High-strength steel plate with excellent workability and manufacturing method thereof

A high-strength steel plate with a tailored composition and microstructure addresses the balance between strength and workability by optimizing C, Mn, and Si/Al ratios, achieving superior ductility, bending, and hole expandability through controlled manufacturing processes.

JP7554827B2Active Publication Date: 2024-09-20CLEANSOLUTION CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2022536956
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-18
Filing Date
2020-11-24
Publication Date
2024-09-20
Estimated Expiration
2040-11-24

AI Technical Summary

Technical Problem

Existing high-strength steel sheets for automobile parts face challenges in achieving a balance between high strength and excellent workability, such as ductility, bending workability, and hole expandability, as current methods fail to satisfy a tensile strength and elongation rate of 22,000 MPa% or more.

Method used

A high-strength steel plate with a specific composition and microstructure, including 0.25 to 0.75% C, 0.9 to 5.0% Mn, 0.15% P or less, and a microstructure of 30 to 70% tempered martensite, 10 to 45% bainite, 10 to 40% retained austenite, and 3 to 20% ferrite, along with controlled Si and Al content ratios, is manufactured through a process involving hot rolling, annealing, and controlled cooling.

Benefits of technology

The steel plate achieves a balance between tensile strength and elongation ratio of 22,000 MPa% or more, hole expansion rate of 7×10^6 (MPa^2 %^1/2) or more, and bending radius of 0.5 to 3.0, ensuring excellent strength and workability for automobile parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554827000009
    Figure 0007554827000009
  • Figure 0007554827000010
    Figure 0007554827000010
  • Figure 0007554827000007
    Figure 0007554827000007
Patent Text Reader

Abstract

The present invention relates to a steel sheet that can be used for automobile parts, etc., and has an excellent balance between strength and ductility and a balance between strength and hole expandability, and is excellent in bending workability. The present invention relates to a steel sheet and a method for producing the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel sheet that can be used for automobile parts and the like, and relates to a steel sheet that has high strength properties and excellent workability, and a method for producing the same. [Background technology]

[0002] In recent years, the automobile industry has been focusing on ways to reduce the weight of materials in order to protect the global environment while at the same time ensuring the stability of passengers. In order to meet the demands for stability and weight reduction, the use of high-strength steel sheets has been rapidly increasing. It is generally known that the higher the strength of a steel sheet, the lower the workability of the steel sheet. Therefore, there is a demand for steel sheets for automobile parts that have high strength properties while also having excellent workability, such as ductility, bending workability, and hole expandability.

[0003] As a technique for improving the workability of steel sheets, a method of utilizing tempered martensite is disclosed in Patent Documents 1 and 2. Since tempered martensite made by tempering hard martensite is softened martensite, there is a difference in strength between tempered martensite and existing untempered martensite (fresh martensite). Therefore, by forming tempered martensite by suppressing fresh martensite, workability can be improved.

[0004] However, the techniques disclosed in Patent Documents 1 and 2 do not satisfy the balance between tensile strength and elongation (TS×El) of 22,000 MPa% or more, which means that it is difficult to obtain steel sheets with both excellent strength and ductility.

[0005] Meanwhile, in order to obtain both high strength and excellent workability in steel sheets for automotive components, TRIP (Transformation Induced Plasticity) steel, which uses organic sintering to transform retained austenite, has been developed. Patent Document 3 discloses TRIP steel with excellent strength and workability.

[0006] In Patent Document 3, polygonal ferrite, retained austenite, and martensite are included to improve ductility and workability. However, since bainite is the main phase, high strength cannot be ensured, and the balance between tensile strength and elongation (TS×El) does not satisfy the requirement of 22,000 MPa% or more.

[0007] That is, the current situation is that the demand for a steel sheet having high strength and excellent workability, such as ductility, bending workability, and hole expandability, is not met. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Korean Patent Publication No. 10-2006-0118602 [Patent Document 2] JP 2009-019258 A [Patent Document 3] Korean Patent Publication No. 10-2014-0012167 Summary of the Invention [Problem to be solved by the invention]

[0009] According to one aspect of the present invention, it is possible to provide a high-strength steel sheet having excellent ductility, bending workability, and hole expandability by optimizing the composition and microstructure of the steel sheet, and a method for manufacturing the same.

[0010] The object of the present invention is not limited to the above. Further object of the present invention is described in the entire contents of the specification, and a person having ordinary skill in the art to which the present invention pertains will have no difficulty in understanding the further object of the present invention from the contents described in the specification of the present invention. [Means for solving the problem]

[0011] A high-strength steel plate with excellent workability according to one aspect of the present invention contains, by weight, 0.25 to 0.75% C, 4.0% or less Si, 0.9 to 5.0% Mn, 5.0% or less Al, 0.15% or less P, 0.03% or less S, 0.03% or less N, with the remainder being Fe and unavoidable impurities, and contains, as a microstructure, 30 to 70% by volume of tempered martensite, 10 to 45% by volume of bainite, 10 to 40% by volume of retained austenite, 3 to 20% by volume of ferrite, and unavoidable structures, and can satisfy the following [Relational Formula 1]. [Equation 1] 1.1≦[Si+Al] F / [Si+Al] γ <=3.0 In the above formula 1, [Si+Al] F is the average total content (wt%) of Si and Al contained in ferrite, [Si+Al] γ is the average total content (wt%) of Si and Al contained in the retained austenite.

[0012] The steel sheet may further include any one or more of the following (1) to (9). (1) One or more of Ti: 0-0.5%, Nb: 0-0.5%, and V: 0-0.5% (2) At least one of Cr: 0-3.0% and Mo: 0-3.0% (3) One or more of Cu: 0-4.5% and Ni: 0-4.5% (4) B: 0 to 0.005% (5) One or more of Ca: 0-0.05%, REM excluding Y: 0-0.05%, and Mg: 0-0.05%. (6) One or more of W: 0-0.5% and Zr: 0-0.5% (7) One or more of Sb: 0-0.5% and Sn: 0-0.5% (8) One or more of Y: 0-0.2% and Hf: 0-0.2% (9) Co: 0-1.5%

[0013] The total content of Si and Al (Si+Al) may be 1.0 to 6.0% by weight.

[0014] The above steel sheet has a balance between tensile strength and elongation (B T·E ) is 22,000 (MPa%) or more, and the balance between tensile strength and hole expansion ratio (B T·H ) is 7 x 10 6 (MPa 2 % 1 / 2 ) or more, and the bending rate (B R ) may be in the range of 0.5 to 3.0. [Equation 2] B T·E = [tensile strength (TS, MPa)] × [elongation rate (El, %)] [Equation 3] B T·H =[Tensile strength (TS, MPa)] 2 × [Hole expansion rate (HER,%)] 1 / 2 [Equation 4] B R =R / t In the above Relational Formula 4, R means the minimum bending radius (mm) at which no cracks occur after a 90° bending test, and t means the thickness (mm) of the steel plate.

