Glass cloth, prepreg, and printed wiring boards

The glass cloth manufacturing process, involving sodium-ion-controlled washing and high-temperature deoiling with silane coupling agents, addresses dielectric and strength issues in glass cloths, improving the performance and reliability of prepregs and printed wiring boards.

JP7554949B2Active Publication Date: 2024-09-20ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2024008207
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-08
Filing Date
2024-01-23
Publication Date
2024-09-20
Estimated Expiration
2043-03-07

AI Technical Summary

Technical Problem

Existing methods for improving dielectric properties and strength of glass cloths and prepregs used in printed wiring boards are inadequate, leading to issues such as high dielectric loss tangent, strength reduction, and appearance defects like wrinkles and tears, which affect the reliability and yield of electronic devices.

Method used

A glass cloth manufacturing process involving washing with water containing 20 ppm or less sodium ions, followed by high-temperature deoiling and surface treatment with specific silane coupling agents, to maintain strength and reduce dielectric loss tangent, ensuring uniformity and low appearance defects.

Benefits of technology

The process results in glass cloths with low dielectric loss tangent, stable strength, and reduced appearance defects, enhancing the performance and yield of prepregs and printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554949000001
    Figure 0007554949000001
  • Figure 0007554949000002
    Figure 0007554949000002
  • Figure 0007554949000003
    Figure 0007554949000003
Patent Text Reader

Abstract

To provide a glass cloth, a prepreg and a printed wiring board.SOLUTION: In a glass cloth formed by weaving a glass yarn including a plurality of filaments: a bulk dielectric loss tangent of the glass of the glass yarn is 0.0010 or less; a tensile strength of the warp per thickness of the glass cloth expressed by the following formula (A): tensile strength (N / 25 mm) in the warp direction of the glass cloth / thickness (μm) of the glass cloth...(A) is in the range of 0.50 to 6.0; a coefficient of variation in tensile strength in the warp direction of the glass cloth is 15% or less; and a dielectric dissipation factor of the glass cloth at 10 GHz is in the range of more than 0 to 0.0010 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a glass cloth, a prepreg, and a printed wiring board. [Background technology]

[0002] Currently, the performance of information terminals such as smartphones is improving, and high-speed communication, as typified by 5G communication, is progressing. In response to this background, not only is there a need for improved heat resistance, which has been conventionally required, but there is also a need for further improvement in the dielectric properties of the insulating material (e.g., lowering the dielectric tangent), particularly for printed wiring boards for high-speed communication. Similarly, there is a background to the need for improved dielectric properties for prepregs used as insulating materials for printed wiring boards, and for the glass yarns and glass cloths contained in the prepregs.

[0003] In order to reduce the dielectric constant of insulating materials, a method is known in which insulating materials are constructed using prepregs in which a low dielectric resin (hereinafter referred to as a "matrix resin") is impregnated into glass cloth (Patent Documents 1 and 2). Patent Documents 1 and 2 state that polyphenylene ether terminally modified with vinyl or methacryloxy groups is advantageous in terms of low dielectric properties and heat resistance, and that this modified polyphenylene ether is used as a matrix resin.

[0004] Also, a method of constructing a prepreg using low dielectric glass to improve the dielectric properties of the prepreg is known (Patent Document 3). In Patent Document 3, glass yarn with a silicon dioxide (SiO2) composition of 98 to 100 mass% is used. Patent Document 3 also describes a method of constructing a prepreg using low dielectric glass cloth that is surface-treated with a silane coupling agent having an unsaturated double bond group and has various requirements such as an ignition loss value of 0.12 to 0.40 mass%.

[0005] Here, it has been reported that silanol groups present on the surface of the glass cloth are the cause of the deterioration of the dielectric properties (Patent Documents 4 and 5). Patent Documents 4 and 5 describe a method of treating the surface of the glass cloth with polysilazane to reduce the number of silanol groups present on the surface of the glass cloth in order to improve the dielectric properties. Patent Documents 6 and 7 describe the reduction of the dielectric tangent of silica glass cloth by heat treatment.

[0006] Generally, a sizing agent mainly composed of starch is applied to the surface of the glass yarn, for example, to suppress the generation of fluff in the glass yarn and to prevent water absorption. Then, before, after, or during the weaving of the glass yarn, the glass yarn or glass cloth is washed for the purpose of reducing the amount of the sizing agent (for the purpose of desizing).

[0007] Patent Documents 8 and 9 report that thermal deoiling is possible at relatively low temperatures by using a quartz glass fiber sizing agent containing ammonium nitrate or a quartz glass fiber sizing agent in which at least a portion of starch is converted into a nitrate ester.

[0008] In addition, the increased density of printed wiring boards has narrowed the gaps between through-holes and / or between inner-layer lines and through-holes, resulting in a phenomenon of reduced insulation resistance, and printed wiring boards are required to have higher reliability than ever before. One of the causes of reduced insulation resistance in printed wiring boards is the effect of copper migration (electrolytic corrosion). Electrolytic corrosion is a phenomenon in which copper, a conductor, dissolves and precipitates from the anode in a high-humidity environment under voltage application, and passes through an insulating material to conduct electricity to the cathode. Electrolytic corrosion is divided into dendrites that occur in the surface resist and / or adhesive layer, and CAF (Conductive Anodic Filaments) that occur at the interface between the inner-layer glass fiber and resin. Ion components at the interface between the glass fiber and resin are known as one of the causes of CAF. Patent Document 10 describes that the CAF resistance of printed wiring boards is improved by making the amount of alkali metals and / or alkaline earth metals extracted from glass cloth of E-glass composition 20 ppm or less. Patent Document 11 describes that the amount of calcium ions adhering to the glass cloth surface is reduced and CAF resistance is improved by spraying a water vapor flow after surface treatment of the glass cloth with a surface treatment agent mainly composed of a coupling agent. Patent Document 12 describes that CAF resistance is improved by using a warp sizing agent mainly composed of polyvinyl alcohol and / or a polyvinyl alcohol derivative with an alkali metal compound content of 0.5% by weight or less. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2019 / 065940 [Patent Document 2] International Publication No. 2019 / 065941 [Patent Document 3] JP 2018-127747 A [Patent Document 4] JP 2020-194888 A [Patent Document 5] Patent Publication No. 2021-88488 [Patent Document 6] Patent Publication No. 2021-63320 [Patent Document 7] JP 2021-195689 A [Patent Document 8] JP 2016-108162 A [Patent Document 9] JP 2016-113322 A [Patent Document 10] JP 2001-73253 A [Patent Document 11] JP 2005-42245 A [Patent Document 12] Japanese Patent Application Publication No. 7-279055 Summary of the Invention [Problem to be solved by the invention]

