A high-strength steel plate with optimized composition and microstructure addresses the balance between strength and workability by incorporating specific elements and phases, achieving enhanced ductility, bending workability, and hole expandability for automotive applications.
Patent Information
- Application Number
- JP2022536968
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-18
- Filing Date
- 2020-11-24
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-11-24
AI Technical Summary
Existing high-strength steel sheets for automobile parts face challenges in achieving a balance between high strength and excellent workability, particularly in terms of ductility, bending workability, and hole expandability, as previous technologies struggle to optimize the composition and microstructure for this balance.
A high-strength steel plate with a specific composition and microstructure, including 0.25 to 0.75% C, 0.9 to 5.0% Mn, 0.15% P or less, and a balanced microstructure of 30 to 70% tempered martensite, 10 to 45% bainite, 10 to 40% retained austenite, and 3 to 20% ferrite, along with controlled Si and Al content, is developed to enhance workability.
The steel plate achieves a balance between tensile strength and elongation rate of 22,000 MPa% or more, hole expansion rate of 7×10^6 (MPa^2 %^1/2) or more, and bending rate of 0.5 to 3.0, ensuring excellent strength and workability suitable for automobile parts.
Smart Images

Figure 0007554828000006 
Figure 0007554828000005 
Figure 0007554828000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel sheet that can be used for automobile parts and the like, and relates to a steel sheet that has high strength properties and excellent workability, and a method for producing the same. [Background technology]
[0002] Recently, the automobile industry has been trying to reduce the weight of materials in order to protect the global environment, while at the same time paying attention to ways to ensure the stability of passengers. In order to meet such demands for stability and weight reduction, the application of high-strength steel sheets has rapidly increased. It is generally known that the higher the strength of a steel sheet, the lower the workability of the steel sheet. Therefore, there is a demand for steel sheets for automobile parts that have high strength properties while also having excellent workability, such as ductility, bending workability, and hole expandability.
[0003] Patent Documents 1 and 2 disclose a method of utilizing tempered martensite as a technique for improving the workability of steel sheets. Tempered martensite, which is produced by tempering hard martensite, is softened martensite, and therefore has a difference in strength from existing untempered martensite (fresh martensite). Therefore, by suppressing fresh martensite and forming tempered martensite, the workability can be improved.
[0004] However, the techniques disclosed in Patent Documents 1 and 2 fail to achieve a balance between tensile strength and elongation (TS×El) of 22,000 MPa% or more, which means that it is difficult to obtain a steel sheet with excellent strength and ductility.
[0005] Meanwhile, in order to obtain both high strength and excellent workability in steel sheets for automotive components, TRIP (Transformation Induced Plasticity) steel that utilizes the transformation induced plasticity of retained austenite has been developed. Patent Document 3 discloses TRIP steel with excellent strength and workability.
[0006] In Patent Document 3, polygonal ferrite, retained austenite, and martensite are incorporated to improve ductility and workability. However, because bainite is the main phase, high strength cannot be ensured, and the balance between tensile strength and elongation (TS×El) does not satisfy the requirement of 22,000 MPa% or more.
[0007] That is, the current situation is that the demand for a steel sheet having high strength and excellent workability, such as ductility, bending workability, and hole expandability, is not met. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Korean Patent Publication No. 10-2006-0118602 [Patent Document 2] Japanese Patent Publication No. 2009-019258 [Patent Document 3] Korean Patent Publication No. 10-2014-0012167 Summary of the Invention [Problem to be solved by the invention]
[0009] According to one aspect of the present invention, it is possible to provide a high-strength steel sheet having excellent ductility, bending workability, and hole expandability by optimizing the composition and microstructure of the steel sheet, and a method for producing the same.
[0010] The object of the present invention is not limited to the above. Further objects of the present invention are described in the general contents of the specification, and a person having ordinary knowledge in the technical field to which the present invention pertains will have no difficulty in understanding the further objects of the present invention from the contents described in the specification of the present invention. [Means for solving the problem]
[0011] A high-strength steel plate with excellent workability according to one aspect of the present invention contains, by weight, 0.25 to 0.75% C, 4.0% or less Si, 0.9 to 5.0% Mn, 5.0% or less Al, 0.15% or less P, 0.03% or less S, 0.03% or less N, with the remainder being Fe and unavoidable impurities, and contains, as a microstructure, 30 to 70% by volume of tempered martensite, 10 to 45% by volume of bainite, 10 to 40% by volume of retained austenite, 3 to 20% by volume of ferrite and unavoidable structures, and can satisfy the following [Relational Formula 1].
[0012] [Equation 1] 1.02≦[Si+Al] F / [Si+Al] av ≦1.45 In the above formula 1, [Si+Al] F is the average total content (wt%) of Si and Al contained in ferrite, [Si+Al] av is the average total content (wt%) of Si and Al contained in the steel sheet.
[0013] The steel sheet may further include one or more of the following (1) to (9). (1) One or more of Ti: 0-0.5%, Nb: 0-0.5%, and V: 0-0.5% (2) At least one of Cr: 0-3.0% and Mo: 0-3.0% (3) One or more of Cu: 0-4.5% and Ni: 0-4.5% (4) B: 0 to 0.005% (5) One or more of Ca: 0-0.05%, REM excluding Y: 0-0.05%, and Mg: 0-0.05%. (6) One or more of W: 0-0.5% and Zr: 0-0.5% (7) One or more of Sb: 0-0.5% and Sn: 0-0.5% (8) One or more of Y: 0-0.2% and Hf: 0-0.2% (9) Co: 0-1.5% The total content of Si and Al (Si+Al) may be 1.0 to 6.0% by weight.
[0014] The above steel sheet has a balance between tensile strength and elongation (B T·E ) is 22,000 (MPa%) or more, and the balance between tensile strength and hole expansion ratio (B T·H ) is 7 x 10 6 (MPa 2 % 1 / 2 ) or more, and the bending rate (B R ) can be in the range of 0.5 to 3.0.
[0015] [Equation 2] B T·E = [Tensile strength (TS, MPa)] × [Elongation (El, %)] [Equation 3] B T·H =[Tensile strength (TS, MPa)] 2 ×[Hole expansion rate (HER,%)] 1 / 2 [Equation 4] B R =R / t In the above Relational Formula 4, R means the minimum bending radius (mm) at which no cracks occur after a 90° bending test, and t means the thickness (mm) of the steel plate.
