Method for improving water absorption under load of water-absorbent resin particles, and method for producing water-absorbent resin particles

Shaking water-absorbing resin particles under load improves their absorption capacity by up to 150% through a method that applies pressure during shaking, addressing the challenge of maintaining absorption under pressure.

JP7554750B2Active Publication Date: 2024-09-20SUMITOMO SEIKA CHEM CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021530649
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-05
Filing Date
2020-07-01
Publication Date
2024-09-20
Estimated Expiration
2040-07-01

AI Technical Summary

Technical Problem

Existing water-absorbing resin particles struggle to maintain a high water absorption capacity under load or pressure.

Method used

A method involving shaking water-absorbing resin particles while applying a load to improve their water absorption capacity under load, which includes steps such as using a container with a weight to apply pressure and shaking the particles.

Benefits of technology

Enhances the water absorption capacity of resin particles under load, achieving improvements up to 150% or more compared to the initial absorption capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554750000003
    Figure 0007554750000003
  • Figure 0007554750000004
    Figure 0007554750000004
  • Figure 0007554750000002
    Figure 0007554750000002
Patent Text Reader

Abstract

Disclosed is a method for improving the water absorption of a powder under a load, the method including a step that shakes a powder that includes water-absorbent resin particles while applying a load to the powder . The maximum value of the acceleration undergone by the shaken powder may be 0.050-4.0 G.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for improving the water absorption under load of water-absorbent resin particles, and a method for producing water-absorbent resin particles. [Background technology]

[0002] Water-absorbent resin particles are widely used in the field of sanitary materials, etc. Water-absorbent resin particles are sometimes required to maintain a large water absorption capacity even under load or pressure (for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2002-212301 A [Patent Document 2] JP 2011-231255 A Summary of the Invention [Problem to be solved by the invention]

[0004] One aspect of the present invention provides a method for easily improving the water absorption under load of water-absorbent resin particles. [Means for solving the problem]

[0005] One aspect of the present invention relates to a method for improving the water absorption under load of water-absorbent resin particles, the method comprising a step of shaking a powder containing a plurality of water-absorbent resin particles while applying a load to the powder.

[0006] Another aspect of the present invention relates to a method for producing water-absorbent resin particles, comprising the step of improving the water absorption under load of the water-absorbent resin particles by the above-mentioned method. Effect of the Invention

[0007] According to one aspect of the present invention, the water absorption capacity under load of water-absorbent resin particles can be easily improved. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a schematic diagram showing one embodiment of a step of shaking powder containing water-absorbent resin particles. [Diagram 2] FIG. 2 is a schematic diagram showing a method for measuring the water absorption under load of water-absorbent resin particles. [Diagram 3] 1 is a graph showing the relationship between the water absorption under load and the pressure applied to powder containing water-absorbent resin particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, several embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments.

[0010] In this specification, "(meth)acrylic" means both acrylic and methacrylic. "Acrylate" and "methacrylate" are also written as "(meth)acrylate". The same applies to other similar terms. "(Poly)" means both cases with and without the prefix "poly". In the numerical ranges described in stages in this specification, the upper limit or lower limit of a certain numerical range can be arbitrarily combined with the upper limit or lower limit of a numerical range of another stage. In the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the examples. "Water-soluble" means that the material has a solubility of 5% by mass or more in water at 25°C. The materials exemplified in this specification may be used alone or in combination of two or more types. "Physiological saline" means a 0.9% by mass aqueous solution of sodium chloride.

[0011] FIG. 1 is a schematic diagram showing one embodiment of a step of shaking a powder containing a plurality of water-absorbent resin particles. In the method of FIG. 1, a powder 1 contained in a container 3 is shaken. The container 3 is placed on a support 5, and the powder 1 in the container 3 can be shaken by vibrating the support 5. During shaking, a load is applied to the entire powder 1 by a weight 7 placed on the upper part of the container 3. By shaking the powder 1 while applying a load, water-absorbent resin particles exhibiting a larger water absorption amount under load can be obtained. Typically, the powder 1 is substantially composed of only water-absorbent resin particles, but other particles may be contained in the powder 1. The ratio of the water-absorbent resin particles to the total amount of the powder 1 may be 80 to 100 mass%, 90 to 100 mass%, or 95 to 100 mass%.