[0010] However, Patent Documents 1 and 2 leave room for further improvement in dielectric properties. For example, Patent Documents 1 and 2 do not consider the use of low dielectric glass as described in Patent Document 3. Patent Document 3 also describes that glass with an SiO2 composition amount of 98 to 100 mass % is problematic from the practical viewpoint, and therefore, there has been a need for another method for suitably providing glass cloth and therefore prepreg using this type of glass yarn.

[0011] As pointed out in Patent Documents 4 and 5, the method of reducing the silanol groups present on the surface of the glass cloth improves the dielectric tangent of the silica glass cloth at 10 GHz by 1.0 × 10 -3 ~1.0×10 -4However, the improvement effect is considered to be small. From this, it is considered that there is a factor that increases the dielectric tangent of the glass cloth other than the presence of hydroxyl groups on the glass surface, and there is room for improvement. In addition, as pointed out in Patent Document 6, in the method of reducing the dielectric tangent by heat-treating silica glass cloth at high temperatures, there is a problem that excessive heat treatment may reduce the strength of the glass cloth. Furthermore, while surface treatment with a silane coupling agent or the like is generally performed on glass cloth used for printed wiring boards, the glass cloth in Patent Document 6 is not surface-treated, and is not practical as a glass cloth for printed wiring boards, so there is room for improvement. In addition, Patent Document 7 reports a method of recovering the tensile strength of glass cloth after high-temperature heat treatment by removing the strained layer of quartz glass by etching. However, since the strength is significantly reduced by high-temperature heat treatment, there is a problem that the glass cloth is likely to be "cut (torn off)" in the strained layer removal process. In addition, there is a possibility that the strained layer is not sufficiently removed at parts where the etching solution is difficult to penetrate, such as the weave intersections of the glass cloth and / or the twisted parts of the glass fibers. Therefore, there is a problem that the tensile strength of the glass cloth and / or the filament diameter of the glass fiber vary, and the glass cloth is likely to wrinkle, break, or the like during transportation. Furthermore, there is a problem that the basis weight of the glass cloth is excessively reduced because the glass is dissolved by the etching process. The amount of matrix resin in the prepreg, called the resin content, needs to be accurately controlled, but the etching process, which causes the basis weight of the glass cloth itself to vary, makes it difficult to control the resin content of the prepreg. For this reason, there is a strong demand for a processing method that can suppress the variation in the basis weight of the glass cloth and uniformly improve the tensile strength of the glass cloth.

[0012] When the strength of the glass cloth is reduced, the tension control range during the glass cloth transport becomes extremely low and narrow, and there is a concern that the glass cloth may develop "wrinkles" and / or "scratches" due to contact with members during transport. In order to suppress the decrease in strength of the glass cloth, Patent Documents 8 and 9 disclose a method of deoiling the glass cloth by heating at a relatively low temperature. However, in order to further improve the dielectric properties of the glass cloth, there is a strong demand for the development of a method that not only suppresses the decrease in strength of the glass cloth but also reduces the dielectric tangent of the glass cloth. Thus, there is a strong demand for a processing method that can reduce appearance defects such as cuts and wrinkles of the glass cloth.

[0013] Patent documents 10, 11 and 12 describe a method for reducing alkali metals and / or alkaline earth metals in the glass surface. In the prior art including Patent documents 10, 11 and 12, reports have been made on alkali metals and / or alkaline earth metals and CAF resistance, but from the viewpoint of maintaining the strength of glass cloth, sufficient study has not yet been made. Patent documents 8 and 9 describe that the presence of alkali metals causes a recrystallization phenomenon called devitrification of quartz glass fibers, which significantly reduces the strength of glass, but do not describe a method for suppressing the devitrification phenomenon. There has been a strong demand for technological development for glass cloth for printed wiring boards for high-speed communication from the viewpoint of reducing the dielectric loss tangent of glass cloth and suppressing the decrease in strength of glass cloth.

[0014] Therefore, an object of the present invention is to provide a low dielectric glass cloth that can suppress fluctuations in basis weight, has excellent dielectric properties (e.g., low dielectric tangent), has few wrinkles and / or scratches, and is less likely to tear, and to provide a prepreg containing the glass cloth. Another object of the present invention is to provide a printed wiring board, an integrated circuit, and an electronic device that can improve yields by using the prepreg. Another object of the present invention is to provide a method for producing the glass cloth to suitably obtain the above-mentioned glass cloth. [Means for solving the problem]

