Method for improving water absorption under load of water-absorbent resin particles, and method for producing water-absorbent resin particles
Shaking water-absorbing resin particles in a controlled manner improves their absorption capacity under load, addressing the challenge of maintaining high absorption levels despite pressure.
Patent Information
- Application Number
- JP2021530648
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-05
- Filing Date
- 2020-07-01
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-07-01
AI Technical Summary
Existing water-absorbing resin particles struggle to maintain a high water absorption capacity under load or pressure.
A method involving shaking a container filled with water-absorbing resin particles to improve their water absorption capacity under load, which includes adjusting parameters such as container type, filling rate, shaking time, and acceleration.
Enhances the water absorption capacity of resin particles under load, achieving improvements up to 150% or more compared to the initial absorption capacity.
Smart Images

Figure 0007554749000006 
Figure 0007554749000005 
Figure 0007554749000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for improving the water absorption under load of water-absorbent resin particles, and a method for producing water-absorbent resin particles. [Background technology]
[0002] Water-absorbent resin particles are widely used in the field of sanitary materials, etc. Water-absorbent resin particles are sometimes required to maintain a large water absorption capacity even under load or pressure (for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2002-212301 A [Patent Document 2] JP 2011-231255 A Summary of the Invention [Problem to be solved by the invention]
[0004] One aspect of the present invention provides a method for easily improving the water absorption under load of water-absorbent resin particles. [Means for solving the problem]
[0005] One aspect of the present invention relates to a method for improving the water absorption under load of water-absorbent resin particles, the method comprising a step of shaking a powder containing a plurality of water-absorbent resin particles contained in a container.
[0006] Another aspect of the present invention relates to a method for producing water-absorbent resin particles, comprising the step of improving the water absorption under load of the water-absorbent resin particles by the above-mentioned method. Effect of the Invention
[0007] According to one aspect of the present invention, the water absorption capacity under load of water-absorbent resin particles can be easily improved. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a schematic diagram showing one embodiment of a step of shaking powder containing water-absorbent resin particles. [Diagram 2] FIG. 2 is a schematic diagram showing a method for measuring the water absorption under load of water-absorbent resin particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, several embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments.
[0010] In this specification, "(meth)acrylic" means both acrylic and methacrylic. "Acrylate" and "methacrylate" are also written as "(meth)acrylate". The same applies to other similar terms. "(Poly)" means both cases with and without the prefix "poly". In the numerical ranges described in stages in this specification, the upper limit or lower limit of a certain numerical range can be arbitrarily combined with the upper limit or lower limit of a numerical range of another stage. In the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the examples. "Water-soluble" means that the material has a solubility of 5% by mass or more in water at 25°C. The materials exemplified in this specification may be used alone or in combination of two or more types. "Physiological saline" means a 0.9% by mass aqueous solution of sodium chloride.
[0011] FIG. 1 is a schematic diagram showing one embodiment of a step of shaking a powder containing a plurality of water-absorbent resin particles. In the method of FIG. 1, a powder 1 contained in a container 3 is shaken. The container 3 is placed on a support 5, and the powder 1 in the container 3 can be shaken by vibrating the support 5. By shaking, water-absorbent resin particles exhibiting a larger water absorption under load can be obtained. Typically, the powder 1 is substantially composed of only water-absorbent resin particles, but other particles may be contained in the powder 1. The ratio of the water-absorbent resin particles to the total amount of the powder 1 may be 80 to 100 mass%, 90 to 100 mass%, or 95 to 100 mass%.
[0012] The container 3 has a bag-shaped main body 3A and a lid 3B provided at one end of the main body 3A. The main body 3A is not particularly limited and may be, for example, a wooden box, a cardboard box, a plastic bag, or a cloth bag. A flexible bag such as a plastic bag as the main body of the container may be attached inside a harder outer box (for example, a cardboard box). The lid 3B may have an openable and closable structure. The powder 1 may be shaken in a state where the lid 3B is closed, that is, in a state where the powder 1 is sealed in the main body 3A. The powder 1 may be shaken while the container 3 containing the powder 1 is being transported.
