Blank mask and photomask using same
A multilayered light-shielding film with controlled etching rates and optical densities in photomasks addresses the issue of pattern resolution loss, enhancing the precision of fine circuit pattern formation on semiconductor wafers.
Patent Information
- Application Number
- JP2023123420
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-05-21
- Filing Date
- 2023-07-28
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2042-04-19
AI Technical Summary
The challenge in semiconductor manufacturing is the decrease in pattern resolution due to light diffraction and non-uniform etching during the formation of fine circuit patterns, particularly in binary masks and phase shift masks, which affects the precision and integrity of photomasks.
A multilayered light-shielding film structure is introduced in the photomask, comprising a first and second light-shielding layer with specific compositions and densities, optimized to minimize pattern edge loss and enhance the side profile precision through controlled etching, using transition metals like Cr, Ta, Ti, and Hf, and elements such as oxygen and nitrogen, with precise control of etching rates and optical densities.
The solution effectively suppresses the decrease in pattern resolution, ensuring precise control of the side profile and critical dimension deviation, thereby improving the photomask's ability to form finer circuit patterns on semiconductor wafers.
Smart Images

Figure 0007554885000007 
Figure 0007554885000008 
Figure 0007554885000006
Abstract
Description
[Technical field]
[0001] The embodiment relates to a blank mask and a photomask using the same. [Background technology]
[0002] The increasing integration of semiconductor devices and other devices requires finer circuit patterns, which increases the importance of lithography, a technique for developing circuit patterns on the surface of a wafer using a photomask.
[0003] In order to develop fine circuit patterns, the exposure light source used in the exposure process must have a shorter wavelength. Recent exposure light sources include the ArF excimer laser (wavelength 193 nm).
[0004] Meanwhile, photomasks include binary masks and phase shift masks.
[0005] A binary mask has a structure in which a light-shielding layer pattern is formed on a light-transmitting substrate. In the binary mask, on the surface on which the pattern is formed, the transparent portion not including the light-shielding layer transmits the exposure light, and the light-shielding portion including the light-shielding layer blocks the exposure light, thereby exposing the pattern on the resist film on the wafer surface. However, as the pattern becomes finer, the binary mask may cause problems in developing the fine pattern due to the diffraction of light that occurs at the edge of the transparent portion during the exposure process.
[0006] Phase shift masks include the Levenson type, the outrigger type, and the half-tone type. Among them, the half-tone type phase shift mask has a configuration in which a pattern formed of a semi-transmitting film is arranged on a light-transmitting substrate. In the half-tone type phase shift mask, on the surface on which the pattern is arranged, the transmissive portion not including the semi-transmitting layer transmits the exposure light, and the semi-transmitting portion including the semi-transmitting layer transmits the attenuated exposure light. The attenuated exposure light has a phase difference compared to the exposure light that has passed through the transmissive portion. As a result, the diffracted light generated at the edge of the transmissive portion is offset by the exposure light that has passed through the semi-transmitting portion, and the phase shift mask can form a more elaborate fine pattern on the surface of the wafer. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Korean Patent No. 10-1579843 [Patent Document 2] Korean Patent No. 10-1584383 [Patent Document 3] Korean Patent No. 10-1207724 Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the embodiment is to provide a blank mask capable of effectively suppressing a decrease in resolution of a pattern when a light-shielding film is patterned, and a photomask using the blank mask. [Means for solving the problem]
[0009] A blank mask according to an embodiment of the present specification includes a light-transmitting substrate and a light-shielding film disposed on the light-transmitting substrate.
[0010] The light-shielding film contains a transition metal and at least one of oxygen and nitrogen.
[0011] The light-shielding film includes a first light-shielding layer and a second light-shielding layer disposed on the first light-shielding layer.
[0012] The loss area of the pattern edge measured after patterning the light-shielding film was 10 nm 2 The following is the result.
[0013] The pattern edge loss area is an area surrounded by the first line, the second line, and the pattern edge profile of the light-shielding pattern film when a transmission electron microscopy (TEM) image of the light-shielding pattern film formed by patterning the light-shielding film is measured and the TEM image is observed.
[0014] The first line is an extension line connecting a first point located at a height of 20% and a second point located at a height of 40% in a side profile of the light-shielding pattern film, when the total height of the light-shielding pattern film is 100%.
[0015] The second line is an extension line including the intersection of the pattern film and disposed parallel to the upper surface of the light-transmitting substrate.
[0016] The pattern film intersection point is a point where a center line of the pattern film intersects with an upper surface profile of the light-shielding pattern film.
[0017] The pattern film center line is an extension line that passes through a pattern film center point, which is the center point of the bottom surface of the light-shielding pattern film, and is perpendicular to the upper surface of the light-transmitting substrate.
[0018] The light-shielding film may have a Do value of less than 0.05 in the following formula 2:
[0019] [Formula 2] Do=Bo-Po
[0020] In the formula 2, the Bo value is the optical density of the light-shielding film measured with exposure light having a wavelength of 193 nm.
[0021] The Po value is the optical density measured by irradiating an exposure light having a wavelength of 193 nm onto a measurement area corresponding to a region from one edge formed by patterning the light-shielding pattern film to a position 4 nm away inward of the light-shielding pattern film when the light-shielding pattern film formed by patterning the light-shielding film is observed from above.
[0022] The transition metal may include at least one of Cr, Ta, Ti, and Hf.
[0023] The etching rate of the light-shielding film with respect to a chlorine-based gas may be 1.55 Å / s or more.
[0024] The second light-shielding layer may contain 50 to 80 at % of a transition metal.
[0025] The content of the element corresponding to oxygen or nitrogen in the second light-shielding layer may be 10 to 35 at %.
[0026] The first light-shielding layer may contain 30 to 60 at % of a transition metal.
[0027] The total content of oxygen and nitrogen in the first light-shielding layer may be 40 to 70 at %.
[0028] The ratio of the thickness of the second light-shielding layer to the thickness of the first light-shielding layer may be 0.05 to 0.3.
[0029] A photomask according to another embodiment of the present specification includes a light-transmitting substrate and a light-shielding pattern film disposed on the light-transmitting substrate.
[0030] The light-shielding pattern film contains a transition metal and at least one of oxygen and nitrogen.
[0031] The light-shielding pattern film includes a first light-shielding layer and a second light-shielding layer disposed on the first light-shielding layer.
[0032] The loss area of the pattern edge measured in the light-shielding pattern film was 10 nm 2 The following is the result.
[0033] The pattern edge loss area is an area surrounded by the first line, the second line, and the pattern edge profile of the light-shielding pattern film when a transmission electron microscopy (TEM) image of the light-shielding pattern film is measured and the TEM image is observed.
[0034] The first line is an extension line connecting a first point located at a height of 20% and a second point located at a height of 40% in a side profile of the light-shielding pattern film, when the total height of the light-shielding pattern film is 100%.
[0035] The second line is an extension line including the intersection of the pattern film and disposed parallel to the upper surface of the light-transmitting substrate.
[0036] The pattern film intersection point is a point where a center line of the pattern film intersects with an upper surface profile of the light-shielding pattern film.
[0037] The pattern film center line is an extension line that passes through a pattern film center point, which is the center point of the bottom surface of the light-shielding pattern film, and is perpendicular to the upper surface of the light-transmitting substrate.
[0038] A method for manufacturing a semiconductor element according to yet another embodiment of the present specification includes a preparation step of arranging a light source, a photomask, and a semiconductor wafer coated with a resist film, an exposure step of selectively transmitting and emitting light incident from the light source through the photomask onto the semiconductor wafer, and a development step of developing a pattern on the semiconductor wafer.
[0039] The photomask includes a light-transmitting substrate and a light-shielding pattern film disposed on the light-transmitting substrate.
[0040] The light-shielding pattern film contains a transition metal and at least one of oxygen and nitrogen.
[0041] The light-shielding pattern film includes a first light-shielding layer and a second light-shielding layer disposed on the first light-shielding layer.
[0042] The loss area of the pattern edge measured in the light-shielding pattern film was 10 nm 2 The following is the result.
[0043] The pattern edge loss area is an area surrounded by the first line, the second line, and the pattern edge profile of the light-shielding pattern film when a transmission electron microscopy (TEM) image of the light-shielding pattern film formed by patterning the light-shielding film is measured and the TEM image is observed.
[0044] The first line is an extension line connecting a first point located at a height of 20% and a second point located at a height of 40% in a side profile of the light-shielding pattern film, when the total height of the light-shielding pattern film is 100%.
[0045] The second line is an extension line including the intersection of the pattern film and disposed parallel to the upper surface of the light-transmitting substrate.
[0046] The pattern film intersection point is a point where a center line of the pattern film intersects with an upper surface profile of the light-shielding pattern film.
[0047] The pattern film center line is an extension line that passes through a pattern film center point, which is the center point of the bottom surface of the light-shielding pattern film, and is perpendicular to the upper surface of the light-transmitting substrate. Effect of the Invention
[0048] The blank mask according to the embodiment may effectively suppress a decrease in resolution of a pattern that may occur during patterning of a light-shielding film. [Brief description of the drawings]
[0049] [Figure 1] FIG. 1 is a conceptual diagram illustrating a blank mask according to an embodiment disclosed in this specification. [Diagram 2] 1 is a conceptual diagram illustrating a method for measuring a loss area of a pattern edge of a light-shielding pattern film formed by patterning a light-shielding film. [Diagram 3] 1 is a conceptual diagram illustrating a light-shielding pattern film formed by patterning a light-shielding film of a blank mask to be measured according to one embodiment. FIG. [Figure 4] 1 is a plan view of a light-shielding pattern film formed by patterning a light-shielding film according to an embodiment of the present invention, observed from above; [Diagram 5] FIG. 13 is a conceptual diagram illustrating a blank mask according to another embodiment. [Figure 6] FIG. 13 is a conceptual diagram illustrating a photomask according to yet another embodiment. BEST MODE FOR CARRYING OUT THEINVENTION
[0050] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention is not limited to the embodiments described herein, but may be practiced in various different forms.
