Lithium-ion battery separator coated with surface-treated alumina

A separator coated with surface-treated alumina particles addresses the issues of wettability and mechanical stability in lithium-ion batteries, improving performance and safety by enhancing compatibility and stability.

JP7554773B2Active Publication Date: 2024-09-20EVONIK OPERATIONS GMBH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021566122
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-07
Filing Date
2020-04-28
Publication Date
2024-09-20
Estimated Expiration
2040-04-28

AI Technical Summary

Technical Problem

Conventional polyolefin separators in lithium-ion batteries face issues with low wettability by polar electrolytes and mechanical instability at high temperatures, leading to reduced performance and safety risks due to potential gas formation and electrolyte leakage.

Method used

A separator coated with a binder and surface-treated alumina particles, specifically fumed alumina treated with silane compounds, enhances hydrophobicity and adhesion, improving compatibility with hydrophobic binders and maintaining mechanical stability.

Benefits of technology

The surface-treated alumina coating improves the compatibility and stability of the separator, enhancing the battery's performance and safety by maintaining capacity retention and reducing gas formation, even at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554773000003
    Figure 0007554773000003
  • Figure 0007554773000007
    Figure 0007554773000007
  • Figure 0007554773000002
    Figure 0007554773000002
Patent Text Reader

Abstract

The present invention relates to a separator for a lithium ion battery comprising an organic substrate coated with a coating layer comprising a binder and alumina particles surface-treated with a silane of general formula (I) or (Ia), a method for synthesizing said separator, and its use in a lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a separator for a lithium ion battery comprising an organic substrate coated with a coating layer comprising a binder and alumina particles surface-treated with a silane of general formula (I) or (Ia), a method for the synthesis of said separator and its use in lithium ion batteries.

[0002] In recent years, various energy storage technologies have increasingly attracted public attention and have been the subject of intensive research and development in industry and academia. As energy storage technology expands into devices such as mobile phones, camcorders, laptops, and even electric vehicles, there is an increasing demand for high-energy density batteries to be used as power sources for these devices. Lithium-ion secondary batteries are one of the most important types of batteries currently in use.

[0003] Lithium-ion secondary batteries are usually composed of an anode made of a carbon material or a lithium metal alloy, a cathode made of lithium metal oxide, and an electrolyte in which a lithium salt is dissolved in an organic solvent. The separator in a lithium-ion battery provides the passage of lithium ions between the positive and negative electrodes during the charging and discharging process.

[0004] The safety of lithium-ion batteries is an important issue.

[0005] The separator prevents direct contact between the two electrodes, which would lead to an internal short circuit, and therefore the structure of such a separator is considered to be very important for the safety of lithium-ion batteries.

[0006] Polyolefin separators, such as those made of polyethylene or polypropylene, are the most widely used in lithium-ion batteries due to their excellent mechanical strength, chemical stability, and low cost. However, typical polyolefin separators can exhibit some significant drawbacks. Polyolefin separators are highly hydrophobic, which means that they are rather poorly wetted by polar electrolytes, which can lead to poor performance in lithium-ion batteries. Furthermore, such polyolefin separators can lose mechanical stability and shrink when exposed to high temperatures.

[0007] One possible method to improve the performance of conventional polyolefin separators is to coat such separators with some thermally stable materials, such as inorganic particles.

[0008] EP 2639854 A1 discloses a separator for a lithium secondary battery, comprising a substrate and a coating layer on the surface of the substrate, the coating layer comprising metal oxide particles selected from the group consisting of oxides of the elements Sn, Ce, Mg, Ni, Ca, Zn, Zr, Y, Al, Ti coated with a silane compound, and a binder. The silane preferably has reactive substituents comprising amino, isocyanate, epoxy or mercapto groups. Such reactive groups of the silane allow reaction with the binder, which preferably comprises -COOH or -OH groups.

[0009] The safety of lithium-ion batteries also depends heavily on the type of electrolyte used. Liquid electrolytes, which are currently the most widely used in lithium-ion batteries, are prone to leakage and can easily cause fires or even explosions if the battery is damaged or exposed to high temperatures. These issues could potentially be resolved by using polymer gel electrolytes, which are safer than liquid electrolytes for use in lithium-ion batteries.

[0010] Korean Patent Publication No. 20150099648 discloses a separator membrane coated with inorganic particles modified with a modifying agent having a polymerizable vinyl functional group, such as Si, Sn, Ge, Cr, Al, Mn, Ni, Zn, Zr, Co, In, Cd, Bi, Pb or V oxide. In particular, the production of a polyethylene separator coated with vinyl-modified silica particles is described, which can be used in lithium-ion batteries with gel polymer electrolytes. The vinyl-modified colloidal silica particles are produced by hydrolysis of vinyltrimethoxysilane, followed by separation of the precipitate and drying it at 70°C.