[0013] The powder 1 may completely fill the container 3, or, as shown in the figure, the amount of powder 1 may be somewhat less than the maximum capacity of the container 3. For example, the container 3 may contain an amount of powder 1 corresponding to a theoretical filling rate of less than 100%. The theoretical filling rate here is calculated using the following formula: Theoretical filling rate [%]={(X[g] / D[g / mL]) / V[mL]}×100 In the formula, X is the mass of the powder 1, D is the packed bulk density of the powder 1, and V is the maximum volume of the container 3. When the amount of the powder 1 is an amount corresponding to a theoretical filling rate of less than 100%, there is a tendency that water-absorbent resin particles exhibiting a larger water absorption amount under load are easily obtained. From the same viewpoint, the amount of the powder 1 may be an amount corresponding to a theoretical filling rate of 95% or less, or 90% or less. From the viewpoint of efficiency, the amount of the powder 1 may be an amount corresponding to a theoretical filling rate of 50% or more, 60% or more, or 65% or more.
[0014] The packed bulk density of the powder containing the water-absorbent resin particles is measured by a method described in the examples below. The maximum volume V of the container is the maximum volume of the part capable of accommodating the powder (main body 3A in the example of FIG. 1). If the maximum capacity is described in the specifications of the container, the numerical value may be regarded as the maximum volume V of the container for convenience. The maximum volume V may be obtained by actually measuring the volume of water that completely fills the container. The calculated value of the volume calculated from the size and shape of the members constituting the container may also be regarded as the maximum volume V of the container. When the container has an opening that can be opened and closed, the maximum volume V is the maximum volume in a state in which the opening is closed. When the main body of the container is a flexible bag such as a plastic bag or a cloth bag, the calculated value of the volume in a state in which the main body (bag) is expanded to the maximum volume is regarded as the maximum volume V of the container. In addition, when the flexible bag is attached inside a hard outer box, the internal volume of the outer box is regarded as the maximum volume V of the container. In the case of the container 3 of FIG. 1, the main body 3A has a rectangular parallelepiped shape having a bottom surface S, and the maximum volume V of the container 3 can be calculated from the area of the bottom surface S and the height H.
[0015] The maximum volume of the container in which the powder containing the water-absorbent resin particles is accommodated for shaking is not particularly limited, but may be, for example, 10 mL to 2000 L. The total mass of the water-absorbent resin particles to be shaken is not particularly limited, but may be, for example, 10 g to 2000 kg.
[0016] The maximum value of acceleration that the powder experiences during shaking may be 0.050 to 4.0 G. When the acceleration is within this range, the water absorption under load tends to be improved more significantly. From the same viewpoint, the maximum value of acceleration may be 0.10 to 3.0 G, 0.30 to 2.5 G, 0.5 to 2.5 G, or 1.0 G to 2.5 G. The maximum value of acceleration can be calculated based on the amplitude and frequency of vibration for shaking.
[0017] The time for shaking the powder containing the water-absorbent resin particles (shaking time) may be any length that improves the water absorption under load of the water-absorbent resin particles, and may be, for example, 10 minutes or more, 20 minutes or more, or 30 minutes or more, or may be 24 hours or less. It is not necessary to shake the powder contained in the container continuously, and the powder may be shaken intermittently while stopping the shaking at least once during the process. When shaking the powder containing the water-absorbent resin particles intermittently, the total shaking time may be within the above range.
[0018] The water absorption under load of the water absorbent resin particles after shaking may be, for example, 15 to 30 g / g. The ratio of the water absorption under load of the water absorbent resin particles after shaking to the water absorption under load of the water absorbent resin particles before shaking may be 103% or more, 105% or more, or 110% or more, or may be 150% or less. The water absorption under load here is a value measured by the method described in the Examples below.
[0019] The water-absorbing resin particles are not particularly limited, and may be particles containing a polymer containing an ethylenically unsaturated monomer as a monomer unit. The ethylenically unsaturated monomer may be a water-soluble monomer, and examples thereof include (meth)acrylic acid and its salts, 2-(meth)acrylamido-2-methylpropanesulfonic acid and its salts, (meth)acrylamide, N,N-dimethyl(meth)acrylamide, 2-hydroxyethyl(meth)acrylate, N-methylol(meth)acrylamide, polyethylene glycol mono(meth)acrylate, N,N-diethylaminoethyl(meth)acrylate, N,N-diethylaminopropyl(meth)acrylate, and diethylaminopropyl(meth)acrylamide. The ethylenically unsaturated monomer may be used alone or in combination of two or more kinds. When the ethylenically unsaturated monomer has a functional group such as a carboxyl group or an amino group, it may function as a functional group that crosslinks the polymer. The water-absorbent resin particles may be particles containing a polymer that contains at least one of (meth)acrylic acid and a salt of (meth)acrylic acid as a monomer unit.