[0016] According to another aspect of the present invention, there is provided a high strength steel sheet having excellent workability, comprising the steps of heating and hot rolling a steel slab containing, by weight, 0.25-0.75% C, 4.0% or less Si, 0.9-5.0% Mn, 5.0% or less Al, 0.15% or less P, 0.03% or less S, 0.03% or less N, and the remainder being Fe and inevitable impurities; coiling the hot rolled steel sheet; and subjecting the coiled steel sheet to hot rolling annealing heat treatment at a temperature range of 650-850° C. for 600-1700 seconds. the step of heating the cold-rolled steel sheet to a temperature range of Ac1 to Ac3 at an average heating rate of 5°C / s or more (primary heating) and holding the temperature for 50 seconds or more (primary holding), the step of cooling the cold-rolled steel sheet to a temperature range of 100 to 300°C at an average cooling rate of 1°C / s or more (primary cooling), the step of heating the primarily cooled steel sheet to a temperature range of 300 to 500°C (secondary heating) and holding the temperature for 50 seconds or more (secondary holding), and the step of cooling the steel sheet to room temperature (secondary cooling).
[0017] The steel slab may further include one or more of the following (1) to (9). (1) One or more of Ti: 0-0.5%, Nb: 0-0.5%, and V: 0-0.5% (2) At least one of Cr: 0-3.0% and Mo: 0-3.0% (3) One or more of Cu: 0-4.5% and Ni: 0-4.5% (4) B: 0 to 0.005% (5) One or more of Ca: 0-0.05%, REM excluding Y: 0-0.05%, and Mg: 0-0.05%. (6) One or more of W: 0-0.5% and Zr: 0-0.5% (7) One or more of Sb: 0-0.5% and Sn: 0-0.5% (8) One or more of Y: 0-0.2% and Hf: 0-0.2% (9) Co: 0-1.5%
[0018] The total content of Si and Al (Si+Al) contained in the steel slab may be 1.0-6.0 wt%. The steel slab may be heated to a temperature range of 1000-1350°C and finish hot rolled at a temperature range of 800-1000°C. The hot rolled steel sheet may be coiled at a temperature range of 300-600°C. The reduction ratio of the cold rolling may be 30-90%. The cooling rate of the secondary cooling may be 1°C / s or more. Effect of the Invention
[0019] According to a preferred aspect of the present invention, it is possible to provide a steel sheet which is not only excellent in strength but also excellent in workability such as ductility, bending workability, and hole expandability, and is particularly suitable for automobile parts. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention relates to a high-strength steel plate having excellent workability and a manufacturing method thereof, and preferred embodiments of the present invention will be described below. The embodiments of the present invention may be modified in various forms, and the scope of the present invention should not be construed as being limited to the embodiments described below. The embodiments are provided to further explain the present invention in detail to those skilled in the art to which the present invention pertains.
[0021] The inventors of the present invention have recognized that in a transformation induced plasticity (TRIP) steel containing bainite, tempered martensite, retained austenite, and ferrite, when the ratio of a specific component contained in the retained austenite and ferrite is controlled within a certain range while stabilizing the retained austenite, it is possible to ensure both the workability and strength of the steel sheet by reducing the hardness difference between the retained austenite and ferrite phases. By investigating this, the inventors have found a method for improving the ductility and workability of high strength steel, which has led to the present invention. Hereinafter, a high strength steel sheet with excellent workability according to one aspect of the present invention will be described in more detail.
[0022] A high-strength steel plate with excellent workability according to one aspect of the present invention contains, by weight, 0.25 to 0.75% C, 4.0% or less Si, 0.9 to 5.0% Mn, 5.0% or less Al, 0.15% or less P, 0.03% or less S, 0.03% or less N, with the remainder being Fe and unavoidable impurities, and contains, as a microstructure, 30 to 70% by volume of tempered martensite, 10 to 45% by volume of bainite, 10 to 40% by volume of retained austenite, 3 to 20% by volume of ferrite and unavoidable structures, and can satisfy the following [Relational Formula 1].
[0023] [Equation 1] 1.02≦[Si+Al] F / [Si+Al] av ≦1.45 In the above formula 1, [Si+Al] F is the average total content (wt%) of Si and Al contained in ferrite, [Si+Al] av is the average total content (wt%) of Si and Al contained in the steel sheet.
[0024] The steel composition of the present invention will be described in more detail below. In the following, unless otherwise specified, % indicating the content of each element is based on weight.
[0025] A high-strength steel sheet with excellent workability according to one aspect of the present invention contains, by weight percent, C: 0.25 to 0.75%, Si: 4.0% or less, Mn: 0.9 to 5.0%, Al: 5.0% or less, P: 0.15% or less, S: 0.03% or less, N: 0.03% or less, the balance being Fe and inevitable impurities, and additionally Ti: 0.5% or less (including 0%), Nb: 0.5% or less (including 0%), V: 0.5% or less (including 0%), Cr: 3.0% or less (including 0%), Mo: 3.0% or less (including 0%), Cu: 4.5% or less (including 0%), Ni: 4.5% or less (including 0%), B: 0.005% or less (including 0%), Ca: 0.05% or less (including 0%), REM excluding Y: It may further contain one or more of the following: 0.05% or less (including 0%), Mg: 0.05% or less (including 0%), W: 0.5% or less (including 0%), Zr: 0.5% or less (including 0%), Sb: 0.5% or less (including 0%), Sn: 0.5% or less (including 0%), Y: 0.2% or less (including 0%), Hf: 0.2% or less (including 0%), Co: 1.5% or less (including 0%). The total content of Si and Al (Si+Al) may be 1.0 to 6.0%.
[0026] Carbon (C): 0.25~0.75% Carbon (C) is an essential element for ensuring the strength of the steel plate, and also an element for stabilizing the retained austenite that contributes to improving the ductility of the steel plate. Therefore, the present invention can contain 0.25% or more of carbon (C) to achieve such an effect. A preferred carbon (C) content may be more than 0.25%, 0.27% or more, or 0.30% or more. A more preferred carbon (C) content may be 0.31% or more. On the other hand, if the carbon (C) content exceeds a certain level, there is a possibility that the cold rolling becomes difficult due to an excessive increase in strength. Therefore, the present invention can limit the upper limit of the carbon (C) content to 0.75%. The carbon (C) content may be 0.70% or less, and a more preferred carbon (C) content may be 0.67% or less.
