Semiconductor light emitting device and its manufacturing method

The semiconductor light-emitting device addresses airtightness and bonding reliability issues by using dimpled metal layers to disperse stress and form an airtight joint, enhancing durability and environmental resistance.

JP7554694B2Active Publication Date: 2024-09-20STANLEY ELECTRIC CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021039981
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-12
Publication Date
2024-09-20
Estimated Expiration
2041-03-12

AI Technical Summary

Technical Problem

Semiconductor light-emitting devices, particularly those emitting ultraviolet light, face issues with insufficient airtightness and bonding reliability, leading to deterioration due to moisture and stress-induced cracks, which compromise their long-term performance and reliability.

Method used

A semiconductor light-emitting device design featuring a substrate with a ring-shaped metal layer and a cap metal layer, where dimples on one layer allow bonding material to flow into, forming an airtight joint by melting and cooling AuSn bumps, thereby dispersing stress and preventing cracks.

Benefits of technology

The design maintains high airtightness and environmental resistance, suppressing crack generation and improving bonding reliability, ensuring long-term durability and resistance to moisture and corrosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554694000012
    Figure 0007554694000012
  • Figure 0007554694000004
    Figure 0007554694000004
  • Figure 0007554694000006
    Figure 0007554694000006
Patent Text Reader

Abstract

To provide a semiconductor device capable of suppressing occurrence of a crack in a junction part and having a highly-reliable airtight junction allowing for maintaining high airtightness even in long-time use, and a method for manufacturing the same.SOLUTION: A semiconductor light-emitting device comprises: a semiconductor light-emitting element; an airtight substrate including a wiring connected to the semiconductor light-emitting element and a substrate bonding surface to which an annular-shape substrate metal layer 12 surrounding the semiconductor light-emitting element is fastened; and an airtight translucent cap including a window part for transmitting radiant light of the semiconductor light-emitting element, a cap junction part to which an annular-shape cap metal layer corresponding to the substrate metal layer is fastened, and an internal space for housing the semiconductor light-emitting element, a cap metal layer 21 joined to the substrate metal layer 12 by a junction layer 22. One of the substrate metal layer and the cap metal layer includes a plurality of dimples 12D arranged along an extension direction of the metal layer. A joining material of the junction layer flows into the plurality of dimples.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor light emitting device and a manufacturing method thereof, and more particularly to a semiconductor light emitting device in which a semiconductor light emitting element that emits ultraviolet light is enclosed, and a manufacturing method thereof. [Background technology]

[0002] Conventionally, there has been known a semiconductor device in which a semiconductor element is enclosed inside a semiconductor package. In the case of a semiconductor light emitting module, a transparent window member such as glass that transmits light from the light emitting element is bonded to a support on which the semiconductor light emitting element is mounted, thereby hermetically sealing the semiconductor light emitting element.

[0003] For example, Patent Document 1 discloses a structure in which a fillet is formed in a sealing portion when a glass window member is bonded to a ceramic substrate having a recess.

[0004] Patent Document 2 discloses a structure in which a metal layer provided on a glass cover is embedded in a metal bonding member on a ceramic substrate provided with a recess for accommodating a semiconductor light emitting element.

[0005] Moreover, Patent Document 3 discloses a structure in which a ceramic support and a spacer body are bonded with an AuSn bonding layer.

[0006] Furthermore, Patent Document 4 discloses a structure in which a second metal layer provided on a glass window member is embedded in a metal bonding member on a ceramic substrate having a recess. An optical semiconductor device is disclosed in which light output from a side surface of an optical semiconductor element is reflected by a metal layer provided on an inclined light reflecting surface and directed toward a window member, thereby increasing optical output. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2015-18873 A [Patent Document 2] JP 2018-93137 A [Patent Document 3] JP 2016-127255 A [Patent Document 4] JP 2018-037583 A [Non-patent literature]

[0008] [Non-Patent Document 1] Nagase & Co., Ltd. https: / / www.nagase-pactech.jp / solder / spec / Summary of the Invention [Problem to be solved by the invention]

[0009] However, there is a demand for further improvements in the sealing performance and bonding reliability between the substrate and the window member. In particular, semiconductor light-emitting elements that emit ultraviolet light, such as AlGaN-based semiconductor light-emitting elements, are prone to deterioration if the airtightness is insufficient, and therefore high airtightness is required for semiconductor devices equipped with such semiconductor light-emitting elements.

[0010] Furthermore, AlGaN crystals are subject to degradation due to moisture. In particular, the shorter the wavelength of emitted light, the greater the Al composition, making them more susceptible to degradation. To prevent moisture from entering the package that houses the light-emitting element, a structure was adopted in which the substrate and glass lid were sealed with a metal bonding material, but this was problematic in that the airtightness was insufficient when used in humid environments or around water.

[0011] For example, a metal layer is provided on each of the ceramic substrate and the window member, and a bonding material such as a gold-tin (AuSn) sheet or bumps is sandwiched between these metal layers and fused to form an airtight structure.