[0020] The polymer constituting the water-absorbent resin particles may be a crosslinked polymer. In this case, the polymer may be crosslinked by self-crosslinking, crosslinking by reaction with a crosslinking agent, or both. The water-absorbent resin particles may be surface-crosslinked by crosslinking at least the polymer in the surface layer portion with a crosslinking agent. The water absorption under load of the surface-crosslinked water-absorbent resin particles may be further improved by shaking. The crosslinking agent for surface crosslinking may be called a surface crosslinking agent.
[0021] Examples of the crosslinking agent include polyols such as ethylene glycol, propylene glycol, 1,4-butanediol, trimethylolpropane, glycerin, polyoxyethylene glycol, polyoxypropylene glycol, and polyglycerin; compounds having two or more epoxy groups such as (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, and (poly)glycerin diglycidyl ether; haloepoxy compounds such as epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin; compounds having two or more isocyanate groups such as 2,4-tolylene diisocyanate and hexamethylene diisocyanate; oxazoline compounds such as 1,2-ethylenebisoxazoline; carbonate compounds such as ethylene carbonate; and hydroxyalkylamide compounds such as bis[N,N-di(β-hydroxyethyl)]adipamide. The crosslinking agent may include a polyglycidyl compound such as (poly)ethylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, (poly)glycerin triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and polyglycerol polyglycidyl ether. These crosslinking agents may be used alone or in combination of two or more.
[0022] The water-absorbing resin particles may contain various additional components in addition to the polymer of the ethylenically unsaturated monomer. Examples of the additional components include gel stabilizers, metal chelating agents, and flow improvers (lubricants). The additional components may be located inside the polymer particles containing the polymer, on the surface of the polymer particles, or both. The additional component may be a flow improver (lubricant). The flow improver may include inorganic particles. The inorganic particles may include, for example, silica particles such as amorphous silica.
[0023] The shape of the water-absorbent resin particles is not particularly limited, and may be, for example, substantially spherical, crushed, or granular, and primary particles having these shapes may be aggregated to form particles. The median particle size of the water-absorbent resin particles may be 250 to 850 μm, 300 to 700 μm, or 300 to 600 μm.
[0024] The water-absorbent resin particles can be manufactured by a method including, for example, a step of obtaining water-absorbent resin particles containing a polymer containing an ethylenically unsaturated monomer as a monomer unit by a method including polymerizing a monomer containing an ethylenically unsaturated monomer, and a step of improving the water absorption amount under load of the water-absorbent resin particles by the method according to the above-mentioned embodiment. The polymerization method of the monomer can be selected from, for example, a reversed-phase suspension polymerization method, an aqueous solution polymerization method, a bulk polymerization method, and a precipitation polymerization method. From the viewpoint of ensuring good water absorption characteristics of the water-absorbent resin particles and easy control of the polymerization reaction, a reversed-phase suspension polymerization method or an aqueous solution polymerization method may be adopted. Steps such as a crosslinking reaction during or after polymerization, particle formation by pulverization, and drying can be carried out by a normal method as necessary. Surface-crosslinked water-absorbent resin particles can be obtained by a reaction between the particles after polymerization and drying and a surface crosslinking agent.
[0025] The water-absorbent resin particles having improved water absorption under load can be used to manufacture various absorbent articles such as diapers. EXAMPLES
[0026] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.
