Hydrophilic paint, aluminum material, aluminum fin material and heat exchanger
A hydrophilic paint with specific inorganic metal compound particles and alkali metal silicate forms a durable coating on aluminum fins, addressing the issue of hydrophilicity loss in heat exchangers, thereby improving their operational efficiency and reducing resistance.
Patent Information
- Application Number
- JP2021050512
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-24
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2041-03-24
AI Technical Summary
Conventional surface treatments on aluminum fin materials for heat exchangers fail to maintain hydrophilicity over an extended period, leading to increased ventilation resistance and reduced cooling/heating capacity due to dew condensation and water accumulation.
A hydrophilic paint containing specific inorganic metal compound particles, alkali metal silicate, and water-soluble resin is applied to form a coating film that maintains hydrophilicity over time, using a blend with predetermined ratios of these components.
The coating film maintains excellent hydrophilicity and reduces ventilation resistance, enhancing the long-term performance and efficiency of heat exchangers by preventing dew condensation and water accumulation.
Smart Images

Figure 0007554697000003 
Figure 0007554697000001 
Figure 0007554697000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a hydrophilic paint that is useful when forming an aluminum material into a fin material, an aluminum material having a hydrophilic coating film formed on its surface by the hydrophilic paint, a fin material formed from the aluminum material, and a heat exchanger including the fin material. [Background technology]
[0002] Aluminum and its alloys are widely used as fin materials for heat exchangers in air conditioners because they are lightweight and have excellent workability and thermal conductivity. However, the surface of aluminum and its alloys is not sufficiently hydrophilic, and moisture in the air can adhere to the surface of the evaporator fins as condensation water when the air conditioner is operating. If this condensation water accumulates on the fin surface and forms a bridge between adjacent fins, the resistance (ventilation resistance) when blowing air increases, causing a decrease in cooling and heating capacity and water splashing into the room.
[0003] To avoid these problems, hydrophilic surface treatments with excellent water wettability have been implemented, such as forming an inorganic hydrophilic coating mainly made of silicate on the fin surface (see Patent Document 1) or forming a resin-based hydrophilic coating using a resin that does not inhibit hydrophilicity (see Patent Document 2). Also known is an aluminum fin material (see Patent Document 3) in which two hydrophilic resin layers are provided on the fin surface and TiO2 fine particles are dispersed in the second hydrophilic resin layer on the surface side, and an aluminum fin material (see Patent Document 4) in which inorganic oxide fine particles and a resin-based lubricant layer are provided on a hydrophilic layer provided on a substrate. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 3-77440 [Patent Document 2] Japanese Patent Application Publication No. 9-14888 [Patent Document 3] JP 2012-215347 A [Patent Document 4] JP 2010-223520 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, these conventional surface treatment methods could not provide a surface that could maintain good hydrophilicity while withstanding long-term operation, even if the initial hydrophilicity was good. In addition, in recent years, there has been a demand for fin materials with good water wettability and excellent hydrophilicity due to the improvement of APF (All-year Energy Consumption Efficiency) and the growing market demand for heaters.
[0006] The present invention has been made to solve the above-mentioned problems, and has an object to provide a hydrophilic paint capable of forming a coating film on an aluminum material that can maintain hydrophilicity for a long period of time, an aluminum material or aluminum fin material having a hydrophilic coating film formed on its surface by applying the hydrophilic paint, and a heat exchanger including the aluminum fin material. [Means for solving the problem]
[0007] Means for Solving the Problems The present inventors conducted intensive research to solve the above problems and discovered that a hydrophilic paint that can be produced by mixing predetermined amounts of specific inorganic metal compound particles or organic resin particles (A), an alkali metal silicate (B), and a specific water-soluble resin or a salt thereof (C) with water can form a coating film on aluminum materials that can maintain hydrophilicity for a long period of time, thereby completing the present invention.
