to FIG. 2A, the semiconductor light-emitting device 10 is configured to be mounted on a wiring circuit board (not shown). When a voltage is applied to the first mounting electrode 17A and the second mounting electrode 17B, the light-emitting element 15 emits light, and the emitted light LE from the surface (light extraction surface) of the light-emitting element 15 is radiated to the outside through the translucent cap 13. [Method of manufacturing the light emitting device 10] A method for manufacturing the light emitting device 10 will now be described in detail and specifically. (Element bonding process) First, a volatile solder paste solder for element bonding is applied onto the first wiring electrode 14A of the substrate 11. As the volatile solder paste, a volatile solder paste solder consisting of a flux having a boiling point near the melting point and fine particles of a gold-tin alloy (AuSn) is used. The gold-tin alloy used has a composition of Au-Sn: 20wt% with a melting temperature of about 280°C. The particle size is several nm to several tens of μm. The flux is, for example, rosins, alcohols, sugars, esters, fatty acids, oils and fats, polymerized oils, surfactants, organic acids, etc. that are carbonized by the light (365 nm) of the light emitting element 15.
[0037] Next, the light emitting element 15 is placed on the AuSn paste, and the substrate is heated to 300°C to melt and solidify the AuSn, thereby bonding the light emitting element 15 onto the first wiring electrode 14A. The light emitting element 15 is bonded while being self-aligned by the molten AuSn alloy. If a protective element 16 is to be mounted, this is done at the same time. At this time, most of the flux contained in the AuSn paste volatilizes.
[0038] Next, the bonding pad 15B of the upper electrode of the light emitting element 15 and the second wiring electrode 14B are electrically connected by a bonding wire 18C (Au wire). (Joining of light-transmitting cap 13 and substrate 11) The bonding process between the light-transmitting cap 13 and the substrate 11 will be described in detail with reference to Figures 3A and 3B. Figures 3A and 3B are schematic diagrams showing the bond between the cap metal layer 21 and the substrate metal layer 12 in steps 1 to 3 (STEP 1 to STEP 3) and steps 4 to 6 (STEP 4 to STEP 6), respectively. Cross-sectional views in each step are shown on the upper side, and plan views in a plane parallel to line AA of the cross-sectional views are shown on the lower side. Each of these diagrams shows a cross section and a plan view along the extension direction of the substrate metal layer 12. (STEP 1) First, the substrate 11 and the light-transmitting cap 13 are set in a cap bonding device. Next, the atmosphere of the substrate 11 and the light-transmitting cap 13 is evacuated, and the substrate 11 and the light-transmitting cap 13 are heat-treated (annealed) for 15 minutes at a temperature of 275° C. As described above, the substrate 11 and the light-transmitting cap 13 are airtight.
[0039] Next, the atmosphere of the substrate 11 and the light-transmitting cap 13 was filled with dry nitrogen (N2) gas at 1 atmosphere (101.3 kPa). Next, as shown in the cross-sectional view (upper side) and the plan view (lower side) of step 1 (STEP 1) in FIG. 3A, molten AuSn liquid 22D was sprayed from a nozzle NZ1 onto the substrate metal layer 12 to form an AuSn bump 22B.
[0040] The AuSn bumps 22B are preferably formed at regular intervals along line BB (circle CF in the case of FIG. 1D), which is the center line in the extension direction of the substrate metal layer 12. The AuSn bumps 22B preferably have the same size. The AuSn bumps 22B are formed over the entire extension direction of the annular substrate metal layer 12.
[0041] 1A and 1D are schematic diagrams showing the arrangement of AuSn bumps 22B when viewed from above (top view). The multiple AuSn bumps 22B are preferably formed along a circumference centered on center C of the annular substrate metal layer 12, particularly along a circumference CF passing through the center of the width of the annular ring.
[0042] The AuSn bump 22B is preferably formed to have a spherical or semispherical shape. For example, as described in Non-Patent Document 1 (Nagase & Co., Ltd. / Laser Reflow Solder Ball Jet System / Principle), a molten solder ball can be ejected from a capillary to form a semispherical solder bump on a substrate. (STEP 2) Next, a nano gold particle paste (hereinafter simply referred to as nano Au paste) 22N was discharged from the nozzle NZ2 and applied along the AnSn bumps 22B so as to cover the AnSn bumps 22B. At this time, the nano Au paste 22N was applied while being guided by the AnSn bumps 22B.