[0027] 1.Measurement method 1-1.Packed bulk density of powder made of water-absorbent resin particles Using a powder property evaluation device (manufactured by Hosokawa Micron Corporation, model number: PT-X), the packed bulk density of the powder consisting of water-absorbent resin particles was measured according to the following procedure. The packed bulk density was measured under the conditions of room temperature (25°C ± 2°C) and humidity of 50% ± 10%. The mass W0 of the empty cup-shaped container (volume 100 mL, inner diameter about 50 mm, height about 50 mm) was measured. Next, a cylindrical cap (inner diameter about 51 mm, height about 51 mm) was attached to the top of the container. 100 g of powder was put into the container from the upper opening of the cap using a scoop attached to the device. Next, the container was placed on a tapping lift bar (tapping device) and impacted on the powder in the container by tapping 180 times with a stroke of 18 mm. After that, the cap was removed and the powder in the part that protruded from the upper opening of the container was removed by scraping it off with a blade. Next, the mass W1 of the container containing the powder was measured. Based on the mass W0 and the mass W1, the packed bulk density was calculated from the following formula. The packed bulk density was measured three times in total, and the average value was recorded as the packed bulk density D [g / mL] of the powder consisting of water-absorbent resin particles. Compacted bulk density [g / mL] = (W1 [g] - W0 [g]) / 100 [mL]
[0028] 1-2. Theoretical filling rate The theoretical filling rate when a powder made of water-absorbent resin particles was placed in a polyethylene bag with a zipper was calculated by the following formula. Theoretical filling rate [%]={(X[g] / D[g / mL]) / V[mL]}×100 In the formula, X is the mass of the powder, D is the packed bulk density of the powder, and V is the capacity of the polyethylene bag. The maximum volume of pure water that can be filled into the polyethylene bag with the zipper closed was measured, and this was regarded as the maximum capacity of the polyethylene bag.
[0029] 1-3. Water absorption under load (load: 4.14kPa) The water absorption under load was measured at room temperature (25°C ± 2°C) and humidity 50% ± 10%. Figure 2 is a schematic diagram showing a method for measuring the water absorption under load. A glass filter 19 (diameter 9 cm, thickness 7 mm, standard: ISO4793, P-250) was placed in a petri dish 17 with an inner diameter of 12 cm. Then, physiological saline 20 was poured into the petri dish 17 up to the height of the glass filter 19. Powder 1 consisting of water-absorbent resin particles with a mass X [g] was uniformly placed in a cylinder 11 (inner diameter 2.0 cm: outer diameter 3.0 cm: height 5.0 cm) with a 255 mesh bolting cloth (nylon mesh) 13 attached to the end. Here, X was set to 0.1000 ± 0.0005 g. A cylindrical weight 15 having a mass that applies a pressure of 4.14 kPa to the powder 1 was placed on the powder 1 in the cylinder. The weight 15 has an outer diameter slightly smaller than the inner diameter of the cylinder, and can move smoothly up and down inside the cylinder. In this state, the total mass W1 [g] (total mass of the powder 1, cylinder 11, bolting cloth 13 and weight 15) was measured. The cylinder 11 containing the powder 1 and weight 15 was placed on a glass filter 19 in a petri dish 17, and the powder 1 was allowed to swell with physiological saline 20 for one hour. The total mass W2 [g] of the powder 1, cylinder 11, bolting cloth 13 and weight 15 after swelling was measured. The drying loss A [%] of the powder made of water-absorbent resin particles was also measured separately by the method described below. The water absorption under load was calculated by the following formula. Water absorption under load [g / g]=(W2-W1) / {X×(100-A) / 100} The water absorption under load was measured five times, and the average value of the obtained measurements was recorded as the water absorption under load of the water-absorbent resin particles. According to this method, the water absorption under load is measured after removing the influence of the change in the drying loss on the measured value. Therefore, even when the drying loss increases or decreases, the numerical value of the water absorption under load can be compared.
[0030] 1-4.Drying loss 2.0 g of powder consisting of water-absorbent resin particles was placed in an aluminum wheel case (No. 8) previously adjusted to a constant weight (W3 (g)), and its mass W4 (g) was precisely weighed. The precisely weighed powder was dried for 2 hours in a hot air dryer (manufactured by ADVANTEC, model: FV-320) with the internal temperature set to 105°C. After the powder was allowed to cool in a desiccator, its mass W5 (g) was measured as the dry mass. The loss on drying of the water-absorbent resin particles was calculated from the following formula. Loss on drying (mass%) = [{(W4-W3)-(W5-W3)} / (W4-W3)]×100
[0031] 2. Water-absorbing resin particles Example 1 AQUAKEEP SA60SXII (trade name, particles containing sodium polyacrylate) manufactured by Sumitomo Seika Chemicals Co., Ltd. was prepared as the water-absorbent resin particles of Example 1.
[0032] Example 2 A round-bottomed cylindrical separable flask with an inner diameter of 11 cm and a volume of 2 L was prepared, equipped with a reflux condenser, a dropping funnel, a nitrogen gas inlet tube, and a stirrer with a stirring blade having four inclined paddle blades with a blade diameter of 5 cm in two stages. 293 g of n-heptane and 0.736 g of maleic anhydride-modified ethylene-propylene copolymer (Hiwax 1105A, manufactured by Mitsui Chemicals, Inc.) as a dispersant were mixed in this flask. The mixture in the separable flask was heated to 80°C while being stirred with a stirrer, thereby dissolving the dispersant in n-heptane. The resulting solution was cooled to 50°C.