[0015] A method for producing a high strength steel sheet having excellent workability according to another aspect of the present invention includes the steps of heating and hot rolling a steel slab containing, by weight, C: 0.25 to 0.75%, Si: 4.0% or less, Mn: 0.9 to 5.0%, Al: 5.0% or less, P: 0.15% or less, S: 0.03% or less, N: 0.03% or less, and the remainder being Fe and inevitable impurities; coiling the hot rolled steel sheet; and heat treating the coiled steel sheet by hot rolling annealing at a temperature range of 650 to 850° C. for 600 to 1700 seconds. The method may include the steps of: cold rolling the steel sheet heat-treated by the hot rolling annealing; heating the cold rolled steel sheet to a temperature range of Ac1 or more and less than Ac3 (primary heating) and maintaining the temperature for 50 seconds or more (primary maintenance); cooling to a temperature range of 100 to 300°C at an average cooling rate of 1°C / s or more (primary cooling); heating the primarily cooled steel sheet to a temperature range of 300 to 500°C (secondary heating) and maintaining the temperature for 50 seconds or more (secondary maintenance); and cooling to room temperature (secondary cooling).

[0016] The steel slab may further include any one or more of the following (1) to (9). (1) One or more of Ti: 0-0.5%, Nb: 0-0.5%, and V: 0-0.5% (2) At least one of Cr: 0-3.0% and Mo: 0-3.0% (3) One or more of Cu: 0-4.5% and Ni: 0-4.5% (4) B: 0 to 0.005% (5) One or more of Ca: 0-0.05%, REM excluding Y: 0-0.05%, and Mg: 0-0.05%. (6) One or more of W: 0-0.5% and Zr: 0-0.5% (7) One or more of Sb: 0-0.5% and Sn: 0-0.5% (8) One or more of Y: 0-0.2% and Hf: 0-0.2% (9) Co: 0-1.5%

[0017] The total content of Si and Al (Si+Al) contained in the steel slab may be 1.0 to 6.0% by weight.

[0018] The steel slab may be heated in a temperature range of 1000 to 1350°C and finish hot rolled in a temperature range of 800 to 1000°C.

[0019] The hot-rolled steel sheet may be coiled at a temperature in the range of 300 to 600°C.

[0020] The cold rolling may have a reduction rate of 30 to 90%.

[0021] The cooling rate of the secondary cooling may be 1° C. / s or more. Effect of the Invention

[0022] According to a preferred aspect of the present invention, it is possible to provide a steel sheet which is not only excellent in strength but also excellent in workability such as ductility, bending workability, and hole expandability, and is particularly suitable for automobile parts. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The present invention relates to a high-strength steel plate having excellent workability and a manufacturing method thereof, and preferred embodiments of the present invention will be described below. The embodiments of the present invention may be modified in various ways, and the scope of the present invention should not be construed as being limited to the embodiments described below. The embodiments are provided to further explain the present invention in detail to those skilled in the art to which the present invention pertains.

[0024] The inventors of the present invention have come to realize that in a transformation induced plasticity (TRIP) steel containing bainite, tempered martensite, retained austenite, and ferrite, when the ratio of a specific component contained in the retained austenite and ferrite is controlled within a certain range while stabilizing the retained austenite, it is possible to simultaneously ensure the workability and strength of the steel sheet by reducing the interphase hardness difference between the retained austenite and ferrite. Having investigated this, the inventors have devised a method for improving the ductility and workability of high-strength steel, and have arrived at the present invention.

[0025] Hereinafter, a high-strength steel sheet with excellent workability according to one aspect of the present invention will be described in more detail.

[0026] A high-strength steel plate with excellent workability according to one aspect of the present invention contains, by weight, 0.25 to 0.75% C, 4.0% or less Si, 0.9 to 5.0% Mn, 5.0% or less Al, 0.15% or less P, 0.03% or less S, 0.03% or less N, with the remainder being Fe and unavoidable impurities, and contains, as a microstructure, 30 to 70% by volume of tempered martensite, 10 to 45% by volume of bainite, 10 to 40% by volume of retained austenite, 3 to 20% by volume of ferrite, and unavoidable structures, and can satisfy the following [Relational Formula 1]. [Equation 1] 1.1≦[Si+Al] F / [Si+Al] γ <=3.0 In the above formula 1, [Si+Al] F is the average total content (wt%) of Si and Al contained in ferrite, [Si+Al] γ is the average total content (wt%) of Si and Al contained in the retained austenite.

[0027] The steel composition of the present invention will be described in more detail below. Unless otherwise specified, % representing the content of each element is based on weight.

[0028] A high-strength steel sheet with excellent workability according to one aspect of the present invention contains, by weight percent, C: 0.25 to 0.75%, Si: 4.0% or less, Mn: 0.9 to 5.0%, Al: 5.0% or less, P: 0.15% or less, S: 0.03% or less, N: 0.03% or less, the balance being Fe and inevitable impurities, and additionally Ti: 0.5% or less (including 0%), Nb: 0.5% or less (including 0%), V: 0.5% or less (including 0%), Cr: 3.0% or less (including 0%), Mo: 3.0% or less (including 0%), Cu: 4.5% or less (including 0%), Ni: 4.5% or less (including 0%), B: 0.005% or less (including 0%), Ca: 0.05% or less (including 0%), REM excluding Y: It may further contain one or more of the following: 0.05% or less (including 0%), Mg: 0.05% or less (including 0%), W: 0.5% or less (including 0%), Zr: 0.5% or less (including 0%), Sb: 0.5% or less (including 0%), Sn: 0.5% or less (including 0%), Y: 0.2% or less (including 0%), Hf: 0.2% or less (including 0%), Co: 1.5% or less (including 0%). The total content of Si and Al (Si+Al) may be 1.0 to 6.0%.

[0029] Carbon (C): 0.25~0.75% Carbon (C) is an essential element for ensuring the strength of the steel sheet, and also an element for stabilizing the retained austenite that contributes to improving the ductility of the steel sheet. Therefore, in order to achieve this effect, the present invention may contain 0.25% or more of carbon (C). A preferred carbon (C) content may be more than 0.25%, 0.27% or more, or 0.30% or more. A more preferred carbon (C) content may be 0.31% or more. On the other hand, if the carbon (C) content exceeds a certain level, cold rolling may become difficult due to an excessive increase in strength. Therefore, the present invention may limit the upper limit of the carbon (C) content to 0.75%. The carbon (C) content may be 0.70% or less, and a more preferred carbon content (C) may be 0.67% or less.