[0011] Korean Patent Publication No. 20170103049 describes a method for producing a separator for lithium ion batteries coated with inorganic particles, comprising the steps of (a) producing suitable inorganic particles, (b) mixing the inorganic particles with a solvent, (c) immersing a separator film in the mixture of inorganic particles and a solvent, and (d) drying the separator film to produce a coated separator film. In particular, the example in Korean Patent Publication No. 20170103049 shows the production of colloidal silica by hydrolysis of tetraorthosilicate (TEOS), free radical polymerization of styrene in the presence of these silica particles, followed by heat treatment at 550° C. to produce modified silica aggregates, which are then treated with 3-methacryloxypropyltrimethoxysilane. These functionalized silica particles are then used to coat separator membranes for lithium ion batteries.

[0012] One problem that can occur when repeatedly charging and discharging a lithium-ion battery is the deterioration of the lithium salts used in the battery electrolyte, such as LiPF 6The problem is that hydrofluoric acid (HF) is produced as a product of hydrolysis of the cathode active material of the battery by trace amounts of water present in the system. HF may react with the cathode active material of the battery, degrading the long-term performance of the battery. As described in Korean Patent Publication No. 20150099648 and Korean Patent Publication No. 20170103049, the presence of silica particles in the coating layer surrounding the separator material can cause the HF and SiO 2 reacts to produce gaseous silicon tetrafluoride (SiF 4 The formation of gas during the operation of a battery cell is particularly disadvantageous as it poses the risk of battery damage or even explosion under the pressure of the gases that are generated.

[0013] WO2014104687 discloses a method for producing a separator for a secondary battery, which comprises a porous polyolefin substrate and an active layer coated on the surface of the substrate. The active layer is made of SiO 2 , Al 2 O 3 , TiO 2 , SnO 2 , CEO 2 , ZrO 2 , BaTiO 3 , Y 2 O 3 and various silane coupling agents. Examples 3 and 4 list alumina particles with an average particle size of 400 nm that are surface-treated with 3-aminopropyltriethoxysilane. In these examples, such surface-treated alumina particles are treated with ZrO (through the existing amino groups of the silane coupling agent). 2 The resulting Al was coupled with the particles. 2 O 3 -Silane-ZrO 2 The hybrid body is coated onto a polyethylene separator membrane.

[0014] US Patent Publication No. 20120301774 describes a method for producing a porous substrate by mixing a binder such as a silane or siloxane with SiO. 2 , Al 2O 3 , CaO, TiO 2 , ZnO, MgO, ZrO 2 , SnO 2 Separators with enhanced antioxidant performance are disclosed, including an active layer containing a mixture of inorganic particles such as dimethylsilane and alumina particles. No combination of (meth)acrylsilane and alumina particles is disclosed. Examples 2 and 3 disclose the preparation of inorganic / organic composite separators, including the treatment of alumina powder with a solution containing polyacrylic acid-sodium polyacrylate and 3-glycidoxypropyltrimethoxysilane.

[0015] The problem addressed by the present invention is to provide an improved separator for use in lithium ion batteries, and such batteries, that provides high capacity retention during charge / discharge processes, especially at high temperatures, without the use of silica as a component of the separator coating.

[0016] The present invention provides a separator for a lithium ion battery comprising an organic substrate coated with a coating layer comprising a binder and a surface-treated alumina, the surface-treated alumina being represented by the general formula (I) or (Ia): [ka] [In the formula, R=H or CH 3 and 0≦h≦2, A is H or a branched or unbranched C1-C4 alkyl group; B is a branched or unbranched, aliphatic, aromatic or mixed aliphatic-aromatic C1-C30 carbon-based group; X is selected from Cl or a group OY, where Y is H, or a C1 to C30 branched or unbranched alkyl, alkenyl, aryl, or aralkyl group, a branched or unbranched C2 to C30 alkyl ether group, or a branched or unbranched C2 to C30 alkyl polyether group, or a mixture thereof.

[0017] Coating Layer The separator of the present invention is coated with a coating layer that includes a binder and surface-treated alumina.

[0018] Surface treated alumina The terms "alumina" and "aluminum oxide" may be used interchangeably in the context of the present invention and refer to alumina particles, for example in the form of a powder or granules.

[0019] The alumina present in the separator according to the invention is surface-treated, in particular a hydrophobic surface treatment, which can improve the compatibility of the alumina particles with the hydrophobic binder and the separator material.