[0033] In a 300 mL beaker, 92.0 g (1.03 mol) of 80.5% by mass acrylic acid aqueous solution was placed as a water-soluble ethylenically unsaturated monomer, and 147.7 g of 20.9% by mass sodium hydroxide aqueous solution was dropped into the beaker while cooling from the outside, to perform 75 mol% neutralization. Then, 0.092 g of hydroxyethyl cellulose (Sumitomo Seika Chemicals Co., Ltd., HEC AW-15F) as a thickener, 0.092 g (0.339 mmol) of 2,2'-azobis(2-amidinopropane) dihydrochloride and 0.018 g (0.067 mmol) of potassium persulfate as radical polymerization initiators, and 0.0046 g (0.026 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added and dissolved to prepare the first stage aqueous liquid.
[0034] The first-stage aqueous solution was added to the n-heptane solution containing the dispersant in the separable flask, and the reaction solution formed was stirred for 10 minutes. A surfactant solution in which 0.736 g of sucrose stearate (Mitsubishi Chemical Foods Corporation, Ryoto Sugar Ester S-370, HLB: 3) was dissolved in 6.62 g of n-heptane was further added thereto, and the reaction solution was stirred at a stirrer speed of 550 rpm while the system was thoroughly replaced with nitrogen. The separable flask was then immersed in a 70°C water bath to heat the reaction solution, and the polymerization reaction was allowed to proceed for 60 minutes, yielding a first-stage polymerization slurry.
[0035] In another 500 mL beaker, 128.8 g (1.44 mol) of an acrylic acid aqueous solution with a concentration of 80.5% by mass was placed. While cooling from the outside, 159.0 g of a sodium hydroxide aqueous solution with a concentration of 27% by mass was dropped thereto to neutralize 75 mol% of the acrylic acid. After the neutralization, 0.129 g (0.476 mmol) of 2,2'-azobis(2-amidinopropane) dihydrochloride and 0.026 g (0.096 mmol) of potassium persulfate as radical polymerization initiators, and 0.0116 g (0.067 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added to the beaker of the acrylic acid aqueous solution and dissolved to prepare the second stage aqueous solution.
[0036] While stirring at a stirrer speed of 1000 rpm, the first-stage polymerization slurry liquid in the separable flask was cooled to 25°C, and the entire amount of the second-stage aqueous liquid was added thereto. After the atmosphere in the separable flask was replaced with nitrogen for 30 minutes, the separable flask was again immersed in a water bath at 70°C to raise the temperature of the reaction liquid, and a hydrous gel polymer was obtained by a second-stage polymerization reaction for 60 minutes.
[0037] 0.589 g of 45% by mass aqueous solution of pentasodium diethylenetriaminepentaacetate was added to the hydrous gel polymer after the second-stage polymerization under stirring. After that, the separable flask was immersed in an oil bath set at 125°C, and 216.7 g of water was extracted from the system by azeotropic distillation of n-heptane and water. Next, 4.42 g of an aqueous solution containing ethylene glycol diglycidyl ether (0.507 mmol) at a concentration of 2% by mass as a surface crosslinking agent was added to the separable flask, and the temperature was maintained at 83°C for 2 hours.
[0038] Thereafter, n-heptane was removed by drying at 125°C to obtain polymer particles (dried product). The polymer particles were passed through a sieve with an opening of 850 μm, and then 0.2 mass% of amorphous silica (Oriental Silicas Corporation, Toxil NP-S) based on the mass of the polymer particles was mixed with the polymer particles to obtain 229.0 g of water-absorbing resin particles containing amorphous silica. The median particle size of the water-absorbing resin particles was 348 μm.
[0039] Example 3 Water-absorbent resin particles (irregularly crushed) collected from the absorbent body of the diaper "GOO.N Pants, Fresh and Breathable, for Boys, Size L" (purchased in 2019) manufactured by Daio Paper Co., Ltd. were used as the water-absorbent resin particles in Example 3. Since the water-absorbent resin particles in the absorbent body were mixed with pulp, the pulp was removed as much as possible by air injection.