[0012] However, the inventors of the present application have discovered a joint formed by sandwiching a piece of bonding material arranged in a bump shape between metal layers and bonding the bonding material by pressing and melting it. That is, when melting and bonding, adjacent bumps are combined. Then, stress is applied to the combined part, which causes cracks and the like in the joint, resulting in poor airtightness and reduced reliability. In addition, excess bonding material may flow out of the package, causing poor appearance and short circuit defects.

[0013] The present invention has been made in consideration of the above-mentioned points, and aims to provide a semiconductor device having high reliability, in which high airtightness is maintained even during long-term use, and high environmental resistance, such as moisture resistance, corrosion resistance, etc., and a manufacturing method thereof. Another aim is to provide a semiconductor device having a highly reliable airtight bond, in which stress that causes cracks in the bonded portion is suppressed and deterioration inside the bonded layer can be prevented, and a manufacturing method thereof. [Means for solving the problem]

[0014] A semiconductor light emitting device according to one embodiment of the present invention comprises: A semiconductor light emitting element; an airtight substrate having a substrate bonding surface to which a wiring connected to the semiconductor light emitting device and a ring-shaped substrate metal layer surrounding the semiconductor light emitting device are fixed; a window portion that transmits the emitted light of the semiconductor light emitting element, and a cap bonding portion to which a ring-shaped cap metal layer corresponding to the substrate metal layer is fixed, the cap metal layer being bonded to the substrate metal layer by a bonding layer, and an airtight light-transmitting cap having an internal space for accommodating the semiconductor light emitting element and airtightly bonded to the substrate, one of the substrate metal layer and the cap metal layer has a plurality of dimples arranged along an extension direction of the one metal layer; The bonding material of the bonding layer flows into the plurality of dimples.

[0015] A method for manufacturing a semiconductor light emitting device according to another embodiment of the present invention is a method for manufacturing the semiconductor light emitting device described above, comprising the steps of: (a) arranging a plurality of bonding material bumps on the substrate metal layer along an extending direction of the substrate metal layer; (b) placing the cap metal layer on the plurality of bonding material bumps, and heating the cap bonding portion while pressing the cap metal layer to melt the plurality of bonding material bumps; (c) melting and then cooling the plurality of bonding material bumps to bond the substrate metal layer and the cap metal layer; The plurality of bonding material bumps are arranged at positions such that, when the plurality of bonding material bumps melt, the bonding material of the adjacent bonding material bumps flows into each of the plurality of dimples. [Brief description of the drawings]

[0016] [Figure 1A] 1 is a plan view diagrammatically illustrating the upper surface of a semiconductor light emitting device 10 according to a first embodiment. [Figure 1B] 1 is a diagram illustrating a schematic side view of a semiconductor light emitting device 10. FIG. [Figure 1C] 2 is a plan view showing a schematic view of the back surface of the semiconductor light emitting device 10. FIG. [Figure 1D] 1 is a diagram illustrating a schematic internal structure of a semiconductor light emitting device 10. FIG. [Figure 2A] 1B is a cross-sectional view that illustrates a schematic cross section of the semiconductor light-emitting device 10 taken along line AA in FIG. 1A. [Figure 2B] 2B is a partially enlarged cross-sectional view showing a cross section of a joint (part W) in FIG. 2A. FIG. [Diagram 3] FIG. 2 is a diagram showing a schematic view of a joint between a substrate metal layer and a cap metal layer. [Figure 4] 10A to 10C are cross-sectional views each showing a schematic diagram of a bonding process between the light-transmitting cap and the substrate. [Diagram 5] FIG. 1 is a plan view showing a schematic diagram of how AuSn bumps spread and coalesce when heated and melted. [Figure 6] FIG. 11 is a plan view showing a schematic arrangement of AuSn bumps according to a second embodiment of the present invention. [Figure 7A] FIG. 13 is a plan view showing a schematic arrangement of AuSn bumps according to a third embodiment of the present invention. [Figure 7B] FIG. 13 is a schematic diagram showing a cavity when AuSn bumps are combined. [Figure 8] FIG. 11 is a diagram illustrating a modified example of the first embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] In the following, preferred embodiments of the present invention will be described, which may be modified and combined as appropriate. In the following description and accompanying drawings, substantially the same or equivalent parts are designated by the same reference numerals.

[0018] [First embodiment] Fig. 1A is a plan view typically showing the top surface of a semiconductor light emitting device 10 according to a first embodiment of the present invention. Fig. 1B is a diagram typically showing a side surface of the semiconductor light emitting device 10. Fig. 1C is a plan view typically showing the back surface of the semiconductor light emitting device 10. Fig. 1D is a diagram typically showing the internal structure of the semiconductor light emitting device 10.

[0019] Moreover, Fig. 2A is a cross-sectional view that illustrates a cross section of the semiconductor light emitting device 10 taken along the line AA in Fig. 1A. Fig. 2B is a partially enlarged cross-sectional view that illustrates an enlarged cross section of the joint portion (portion W) in Fig. 2A.