[0020] The surface-treated alumina used in the present invention is preferably hydrophobic and has a methanol wettability in a methanol / water mixture of more than 5% by volume, preferably 10% to 80% by volume, more preferably 15% to 70% by volume, particularly preferably 20% to 65% by volume, and most preferably 25% to 60% by volume.

[0021] The term "hydrophobic" in the context of the present invention refers to particles that have a low affinity for polar media such as water. In contrast, hydrophilic particles have a high affinity for polar media such as water. The hydrophobicity of a hydrophobic material can usually be achieved by providing the surface of the particle with suitable non-polar groups. The degree of hydrophobicity of an inorganic oxide such as hydrophobic alumina can be determined by parameters including its methanol wettability, as described in detail, for example, in WO 2011 / 076518, pages 5-6. In pure water, hydrophobic particles of, for example, alumina, completely separate from the water and float on its surface without being wetted by the solvent. In contrast, in pure methanol, the hydrophobic particles are distributed throughout the volume of the solvent and complete wetting occurs. In the measurement of methanol wettability, the maximum methanol content is determined in a methanol / water test mixture when the alumina is still not wetted, i.e. when 100% of the alumina used remains separated from the test mixture in an unwetted form after contact with the test mixture. This methanol content (volume %) in the methanol / water mixture is called the methanol wettability. The higher the level of methanol wettability, the more hydrophobic the alumina is. The lower the methanol wettability, the less hydrophobic and more hydrophilic the material is.

[0022] The separator of the present invention is represented by general formula (I) or (Ia): R=H or CH 3 , preferably CH 3 and 0≦h≦2, preferably h=0 or 1; A is H or a branched or unbranched C1-C4 alkyl group, preferably A=H or CH 3 and B is a branched or unbranched aliphatic, aromatic or mixed aliphatic-aromatic C1-C30 carbon-based group, preferably B=-(CH 2 ) 3 - and X is selected from Cl or a group OY, where Y is H, or a C1-C30 branched or unbranched alkyl, alkenyl, aryl, or aralkyl group, a branched or unbranched C2-C30 alkyl ether group, or a branched or unbranched C2-C30 alkyl polyether group, or mixtures thereof. Most preferably, X=Cl or OCH 3 It is.

[0023] The compound of general formula (I) is preferably 3-(triethoxysilyl)propyl methacrylate (I, R=Me, h=0, B=-(CH 2 ) 3 -, X=OEt), 3-(trimethoxysilyl)propyl methacrylate (I, R=Me, h=0, B=-(CH 2 ) 3 -, X=OMe), 3-(trichlorosilyl)propyl methacrylate (I, R=Me, h=0, B=-(CH 2 ) 3 -, X=Cl), and mixtures thereof.

[0024] The compound of general formula (Ia) is preferably (dichlorosilanediyl)bis(propane-3,1-diyl)bis(2-methylacrylate) (Ia, R=CH 3 , B=-(CH 2 ) 3 -, X=Cl), (dimethoxysilanediyl)bis(propane-3,1-diyl)bis(2-methylacrylate) (Ia, R=CH 3 , B=-(CH 2 ) 3 -, X=OCH 3 ), (diethoxysilanediyl)bis(propane-3,1-diyl)bis(2-methylacrylate) (Ia, R=CH 3 , B=-(CH 2 ) 3 -, X=OC 2 H 5 ), and mixtures thereof.

[0025] The surface treated alumina is preferably fumed alumina.

[0026] Fumed alumina is alumina obtained from pyrothermal processes, such as flame hydrolysis or flame pyrolysis. In the flame hydrolysis process, an aluminum compound, preferably aluminum chloride, is vaporized, which reacts in a flame generated by the reaction of hydrogen with oxygen to form alumina particles. The powder thus obtained is called "pyrogenic" or "fumed" alumina. This reaction first forms highly dispersed primary particles, which in the further course of the reaction coalesce to form agglomerates. The dimensions of the agglomerates of these powders generally range from 0.2 μm to 1 μm. The powders can be partially broken by suitable grinding and converted into particles in the nanometer (nm) range, which is advantageous for the present invention. Pyrogenically produced aluminum oxide is characterized by a very small particle size, a high specific surface area (BET), a very high purity, a spherical shape of the primary particles, and the absence of pores. The production of fumed alumina by the flame hydrolysis process is described in detail, for example, in DE 19943291 A1.

[0027] The surface-treated alumina is preferably 30 mm 2 / g~200m 2 / g, more preferably 50m 2 / g~150m 2 / g. The specific surface area (BET), also referred to simply as the BET surface area, can be determined by nitrogen adsorption according to the Brunauer-Emmett-Teller method in accordance with DIN 9277:2014.