[0008] That is, the present invention provides [1] A composition comprising inorganic metal compound particles or organic resin particles (A), an alkali metal silicate (B), a water-soluble resin or a salt thereof (C), and water; The alkali metal silicate (B) is MO·nSiO (n is within the range of 1.9 or more and 8.0 or less, and M represents an alkali metal), The water-soluble resin is a homopolymer or copolymer having a -[CC(COOH)]- structure and an acid value of 700 mgKOH / g or more, The total mass (T M ) the mass (C M ) ratio (C M / T M ) is within the range of 0.2 to 2.5, The SiO2 equivalent mass (B M ) the mass (A M ) ratio (A M / B M ) is within the range of 0.10 to 4.0, the inorganic metal compound particles are one or more selected from cerium carbonate, copper carbonate, zinc carbonate, nickel carbonate, manganese carbonate, cobalt carbonate, calcium oxide, tin oxide, iron oxide, manganese oxide, and aluminum hydroxide; a hydrophilic coating material for aluminum materials, wherein the organic resin particles are one or more selected from the group consisting of particles of polyacrylic acid, its esters, its salts, and crosslinked products thereof, and particles of polymethacrylic acid, its esters, its salts, and crosslinked products thereof; [2] A hydrophilic coating film on the surface of the coating film contains inorganic metal compound particles or organic resin particles (A), an alkali metal silicate (B), and a water-soluble resin or a salt thereof (C), The alkali metal silicate (B) is MO·nSiO (n is within the range of 1.9 or more and 8.0 or less, and M represents an alkali metal), The water-soluble resin is a homopolymer or copolymer having a -[CC(COOH)]- structure and an acid value of 700 mgKOH / g or more, The total mass (T M) the mass (C M ) ratio (C M / T M ) is within the range of 0.2 to 2.5, The SiO2 equivalent mass (B M ) the mass (A M ) ratio (A M / B M ) is within the range of 0.10 to 4.0, the inorganic metal compound particles are one or more selected from cerium carbonate, copper carbonate, zinc carbonate, nickel carbonate, manganese carbonate, cobalt carbonate, calcium oxide, tin oxide, iron oxide, manganese oxide, and aluminum hydroxide; an aluminum material, wherein the organic resin particles are one or more selected from particles of polyacrylic acid, its esters, its salts, and crosslinked products thereof, and particles of polymethacrylic acid, its esters, its salts, and crosslinked products thereof; [3] The aluminum material according to the above [2], which has a lubricating oil and / or a lubricating film on the hydrophilic coating; [4] A hydrophilic coating film on the surface of the coating film contains inorganic metal compound particles or organic resin particles (A), an alkali metal silicate (B), and a water-soluble resin or a salt thereof (C), The alkali metal silicate (B) is MO·nSiO (n is within the range of 1.9 or more and 8.0 or less, and M represents an alkali metal), The water-soluble resin is a homopolymer or copolymer having a -[CC(COOH)]- structure and an acid value of 700 mgKOH / g or more, The total mass (T M ) the mass (C M ) ratio (C M / T M ) is within the range of 0.2 to 2.5, The SiO2 equivalent mass (B M) the mass (A M ) ratio (A M / B M ) is within the range of 0.10 to 4.0, the inorganic metal compound particles are one or more selected from cerium carbonate, copper carbonate, zinc carbonate, nickel carbonate, manganese carbonate, cobalt carbonate, calcium oxide, tin oxide, iron oxide, manganese oxide, and aluminum hydroxide; the organic resin particles are one or more selected from the group consisting of particles of polyacrylic acid, its esters, its salts, and crosslinked products thereof, and particles of polymethacrylic acid, its esters, its salts, and crosslinked products thereof; and an aluminum fin material; [5] The aluminum fin material according to [4] above, having a lubricating oil and / or lubricating coating on the hydrophilic coating; [6] A heat exchanger comprising the aluminum fin material according to [4] or [5] above; And so on. Effect of the Invention
[0009] The present invention can provide a hydrophilic paint capable of forming a coating film on an aluminum material that can maintain hydrophilicity for a long period of time, an aluminum material or aluminum fin material having a hydrophilic coating film formed on the surface by applying the hydrophilic paint, and a heat exchanger including the aluminum fin material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] <Hydrophilic paint for aluminum materials> The hydrophilic coating material for aluminum materials according to the present invention can be produced by mixing specific inorganic metal compound particles or organic resin particles (A), alkali metal silicate (B), and specific water-soluble resin or its salt (C) in predetermined amounts in water. By using the hydrophilic coating material for aluminum materials produced in this manner, a coating film capable of maintaining hydrophilicity for a long period of time can be formed on the surface of the aluminum material.
[0011] <Inorganic metal compound particles or organic resin particles (A)> Examples of inorganic metal compound particles include cerium carbonate, copper carbonate, zinc carbonate, nickel carbonate, manganese carbonate, cobalt carbonate, calcium oxide, tin oxide, iron oxide (ferric oxide), manganese oxide, and aluminum hydroxide. The organic resin particles are not particularly limited as long as they are organic resins that exist as particles in water at 25°C, and examples thereof include particles of polyacrylic acid, its esters or salts, or crosslinked products thereof, and particles of polymethacrylic acid, its esters or salts, or crosslinked products thereof. Examples of salts of polyacrylic acid or polymethacrylic acid include, but are not limited to, lithium salts, sodium salts, potassium salts, calcium salts, and ammonium salts. Examples of esters of polyacrylic acid or polymethacrylic acid include, but are not limited to, methyl polyacrylate, ethyl polyacrylate, methyl polymethacrylate, and ethyl polymethacrylate. The inorganic metal compound particles or organic resin particles (A) may be used alone or in combination of two or more. In this specification, the organic resin particles (A) do not include those that can dissolve in 0.1 g or more in 100 g of water at 20° C. Therefore, the organic resin particles (A) are different from the water-soluble resin or its salt (C) described later.