[0030] Silicon (Si): 4.0% or less (excluding 0%) Silicon (Si) is an element that contributes to improving strength through solid solution strengthening, and is also an element that improves workability by strengthening ferrite and homogenizing the structure. Silicon (Si) is also an element that inhibits the precipitation of cementite and contributes to the generation of retained austenite. Therefore, in the present invention, silicon (Si) can be added as an essential component to achieve such effects. A preferred silicon (Si) content may be 0.02% or more, and a more preferred silicon (Si) content may be 0.05% or more. However, if the silicon (Si) content exceeds a certain level, it may not only cause a coating defect problem like non-coating in the coating process, but also may reduce the weldability of the steel sheet, so the present invention may limit the upper limit of the silicon (Si) content to 4.0%. A preferred upper limit of the silicon (Si) content may be 3.8%, and a more preferred upper limit of the silicon (Si) content may be 3.5%.

[0031] Aluminum (Al): 5.0% or less (excluding 0%) Aluminum (Al) is an element that combines with oxygen in steel to perform deoxidation. Aluminum (Al) is also an element that inhibits cementite precipitation and stabilizes retained austenite, similar to silicon (Si). Therefore, in the present invention, aluminum (Al) can be added as an essential component to achieve such effects. A preferred aluminum (Al) content may be 0.05% or more, and a more preferred aluminum (Al) content may be 0.1% or more. On the other hand, when aluminum (Al) is added excessively, not only the inclusions in the steel sheet are increased, but also the workability of the steel sheet may be reduced, so that the present invention can limit the upper limit of the aluminum (Al) content to 5.0%. A preferred upper limit of the aluminum (Al) content may be 4.75%, and a more preferred upper limit of the aluminum (Al) content may be 4.5%.

[0032] On the other hand, the total content (Si+Al) of silicon (Si) and aluminum (Al) is preferably 1.0 to 6.0%. In the present invention, silicon (Si) and aluminum (Al) are components that affect the formation of a microstructure and influence ductility, bending workability, and hole expandability, so the total content of silicon (Si) and aluminum (Al) is preferably 1.0 to 6.0%. More preferably, the total content (Si+Al) of silicon (Si) and aluminum (Al) may be 1.5% or more, or 4.0% or less.

[0033] Manganese (Mn): 0.9-5.0% Manganese (Mn) is an element useful for increasing both strength and ductility. Therefore, in order to achieve this effect, the present invention may limit the lower limit of the manganese (Mn) content to 0.9%. A preferred lower limit of the manganese (Mn) content may be 1.0%, and a more preferred lower limit of the manganese (Mn) content may be 1.1%. On the other hand, when manganese (Mn) is added in excess, the bainite transformation time increases and the carbon (C) concentration in the austenite becomes insufficient, so that the desired austenite fraction cannot be secured. Therefore, in the present invention, the upper limit of the manganese (Mn) content may be limited to 5.0%. A preferred upper limit of the manganese (Mn) content may be 4.7%, and a more preferred upper limit of the manganese (Mn) content may be 4.5%.

[0034] Phosphorus (P): 0.15% or less (including 0%) Phosphorus (P) is an element that is contained as an impurity and reduces impact toughness, so the phosphorus (P) content is preferably controlled to 0.15% or less.

[0035] Sulfur (S): 0.03% or less (including 0%) Sulfur (S) is an element that is contained as an impurity and forms MnS in the steel sheet, thereby reducing ductility, and therefore the sulfur (S) content is preferably 0.03% or less.

[0036] Nitrogen (N): 0.03% or less (including 0%) Nitrogen (N) is an element that, when contained as an impurity, forms nitrides during continuous casting and causes cracks in the slab. Therefore, the nitrogen (N) content is preferably 0.03% or less.

[0037] Meanwhile, the steel sheet of the present invention may contain additional alloy components in addition to the above-mentioned alloy components, which will be described in detail below.

[0038] Titanium (Ti): 0-0.5%, Niobium (Nb): 0-0.5%, and Vanadium (V): 0-0.5% Titanium (Ti), niobium (Nb) and vanadium (V) are elements that form precipitates to refine crystal grains and also contribute to improving the strength and impact toughness of steel sheets, so the present invention may add at least one of titanium (Ti), niobium (Nb) and vanadium (V) for this effect. However, if the content of titanium (Ti), niobium (Nb) and vanadium (V) exceeds a certain level, excessive precipitates are formed, which not only reduces impact toughness but also causes an increase in manufacturing costs, so the present invention may limit the content of titanium (Ti), niobium (Nb) and vanadium (V) to 0.5% or less, respectively.

[0039] Chromium (Cr): 0-3.0% and Molybdenum (Mo): 0-3.0% Chromium (Cr) and molybdenum (Mo) are elements that not only suppress austenite decomposition during alloying treatment, but also stabilize austenite like manganese (Mn), so the present invention can add at least one of chromium (Cr) and molybdenum (Mo) for this effect. However, if the content of chromium (Cr) and molybdenum (Mo) exceeds a certain level, the bainite transformation time increases and the amount of carbon (C) enriched in the austenite becomes insufficient, so that the desired fraction of retained austenite cannot be secured. Therefore, the present invention can limit the content of chromium (Cr) and molybdenum (Mo) to 3.0% or less, respectively.

[0040] Copper (Cu): 0-4.5% and Nickel (Ni): 0-4.5% or more Copper (Cu) and nickel (Ni) are elements that stabilize austenite and inhibit corrosion. Copper (Cu) and nickel (Ni) are also elements that concentrate on the surface of the steel sheet, prevent hydrogen from moving into the steel sheet, and inhibit delayed hydrogen fracture. Therefore, in the present invention, one or more of copper (Cu) and nickel (Ni) can be added to achieve this effect. However, if the content of copper (Cu) and nickel (Ni) exceeds a certain level, it not only causes excessive property effects but also increases manufacturing costs, so in the present invention, the content of copper (Cu) and nickel (Ni) can be limited to 4.5% or less, respectively.

[0041] Boron (B): 0 to 0.005% Boron (B) is an element that improves hardenability and strength, and also suppresses nucleation of grain boundaries. Therefore, in the present invention, boron (B) can be added for these effects. However, if the content of boron (B) exceeds a certain level, it not only has an excessive effect on properties, but also causes an increase in manufacturing costs, so the content of boron (B) can be limited to 0.005% or less in the present invention.