[0051] As used herein, terms of degree such as "about," "substantially," and the like are used in a numerical or approximate sense when the tolerances of manufacturing and materials inherent in the referred meaning are given, and are used to prevent unscrupulous infringers from unfairly taking advantage of disclosures in which precise or absolute numerical values are referred to to aid in the understanding of the embodiments.
[0052] Throughout this specification, the term "combinations thereof" in a Markush form phrase means a mixture or combination of one or more selected from the group of elements set forth in the Markush form phrase, including one or more selected from the group of elements.
[0053] Throughout this specification, the phrase "A and / or B" means "A, B, or A and B."
[0054] Throughout this specification, terms such as "first", "second" or "A", "B" are used to distinguish identical terms from one another, unless otherwise specified.
[0055] In this specification, the term "B is located on A" means that B can be located on A, or B can be located on A with another layer located therebetween, and is not to be interpreted as being limited to B being located in contact with the surface of A.
[0056] In this specification, the term "singular" is to be construed as including the singular or plural as the context requires, unless otherwise specified.
[0057] In this specification, normal temperature means 20 to 25°C.
[0058] In this specification, the surface profile of the light-shielding pattern film refers to the outline of the light-shielding pattern film observed in a cross section when the cross section of the light-shielding pattern film is observed using a TEM (Transmission Electron Microscopy) measuring device or the like.
[0059] In this specification, the side profile of the light-shielding pattern film refers to the outline of the side of the light-shielding pattern film observed in a cross section when the cross section of the light-shielding pattern film is observed using a TEM measuring device or the like.
[0060] In this specification, the pattern edge profile of a light-shielding pattern film refers to the outline of the upper corners and their surroundings of the light-shielding pattern film observed in a cross section of the light-shielding pattern film when the cross section of the light-shielding pattern film is observed using a TEM measurement device or the like.
[0061] As semiconductors become more highly integrated, there is a demand for finer circuit patterns to be formed on semiconductor wafers. As the line width of patterns developed on semiconductor wafers becomes smaller, problems related to the resolution of photomasks also tend to increase.
[0062] The light-shielding film included in the blank mask may be formed into a light-shielding pattern film through etching, etc. The light-shielding pattern film may be formed through etching using an etching gas as an etchant, using a resist pattern or other thin film pattern disposed on the light-shielding film as a mask.
[0063] When the light-shielding film is patterned by a dry etching method using an etching gas as an etchant, the light-shielding pattern film formed through patterning may exhibit non-uniform optical characteristics in the in-plane direction. Specifically, the etching gas may etch the light-shielding film from the surface of the light-shielding film toward the lower part of the light-shielding film along the resist pattern or etching mask. In the etching process, the upper region of the side of the light-shielding pattern film formed may be exposed to the etching gas for a relatively long time compared to the lower region of the side. As a result, excessive etching may occur in the upper region of the side of the light-shielding pattern film in the in-plane direction of the light-shielding film. This may be one of the factors that reduce the resolution of the blank mask.
[0064] The inventors of the embodiment confirmed that the degradation of the resolution of the blank mask can be effectively suppressed by introducing a multi-layer structure into the light-shielding film, with the upper layer having a denser structure than the lower layer, and thus completed the embodiment.
[0065] Hereinafter, the embodiment will be described in detail.
[0066] 1 is a conceptual diagram illustrating a blank mask according to an embodiment disclosed herein. A blank mask of an embodiment will be described with reference to FIG.
[0067] The blank mask 100 includes a light-transmitting substrate 10 and a light-shielding film 20 located on the light-transmitting substrate 10 .
[0068] The material of the light-transmitting substrate 10 is not limited as long as it has light transmittance to the exposure light and can be applied to the blank mask 100. Specifically, the transmittance of the light-transmitting substrate 10 to the exposure light with a wavelength of 193 nm may be 85% or more. The transmittance may be 87% or more. The transmittance may be 99.99% or less. Exemplarily, a synthetic quartz substrate may be applied as the light-transmitting substrate 10. In such a case, the light-transmitting substrate 10 can suppress the attenuation of the light passing through the light-transmitting substrate 10.
[0069] In addition, the light-transmitting substrate 10 can suppress the occurrence of optical distortion by adjusting surface characteristics such as flatness and roughness.
[0070] The light-shielding film 20 may be located on the top side of the light-transmitting substrate 10 .
[0071] The light-shielding film 20 may have a property of blocking at least a certain portion of the exposure light incident on the bottom side of the light-transmitting substrate 10. In addition, a phase shifting film 30 (see FIG. 5) or the like may be located between the light-transmitting substrate 10 and the light-shielding film 20. In this case, the light-shielding film 20 may be used as an etching mask in a process of etching the phase shifting film 30 or the like according to a pattern shape.
[0072] The light-shielding film 20 contains a transition metal and at least one of oxygen and nitrogen.
[0073] The light-shielding film 20 includes a first light-shielding layer 21 and a second light-shielding layer 22 disposed on the first light-shielding layer 21 .
[0074] Loss area of light-shielding film pattern edge
[0075] The loss area of the pattern edge measured by patterning the light-shielding film was 10 nm 2 The following is the result.
[0076] The pattern edge loss area is the area surrounded by the first line, the second line, and the pattern edge profile of the light-shielding pattern film when a TEM (Transmission Electron Microscopy) image of the light-shielding pattern film formed by patterning the light-shielding film is measured and the TEM image is observed.
[0077] The first line is an extension line connecting a first point located at a height of 20% and a second point located at a height of 40% in the side profile of the light-shielding pattern film, when the total height of the light-shielding pattern film is 100%.
[0078] The second line is an extension line that includes the pattern film intersection point and is disposed parallel to the upper surface of the light-transmitting substrate.
[0079] The pattern film intersection point is a point where the center line of the pattern film intersects with the top surface profile of the light-shielding pattern film.
[0080] The pattern film center line is an extension line that passes through the pattern film center point, which is the center point of the bottom surface of the light-shielding pattern film, and is perpendicular to the upper surface of the light-transmitting substrate.
[0081] The light-shielding film 20 can be etched through a resist pattern or an etching mask film disposed on the light-shielding film 20. The closer the side profile of the light-shielding pattern film formed after etching is to a surface of the light-transmitting substrate 10 disposed below the light-shielding pattern film, the higher the resolution of the photomask 200 can be. If the side profile of the light-shielding pattern film is not precisely controlled, the CD (Critical Dimension) deviation of the pattern developed on the semiconductor wafer may become larger.
[0082] In the embodiment, a light-shielding film 20 may be provided that can precisely control the side profile of the light-shielding pattern film formed during patterning by adjusting the loss area of the pattern edge of the light-shielding film 20.
[0083] 2 is a conceptual diagram illustrating a method for measuring the loss area of a pattern edge of a light-shielding film, and an embodiment will be described below with reference to FIG.
[0084] The light-shielding film is patterned to form a light-shielding pattern film 23 .
[0085] Then, a test piece is prepared by processing the substrate including the light-shielding pattern film 23 to a size of 15 mm in width and 15 mm in length. The surface of the test piece is subjected to FIB (Focused Ion Beam) processing, and then the test piece is placed in a TEM image measuring device to measure the TEM image of the test piece.
[0086] For example, the TEM image can be measured using a JEM-2100F HR model manufactured by JEOL LTD.
[0087] Hereinafter, in the side profile of the light-shielding pattern film 23 observed in the TEM image, when the total height of the light-shielding pattern film 23 is taken as 100%, a first point p1 located at a height of 20% and a second point p2 located at a height of 40% are identified, and an extension line connecting the two points is identified. The extension line is defined as a first line L1.
[0088] The pattern film center point p c A pattern film intersection point p is a point where a pattern film center line L0 that passes through the light transmitting substrate 10 and is perpendicular to the light transmitting substrate 10 intersects with the upper surface profile. i The pattern film intersection p i and an extension line disposed parallel to the light-transmitting substrate 10. The extension line is defined as a second line L2.
[0089] The pattern edge loss area Ap is defined as the area surrounded by the first line L1, the second line L2, and the pattern edge profile of the light-shielding pattern film 23. The pattern edge loss area Ap is measured from the TEM image.
[0090] The loss area Ap of the pattern edge of the light-shielding film 20 is 10 nm 2 The loss area Ap of the pattern edge of the light-shielding film 20 may be 8 nm or less. 2 The loss area Ap of the pattern edge of the light-shielding film 20 may be 6 nm or less. 2 The loss area Ap of the pattern edge of the light-shielding film 20 may be 0.5 nm or less. 2 In such a case, it is possible to realize a photomask 200 in which the decrease in resolution is effectively suppressed from the blank mask 100.
[0091] Layer density of light-shielding film The light-shielding film 20 has an Rd value of 0.4 to 0.8 in the following formula 1.