[0015] The present inventors considered that it would be very meaningful from the viewpoint of industrial production of glass cloth to clarify the relationship between the strength of the glass cloth and metal ions (including alkali metal ions and / or alkaline earth metal ions, etc.) and came up with the idea that by maintaining the strength of the quartz glass cloth, it is possible to apply sufficient tension to the glass cloth, and by utilizing this, it is possible to suppress the occurrence of wrinkles and / or scratches during transportation. Based on this idea, the present inventors have conducted intensive research to solve the above problems, and have focused on the amount of sodium ions attached to the glass cloth before the thermal deoiling process. They have found that washing the glass cloth with water containing 20 ppm or less of sodium ions makes it possible to suppress the decrease in strength of the glass cloth caused by the devitrification phenomenon of the quartz glass cloth even at high temperatures of 700°C or higher, and have completed the present invention. By suppressing the decrease in strength of the glass cloth caused by the devitrification phenomenon of the quartz glass, it becomes easier to control the tension during the conveyance of the glass cloth, and it is possible to suppress the fluctuation of the basis weight of the glass cloth, and to obtain a glass cloth with fewer wrinkles and / or scratches and less breakage. Some of the aspects of the present invention are exemplified below. [1] A glass cloth made by weaving glass yarns containing a plurality of filaments, The bulk dielectric tangent of the glass in the glass yarn is 0.0010 or less; The following formula (A): Tensile strength in the warp direction of the glass cloth (N / 25 mm) / thickness of the glass cloth (μm) (A) The tensile strength of the warp yarn per thickness of the glass cloth is in the range of 0.50 to 6.0, The coefficient of variation of the tensile strength in the warp direction of the glass cloth is in the range of 15% or less, The glass cloth has a dielectric loss tangent at 10 GHz in the range of more than 0 and not more than 0.0010. [2] A glass cloth made by weaving glass yarns containing a plurality of filaments, The bulk dielectric tangent of the glass in the glass yarn is 0.0010 or less; The following formula (A): Tensile strength in the warp direction of the glass cloth (N / 25 mm) / thickness of the glass cloth (μm) (A) The tensile strength of the warp yarn per thickness of the glass cloth is in the range of 0.50 to 6.0, The coefficient of variation of the filament diameter of the glass fibers constituting the glass cloth is in the range of 10% or less, The glass cloth has a dielectric loss tangent at 10 GHz in the range of more than 0 and not more than 0.0010. [3] 3. The glass cloth according to item 1 or 2, wherein the glass cloth has a dielectric tangent at 10 GHz in the range of more than 0 and not more than 0.0055. [4] 4. The glass cloth according to any one of items 1 to 3, wherein the silicon (Si) content in the glass yarn is 95.0 to 100 mass % calculated as silicon dioxide (SiO2). [5] 5. The glass cloth according to any one of items 1 to 4, wherein the silicon (Si) content in the glass yarn is 99.0 to 100 mass % calculated as silicon dioxide (SiO2). [6] 6. The glass cloth according to any one of items 1 to 5, wherein the glass yarn is treated with a surface treatment agent containing a silane coupling agent. [7] The surface treatment agent is represented by the following formula (1): X(R) 3-n SiY n (1) (In formula (1), X is an organic functional group having at least one of an amino group and an unsaturated double bond group having radical reactivity, each Y is independently an alkoxy group, n is an integer of 1 to 3, and each R is independently a group selected from the group consisting of a methyl group, an ethyl group, and a phenyl group.) Item 7. The glass cloth according to item 6, comprising the silane coupling agent represented by the formula: [8] 8. The glass cloth according to item 7, wherein X in the formula (1) is an organic functional group that does not form a salt with an ionic compound. [9] Item 9. The glass cloth according to item 7 or 8, wherein X in the formula (1) does not contain an amine or an ammonium cation.

[10] 10. The glass cloth according to any one of items 7 to 9, wherein X in the formula (1) is an organic functional group having one or more methacryloxy groups or acryloxy groups.

[11] 11. The glass cloth according to any one of items 1 to 10, wherein the ignition loss value of the glass cloth is 0.01% by mass or more and less than 0.18% by mass.

[12] 12. The glass cloth according to any one of items 1 to 11, wherein the glass cloth has a dielectric loss tangent at 10 GHz in the range of 0.00050 or less.

[13] 13. The glass cloth according to any one of items 1 to 12, wherein the glass cloth has a thickness of 60 μm or less.

[14] The weight of the glass cloth (g / m 2 14. The glass cloth according to any one of items 1 to 13, wherein the coefficient of variation of the above is 3% or less.

[15] The weight of the glass cloth (g / m 2 5. The glass cloth according to any one of items 1 to 4, wherein the coefficient of variation of the above-mentioned is 1.5% or less.

[16] 16. The glass cloth according to any one of items 1 to 15, wherein the number of voids in the glass cloth after 5 minutes of being impregnated with castor oil is 180 or less.

[17] 17. The glass cloth according to any one of items 1 to 16, which is for a printed wiring board.

[18] 18. A prepreg comprising the glass cloth according to any one of items 1 to 17, a thermosetting resin, and an inorganic filler.

[19] Item 19. A printed wiring board comprising the prepreg according to item 18.

[20] 20. An integrated circuit comprising the printed wiring board according to item 19. [twenty one] 20. An electronic device comprising the printed wiring board according to item 19. [twenty two] A method for producing glass cloth, comprising the step of washing glass cloth with water having a sodium ion content of 20 ppm or less. [twenty three] Item 23. The method for producing a glass cloth according to item 22, further comprising a step of heating and deoiling the glass cloth after the step of washing the glass cloth. [twenty four] Item 24. The method for producing a glass cloth according to item 23, wherein the step of thermal deoiling includes a step of thermal deoiling at 700° C. or higher. [twenty five] 25. The method for producing a glass cloth according to any one of items 22 to 24, wherein the step of washing the glass cloth comprises a step of immersing the glass cloth in water having a sodium ion content of 20 ppm or less.

[26] 26. The method for producing a glass cloth according to any one of Items 22 to 25, wherein the step of washing the glass cloth comprises a step of washing the glass cloth by using ultrasonic waves while immersing the glass cloth in water having a sodium ion content of 20 ppm or less.

[27] 27. The method for producing a glass cloth according to any one of Items 22 to 26, wherein the step of washing the glass cloth comprises a step of washing the glass cloth with water having a sodium ion content of 20 ppm or less by using a spray.

[28] 28. The method for producing a glass cloth according to any one of items 22 to 27, wherein the step of washing the glass cloth comprises a step of washing the glass cloth with water having a sodium ion content of 20 ppm or less while conveying the glass cloth.

[29] 29. The method for producing a glass cloth according to any one of items 22 to 28, comprising: washing the glass cloth with water having a sodium ion content of 20 ppm or less while transporting the glass cloth; and heating the glass cloth at a temperature of 700° C. or more.