[0028] The surface-treated alumina preferably has a carbon content of 0.1% to 15.0% by weight, more preferably 0.5% to 5.0% by weight. The carbon content can be determined by elemental analysis. The sample to be analyzed is weighed into a ceramic crucible supplied with a combustion additive and heated in an induction furnace under a flow of oxygen. The carbon present is determined by the addition of CO 2is oxidized to CO 2 The amount of gas is quantified by an infrared detector.

[0029] The surface-treated alumina preferably has a number average particle size d of less than 1 μm, more preferably less than 900 nm, even more preferably from 20 nm to 800 nm, even more preferably from 30 nm to 700 nm, and most preferably from 50 nm to 500 nm. 50 The number average particle size can be determined by dynamic light scattering (DLS). Alumina can be present partially or completely in the form of individual primary particles. However, in the case of fumed alumina, the particles are usually present mostly in the form of aggregates. In the case of aggregate particles, the number average particle size refers to the size of the aggregates.

[0030] The surface-treated alumina preferably has a tap density of 25 g / L to 130 g / L, which can be determined in accordance with DIN ISO 787 / XI and is equal to the quotient of the weight and volume of the powder after tapping with a tap volumeter under defined conditions.

[0031] The pH value of the surface-treated alumina is preferably 3 to 9, more preferably 4 to 8. The pH value can be determined on a 4% aqueous dispersion of the surface-treated fumed alumina in a 1:1 (wt%:wt%) mixture of water:methanol.

[0032] binder The coating layer of the separator of the present invention includes a binder. The material of the binder is not particularly limited, as long as it allows efficient adhesion between the alumina particles and the surface of the organic substrate. The binder can be selected from the group consisting of poly(vinylidene fluoride), copolymers of vinylidene fluoride and hexafluoropropylene, poly(vinyl acetate), poly(ethylene oxide), poly(methyl methacrylate), poly(ethyl acrylate), poly(vinyl chloride), poly(urethane), poly(acrylonitrile), copolymers of ethylene and vinyl acetate, carboxymethyl cellulose, poly(imide), and mixtures thereof.

[0033] The weight ratio of the binder to the alumina can be 0.1:99.9-99:1, preferably 1:99-90:10. If less than 1 wt% of the binder is used relative to the mixture of the binder and the alumina, the adhesion between the alumina particles and the surface of the organic substrate may be insufficient. If the binder exceeds 90 wt%, the porosity of the coating layer containing the binder and the alumina may be reduced.

[0034] The thickness of the coating layer is preferably 0.1 μm to 20 μm, and more preferably 0.1 μm to 10 μm.

[0035] organic base material The separator according to the present invention includes an organic substrate. The material of such an organic substrate is not particularly limited as long as it can be used as a separator for a battery.

[0036] Such organic substrates are usually porous. The porosity of an organic substrate is the ratio of the total pore volume of a certain unit of the organic substrate to the total volume of this unit of the organic substrate, which is preferably more than 30%, more preferably 30% to 80%. If the porosity of the organic substrate is less than 30%, the ion conductivity through the separator membrane may be hindered. On the other hand, if the porosity of the organic substrate is more than 80%, the mechanical stability of the separator membrane may be insufficient, which may increase safety issues.

[0037] The organic substrate may comprise a polyolefin resin, a fluorinated polyolefin resin, a polyester resin, a polyacrylonitrile resin, a cellulose resin, a nonwoven fabric, or a mixture thereof. Preferably, the organic substrate comprises a polyolefin resin, such as a polyethylene or polypropylene-based polymer, a fluorinated resin, such as a polyvinylidene fluoride polymer or polytetrafluoroethylene, a polyester resin, such as polyethylene terephthalate and polybutylene terephthalate, a polyacrylonitrile resin, a cellulose resin, a nonwoven fabric, or a mixture thereof.

[0038] The separator according to the present invention preferably has a total thickness of 5 μm to 200 μm, more preferably 5 μm to 100 μm.

[0039] Separator manufacturing method The present invention further provides a method for producing a separator according to the present invention, comprising the steps of: 1) producing a surface-treated alumina by surface-treating alumina with a surface treatment agent; 2) preparing a coating mixture comprising the surface treated alumina and a binder; 3) coating the surface of the organic substrate with the coating mixture to form a coating layer on the surface of the organic substrate, the coating layer including the surface-treated alumina and the binder; The present invention provides a method comprising:

[0040] Step 1) of the inventive method for producing the inventive separator can be carried out by treating non-surface-treated (hydrophilic) alumina with a surface treatment agent.