[0012] <Alkali metal silicate (B)> The alkali metal silicate (B) is not particularly limited as long as it is a known one and the molar ratio (n) of silica (SiO2) to alkali metal oxide (MO) is within the range of 1.9 to 8.0. That is, the alkali metal silicate (B) can be expressed as MO·nSiO2 (n is within the range of 1.9 to 8.0, and M represents an alkali metal). Examples of the alkali metal (M) include lithium, potassium, and sodium. The alkali metal silicate (B) may be used alone or in combination of two or more.
[0013] <Water-soluble resin or its salt (C)> The water-soluble resin is not particularly limited as long as it has a -[CC(COOH)]- structure and is a water-soluble homopolymer or copolymer with an acid value of 700 mgKOH / g or more. The copolymer is not particularly limited as long as it has two or more repeating structures, and may be any of an alternating copolymer, a random copolymer, a block copolymer, and a graft copolymer. In this specification, the "water-soluble" of the water-soluble resin or its salt (C) means that 0.1 g or more can be dissolved in 100 g of water at 20°C.
[0014] Specific examples of the water-soluble resin or a salt thereof (C) include polymers composed of monomers such as (meth)acrylic acid, crotonic acid, 2-acrylamido-2-methylpropanecarboxylic acid, maleic acid, fumaric acid, itaconic acid, muconic acid, citraconic acid, etc., or their alkali metal salts or ammonium salts; copolymers of such monomers with other monomers copolymerizable with such monomers, or their alkali metal salts or ammonium salts; copolymers of acrylic acid, methacrylic acid, and a sulfonic acid group-containing monomer such as sulfoethyl acrylate, styrene sulfonic acid, (meth)allyl sulfonic acid, vinyl sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, etc., or their alkali metal salts or ammonium salts; styrene-maleic acid copolymers or their salts. Examples of the copolymer of the monomers such as (meth)acrylic acid, crotonic acid, 2-acrylamido-2-methylpropanecarboxylic acid, maleic acid, fumaric acid, itaconic acid, muconic acid, citraconic acid, and the like, and other monomers copolymerizable with the monomers include copolymers of the monomers and the sulfonic acid group-containing monomers; copolymers composed of two of the monomers, such as copolymers of acrylic acid and methacrylic acid; and the like. Examples of the alkali metal salts include lithium salts, sodium salts, potassium salts, and the like. The upper limit of the acid value of the water-soluble resin is not particularly limited, but is preferably 3000 mgKOH / g or less, more preferably 2000 mgKOH / g or less, and even more preferably 1100 mgKOH / g or less. The water-soluble resin or its salt (C) may be used alone or in combination of two or more.
[0015] In this embodiment, preferred combinations of the specific inorganic metal compound particles or organic resin particles (A), the alkali metal silicate (B), and the specific water-soluble resin or its salt (C) to be contained in the hydrophilic coating material for aluminum materials include, for example, a combination of cerium carbonate, lithium silicate (Li2O·nSiO2; n=3 to 8), and any of the above water-soluble resins and their salts, a combination of cerium carbonate, potassium silicate (K2O·nSiO2; n=1.9 to 3.7), and any of the above water-soluble resins and their salts, a combination of cerium carbonate, sodium silicate (Na2O· nSiO2; n=2.8-3.3) and any of the above water-soluble resins and their salts, combinations of copper carbonate and lithium silicate (Li2O·nSiO2; n=3-8) and any of the above water-soluble resins and their salts, combinations of copper carbonate and potassium silicate (K2O·nSiO2; n=1.9-3.7) and any of the above water-soluble resins and their salts, combinations of copper carbonate and sodium silicate (Na2O·nSiO2; n=2.8-3.3) and any of the above water-soluble resins and their salts, combinations of zinc carbonate and lithium silicate (Li2O·nSiO2; n=3 combination of zinc carbonate and potassium silicate (K2O·nSiO2; n=1.9-3.7) and any of the above water-soluble resins and salts thereof; combination of zinc carbonate and sodium silicate (Na2O·nSiO2; n=2.8-3.3) and any of the above water-soluble resins and salts thereof; combination of nickel carbonate and lithium silicate (Li2O·nSiO2; n=3-8) and any of the above water-soluble resins and salts thereof; combination of nickel carbonate and potassium silicate (K2O·nSiO2; n=1.9-3.7) and any of the above water-soluble resins and their salts, combinations of nickel carbonate and sodium silicate (Na2O·nSiO2; n=2.8-3.3) and any of the above water-soluble resins and their salts, combinations of manganese carbonate and lithium silicate (Li2O·nSiO2; n=3-8) and any of the above water-soluble resins and their salts, combinations of manganese carbonate and potassium silicate (K2O·nSiO2; n=1.9-3.7) and any of the above water-soluble resins and their salts, combinations of manganese carbonate and sodium silicate (Na2O·nSiO2; n=2.8-3.3) and any of the above water-soluble resins and their salts; combinations of cobalt carbonate and lithium silicate (Li2O·nSiO2; n=3-8) and any of the above water-soluble resins and their salts; combinations of cobalt carbonate and potassium silicate (K2O·nSiO2; n=1.9-3.7) and any of the above water-soluble resins and their salts; combinations of cobalt carbonate and sodium silicate (Na2O·nSiO2; n=2.8-3.3) and any of the above water-soluble resins and their salts; combinations of calcium oxide and lithium silicate (Li2O·nSiO2; n=3-8) and any of the above water-soluble resins and their salts; combinations of calcium oxide and potassium silicate (K2O·nSiO2; n=1.9-3.7) and any of the above water-soluble resins and their salts; or a combination thereof, a combination of tin oxide and lithium silicate (Li2O·nSiO2; n=3-8) and any of the above water-soluble resins and their salts, a combination of tin oxide and potassium silicate (K2O·nSiO2; n=1.9-3.7) and any of the above water-soluble resins and their salts, a combination of tin oxide and sodium silicate (Na2O·nSiO2; n=2.8-3.3) and any of the above water-soluble resins and their salts, a combination of iron oxide (ferric oxide) and lithium silicate (Li2O·nSiO2; n=3-8) and any of the above water-soluble resins and their salts, a combination of iron oxide (ferric oxide) and potassium silicate (K2O·nSiO2; n=1.9-3.7) and any of the above water-soluble resins and their salts, a combination of iron oxide (ferric oxide) and sodium silicate (Na2O·nSiO2; n=2.8-3.3) and any of the above water-soluble resins and their salts, and the like.