[0092] [Formula 1] JPEG0007554885000001.jpg916
[0093] In the formula 1, the er1 value is the etching rate of the first light-shielding layer 21 measured by etching with argon gas.
[0094] The er2 value is the etching rate of the second light-shielding layer 22 measured by etching with argon gas.
[0095] In the process of patterning the light-shielding film 20, the upper side of the side of the light-shielding pattern film may be exposed to the etching gas for a relatively long time compared to the lower side. As a result, more etching than necessary may occur in the in-plane direction of the light-shielding film 20 in the upper region of the side of the light-shielding pattern film. This may make it difficult for the side of the light-shielding pattern film to form an angle close to perpendicular to the surface of the light-transmitting substrate 10.
[0096] In order to solve the above problem, a method may be considered in which the transition metal content of the second light-shielding layer 22 is adjusted to have a relatively larger value than that of the first light-shielding layer 21, and the etching rate of the second light-shielding layer 22 by the etchant is controlled to have a lower value than that of the first light-shielding layer 21. However, even if the degree of damage formed at the edge of the second light-shielding layer 22 is reduced by applying this method, the damage formed at the edge may still cause problems related to the resolution of the photomask due to the trend of the required line width becoming finer and finer. In addition, if the transition metal content included in the second light-shielding layer 22 is adjusted only with consideration given to the precise control of the side profile of the light-shielding pattern film, a decrease in the etching rate of the light-shielding film and defects due to chromium migration may occur. That is, in addition to controlling the composition content of each layer of the light-shielding film, it is necessary to control other characteristics, including the degree of denseness of each layer, to more precisely control the side profile of the light-shielding pattern film formed through the patterning process.
[0097] Meanwhile, the etching gas used in patterning the light-shielding film 20 undergoes a chemical reaction with the light-shielding film 20. Therefore, the etching rate of each layer in the light-shielding film 20 measured using the etching gas may be significantly affected by the reactivity of the elements constituting each layer with the etching gas. The inventors of the embodiment have determined that it is difficult for the value measured using the etching gas to directly reflect the degree of density of each layer.
[0098] On the other hand, etching using argon gas corresponds to physical etching that does not substantially involve a chemical reaction with the etching target, light-shielding film 20. Therefore, the etching rate measured by etching using argon gas under all other conditions being the same is independent of the composition, chemical reactivity, etc. of each layer in the light-shielding film 20, and is considered to be a parameter that can effectively reflect the degree of denseness of each layer in the light-shielding film 20.
[0099] Therefore, the inventors of the embodiment have confirmed that by controlling the Rd value, which can reflect the degree to which the first light-shielding layer 21 and the second light-shielding layer 22 are densely formed, the side profile of the light-shielding pattern film formed when the light-shielding film 20 is patterned can be more precisely controlled.
[0100] The er1 value, er2 value, and Rd value can be controlled by various factors. Specifically, the values can be influenced by various factors such as the density of the light-shielding layer, the degree of crystallization of the elements contained in the light-shielding layer, the content of non-metallic elements in the light-shielding layer, and the arrangement of each constituent element in the light-shielding layer. In particular, the values can change during deposition of each layer in the light-shielding film 20 depending on process conditions such as the rotation speed of the magnet, and post-process conditions such as cooling after deposition. A detailed explanation of the means for controlling the Rd value will be omitted as it overlaps with the contents below.
[0101] The method for measuring the Rd value of the light-shielding film 20 is as follows.
[0102] First, the thicknesses of the first light-shielding layer 21 and the second light-shielding layer 22 are measured using a TEM (Transmission Electron Microscopy). A blank mask 100 to be measured is processed to a size of 15 mm wide and 15 mm long to prepare a test piece. The surface of the test piece is subjected to a FIB (Focussed Ion Beam) treatment, and then the test piece is placed in a TEM image measuring device to measure a TEM image of the test piece. The thicknesses of the first light-shielding layer 21 and the second light-shielding layer 22 are calculated from the TEM image.
[0103] For example, the TEM image can be measured using a JEM-2100F HR model manufactured by JEOL LTD.
[0104] The test piece is then etched with argon gas to measure the etching time of the first light-shielding layer 21 and the second light-shielding layer 22. The test piece is placed in an XPS (X-ray Photoelectron Spectroscopy) measurement device, and an area of 4 mm in width and 2 mm in length located in the center of the test piece is etched with argon gas to measure the etching time for each layer. When measuring the etching time for each layer, the degree of vacuum in the measurement device was 1.0×10 -8 The X-ray source was a Monochromator Al Kα (1486.6 eV), the anode power was 72 W, the anode voltage was 12 kV, and the argon ion beam voltage was 1 kV.
[0105] For example, the XPS measurement equipment may be a K-Alpha model manufactured by Thermo Scientific.
[0106] The er1 value, the er2 value, and the Rd value are calculated from the measured thicknesses and etching rates of the first light-shielding layer 21 and the second light-shielding layer 22.
[0107] The Rd value of the light-shielding film 20 may be 0.4 to 0.8. The Rd value of the light-shielding film 20 may be 0.5 to 0.77. The Rd value of the light-shielding film 20 may be 0.6 to 0.8. The Rd value of the light-shielding film 20 may be 0.6 to 0.7. In such cases, the side profile of the light-shielding pattern film in which the light-shielding film is patterned can be controlled more precisely.
[0108] The er2 value of the light-shielding film 20 may be 0.4 to 0.5 Å / s. The er2 value of the light-shielding film 20 may be 0.4 to 0.47 Å / s. The er2 value of the light-shielding film 20 may be 0.42 to 0.45 Å / s. In such cases, the Rd value of the light-shielding film 20 can be more easily controlled within a preset range in accordance with an embodiment, and the formation of particles due to redeposition of sputtered particles, which will be described in detail below, can be effectively suppressed.
[0109] The er1 value of the light-shielding film 20 may be 0.51 Å / s or more. The er1 value of the light-shielding film 20 may be 0.55 Å / s or more. The er1 value of the light-shielding film 20 may be 0.6 Å / s or more. The er1 value of the light-shielding film 20 may be 1.0 Å / s or less. The er1 value of the light-shielding film 20 may be 0.8 Å / s or less. The er1 value of the light-shielding film 20 may be 0.7 Å / s or less. In such cases, the Rd value of the light-shielding film can be adjusted more easily, and at the same time, etching of the light-shielding film can be performed more efficiently.
[0110] Optical properties of light-shielding film The light-shielding film 20 may have a Do value of less than 0.05 in the following formula 2.
[0111] [Formula 2] Do=Bo-Po
[0112] In the formula 2, the Bo value is the optical density of the light-shielding film 20 measured by irradiating it with exposure light having a wavelength of 193 nm.
[0113] The Po value is the optical density measured by irradiating exposure light having a wavelength of 193 nm onto a measurement area corresponding to a region from one edge (Le) (see FIG. 3) formed by patterning the light-shielding pattern film to a position 4 nm away inward of the light-shielding pattern film when the light-shielding pattern film formed by patterning the light-shielding film 20 is observed from above.
[0114] 3 is a conceptual diagram illustrating a light-shielding pattern film formed by patterning a light-shielding film of a blank mask to be measured. Hereinafter, an embodiment will be described with reference to FIG.
[0115] The light-shielding pattern film 23 is formed by patterning a light-shielding film. The side of the light-shielding pattern film 23 (yz plane of the light-shielding pattern film) is usually formed by etching unless it is the side of the blank mask itself. The upper region of the side formed by the etching (the region located on the upper side in the z-axis direction in the yz plane of the light-shielding pattern film) is exposed to the etchant for a longer time, so that more etching may occur than the lower region of the side (the region located on the lower side in the z-axis direction in the yz plane of the light-shielding pattern film). As a result, the portions adjacent to both ends of the light-shielding pattern film 23 (the edges of the light-shielding pattern film located in the x-axis direction) may be formed with a relatively thin thickness compared to the center of the light-shielding pattern film 23 (the portion located at the center of the light-shielding pattern film in the x-axis direction). As a result, the extinction characteristics of the light-shielding pattern film 23 in the in-plane direction may vary. The embodiment may provide a blank mask that effectively suppresses the decrease in resolution due to patterning by controlling the Do value of the light-shielding film.
[0116] In order to control the Do value of the light-shielding film 20, it is necessary to control the density of the layers themselves contained in the light-shielding film so that differences occur, along with other conditions of each layer in the light-shielding film 20. This density can be influenced not only by the composition, but also by the process conditions during sputtering, the conditions of post-processing steps such as the cooling step after sputtering, and the like. The explanation of the control means is omitted here because it overlaps with the contents below.
[0117] 4 is a plan view of a light-shielding pattern film formed by patterning a light-shielding film, as viewed from above. Hereinafter, an embodiment will be described with reference to FIG.
[0118] The Bo value is measured by irradiating the surface of the light-shielding film before patterning with exposure light having a wavelength of 193 nm. When another thin film (e.g., a hard mask) is formed on the light-shielding film, the other thin film is removed by etching, and then the Bo value is measured. When the other thin film formed on the light-shielding film is etched, the difference between the thickness of the light-shielding film before etching and the thickness of the light-shielding film after etching should be within 3 nm.
[0119] Thereafter, Po is measured for the light-shielding pattern film 23 formed by patterning the light-shielding film. When the light-shielding pattern film 23 is observed from above, a region corresponding to a region from one edge (Le) formed by patterning the light-shielding pattern film 23 to a position 4 nm away inward of the light-shielding pattern film 23 is defined as a measurement region (Am). The measurement region (Am) is irradiated with exposure light having a wavelength of 193 nm to measure the Po value.