[0012] The container 3 is not particularly limited as long as it can contain the powder 1 and can apply a load to the powder 1. The container 3 may be, for example, a wooden box, a cardboard box, a plastic bag, or a cloth bag. When the container 3 is a flexible bag such as a plastic bag or a cloth bag, a load can be particularly easily applied to the powder 1 by placing a weight 7 on the container 3. The container 3 may have a lid that can be opened and closed. In this case, the powder 1 may be shaken in a state where the lid is closed, i.e., in a state where the powder 1 is sealed in the container 3. The powder 1 may be shaken while the container 3 containing the powder 1 is being transported.

[0013] The magnitude of the load applied to the powder 1 by the weight 7 is not particularly limited, and may be, for example, a magnitude such that a pressure of 1.0 to 20.0 kPa is applied to the entire powder 1. When the pressure applied to the powder 1 is within this range, the water absorption amount under load of the water absorbent resin particles constituting the powder 1 can be particularly effectively improved while suppressing damage to the water absorbent resin particles constituting the powder 1. From the same viewpoint, the pressure applied to the entire powder 1 may be 2.5 to 15.0 kPa, or 5.0 to 12.0 kPa. For example, when the container 3 is a flexible bag and a load is applied to the entire powder 1 by the weight 7 placed on the container 3, when the horizontal projection area of ​​the powder 1 in the state of being contained in the container 3 can be regarded as the acting area on which the load of the weight 7 is applied to the powder 1, the pressure can be calculated by the following formula. Pressure = weight mass / horizontal projection area of ​​powder

[0014] The method of applying a load to the powder containing water-absorbent resin particles is not limited to the method of placing a weight on the top of the container. For example, a load may be applied to the powder containing water-absorbent resin particles by stacking another container containing the powder containing water-absorbent resin particles.

[0015] The powder 1 may completely fill the container 3, or the amount of powder 1 may be somewhat less than the capacity of the container 3, as long as the powder 1 can be adequately loaded.

[0016] The volume of the container in which the powder containing the water-absorbent resin particles is accommodated for shaking is not particularly limited, but may be, for example, 10 mL to 2000 L. The total mass of the powder to be shaken is not particularly limited, but may be, for example, 10 g to 2000 kg.

[0017] The maximum value of acceleration to which the powder undergoes shaking may be 0.050 to 4.0 G. When the acceleration is within this range, the water absorption under load tends to be improved more significantly. From the same viewpoint, the maximum value of acceleration may be 0.10 to 3.0 G, 0.30 to 2.5 G, 0.5 to 2.5 G, or 1.0 G to 2.5 G. The maximum value of acceleration can be calculated based on the amplitude and frequency of vibration for shaking.

[0018] The time for shaking the powder containing the water-absorbent resin particles (shaking time) may be any length that improves the water absorption capacity under load of the water-absorbent resin particles, and may be, for example, 10 minutes or more, 20 minutes or more, or 30 minutes or more, or may be 24 hours or less. It is not necessary to shake the powder contained in the container continuously, and the powder may be shaken intermittently while stopping the shaking at least once during the process. When shaking the water-absorbent resin particles intermittently, the total shaking time may be within the above range.

[0019] The water absorption under load of the water absorbent resin particles after shaking may be, for example, 15 to 30 g / g. The ratio of the water absorption under load of the water absorbent resin particles after shaking to the water absorption under load of the water absorbent resin particles before shaking may be 103% or more, 105% or more, or 110% or more, or may be 150% or less. The water absorption under load here is a value measured by the method described in the Examples below.