[0020] 1A and 2A, the substrate 11 of the semiconductor light emitting device 10 has a recess HS which is a space for accommodating the semiconductor light emitting element 15 therein. More specifically, the substrate 11 is configured as a housing structure (frame structure) having a rectangular columnar recess RC defined by a frame 11A which is a frame portion formed in an upright position on the outer periphery of the substrate 11.

[0021] The side surfaces of the substrate 11 are parallel to the x and y directions, and the top surface of the substrate 11 is parallel to the xy plane. (Substrate 11, light-transmitting cap 13, substrate metal layer 12, and cap metal layer 21) As shown in FIGS. 1A to 1D, a semiconductor light emitting device 10 is configured by bonding a rectangular frame-shaped substrate 11 to a light-transmitting cap 13 which is a light-transmitting window made of rectangular flat glass plate.

[0022] The substrate 11 is a ceramic substrate that is impermeable to gases and has excellent airtightness. For example, aluminum nitride (AlN), which has high thermal conductivity and excellent airtightness against gases, is used. The thermal conductivity of AlN ceramic is 150 to 170 (W / m K), and the thermal expansion coefficient is 4.5 to 4.6 (10 -6 ·K -1 ).

[0023] The base material of the substrate 11 may be silicon carbide (SiC), which has high thermal conductivity, or white alumina (Al2O3), which has high reflectivity. The thermal conductivity of SiC is 200 (W / m K) and the thermal expansion coefficient is 4.4 (10 -6 ·K -1 ), and the thermal conductivity of Al2O3 is 29~32 (W / m K) and the thermal expansion coefficient is 7.7~8 (10 -6 ·K -1 ).

[0024] As shown in FIG. 2A, a rectangular ring-shaped metal layer 12 (hereinafter also referred to as substrate metal layer 12) is formed on the top surface 11T of the frame 11A of the substrate 11 and is joined to an airtight translucent cap 13.

[0025] Substrate metal layer 12 has a structure (W (or Cu) / Ni / Au) in which tungsten (or copper), nickel, and gold are laminated in this order on substrate 11 (the Au layer is the outermost layer). Alternatively, a structure (NiCr / Au / Ni / Au) in which nickel chromium, gold, nickel, and gold are laminated can be used. When forming the substrate metal layer 12 after firing the substrate ceramic of substrate 11, high adhesion to substrate 11 can be obtained by selecting a metal that is easily nitrided (or oxidized in the case of oxide ceramic) for the metal in contact with the substrate ceramic.

[0026] The light-transmitting cap 13 has a window portion 13A and a cap joint portion 13B. More specifically, the outer edge portion of the rectangular ring shape of the light-transmitting cap 13 is the cap joint portion 13B, and the inside thereof is the window portion 13A which is a light-transmitting portion.

[0027] The light-transmitting cap 13 is made of light-transmitting glass that transmits the light emitted from the light-emitting element 15 disposed in the semiconductor light-emitting device 10. For example, quartz glass, borosilicate glass, or sapphire glass can be suitably used.

[0028] A rectangular ring-shaped cap metal layer 21 is fixed to the bottom surface of the cap bonding portion 13B, and a bonding surface 13S (hereinafter also referred to as the cap bonding surface) is formed. The window portion 13A of the light-transmitting cap 13 can also be convex, concave, convex lens-like, or concave lens-like.

[0029] The cap metal layer 21 may be, for example, a chromium / nickel / gold (Cr / Ni / Au) layer or a titanium / palladium / copper / nickel / gold (Ti / Pd / Cu / Ni / Au) layer (with the Au layer being the outermost layer).

[0030] 2A, the cap metal layer 21 is bonded to the substrate metal layer 12 by the bonding layer 22 to form a bonding portion 24, thereby maintaining airtightness between the substrate 11 and the light-transmitting cap 13. That is, the cap metal layer 21 has a shape and size corresponding to the substrate metal layer 12, and they are bonded to each other by the bonding layer 22 so as to be concentric.

[0031] It is preferable that the surface (substrate bonding surface) 11S of the substrate 11 to which the substrate metal layer 12 is fixed and the cap bonding surface 13S to which the cap metal layer 21 is fixed are flat surfaces.

[0032] (Wiring electrodes, light-emitting elements, protective elements) As shown in Figures 1D and 2A, a first wiring electrode (e.g., an anode electrode) 14A and a second wiring electrode (e.g., a cathode electrode) 14B, which are wiring electrodes within the semiconductor light-emitting device 10, are provided on the main surface of the substrate 11 (hereinafter, unless otherwise specified, they will be collectively referred to as wiring electrodes 14).

[0033] In addition, a semiconductor light-emitting element 15 such as a light-emitting diode (LED) or a semiconductor laser is bonded onto the first wiring electrode 14A by a metal bonding layer 15A, and a bonding pad 15B of the light-emitting element 15 is electrically connected to the second wiring electrode 14B via a bonding wire 18C.

[0034] The light emitting element 15 is an aluminum gallium nitride (AlGaN)-based semiconductor light emitting element (LED) in which a semiconductor structure layer including an n-type semiconductor layer, a light emitting layer, and a p-type semiconductor layer is formed. In the light emitting element 15, the semiconductor structure layer is formed (bonded) on a conductive support substrate (silicon: Si) via a reflective layer.