[0120] The Do value is calculated from the measured Bo value and Po value.
[0121] The Bo value and the Po value can be measured by an ellipsometer, for example, the MG Pro model manufactured by Nanoview Corporation.
[0122] The Do value of the light-shielding film 20 may be less than 0.05. The Do value of the light-shielding film 20 may be 0.04 or less. The Do value of the light-shielding film 20 may be 0.03 or less. The Do value of the light-shielding film 20 may be 0.02 or less. The Do value of the light-shielding film 20 may be 0.01 or more. In such cases, a decrease in the resolution of the blank mask 100 due to patterning of the light-shielding film 20 can be effectively suppressed.
[0123] The Bo value of the light-shielding film 20 may be 1.8 or more. The Bo value of the light-shielding film 20 may be 1.85 or more. The Bo value of the light-shielding film 20 may be 3 or less. In such cases, the thin film laminate including the light-shielding film 20 can effectively block the transmission of exposure light.
[0124] The Po value of the light-shielding film 20 may be 1.8 or more. The Po value of the light-shielding film 20 may be 1.82 or more. The Po value of the light-shielding film 20 may be 3 or less. The Po value of the light-shielding film 20 may be 2 or less. The Po value of the light-shielding film 20 may be 1.9 or less. In such cases, it is possible to effectively help suppress a decrease in the resolution of the blank mask 100.
[0125] The transmittance of the light-shielding film 20 for light with a wavelength of 193 nm may be 1% or more. The transmittance of the light-shielding film 20 for light with a wavelength of 193 nm may be 1.3% or more. The transmittance of the light-shielding film 20 for light with a wavelength of 193 nm may be 1.4% or more. The transmittance of the light-shielding film 20 for light with a wavelength of 193 nm may be 2% or less. In such cases, the thin film including the light-shielding film 20 can effectively suppress the transmission of the exposure light.
[0126] Etching characteristics of light-shielding film The etching rate of the light-shielding film 20 with respect to a chlorine-based gas may be 1.55 Å / s or more.
[0127] In order to improve the resolution of the blank mask 100, it may be necessary to thin the resist film or etching mask film disposed on the light-shielding film 20. By controlling the etching speed of the light-shielding film 20 with respect to the etchant when patterning the light-shielding film 20, it is possible to pattern the light-shielding film 20 even if a relatively thin resist film or the like is formed on the light-shielding film 20.
[0128] A chlorine-based gas may be included as an etchant for the light-shielding film 20. The chlorine-based gas may include chlorine gas (Cl2) and oxygen gas (O2).
[0129] The etching characteristics of the light-shielding film 20 with respect to chlorine-based gases can be controlled by the density of each layer of the light-shielding film 20, the elemental content distribution in the thickness direction of the light-shielding film 20, the process conditions during deposition of the light-shielding film 20, the cooling rate after deposition, and the like.
[0130] The etching rate of the light-shielding film 20 with respect to a chlorine-based gas is measured as follows.
[0131] First, the thickness of the light-shielding film 20 is measured by measuring a TEM image of the light-shielding film 20. A blank mask 100 to be measured is processed to a size of 15 mm in width and 15 mm in length to prepare a test piece. The surface of the test piece is treated with a Focused Ion Beam (FIB), and then the test piece is placed in a TEM image measuring device to measure the TEM image of the test piece. The thickness of the light-shielding film 20 is calculated from the TEM image.
[0132] For example, the TEM image can be measured using a JEM-2100F HR model manufactured by JEOL LTD.
[0133] Thereafter, the etching time of the light-shielding film 20 with respect to the chlorine-based gas is measured. As the chlorine-based gas, a gas containing 90 to 95% by volume of chlorine gas and 5 to 10% by volume of oxygen gas is applied. From the thickness of the light-shielding film 20 and the etching time of the light-shielding film 20, the etching rate of the light-shielding film 20 with respect to the chlorine-based gas is calculated.
[0134] The etching rate of the light-shielding film 20 with respect to the chlorine-based gas may be 1.55 Å / s or more. The etching rate may be 1.6 Å / s or more. The etching rate may be 1.7 Å / s or more. The etching rate may be 3 Å / s or less. In such a case, the resist film disposed on the light-shielding film 20 can be made thinner, which can contribute to effectively suppressing a decrease in the resolution of the blank mask 100.
[0135] Composition and thickness of the light-shielding film The light-shielding film 20 may contain a transition metal and at least one of oxygen and nitrogen.
[0136] The light-shielding film 20 may include a first light-shielding layer 21 and a second light-shielding layer 22 located on the first light-shielding layer 21 .
[0137] In the embodiment, by controlling the content of each element contained in the second light-shielding layer 22, the light-shielding film 20 can be helped to exhibit the desired extinction characteristics, and when the light-shielding film 20 is patterned, the side profile of the light-shielding pattern film 23 can form an angle close to perpendicular to the light-transmitting substrate.
[0138] The second light-shielding layer 22 may contain a transition metal and at least one of oxygen and nitrogen. The second light-shielding layer 22 may contain 50 to 80 at % of the transition metal. The second light-shielding layer 22 may contain 55 to 75 at % of the transition metal. The second light-shielding layer 22 may contain 60 to 70 at % of the transition metal.
[0139] The content of the element corresponding to oxygen or nitrogen in the second light-shielding layer 22 may be 10 to 35 at %. The content of the element corresponding to oxygen or nitrogen in the second light-shielding layer 22 may be 15 to 25 at %.
[0140] The second light-shielding layer 22 may contain nitrogen at 5 to 20 at %. The second light-shielding layer 22 may contain nitrogen at 7 to 13 at %.
[0141] In this case, the second light-shielding layer 22 can help the light-shielding film 20 to have excellent extinction properties. In addition, the side profile of the light-shielding pattern film formed by patterning the light-shielding film 20 can be more precisely controlled.
[0142] The first light-shielding layer 21 may contain a transition metal, oxygen, and nitrogen. The first light-shielding layer 21 may contain 30 to 60 at % of the transition metal. The first light-shielding layer 21 may contain 35 to 55 at % of the transition metal. The first light-shielding layer 21 may contain 40 to 50 at % of the transition metal.
[0143] The combined oxygen and nitrogen content of the first light-shielding layer 21 may be 40 to 70 at %. The combined oxygen and nitrogen content of the first light-shielding layer 21 may be 45 to 65 at %. The combined oxygen and nitrogen content of the first light-shielding layer 21 may be 50 to 60 at %.
[0144] The first light-shielding layer 21 may contain 20 to 40 at % of oxygen.The first light-shielding layer 21 may contain 23 to 33 at % of oxygen.The first light-shielding layer 21 may contain 25 to 30 at % of oxygen.
[0145] The first light-shielding layer 21 may contain nitrogen at 5 to 20 at %. The first light-shielding layer 21 may contain nitrogen at 7 to 17 at %. The first light-shielding layer 21 may contain nitrogen at 10 to 15 at %.
[0146] In this case, the first light-shielding layer 21 can help the light-shielding film 20 to have excellent light-extinguishing properties and can help improve the etching rate of the light-shielding film 20.
[0147] The transition metal may include at least one of Cr, Ta, Ti, and Hf. The transition metal may be Cr.
[0148] The film thickness of the first light-shielding layer 21 may be 250 to 650 Å. The film thickness of the first light-shielding layer 21 may be 350 to 600 Å. The film thickness of the first light-shielding layer 21 may be 400 to 550 Å. In such cases, the first light-shielding layer 21 can help the light-shielding film 20 to effectively block the exposure light.
[0149] The second light-shielding layer 22 may have a thickness of 30 to 200 Å. The second light-shielding layer 22 may have a thickness of 30 to 100 Å. The second light-shielding layer 22 may have a thickness of 40 to 80 Å. In such cases, the second light-shielding layer 22 can improve the extinction characteristics of the light-shielding film 20 and help to more precisely control the side profile of the light-shielding pattern film.
[0150] The ratio of the thickness of the second light-shielding layer 22 to the thickness of the first light-shielding layer 21 may be 0.05 to 0.3. The thickness ratio may be 0.07 to 0.25. The thickness ratio may be 0.1 to 0.2. In such a case, the light-shielding film 20 has sufficient extinction properties, while being able to form a side profile that is nearly perpendicular to the surface of the light-transmitting substrate during patterning.
[0151] Other thin films 5 is a conceptual diagram illustrating a blank mask according to another embodiment of the present disclosure, with reference to FIG.
[0152] The phase shift film 30 may be located between the light-transmitting substrate 10 and the light-shielding film 20. The phase shift film 30 is a thin film that attenuates the light intensity of the exposure light passing through the phase shift film 30, adjusts the phase difference, and substantially suppresses diffracted light generated at the edge of the pattern.
[0153] The phase shift film 30 may have a phase difference of 170 to 190° with respect to light having a wavelength of 193 nm. The phase shift film 30 may have a phase difference of 175 to 185° with respect to light having a wavelength of 193 nm. The phase shift film 30 may have a transmittance of 3 to 10% with respect to light having a wavelength of 193 nm. The phase shift film 30 may have a transmittance of 4 to 8% with respect to light having a wavelength of 193 nm. In such cases, the resolution of the photomask 200 including the phase shift film 30 can be improved.