[0027] Silicon (Si): 4.0% or less (excluding 0%) Silicon (Si) is an element that contributes to improving strength through solid solution strengthening, and is also an element that improves workability by strengthening ferrite and homogenizing the structure. Silicon (Si) is also an element that inhibits the precipitation of cementite and contributes to the generation of retained austenite. Therefore, in the present invention, silicon (Si) can be added as an essential component to achieve such effects. A preferred silicon (Si) content may be 0.02% or more, and a more preferred silicon (Si) content may be 0.05% or more. However, if the silicon (Si) content exceeds a certain level, it may not only induce problems with plating defects such as non-plating in the plating process, but also reduce the weldability of the steel sheet, so the present invention may limit the upper limit of the silicon (Si) content to 4.0%. A preferred upper limit of the silicon (Si) content may be 3.8%, and a more preferred upper limit of the silicon (Si) content may be 3.5%.
[0028] Aluminum (Al): 5.0% or less (excluding 0%) Aluminum (Al) is an element that combines with oxygen in steel to perform deoxidation. Aluminum (Al) is also an element that inhibits cementite precipitation and stabilizes retained austenite, similar to silicon (Si). Therefore, in the present invention, aluminum (Al) can be added as an essential component to achieve such effects. A preferred aluminum (Al) content may be 0.05% or more, and a more preferred aluminum (Al) content may be 0.1% or more. On the other hand, when aluminum (Al) is added excessively, not only the inclusions in the steel sheet may increase, but also the workability of the steel sheet may be reduced, so that the present invention can limit the upper limit of the aluminum (Al) content to 5.0%. A preferred upper limit of the aluminum (Al) content may be 4.75%, and a more preferred upper limit of the aluminum (Al) content may be 4.5%.
[0029] On the other hand, the total content (Si+Al) of silicon (Si) and aluminum (Al) is preferably 1.0 to 6.0%. In the present invention, silicon (Si) and aluminum (Al) are components that affect the formation of a microstructure and influence ductility, bending workability, and hole expandability, so the total content of silicon (Si) and aluminum (Al) is preferably 1.0 to 6.0%. More preferably, the total content (Si+Al) of silicon (Si) and aluminum (Al) may be 1.5% or more, or 4.0% or less.
[0030] Manganese (Mn): 0.9-5.0% Manganese (Mn) is an element useful for increasing both strength and ductility. Therefore, in order to achieve such an effect, the present invention can limit the lower limit of the manganese (Mn) content to 0.9%. The preferred lower limit of the manganese (Mn) content may be 1.0%, and the more preferred lower limit of the manganese (Mn) content may be 1.1%. On the other hand, when manganese (Mn) is added in excess, the bainite transformation time increases and the concentration of carbon (C) in the austenite becomes insufficient, so that the desired austenite fraction cannot be secured. Therefore, in the present invention, the upper limit of the manganese (Mn) content may be limited to 5.0%. The preferred upper limit of the manganese (Mn) content may be 4.7%, and the more preferred upper limit of the manganese (Mn) content may be 4.5%.
[0031] Phosphorus (P): 0.15% or less (including 0%) Phosphorus (P) is an element that deteriorates impact toughness when contained as an impurity, so the phosphorus (P) content is preferably controlled to 0.15% or less.
[0032] Sulfur (S): 0.03% or less (including 0%) Sulfur (S) is an element that is contained as an impurity and forms MnS in the steel sheet, which deteriorates ductility, and therefore the sulfur (S) content is preferably 0.03% or less.
[0033] Nitrogen (N): 0.03% or less (including 0%) Nitrogen (N) is an element that is contained as an impurity and forms nitrides during continuous casting, which causes cracks in the slab. Therefore, the nitrogen (N) content is preferably 0.03% or less.
[0034] Meanwhile, the steel sheet of the present invention may further contain alloy components other than the alloy components described above, which will be described in detail below.
[0035] Titanium (Ti): 0-0.5%, Niobium (Nb): 0-0.5%, and Vanadium (V): 0-0.5% Titanium (Ti), niobium (Nb) and vanadium (V) are elements that form precipitates to refine crystal grains and also contribute to improving the strength and impact toughness of steel sheets, so in the present invention, one or more of titanium (Ti), niobium (Nb) and vanadium (V) can be added for this effect. However, if the content of titanium (Ti), niobium (Nb) and vanadium (V) exceeds a certain level, excessive precipitates are formed, which not only reduces impact toughness but also causes an increase in manufacturing costs, so in the present invention, the content of titanium (Ti), niobium (Nb) and vanadium (V) can be limited to 0.5% or less, respectively.
[0036] Chromium (Cr): 0-3.0% and Molybdenum (Mo): 0-3.0% Chromium (Cr) and molybdenum (Mo) are elements that not only suppress austenite decomposition during alloying treatment, but also stabilize austenite like manganese (Mn), so the present invention can add at least one of chromium (Cr) and molybdenum (Mo) for this effect. However, if the chromium (Cr) and molybdenum (Mo) contents exceed a certain level, the bainite transformation time increases and the concentration of carbon (C) in the austenite becomes insufficient, making it impossible to ensure the desired retained austenite fraction. Therefore, the present invention can limit the chromium (Cr) and molybdenum (Mo) contents to 3.0% or less, respectively.
[0037] Copper (Cu): 0-4.5% and Nickel (Ni): 0-4.5% or more Copper (Cu) and nickel (Ni) are elements that stabilize austenite and inhibit corrosion. Copper (Cu) and nickel (Ni) are also elements that concentrate on the surface of the steel sheet to prevent the intrusion of hydrogen that moves into the steel sheet and inhibit hydrogen delayed fracture. Therefore, in the present invention, one or more of copper (Cu) and nickel (Ni) can be added for this effect. However, if the content of copper (Cu) and nickel (Ni) exceeds a certain level, it not only causes excessive property effects but also increases manufacturing costs, so in the present invention, the content of copper (Cu) and nickel (Ni) can be limited to 4.5% or less, respectively.
[0038] Boron (B): 0 to 0.005% Boron (B) is an element that improves hardenability and strength, and also suppresses nucleation of grain boundaries. Therefore, the present invention can add boron (B) for these effects. However, if the content of boron (B) exceeds a certain level, it not only causes excessive property effects but also increases manufacturing costs, so the present invention can limit the content of boron (B) to 0.005% or less.
[0039] One or more of the following: calcium (Ca): 0-0.05%, magnesium (Mg): 0-0.05%, and rare earth elements (REM) excluding yttrium (Y): 0-0.05% Here, the rare earth elements (REM) refer to scandium (Sc), yttrium (Y) and lanthanum group elements. The rare earth elements (REM) other than calcium (Ca), magnesium (Mg) and yttrium (Y) are elements that contribute to improving the ductility of the steel sheet by spheroidizing sulfides, so the present invention may add one or more of the rare earth elements (REM) other than calcium (Ca), magnesium (Mg) and yttrium (Y) for this effect. However, if the content of the rare earth elements (REM) other than calcium (Ca), magnesium (Mg) and yttrium (Y) exceeds a certain level, it not only causes excessive property effects but also causes an increase in manufacturing costs, so the present invention may limit the content of the rare earth elements (REM) other than calcium (Ca), magnesium (Mg) and yttrium (Y) to 0.05% or less.