[0035] The light emitting element 15 has an anode electrode (not shown) on the surface of the support substrate opposite to the surface to which the semiconductor structure layer is bonded (the back surface of the light emitting element 15), and is electrically connected to the first wiring electrode 14A on the substrate 11. The light emitting element 15 also has a cathode electrode (pad 15B) on the surface of the semiconductor structure layer opposite to the surface to which the support substrate is bonded (also referred to as the front surface of the light emitting element 15), and is electrically connected to the second wiring electrode 14B via a bonding wire.

[0036] The light emitting element 15 is preferably an aluminum nitride type light emitting element that emits ultraviolet light with a wavelength of 265 to 415 nm. Specifically, a light emitting element with a central emission wavelength of 265 nm, 275 nm, 355 nm, 365 nm, 385 nm, 405 nm, or 415 nm is used.

[0037] The aluminum composition of the semiconductor crystals constituting aluminum nitride-based ultraviolet-emitting light-emitting elements (UV-LED elements) is high, and they are easily oxidized and deteriorated by oxygen (O2) and moisture (H2O). If a bonding material containing an organic substance such as flux is used to bond the light-emitting element 15 to the first wiring electrode 14A, the residual flux (organic substance) causes carbide deposition on the surface of the light-emitting element.

[0038] It is preferable to use a mixed gas containing 3 to 20% of dry nitrogen gas (or an inert gas) and dry oxygen gas as the gas filled in the semiconductor light emitting device 10. By mixing a small amount of O2 into the filled gas, carbide deposition can be prevented, and at the same time, the mixed O2 is inactivated before it can deteriorate the light emitting element 15, so this does not cause any problems.

[0039] The light emitting element 15 may be of the type in which a semiconductor structure layer is bonded to a support substrate as described above, or may be of the type having a semiconductor structure layer on a growth substrate that transmits light emitted from the semiconductor structure layer.

[0040] For example, when the growth substrate is conductive, a cathode electrode (not shown) is provided on the back surface of the growth substrate (the surface opposite to the semiconductor structure layer), and an anode electrode (a pad electrode for bonding wire connection) is provided on the upper surface of the semiconductor structure layer. In the light emitting element, the cathode electrode is bonded onto the first wiring electrode 14A via a metal bonding layer 15A, and the pad electrode and the second wiring electrode 14B are electrically connected via a bonding wire 18C.

[0041] In addition, when the growth substrate is insulating, an anode electrode is provided on the p-type semiconductor layer on the upper surface side of the semiconductor structure layer, and a cathode electrode is provided on the n-type semiconductor layer. In the light emitting element, the anode electrode and the cathode electrode are bonded to the first wiring electrode 14A and the second wiring electrode 14B, respectively, via a metal bonding layer.

[0042] Further, on the substrate 11, a protection element 16 which is a Zener diode (ZD) connected to the first wiring electrode 14A and the second wiring electrode 14B is provided to prevent the light emitting element 15 from being damaged by electrostatic discharge.

[0043] The substrate metal layer 12 is electrically insulated from the first wiring electrode 14A, the second wiring electrode 14B, the light emitting element 15, and the protective element 16, and is formed so as to surround these.

[0044] 1C, a first mounting electrode 17A and a second mounting electrode 17B (hereinafter, referred to as mounting electrodes 17 unless otherwise specified) connected to the first wiring electrode 14A and the second wiring electrode 14B, respectively, are provided on the back surface of the substrate 11. Specifically, the first wiring electrode 14A and the second wiring electrode 14B are each connected to the first mounting electrode 17A and the second mounting electrode 17B via metal vias 18A and 18B (hereinafter, referred to as metal vias 18 unless otherwise specified).

[0045] The wiring electrodes 14 and the mounting electrodes 17 are made of, for example, tungsten / nickel / gold (W / Ni / Au) or copper / nickel / gold (Cu / Ni / Au), and the metal vias 18 are made of tungsten (W) or copper (Cu).

[0046] Referring to FIG. 2A, the semiconductor light-emitting device 10 is configured to be mounted on a wiring circuit board (not shown). When a voltage is applied to the first mounting electrode 17A and the second mounting electrode 17B, the light-emitting element 15 emits light, and the emitted light LE from the surface (light extraction surface) of the light-emitting element 15 is radiated to the outside through the translucent cap 13.

[0047] [Method of manufacturing the light emitting device 10] A method for manufacturing the light emitting device 10 will now be described in detail and specifically.

[0048] (Element bonding process) First, a volatile solder paste solder for element bonding is applied onto the first wiring electrode 14A of the substrate 11. The volatile solder paste used is a volatile solder paste solder consisting of flux that volatilizes near the melting point and fine particles of a gold-tin alloy (AuSn). The gold-tin alloy used has a composition of Au-Sn: 20wt% with a melting temperature of about 280°C. The particle size is several nm to several tens of μm. The flux is, for example, rosins, alcohols, sugars, esters, fatty acids, oils and fats, polymerized oils, surfactants, organic acids, etc. that are carbonized by the light (365 nm) of the light emitting element 15.