[0042] One or more of the following: calcium (Ca): 0-0.05%, magnesium (Mg): 0-0.05%, and rare earth elements (REM) excluding yttrium (Y): 0-0.05% Here, rare earth elements (REM) refer to scandium (Sc), yttrium (Y) and lanthanum group elements. Rare earth elements (REM) other than calcium (Ca), magnesium (Mg) and yttrium (Y) are elements that contribute to improving the ductility of steel sheets by spheroidizing sulfides, and the present invention may add one or more of rare earth elements (REM) other than calcium (Ca), magnesium (Mg) and yttrium (Y) for this effect. However, if the content of rare earth elements (REM) other than calcium (Ca), magnesium (Mg) and yttrium (Y) exceeds a certain level, it not only causes excessive property effects but also increases manufacturing costs, so the present invention may limit the content of rare earth elements (REM) other than calcium (Ca), magnesium (Mg) and yttrium (Y) to 0.05% or less.

[0043] Tungsten (W): 0-0.5% and zirconium (Zr): 0-0.5% or more Tungsten (W) and zirconium (Zr) are elements that improve hardenability and increase the strength of steel sheet, so the present invention may add at least one of tungsten (W) and zirconium (Zr) for this effect. However, if the content of tungsten (W) and zirconium (Zr) exceeds a certain level, it may cause excessive property effects as well as an increase in manufacturing costs, so the present invention may limit the content of tungsten (W) and zirconium (Zr) to 0.5% or less, respectively.

[0044] Antimony (Sb): 0-0.5% and Tin (Sn): 0-0.5% Antimony (Sb) and tin (Sn) are elements that improve the plating wettability and plating adhesion of steel sheets, so in the present invention, one or more of antimony (Sb) and tin (Sn) can be added to achieve this effect. However, if the content of antimony (Sb) and tin (Sn) exceeds a certain level, the brittleness of the steel sheet increases and cracks may occur during hot working or cold working, so in the present invention, the content of antimony (Sb) and tin (Sn) can be limited to 0.5% or less, respectively.

[0045] At least one of yttrium (Y): 0-0.2% and hafnium (Hf): 0-0.2% Yttrium (Y) and hafnium (Hf) are elements that improve the corrosion resistance of steel sheets, so in the present invention, one or more of yttrium (Y) and hafnium (Hf) can be added to achieve this effect. However, if the content of yttrium (Y) and hafnium (Hf) exceeds a certain level, the ductility of the steel sheet may deteriorate, so in the present invention, the content of yttrium (Y) and hafnium (Hf) can be limited to 0.2% or less, respectively.

[0046] Cobalt (Co): 0~1.5% Cobalt (Co) is an element that promotes bainite transformation and increases the TRIP effect, so in the present invention, cobalt (Co) can be added for this effect. However, if the cobalt (Co) content exceeds a certain level, the weldability and ductility of the steel sheet may decrease, so in the present invention, the cobalt (Co) content can be limited to 1.5% or less.

[0047] The high strength steel sheet with excellent workability according to one aspect of the present invention may contain the remaining Fe and other inevitable impurities in addition to the above-mentioned components. However, since unintended impurities may be inevitably mixed in from raw materials or the surrounding environment during normal manufacturing processes, it is not possible to completely exclude them. Since these impurities are known to anyone having ordinary skill in the art, the entire contents of the impurities will not be specifically mentioned in this specification. Furthermore, the addition of additional effective components in addition to the above-mentioned components is not completely excluded.

[0048] The high-strength steel sheet having excellent workability according to one aspect of the present invention may contain tempered martensite, bainite, retained austenite, and ferrite as a microstructure. As a preferred example, the high-strength steel sheet having excellent workability according to one aspect of the present invention may contain, by volume fraction, 30 to 70% tempered martensite, 10 to 45% bainite, 10 to 40% retained austenite, 3 to 20% ferrite, and unavoidable structures. The unavoidable structures of the present invention may include fresh martensite, pearlite, island martensite (Martensite Austenite Constituent, MA), and the like. If fresh martensite or pearlite is formed excessively, the workability of the steel sheet may decrease or the fraction of retained austenite may be reduced.

[0049] The high strength steel sheet having excellent formability according to one aspect of the present invention has an average total content of silicon (Si) and aluminum (Al) contained in retained austenite ([Si+Al]) as shown in the following [Relation 1]. γ The average total content of silicon (Si) and aluminum (Al) in ferrite ([Si+Al] F %, by weight, can be in the range of 1.1 to 3.0. [Equation 1] 1.1≦[Si+Al] F / [Si+Al] γ <=3.0

[0050] In addition, the high strength steel sheet having excellent formability according to one aspect of the present invention has a balance between tensile strength and elongation (B T·E ) is 22,000 (MPa%) or more, and the balance between tensile strength and hole expansion ratio (B T·H ) is 7 x 10 6 (MPa 2 % 1 / 2 ) or more, and the bending rate (B R ) satisfies the range of 0.5 to 3.0, it is possible to have not only an excellent balance between strength and ductility and a good balance between strength and hole expandability, but also excellent bending workability. [Equation 2] B T·E = [tensile strength (TS, MPa)] × [elongation rate (El, %)] [Equation 3] B T·H =[Tensile strength (TS, MPa)] 2 × [Hole expansion rate (HER,%)] 1 / 2 [Equation 4] B R =R / t In the above Relational Formula 4, R means the minimum bending radius (mm) at which no cracks occur after a 90° bending test, and t means the thickness (mm) of the steel plate.

[0051] In the present invention, it is important to stabilize the retained austenite of the steel sheet in order to simultaneously secure not only high strength properties but also excellent ductility and bending workability. In order to stabilize the retained austenite, it is necessary to concentrate carbon (C) and manganese (Mn) in the ferrite, bainite and tempered martensite of the steel sheet in the austenite. However, if carbon (C) is concentrated in the austenite using ferrite, the strength of the steel sheet may be insufficient due to the low strength properties of ferrite, and excessive interphase hardness difference may occur, resulting in a decrease in the hole expansion ratio (HER). Therefore, the present invention concentrates carbon (C) and manganese (Mn) in the austenite using bainite and tempered martensite.

[0052] When the content of silicon (Si) and aluminum (Al) in the retained austenite is limited to a certain range, carbon (C) and manganese (Mn) can be concentrated in large amounts from bainite and tempered martensite into the retained austenite, and the retained austenite can be effectively stabilized. In addition, the content of silicon (Si) and aluminum (Al) in the austenite can be increased by limiting the content of silicon (Si) and aluminum (Al) in the austenite to a certain range. As the content of silicon (Si) and aluminum (Al) in the ferrite increases, the hardness of the ferrite increases, and the interphase hardness difference between the soft structure of ferrite and the hard structures of tempered martensite, bainite, and retained austenite can be effectively reduced.