[0040] Tungsten (W): 0-0.5% and zirconium (Zr): 0-0.5% or more Tungsten (W) and zirconium (Zr) are elements that improve hardenability and increase the strength of steel sheet, so the present invention may add at least one of tungsten (W) and zirconium (Zr) for this effect. However, if the content of tungsten (W) and zirconium (Zr) exceeds a certain level, it may cause excessive property effects as well as increased manufacturing costs, so the present invention may limit the content of tungsten (W) and zirconium (Zr) to 0.5% or less, respectively.
[0041] Antimony (Sb): 0-0.5% and Tin (Sn): 0-0.5% or more Antimony (Sb) and tin (Sn) are elements that improve the plating wettability and plating adhesion of steel sheets, so in the present invention, one or more of antimony (Sb) and tin (Sn) may be added to achieve this effect. However, if the content of antimony (Sb) and tin (Sn) exceeds a certain level, the brittleness of the steel sheet increases, and cracks may occur during hot working or cold working, so in the present invention, the content of antimony (Sb) and tin (Sn) may be limited to 0.5% or less, respectively.
[0042] At least one of yttrium (Y): 0-0.2% and hafnium (Hf): 0-0.2% Yttrium (Y) and hafnium (Hf) are elements that improve the corrosion resistance of steel sheets, so the present invention may add at least one of yttrium (Y) and hafnium (Hf) for this effect. However, if the content of yttrium (Y) and hafnium (Hf) exceeds a certain level, the ductility of the steel sheet may deteriorate, so the present invention may limit the content of yttrium (Y) and hafnium (Hf) to 0.2% or less, respectively.
[0043] Cobalt (Co): 0~1.5% Cobalt (Co) is an element that promotes bainite transformation and increases the TRIP effect, so in the present invention, cobalt (Co) can be added for this effect. However, if the cobalt (Co) content exceeds a certain level, the weldability and ductility of the steel sheet may deteriorate, so in the present invention, the cobalt (Co) content can be limited to 1.5% or less.
[0044] The high strength steel sheet with excellent workability according to one aspect of the present invention may contain the remaining Fe and other inevitable impurities in addition to the above-mentioned components. However, since unintended impurities may be inevitably mixed in from raw materials or the surrounding environment during normal manufacturing processes, it is not possible to completely exclude them. Since these impurities are known to anyone having ordinary skill in the art, the entire contents of the impurities will not be specifically mentioned in this specification. Furthermore, the addition of further effective components in addition to the above-mentioned components is not completely excluded.
[0045] The high-strength steel sheet with excellent workability according to one aspect of the present invention may include tempered martensite, bainite, retained austenite, and ferrite as microstructures. As a preferred example, the high-strength steel sheet with excellent workability according to one aspect of the present invention may include, by volume fraction, 30 to 70% tempered martensite, 10 to 45% bainite, 10 to 40% retained austenite, 3 to 20% ferrite, and unavoidable structures. The unavoidable structures of the present invention may include fresh martensite, pearlite, island martensite (Martensite Austenite Constituent, MA), and the like. If fresh martensite or pearlite is formed excessively, the workability of the steel sheet may decrease or the fraction of retained austenite may be reduced.
[0046] According to one aspect of the present invention, a high-strength steel sheet having excellent formability has an average total content of silicon (Si) and aluminum (Al) contained in the steel sheet ([Si+Al]) as shown in the following [Relation 1]. av The average total content of silicon (Si) and aluminum (Al) in ferrite ([Si+Al] , wt%) F %, by weight, can be in the range of 1.02 to 1.45.
[0047] [Equation 1] 1.02≦[Si+Al] F / [Si+Al] av ≦1.45
[0048] In addition, the high strength steel sheet excellent in formability according to one aspect of the present invention has a balance between tensile strength and elongation (B T·E ) is 22,000 (MPa%) or more, and the balance between tensile strength and hole expansion ratio (B T·H ) is 7 x 10 6 (MPa 2 % 1 / 2 ) or more, and the bending rate (B R ) satisfies the range of 0.5 to 3.0, it is possible to have not only an excellent balance between strength and ductility and a good balance between strength and hole expandability, but also excellent bending workability.
[0049] [Equation 2] B T·E = [Tensile strength (TS, MPa)] × [Elongation (El, %)]
[0050] [Equation 3] B T·H =[Tensile strength (TS, MPa)] 2 ×[Hole expansion rate (HER,%)] 1 / 2
[0051] [Equation 4] B R =R / t In the above Relational Formula 4, R means the minimum bending radius (mm) at which no cracks occur after a 90° bending test, and t means the thickness (mm) of the steel plate.
[0052] Since the present invention aims to ensure not only high strength properties but also excellent ductility and bending workability, it is important to stabilize the retained austenite in the steel sheet. In order to stabilize the retained austenite, it is necessary to concentrate carbon (C) and manganese (Mn) in the ferrite, bainite, and tempered martensite of the steel sheet in the austenite. However, if carbon (C) is concentrated in austenite using ferrite, the strength of the steel sheet may be insufficient due to the low strength properties of ferrite, and an excessive hardness difference between phases may occur, resulting in a decrease in the hole expansion ratio (HER). Therefore, the present invention concentrates carbon (C) and manganese (Mn) in austenite using bainite and tempered martensite.
[0053] When the content of silicon (Si) and aluminum (Al) in the retained austenite is limited to a certain range, carbon (C) and manganese (Mn) can be concentrated in the retained austenite from bainite and tempered martensite, so that the retained austenite can be effectively stabilized. In addition, by limiting the content of silicon (Si) and aluminum (Al) in the austenite to a certain range, the content of silicon (Si) and aluminum (Al) in the ferrite can be increased. As the content of silicon (Si) and aluminum (Al) in the ferrite increases, the hardness of the ferrite increases, and the hardness difference between the soft structure of ferrite and the hard structures of tempered martensite, bainite, and retained austenite can be effectively reduced.