[0016] Other examples include combinations of manganese oxide, lithium silicate (Li2O·nSiO2; n=3-8) and any of the above water-soluble resins and their salts, combinations of manganese oxide, potassium silicate (K2O·nSiO2; n=1.9-3.7) and any of the above water-soluble resins and their salts, combinations of manganese oxide, sodium silicate (Na2O·nSiO2; n=2.8-3.3) and any of the above water-soluble resins and their salts, combinations of aluminum hydroxide, lithium silicate (Li2O·nSiO2; n=3-8) and any of the above water-soluble resins and their salts, and combinations of aluminum hydroxide, lithium silicate (Li2O·nSiO2; n=3-8) and any of the above water-soluble resins and their salts. a combination of aluminum hydroxide and potassium silicate (K2O·nSiO2; n=1.9-3.7) and any of the above water-soluble resins and salts thereof; a combination of aluminum hydroxide and sodium silicate (Na2O·nSiO2; n=2.8-3.3) and any of the above water-soluble resins and salts thereof; a combination of particles of polyacrylic acid, its ester or its salt or a crosslinked product thereof, lithium silicate (Li2O·nSiO2; n=3-8) and any of the above water-soluble resins and salts thereof; a combination of particles of polyacrylic acid, its ester or its salt or a crosslinked product thereof, potassium silicate (K2O·nSiO2; n=1.9-3.7) and any of the above water-soluble resins and salts thereof; a combination of particles of polyacrylic acid, its ester or its salt or a crosslinked product thereof, sodium silicate (Na2O·nSiO2; n=2.8-3.3) and any of the above water-soluble resins and salts thereof; combinations of particles of polymethacrylic acid, its esters or salts thereof, or crosslinked particles of these with potassium silicate (K2O·nSiO2; n=1.9 to 3.7) and any of the above-mentioned water-soluble resins or salts thereof; and combinations of particles of polymethacrylic acid, its esters or salts thereof, or crosslinked particles of these with sodium silicate (Na2O·nSiO2; n=2.8 to 3.3) and any of the above-mentioned water-soluble resins or salts thereof.
[0017] <Other ingredients> In this embodiment, the hydrophilic coating material for aluminum materials may consist only of inorganic metal compound particles or organic resin particles (A), alkali metal silicate (B), and water-soluble resin or its salt (C) in addition to water, but may further contain other components, such as crosslinking components, surfactants, dispersants, water-miscible organic solvents, etc.
[0018] The crosslinking component is not particularly limited as long as it is other than the water-soluble resin or its salt (C) and links the water-soluble resin or its salt (C), and examples thereof include carboxyl group-containing compounds, water-soluble metal compounds, etc. Examples of the carboxyl group-containing compounds include citric acid, 1,2,3,4-butanetetracarboxylic acid, tartaric acid, malic acid, isophthalic acid, adipic acid, pyromellitic acid, maleic acid, itaconic acid, fumaric acid, 1,2,4-trimellitic acid, 3,3',4,4'-diphenylsulfonetetracarboxylic acid, cyclohexane-1,2,4-tricarboxylic acid, and 2-phosphonobutane-1,2,4-tricarboxylic acid. The water solubility of the water-soluble metal compound means that 1 g can be dissolved in 1 L of water at 25°C. The water-soluble metal compound is not particularly limited as long as it is water-soluble, and examples thereof include organic titanium compounds such as diisopropoxytitanium bis(triethanolamine)titanium; chromium-containing compounds such as chromium(III) sulfate and chromium(III) nitrate; inorganic zirconium-containing compounds such as hexafluorozirconium acid; and inorganic titanium-containing compounds such as hexafluorotitanium acid. The organic titanium compound means a titanium-containing compound having an organic group. These crosslinking components may be used alone or in combination of two or more.