[0053] Therefore, the present invention relates to a method for manufacturing a steel having a low average total content of silicon (Si) and aluminum (Al) contained in the retained austenite ([Si+Al] γ The average total content of silicon (Si) and aluminum (Al) in ferrite ([Si+Al] F In order to limit the ratio of silicon (Si) and aluminum (Al) in the ferrite to 1.1 or more, the interphase hardness difference between the soft structure and the hard structure can be effectively reduced. On the other hand, if the content of silicon (Si) and aluminum (Al) in the ferrite is excessive, the ferrite becomes excessively hard and the workability decreases, so the balance between the desired tensile strength and elongation rate (TS×El) and the balance between the tensile strength and the hole expansion rate (TS 2 ×HER 1 / 2 ) and bending rate (R / t) cannot be ensured. Therefore, in the present invention, the average total content ([Si+Al] γ The average total content of silicon (Si) and aluminum (Al) in ferrite ([Si+Al] F %, by weight, can be limited to not more than 3.0.

[0054] A steel sheet containing retained austenite has excellent ductility and bending workability due to transformation organic sintering that occurs when austenite transforms into martensite during processing. If the fraction of retained austenite is less than a certain level, the balance between tensile strength and elongation (TS×El) may be less than 22,000 MPa% or the bending workability (R / t) may exceed 3.0. On the other hand, if the fraction of retained austenite exceeds a certain level, local elongation may decrease. Therefore, in the present invention, in order to obtain a steel sheet having an excellent balance between tensile strength and elongation (TS×El) as well as an excellent bending workability (R / t), the fraction of retained austenite may be limited to a range of 10 to 40 volume %.

[0055] On the other hand, both untempered martensite (fresh martensite) and tempered martensite are microstructures that improve the strength of steel sheets. However, compared with tempered martensite, fresh martensite has the property of significantly reducing the ductility and hole expandability of steel sheets. This is because the microstructure of tempered martensite is softened by tempering heat treatment. Therefore, in the present invention, it is preferable to utilize tempered martensite in order to provide a steel sheet that is excellent in balance between strength and ductility, balance between strength and hole expandability, and bending workability. When the fraction of tempered martensite is less than a certain level, the balance between tensile strength and elongation (TS×El) of 22,000 MPa% or more or the balance between tensile strength and elongation (TS×El) of 7×10 6 (MPa 2 % 1 / 2 ) or higher balance of tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 ), and if the fraction of tempered martensite exceeds a certain level, ductility and workability decrease, and the balance between tensile strength and elongation (TS×El) is less than 22,000 MPa% or the bending work ratio (R / t) exceeds 3.0, which is undesirable. Therefore, the present invention provides a balance between tensile strength and elongation (TS×El) and a balance between tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2In order to obtain a steel sheet excellent in hardness (H) and bending workability (R / t), the fraction of tempered martensite can be limited to the range of 30 to 70 volume %.

[0056] Balance between tensile strength and elongation rate (TS×El), balance between tensile strength and hole expansion rate (TS 2 ×HER 1 / 2 In order to improve the bending workability (R / t) and bending rate (R / t), it is preferable that bainite is appropriately contained as a microstructure. Only when the bainite fraction is at a certain level or higher, the balance between tensile strength and elongation rate (TS×El) of 22,000 MPa% or more and 7×10 6 (MPa 2 % 1 / 2 ) or higher balance of tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 ) and a bending ratio (R / t) of 0.5 to 3.0 can be ensured. On the other hand, if the fraction of bainite is excessive, the fraction of tempered martensite inevitably decreases, and as a result, the balance between tensile strength and elongation (TS×El) and the balance between tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 ), and the bending ratio (R / t) cannot be ensured. Therefore, in the present invention, the fraction of bainite can be limited to the range of 10 to 45 volume %.

[0057] Since ferrite is an element that contributes to improving ductility, the balance between tensile strength and elongation (TS×El) targeted by the present invention can be ensured only when the ferrite fraction is at a certain level or higher. However, if the ferrite fraction is excessive, the interphase hardness difference increases and the hole expansion ratio (HER) may decrease, so the balance between tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 ) cannot be ensured. Therefore, in the present invention, the ferrite fraction can be limited to the range of 3 to 20 volume %.

[0058] An example of a method for producing the steel sheet of the present invention will now be described in detail.

[0059] A method for producing a high strength steel sheet according to one aspect of the present invention includes the steps of preparing a steel slab having a predetermined composition, heating the steel slab, and hot rolling the steel slab; coiling the hot rolled steel sheet; heat treating the coiled steel sheet by hot rolling annealing at a temperature range of 650 to 850°C for 600 to 1700 seconds; cold rolling the steel sheet heat treated by hot rolling annealing; heating the cold rolled steel sheet to a temperature range of Ac1 to Ac3 at an average heating rate of 5°C / s or more (primary heating) and maintaining the temperature for 50 seconds or more (primary maintenance); cooling to a temperature range of 100 to 300°C at an average cooling rate of 1°C / s or more (primary cooling); heating the primarily cooled steel sheet to a temperature range of 300 to 500°C (secondary heating) and maintaining the temperature for 50 seconds or more (secondary maintenance); and cooling to room temperature (secondary cooling).

[0060] Preparation and heating of steel slabs A steel slab having a predetermined composition is prepared. Since the steel slab of the present invention has an alloy composition corresponding to the alloy composition of the steel plate described above, the description of the alloy composition of the steel slab replaces the description of the alloy composition of the steel plate described above.

[0061] The prepared steel slab can be heated to a certain temperature range, and the heating temperature of the steel slab may be in the range of 1000 to 1350° C. If the heating temperature of the steel slab is less than 1000° C., there is a risk that the steel slab will be hot rolled in a temperature range below the temperature range of the intended finish hot rolling, and if the heating temperature of the steel slab exceeds 1350° C., there is a risk that the steel will reach its melting point and melt.

[0062] Hot rolling and coiling The heated steel slab may be hot-rolled to provide a hot-rolled steel sheet. The finish hot-rolling temperature during hot-rolling is preferably in the range of 800 to 1000° C. If the finish hot-rolling temperature is less than 800° C., excessive rolling load may become a problem, and if the finish hot-rolling temperature exceeds 1000° C., the crystal grains of the hot-rolled steel sheet may be formed coarsely, which may cause a decrease in the physical properties of the final steel sheet.

[0063] The hot-rolled steel sheet after the hot rolling may be cooled at an average cooling rate of 10° C. / s or more, and may be coiled at a temperature of 300 to 600° C. If the coiling temperature is less than 300° C., coiling is not easy, and if the coiling temperature exceeds 600° C., surface scale may be formed inside the hot-rolled steel sheet, making pickling difficult.