[0054] Therefore, the present invention relates to a method for determining the average total content of silicon (Si) and aluminum (Al) contained in a steel sheet ([Si+Al] av The average total content of silicon (Si) and aluminum (Al) in ferrite ([Si+Al] , wt%) FIn order to effectively reduce the hardness difference between the soft and hard structures, the ratio of tensile strength and elongation (TS×El) and tensile strength and hole expansion ratio (TS × El) is limited to 1.02 or more by limiting the ratio of tensile strength and elongation (TS × El) to 1.02 or more by weight. On the other hand, when the silicon (Si) and aluminum (Al) content in the ferrite is excessive, the ferrite becomes excessively hard and the workability decreases. 2 ×HER 1 / 2 ) and bending rate (R / t). Therefore, the present invention provides a method for reducing the average total content of silicon (Si) and aluminum (Al) contained in the steel sheet ([Si+Al] av The average total content of silicon (Si) and aluminum (Al) in ferrite ([Si+Al] , wt%) F %, by weight, may be limited to not more than 1.45.
[0055] A steel sheet containing retained austenite has excellent ductility and bending workability due to transformation-induced plasticity that occurs when austenite transforms into martensite during processing. When the fraction of retained austenite is less than a certain level, the balance between tensile strength and elongation (TS×El) may be less than 22,000 MPa% or the bending workability (R / t) may exceed 3.0. On the other hand, when the fraction of retained austenite exceeds a certain level, local elongation may decrease. Therefore, in order to obtain a steel sheet having an excellent bending workability (R / t) as well as a good balance between tensile strength and elongation (TS×El), the fraction of retained austenite may be limited to a range of 10 to 40 volume %.
[0056] On the other hand, both untempered martensite (fresh martensite) and tempered martensite are microstructures that improve the strength of steel sheets. However, compared with tempered martensite, fresh martensite has the property of significantly reducing the ductility and hole expandability of steel sheets. This is because the microstructure of tempered martensite is softened by tempering heat treatment. Therefore, in the present invention, it is preferable to utilize tempered martensite in order to provide a steel sheet that is excellent in balance between strength and ductility, balance between strength and hole expandability, and bending workability. When the fraction of tempered martensite is less than a certain level, the balance between tensile strength and elongation (TS×El) of 22,000 MPa% or more or the balance between tensile strength and elongation of 7×10 6 (MPa 2 % 1 / 2 ) or higher balance of tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 ), and if the fraction of tempered martensite exceeds a certain level, ductility and workability decrease, and the balance between tensile strength and elongation (TS×El) is less than 22,000 MPa% or the bending work ratio (R / t) exceeds 3.0, which is undesirable. Therefore, the present invention provides a balance between tensile strength and elongation (TS×El) and a balance between tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 In order to obtain a steel sheet excellent in hardness (H) and bending workability (R / t), the fraction of tempered martensite can be limited to the range of 30 to 70 volume %.
[0057] Balance of tensile strength and elongation rate (TS×El), balance of tensile strength and hole expansion rate (TS 2 ×HER 1 / 2 In order to improve the bending workability (R / t) and bending rate (R / t), it is preferable that bainite is appropriately contained as a microstructure. Only when the bainite fraction is at a certain level or higher, the balance between tensile strength and elongation (TS×El) of 22,000 MPa% or more and 7×10 6 (MPa 2 % 1 / 2 ) or higher balance of tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2) and a bending ratio (R / t) of 0.5 to 3.0 can be ensured. On the other hand, if the fraction of bainite is excessive, a decrease in the fraction of tempered martensite is inevitably accompanied, and ultimately, the balance between tensile strength and elongation (TS×El) and the balance between tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 ) and bending ratio (R / t) cannot be ensured. Therefore, in the present invention, the fraction of bainite can be limited to the range of 10 to 45 volume %.
[0058] Since ferrite is an element that contributes to improving ductility, the balance between tensile strength and elongation (TS×El) targeted by the present invention can be ensured only when the fraction of ferrite is at a certain level or higher. However, if the fraction of ferrite is excessive, the hardness difference between the phases increases and the hole expansion ratio (HER) may decrease, so the balance between tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 ) cannot be ensured. Therefore, in the present invention, the ferrite fraction can be limited to the range of 3 to 20 volume %.
[0059] An example of a method for producing the steel sheet of the present invention will be described in detail below. A method for producing a high strength steel sheet according to one aspect of the present invention includes the steps of preparing a steel slab having a predetermined composition, heating the steel slab, and hot rolling the steel slab; coiling the hot rolled steel sheet; subjecting the coiled steel sheet to a hot rolling annealing heat treatment at a temperature range of 650 to 850°C for 600 to 1700 seconds; cold rolling the hot rolled annealed steel sheet; heating the cold rolled steel sheet to a temperature range of Ac1 to Ac3 at an average heating rate of 5°C / s or more (primary heating) and holding the temperature for 50 seconds or more (primary holding); cooling the cold rolled steel sheet to a temperature range of 100 to 300°C at an average cooling rate of 1°C / s or more (primary cooling); heating the primarily cooled steel sheet to a temperature range of 300 to 500°C (secondary heating) and holding the temperature for 50 seconds or more (secondary holding); and cooling to room temperature (secondary cooling).
[0060] Preparation and heating of steel slabs A steel slab having a predetermined composition is prepared. Since the steel slab of the present invention has an alloy composition corresponding to the alloy composition of the steel plate described above, the description of the alloy composition of the steel slab is substituted for the description of the alloy composition of the steel plate described above.
[0061] The prepared steel slab can be heated to a certain temperature range. The heating temperature of the steel slab may be in the range of 1000 to 1350°C. If the heating temperature of the steel slab is less than 1000°C, there is a risk that the steel slab will be hot rolled in a temperature range below the intended finish hot rolling temperature range, and if the heating temperature of the steel slab is more than 1350°C, there is a risk that the steel will reach its melting point and melt.
[0062] Hot rolling and coiling The heated steel slab can be hot rolled to provide a hot rolled steel sheet. The finish hot rolling temperature during hot rolling is preferably in the range of 800 to 1000° C. If the finish hot rolling temperature is less than 800° C., excessive rolling load may become a problem, and if the finish hot rolling temperature exceeds 1000° C., the crystal grains of the hot rolled steel sheet may be formed coarsely, which may lead to a deterioration in the physical properties of the final steel sheet.
[0063] After hot rolling, the hot-rolled steel sheet can be cooled at an average cooling rate of 10° C. / s or more and coiled at a temperature of 300 to 600° C. If the coiling temperature is less than 300° C., coiling is not easy, and if the coiling temperature exceeds 600° C., surface scale may form inside the hot-rolled steel sheet, making pickling difficult.