[0041] In this step 1), it is preferred to spray the untreated alumina with a suitable surface treatment agent at ambient temperature (about 25°C) and subsequently heat treat the mixture at a temperature between 50°C and 400°C for a period of 1 to 6 hours.

[0042] An alternative method of surface treatment of alumina in step 1) can be carried out by treating the alumina with a suitable surface treatment agent in the form of vapor, followed by heat treatment of the mixture at a temperature between 50°C and 800°C for a period of 0.5 to 6 hours.

[0043] The heat treatment in step 1) can be carried out under a protective gas, for example nitrogen. The surface treatment can be carried out continuously or batchwise in heatable mixers and dryers equipped with spraying devices. Suitable devices can be, for example, ploughshare mixers or plates, cyclones or fluidized bed dryers.

[0044] The amount of surface treatment agent used varies depending on the type of alumina and the type of surface treatment agent applied, but typically 1% to 15% by weight, preferably 2% to 10% by weight of the surface treatment agent is used relative to the amount of alumina.

[0045] In step 2) of the method of the present invention for producing the separator of the present invention, a mixture is produced that includes the surface-treated alumina, a binder, and optionally a solvent. The weight ratio of the binder to the alumina can be 1:99 to 99:1, preferably 10:90 to 90:10. Preferably, the mixture that includes the surface-treated alumina and the binder further includes 1% by weight to 30% by weight of a solvent based on the total mixture. The solvent is not particularly limited as long as it can dissolve the binder. Examples of suitable solvents are acetone, toluene, ethyl acetate, dichloromethane, chloroform, methanol, ethanol, n-butanol, and N-methylpyrrolidone.

[0046] In step 3) of the method of the present invention for producing the separator of the present invention, the surface of the organic substrate is coated with the coating mixture to form a coating layer comprising the surface-treated alumina and the binder on the surface of the organic substrate. Any suitable coating method that allows the application of a relatively thin coating layer can be applied. An example of an apparatus suitable for the coating step is a doctor blade device SA-202 (manufacturer: Tester Sangyo).

[0047] The coating mixture can be further dried or cured on the surface of the organic substrate to form a final coating layer.

[0048] Using Separators The present invention further provides the use of a separator according to the present invention as a component of a lithium ion battery.

[0049] In particular, the present invention provides the use of the separator of the present invention as a component of a lithium ion battery, wherein the lithium ion battery comprises a gel electrolyte.

[0050] The separator of the present invention is 1) preparing an electrolyte precursor solution including a crosslinker, an initiator, and a liquid electrolyte; 2) assembling a lithium ion battery comprising the electrolyte precursor solution, a separator of the present invention, a cathode, and an anode; 3) cross-linking the electrolyte precursor solution to produce a lithium ion battery containing a gel electrolyte; The present invention can be used in a method for producing a lithium ion battery comprising a gel electrolyte, comprising:

[0051] Lithium-ion battery The present invention further provides a lithium ion battery comprising a separator according to the present invention.

[0052] In addition to the separator, the lithium-ion battery of the present invention typically includes a cathode, an anode, and an electrolyte that includes a lithium salt.

[0053] The cathode of a lithium-ion battery typically includes a current collector and a layer of cathode active material formed on the current collector.

[0054] The current collector can be copper foil, nickel foil, stainless steel foil, titanium foil, a polymer substrate coated with a conductive metal, or a combination thereof.

[0055] Cathode active materials include materials capable of reversibly inserting / deintercalating lithium ions and are well known in the art. Such cathode active materials include lithium metal, lithium alloys, silicon, silicon oxide, silicon carbide composites, silicon alloys, Sn, SnO 2 , or transition metal oxides, for example mixed oxides containing Li, Ni, Co, Mn, V or other transition metals.

[0056] The anode of a lithium ion battery includes any suitable material commonly used in lithium ion secondary batteries that can reversibly insert / desorb lithium ions, typical examples of which are carbonaceous materials, including crystalline carbon, such as natural or artificial graphite in the form of plate-like, flake-like, spherical or fibrous types of graphite; amorphous carbon, such as soft carbon, hard carbon, mesophase pitch carbide, calcined coke, etc., or mixtures thereof.

[0057] The liquid electrolyte of the lithium ion battery of the present invention can include any suitable organic solvent commonly used in lithium ion batteries, such as anhydrous ethylene carbonate (EC), dimethyl carbonate (DMC), propylene carbonate, methyl ethyl carbonate, diethyl carbonate, γ-butyrolactone, dimethoxyethane, fluoroethylene carbonate, vinyl ethylene carbonate, or mixtures thereof.