[0064] Heat treatment by hot rolling and annealing In order to facilitate pickling and cold rolling, which are subsequent processes after coiling, it is preferable to perform a heat treatment process by hot rolling annealing. The heat treatment by hot rolling annealing can be performed for 600 to 1700 seconds at a temperature range of 650 to 850°C. If the heat treatment temperature by hot rolling annealing is less than 650°C or the heat treatment time by hot rolling annealing is less than 600 seconds, the strength of the steel sheet heat-treated by hot rolling annealing is high, and the subsequent cold rolling may not be easy. On the other hand, if the heat treatment temperature by hot rolling annealing exceeds 850°C or the heat treatment time by hot rolling annealing exceeds 1700 seconds, pickling may not be easy due to scale formed deep inside the steel sheet.

[0065] Pickling and cold rolling After the heat treatment by hot rolling annealing, the steel sheet may be pickled to remove scale formed on the surface thereof, and then cold rolled. In the present invention, the conditions for pickling and cold rolling are not particularly limited, but the cold rolling is preferably performed at a cumulative reduction of 30 to 90%. If the cumulative reduction of cold rolling exceeds 90%, it may be difficult to perform cold rolling in a short time due to the high strength of the steel sheet.

[0066] The cold-rolled steel sheet may be produced as an uncoated cold-rolled steel sheet through an annealing heat treatment process, or may be produced as a coated steel sheet through a coating process to impart corrosion resistance. Coating may be performed by a coating method such as hot-dip galvanizing, electrolytic galvanizing, or hot-dip aluminum coating, and the method and type are not particularly limited.

[0067] Annealing heat treatment In the present invention, an annealing heat treatment step is carried out in order to simultaneously ensure the strength and workability of the steel sheet.

[0068] Cold-rolled steel sheets are heated (primary heating) in the temperature range of Ac1 or more but less than Ac3 (two-phase region) and maintained at that temperature range for 50 seconds or more (primary maintenance). If the primary heating or primary maintenance temperature is Ac3 or more (single-phase region), the desired ferrite structure cannot be achieved, so the desired level of [Si+Al] F / [Si+Al] γ And the balance between tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 ) cannot be realized. In addition, if the primary heating or primary maintenance temperature is in a temperature range below Ac1, sufficient heating may not be performed, and the microstructure targeted by the present invention may not be realized even by the subsequent heat treatment. The average heating rate of the primary heating may be 5°C / s or more.

[0069] If the first holding time is less than 50 seconds, the structure cannot be sufficiently homogenized, and the physical properties of the steel sheet may deteriorate. Although there is no particular upper limit to the first holding time, it is preferable to limit the first heating time to 1200 seconds or less in order to prevent a decrease in toughness due to grain coarsening.

[0070] After the first maintenance, the steel sheet can be cooled to a first cooling stop temperature of 100 to 300°C (first cooling) at an average cooling rate of 1°C / s or more. There is no particular need to specify an upper limit for the first cooling rate, but it is preferably set to 100°C or less. If the first cooling stop temperature is less than 100°C, tempered martensite is formed excessively and the amount of retained austenite formed is insufficient, resulting in a decrease in the [Si+Al] of the steel sheet. F / [Si+Al] γ On the other hand, if the primary cooling stop temperature exceeds 300°C, bainite is excessively formed and the amount of tempered martensite formed is insufficient, so that the balance between tensile strength and elongation rate (TS×El) and the balance between tensile strength and hole expansion rate (TS 2 ×HER 1 / 2) may be reduced.

[0071] After the above primary cooling, the steel sheet is heated to a secondary heating temperature of 300 to 500°C at an average heating rate of 5°C / s or more (secondary heating), and the steel sheet is maintained at the temperature range for 50 seconds or more (secondary maintenance). The upper limit of the secondary heating rate does not need to be specified, but it is preferably set to 100°C or less. If the secondary heating or secondary maintenance temperature is less than 300°C or the maintenance time is less than 50 seconds, tempered martensite is excessively formed, and the content of silicon (Si) and aluminum (Al) in the steel is insufficiently controlled, making it difficult to ensure the desired fraction of retained austenite. As a result, the [Si+Al] of the steel sheet is F / [Si+Al] γ However, the balance between tensile strength and elongation (TS×El) and bending workability (R / t) may decrease. On the other hand, if the secondary heating or holding temperature exceeds 500°C or the secondary holding time is 144,000 seconds or longer, the silicon (Si) and aluminum (Al) contents in the steel are not sufficiently controlled, making it difficult to ensure the fraction of retained austenite. As a result, the [Si+Al] of the steel sheet F / [Si+Al] γ And the balance between tensile strength and elongation (TS×El) may decrease.

[0072] After the secondary hold, it can be cooled to room temperature (secondary cooling) at an average cooling rate of 1°C / s or more.

[0073] The high-strength steel plate with excellent workability produced by the above-mentioned production method may contain, as a microstructure, tempered martensite, bainite, retained austenite, and ferrite, and as a preferred example, may contain, by volume fraction, 30 to 70% tempered martensite, 10 to 45% bainite, 10 to 40% retained austenite, 3 to 20% ferrite, and unavoidable structures.

[0074] In addition, the high-strength steel plate with excellent formability manufactured by the above-mentioned manufacturing method has an average total content of silicon (Si) and aluminum (Al) contained in retained austenite ([Si+Al]) as shown in the following [Relationship 1]. γ The average total content of silicon (Si) and aluminum (Al) in ferrite ([Si+Al] F The ratio of (wt%) can be in the range of 1.1 to 3.0, and the balance between tensile strength and elongation (B T·E ) is 22,000 (MPa%) or more, and the balance between tensile strength and hole expansion ratio (B T·H ) is 7 x 10 6 (MPa 2 % 1 / 2 ) or more, and the bending rate (B R ) can be in the range of 0.5 to 3.0. [Equation 1] 1.1≦[Si+Al] F / [Si+Al] γ <=3.0 [Equation 2] B T·E = [tensile strength (TS, MPa)] × [elongation rate (EL, %)] [Equation 3] B T·H =[Tensile strength (TS, MPa)] 2 × [Hole expansion rate (HER,%)] 1 / 2 [Equation 4] B R =R / t In the above Relational Formula 4, R means the minimum bending radius (mm) at which no cracks occur after a 90° bending test, and t means the thickness (mm) of the steel plate. EXAMPLES

[0075] Hereinafter, a high strength steel sheet having excellent workability and a manufacturing method thereof according to one aspect of the present invention will be described in more detail with reference to specific examples. It should be noted that the following examples are provided to aid in understanding the present invention and are not intended to limit the scope of the present invention. This is because the scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom.

[0076] (Example) A steel slab having a thickness of 100 mm and having the alloy composition shown in Table 1 below (the remainder being Fe and unavoidable impurities) was manufactured, heated to 1200°C, and then finish hot-rolled at 900°C. It was then cooled at an average cooling rate of 30°C / s and coiled at the coiling temperatures shown in Tables 2 and 3 to manufacture a hot-rolled steel sheet having a thickness of 3 mm. The hot-rolled steel sheet was heat-treated by hot-rolling annealing under the conditions shown in Tables 2 and 3. Thereafter, it was pickled to remove surface scale, and then cold-rolled to a thickness of 1.5 mm.