[30] 30. The method for producing a glass cloth according to any one of items 22 to 29, wherein the silicon (Si) content in the glass yarn constituting the glass cloth is 95.0 to 100 mass % calculated as silicon dioxide (SiO2). Effect of the Invention

[0016] According to the present invention, it is possible to provide a low dielectric glass cloth that can suppress fluctuations in basis weight, has excellent dielectric properties (e.g., low dielectric tangent) and has few appearance defects, and a prepreg containing the glass cloth. The present invention also provides a printed wiring board, an integrated circuit, and an electronic device that can improve yields by using the prepreg. Furthermore, the present invention also provides a method for producing the glass cloth to suitably obtain the above-mentioned glass cloth. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described, but the present invention is not limited thereto, and various modifications are possible within the scope of the present invention. In this embodiment, a numerical range described using "~" represents a numerical range including the numerical values ​​before and after "~" as the lower limit and upper limit. In addition, in this embodiment, in a numerical range described in stages, the upper limit or lower limit described in a certain numerical range can be replaced with the upper limit or lower limit of another numerical range described in stages. Furthermore, in this embodiment, the upper limit or lower limit described in a certain numerical range can also be replaced with a value shown in the example. In this embodiment, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the function of the process is achieved.

[0018] [Glass cloth] [Overall structure] The glass cloth according to the present embodiment is a glass cloth obtained by weaving glass yarns, The bulk dielectric tangent of the glass in the glass yarn is 0.0010 or less; The following formula (A): Tensile strength of glass cloth in the warp direction (N / 25mm) / thickness of glass cloth (μm) (A) The tensile strength of the warp yarn per thickness of the glass cloth is in the range of 0.50 to 6.0, The coefficient of variation (CV) of the tensile strength in the warp direction of the glass cloth is 15% or less, The dielectric loss tangent of the glass cloth at 10 GHz is in the range of more than 0 and not more than 0.0010. This makes it possible to provide a glass cloth and a prepreg that can suppress fluctuations in basis weight, has excellent dielectric properties (for example, a low dielectric tangent), and has few defects in appearance. Incidentally, as described in the Examples, whether the variation in the basis weight of the glass cloth can be suppressed can be confirmed by the fact that the coefficient of variation in the basis weight of the glass cloth is equal to or less than a predetermined value. In this specification, the concept of "capable of suppressing fluctuations in basis weight" also includes the case where the basis weight does not fluctuate.

[0019] The glass cloth according to the present embodiment can be produced by weaving glass yarns (e.g., glass yarns consisting of a plurality of glass filaments) as warp and weft yarns. Examples of the weaving structure of the glass cloth include plain weave, sash weave, satin weave, and twill weave. Among these, the plain weave structure is preferred.

[0020] The weft density of the warp and weft yarns constituting the glass cloth according to the present embodiment is preferably 10 to 120 yarns / inch (=10 to 120 yarns / 25 mm), more preferably 40 to 100 yarns / inch. If the weft density is within the above range, the effects of the present invention can be easily obtained. The weft densities of the warp and weft yarns may be different.

[0021] The basis weight (mass of the glass cloth) of the glass cloth according to this embodiment is preferably 8 to 250 g / m 2 and more preferably 8 to 100 g / m 2 and more preferably 8 to 80 g / m 2 and particularly preferably 8 to 50 g / m 2 When the basis weight of the glass cloth is within the above range, the effects of the present invention are easily obtained.

[0022] The coefficient of variation (CV) of the basis weight of the glass cloth according to this embodiment is preferably 3% or less, more preferably 1.5% or less, even more preferably 1.3% or less, even more preferably 1% or less, and particularly preferably 0.9% or less. If the coefficient of variation of the basis weight of the glass cloth is within the above range, the variation in the tensile strength of the glass cloth is small, and it is easy to obtain a glass cloth with excellent appearance. Another major advantage is that it is possible to easily control the resin content of the prepreg. Theoretically, the lower limit of the coefficient of variation is 0.

[0023] In this embodiment, the tensile strength in the warp direction per thickness of the glass cloth is preferably in the range of 0.50 or more, more preferably in the range of 0.52 or more, even more preferably in the range of 0.54 or more, even more preferably in the range of 0.56 or more, and particularly preferably in the range of 0.58 or more. If the tensile strength in the warp direction per thickness of the glass cloth is less than 0.50, the tension applied during the glass cloth transport cannot be sufficiently applied, and wrinkles and / or scratches due to unexpected contact with equipment, etc. are likely to occur. The tensile strength in the warp direction per thickness of the glass cloth may be 6.0 or less, 5.0 or less, 4.0 or less, 3.5 or less, or 3.0 or less.

[0024] The coefficient of variation of the tensile strength in the warp direction of the glass cloth according to this embodiment is preferably less than 15%, more preferably 10% or less, even more preferably 7% or less, still more preferably 5% or less, and particularly preferably 3% or less. If the coefficient of variation of the tensile strength exceeds 15%, the glass cloth is prone to wrinkles and the like during transport.

[0025] Another aspect of the glass cloth according to the present embodiment is a glass cloth formed by weaving glass yarns including a plurality of filaments, The bulk dielectric tangent of the glass in the glass yarn is 0.0010 or less; The following formula (A): Tensile strength of glass cloth in the warp direction (N / 25mm) / thickness of glass cloth (μm) (A) The tensile strength of the warp yarn per thickness of the glass cloth is in the range of 0.50 to 6.0, The coefficient of variation of the filament diameter of the glass fiber constituting the glass cloth is within a range of 10% or less, The dielectric loss tangent of the glass cloth at 10 GHz is in the range of more than 0 and not more than 0.0010. This makes it possible to provide glass cloth and prepregs that can suppress variations in basis weight, have excellent dielectric properties, and have few defects in appearance.

[0026] The coefficient of variation of the filament diameter is preferably less than 10%, more preferably 7% or less, even more preferably 5% or less, still more preferably 4% or less, and particularly preferably 3% or less. If the coefficient of variation of the filament diameter of the glass fiber exceeds 10%, the glass cloth is likely to develop wrinkles or the like during transportation.