[0019] As the surfactant, cationic, anionic, amphoteric, nonionic, etc. surfactants can be used. Examples of cationic surfactants include alkyl amine salts such as alkyl trimethyl ammonium halides, stearyl amine acetate, and stearyl amine hydrochloride, quaternary ammonium salts such as lauryl trimethyl ammonium chloride, stearyl trimethyl ammonium chloride, and distearyl dimethyl ammonium, alkyl betaines such as lauryl betaine and stearyl betaine, and amine oxides. Examples of anionic surfactants include alkyl benzene sulfonates, alkyl naphthalene sulfonates, alkyl sulfosuccinates, alkyl diphenyl ether disulfonates, alkyl phosphates, polyoxyethylene alkyl sulfates, alkyl sulfonates, polyoxyethylene alkyl phenyl ether sulfates, sodium dodecyl diphenyl ether disulfonate, fatty acid salts such as sodium stearate and potassium oleate, and alkyl sulfates such as sodium lauryl sulfate, triethanolamine lauryl sulfate, ammonium lauryl sulfate, and sodium dodecyl sulfate. Examples of amphoteric surfactants include alkylaminopropionates and alkyldimethylbetaines. Other examples include imidazoline-type amphoteric surfactants, glycine-type amphoteric surfactants, and amine oxide-type amphoteric surfactants. Examples of nonionic surfactants include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, and polyoxyethylene cetyl ether; polyoxyethylene alkylphenyl ethers such as polyoxyethylene octylphenyl ether; polyoxyethylene alkylaryl ethers; oxyethylene-oxypropylene block copolymers; polyoxyalkylene fatty acid esters; sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monostearate, and sorbitan trioleate; glycerin fatty acid esters; polyoxyethylene glycerin fatty acids; polyoxyethylene propylene glycol fatty acid esters; polyoxyethylene fatty acid esters; and the like.These surfactants may be used alone or in combination of two or more.
[0020] Examples of the dispersant include sodium polycarboxylate, ammonium polycarboxylate, and quaternary cationic polymers. These may be used alone or in combination of two or more.
[0021] The water-miscible organic solvent is not particularly limited as long as it is miscible with water, and examples thereof include ketone-based solvents such as acetone and methyl ethyl ketone; amide-based solvents such as N,N'-dimethylformamide and dimethylacetamide; alcohol-based solvents such as methanol, ethanol, and isopropanol; ether-based solvents such as ethylene glycol monobutyl ether and ethylene glycol monohexyl ether; and pyrrolidone-based solvents such as 1-methyl-2-pyrrolidone and 1-ethyl-2-pyrrolidone. One of these water-miscible organic solvents may be mixed with water, or two or more of them may be mixed with water. The ratio of the water-miscible organic solvent to be mixed in the hydrophilic coating material for aluminum materials is not particularly limited as long as it is 50% by mass or less relative to the total mass of water and the water-miscible organic solvent, and may be 40% by mass or less, 30% by mass or less, 20% by mass or less, 10% by mass or less, or 0% by mass.
[0022] <Composition ratio of each ingredient> In this embodiment, the total mass (T M ) the mass (C M ) ratio (C M / T M ) is in the range of 0.2 to 2.5, preferably in the range of 0.2 to 2.3, and more preferably in the range of 0.2 to 2.2. When two or more water-soluble resins or salts thereof are used in combination, the mass (C MIn this embodiment, the mass (A M ) and the SiO2 equivalent mass of the above alkali metal silicate (B) (B M ) and the ratio (A M / B M ) is in the range of 0.10 or more and 4.0 or less, preferably in the range of 0.10 or more and 3.8 or less, and more preferably in the range of 0.10 or more and 3.6 or less.
[0023] <Aluminum material or aluminum fin material having hydrophilic coating> The aluminum material or aluminum fin material having a hydrophilic coating film on its surface can be produced by applying the above-mentioned hydrophilic coating material for aluminum materials to the surface of the aluminum material or aluminum fin material and then drying it. The above-mentioned hydrophilic coating film is obtained by drying the water or water-miscible organic solvent in the hydrophilic coating material for aluminum materials applied to the aluminum material or aluminum fin material, so that the ratio of inorganic metal compound particles or organic resin particles (A), alkali metal silicate (B), and water-soluble resin or its salt (C) in the hydrophilic coating film is the same as the mixing ratio of inorganic metal compound particles or organic resin particles (A), alkali metal silicate (B), and water-soluble resin or its salt (C) in the hydrophilic coating material for aluminum materials. The aluminum material having a hydrophilic coating film on its surface produced in this way is useful for forming an aluminum fin material. In addition, the aluminum fin material having a hydrophilic coating film on its surface is useful as a part of a heat exchanger.