[0058] The electrolyte of a lithium-ion battery typically contains a lithium salt. An example of such a lithium salt is lithium hexafluorophosphate (LiPF 6 ), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium perchlorate (LiClO 4 ), lithium tetrafluoroborate (LiBF 4 ), Li 2 SiF 6 , lithium triflate, LiN(SO 2 CF 2 CF 3 ) 2 and mixtures thereof.

[0059] The lithium ion battery of the present invention may include a liquid electrolyte or a gel electrolyte. A liquid mixture of a lithium salt and an organic solvent that is not cured, polymerized or crosslinked is referred to in the context of the present invention as a "liquid electrolyte". A gel or solid mixture containing a cured, polymerized or crosslinked compound or mixtures thereof, optionally a solvent, and a lithium salt is referred to as a "gel electrolyte". Such a gel electrolyte can be produced by polymerization or crosslinking of a mixture containing at least one reactive, i.e. polymerizable or crosslinkable, compound and a lithium salt.

[0060] The lithium ion battery of the present invention preferably comprises a gel electrolyte prepared from a liquid electrolyte precursor solution, which comprises a crosslinker, an initiator, a lithium salt, and a liquid electrolyte, which preferably comprises a reactive, i.e., polymerizable or crosslinkable, compound. Such reactive compounds may comprise reactive functional groups such as double bonds of vinyl groups, acrylate or methacrylate groups, or combinations thereof. One example of such a reactive compound is vinyl ethylene carbonate.

[0061] The crosslinker may contain two or more reactive functional groups, such as a vinyl group, an acrylate or methacrylate group, or a double bond of a combination thereof. One example of such a crosslinker is tetra(ethylene glycol) diacrylate (TEGDA). The content of the crosslinker in the electrolyte precursor solution may be 0.1% to 10% by weight, more preferably 0.1% to 5% by weight.

[0062] Examples of suitable initiators are t-amyl peroxide, benzoyl peroxide, azobis compounds such as 2,2'-azobis(isobutyronitrile) (AIBN), or combinations thereof.

[0063] The lithium ion battery of the present invention is 1) preparing an electrolyte precursor solution including a crosslinker, an initiator, and a liquid electrolyte; 2) assembling a lithium ion battery comprising the electrolyte precursor solution, a separator of the present invention, a cathode, and an anode; 3) cross-linking the electrolyte precursor solution to produce a lithium ion battery containing a gel electrolyte; The composition can be produced by a method comprising the steps of:

[0064] Experimental section inorganic particles Fumed Alumina 1 The preparation of fumed alumina 1 surface-treated with 3-(trimethoxysilyl)propyl methacrylate was carried out according to Example 11 of EP 1628916. The BET of alumina 1 was 93m. 2 / g and the C content was 4.0 wt%.

[0065] AEROXIDE® Alu C 805 Fumed alumina surface treated with n-octyltrimethoxysilane: AEROXIDE® Alu C 805, manufacturer: Evonik Resource Efficiency GmbH. According to the data sheet, the BET of AEROXIDE® Alu C 805 is 75-105m 2 / g, and the C content was 3.5 to 4.5 wt%.

[0066] AEROSIL® R 711 Fumed silica surface treated with 3-(trimethoxysilyl)propyl methacrylate: AEROSIL® R711, manufacturer: Evonik Resource Efficiency GmbH. According to the data sheet, the BET of AEROSIL® R711 is 125-175m 2 / g, and the C content was 4.5 to 6.5 wt%.

[0067] Separator 9 μm thick polyethylene film (manufacturer: SK Innovation).

[0068] binder Copolymer of polyvinylidene fluoride and hexafluoropropylene (Kynar Flex® 2801-00, manufactured by Arkema).

[0069] Separator Coating: General Procedure A doctor blade device SA-202 (manufacturer: Tester Sangyo) was used to coat the polyethylene separator film with a mixture of inorganic particles and binder (inorganic particles:binder:NMP=5:5:90 (by weight)) diluted with N-methyl-2-pyrrolidone as a solvent to give a total thickness of the coated polyethylene separator of 15 μm.