[0043] Here, as the nano Au paste 22N, for example, the low-temperature sintering paste AuRoFUSE (registered trademark) made by Tanaka Precious Metals, described in Non-Patent Document 2, can be used (https: / / tanaka-preciousmetals.com / jp / products / detail / aurofuse / ?nav=use). The nano Au paste is composed only of submicron-sized gold particles and a solvent, has low-temperature sintering performance, and is a halogen-free Au paste capable of gold-gold bonding at 200°C. In addition, it is capable of metal bonding with low electrical resistance and high thermal conductivity (150 W / m·K). (STEP3,4) Next, the flange metal layer 21 of the light-transmitting cap 13 is placed on the nano Au paste 22N (STEP 3), and the flange 13B (not shown) of the light-transmitting cap 13 is pressed (STEP 4). At this time, the flange 13B may be pressed so that the flange metal layer 21 abuts against the AnSn bump 22B. In this case, the AnSn bump 22B functions as a spacer.
[0044] By pressing the flange metal layer 21, the AnSn bumps 22B were embedded in the nano Au paste 22N. The nano Au paste 22N was formed spreading in a band shape on the substrate metal layer 12 (indicated by the arrow in the figure). (STEP5: necking process) Next, by performing a heat treatment at 200°C (first heat treatment), the flux evaporates and the nano-Au particles are sintered at a low temperature, bonding (necking) between adjacent particles. As a result, the nano-Au particle sintered layer becomes an Au mesh structure 22M, which is a breathable mesh (mesh) body. Note that the AuSn alloy does not melt in this heat treatment process (200°C). (STEP 5: Gas replacement process) In a nitrogen atmosphere, the environment of the bonded body of the light-transmitting cap 13 and the substrate 11 was alternately reduced and normal pressure several times under heat treatment at 200° C., and gas replacement was performed in the semiconductor light-emitting device 10 via the Au network structure 22M. Flux gas in the semiconductor light-emitting device 10 was exhausted by this operation.
[0045] Next, after reducing the pressure inside the semiconductor light-emitting device 10, a mixed gas of nitrogen (N2) and oxygen (O2) in a desired ratio (for example, 4:1) was used to return the pressure to normal, thereby introducing oxygen into the semiconductor light-emitting device 10. In this way, it is possible to replace the gas inside the semiconductor light-emitting device 10 via the nano Au mesh structure 22M, and a desired amount of oxygen (O2) gas can be introduced into the semiconductor light-emitting device 10. (STEP 6) Next, the temperature was raised to the melting temperature of the AuSn bumps 22B (i.e., a second heat treatment temperature higher than the first heat treatment temperature). For example, when the temperature was raised to 280°C, the molten AuSn (bonding metal) impregnated the gaps in the nano Au mesh structure 22M to form a highly airtight AuSn-impregnated mesh structure 22P.
[0046] Furthermore, the second heat treatment causes AuSn to permeate into the nano Au mesh structure 22M (arrow in the figure), forming an airtight bonding layer 22, while at the same time forming a cavity 22C inside the AuSn bump 22B from which the AuSn has been removed by the impregnation.
[0047] That is, as shown in Figures 3B and 2B, the bonding layer 22 is a bonding layer in which the nano Au network structure 22M is impregnated with AuSn, and contains cavities 22C with a size according to the impregnation of AuSn. The cavities 22C preferably have a hemispherical shape as shown in Figure 3B. In this case, the hemispherical surface serves as a stress dispersion surface, so that a bond with even higher stress resistance can be formed.
[0048] The above steps produced the semiconductor light-emitting device 10 in which the substrate 11 and the light-transmitting cap 13 were hermetically bonded. As described above, the substrate 11 and the light-transmitting cap 13 were bonded by the bonding layer 22, which is an impregnated bonded body having high airtightness and formed by impregnating the nano Au network structure 22M with a bonding metal.