[0077] Thereafter, heat treatment was carried out under the annealing heat treatment conditions shown in Tables 2 to 5 to produce steel sheets.

[0078] The microstructure of the steel sheets manufactured in this manner was observed, and the results are shown in Tables 6 and 7. Among the microstructures, ferrite (F), bainite (B), tempered martensite (TM), and pearlite (P) were observed through SEM after nital etching of the polished cross section of the test specimen. Among these, the fractions of bainite and tempered martensite, which are difficult to distinguish, were calculated using dilatation curves after dilatation evaluation. Meanwhile, since it is also difficult to distinguish between fresh martensite (FM) and retained austenite (residual γ), the fraction of retained austenite calculated by X-ray diffraction method was subtracted from the fractions of martensite and retained austenite observed by SEM as described above to determine the fraction of fresh martensite.

[0079] On the other hand, the [Si+Al] of steel plate F / [Si+Al] γ , balance between tensile strength and elongation rate (TS×El), balance between tensile strength and hole expansion rate (TS2 ×HER 1 / 2 ) and bending rate (R / t) were observed, and the results are shown in Tables 8 and 9.

[0080] The average total content of silicon (Si) and aluminum (Al) contained in retained austenite ([Si+Al] γ , wt%) and the average total content of silicon (Si) and aluminum (Al) in ferrite ([Si+Al] F %, wt %, were measured using an EPMA (Electron Probe MicroAnalyser).

[0081] The tensile strength (TS) and elongation rate (El) were evaluated by a tensile test, and the tensile strength (TS) and elongation rate (El) were measured by evaluating the test pieces taken based on the 90° direction to the rolling direction of the rolled plate material according to the JIS No. 5 standard. The bending rate (R / t) was evaluated by a V-bending test, and the test pieces were taken based on the 90° direction to the rolling direction of the rolled plate material, and the minimum bending radius R at which no cracks occurred after the 90° bending test was determined and calculated by dividing it by the thickness t of the plate material. The hole expansion rate (HER) was evaluated by a hole expansion test, and after forming a punching hole of 10 mmφ (die inner diameter 10.3 mm, clearance 12.5%), a conical punch with an apex angle of 60° was inserted into the punching hole in the direction in which the burr of the punching hole was on the outside, and the periphery of the punching hole was compressed and expanded at a moving speed of 20 mm / min, and then the calculation was performed using the following [Relationship 5]. [Equation 5] Hole expansion ratio (HER,%) = {(DD 0 ) / D 0}×100 In the above formula 5, D means the hole diameter (mm) when the crack penetrates the steel plate along the thickness direction, and D 0 means the initial pore diameter (mm).

[0082] [Table 1] JPEG0007554827000002.jpg99170

[0083] [Table 2]

[0084] [Table 3]

[0085] [Table 4]

[0086] [Table 5]

[0087] [Table 6]

[0088] [Table 7]

[0089] [Table 8]

[0090] [Table 9]

[0091] As shown in Tables 1 to 9 above, in the case of test pieces that satisfy the conditions presented in this invention, [Si+Al] F / [Si+Al] γ The value of 1.1 to 3.0 is satisfied, the balance between tensile strength and elongation rate (TS × El) is 22,000 MPa% or more, and the balance between tensile strength and hole expansion rate (TS 2 ×HER 1 / 2 ) is 7 x 10 6 (MPa 2 %1 / 2 ) or more, and it can be seen that by satisfying the bending ratio (R / t) range of 0.5 to 3.0, excellent strength and workability are simultaneously provided.

[0092] Although the alloy composition ranges of test pieces 2 to 5 overlap with those of the present invention, it can be confirmed that poor pickling occurred or fracture occurred during cold rolling because the hot rolling annealing temperature and time were outside the ranges of the present invention.

[0093] In the case of test piece 6, the amount of ferrite formation was insufficient because the primary heating or maintenance temperature during the annealing heat treatment after cold rolling exceeded the range limited by the present invention. As a result, test piece 6 had a low [Si+Al] F / [Si+Al] γ The value of tensile strength is less than 1.1, and the balance between tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 ) is 7 x 10 6 (MPa 2 % 1 / 2 ) or less.

[0094] In the test piece 7, the primary cooling rate in the annealing heat treatment process after cold rolling was not within the range limited by the present invention, so that ferrite was formed excessively and retained austenite was formed in small amounts. As a result, the test piece 7 had a [Si+Al] F / [Si+Al] γ It can be confirmed that the value exceeds 3.0 and the balance between tensile strength and elongation (TS × El) is less than 22,000 MPa%.

[0095] In the test piece 12, the first cooling stop temperature was low, so that tempered martensite was formed excessively and retained austenite was formed in small amounts. As a result, the test piece 12 had a low [Si+Al] F / [Si+Al] γ It can be confirmed that the value exceeds 3.0, the balance between tensile strength and elongation (TS × El) is less than 22,000 MPa%, and the bending work ratio (R / t) exceeds 3.0.

[0096] In the case of test piece 13, the first cooling stop temperature was high, so that bainite was excessively formed and tempered martensite was not formed much. As a result, the balance between tensile strength and elongation rate (TS × El) of test piece 13 was less than 22,000 MPa%, and the balance between tensile strength and hole expansion rate (TS 2 ×HER 1 / 2 ) is 7 x 10 6 (MPa 2 % 1 / 2 ) or less.

[0097] In the test piece 14, the secondary heating or holding temperature was low, so that tempered martensite was formed excessively and retained austenite was formed in small amounts. As a result, the test piece 14 had a [Si+Al] F / [Si+Al] γ It can be confirmed that the value exceeds 3.0, the balance between tensile strength and elongation (TS × El) is less than 22,000 MPa%, and the bending work ratio (R / t) exceeds 3.0.

[0098] In test piece 15, the secondary heating or maintenance temperature was high, so the amount of retained austenite formed was insufficient, and [Si+Al] F / [Si+Al] γ It can be confirmed that the value exceeds 3.0 and the balance between tensile strength and elongation (TS × El) is less than 22,000 MPa%.

[0099] In the case of the test piece 16, the second holding time was insufficient, so that the tempered martensite was formed excessively and the retained austenite was formed insufficiently. As a result, the test piece 16 had a [Si+Al] F / [Si+Al] γ It can be confirmed that the value exceeds 3.0, the balance between tensile strength and elongation (TS × El) is less than 22,000 MPa%, and the bending work ratio (R / t) exceeds 3.0.