[0024] <Metal components of aluminum material or aluminum fin material> The metal components constituting the aluminum material or aluminum fin material may be pure aluminum, or may be an aluminum alloy.
[0025] <Coating process> The method of applying the hydrophilic coating material for aluminum materials is not particularly limited, but examples thereof include roll coating, spraying, and immersion. The application temperature is usually within the range of 10° C. to 60° C., and the application time is within the range of 0.01 seconds to 600 seconds, but is not limited thereto.
[0026] <Drying process> The drying method of the hydrophilic coating material for aluminum materials is not particularly limited as long as the water or water-miscible organic solvent in the hydrophilic coating material for aluminum materials evaporates, and includes drying methods using known drying equipment such as ovens, batch drying ovens, continuous hot air circulation drying ovens, conveyer hot air drying ovens, and electromagnetic induction heating ovens using IH heaters. The drying temperature is not particularly limited, but is usually in the range of 80°C to 270°C, preferably 100°C to 270°C. The drying time is also not particularly limited, but is usually in the range of 5 seconds to 120 minutes.
[0027] <Weight of hydrophilic coating film> In this embodiment, the mass of the hydrophilic coating film in the aluminum material or aluminum fin material having the hydrophilic coating film is not particularly limited as long as it is an amount that can exhibit the effects of the present invention. 2 Preferably, the weight is within the range of 0.15 g or more and 1.0 g or less, more preferably within the range of 0.25 g or more and 0.7 g or less, and particularly preferably within the range of 0.3 g or more and 0.5 g or less.
[0028] <Other processing steps> In this embodiment, a pretreatment step may be performed before applying the hydrophilic coating material for aluminum materials to the surface of the aluminum material or aluminum fin material, or a posttreatment step may be performed after the drying step.
[0029] <Pretreatment process> Examples of the pretreatment process include a cleaning process and an anti-rust process. One of these processes may be carried out alone, or two of these processes may be carried out in sequence. Examples of the cleaning process include a process for removing surface dirt with an alkaline or acidic cleaner. Examples of the anti-rust process include a known chromate process, a zinc phosphate process, a titanium-based chemical conversion process, a zirconium-based chemical conversion process, and a process for forming a corrosion-resistant film such as an organic film.
[0030] <Post-processing process> Examples of the post-treatment process include a lubricating oil application process or a lubricating film formation process. More specifically, a process of applying a lubricating oil or a lubricant to form a lubricating film on the hydrophilic coating film on the surface of the aluminum material or aluminum fin material can be mentioned. In this way, it is possible to obtain an aluminum material or aluminum fin material having a multi-layer coating in which a lubricating oil is applied or a lubricating film is formed on the hydrophilic coating film. The aluminum material having a multi-layer coating thus obtained is useful for forming an aluminum fin material by molding. In addition, the aluminum fin material having a multi-layer coating is useful as a part of a heat exchanger. The method of applying the lubricating oil or lubricant is not particularly limited, but examples thereof include a roll coating method, a spray method, and a dipping method.
[0031] As the lubricating oil, any known lubricant used in molding can be used. As the lubricating film forming lubricating agent, for example, water-soluble polyether, polyethylene glycol, polyoxyethylene alkyl ether, polyoxyethylene hydrogenated castor oil ether, and other known lubricants can be used. EXAMPLES
[0032] The present invention will be described in more detail below by showing examples, but the present invention is not limited to these examples. <Sample Preparation> An aluminum material for fins (length 300 mm, width 200 mm, thickness 0.1 mm) made of industrial pure aluminum of alloy number 1050 series specified in JIS H4000:2014 was degreased by spraying a 2% aqueous solution of an alkaline degreasing treatment agent (product name: Fine Cleaner FC-4477, manufactured by Nihon Parkerizing Co., Ltd.) at 50°C for 5 seconds, and then rinsed with tap water. Next, a 4% aqueous solution of a phosphate chromate treatment agent (product name: Alchrom-K702, manufactured by Nihon Parkerizing Co., Ltd.) was sprayed at 50°C for 5 seconds, followed by rinsing with water and drying at 80°C for 1 minute, resulting in a chromium deposition amount of 20 mg / m 2 The aluminum material for the fin on which the phosphate chromate film was formed was subjected to a comparative test (C M / T M ) and the ratio (A M / B M The components were mixed with water to prepare a hydrophilic paint for aluminum materials so that the hydrophilic coating film had the value shown in Table 1 below. The paint was applied by a bar coating method (#3 bar) and dried at 220°C for 30 seconds to obtain an aluminum material for fins having a hydrophilic coating film on its surface. The hydrophilic paint for aluminum materials was prepared so that the solid content mass concentration was 7%. The masses of the samples before and after the formation of the hydrophilic coating film were measured, and it was found that the hydrophilic coating film had a hydrophilic coating film of 1m 2 The mass of the hydrophilic coating film per unit was 0.5 g.