[0020] The water-absorbing resin particles are not particularly limited, and may be particles containing a polymer containing an ethylenically unsaturated monomer as a monomer unit. The ethylenically unsaturated monomer may be a water-soluble monomer, and examples thereof include (meth)acrylic acid and its salts, 2-(meth)acrylamido-2-methylpropanesulfonic acid and its salts, (meth)acrylamide, N,N-dimethyl(meth)acrylamide, 2-hydroxyethyl(meth)acrylate, N-methylol(meth)acrylamide, polyethylene glycol mono(meth)acrylate, N,N-diethylaminoethyl(meth)acrylate, N,N-diethylaminopropyl(meth)acrylate, and diethylaminopropyl(meth)acrylamide. The ethylenically unsaturated monomer may be used alone or in combination of two or more kinds. When the ethylenically unsaturated monomer has a functional group such as a carboxyl group or an amino group, it may function as a functional group that crosslinks the polymer. The water-absorbent resin particles may be particles containing a polymer that contains at least one of (meth)acrylic acid and a salt of (meth)acrylic acid as a monomer unit.

[0021] The polymer constituting the water-absorbent resin particles may be a crosslinked polymer. In this case, the polymer may be crosslinked by self-crosslinking, crosslinking by reaction with a crosslinking agent, or both. The water-absorbent resin particles may be surface-crosslinked by crosslinking at least the polymer in the surface layer portion with a crosslinking agent. The water absorption under load of the surface-crosslinked water-absorbent resin particles may be further improved by shaking. The crosslinking agent for surface crosslinking may be called a surface crosslinking agent.

[0022] Examples of the crosslinking agent include polyols such as ethylene glycol, propylene glycol, 1,4-butanediol, trimethylolpropane, glycerin, polyoxyethylene glycol, polyoxypropylene glycol, and polyglycerin; compounds having two or more epoxy groups such as (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, and (poly)glycerin diglycidyl ether; haloepoxy compounds such as epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin; compounds having two or more isocyanate groups such as 2,4-tolylene diisocyanate and hexamethylene diisocyanate; oxazoline compounds such as 1,2-ethylenebisoxazoline; carbonate compounds such as ethylene carbonate; and hydroxyalkylamide compounds such as bis[N,N-di(β-hydroxyethyl)]adipamide. The crosslinking agent may include a polyglycidyl compound such as (poly)ethylene glycol diglycidyl ether, (poly)glycerin diglycidyl ether, (poly)glycerin triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and polyglycerol polyglycidyl ether. These crosslinking agents may be used alone or in combination of two or more.

[0023] The water-absorbing resin particles may contain various additional components in addition to the polymer of the ethylenically unsaturated monomer. Examples of the additional components include gel stabilizers, metal chelating agents, and flow improvers (lubricants). The additional components may be located inside the polymer particles containing the polymer, on the surface of the polymer particles, or both. The additional component may be a flow improver (lubricant). The flow improver may include inorganic particles. The inorganic particles may include, for example, silica particles such as amorphous silica.

[0024] The shape of the water-absorbent resin particles is not particularly limited, and may be, for example, substantially spherical, crushed, or granular, and primary particles having these shapes may be aggregated to form particles. The median particle size of the water-absorbent resin particles may be 250 to 850 μm, 300 to 700 μm, or 300 to 600 μm.

[0025] The water-absorbent resin particles can be manufactured by a method including, for example, a step of obtaining water-absorbent resin particles containing a polymer containing an ethylenically unsaturated monomer as a monomer unit by a method including polymerizing a monomer containing an ethylenically unsaturated monomer, and a step of improving the water absorption amount under load of the water-absorbent resin particles by the method according to the above-mentioned embodiment. The polymerization method of the monomer can be selected from, for example, a reversed-phase suspension polymerization method, an aqueous solution polymerization method, a bulk polymerization method, and a precipitation polymerization method. From the viewpoint of ensuring good water absorption characteristics of the water-absorbent resin particles and easy control of the polymerization reaction, a reversed-phase suspension polymerization method or an aqueous solution polymerization method may be adopted. Steps such as a crosslinking reaction during or after polymerization, particle formation by pulverization, and drying can be carried out by a normal method as necessary. Surface-crosslinked water-absorbent resin particles can be obtained by a reaction between the particles after polymerization and drying and a surface crosslinking agent.

[0026] The water-absorbent resin particles having improved water absorption capacity under load can be used to manufacture various absorbent articles such as diapers. EXAMPLES

[0027] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.