[0049] Next, the light emitting element 15 is placed on the AuSn paste, and the substrate is heated to 300°C to melt and solidify the AuSn, thereby bonding the light emitting element 15 onto the first wiring electrode 14A. The light emitting element 15 is bonded while being self-aligned by the molten AuSn alloy. If a protective element 16 is to be mounted, this is done at the same time. At this time, most of the flux contained in the AuSn paste volatilizes.

[0050] Next, the bonding pad 15B of the upper electrode of the light emitting element 15 and the second wiring electrode 14B are electrically connected by a bonding wire 18C (Au wire). (Joining of light-transmitting cap 13 and substrate 11) Fig. 3 is a diagram showing a schematic diagram of a bond 24 between the substrate metal layer 12 and the cap metal layer 21. Specifically, a cross-sectional view of the bond 24 is shown on the lower side of Fig. 3, and a cross-sectional view (as viewed from above) on a plane parallel to the line AA shown in the cross-sectional view is shown on the upper side.

[0051] A bonding layer 22 is formed along a center line CX in the extension direction (x direction) of the substrate metal layer 12. Dimples (depressions) 12D are formed at a constant period DP (FIG. 5) along the center line CX in the substrate metal layer 12. In this embodiment, the dimples 12D are formed as hemispherical depressions.

[0052] 4 is a cross-sectional view that typically illustrates a step of bonding the light-transmitting cap 13 to the substrate 11. The step of bonding the substrate metal layer 12 of the substrate 11 to the cap metal layer 21 of the light-transmitting cap 13 will be described in detail below with reference to FIG.

[0053] (STEP 1) First, the substrate 11 and the light-transmitting cap 13 were set in a cap bonding device. Next, the atmosphere around the substrate 11 and the light-transmitting cap 13 was evacuated, and the substrate 11 and the light-transmitting cap 13 were subjected to a heat treatment (annealing treatment) at a temperature of 275° C. for 15 minutes.

[0054] Next, the atmosphere of the substrate 11 and the light-transmitting cap 13 was filled with dry nitrogen (N2) gas at 1 atmosphere (101.3 kPa). Next, as shown in the cross-sectional view of step 1 (STEP 1) in FIG. 4, a molten AuSn liquid 22D was sprayed from a nozzle NZ1 onto the substrate metal layer 12 to form a bump 22B of a bonding material (AuSn).

[0055] The AuSn bumps 22B are preferably formed at regular intervals so as to be positioned midway between adjacent dimples 12D along the center line CX in the extending direction of the substrate metal layer 12. Also, the AuSn bumps 22B preferably have the same size and shape.

[0056] Similarly, AuSn bumps 22B were formed at regular intervals along center line CY in the other extension direction (y direction) of substrate metal layer 12. That is, they were formed along the entire extension direction of rectangular ring-shaped substrate metal layer 12.

[0057] The AuSn bump 22B is preferably formed to have a spherical or semispherical shape. For example, as described in Non-Patent Document 1, a molten solder ball can be ejected from a capillary to form a semispherical solder bump on a substrate.

[0058] (STEP 2) Next, the cap metal layer 21 of the light-transmitting cap 13 was placed on the AuSn bumps 22B, and the light-transmitting cap 13 was pressed while melting the AuSn bumps 22B. As a result, the AuSn bumps 22B spread between the substrate metal layer 12 and the cap metal layer 21, and adjacent AuSn bumps 22B merged. AuSn flowed into the dimples 12D due to the melting.

[0059] (STEP 3) After the light-transmitting cap 13 was sufficiently pressed, it was cooled to room temperature, whereby a bonding layer 22 was formed between the substrate metal layer 12 and the cap metal layer 21.

[0060] (Reduction of stress) 5 is a plan view showing a schematic diagram of AuSn bumps 22B (centers C) spreading and merging when heated and melted. AuSn bumps 22B are formed at regular intervals along center line CX in the extending direction of substrate metal layer 12.

[0061] When heated and melted, the hemispherical AuSn bumps 22B wet and spread (indicated by dashed arrows in the figure) in concentric circles (indicated by dashed lines and dashed lines in the figure), and adjacent bumps 22B join together to form a bonding layer 22 that is an airtight bond.

[0062] At this time, the merger boundary line where adjacent bumps 22B merge is formed linearly in a direction RS perpendicular to the center line CX, with the dimple 12D as the boundary, and at the same time, stress generated at the merger boundary line is dissipated in the direction RS perpendicular to the center line CX. In the present invention, since the dimple 12 is disposed approximately at the center of the merger boundary line, the molten AuSn of the adjacent bumps 22B flows into and mixes with the dimple 12D. As a result, the merger boundary line disappears or becomes distorted at the dimple 12D, and is divided into two parts, upper and lower.

[0063] Furthermore, residual stress that occurs when the molten AuSn solidifies within the dimples 12D is dispersed radially by the dimples 12D.