[0027] The coefficient of variation of the tensile strength in the warp direction and the coefficient of variation of the filament diameter are calculated by the following formulas: (Standard deviation of tensile strength in the warp direction / Average tensile strength in the warp direction) x 100 (Standard deviation of filament diameter / average filament diameter) x 100 The average tensile strength is the average value of tensile strengths measured at five points in the warp direction of the glass cloth, and the average filament diameter is the average value of filament diameters measured at ten points. Each of the tensile strength values ​​measured at multiple points and each of the filament diameter values ​​measured at multiple points may be used to calculate the standard deviation of the tensile strength and the standard deviation of the filament diameter, respectively. A glass cloth having a small coefficient of variation has a relatively low variation in the tensile strength or filament diameter in the warp direction, and therefore has high uniformity and less appearance defects. The lower limit of the coefficient of variation is theoretically 0. The coefficient of variation can be controlled by adjusting the amount of sodium ions attached to the glass cloth surface before the thermal deoiling treatment (washing the glass cloth surface with high-purity washing water to adjust the amount of sodium ions). For example, the coefficient of variation can be controlled by controlling the immersion time (seconds) of the greige cloth in washing water containing sodium ions. By ensuring the immersion time (seconds) for a predetermined time, it is easy to obtain a sufficient washing effect by the washing liquid, and therefore the effect of this embodiment is easy to achieve.

[0028] The thickness of the glass cloth according to the present embodiment is preferably 60 μm or less, more preferably 55 μm or less, and even more preferably 50 μm or less. If the thickness of the glass cloth is within the above range, the effects of the present invention can be easily obtained. The thickness of the glass cloth may be more than 0, 5 μm or more, or 5 μm or more.

[0029] [Glass thread] The glass yarn constituting the glass cloth according to the present embodiment is obtained by using low dielectric glass as a raw material. Specifically, the Si content in the glass yarn is in the range of 95.0 to 100 mass% in terms of SiO2. By using such glass yarn, for example, it is possible to improve the dielectric properties of the obtained glass cloth. From the viewpoint of improving the dielectric properties of the obtained glass cloth, the Si content is preferably in the range of 99.0 to 100 mass%, more preferably in the range of 99.5 to 100 mass%, and even more preferably in the range of 99.9 to 100 mass%.

[0030] When glass having a content of 99.0% by mass or more calculated as SiO2 is in a bulk state having a certain thickness, its dielectric loss tangent (bulk dielectric loss tangent) is generally expressed by the following formula (2): Bulk dielectric loss ≦1.2×10 -3 (2) The relationship is shown below.

[0031] The average filament diameter of the glass filaments constituting the glass yarn is preferably 2.5 to 9.0 μm, more preferably 2.5 to 7.5 μm, even more preferably 3.5 to 7.0 μm, even more preferably 3.5 to 6.0 μm, and particularly preferably 3.5 to 5.0 μm. If the filament diameter is less than the above value, the filament breaking strength is low, and the resulting glass cloth is likely to generate fluff. If the filament diameter exceeds the above value, the mass of the glass cloth is large, and it is difficult to carry or process it. If the average filament diameter of the glass filaments is within the above range, the effects of the present invention are easily obtained.

[0032] [Silane coupling agent] The glass yarns (including glass filaments) constituting the glass cloth are preferably surface-treated with a silane coupling agent. That is, in one embodiment, the surface treatment agent for the glass yarns contains a silane coupling agent. Examples of the silane coupling agent include those represented by the following formula (1): X(R) 3-n SiY n (1) In formula (1), X is an organic functional group having at least one of an amino group and an unsaturated double bond group having radical reactivity, such as a carbon-carbon double bond having radical reactivity, each Y is independently an alkoxy group, n is an integer of 1 to 3, and R is a group selected from the group consisting of a methyl group, an ethyl group, and a phenyl group. It is preferable to use a silane coupling agent represented by the following formula:

[0033] In the present embodiment, the reason why the dielectric tangent of the glass cloth has been increased in the past is that (i) Thermally oxidative degradation products of very small amounts of sizing agent remaining physically attached to the glass yarn surface; and (ii) Residues of surface treatment agents or their modifications that are physically attached to the glass surface without forming a chemical bond and cannot be reduced by washing with water The present invention focuses on the fact that the above (i) generation of thermal oxidation degradation products and / or (ii) generation of residues or denatured products are suppressed, it is preferable that X in formula (1) is an organic functional group that does not form a salt with an ionic compound. In addition, it is more preferable that X in formula (1) is an organic functional group having one or more methacryloxy groups or acryloxy groups, in terms of reactivity with the matrix resin. In addition, it is preferable that X in formula (1) does not contain amines such as primary amines, secondary amines, and tertiary amines, or ammonium cations such as quaternary ammonium cations, in terms of the ease with which the effects of the present invention are exhibited.

[0034] Regarding Y in the above formula (1), the alkoxy group is preferably an alkoxy group having 1 to 5 carbon atoms (having 1, 2, 3, 4 or 5 carbon atoms) in order to stabilize the glass cloth.

[0035] As a surface treatment agent, the silane coupling agent shown in formula (1) may be used alone or in a mixture of two or more silane coupling agents having different X in formula (1). In addition, as the silane coupling agent shown in formula (1), for example, vinyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, acryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 5-hexenyltrimethoxysilane, etc. may be used alone or as a mixture thereof.

[0036] The molecular weight of the silane coupling agent is preferably 100 to 600, more preferably 150 to 500, and even more preferably 200 to 450. In particular, it is particularly preferable to use two or more silane coupling agents having different molecular weights. By treating the glass fiber surface with two or more silane coupling agents having different molecular weights, the density of the treatment agent on the glass surface tends to increase, and the reactivity with the matrix resin tends to be further improved.

[0037] From the viewpoint of not inhibiting reactivity with resin, the silane coupling agent is preferably non-ionic. Among non-ionic silane coupling agents, silane coupling agents having at least one group selected from the group consisting of vinyl group, methacryloxy group, and acryloxy group are preferred, and silane coupling agents having at least one methacryloxy group or acryloxy group are particularly preferred. By not inhibiting reactivity with resin, the heat resistance and reliability of the printed wiring board can be improved.

[0038] In one embodiment, in formula (1), X is an organic functional group having at least one of the unsaturated double bond group and the amino group. Therefore, not only the embodiment in which X has both the unsaturated double bond group and the amino group, but also the embodiment in which X has the unsaturated double bond group but does not have the amino group, and the embodiment in which X does not have the unsaturated double bond group but has the amino group are all included in the scope of formula (1). However, X in formula (1) is preferably the unsaturated double bond group, and preferably does not contain an amino group.