[0028] 1.Measurement method 1-1.Packed bulk density of powder made of water-absorbent resin particles Using a powder property evaluation device (manufactured by Hosokawa Micron Corporation, model number: PT-X), the packed bulk density of the powder consisting of water-absorbent resin particles was measured according to the following procedure. The packed bulk density was measured under the conditions of room temperature (25°C ± 2°C) and humidity of 50% ± 10%. The mass W0 of the empty cup-shaped container (volume 100 mL, inner diameter about 50 mm, height about 50 mm) was measured. Next, a cylindrical cap (inner diameter 51 mm, height 51 mm) was attached to the top of the container. 100 g of powder was put into the container from the upper opening of the cap using a scoop attached to the device. Next, the container was placed on a tapping lift bar (tapping device) and impacted the powder in the container by tapping 180 times with a stroke of 18 mm. After that, the cap was removed and the powder in the raised part from the upper opening of the container was removed by scraping it off with a blade. Next, the mass W1 of the container containing the powder was measured. Based on the mass W0 and the mass W1, the packed bulk density was calculated from the following formula. The packed bulk density was measured three times in total, and the average value was recorded as the packed bulk density D [g / mL] of the powder consisting of water-absorbent resin particles. Compacted bulk density [g / mL] = (W1 [g] - W0 [g]) / 100 [mL]

[0029] 1-2. Theoretical filling rate The theoretical filling rate when a powder made of water-absorbent resin particles was placed in a polyethylene bag with a zipper was calculated by the following formula. Theoretical filling rate [%]={(X[g] / D[g / mL]) / V[mL]}×100 In the formula, X is the mass of the powder, D is the packed bulk density of the powder, and V is the capacity of the polyethylene bag. The maximum volume of pure water that can be filled into the polyethylene bag with the zipper closed was measured, and this was regarded as the maximum capacity of the polyethylene bag.

[0030] 1-3. Water absorption under load (load: 4.14kPa) The water absorption under load was measured under the conditions of room temperature (25°C ± 2°C) and humidity 50% ± 10%. Figure 2 is a schematic diagram showing a method for measuring the water absorption under load. A glass filter 19 (diameter 9 cm, thickness 7 mm, standard: ISO4793, P-250) was placed in a petri dish 17 with an inner diameter of 12 cm. Then, physiological saline 20 was poured into the petri dish 17 up to the height of the glass filter 19. Powder 1 consisting of water-absorbent resin particles with a mass X [g] was uniformly placed in a cylinder 11 (inner diameter 2.0 cm: outer diameter 3.0 cm: height 5.0 cm) with a 255 mesh bolting cloth (nylon mesh) 13 attached to the end. Here, X was set to 0.1000 ± 0.0005 g. A cylindrical weight 15 having a mass that applies a pressure of 4.14 kPa to the powder 1 was placed on the powder 1 in the cylinder. The weight 15 has an outer diameter slightly smaller than the inner diameter of the cylinder, and can move smoothly up and down inside the cylinder. In this state, the total mass W1 [g] (total mass of the powder 1, cylinder 11, bolting cloth 13 and weight 15) was measured. The cylinder 11 containing the powder 1 and weight 15 was placed on a glass filter 19 in a petri dish 17, and the powder 1 was allowed to swell with physiological saline 20 for one hour. The total mass W2 [g] of the powder 1, cylinder 11, bolting cloth 13 and weight 15 after swelling was measured. The drying loss A [%] of the powder made of water-absorbent resin particles was also measured separately by the method described below. The water absorption under load was calculated by the following formula. Water absorption under load [g / g]=(W2-W1) / {X×(100-A) / 100} The water absorption under load was measured five times, and the average value of the obtained measurements was recorded as the water absorption under load of the water-absorbent resin particles. According to this method, the water absorption under load is measured after removing the influence of the change in the drying loss on the measured value. Therefore, even when the drying loss increases or decreases, the numerical value of the water absorption under load can be compared.