[0064] Therefore, according to this embodiment, the stress generated in the joint portion of the bonding material (AuSn) can be dissipated, and is also dispersed within the dimple 12D, improving the bonding reliability. For example, even if a heat shock caused by soldering when mounting the light emitting device 10 on a wiring circuit board (not shown) or stress caused by temperature changes (power ON / OFF, ambient temperature) when the light emitting device 10 is in use acts on the bonding layer 22 and causes a crack at the combined boundary line, the dimple 12D can prevent the crack from growing.

[0065] [Second embodiment] 6 is a plan view showing a schematic arrangement of AuSn bumps 22B according to the second embodiment of the present invention. The second embodiment is similar to the first embodiment in that dimples 12D are formed at regular intervals in the extension directions (x and y directions) of substrate metal layer 12.

[0066] Referring to Figure 6, in forming the bonding layer 22 in the second embodiment, the AuSn bumps 22B are arranged as two rows of bumps on center lines B1 and B2 spaced apart by d1 and d2, respectively, on both sides of the extension direction of the substrate metal layer 12, i.e., in a direction perpendicular to the center line CX of the extension direction of the substrate metal layer 12 (in this case, the y direction).

[0067] More specifically, in the step (STEP 1) of arranging the AuSn bumps 22B, the line on which the dimples 12D are arranged is set as the center line (in this case, CX), and the AuSn bumps 22B1 and 22B2 (centers C1, C2, respectively) are arranged alternately on either side of the center line CX along the center line CX in two rows of bumps in a staggered pattern at a certain angle (e.g., 45°).

[0068] 6, the AuSn bumps 22B1 and 22B2 have the same size, and the lines B1 and B2 have the same interval d (=d1=d2). That is, the hemispherical AuSn bumps 22B1 and 22B2 expand concentrically when heated and melted (indicated by dashed arrows in the figure), and adjacent bumps 22B are joined together to form the bonding layer 22, which is an airtight bond.

[0069] The size and arrangement of the AuSn bumps 22B1 and 22B2 may be determined so that the AuSn of the AuSn bumps 22B1 and 22B2 spreads when melted and the combined portion of the AuSn bumps matches the dimple 12D.

[0070] In the second embodiment, the stress at the joining portion of the bump 22B is also dispersed by the dimple 12D. Moreover, the stress generated at the joining portion is dispersed radially within the hemispherical dimple 12D. Note that the dimple 12D is not limited to a hemispherical shape, but may be a hemispherical or semi-ellipsoidal shape. In this specification, the term hemispherical includes a hemispherical or semi-ellipsoidal shape.

[0071] According to the second embodiment, stress is dissipated in a direction RS that is inclined (θ=45°) with respect to the extension direction (x direction) of the substrate metal layer 12 (arrow in the figure). Since the extension direction (x direction) of the substrate metal layer 12 is the main direction of thermal expansion when heat is generated, the tensile stress (x direction) acting on the combined portion of the bump 22B (the combined boundary line inclined in the direction RS) is dispersed and reduced by the amount of the inclination, and the occurrence and growth of cracks can be suppressed. The arrangement angle θ of the AuSn bumps 22B1 and 22B2 with respect to the extension direction of the substrate metal layer 12 is not limited to 45°, but it is preferable that 30°≦θ<60° in terms of stress dispersion and offsetting of stress components.

[0072] In the second embodiment, by arranging the AuSn bumps 22B1 and 22B2 in a staggered pattern, the width of the bonding material (AuSn) that spreads when melted during bonding can be narrowed, and the bonding material can be prevented from leaking inside and outside the package.

[0073] Furthermore, in the second embodiment, a plurality of dimples 12E (additional dimples) are arranged along the sides of both ends of the annular substrate metal layer 12. At least one dimple 12E is provided at each position corresponding to the positions of the AuSn bumps 22B1 and 22B2. The bonding material that spreads due to melting is trapped by the dimples 12E, so that the bonding material can be prevented from leaking to the inside and outside of the package.

[0074] Therefore, also in the second embodiment, the stress generated in the joint portion of the bonding material (AuSn) can be dissipated, and is dispersed within the dimple 12D, improving the bonding reliability.

[0075] [Third embodiment] 7A is a plan view showing a schematic arrangement of AuSn bumps 22B according to a third embodiment of the present invention. In the third embodiment, dimple group 12D is formed at a constant period DP in the extension directions (x and y directions) of substrate metal layer 12. Dimple group 12D has dimples 12D1, 12D2A, and 12D2B (hereinafter referred to as 12D2 when no distinction is made), and 12D3.

[0076] Dimples 12D1, 12D2, and 12D3 of dimple group 12D are arranged in a row on center line GC. In the third embodiment, center line GC of dimple group 12D consisting of dimples 12D1, 12D2A, and 12D3 is inclined at an inclination angle θ=θ D (hereinafter referred to as θ) The same is true for dimple group 12D consisting of dimples 12D1, 12D2B, and 12D3.