[0070] Lithium-ion battery The anode and cathode electrodes, separator, and electrolyte were purchased from Bexel, Korea. The negative and positive electrodes had a design area capacity ratio (N / P ratio) of 1.175 and an area capacity of 2.0 mAh / cm. 2 A lithium-ion battery was constructed using the following materials: Anode Electrode: Showa Denko artificial graphite (loading amount: 6.86 mg / cm 2 ) 90% by weight + conductive carbon 3% by weight + PVdF binder KF9130 (Kureha) 7% by weight Cathode Electrode: NCM 622, LiNi 0.6 Co 0.2 Mn 0.2 O 2 (Loading amount: 12.0 mg / cm 2 ) 95% by weight + conductive carbon 3% by weight + PVdF binder KF7208 (Kureha) 2% by weight Separator: Polyethylene film coated with the above inorganic particles Electrolytes: Liquid electrolyte (LE): LiPF in ethylene carbonate (EC) / ethyl methyl carbonate (EMC) / diethyl carbonate (DEC) (3:5:2 vol:vol:vol) (manufacturer: Panax Etec) 6 A mixture of 100% by weight of a 1.15M solution of fluoroethylene carbonate (FEC, manufacturer: Panax Etec) and 5% by weight of vinylethylene carbonate (VEC, manufacturer: Panax Etec) Gel Electrolyte (GE): A mixture of 100% by weight of the above liquid electrolyte, 6% by weight of tetra(ethylene glycol) diacrylate (TEGDA, manufacturer: Sigma-Aldrich), and 0.06% by weight of 2,2'-azobis(isobutyronitrile) (AIBN, manufacturer: Sigma-Aldrich).

[0071] Lithium-ion battery (coin cell) assembly: (1) Cut the cathode electrode to a diameter of 14 mm, the anode electrode to a diameter of 16 mm, and the separator to a diameter of 18 mm.

[0072] (2) The circular cathode, anode and separator are placed in a glove box for assembly.

[0073] (3) Prepare a coin cell (CR2032) as a coin cell part consisting of a case, a gasket, a disk (thickness 1 mm), a spring and a cap.

[0074] (4) Place the case and cathode electrode in the center with the coated side facing up.

[0075] (5) Using a micropipette, measure out 40 μL of the gel electrolyte precursor solution or liquid electrolyte and drop it into the well of the cathode electrode.

[0076] (6) Place the separator on top of the cathode electrode. Be careful not to form any air bubbles between the cathode electrode and the separator. If there are any air bubbles, use Teflon tweezers to remove them from between the separator and the cathode electrode. If the separator is coated, place the coated side up so that it contacts the anode electrode.

[0077] (7) Insert the gasket in the correct direction to prevent the cathode and anode electrodes from moving.

[0078] (8) Using a micropipette, measure out 40 μL of the gel electrolyte precursor solution or liquid electrolyte and drop it onto the center of the separator fixed with a gasket.

[0079] (9) Place the anode electrode with the coated surface facing down, and place the disk portion, spring portion, and cap portion on the anode copper foil in that order.

[0080] (10) Press the assembled cell with the top surface of a pair of Teflon tweezers to ensure that all parts fit well, then use a crimping machine to complete the CR2032 coin cell.

[0081] (11) For the aging process, the coin cell was placed in an oven at 25 °C for 12 h to thoroughly wet the separator and electrodes with the liquid electrolyte or gel electrolyte precursor.

[0082] (12) After the aging process, the coin cells are placed in an oven at 70 °C for 2 h to induce chemical cross-linking of the gel electrolyte precursor.

[0083] (13) Remove the coin cell from the oven and proceed with further testing.

[0084] Lithium-ion battery testing Alternating current (AC) impedance AC impedance was measured using an AC impedance analyzer CHI 660D (manufacturer: CH instruments) at 25° C. or 55° C. The values ​​measured using one coin cell are shown in Tables 1 and 2 below.

[0085] [Table 1]

[0086] [Table 2]

[0087] Tables 1 and 2 show that lithium ion batteries with the separators of the present invention coated with surface treated alumina particles demonstrate less increase in AC impedance after 300 recharge cycles at 25° C. and 100 cycles at 55° C. compared to the same uncoated separators and separators coated with other inorganic particles.

[0088] Cycle Performance Cycle performance was measured at 25°C or 55°C using a battery cycler PEBC 50.2 (manufacturer: PNE solutions) with a cut-off voltage of 3.0 to 4.3 V, a charge rate of 0.5 C CC / CV, and a discharge rate of 0.5 C CC / CV (0.5 C rate is 1.0 mAh / cm). 2 The measurements were performed at a current density of 1000 kV (corresponding to a current density of 1000 kV). To ensure reproducibility of the results, at least 3-5 cells were assembled and tested in each case. The average values ​​of these tests are shown in Tables 3 and 4 below.

[0089] [Table 3]

[0090] [Table 4]

[0091] Tables 3 and 4 show that lithium ion batteries with the separators of the present invention coated with surface treated alumina particles demonstrate higher retention after 300 recharge cycles at 25° C. and 100 cycles at 55° C. compared to the same uncoated separators and separators coated with other inorganic particles.