[0154] The phase shifter film 30 may include a transition metal and silicon. The phase shifter film 30 may include a transition metal, silicon, oxygen, and nitrogen. The transition metal may be molybdenum.
[0155] The explanation of the light-transmitting substrate 10 and the light-shielding film 20 is omitted since it overlaps with the contents described above.
[0156] A hard mask (not shown) may be positioned on the light-shielding layer 20. The hard mask may function as an etching mask layer when pattern-etching the light-shielding layer 20. The hard mask may include silicon, nitrogen, and oxygen.
[0157] Photomask 6 is a conceptual diagram illustrating a photomask according to another embodiment of the present disclosure, and a photomask according to the embodiment will be described with reference to FIG.
[0158] A photomask 200 according to another embodiment of the present specification includes a light-transmitting substrate 10 and a light-shielding pattern film 25 located on the light-transmitting substrate 10 .
[0159] The light-shielding pattern film 25 contains a transition metal and at least one of oxygen and nitrogen.
[0160] The light-shielding pattern film 25 includes a first light-shielding layer 21 and a second light-shielding layer 22 disposed on the first light-shielding layer 21 .
[0161] The light-shielding pattern film 25 has an Rd value of 0.4 to 0.8 in the following formula 1.
[0162] [Formula 1] JPEG0007554885000002.jpg1117
[0163] In the formula 1, the er1 value is the etching rate of the first light-shielding layer 21 measured by etching with argon gas.
[0164] The er2 value is the etching rate of the second light-shielding layer 22 measured by etching with argon gas.
[0165] The light-shielding pattern film 25 can be formed by patterning the light-shielding film 20 of the blank mask 100 described above.
[0166] The method for measuring the Rd value of the light-shielding pattern film 25 is the same as the method for measuring the Rd value of the light-shielding film 20 in the blank mask 100.
[0167] The loss area of the pattern edge of the light-shielding pattern film 25 is 10 nm 2 It may be the following.
[0168] The method for measuring the loss area of the pattern edge of the light-shielding pattern film 25 is the same as the method for measuring the loss area of the pattern edge of the light-shielding film 20, except that the process of patterning the light-shielding film 20 is omitted.
[0169] The light-shielding pattern film 25 may have a PDo value of the following formula 3 that is less than 0.05.
[0170] [Formula 3] PDo=PBo-PPo
[0171] In the formula 3, the PBo value is the optical density of the light-shielding pattern film 25 measured by irradiating it with exposure light having a wavelength of 193 nm.
[0172] The PPo value is the average optical density measured by irradiating an exposure light having a wavelength of 193 nm onto a measurement area corresponding to a region from one edge of the light-shielding pattern film 25 to a position 4 nm away inward of the light-shielding pattern film 25 when the light-shielding pattern film 25 is observed from above.
[0173] The one edge means an edge of the light-shielding pattern film 25 that is formed by etching.
[0174] The methods for measuring the PDo value, PBo value, and PPo value of the light-shielding pattern film 25 are the same as the methods for measuring the Do value, Bo value, and Po value of the light-shielding film 20. However, the process of patterning the light-shielding film is omitted when measuring the PDo value, PBo value, and PPo value of the light-shielding pattern film 25. In addition, when measuring the PBo value, the surface to be measured is the surface of the light-shielding pattern film 25, not the light-shielding film before patterning.
[0175] The physical properties, composition, structure, etc. of the light-shielding pattern film 25 will be omitted since they overlap with the description of the light-shielding film of the blank mask.
[0176] Manufacturing method of light-shielding film A method for manufacturing a blank mask according to an embodiment of the present disclosure may include a preparation step of placing a light-transmitting substrate, a sputtering target, and a magnet in a sputtering chamber.
[0177] A manufacturing method of a blank mask according to an embodiment of the present specification may include a deposition step of injecting an atmospheric gas into a sputtering chamber, controlling the rotation speed of a magnet, and applying power to a sputtering target to deposit a light-shielding film on a light-transmitting substrate.
[0178] The method for manufacturing a blank mask according to an embodiment of the present specification may include a heat treatment step of performing heat treatment at 150 to 330° C. for 5 to 30 minutes.
[0179] The method for manufacturing a blank mask according to an embodiment of the present disclosure may include a cooling step of cooling the light-shielding film that has been subjected to the heat treatment step.
[0180] The method for producing a blank mask according to an embodiment of the present specification may include a stabilization step of stabilizing the blank mask after the cooling step at 30 to 50° C. for 1 to 5 minutes.
[0181] The film forming step includes a first light-shielding layer forming process of forming a first light-shielding layer on a light-transmitting substrate, and a second light-shielding layer forming process of forming a second light-shielding layer on the first light-shielding layer.
[0182] In the preparation step, a target for forming the light-shielding film can be selected in consideration of the composition of the light-shielding film. The sputtering target may be one target containing a transition metal. The sputtering target may be two or more targets including one target containing a transition metal. The target containing a transition metal may contain 90 at% or more of the transition metal. The target containing a transition metal may contain 95 at% or more of the transition metal. The target containing a transition metal may contain 99 at% of the transition metal.
[0183] The transition metal may include at least one of Cr, Ta, Ti, and Hf. The transition metal may include Cr.
[0184] The light-transmitting substrate disposed in the sputtering chamber will not be described here since it is the same as that described above.
[0185] In a preparation step, a magnet can be placed in the sputtering chamber, the magnet being positioned on a surface of the sputtering target opposite the surface on which sputtering occurs.
[0186] In the step of forming the light-shielding film, different film forming process conditions may be applied when forming each layer included in the light-shielding film. In particular, various process conditions such as the composition of the atmospheric gas, the pressure in the chamber, the power applied to the sputtering target, the rotation speed of the magnet, the film forming time, and the rotation speed of the substrate may be applied to each layer in consideration of the extinction characteristic and etching characteristic of the light-shielding film.
[0187] The atmospheric gas may include an inert gas, a reactive gas, and a sputtering gas. The inert gas is a gas containing an element that does not constitute the thin film to be formed. The reactive gas is a gas containing an element that constitutes the thin film to be formed. The sputtering gas is a gas that is ionized in a plasma atmosphere and collides with a target. The inert gas may include helium. The reactive gas may include a gas containing nitrogen. The nitrogen-containing gas may be, for example, N2, NO, NO2, N2O, N2O3, N2O4, N2O5, etc. The reactive gas may include a gas containing oxygen. The oxygen-containing gas may be, for example, O2, CO2, etc. The reactive gas may include a gas containing nitrogen and a gas containing oxygen. The reactive gas may include a gas containing both nitrogen and oxygen. The nitrogen-containing gas may be, for example, NO, NO2, N2O, N2O3, N2O4, N2O5, etc.
[0188] The sputtering gas may be argon (Ar) gas.
[0189] The power source for applying power to the sputtering target may be a DC power source or an RF power source.
[0190] In the step of forming the light-shielding film, the rotation speed of the magnet can be adjusted. The rotation speed of the magnet can affect the distribution area of the plasma formed in the sputtering chamber. Specifically, the faster the rotation speed of the magnet, the more the plasma tends to be formed around the sputtering target, and the slower the rotation speed of the magnet, the more the plasma tends to be formed around the light-transmitting substrate.
[0191] The density of the thin film formed may vary depending on the position of the plasma formed in the sputtering chamber. The closer the plasma is formed to the periphery of the sputtering target, the more the number of collisions between argon ions and one surface of the sputtering target increases, and the thinner the thin film tends to be. When the rotation speed of the magnet is controlled in consideration of such plasma characteristics, the density of the first and second light-shielding layers formed in the light-shielding film can be relatively easily controlled.
[0192] In the process of forming the first light-shielding layer, the power applied to the sputtering target may be 1.5 to 2.5 kW, or 1.6 to 2 kW.
[0193] In the process of forming the first light-shielding layer, the ratio of the flow rate of the reactive gas to the flow rate of the inert gas in the atmospheric gas may be 1.5 to 3. The flow rate ratio may be 1.8 to 2.7. The flow rate ratio may be 2 to 2.5.
[0194] The ratio of the oxygen content to the nitrogen content contained in the reactive gas may be 1.5 to 4. The ratio of the oxygen content to the nitrogen content contained in the reactive gas may be 2 to 3. The ratio of the oxygen content to the nitrogen content contained in the reactive gas may be 2.2 to 2.7.
[0195] In this case, the first light-shielding layer can help the light-shielding film to have sufficient extinction properties, and the etching properties of the first light-shielding layer can be controlled to help the side profile of the light-shielding pattern film after patterning to have a shape close to perpendicular to the surface of the light-transmitting substrate.
[0196] In the process of forming the first light-shielding layer, the rotation speed of the magnet may be set to 90 to 140 rpm. In the process of forming the first light-shielding layer, the rotation speed of the magnet may be set to 100 to 120 rpm. In such a case, it is possible to help improve the etching speed of the first light-shielding layer.
[0197] The deposition time of the first light-shielding layer may be 200 to 300 seconds. The deposition time of the first light-shielding layer may be 210 to 240 seconds. In such a case, the first light-shielding layer can help the light-shielding film to have sufficient extinction properties.
[0198] In the process of forming the second light-shielding layer, the power applied to the sputtering target may be 1 to 2 kW. In the process of forming the second light-shielding layer, the power applied to the sputtering target may be 1.2 to 1.7 kW. In such a case, it can contribute to the second light-shielding layer having a density within a preset range.