[0077] In the third embodiment, the inclination angle θ of the center line GC of the dimple group 12D relative to the center line CX of the substrate metal layer 12 is 60°. The dimple group 12D is arranged so as to form one side of a densely-arranged equilateral triangle TR. That is, the dimple group 12D is arranged at an inclination angle θ (=60° or -60°) and at regular intervals DP in the extension direction (x direction) of the substrate metal layer 12, and the length of the dimple group 12D (the distance from the center of dimple 12D1 to the center of dimple 12D3) is equal to the length of one side of the equilateral triangle TR. Note that one of the dimples 12D2, i.e., one of dimples 12D2A or 12D2B, may not be provided.

[0078] More specifically, in forming the bonding layer 22, the AuSn bumps 22B are arranged in two bump rows on centerlines B1 and B2 spaced apart by a distance d on either side of the centerline CX of the substrate metal layer 12.

[0079] More specifically, in the step (STEP 1) of arranging the AuSn bumps 22B, the AuSn bumps 22B1 and 22B2 (centers C1 and C2, respectively) are arranged alternately on both sides of the center line CX as two bump rows in a staggered manner at an angle of 60 degrees.

[0080] In other words, the AuSn bumps 22B1 and 22B2 are arranged so that their centers C1, C2 are located at the vertices of an equilateral triangle. The AuSn bumps 22B1 and 22B2 are the same size, and the joining portions of adjacent AuSn bumps 22B1 and 22B2 match with the dimples 12D1, 12D2, and 12D3.

[0081] With this arrangement, when the bonding material (AuSn) is heated and melted, the hemispherical AuSn bumps 22B wet and spread (dashed arrows in the figure) in a concentric manner (dashed lines and dashed lines in the figure), and adjacent bumps 22B merge with each other to form a bonding layer 22 with an airtight bond.

[0082] The stress is then dissipated at the joining portion of the AuSn bumps 22B1 and 22B2. The stress generated in the dimple 12D is dispersed radially within the hemispherical dimple 12D.

[0083] Furthermore, in this embodiment, leakage will not occur unless the combined portions on a straight line inclined to the extending direction of substrate metal layer 12, ie, dimples 12D1, 12D2, and 12D3, are simultaneously broken, improving leakage resistance.

[0084] Furthermore, as shown in FIG. 7B, a portion (cavity) 12C without the bonding material (AuSn) remains in the portion where the AuSn bumps 22B1 and 22B2 are not joined. The cavity 12C divides the bonding portion (bonding boundary line) and breaks the propagation of stress. Therefore, it is difficult to break and the leak resistance is improved.

[0085] Therefore, in the second embodiment, the stress generated in the bonding portion of the bonding material (AuSn) is dispersed and reduced, improving the bonding reliability. Also, since no leakage occurs unless the three bonding portions of the bonding material formed on a straight line inclined with respect to the extending direction of the substrate metal layer 12 are simultaneously broken, a sealing structure with high leakage resistance is obtained.

[0086] [Modifications of the first to third embodiments] 8 is a plan view diagrammatically illustrating an arrangement of AuSn bumps 22B according to a modified example of the first embodiment of the present invention. In the above-described first to third embodiments, the case where dimples 12D are provided on substrate metal layer 12 has been described, but dimples 21D may be provided on cap metal layer 21.

[0087] FIG. 8 is a diagram showing a bonding process of a modified example of the first embodiment described with reference to FIG.

[0088] First, in STEP 1, AuSn bumps 22B are formed and arranged at a constant period along a center line CX in the extending direction of substrate metal layer 12. The period is the same as the period of dimples 21D arranged in cap metal layer 21.

[0089] Next, in STEP 2, the cap metal layer 21 of the light-transmitting cap 13 is placed on the AuSn bumps 22B such that each dimple 21D of the cap metal layer 21 is positioned midway between adjacent AuSn bumps 22B.

[0090] While melting the AuSn bumps 22B, the transparent cap 13 was pressed. As a result, the AuSn bumps 22B spread between the substrate metal layer 12 and the cap metal layer 21, and adjacent AuSn bumps 22B merged. The AuSn of the adjacent AuSn bumps 22B flowed into the dimples 21D due to the melting.

[0091] Next, in STEP 3, the light-transmitting cap 13 was sufficiently pressed and then cooled to room temperature, so that a bonding layer 22 was formed between the substrate metal layer 12 and the cap metal layer 21.

[0092] Although the modified examples of the first embodiment have been described above, in the second and third embodiments, the dimples 21D or the dimple group 21D may be provided in the cap metal layer 21. In these modified examples as well, the same effects as those of the first to third embodiments can be obtained.

[0093] The semiconductor light emitting device and the manufacturing method thereof according to the present invention have been described in detail above. Note that in the above embodiment, the semiconductor light emitting device is composed of a rectangular frame-shaped substrate and a rectangular flat glass light-transmitting cap, but the present invention is not limited to this.

[0094] For example, the bonded portion of the substrate may be in a polygonal ring shape, a circular ring shape, an elliptical shape, etc., and the shape of the light-transmitting cap may be in a polygonal plate shape, a circular plate shape, an elliptical plate shape, a hemisphere shape, etc. Therefore, the shapes of the substrate metal layer and the cap metal layer are not limited to a rectangular ring shape, and may be in a polygonal ring shape, a circular ring shape, an elliptical shape, etc.