[0049] More specifically, a flexible and strong bonding layer can be formed by the soft Au network and the hard AuSn medium, so that a bond with high stress resistance can be provided.
[0050] That is, the residual stress of the AuSn medium is absorbed by the Au network due to the bonding metal (AuSn) medium structure impregnated in the Au network, so that grain boundary fracture can be prevented (initiation prevention).
[0051] Furthermore, the Au network can prevent the growth of cracks (grain boundary fracture) that have occurred (prevention of crack growth).The cavity structure in the impregnated joint (AuSn bump) can break up the cracks that have occurred (or bend the growth path) (internal termination of crack growth).
[0052] In addition, the flux of the nano Au paste is removed, and the inside of the package is filled with a predetermined gas mixture. In other words, in the pre-impregnation state consisting of the breathable Au mesh body and the bonding metal (AuSn) bumps, after exhausting the inside of the package and removing the flux, it is possible to introduce the mixed gas into the inside of the package.
[0053] That is, without providing a gas replacement port (vent port) in the light-emitting element package consisting of the substrate 11 and the light-transmitting cap 13, gas replacement can be performed in the light-emitting element package, and the package can be filled with a desired gas. [Second embodiment] Fig. 4A is a cross-sectional view that typically shows a cross section of a semiconductor light-emitting device 50 according to a second embodiment of the present invention. In the semiconductor light-emitting device 10 of the first embodiment, the light-transmitting cap 13 is a package that includes a semispherical light-transmitting window and a flat flange, but this is not limiting. In the second embodiment, the light-transmitting cap 13 is configured as a disk-shaped flat plate. Fig. 4B is a partially enlarged cross-sectional view that shows an enlarged portion W where the substrate 11 and the light-transmitting cap 13 are joined.
[0054] More specifically, the annular outer edge of the light-transmitting cap 13 is the flange 13B, which is the cap joint, and the inside of that is the window portion 13A, which is the light-transmitting portion. For example, it is formed from a single disk-shaped glass. A ring-shaped flange metal layer 21 is fixed to the bottom surface of the flange 13B (i.e., the annular outer periphery of the bottom surface of the light-transmitting cap 13).
[0055] 4B, the flange metal layer 21 is joined to the substrate metal layer 12 by a bonding layer 22, which is an impregnated bonding material, to form a bonding portion 24, thereby maintaining airtightness between the substrate 11 and the light-transmitting cap 13. As in the first embodiment, the airtight substrate 11 and the airtight light-transmitting cap 13 are bonded to each other by the bonding layer 22 to form the semiconductor light-emitting device 50.
[0056] The semiconductor light emitting device 50 of this embodiment has a space HS for accommodating the semiconductor light emitting element 15 therein. More specifically, it is configured as a housing structure (frame structure) having the accommodating space HS which is a cylindrical recess defined by the substrate 11, a frame 11A formed and standing on the outer periphery of the substrate 11, and a light-transmitting cap 13. The light-transmitting cap 13 is joined onto the flat top surface of the frame 11A.
[0057] The bonding layer 22, which is an impregnated bonded body, is formed in the same manner as in the first embodiment. That is, as shown in Fig. 4B, the bonding layer 22 has a highly airtight AuSn-impregnated network structure 22P in which a nano Au network structure is impregnated with AuSn, and cavities 22C arranged on and along the substrate metal layer 12 and formed therein.
[0058] Therefore, the substrate 11 and the light-transmitting cap 13 are joined by a highly airtight joining layer 22 formed by impregnating the nano Au network structure 22M with a joining metal. Also, without providing a gas replacement port (vent port) in the light-emitting element package consisting of the substrate 11 and the light-transmitting cap 13, gas replacement can be performed in the accommodation space HS of the semiconductor light-emitting element in the light-emitting element package, and the inside of the package can be filled with a desired gas. Further embodiments In the above embodiment, the flange 13B bonding surface, i.e., the flange metal layer 21, has a circular ring shape, but this is not limited thereto. For example, the flange metal layer 21 may have a rectangular shape or an n-sided polygonal shape (n is an integer of 3 or more), and the substrate metal layer 12 may be configured to be bonded to the flange metal layer 21 with a shape and size corresponding to the flange metal layer 21.