[0033] Next, for the examples and comparative examples in which the "lubricating film" in Table 1 is "present," a 5% aqueous solution of polyethylene glycol (weight average molecular weight 20,000) was applied to the aluminum material for fins on which the hydrophilic coating film had been formed at 25°C by the bar coating method (#2 bar), and the aluminum material was dried at 120°C for 30 seconds to form a lubricating film, thereby obtaining aluminum materials with multi-layer coatings (samples of Examples 1 to 18 and Comparative Examples 1 to 10). The masses of the samples before and after the formation of the lubricating film were measured, and the masses of all the samples were 1 m 2 The mass of the lubricating film per unit was 0.15 g. The symbols shown in each column of Table 1 represent the substances shown in Table 2.
[0034] [Table 1]
[0035] [Table 2]
[0036] Using the samples of Examples 1 to 18 and Comparative Examples 1 to 10, evaluation of hydrophilicity sustainability, workability, and corrosion resistance before and after processing were performed.
[0037] <Hydrophilicity sustainability evaluation> 1 μL of deionized water was dropped onto each sample, and the contact angle of the water droplet formed 10 seconds after dropping was measured using a contact angle meter (Kyowa Interface Science Co., Ltd.: automatic contact angle meter DM300 type). The contact angle of the sample cooled to 25°C after preparation was taken as the initial hydrophilicity. Each sample was immersed in running tap water for 8 hours, and then dried at 80°C for 16 hours, which was considered as one cycle. The contact angle after five such cycles was taken as the hydrophilicity after the wet-dry cycle. The contact angles obtained were evaluated according to the following evaluation criteria, and a score of 4 or more was considered to be acceptable. The results are shown in Table 3. (Evaluation Criteria for Hydrophilicity) 5 points: Water contact angle less than 5° 4 points: Water contact angle 5° or more, less than 10° 3 points: Water contact angle 10° or more, less than 20° 2 points: Water contact angle 20° or more, less than 30° 1 point: Water contact angle of 30° or more
[0038] <Evaluation of hydrophilicity after processing> Using an Erichsen tester, each sample was extruded 20 mm so that the hydrophilic coating side of the sample would be the convex part. 1 μL of deionized water was dropped onto the midpoint of a straight line connecting the center of the convex part and the circumference, and the contact angle of the water droplet formed 10 seconds after the drop was measured using a contact angle meter (Kyowa Interface Science Co., Ltd.: Automatic Contact Angle Meter DM300 Type) to evaluate the initial hydrophilicity after processing. Each sample was immersed in running tap water for 8 hours, and then dried at 80°C for 16 hours, which was considered as one cycle. The contact angle after five cycles of this cycle was considered to be the hydrophilicity after the dry-wet cycle. The contact angles obtained were evaluated according to the following evaluation criteria, and a score of 4 or more was considered to be acceptable. The results are shown in Table 3. (Evaluation criteria for hydrophilicity after processing) 5 points: Water contact angle less than 5° 4 points: Water contact angle 5° or more, less than 10° 3 points: Water contact angle 10° or more, less than 20° 2 points: Water contact angle 20° or more, less than 30° 1 point: Water contact angle of 30° or more
[0039] <Processability evaluation> The coefficient of dynamic friction of the samples was measured using a Bowden dynamic friction coefficient tester (Kyowa Interface Science Co., Ltd.: Bowden dynamic friction tester TS501 type) at a sliding speed of 4 mm / s, a load of 200 g, and a sliding distance of 10 mm, and was evaluated according to the following evaluation criteria, with a score of 2 or more being considered a pass. The results are shown in Table 3. (Evaluation criteria for workability) 4 points: Dynamic friction coefficient less than 0.05 3 points: Dynamic friction coefficient 0.05 or more, less than 0.1 2 points: Dynamic friction coefficient 0.1 or more, less than 0.2 1 point: Dynamic friction coefficient 0.2 or more
[0040] <Corrosion resistance evaluation> The samples were subjected to a 240-hour test using a neutral salt spray tester in accordance with JIS Z2371:2015, and were evaluated according to the following criteria, with a score of 9.8 or higher being considered a pass. The results are shown in Table 3. (Corrosion resistance evaluation criteria) 10 points: 0% corrosion area 9.8 points: Corrosion area ratio is over 0% and 0.02% or less 9.5 points: Corrosion area ratio is greater than 0.02% and less than 0.05% 9.3 points: Corrosion area ratio is over 0.05% and 0.07% or less 9 points: Corrosion area ratio is over 0.07% and 0.10% or less 8 points: Corrosion area ratio is over 0.10% and 0.25% or less 7 points: Corrosion area ratio is over 0.25% and 0.50% or less 6 points: Corrosion area ratio is over 0.50% and 1.00% or less 5 points: Corrosion area ratio is over 1.00% and 2.50% or less 4 points: Corrosion area ratio is over 2.50% and 5.00% or less 3 points: Corrosion area ratio is over 5.00% and 10.00% or less 2 points: Corrosion area ratio is over 10.00% and 25.00% or less 1 point: Corrosion area ratio is over 25.00% and 50.00% or less 0 points: Corrosion area rate exceeds 50.00%