[0095] As described above in detail, the semiconductor light emitting device and the manufacturing method thereof according to the present embodiment can provide a semiconductor device and a manufacturing method thereof that has high reliability, in which high airtightness is maintained even during long-term use, and high environmental resistance, such as moisture resistance and corrosion resistance. Furthermore, it can provide a semiconductor device and a manufacturing method thereof that has a highly reliable airtight bond, in which the generation and growth of cracks in the bonded portion is suppressed and deterioration inside the bonded layer can be prevented. [Explanation of symbols]

[0096] 10: semiconductor light emitting device, 11: substrate, 11A: frame, 11S: substrate bonding surface, 11T: frame top surface, 12: substrate metal layer, 12C: cavity, 12D: dimple (group), 12D1 to 12D3: dimples, 12E: additional dimples, 13: light-transmitting cap, 13A: window portion, 13B: cap bonding portion, 13S: cap bonding surface, 14, 14A, 14B: wiring electrodes, 15: semiconductor light emitting element, 21: cap metal layer, 21D: dimple (group), 22: bonding layer, 22B, 22B1, 22B2: bonding material bump, 24: bonding portion, C, C1, C2: bump center, CX, CY: center line in extension direction, DP: spacing between dimple (group)

Claims

1. A semiconductor light emitting element; an airtight substrate having a substrate bonding surface to which a wiring connected to the semiconductor light emitting device and a ring-shaped substrate metal layer surrounding the semiconductor light emitting device are fixed; a window portion that transmits the emitted light of the semiconductor light emitting element, and a cap bonding portion to which a ring-shaped cap metal layer corresponding to the substrate metal layer is fixed, the cap metal layer being bonded to the substrate metal layer by a bonding layer, and an airtight light-transmitting cap having an internal space for accommodating the semiconductor light emitting element and airtightly bonded to the substrate, one of the substrate metal layer and the cap metal layer has a plurality of dimples arranged along an extending direction of the one metal layer; A semiconductor light emitting device, wherein the bonding material of the bonding layer flows into the plurality of dimples.

2. The semiconductor light emitting device of claim 1 , wherein the plurality of dimples have a hemispherical shape.

3. 3. The semiconductor light emitting device according to claim 1, wherein an outermost layer of at least one of said substrate metal layer and said cap metal layer is a gold (Au) layer, and said bonding material of said bonding layer contains gold tin (AuSn).

4. The semiconductor light emitting device according to claim 1 , wherein the plurality of dimples are formed at a constant interval in the extending direction.

5. 5. The semiconductor light-emitting device according to claim 1, wherein the plurality of dimples include a dimple group consisting of at least three dimples arranged on a straight line inclined by an inclination angle θ with respect to the extension direction, and the dimple group is formed at a constant period in the extension direction.

6. The semiconductor light emitting device of claim 1 , wherein one of the substrate metal layer and the cap metal layer has a plurality of additional dimples arranged along an edge of the one metal layer.

7. A method for manufacturing the semiconductor light emitting device according to any one of claims 1 to 6, comprising the steps of: (a) arranging a plurality of bonding material bumps on the substrate metal layer along an extending direction of the substrate metal layer; (b) placing the cap metal layer on the plurality of bonding material bumps, and heating the cap bonding portion while pressing the cap metal layer to melt the plurality of bonding material bumps; (c) melting the plurality of bonding material bumps and then cooling them to bond the substrate metal layer and the cap metal layer; A method for manufacturing a semiconductor light emitting device, wherein each of the plurality of bonding material bumps is arranged in a position such that when the plurality of bonding material bumps melt, bonding material of adjacent bonding material bumps flows into each of the plurality of dimples.

8. The method for manufacturing a semiconductor light emitting device according to claim 7 , wherein the plurality of bonding material bumps are hemispherical and have the same size.

9. 9. The method for manufacturing a semiconductor light emitting device according to claim 7, wherein in the step (a) of arranging the plurality of bonding material bumps, two rows of bumps are arranged in a staggered pattern at a certain angle to the extending direction of the substrate metal layer.

10. 10. A method for manufacturing a semiconductor light emitting device according to claim 9, comprising the steps of: The method for manufacturing a semiconductor light emitting device, wherein the plurality of bonding material bumps are hemispherical and have the same size, and the fixed angle is 45°.

11. 10. A method for manufacturing a semiconductor light emitting device according to claim 9, comprising the steps of: the plurality of dimples include at least three dimples arranged on a straight line inclined at an inclination angle θ with respect to the extending direction, The method for manufacturing a semiconductor light emitting device, wherein the plurality of bonding material bumps are hemispherical and have the same size, and the inclination angle θ is 60°.

Citation Information

Patent Citations

  • Package for accommodation of semiconductor element and method of manufacturing the same

    JP2001237335A

  • Light emitting device and lighting system using same

    JP2007234637A

  • Semiconductor module

    JP2015018873A

  • Light emission device

    JP2016127255A

  • Optical semiconductor device and method of manufacturing the same

    JP2018037581A