[0092] Hydrofluoric Acid (HF) Content Measurement After storing a mixture of electrolyte (89.4 wt%), cross-linker (5.7 wt%), initiator (0.1 wt%), and inorganic particles (4.8 wt%) at 55°C for 7 days, the HF content of the mixture was measured by acid-base titration with a 0.01 M solution of triethylamine in dimethyl carbonate (DMC) using methyl orange as indicator.

[0093] [Table 5]

[0094] The HF content measurements (Table 5) show that both samples with hydrophobic silica and alumina coated separators have increased HF content compared to uncoated separators, but the system with silica particles shows twice as much HF as the system with alumina particles. Both silica and alumina powders necessarily contain traces of water, which contributes to the LiPF 6 This leads to partial hydrolysis of

Claims

1. A separator for a lithium ion battery comprising an organic substrate coated with a coating layer comprising a binder and a surface-treated alumina, the surface-treated alumina being represented by the general formula (Ia): [Formula 1] [In the formula, R=H or CH 3 and B is a branched or unbranched aliphatic, aromatic or mixed aliphatic-aromatic C1-C30 carbon-based group; X is selected from Cl or a group OY, where Y is H, or a C1 to C30 branched or unbranched alkyl, alkenyl, aryl, or aralkyl group, a branched or unbranched C2 to C30 alkyl ether group, or a branched or unbranched C2 to C30 alkyl polyether group, or a mixture thereof.

2. The compound of general formula (Ia) is (dichlorosilanediyl)bis(propane-3,1-diyl)bis(2-methylacrylate) (Ia, R=CH 3 , B=-(CH 2 ) 3 -, X=Cl), (dimethoxysilanediyl)bis(propane-3,1-diyl)bis(2-methylacrylate) (Ia, R=CH 3 , B=-(CH 2 ) 3 -, X=OCH 3 ), (diethoxysilanediyl)bis(propane-3,1-diyl)bis(2-methylacrylate) (Ia, R=CH 3 , B=-(CH 2 ) 3 -, X=OC 2 H 5 2. The separator of claim 1, wherein the separator is selected from the group consisting of fluororesin, fluorosilicate, fluoroisotope ... and mixtures thereof.

3. 3. The separator according to claim 1, wherein the surface-treated alumina is fumed alumina.

4. The surface-treated alumina is 50 mm 2 / g ~ 150m 2 4. The separator according to claim 1, having a specific BET surface area of ​​1 / g.

5. The separator according to any one of claims 1 to 4, wherein the surface-treated alumina has a carbon content of 0.5% to 5.0% by weight.

6. The surface-treated alumina has a number average particle diameter d of 20 nm to 400 nm. 50 The separator of claim 1 , having the formula:

7. The separator according to claim 1 , wherein the organic substrate comprises a polyolefin resin, a fluorinated polyolefin resin, a polyester resin, a polyacrylonitrile resin, a cellulose resin, a nonwoven fabric, or a mixture thereof.

8. 8. The separator of claim 1, wherein the binder is selected from the group consisting of poly(vinylidene fluoride), copolymers of vinylidene fluoride and hexafluoropropylene, poly(vinyl acetate), poly(ethylene oxide), poly(methyl methacrylate), poly(ethyl acrylate), poly(vinyl chloride), poly(urethane), poly(acrylonitrile), copolymers of ethylene and vinyl acetate, carboxymethyl cellulose, poly(imide), and mixtures thereof.

9. The separator according to any one of claims 1 to 8, wherein the separator has a total thickness of 5 µm to 200 µm.

10. The separator according to any one of claims 1 to 9, wherein the coating layer has a thickness of 0.1 µm to 20 µm.

11. A method for producing the separator according to any one of claims 1 to 10, comprising the steps of: 1) producing a surface-treated alumina by surface-treating alumina with a surface treatment agent; 2) preparing a coating mixture comprising the surface treated alumina and a binder; 3) coating a surface of an organic substrate with the coating mixture to form a coating layer on the surface of the organic substrate, the coating layer including the surface-treated alumina and the binder; A method comprising:

12. 11. Use of the separator according to any one of claims 1 to 10 as a component of a lithium-ion battery.

13. 13. The use of the separator of claim 12, wherein the lithium ion battery comprises a gel electrolyte.

14. A lithium ion battery comprising a separator according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Pyrolytically produced, surface-modified aluminum oxide

    JP2006526559A

  • Separator for electrochemical cell, and lithium secondary battery

    JP2007294437A

  • Separator for lithium ion secondary battery, and lithium ion secondary battery

    JP2011044419A

  • Self-supporting, heat-resistant microporous film for use in energy storage devices.

    JP2012521615A

  • Lithium secondary battery