[0199] In the process of forming the second light-shielding layer, the ratio of the flow rate of the reactive gas to the flow rate of the inert gas in the atmospheric gas may be 0.3 to 0.8, or the flow rate ratio may be 0.4 to 0.6.
[0200] In the process of forming the second light-shielding layer, the ratio of the oxygen content to the nitrogen content contained in the reactive gas may be 0.3 or less. The ratio of the oxygen content to the nitrogen content contained in the reactive gas may be 0.1 or less. The ratio of the oxygen content to the nitrogen content contained in the reactive gas may be 0.001 or more.
[0201] In this case, the density of the second light-shielding layer is controlled, so that the side of the light-shielding pattern film formed through patterning can have a profile that is relatively close to perpendicular to the surface of the light-transmitting substrate.
[0202] The rotation speed of the magnet may be adjusted during the deposition of the second light-shielding layer. If the rotation speed of the magnet is controlled only in consideration of suppressing excessive etching that may occur on the side of the second light-shielding layer in the light-shielding pattern film during patterning of the light-shielding film, sputtering particles generated from the sputtering target may be redeposited on the surface of the sputtering target instead of being deposited on the surface of the film-forming target. The redeposited sputtering particles may act as a particle source and cause a decrease in the resolution of the blank mask. In the embodiment, the rotation speed of the magnet is controlled within a preset range during the deposition of the second light-shielding layer, so that the side profile of the light-shielding pattern film can be precisely controlled during patterning of the light-shielding film, and the formation of particles can be effectively suppressed.
[0203] In the process of forming the second light-shielding layer, the rotation speed of the magnet may be set to 100 to 150 rpm. In the process of forming the second light-shielding layer, the rotation speed of the magnet may be set to 110 to 140 rpm. In such a case, when the light-shielding film is patterned, the side profile of the light-shielding pattern film can be precisely controlled, and a decrease in the resolution of the pattern due to particles can be suppressed.
[0204] The deposition time for the second light-shielding layer may be 10 to 30 seconds. The deposition time for the second light-shielding layer may be 15 to 25 seconds. In such a case, the second light-shielding layer can help the side surface of the patterned light-shielding film to form an angle close to perpendicular to the surface of the light-transmitting substrate.
[0205] In the heat treatment step, the light-shielding film after the film formation step can be heat-treated. Specifically, the substrate after the light-shielding film formation step can be placed in a heat treatment chamber and then heat-treated.
[0206] In the heat treatment step, the atmospheric temperature may be 150 to 300° C. The atmospheric temperature may be 170 to 280° C. The atmospheric temperature may be 200 to 250° C.
[0207] In the heat treatment step, the heat treatment time may be 5 to 25 minutes. The heat treatment time may be 10 to 20 minutes. In such a case, the stress formed in the light-shielding film can be effectively reduced.
[0208] The blank mask can be subjected to a cooling step within 2 minutes after the heat treatment step is completed, which can suppress the growth of transition metal particles contained in the light-shielding film due to heating.
[0209] In the cooling step, the light-shielding film can be cooled using a cooling plate. Specifically, a cooling plate adjusted to a preset cooling temperature can be placed on the substrate side of the blank mask after the heat treatment step to cool the blank mask. In the cooling step, the cooling speed of the blank mask can be controlled by adjusting the distance between the blank mask and the cooling plate.
[0210] In the cooling step, the cooling temperature applied to the cooling plate may be 10 to 40° C. The cooling temperature may be 20 to 30° C.
[0211] The cooling step may be carried out for 5 to 20 minutes. The cooling step may be carried out for 10 to 15 minutes.
[0212] In the cooling step, the distance between the blank mask and the cooling plate may be 0.01 to 30 mm, the distance may be 0.05 to 5 mm, or the distance may be 0.1 to 2 mm.
[0213] In the cooling step, the cooling rate of the blank mask may be 0.45 to 1° C. / s, or 0.5 to 0.8° C. / s.
[0214] In such a case, damage to the light-shielding film due to cooling can be substantially suppressed, and a decrease in the density of each layer in the light-shielding film, particularly the second light-shielding layer, due to the growth of transition metal particles contained in the light-shielding film after heat treatment can be effectively suppressed.
[0215] In the stabilization step, the blank mask that has undergone the cooling step can be stabilized. In the case of the blank mask that has undergone the cooling step, the sudden temperature change may cause considerable damage to the blank mask. In order to prevent this, the stabilization step may be necessary.
[0216] There may be various methods for stabilizing the blank mask after the cooling step. As one example, the blank mask after the cooling step may be separated from the cooling plate and then left in the air at room temperature for a predetermined time. As another example, the blank mask after the cooling step may be separated from the cooling plate and then stabilized at 30 to 50°C for 1 to 5 minutes. At this time, the blank mask may be rotated at 20 to 50 rpm for 1 to 5 minutes. As yet another example, a gas that does not react with the blank mask may be sprayed onto the blank mask after the cooling step at a flow rate of 5 to 10 L / min for 1 to 5 minutes. At this time, the gas that does not react with the blank mask may have a temperature of 20 to 40°C.
[0217] Method for manufacturing semiconductor device A method for manufacturing a semiconductor device according to another embodiment of the present specification includes a preparation step of arranging a light source, a photomask, and a semiconductor wafer coated with a resist film, an exposure step of selectively transmitting and emitting light incident from the light source through the photomask onto the semiconductor wafer, and a development step of developing a pattern on the semiconductor wafer.
[0218] The photomask includes a light-transmitting substrate and a light-shielding pattern film disposed on the light-transmitting substrate.
[0219] The light-shielding pattern film contains a transition metal and at least one of oxygen and nitrogen.
[0220] The light-shielding pattern film includes a first light-shielding layer and a second light-shielding layer disposed on the first light-shielding layer.
[0221] The light-shielding pattern film has an Rd value of 0.4 to 0.8 in the following formula 1.
[0222] [Formula 1] JPEG0007554885000003.jpg1117
[0223] In the formula 1, the er1 value is the etching rate of the first light-shielding layer measured by etching with argon gas.
[0224] The er2 value is the etching rate of the second light-shielding layer measured by etching with argon gas.
[0225] In the preparation step, the light source is a device capable of generating short-wavelength exposure light. The exposure light may be light with a wavelength of 200 nm or less. The exposure light may be ArF light with a wavelength of 193 nm.
[0226] A lens may be further disposed between the photomask and the semiconductor wafer. The lens has a function of reducing the shape of the circuit pattern on the photomask and transferring it onto the semiconductor wafer. The lens is not limited as long as it is generally applicable to the ArF semiconductor wafer exposure process. Exemplarily, the lens may be a lens made of calcium fluoride (CaF2).
[0227] In the exposure step, the exposure light can be selectively transmitted onto the semiconductor wafer through a photomask, and in such a case, chemical modification can occur in the portion of the resist film on which the exposure light is incident.
[0228] In the developing step, the semiconductor wafer after the exposure step can be treated with a developing solution to develop a pattern on the semiconductor wafer. If the applied resist film is a positive resist, the part of the resist film on which the exposure light is incident can be dissolved by the developing solution. If the applied resist film is a negative resist, the part of the resist film on which the exposure light is not incident can be dissolved by the developing solution. By treating with the developing solution, the resist film is formed as a resist pattern. A pattern can be formed on the semiconductor wafer using the resist pattern as a mask.
[0229] The explanation of the photomask will be omitted since it overlaps with the above content.
[0230] Specific examples will be described in more detail below.
[0231] Manufacturing example: Light-shielding film formation Example 1: A light-transmitting substrate made of quartz, measuring 6 inches wide, 6 inches long, and 0.25 inches thick, was placed in the chamber of a DC sputtering device. A chromium target was placed in the chamber so that the T / S distance was 255 mm and the angle between the substrate and the target was 25°. A magnet was installed behind the chromium target.
[0232] Thereafter, an atmospheric gas mixture of 21% Ar by volume, 11% N by volume, 32% CO by volume, and 36% He by volume was introduced into the chamber, and the power applied to the sputtering target was set to 1.85 kW and the magnet rotation speed was set to 113 rpm. A sputtering process was performed for 250 seconds to form a first light-shielding layer.
[0233] After completing the deposition of the first light-shielding layer, an atmospheric gas mixture of 57 volume percent Ar and 43 volume percent N2 was introduced into the chamber onto the first light-shielding layer, and a sputtering process was performed for 25 seconds with a power of 1.5 kW and a magnet rotation speed of 113 rpm applied to the sputtering target to form a second light-shielding layer, thereby producing a blank mask specimen.
[0234] The test piece after the second light-shielding layer was deposited was placed in a heat treatment chamber. Thereafter, the heat treatment was carried out for 15 minutes at an atmospheric temperature of 250°C. After the heat treatment, the blank mask was taken out of the heat treatment chamber and stabilized by rotating at 30 rpm for 2 minutes in an atmosphere of 40°C.
[0235] A cooling plate with a cooling temperature of 10 to 40° C. was installed on the substrate side of the blank mask that had been stabilized. The distance between the blank mask substrate and the cooling plate was 0.1 mm. The cooling step was performed for 5 to 20 minutes.
[0236] Example 2: A blank mask specimen was manufactured under the same conditions as in Example 1. However, when forming the first light-shielding layer, a gas mixture of 19 volume % Ar, 11 volume % N, 36 volume % CO, and 34 volume % He was used as the atmospheric gas.