[0100] In the test piece 17, the secondary holding time was too long, and the amount of retained austenite formed was insufficient. F / [Si+Al] γIt can be confirmed that the value exceeds 3.0 and the balance between tensile strength and elongation (TS × El) is less than 22,000 MPa%.

[0101] Test pieces 40 to 48 satisfy the manufacturing conditions proposed in the present invention, but are outside the range of the alloy composition. F / [Si+Al] γ , balance between tensile strength and elongation rate (TS×El), balance between tensile strength and hole expansion rate (TS 2 ×HER 1 / 2 ) is 7 x 10 6 (MPa 2 % 1 / 2 On the other hand, the test piece 42 is a case where the total content of aluminum (Al) and silicon (Si) is less than 1.0%, and the condition of [Si+Al] F / [Si+Al] γ It can be seen that the conditions for the balance between tensile strength and elongation rate (TS×El) and the bending rate (R / t) are not satisfied.

[0102] Although the present invention has been described in detail with reference to the embodiments, other embodiments are possible and the scope of the claims set forth below should not be construed as being limited to the embodiments.

Claims

1. In weight percent, C: 0.25 to 0.75%, Si: 4.0% or less, Mn: 0.9 to 5.0%, Al: 5.0% or less, P: 0.15% or less, S: 0.03% or less, N: 0.03% or less, the balance being Fe and unavoidable impurities; The total content of Si and Al (Si+Al) is 1.0 to 6.0 wt.%; The microstructure includes 30 to 70 volume % tempered martensite, 10 to 45 volume % bainite, 10 to 40 volume % retained austenite, 3 to 20 volume % ferrite, and unavoidable structures; A steel plate satisfying the following [Relationship 1]. [Relationship 1] 1.1≦[Si+Al] F / [Si+Al] γ ≦3.0 In the above-mentioned relational formula 1, [Si + Al] F is the average total content (wt%) of Si and Al contained in ferrite, [Si + Al] γ is the average total content (wt%) of Si and Al contained in the retained austenite.

2. The steel plate according to claim 1, further comprising any one or more of the following (1) to (9): (1) One or more of Ti: 0-0.5%, Nb: 0-0.5%, and V: 0-0.5% (2) One or more of Cr: 0-3.0% and Mo: 0-3.0% (3) One or more of Cu: 0-4.5% and Ni: 0-4.5% (4) B: 0-0.005% (5) One or more of Ca: 0-0.05%, REM excluding Y: 0-0.05%, and Mg: 0-0.05%. (6) One or more of W: 0-0.5% and Zr: 0-0.5% (7) One or more of Sb: 0-0.5% and Sn: 0-0.5% (8) One or more of Y: 0-0.2% and Hf: 0-0.2% (9) Co: 0-1.5%

3. The steel sheet has a balance between tensile strength and elongation (B T・E ) is 22,000 (MPa%) or more, and the balance between the tensile strength and the hole expansion ratio (B T・H ) is 7 x 10 6 (MPa 2 % 1/2 ) or more, and the bending rate (B R 2. The steel sheet according to claim 1, wherein the σ is 0.5 to 3.

0. [Relationship 2] B T・E = [tensile strength (TS, MPa)] × [elongation rate (El, %)] [Relationship 3] B T・H = [tensile strength (TS, MPa)] 2 × [Hole expansion rate (HER,%)] 1/2 [Relationship 4] B R =R / t In the above Relational Formula 4, R means the minimum bending radius (mm) at which no cracks occur after a 90° bending test, and t means the thickness (mm) of the steel plate.

4. heating and hot rolling a steel slab having, by weight percent, C: 0.25-0.75%, Si: 4.0% or less, Mn: 0.9-5.0%, Al: 5.0% or less, P: 0.15% or less, S: 0.03% or less, N: 0.03% or less, and the remainder being Fe and unavoidable impurities, and the total content of Si and Al (Si+Al) being 1.0-6.0% by weight; coiling the hot rolled steel sheet; heat treating the coiled steel sheet by hot rolling annealing at a temperature range of 650 to 850° C. for 600 to 1700 seconds; cold rolling the steel sheet heat-treated by the hot rolling annealing; heating the cold-rolled steel sheet to a temperature range of Ac1 or more and less than Ac3 (primary heating) and maintaining the temperature for 50 seconds or more (primary maintenance); a step of cooling (primary cooling) to a temperature range of 100 to 300° C. at an average cooling rate of 1.0° C. / s or more; heating the primarily cooled steel sheet to a temperature range of 300 to 500° C. (secondary heating) and maintaining the temperature for 50 to 144,000 seconds (secondary maintenance); and The method for producing a steel sheet according to any one of claims 1 to 3, further comprising: a step of cooling to room temperature (secondary cooling).

5. The method for producing a steel plate according to claim 4, wherein the steel slab further comprises any one or more of the following (1) to (9): (1) One or more of Ti: 0-0.5%, Nb: 0-0.5%, and V: 0-0.5% (2) One or more of Cr: 0-3.0% and Mo: 0-3.0% (3) One or more of Cu: 0-4.5% and Ni: 0-4.5% (4) B: 0-0.005% (5) One or more of Ca: 0-0.05%, REM excluding Y: 0-0.05%, and Mg: 0-0.05%. (6) One or more of W: 0-0.5% and Zr: 0-0.5% (7) One or more of Sb: 0-0.5% and Sn: 0-0.5% (8) One or more of Y: 0-0.2% and Hf: 0-0.2% (9) Co: 0-1.5%

6. The method for producing a steel plate according to claim 4, wherein the steel slab is heated in a temperature range of 1000 to 1350°C and finish hot rolled in a temperature range of 800 to 1000°C.

7. The method for producing a steel sheet according to claim 4, wherein the hot-rolled steel sheet is coiled at a temperature in the range of 300 to 600°C.

8. The method for producing a steel sheet according to claim 4, wherein the cold rolling reduction is 30 to 90%.

9. The method for producing a steel sheet according to claim 4, wherein the cooling rate of the secondary cooling is 1° C. / s or more.

Citation Information

Patent Citations

  • Hot dip galvannealed high strength steel sheet having tensile strength of &gt;=700 mpa and excellent corrosion resistance, hole expansibility and ductility, and method for producing the same

    JP2009019258A

  • High-strength steel sheet and high-strength hot-dip galvanized steel sheet having excellent workability, and method for producing them

    JP2010275627A

  • High strength thin steel sheet having excellent elongation and press forming stability

    JP2012041573A

  • High-strength hot-dip galvanized steel plate with excellent moldability in ordinary and intermediate temperature range, and method for manufacturing the same

    JP2013234340A

  • High strength steel sheet excellent in ductility and low temperature toughness and manufacturing method therefor

    JP2015200006A