[0041] [Table 3]
Claims
1. The composition comprises inorganic metal compound particles or organic resin particles (A), an alkali metal silicate (B), a water-soluble resin or a salt thereof (C), and water, The alkali metal silicate (B) is M 2 O.nSiO 2 (n is in the range of 1.9 or more and 8.0 or less, and M represents an alkali metal.) the water-soluble resin is a homopolymer or copolymer having a -[C-C(COOH)]- structure and an acid value of 700 mgKOH / g or more, The total mass (T M ) the mass (C M ) ratio (C M / T M ) is in the range of 0.2 or more and 2.5 or less, The SiO of the alkali metal silicate (B) 2 Converted mass (B M The mass (A) of the inorganic metal compound particles or organic resin particles (A) M ) ratio (A M / B M ) is in the range of 0.10 or more and 4.0 or less, the inorganic metal compound particles are one or more selected from the group consisting of cerium carbonate, copper carbonate, zinc carbonate, nickel carbonate, manganese carbonate, cobalt carbonate, calcium oxide, tin oxide, iron oxide, manganese oxide, and aluminum hydroxide; The hydrophilic coating material for aluminum materials, wherein the organic resin particles are one or more selected from particles of polyacrylic acid, its esters, salts thereof, and crosslinked products thereof, and particles of polymethacrylic acid, its esters, salts thereof, and crosslinked products thereof.
2. The present invention has a hydrophilic coating film on its surface, the hydrophilic coating film containing inorganic metal compound particles or organic resin particles (A), an alkali metal silicate (B), and a water-soluble resin or a salt thereof (C), The alkali metal silicate (B) is M 2 O.nSiO 2(n is in the range of 1.9 or more and 8.0 or less, and M represents an alkali metal.) the water-soluble resin is a homopolymer or copolymer having a -[C-C(COOH)]- structure and an acid value of 700 mgKOH / g or more, The total mass (T M ) the mass (C M ) ratio (C M / T M ) is in the range of 0.2 or more and 2.5 or less, The SiO of the alkali metal silicate (B) 2 Converted mass (B M The mass (A) of the inorganic metal compound particles or organic resin particles (A) M ) ratio (A M / B M ) is in the range of 0.10 or more and 4.0 or less, the inorganic metal compound particles are one or more selected from the group consisting of cerium carbonate, copper carbonate, zinc carbonate, nickel carbonate, manganese carbonate, cobalt carbonate, calcium oxide, tin oxide, iron oxide, manganese oxide, and aluminum hydroxide; The organic resin particles of the aluminum material are one or more selected from the group consisting of particles of polyacrylic acid, its esters, its salts, and crosslinked products thereof, and particles of polymethacrylic acid, its esters, its salts, and crosslinked products thereof.
3. The aluminum material according to claim 2 , further comprising a lubricating oil and / or lubricating film on the hydrophilic coating.
4. The present invention has a hydrophilic coating film on its surface, the hydrophilic coating film containing inorganic metal compound particles or organic resin particles (A), an alkali metal silicate (B), and a water-soluble resin or a salt thereof (C), The alkali metal silicate (B) is M 2 O.nSiO 2 (n is in the range of 1.9 or more and 8.0 or less, and M represents an alkali metal.) the water-soluble resin is a homopolymer or copolymer having a -[C-C(COOH)]- structure and an acid value of 700 mgKOH / g or more, The total mass (T M ) the mass (C M ) ratio (C M / T M ) is in the range of 0.2 or more and 2.5 or less, The SiO of the alkali metal silicate (B) 2 Converted mass (B M The mass (A) of the inorganic metal compound particles or organic resin particles (A) M ) ratio (A M / B M ) is in the range of 0.10 or more and 4.0 or less, the inorganic metal compound particles are one or more selected from the group consisting of cerium carbonate, copper carbonate, zinc carbonate, nickel carbonate, manganese carbonate, cobalt carbonate, calcium oxide, tin oxide, iron oxide, manganese oxide, and aluminum hydroxide; The organic resin particles are one or more selected from the group consisting of particles of polyacrylic acid, its esters, salts thereof, and crosslinked products thereof, and particles of polymethacrylic acid, its esters, salts thereof, and crosslinked products thereof.
5. The aluminum fin material according to claim 4, having a lubricating oil and / or lubricating film on the hydrophilic coating.
6. A heat exchanger comprising the aluminum fin material according to claim 4 or 5.
Citation Information
Patent Citations
Composition for coating of fin material
JP1986145263A
Mobile telephone terminal control system
JP1991077440A
Aluminum fin and manufacture thereof
JP1997014888A
Hydrophilifying agent for heat-exchanger fin material
JP2001164175A
Aluminum fin material for heat exchanger
JP2010223520A