[0039] From the viewpoint of lowering the dielectric loss tangent of the glass cloth, the ignition loss value of the glass cloth according to the present embodiment is preferably 0.01% by mass or more and less than 0.180% by mass, preferably 0.01% by mass or more and less than 0.174% by mass, more preferably 0.01% by mass or more and less than 0.150% by mass, and even more preferably 0.01% by mass or more and less than 0.130% by mass. If the ignition loss value is 0.180% by mass or more, the residue of the surface treatment agent that does not form a chemical bond with the glass surface and physically adheres and cannot be reduced by washing with water and / or its modified product will be present in large amounts on the glass cloth surface, and as a result, the dielectric loss tangent of the glass cloth is likely to increase. Also, if the ignition loss value is less than 0.010% by mass, the adhesion between the resin and the glass cloth is likely to be insufficient, and therefore the heat resistance and insulation reliability when made into a printed wiring board are likely to be poor.

[0040] [Bulk dielectric tangent] In this specification, the bulk dielectric loss tangent means the dielectric loss tangent measured at 10 GHz for the raw material of the glass cloth using a split cylinder resonator. The raw material of the glass cloth may be, for example, a glass raw material such as glass species, glass filaments, glass threads, etc., as described later. The bulk dielectric loss tangent of the glass raw material constituting the glass cloth can be measured by using a glass plate having the same type and composition as the glass raw material and a thickness of 300 μm or less, in the same manner as the dielectric loss tangent measurement of the glass cloth.

[0041] From the viewpoint of further improving the effect of the present invention, in the weaving of the glass cloth according to the present embodiment, the bulk dielectric tangent of the glass constituting the glass yarn is 2.5×10 at 10 GHz when measured using a split cylinder resonator. -3 Less than 2.0×10 is preferable. -3 Less than or equal to 1.7×10 is preferable. -3 Less than 1.5×10 is more preferable. -3 Less than 1.2×10 is more preferable. -3 Less than 1.0×10 is even more preferable. -3 The following is particularly preferred: 8.0×10 -4 Most preferably, the bulk dissipation factor may be greater than zero.

[0042] The dielectric tangent, bulk dielectric tangent, and the difference therebetween of the glass cloth may be, for example, as follows, without wishing to be bound by theory: Select a surface treatment agent to suppress the persistence and occurrence of the following (i) or (ii); In the glass cloth manufacturing process, optimize the conditions of the thermal deoiling (thermal desizing) process, residual glue reduction process, adhesion process, washing process, drying process, finish washing process, finish drying process, etc.; In the final cleaning process, the surface-treated glass cloth is washed with an organic solvent; It is considered that the value may be adjusted to fall within the above range by such means. (i) The occurrence of thermal oxidation degradation products of the sizing agent that is physically attached to the glass fiber surface (ii) The occurrence of residues of surface treatment agents that physically adhere to the glass surface without forming a chemical bond and cannot be reduced by washing with water, and / or their denatured products.

[0043] [Method for measuring dielectric tangent of glass cloth] The dielectric properties of the glass cloth according to the present embodiment can be measured using a resonance method. A preferred measuring device using the resonance method is a split cylinder resonator. The resonance method allows simple and accurate measurement compared to the conventional measurement method in which a printed wiring board is prepared as a measurement sample and the dielectric properties are evaluated. The reason for this is that the resonance method is suitable for evaluating low-loss materials in the high frequency range, although not limited by theory. As a method for evaluating dielectric properties other than the resonance method, for example, a lumped parameter method or a reflection transmission method is known. On the other hand, in the lumped parameter method, it is necessary to sandwich the measurement sample between two electrodes to form a capacitor, so the operation is complicated. In addition, in the reflection transmission method, when evaluating a low-loss material, the influence of the matching characteristics of the port is likely to appear, and therefore it is likely to be difficult to evaluate the dielectric tangent of the sample with high accuracy.

[0044] In measuring the dielectric properties of the glass cloth according to the present embodiment, which is applicable to printed wiring boards, particularly printed wiring boards for high-speed communication, the measurable ranges of the measuring device are preferably suitable for both the frequency dielectric constant (Dk) and the dielectric loss tangent (Df). For example, Dk is 1.1 to 50 Fm -1 The range is preferably 1.5 to 10 Fm -1 More preferably, the range is 2.0 to 5 Fm -1 In addition, Df may be more than 0, and is more preferably in the range of 1.0×10 -6 ~1.0×10 -1 The range of 1.0×10 -5 ~5.0×10 -1 The range of 5.0×10 is more preferable. -5 ~1.0×10 -2 The range is more preferable.

[0045] The measurement equipment is preferably capable of measuring frequencies of 10 GHz or higher, which makes it possible to evaluate the characteristics in the frequency band region expected when the material is actually used as glass cloth for printed wiring boards for high-speed communication.

[0046] The measurement area is 10 mm 2 It is preferable that the thickness is 15 mm or more. 2 More preferably, it is 20 mm or more. 2 It is more preferable that the above is satisfied. By measuring the dielectric properties of the glass cloth over a larger area, the reliability of the test results for the glass cloth can be improved.

[0047] The measurable thickness of the sample is preferably 3 to 300 μm, more preferably 5 to 200 μm, and even more preferably 7 to 150 μm, which can increase the reliability of the inspection results for the glass cloth.

[0048] It is possible to estimate the dielectric loss tangent of the glass cloth to some extent from the bulk dielectric loss tangent, and vice versa. On the other hand, there are cases where the dielectric loss tangent of the glass cloth differs from the bulk dielectric loss tangent. Although it is not desired to be bound by theory, the causes of this difference include, for example, (1) the generation of thermal oxides of the sizing agent physically attached to the surface of the glass yarn and / or their deteriorated products, and (2) the remaining and generation of unnecessary components that physically adhere to the surface of the glass yarn without forming a chemical bond with it and cannot be completely washed off. Therefore, the dielectric loss tangent of the glass cloth can be controlled within the above range by selecting the type of sizing agent, optimizing various conditions in the manufacturing process of the glass cloth, etc.