[0031] 1-4.Drying loss 2.0 g of powder consisting of water-absorbent resin particles was placed in an aluminum wheel case (No. 8) previously adjusted to a constant weight (W3 (g)), and its mass W4 (g) was precisely weighed. The precisely weighed powder was dried for 2 hours in a hot air dryer (manufactured by ADVANTEC, model: FV-320) with the internal temperature set to 105°C. After the powder was allowed to cool in a desiccator, its mass W5 (g) was measured as the dry mass. The loss on drying of the water-absorbent resin particles was calculated from the following formula. Loss on drying (mass%) = [{(W4-W3)-(W5-W3)} / (W4-W3)]×100

[0032] 2. Water-absorbing resin particles AquaKeep SA60SXII (trade name, particles containing sodium polyacrylate) manufactured by Sumitomo Seika Chemicals Co., Ltd. was prepared as water-absorbent resin particles. The packed bulk density of the powder made of these water-absorbent resin particles was 0.83 g / mL.

[0033] 3. Shaking test The powder consisting of water-absorbent resin particles was filled into a polyethylene bag with a zipper (inner size of the zipper: 70 mm × 50 mm, thickness 0.04 mm, capacity 35 mL). The amount of the powder filled was 29.05 g, which was an amount equivalent to a theoretical filling rate of 100%. The polyethylene bag filled with the powder was placed on a JIS Z 8801 tray with the zipper facing to the side. A weight (bottom surface: 10 x 10 cm) of 1.0 kg, 2.0 kg, 3.5 kg, or 5.0 kg was placed on the polyethylene bag placed on the tray, and the weight was fixed to the polyethylene bag with adhesive tape. The horizontal projection area of ​​the polyethylene bag placed on the tray was considered to be the acting area where the load was applied from the weight to the powder, and the pressure applied to the entire water-absorbent resin particle powder was estimated by the following formula. Pressure [kPa] = Weight [kg] / 3500 [mm 2 ]×9.81×10 3 Next, the tray was subjected to vibration including vertical motion for 30 minutes using an electromagnetic vibration type sieve shaker Octagon 200 (manufactured by Endecotts) with the vibration intensity set to 1 or 7, so that the powder was shaken for 30 minutes or 300 minutes. The calculated acceleration value that the powder received was a maximum of 0.1 G when the vibration intensity was 1, and a maximum of 2.2 G when the vibration intensity was 7. The water absorption amount under load of the water absorbent resin particles after shaking was measured. For comparison, the water absorption amount under load of the water absorbent resin particles before shaking was also measured.

[0034] [Table 1]

[0035] The measurement results of the water absorption under load are shown in Table 1. Fig. 3 is a graph showing the relationship between the water absorption under load and the pressure applied to the powder. It was confirmed that the water absorption under load was clearly improved by shaking the powder of water-absorbent resin particles while applying a load, compared to before shaking. [Explanation of symbols]

[0036] 1...powder containing water-absorbent resin particles, 3...container, 5...support, 7...weight.

Claims

1. A method for improving a water absorption capacity under load of a water absorbent resin particle, the method comprising a step of shaking a powder containing a plurality of water absorbent resin particles while applying a load to the entire powder, the water absorption capacity under load being a water absorption capacity under load measured under a load in which a pressure of 4.14 kPa is applied to the powder consisting of the water absorbent resin particles.

2. 2. The method of claim 1, wherein the maximum acceleration experienced by the powder while being shaken is between 0.050 and 4.0 G.

3. 3. The method of claim 1 or 2, wherein the powder is shaken for a total time of 10 minutes or more.

4. The method according to any one of claims 1 to 3, wherein the load is applied to the powder such that a pressure of 1.0 to 20.0 kPa is applied across the powder.

5. A method for producing water-absorbent resin particles, comprising a step of improving a water absorption capacity under load of the water-absorbent resin particles by the method according to any one of claims 1 to 4, wherein the water absorption capacity under load is a water absorption capacity under load measured under a load in which a pressure of 4.14 kPa is applied to a powder consisting of the water-absorbent resin particles.

Citation Information

Patent Citations

  • Water absorbent and method for producing the same

    JP2002212301A

  • Process for producing absorbent article

    JP2005015995A

  • Water absorbent composite, its manufacturing method and material using water absorbent composite

    JP2006168324A

  • Absorbent resin particle, absorber containing the same, and absorbent product

    JP2011231255A

  • Absorbent and its manufacturing method

    JP2014094379A