[0064] Hot rolling annealing heat treatment In order to easily perform the subsequent processes of pickling and cold rolling after coiling, it is preferable to perform a hot rolling annealing heat treatment process. The hot rolling annealing heat treatment can be performed in the temperature range of 650 to 850°C for 600 to 1700 seconds. If the hot rolling annealing heat treatment temperature is less than 650°C or the hot rolling annealing heat treatment time is less than 600 seconds, the strength of the hot rolling annealing heat treated steel sheet is high, and the subsequent cold rolling may not be easy. On the other hand, if the hot rolling annealing heat treatment temperature exceeds 850°C or the hot rolling annealing heat treatment time exceeds 1700 seconds, pickling may not be easy due to scale formed deep inside the steel sheet.
[0065] Pickling and cold rolling After the hot rolling annealing heat treatment, the steel sheet may be pickled to remove scale formed on the surface thereof, and then cold rolled. In the present invention, the conditions for pickling and cold rolling are not particularly limited, but the cold rolling is preferably performed at a cumulative reduction of 30 to 90%. If the cumulative reduction of cold rolling exceeds 90%, it may be difficult to perform cold rolling in a short time due to the high strength of the steel sheet.
[0066] The cold-rolled steel sheet can be produced as an uncoated cold-rolled steel sheet through an annealing heat treatment process, or can be produced as a coated steel sheet through a coating process to impart corrosion resistance. Coating can be performed by a coating method such as hot-dip galvanizing, electrolytic galvanizing, or hot-dip aluminum plating, and the method and type are not particularly limited.
[0067] Annealing heat treatment In the present invention, an annealing heat treatment step is carried out in order to ensure both the strength and workability of the steel sheet.
[0068] Cold-rolled steel sheets are heated to a temperature range of Ac1 or more but less than Ac3 (two-phase region) (primary heating) and held at that temperature range for 50 seconds or more (primary holding). If the primary heating or primary holding temperature is Ac3 or more (single-phase region), the desired ferrite structure cannot be realized, so the desired level of [Si+Al] F / [Si+Al] av And the balance between tensile strength and hole expansion ratio (TS2 ×HER 1 / 2 ) cannot be realized. Furthermore, if the primary heating or primary holding temperature is in a temperature range below Ac1, sufficient heating is not performed, and the microstructure targeted by the present invention may not be realized even by the subsequent heat treatment. The average heating rate of the primary heating may be 5°C / s or more.
[0069] If the first holding time is less than 50 seconds, the structure cannot be sufficiently homogenized, and the physical properties of the steel sheet may deteriorate. Although there is no particular upper limit to the first holding time, it is preferable to limit the first heating time to 1200 seconds or less in order to prevent a decrease in toughness due to coarsening of crystal grains.
[0070] After the primary holding, the steel sheet can be cooled (primary cooling) to a primary cooling stop temperature of 100 to 300°C at an average cooling rate of 1°C / s or more. There is no particular need to specify an upper limit for the primary cooling rate, but it is preferably 100°C / s or less. If the primary cooling stop temperature is less than 100°C, tempered martensite is excessively formed, and the amount of retained austenite formed is insufficient, resulting in a decrease in the [Si+Al] of the steel sheet. F / [Si+Al] av On the other hand, if the primary cooling stop temperature exceeds 300°C, bainite is excessively formed and the amount of tempered martensite formed is insufficient, so that the balance between the tensile strength and the elongation rate (TS×El) and the balance between the tensile strength and the hole expansion rate (TS 2 ×HER 1 / 2 ) may be reduced.
[0071] After the above primary cooling, the steel sheet can be heated to a secondary heating temperature of 300 to 500°C at an average heating rate of 5°C / s or more (secondary heating) and held at that temperature range for 50 seconds or more (secondary holding). There is no particular need to specify an upper limit for the secondary heating rate, but it is preferably 100°C / s or less. If the secondary heating or secondary holding temperature is less than 300°C or the holding time is less than 50 seconds, tempered martensite is excessively formed, the silicon (Si) and aluminum (Al) contents in the steel are insufficiently controlled, and it is difficult to ensure the desired retained austenite fraction. As a result, the [Si+Al] of the steel sheet is F / [Si+Al] av However, if the secondary heating or holding temperature exceeds 500°C or the secondary holding time exceeds 126,000 seconds, the silicon (Si) and aluminum (Al) contents in the steel are not sufficiently controlled, making it difficult to ensure the fraction of retained austenite. As a result, the [Si+Al] of the steel sheet is F / [Si+Al] av and the balance between tensile strength and elongation (TS × El) may decrease.
[0072] After the secondary holding, it can be cooled to room temperature (secondary cooling) at an average cooling rate of 1°C / s or more.
[0073] The high-strength steel plate with excellent workability produced by the above-mentioned production method can contain, as a microstructure, tempered martensite, bainite, retained austenite, and ferrite, and as a preferred example, can contain, by volume fraction, 30 to 70% tempered martensite, 10 to 45% bainite, 10 to 40% retained austenite, 3 to 20% ferrite, and unavoidable structures.
[0074] In addition, the high-strength steel plate with excellent workability manufactured by the above-mentioned manufacturing method has an average total content of silicon (Si) and aluminum (Al) contained in the steel plate ([Si+Al]) as shown in the following [Relation 1]. avThe average total content of silicon (Si) and aluminum (Al) in ferrite ([Si+Al] , wt%) F The ratio of (wt%) can be in the range of 1.02 to 1.45, and the balance between tensile strength and elongation (B T·E ) is 22,000 (MPa%) or more, and the balance between tensile strength and hole expansion ratio (B T·H ) is 7 x 10 6 (MPa 2 % 1 / 2 ) or more, and the bending rate (B R ) can be in the range of 0.5 to 3.0.
[0075] [Equation 1] 1.02≦[Si+Al] F / [Si+Al] av ≦1.45
[0076] [Equation 2] B T·E = [Tensile strength (TS, MPa)] × [Elongation (EL, %)]
[0077] [Equation 3] B T·H =[Tensile strength (TS, MPa)] 2 ×[Hole expansion rate (HER,%)] 1 / 2
[0078] [Equation 4] B R =R / t In the above Relational Formula 4, R means the minimum bending radius (mm) at which no cracks occur after a 90° bending test, and t means the thickness (mm) of the steel plate. EXAMPLES
[0079] Hereinafter, a high strength steel sheet having excellent workability and a manufacturing method thereof according to one aspect of the present invention will be described in more detail with reference to specific examples. It should be noted that the following examples are provided to aid in the understanding of the present invention and are not intended to specify the scope of the present invention. The scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom.