[0237] Example 3: A blank mask specimen was manufactured under the same conditions as in Example 1. However, when forming the first light-shielding layer, a gas mixture of 17% by volume of Ar, 24% by volume of N2, 29% by volume of CO2, and 30% by volume of He was used as the atmospheric gas. In addition, when cooling the blank mask specimen, the distance between the surface of the blank mask substrate and the cooling plate was set to 2 mm.
[0238] Example 4: A blank mask specimen was manufactured under the same conditions as in Example 2. However, when forming the second light-shielding layer, the magnet rotation speed was set to 127 rpm. In addition, when cooling the blank mask specimen, the distance between the blank mask substrate and the cooling plate was set to 2 mm.
[0239] Example 5: A blank mask specimen was manufactured under the same conditions as in Example 4. However, the magnet rotation speed was set to 131 rpm when the first light-shielding layer was formed.
[0240] Example 6: A blank mask test piece was manufactured under the same conditions as in Example 2. However, when the blank mask test piece was cooled, the distance between the surface of the blank mask substrate and the cooling plate was set to 5 mm.
[0241] Comparative Example 1: A blank mask specimen was manufactured under the same conditions as in Example 1. However, when the second light-shielding layer was formed, 44 volume % of Ar and 56 volume % of N2 were used as the atmospheric gas.
[0242] Comparative Example 2: A blank mask specimen was produced under the same conditions as in Example 2. However, the magnet rotation speed was set to 89 rpm when the second light-shielding layer was formed.
[0243] Comparative Example 3: A blank mask test piece was manufactured under the same conditions as in Example 2. However, when the blank mask test piece was cooled, the distance between the surface of the blank mask substrate and the cooling plate was set to 10 mm.
[0244] Comparative Example 4: A blank mask test piece was manufactured under the same conditions as in Example 2. However, when the blank mask test piece was cooled, the distance between the surface of the blank mask substrate and the cooling plate was set to 20 mm.
[0245] The film formation, heat treatment and cooling conditions for each of the examples and comparative examples are shown in Table 1 below.
[0246] Evaluation example: Measuring the Rd value of a light-shielding film Each test piece in the examples and comparative examples was processed to a size of 15 mm in width and 15 mm in length. The surface of the processed test piece was treated with a focused ion beam (FIB), and then the test piece was placed in a JEOL Ltd. JEM-2100F HR model device to measure a TEM image of the test piece. The thicknesses of the first and second light-shielding layers were calculated from the TEM image.
[0247] The test piece was then etched with argon gas to measure the etching time of the first and second light-shielding layers. The test piece was placed in a Thermo Scientific K-Alpha model, and an area of 4 mm wide and 2 mm long located in the center of the test piece was etched with argon gas to measure the etching time for each layer. The degree of vacuum in the measurement equipment during the measurement of the etching time for each layer was 1.0×10 -8 The conditions were as follows: pressure, pressure drop, and pressure (MPa), the X-ray source was Monochromator Al Kα (1486.6 eV), the anode power was 72 W, the anode voltage was 12 kV, and the argon ion beam voltage was 1 kV.
[0248] The er1 value, er2 value, and Rd value were calculated from the measured thicknesses and etching rates of the first and second light-shielding layers. The er1 value, er2 value, and Rd value measured for each of the examples and comparative examples are shown in Table 2 below.
[0249] Evaluation example: Measurement of the optical properties of a light-shielding film Examples and Comparative Examples The optical density Bo value and transmittance for exposure light with a wavelength of 193 nm were measured from the surface of the light-shielding film of each test piece using an MG-Pro model manufactured by Nano View Co., Ltd.
[0250] Then, the light-shielding film was patterned to form a light-shielding pattern film. When the light-shielding pattern film was observed from above, a measurement region was measured, which corresponds to a region starting from one edge formed by patterning the light-shielding pattern film and corresponding to a region 4 nm away from the edge toward the inside of the light-shielding pattern film, using an MG-Pro model manufactured by Nano View Co., Ltd., with exposure light having a wavelength of 193 nm.
[0251] The Do value was calculated from the measured Bo and Po values.
[0252] The Do value, Bo value, Po value, and transmittance for light with a wavelength of 193 nm measured for each of the examples and comparative examples are shown in Table 2 below.
[0253] Evaluation example: Measurement of the etching characteristics of a light-shielding film The thickness of the light-shielding film was measured by measuring the TEM image of the light-shielding film included in each test piece in the examples and comparative examples. The test pieces were processed to a size of 15 mm in width and 15 mm in length. The surface of the processed test pieces was treated with FIB (Focused Ion Beam) and placed in a JEOL Ltd. JEM-2100F HR model device, and the TEM image of the test pieces was measured. The thickness of the light-shielding film was calculated from the TEM image.
[0254] Thereafter, the etching time of the light-shielding film with respect to the chlorine-based gas was measured. As the chlorine-based gas, a gas containing 90 to 95% by volume of chlorine gas and 5 to 10% by volume of oxygen gas was used. From the thickness of the light-shielding film and the etching time of the light-shielding film, the etching speed of the light-shielding film with respect to the chlorine-based gas was calculated.
[0255] The measured etching rates for the examples and comparative examples are shown in Table 2 below.
[0256] Evaluation example: Measurement of the loss area of the pattern edge of a light-shielding film The light-shielding film of each test piece in the examples and comparative examples was patterned to form a light-shielding pattern film. Then, the substrate including the light-shielding pattern film was processed to a size of 15 mm in width and 15 mm in length. The surface of the test piece was treated with FIB (Focused Ion Beam), and then placed in a JEM-2100F HR model device manufactured by JEOL LTD. The TEM image of the test piece was measured.
[0257] Thereafter, in the side profile of the light-shielding pattern film observed in the TEM image, a point located at a height of 20% and a point located at a height of 40% were identified, assuming the total height of the light-shielding pattern film to be 100%, and a first line, which is an extension line connecting these two points, was identified.
[0258] An intersection point between a straight line passing through the center of the light-shielding pattern film observed in the TEM image and the top surface profile was identified, and a second line was identified as an extension line that included the intersection point and was arranged parallel to the light-transmitting substrate.
[0259] From the TEM image, the pattern edge loss area, which is the area surrounded by the first line, the second line, and the pattern edge profile of the light-shielding pattern film, was measured.
[0260] The pattern edge loss area measured for each of the examples and comparative examples is shown in Table 2 below.
[0261] JPEG0007554885000004.jpg133165
[0262] JPEG0007554885000005.jpg137165
[0263] In Table 2, Examples 1 to 6 had Rd values of 0.4 to 0.8, whereas Comparative Examples 1 and 2 had Rd values of less than 0.4 or more than 0.8.
[0264] With regard to the Do value, Examples 1 to 6 showed values of less than 0.05, whereas all of the Comparative Examples showed values of 0.05 or more.
[0265] With regard to the transmittance, Examples 1 to 6 exhibited values of 1.55% or less, whereas Comparative Example 2 exhibited a value of 1.7% or more.
[0266] The etching rate in all of the examples and comparative examples was 1.6 Å / s or higher.
[0267] In terms of the loss area of the pattern edge, Examples 1 to 6 were 8 nm 2 The following values are shown, whereas all comparative examples are 8.5 nm. 2 The above values were shown.
[0268] Although the preferred embodiments have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the embodiments defined in the appended claims also fall within the scope of the present invention. [Explanation of symbols]
[0269] 100 Blank Mask 10 Light-transparent substrate 20 Light-shielding film 21 1st light shielding layer 22 Second light shielding layer 30 Phase inversion film 150 A mask formed by patterning the light-shielding film of the blank mask to be measured 23 Light-shielding pattern film obtained by patterning the light-shielding film of the blank mask to be measured 200 Photomasks 25 Light-shielding pattern film Le The edge formed by patterning in the light-shielding pattern film L1 1st line L2 second line L0 pattern membrane centerline p1 1st point p2 second point p c Pattern membrane center point p i Patterned Membrane Intersection Ap Pattern edge loss area Am measurement area
Claims
1. A light-transmitting substrate and a light-shielding film disposed on the light-transmitting substrate, the light-shielding film contains a transition metal and at least one of oxygen and nitrogen, the light-shielding film includes a first light-shielding layer and a second light-shielding layer disposed on the first light-shielding layer, The film thickness of the first light-shielding layer 21 is 250 to 650 Å. The thickness of the second light-shielding layer 22 is 30 to 200 Å. The light-shielding film was patterned and the loss area of the pattern edge was measured to be 10 nm 2 is as follows: A blank mask, in which the light-shielding film has a Do value of less than 0.05 as determined by the following formula 2: The pattern edge loss area is an area surrounded by a first line, a second line, and a pattern edge profile of the light-shielding pattern film when a transmission electron microscopy (TEM) image of the light-shielding pattern film formed by patterning the light-shielding film is measured and the TEM image is observed, the first line is an extension line connecting a first point located at a height of 20% and a second point located at a height of 40% in a side profile of the light-shielding pattern film when the total height of the light-shielding pattern film is 100%, The second line is an extension line including a pattern film intersection point and arranged parallel to the upper surface of the light-transmitting substrate; the pattern film intersection point is a point where a center line of the pattern film intersects with a top surface profile of the light-shielding pattern film; the pattern film center line is an extension line passing through a pattern film center point, which is the center point of the bottom surface of the light-shielding pattern film, and perpendicular to the top surface of the light-transmitting substrate; [Formula 2] Do = Bo - Po In the formula 2, The Bo value is the optical density of the light-shielding film measured by irradiating it with exposure light having a wavelength of 193 nm, The Po value is an optical density measured by irradiating an exposure light having a wavelength of 193 nm onto a measurement region corresponding to a region from one edge formed by patterning the light-shielding pattern film to a position 4 nm away inward of the light-shielding pattern film when the light-shielding pattern film formed by patterning the light-shielding film is observed from above.