[0040] 3. Shaking test Test 1 Each powder consisting of water-absorbent resin particles was filled into a polyethylene bag with a zipper (inner size of zipper: 70 mm × 50 mm, thickness 0.04 mm, capacity 35 mL). The amount of powder filled was set to an amount corresponding to a theoretical filling rate of 100%, 90%, 80%, 70%, or 60%. The polyethylene bag filled with the powder was placed on a JIS standard sieve with an opening of 850 μm. The powder was then shaken for 30 minutes by applying vibrations including vertical motion to the standard sieve using an electromagnetic vibration type sieve shaker Octagon 200 (manufactured by Endecotts) with a vibration intensity set to 7. In the case of a vibration intensity of 7, the calculated acceleration experienced by the powder is a maximum of 2.2 G. The water absorption under load of the water absorbent resin particles after shaking was measured. For comparison, the water absorption under load of the water absorbent resin particles before shaking was also measured. Table 1 shows the packed bulk density of powder made of each water-absorbent resin particle, and the amount of powder (water-absorbent resin particle) corresponding to each theoretical packing rate.
[0041] [Table 1]
[0042] The measurement results of water absorption under load are shown in Table 2. The values in parentheses are the loss on drying. It was confirmed that the water absorption under load was improved by shaking for all water-absorbent resin particles.
[0043] [Table 2]
[0044] Test 2 The powder of the water-absorbent resin particles of Examples 1 to 3, which was filled in a polyethylene bag at a theoretical filling rate of 90%, was shaken in the same manner as in Test 1, except that the shaking time was changed to 300 minutes. For the water-absorbent resin particles of Example 2, an intermittent shaking test was also conducted in which shaking and standing were repeated in the order of 2 hours shaking, 1 hour standing, 2 hours shaking, 1 hour standing, and 1 hour shaking, for a total of 300 minutes. The water absorption under load of the water-absorbent resin particles after shaking was measured. Table 3 shows the evaluation results together with a part of the results of Test 1. The value in parentheses is the loss on drying.
[0045] [Table 3]
[0046] Test 3 A powder consisting of the water-absorbent resin particles of Example 2, packed in a polyethylene bag at a theoretical packing rate of 90%, was shaken in the same manner as in Test 1, except that the vibration intensity of the sieve shaker was changed to 1, 3, or 10. The water absorption amount under load of the water-absorbent resin particles after shaking was measured. Table 4 shows the evaluation results together with some of the results of Test 1. The values in parentheses are the loss on drying. Table 4 also shows the calculated acceleration (maximum value) experienced by the powder for each vibration intensity.
[0047] [Table 4] [Explanation of symbols]
[0048] 1...powder containing water-absorbent resin particles, 3...container, 5...support.
Claims
1. A method for improving a water absorption capacity under load of water-absorbent resin particles, comprising a step of increasing a water absorption capacity under load of the water-absorbent resin particles by shaking a powder containing a plurality of water-absorbent resin particles contained in a container, wherein the water absorption capacity under load is a water absorption capacity under load measured under a load in which a pressure of 4.14 kPa is applied to the powder made of the water-absorbent resin particles.
2. The amount of the powder contained in the container corresponds to a theoretical filling rate of less than 100%, The theoretical filling rate is calculated by the following formula: Theoretical filling rate [%] = {(X [g] / D [g / mL]) / V [mL]}×100 where X is the mass of the powder, D is the packed bulk density of the powder, and V is the maximum volume of the container. The method of claim 1.
3. 3. The method according to claim 1, wherein the maximum acceleration experienced by the powder during shaking is 0.050 to 4.0 G.
4. The method according to any one of claims 1 to 3, wherein the powder contained in the container is shaken for a total time of 10 minutes or more.
5. A method for producing water-absorbent resin particles, comprising a step of improving a water absorption capacity under load of the water-absorbent resin particles by the method according to any one of claims 1 to 4, wherein the water absorption capacity under load is a water absorption capacity under load measured under a load in which a pressure of 4.14 kPa is applied to a powder consisting of the water-absorbent resin particles.
Citation Information
Patent Citations
Water absorbent and method for producing the same
JP2002212301A
Process for producing absorbent article
JP2005015995A
Water absorbent composite, its manufacturing method and material using water absorbent composite
JP2006168324A
Absorbent resin particle, absorber containing the same, and absorbent product
JP2011231255A
Absorbent and its manufacturing method
JP2014094379A