[0080] (Example) A steel slab having a thickness of 100 mm and having the alloy composition shown in Table 1 below (the remainder being Fe and unavoidable impurities) was manufactured, heated at 1200°C, and then finish hot-rolled at 900°C. Then, it was cooled at an average cooling rate of 30°C / s and coiled at the coiling temperature shown in Tables 2 and 3 to manufacture a hot-rolled steel sheet having a thickness of 3 mm. The hot-rolled steel sheet was subjected to a hot-rolling annealing heat treatment under the conditions shown in Tables 2 and 3. Then, the surface scale was removed by pickling, and the steel sheet was cold-rolled to a thickness of 1.5 mm. Then, heat treatment was performed under the annealing heat treatment conditions shown in Tables 2 to 5 to manufacture a steel sheet.
[0081] The microstructure of the steel sheets manufactured in this manner was observed, and the results are shown in Tables 6 and 7. Among the microstructures, ferrite (F), bainite (B), tempered martensite (TM), and pearlite (P) were observed through SEM after nital etching of the polished cross section of the specimen. Among these, the fractions of bainite and tempered martensite, which are difficult to distinguish, were calculated using dilatation curves after dilatation evaluation. Meanwhile, since it is also difficult to distinguish between fresh martensite (FM) and retained austenite (residual γ), the fraction of retained austenite calculated by X-ray diffraction method was determined as the fraction of fresh martensite, since it is also difficult to distinguish between fresh martensite (FM) and retained austenite (residual γ).
[0082] On the other hand, the [Si+Al] of steel plate F / [Si+Al] av , balance of tensile strength and elongation rate (TS×El), balance of tensile strength and hole expansion rate (TS 2 ×HER 1 / 2) and bending rate (R / t) were observed, and the results are shown in Tables 8 and 9.
[0083] The average total content of silicon (Si) and aluminum (Al) in ferrite ([Si+Al] F , wt%) is the average total content of silicon (Si) and aluminum (Al) contained in the steel sheet, measured using an EPMA (Electron Probe MicroAnalyser). av , wt. % was calculated from the content of the alloy composition of the steel sheet.
[0084] Tensile strength (TS) and elongation (El) were evaluated by tensile tests, and specimens were taken based on JIS No. 5 standard, with the 90° direction relative to the rolling direction of the rolled plate material as the reference, and tensile strength (TS) and elongation (El) were measured. Bending ratio (R / t) was evaluated by V-bending tests, and specimens were taken based on the 90° direction relative to the rolling direction of the rolled plate material, and the minimum bending radius R at which no cracks occurred after the 90° bending test was determined and calculated by dividing it by the thickness t of the plate material. Hole expansion ratio (HER) was evaluated by hole expansion tests, and after forming a 10 mmΦ punch hole (die inner diameter 10.3 mm, clearance 12.5%), a conical punch with an apex angle of 60° was inserted into the punch hole in the direction in which the burr of the punch hole was on the outside, and the periphery of the punch hole was compressed and expanded at a moving speed of 20 mm / min, and then the calculation was performed using the following [Relationship 5].
[0085] [Equation 5] Hole expansion ratio (HER,%) = {(D-D0) / D0} x 100 In the above Relational Formula 5, D means the hole diameter (mm) when the crack penetrates the steel plate along the thickness direction, and D0 means the initial hole diameter (mm).
[0086] [Table 1]
[0087] [Table 2]
[0088] [Table 3]
[0089] [Table 4]
[0090] [Table 5]
[0091] [Table 6]
[0092] [Table 7]
[0093] [Table 8]
[0094] [Table 9]
[0095] As shown in Tables 1 to 9, in the case of specimens satisfying the conditions presented in the present invention, [Si+Al] F / [Si+Al] av The value of is in the range of 1.02 to 1.45, the balance of tensile strength and elongation (TS × El) is 22,000 MPa% or more, and the balance of tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 ) is 7 x 10 6 (MPa 2 % 1 / 2) or more, the bending rate (R / t) falls within the range of 0.5 to 3.0, and it is found that the steel has both excellent strength and workability.
[0096] Although the alloy composition ranges of specimens 2 to 5 overlap with those of the present invention, the hot rolling annealing temperature and time are outside the ranges of the present invention, and therefore it can be confirmed that poor pickling occurs and breakage occurs during cold rolling.
[0097] In the case of Sample 6, the primary heating or holding temperature during the annealing heat treatment after cold rolling exceeded the range limited by the present invention, so the amount of ferrite formation was insufficient. As a result, Sample 6 had a [Si+Al] F / [Si+Al] av The balance between tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 ) is 7 x 10 6 (MPa 2 % 1 / 2 ) or less.
[0098] In the case of Sample 7, the primary cooling rate during the annealing heat treatment after cold rolling did not reach the range limited by the present invention, so ferrite was formed excessively and retained austenite was formed in small amounts. As a result, Sample 7 had a [Si+Al] F / [Si+Al] av It can be confirmed that the tensile strength and elongation balance (TS × El) is less than 22,000 MPa%.
[0099] In sample 12, the first cooling stop temperature was low, so tempered martensite was formed excessively and retained austenite was formed in small amounts. As a result, sample 12 had a low [Si+Al] F / [Si+Al] av It can be confirmed that the tensile strength and elongation balance (TS × El) is less than 22,000 MPa%, and the bending work ratio (R / t) is more than 3.0.
[0100] In specimen 13, the first cooling stop temperature was high, so bainite was formed excessively and tempered martensite was formed in small amounts. As a result, the balance between tensile strength and elongation (TS × El) of specimen 13 was less than 22,000 MPa%, and the balance between tensile strength and hole expansion ratio (TS 2 ×HER 1 / 2 ) is 7 x 10 6 (MPa 2 % 1 / 2 ) or less.
[0101] In sample 14, the secondary heating or holding temperature was low, so tempered martensite was formed excessively and retained austenite was formed in small amounts. As a result, sample 14 had a low [Si+Al] F / [Si+Al] av It can be confirmed that the tensile strength and elongation balance (TS × El) is less than 22,000 MPa%, and the bending work ratio (R / t) is more than 3.0.
[0102] In specimen 15, the secondary heating or holding temperature was too high, so the amount of retained austenite formed was insufficient, and [Si+Al] F / [Si+Al] av It can be confirmed that the tensile strength and elongation balance (TS × El) is less than 22,000 MPa%.
[0103] In specimen 16, the second holding time was insufficient, so tempered martensite was formed excessively and retained austenite was not formed. As a result, specimen 16 had a [Si+Al] F / [Si+Al] av It can be confirmed that the tensile strength and elongation balance (TS × El) is less than 22,000 MPa%, and the bending work ratio (R / t) is more than 3.0.