2. The blank mask of claim 1 , wherein the transition metal includes at least one of Cr, Ta, Ti, and Hf.
3. A light-transmitting substrate and a light-shielding film disposed on the light-transmitting substrate, the light-shielding film contains a transition metal and at least one of oxygen and nitrogen, the light-shielding film includes a first light-shielding layer and a second light-shielding layer disposed on the first light-shielding layer, The film thickness of the first light-shielding layer 21 is 250 to 650 Å. The thickness of the second light-shielding layer 22 is 30 to 200 Å. The light-shielding film is patterned and the loss area of the pattern edge is measured to be 10 nm 2 or less; The etching rate of the light-shielding film with respect to a chlorine-based gas is 1.55 Å / s or more. Blank mask: The pattern edge loss area is an area surrounded by a first line, a second line, and a pattern edge profile of the light-shielding pattern film when a transmission electron microscopy (TEM) image of the light-shielding pattern film formed by patterning the light-shielding film is measured and the TEM image is observed, the first line is an extension line connecting a first point located at a height of 20% and a second point located at a height of 40% in a side profile of the light-shielding pattern film when the total height of the light-shielding pattern film is 100%, The second line is an extension line including a pattern film intersection point and arranged parallel to the upper surface of the light-transmitting substrate; the pattern film intersection point is a point where a center line of the pattern film intersects with a top surface profile of the light-shielding pattern film; The pattern film center line is an extension line that passes through a pattern film center point, which is the center point of the bottom surface of the light-shielding pattern film, and is perpendicular to the upper surface of the light-transmitting substrate.
4. A light-transmitting substrate and a light-shielding film disposed on the light-transmitting substrate, the light-shielding film contains a transition metal and at least one of oxygen and nitrogen, the light-shielding film includes a first light-shielding layer and a second light-shielding layer disposed on the first light-shielding layer, The thickness of the first light-shielding layer 21 is 250 to 650 Å. The thickness of the second light-shielding layer 22 is 30 to 200 Å. The light-shielding film is patterned and the loss area of the pattern edge is measured to be 10 nm 2 or less; The second light-shielding layer contains a transition metal at 50 to 80 at %. The pattern edge loss area is an area surrounded by a first line, a second line, and a pattern edge profile of the light-shielding pattern film when a transmission electron microscopy (TEM) image of the light-shielding pattern film formed by patterning the light-shielding film is measured and the TEM image is observed, the first line is an extension line connecting a first point located at a height of 20% and a second point located at a height of 40% in a side profile of the light-shielding pattern film when the total height of the light-shielding pattern film is 100%, The second line is an extension line including a pattern film intersection point and arranged parallel to the upper surface of the light-transmitting substrate; the pattern film intersection point is a point where a center line of the pattern film intersects with a top surface profile of the light-shielding pattern film; The pattern film center line is an extension line that passes through a pattern film center point, which is the center point of the bottom surface of the light-shielding pattern film, and is perpendicular to the upper surface of the light-transmitting substrate.
5. 2. The blank mask of claim 1, wherein the content of the element corresponding to oxygen or nitrogen in the second light-shielding layer is 10 to 35 at %.
6. 2. The blank mask according to claim 1, wherein the first light-shielding layer contains 30 to 60 at % of a transition metal.
7. A light-transmitting substrate and a light-shielding film disposed on the light-transmitting substrate, the light-shielding film contains a transition metal and at least one of oxygen and nitrogen, the light-shielding film includes a first light-shielding layer and a second light-shielding layer disposed on the first light-shielding layer, The thickness of the first light-shielding layer 21 is 250 to 650 Å. The thickness of the second light-shielding layer 22 is 30 to 200 Å. The light-shielding film is patterned and the loss area of the pattern edge is measured to be 10 nm 2 or less; The total content of oxygen and nitrogen in the first light-shielding layer is 40 to 70 at %. The pattern edge loss area is an area surrounded by a first line, a second line, and a pattern edge profile of the light-shielding pattern film when a transmission electron microscopy (TEM) image of the light-shielding pattern film formed by patterning the light-shielding film is measured and the TEM image is observed, the first line is an extension line connecting a first point located at a height of 20% and a second point located at a height of 40% in a side profile of the light-shielding pattern film when the total height of the light-shielding pattern film is 100%, The second line is an extension line including a pattern film intersection point and arranged parallel to the upper surface of the light-transmitting substrate; the pattern film intersection point is a point where a center line of the pattern film intersects with a top surface profile of the light-shielding pattern film; The pattern film center line is an extension line that passes through a pattern film center point, which is the center point of the bottom surface of the light-shielding pattern film, and is perpendicular to the upper surface of the light-transmitting substrate.
8. 2. The blank mask according to claim 1, wherein a ratio of a thickness of the second light-shielding layer to a thickness of the first light-shielding layer is 0.05 to 0.
3.
9. A light-transmitting substrate and a light-shielding pattern film disposed on the light-transmitting substrate, the light-shielding pattern film contains a transition metal and at least one of oxygen and nitrogen, the light-shielding pattern film includes a first light-shielding layer and a second light-shielding layer disposed on the first light-shielding layer, The film thickness of the first light-shielding layer 21 is 250 to 650 Å. The thickness of the second light-shielding layer 22 is 30 to 200 Å. The loss area of the pattern edge of the light-shielding pattern film is 10 nm 2 is as follows: The light-shielding pattern film has a PDo value of less than 0.05 as represented by the following formula 3: The pattern edge loss area is an area surrounded by a first line, a second line, and a pattern edge profile of the light-shielding pattern film when a transmission electron microscopy (TEM) image of the light-shielding pattern film is measured and the TEM image is observed, the first line is an extension line connecting a first point located at a height of 20% and a second point located at a height of 40% in a side profile of the light-shielding pattern film when the total height of the light-shielding pattern film is 100%, The second line is an extension line including a pattern film intersection point and arranged parallel to the upper surface of the light-transmitting substrate; the pattern film intersection point is a point where a center line of the pattern film intersects with a top surface profile of the light-shielding pattern film; the pattern film center line is an extension line passing through a pattern film center point, which is the center point of the bottom surface of the light-shielding pattern film, and perpendicular to the top surface of the light-transmitting substrate; [Formula 3] PDo = PBo - PPo In the formula 3, the PBo value is the optical density of the light-shielding pattern film measured by irradiating the light with an exposure light having a wavelength of 193 nm, The PPo value is the average optical density measured by irradiating an exposure light having a wavelength of 193 nm onto a measurement area corresponding to a region from one edge of the light-shielding pattern film to a position 4 nm away inward of the light-shielding pattern film when the light-shielding pattern film is observed from above.
10. The method includes a preparation step of arranging a light source, a photomask, and a semiconductor wafer coated with a resist film, an exposure step of selectively transmitting and emitting light incident from the light source onto the semiconductor wafer through the photomask, and a development step of developing a pattern on the semiconductor wafer, the photomask includes a light-transmitting substrate and a light-shielding pattern film disposed on the light-transmitting substrate; the light-shielding pattern film contains a transition metal and at least one of oxygen and nitrogen, the light-shielding pattern film includes a first light-shielding layer and a second light-shielding layer disposed on the first light-shielding layer, The thickness of the first light-shielding layer 21 is 250 to 650 Å. The thickness of the second light-shielding layer 22 is 30 to 200 Å. The loss area of the pattern edge of the light-shielding pattern film is 10 nm 2 is as follows: The light-shielding pattern film has a PDo value of less than 0.05 according to the following formula 3. The pattern edge loss area is an area surrounded by a first line, a second line, and a pattern edge profile of the light-shielding pattern film when a transmission electron microscopy (TEM) image of the light-shielding pattern film is measured and the TEM image is observed, the first line is an extension line connecting a first point located at a height of 20% and a second point located at a height of 40% in a side profile of the light-shielding pattern film when the total height of the light-shielding pattern film is 100%, The second line is an extension line including a pattern film intersection point and arranged parallel to the upper surface of the light-transmitting substrate; the pattern film intersection point is a point where a center line of the pattern film intersects with a top surface profile of the light-shielding pattern film; the pattern film center line is an extension line passing through a pattern film center point, which is the center point of the bottom surface of the light-shielding pattern film, and perpendicular to the top surface of the light-transmitting substrate; [Formula 3] PDo = PBo - PPo In the formula 3, the PBo value is the optical density of the light-shielding pattern film measured by irradiating the light with an exposure light having a wavelength of 193 nm, The PPo value is the average optical density measured by irradiating an exposure light having a wavelength of 193 nm onto a measurement area corresponding to a region from one edge of the light-shielding pattern film to a position 4 nm away inward of the light-shielding pattern film when the light-shielding pattern film is observed from above.
Citation Information
Patent Citations
Mask blank, transfer mask, and method of manufacturing the same
JP2011081356A
Mask blank, transfer mask, method for manufacturing transfer mask, and method for manufacturing semiconductor device
JP2013083933A
Photomask blank, and method of manufacturing photomask
JP2019090877A
Photomask blank, photomask and fabrication method thereof
KR101207724B1
Phase shift blank mask and Photomask
KR101579843B1