[0059] Furthermore, when the substrate 11 has a space for accommodating the semiconductor light-emitting element 15, depending on the shapes of the substrate metal layer 12 and the flange metal layer 21, the accommodating space may have a rectangular prism shape or a polygonal prism shape, or may have a rectangular prism shape with rounded corners (chamfered).
[0060] As described above in detail, it is possible to provide a semiconductor light-emitting device and a manufacturing method thereof that can replace the inside of the package with an environment (gas atmosphere) in which the semiconductor light-emitting element is less likely to deteriorate, without providing a gas replacement port in the package, and that has high airtightness. [Explanation of symbols]
[0061] 10,50 Semiconductor light-emitting device 11 Substrate 11S board joint surface 12 Substrate metal layer 13 Translucent Cap 13A Window 13B Cap joint 13S Cap joint surface 14, 14A, 14B Wiring electrodes 15 Semiconductor light emitting device 21 Cap metal layer 22 Bonding layer 22B Bonding bump 22C cavity 22M Au network structure 22N Nano Au Paste 24 Joint HS Package Storage Space
Claims
1. A semiconductor light emitting element; an airtight substrate having a substrate bonding surface to which a wiring connected to the semiconductor light emitting device and a ring-shaped substrate metal layer surrounding the semiconductor light emitting device are fixed; a window portion that transmits the emitted light of the semiconductor light emitting element, and a flange portion to which a ring-shaped cap metal layer corresponding to the substrate metal layer is fixed, the cap metal layer being bonded to the substrate metal layer by a bonding layer, the cap metal layer having an internal space for accommodating the semiconductor light emitting element, and an airtight light-transmitting cap that is airtightly bonded to the substrate, The semiconductor light emitting device, wherein the bonding layer is an impregnated bonded body in which a gold (Au) mesh structure is impregnated with a bonding metal.
2. 2. The semiconductor light emitting device of claim 1, wherein said impregnated joint body has cavities arranged therein.
3. The semiconductor light emitting device of claim 2 , wherein the cavity has a hemispherical shape.
4. 4. The semiconductor light emitting device according to claim 1, wherein the internal space is filled with a mixed gas containing nitrogen and oxygen.
5. 5. The semiconductor light emitting device according to claim 4, wherein the mixed gas contains oxygen in the range of 3 to 20%.
6. 6. The semiconductor light emitting device according to claim 1, wherein the semiconductor light emitting element is an AlGaN-based light emitting element.
7. A method for manufacturing the semiconductor light emitting device according to any one of claims 1 to 6, comprising the steps of: A plurality of bonding material bumps are arranged on the substrate metal layer along an extending direction of the substrate metal layer of the airtight substrate; Applying nano Au paste so as to embed the plurality of bonding material bumps; The flange portion is pressed while the cap metal layer is placed on the nano Au paste. Sintering the nano Au paste at a first heat treatment temperature to form an Au network structure and bond the substrate and the airtight transparent cap; placing the assembly of the substrate and the light-transmitting cap under a reduced pressure environment to evacuate the internal space; After the evacuation, the assembly is placed in an environment of a predetermined gas and a pressure higher than the reduced pressure environment, and the interior space is replaced with the predetermined gas; After the replacement with the predetermined gas, the bonding material of the bonding material bumps is impregnated into the Au mesh structure at a second heat treatment temperature higher than the first heat treatment temperature.
8. The method for manufacturing a semiconductor light emitting device according to claim 7 , wherein the step of evacuating the interior space includes the step of evacuating flux contained in the nano Au paste from the interior space.
9. 9. The method for manufacturing a semiconductor light emitting device according to claim 7, wherein the step of impregnating the Au mesh structure with the bonding material includes a step of forming cavities arranged inside the impregnated bonding body.
10. The method for manufacturing a semiconductor light emitting device according to claim 7 , wherein the bonding material is AuSn.
Citation Information
Patent Citations
Semiconductor device
JP2006093372A
Package for housing optical element, optical device, and its manufacturing method
JP2007123444A
Electronic-component apparatus
JP2007287967A
Light emitting element and method for manufacturing the same
JP2018142690A
Method of manufacturing semiconductor device
JP2019220672A