[0104] In specimen 17, the secondary holding time was too long, and the amount of retained austenite formed was insufficient, resulting in [Si+Al] F / [Si+Al] avIt can be confirmed that the balance between tensile strength and elongation (TS × El) is less than 22,000 MPa%.
[0105] Samples 40 to 48 satisfy the manufacturing conditions proposed by the present invention, but are outside the alloy composition range. F / [Si+Al] av , balance of tensile strength and elongation rate (TS×El), balance of tensile strength and hole expansion rate (TS 2 ×HER 1 / 2 ) is 7 x 10 6 (MPa 2 %) 1 / 2 It can be seen that the conditions of [Si+Al] and bending rate (R / t) are not satisfied at the same time. On the other hand, in the case of specimen 42, the total content of aluminum (Al) and silicon (Si) is less than 1.0%, and the [Si+Al] F / [Si+Al] av It can be seen that the conditions for the balance between tensile strength and elongation (TS×El) and the bending rate (R / t) are not met.
[0106] Although the present invention has been described in detail with reference to the embodiments, other embodiments may be possible, and therefore the scope of the claims set forth below should not be limited to the embodiments.
Claims
1. In weight percent, C: 0.25 to 0.75%, Si: 4.0% or less, Mn: 0.9 to 5.0%, Al: 5.0% or less, P: 0.15% or less, S: 0.03% or less, N: 0.03% or less, the balance being Fe and unavoidable impurities; The total content of Si and Al (Si+Al) is 1.0 to 6.0 wt.%; The microstructure includes 30 to 70 volume % tempered martensite, 10 to 45 volume % bainite, 10 to 40 volume % retained austenite, 3 to 20 volume % ferrite, and unavoidable structures; A steel plate satisfying the following [Relationship 1]. [Relationship 1] 1.02≦[Si+Al] F / [Si+Al] av ≦1.45 In the above-mentioned relational formula 1, [Si + Al] F is the average total content (wt%) of Si and Al contained in ferrite, [Si + Al] av is the average total content (wt%) of Si and Al contained in the steel sheet.
2. The steel plate according to claim 1, further comprising one or more of the following (1) to (9): (1) One or more of Ti: 0-0.5%, Nb: 0-0.5%, and V: 0-0.5% (2) One or more of Cr: 0-3.0% and Mo: 0-3.0% (3) One or more of Cu: 0-4.5% and Ni: 0-4.5% (4) B: 0-0.005% (5) One or more of Ca: 0-0.05%, REM excluding Y: 0-0.05%, and Mg: 0-0.05%. (6) One or more of W: 0-0.5% and Zr: 0-0.5% (7) One or more of Sb: 0-0.5% and Sn: 0-0.5% (8) One or more of Y: 0-0.2% and Hf: 0-0.2% (9) Co: 0-1.5%
3. The steel sheet has a balance between tensile strength and elongation (B T・E ) is 22,000 (MPa%) or more, and the balance between the tensile strength and the hole expansion ratio (B T・H ) is 7 x 10 6 (MPa 2 % 1/2 ) or more, and the bending rate (B R 2. The steel sheet according to claim 1, wherein the value of σ is 0.5 to 3.
0. [Relationship 2] B T・E = [tensile strength (TS, MPa)] × [elongation (El, %)] [Relationship 3] B T・H = [tensile strength (TS, MPa)] 2 × [Hole expansion rate (HER,%)] 1/2 [Relationship 4] B R =R / t In the above Relational Formula 4, R means the minimum bending radius (mm) at which no cracks occur after a 90° bending test, and t means the thickness (mm) of the steel plate.
4. heating and hot rolling a steel slab having, by weight percent, C: 0.25-0.75%, Si: 4.0% or less, Mn: 0.9-5.0%, Al: 5.0% or less, P: 0.15% or less, S: 0.03% or less, N: 0.03% or less, and the remainder being Fe and unavoidable impurities, and the total content of Si and Al (Si+Al) being 1.0-6.0% by weight; coiling the hot rolled steel sheet; subjecting the coiled steel sheet to a hot rolling annealing heat treatment at a temperature range of 650 to 850° C. for 600 to 1700 seconds; cold rolling the hot-rolled annealed steel sheet; Heating the cold-rolled steel sheet to a temperature range of Ac1 or more and less than Ac3 at an average heating rate of 5° C. / s or more (primary heating) and holding the temperature for 50 seconds or more (primary holding); a step of cooling (primary cooling) to a temperature range of 100 to 300° C. at an average cooling rate of 1.0° C. / s or more; heating the primarily cooled steel sheet to a temperature range of 300 to 500° C. (secondary heating) and holding the steel sheet for 50 to 126,000 seconds (secondary holding); The method for producing a steel sheet according to any one of claims 1 to 3, further comprising:
5. The method for producing a steel plate according to claim 4, wherein the steel slab further includes one or more of the following (1) to (9): (1) One or more of Ti: 0-0.5%, Nb: 0-0.5%, and V: 0-0.5% (2) One or more of Cr: 0-3.0% and Mo: 0-3.0% (3) One or more of Cu: 0-4.5% and Ni: 0-4.5% (4) B: 0-0.005% (5) One or more of Ca: 0-0.05%, REM excluding Y: 0-0.05%, and Mg: 0-0.05%. (6) One or more of W: 0-0.5% and Zr: 0-0.5% (7) One or more of Sb: 0-0.5% and Sn: 0-0.5% (8) One or more of Y: 0-0.2% and Hf: 0-0.2% (9) Co: 0-1.5%
6. The method for producing a steel plate according to claim 4, wherein the steel slab is heated to a temperature range of 1000 to 1350°C and finish hot rolled at a temperature range of 800 to 1000°C.
7. The method for producing a steel sheet according to claim 4, wherein the hot-rolled steel sheet is coiled at a temperature in the range of 300 to 600°C.
8. The method for producing a steel sheet according to claim 4, wherein the cold rolling reduction is 30 to 90%.
9. The method for producing a steel sheet according to claim 4, wherein the cooling rate of the secondary cooling is 1° C. / s or more.
Citation Information
Patent Citations
Hot dip galvannealed high strength steel sheet having tensile strength of >=700 mpa and excellent corrosion resistance, hole expansibility and ductility, and method for producing the same
JP2009019258A
High-strength steel sheet and high-strength hot-dip galvanized steel sheet having excellent workability, and method for producing them
JP2010275627A
High strength thin steel sheet having excellent elongation and press forming stability
JP2012041573A
High-strength hot-dip galvanized steel plate with excellent moldability in ordinary and intermediate temperature range, and method for manufacturing the same
JP2013234340A
High strength steel sheet excellent in ductility and low temperature toughness and manufacturing method therefor