[0049] The glass cloth according to the present embodiment has a dielectric loss tangent at 10 GHz of 0.0010 or less, measured by the above-mentioned resonance method. Such a glass cloth can provide a prepreg capable of improving the dielectric properties. The dielectric loss tangent of the glass cloth at 10 GHz is preferably 0.0009 or less, more preferably 0.0008 or less, even more preferably 0.00055 or less, even more preferably 0.00053 or less, even more preferably 0.00050 or less, even more preferably 0.00045 or less, even more preferably 0.00040 or less, and particularly preferably 0.00035 or less. Such a glass cloth can provide a prepreg capable of further improving the dielectric properties. The lower limit may be more than 0.

[0050] [Impregnation of glass cloth] The glass cloth according to the present embodiment preferably has a void number of 180 or less after 5 minutes when impregnated with castor oil. According to this, since the glass cloth has good impregnation with resin, it is easy to improve the insulation and heat resistance of the printed wiring board. The number of voids after 5 minutes is more preferably 160 or less, more preferably 140 or less, even more preferably 120 or less, and particularly preferably 100 or less. The smaller the number of voids after 5 minutes, the better the impregnation, and the stronger the adhesion between the glass cloth and the resin. Therefore, it is easy to provide a printed wiring board with good insulation reliability and heat resistance. In order to control the number of voids after 5 minutes when impregnated with castor oil to 180 or less, for example, it is effective to treat the glass cloth with a silane coupling agent represented by the above formula (1) or to use a fiber opening method such as dry ice blasting or bending.

[0051] [Glass cloth manufacturing method] The method for producing a glass cloth according to the present embodiment includes a step of washing a glass cloth with water having a sodium ion content of 20 ppm or less. The method for producing a glass cloth according to the present embodiment may also include a step of subjecting the glass cloth to a thermal deoiling treatment and a step of treating the glass cloth with a surface treatment agent.

[0052] [Method for thermal deoiling of glass cloth] In the method for thermal deoiling of glass according to the present embodiment, the dielectric loss tangent of the glass cloth can be reduced by thermally deoiling the glass cloth composed of glass yarns having a Si content of 95.0 to 100 mass% calculated as SiO2 at a temperature of 700°C or higher. From the viewpoint of obtaining the effect of the present embodiment, the temperature of thermal deoiling is preferably in the range of 700 to 1500°C, more preferably in the range of 800 to 1300°C, and even more preferably in the range of 900 to 1100°C. If the thermal deoiling temperature is lower than 700°C, the residue of the glue adhering to the glass cloth cannot be sufficiently removed, and therefore it is difficult to reduce the dielectric loss tangent of the glass cloth. On the other hand, if the thermal deoiling temperature exceeds 1500°C, it becomes difficult to suppress the devitrification phenomenon of the glass, and it is difficult to prevent the strength reduction of the glass cloth. The heating time can be appropriately selected, for example, 3 to 120 seconds.

[0053] The means for heating the glass cloth can be any known heating method, heating medium, heating mechanism, heating device, and heating component, as long as the heating is performed so that the thermal deoiling temperature is 700°C or higher. For example, (1) the glass cloth is heated in a heating furnace, (2) the glass cloth is brought into contact with a heating section, (3) high-temperature steam is applied to the glass cloth, and the like. By heating the glass cloth so that the thermal deoiling temperature is 700°C or higher, organic matter adhering to the glass cloth surface can be efficiently removed and the time required for removing the organic matter can be shortened. The glass cloth can be heated sequentially or continuously in a closed or open system, or in a combination of a closed system and an open system.

[0054] In the case of a closed system, it is preferable to place the glass cloth in a heating furnace from the viewpoint of suitable heating by a heating means, and / or it is preferable to heat the glass cloth while storing it in a rolled state from the viewpoint of storage space and heating range. It is also preferable to heat the glass cloth while conveying it in the heating furnace from the viewpoint of increasing the efficiency of removing organic substances and shortening the time required for removing organic substances.

[0055] In the case of an open system, it is preferable to heat the glass cloth while transporting it from the viewpoint of the heated area. The glass cloth can be transported, for example, by an unwinding mechanism and a winding mechanism.

[0056] [Heating furnace] The heating means for the heating furnace is not limited to a specific means and may be various means such as an electric heater or a burner as long as it can heat the material to a thermal deoiling temperature of 700° C. or higher. A combination of multiple means may be used for heating, but it is preferable to use a gas-type single radiant tube burner or an electric heater.

[0057] From the viewpoint of heating efficiency, the heating furnace is preferably equipped with a means for discharging gas generated in the heating furnace and / or an air circulation means. The gas discharge means may be, for example, a nozzle, a gas pipe, a small hole, a gas vent valve, etc. The air circulation means may be, for example, a fan, an air conditioning system, etc.

[0058] In order to efficiently remove organic matter adhering to the surface of the glass cloth, a continuous method is preferred in which the glass cloth is heated while being continuously passed through a heating furnace, rather than a batch method in which a glass fiber fabric is wound around a core and the glass cloth is heated at a predetermined atmospheric temperature. Furthermore, a method in which the glass cloth can be continuously washed with reverse osmosis (RO) water is most preferred.

[0059] [Contact member for heating glass cloth] The above-mentioned heating furnace may be used as a method for heating the glass cloth. However, from the viewpoint of low running costs, the glass cloth may be heated by contacting a member heated to a predetermined temperature with the glass cloth.

[0060] The shape of the contact member is not particularly limited as long as it can heat the glass cloth so that the thermal deoiling temperature is 700°C or higher, but a roll shape is preferable because of the ease of transporting the glass cloth. As a member capable of heating the glass cloth in a roll shape, a roll that can be used in a high temperature range and has relatively little temperature variation in the width direction and heats by an induction heating method is preferable. When the glass cloth is heated by the contact member, it is considered that the temperature of the contact member and the surface temperature of the glass cloth are approximately the same.

[0061] In order to remove carbides adhering to the heating roll as the glass cloth is continuously heated, the above heating roll method is preferably a method equipped with a mechanism for removing adhering foreign matter, such as a mechanism such as a blade.

[0062] [Means for applying high-temperature steam to glass cloth (steam application means)] The steam applied to the glass cloth may contain, for example, a volatile solvent, water vapor, or a gas other than water vapor, but water vapor is preferred from the viewpoint of toxicity to the human body and the viewpoint of facilitating decomposition of the sizing agent used in the glass fiber. The temperature of the high-temperature steam may be a method that can supply high-temperature steam and heated air at any ratio, if necessary, in order to make the surface temperature of the glass cloth higher than 650°C. The temperature of the high-temperature steam is 400°C or higher, preferably 450°C or higher, more preferably 550°C or higher, even more preferably 600°C or higher, and particularly preferably 650°C or higher. The means of applying the steam may be, but is not limited to, spray, shower diffusion, jet nozzle, or the like. Alternatively, gas discharged from a heating furnace may be reused as high-temperature steam.

[0063] As a result of intensive research, the inventors have found that when the amount of sodium ions adhering to the surface of a glass cloth exceeds a predetermined amount, if the glass cloth is subjected to a thermal deoiling treatment at 700°C or higher, the tensile strength of the glass cloth is significantly reduced due to the devitrification phenomenon of the quartz glass. In addition, in order to suppress the devitrification phenomenon, it has been found that if the glass cloth is washed with water containing 20 ppm or less of sodium ions before the thermal deoiling treatment, the amount of sodium ions on the glass surface is reduced, and it is possible to suppress the devitrification phenomenon of the quartz glass even if the thermal deoiling treatment is performed at 700°C or higher. By maintaining the strength of the glass cloth after thermal deoiling, it is possible to suppress wrinkles and / or scratches, etc., during the process of treating the glass cloth with a surface treatment agent. From the viewpoint of obtaining the effect of this embodiment, the sodium ion content of the washing water is preferably 18 ppm or less, more preferably 15 ppm or less, even more preferably 12 ppm or less, even more preferably 10 ppm or less, and particularly preferably 7 ppm or less. If the sodium ion content of the washing water exceeds 20 ppm, the devitrification phenomenon of the quartz glass when heated to deoiling at 700°C or more cannot be suppressed, and the tensile strength of the glass cloth decreases. It is preferable that there is no lower limit for the sodium ion content, but it may be more than 0.

[0064] The means for cleaning the glass cloth with a sodium ion content of 20 ppm or less may be any known cleaning method as long as it can remove sodium ions from the glass surface. For example, a method using ultrasonic waves (e.g., a method using an ultrasonic vibrator), spraying (e.g., spraying with a high-pressure spray), water vapor spraying, etc. are possible. From the viewpoint of low-cost processing, a method is preferred in which the glass cloth is immersed in a water tank containing cleaning water (water with a sodium ion content of 20 ppm or less), and then the excess cleaning water is removed with a squeeze roller or the like, and the glass cloth is then dried. In this case, the immersion time may be, for example, 2 seconds or more, 5 seconds or more, 10 seconds or more, 15 seconds or more, or 120 seconds or less, 90 seconds or less, 60 seconds or less, or 45 seconds or less.

[0065] The method for producing water having a sodium ion content of 20 ppm or less may be a known production method. For example, filtration using an RO membrane, deionization using an ion exchange resin, etc. are possible methods. "Water having a sodium ion content of 20 ppm or less" may contain other liquid components (liquids other than water, etc.) within a range that does not impair the effects of the present invention.

[0066] [Glass cloth thermal deoiling device] As described above, the thermal deoiling device for glass cloth according to this embodiment can heat the glass cloth so that the thermal deoiling temperature of the glass cloth is 700° C. or higher. More specifically, the thermal deoiling device for glass cloth can be configured as follows: The device has an unwinding mechanism and a winding mechanism, The thermal deoiling device for glass cloth is preferably provided with a heating furnace capable of carrying out the steps of washing the glass cloth with water having a sodium ion content of 20 ppm or less while transporting the glass cloth to remove sodium ions from the glass surface, and heating the glass cloth so that the thermal deoiling temperature is 700° C. or higher.

[0067] The unwinding mechanism and the winding mechanism may be, for example, at least a pair of rolls, a roll to roll system, etc. The heating furnace, the air circulating means, the contact member, and the steam applying means are as described in the method for producing glass cloth.

[0068] [Surface treatment method for glass cloth] The glass treatment method according to the present embodiment can be applied to glass yarns and also to glass cloth. In other words, the process of weaving glass yarns to obtain glass cloth may be performed before, during, or after the glass treatment method according to the present embodiment. Note that "reduction" in the glass treatment method according to the present embodiment means, for example, removing at least a part of the surface treatment agent including a sizing agent or a silane coupling agent, and the occurrence of residual substances that cannot be completely removed is permitted.

[0069] The step of attaching the surface treatment agent may, for example, be A coating process in which a silane coupling agent is attached to the surface of the glass using a treatment solution having a concentration of 0.1 to 0.5% by mass; a fixing step of fixing the silane coupling agent to the surface of the glass by heating and drying; This makes it easier to suitably treat the surface of the glass.

[0070] The method of applying the treatment liquid to the glass in the coating step can be (a) a method of immersing or passing the glass in the treatment liquid stored in a bath (hereinafter referred to as the "immersion method"); (b) a method of applying the treatment liquid to the glass using a roll coater, a die coater, a gravure coater, or the like. When the immersion method is adopted, it is preferable to select the immersion time of the glass in the treatment liquid to be 0.5 seconds or more and 1 minute or less. Furthermore, when the immersion method is adopted, the glass can be passed through the treatment liquid at a conveying speed of 10 to 50 m / min while applying a predetermined tension (for example, 100 to 250 N) to the glass. Furthermore, after the treatment liquid is applied to the glass, the solvent contained in the treatment liquid can be heated and dried by a method such as hot air or electromagnetic waves.

[0071] The concentration of the treatment liquid is preferably 0.1 to 0.5% by mass, more preferably 0.1 to 0.45% by mass, and even more preferably 0.1 to 0.4% by mass, which facilitates more suitable surface treatment of glass.

[0072] In the fixing step, the heating and drying temperature is preferably 80° C. or higher, more preferably 90° C. or higher, so that the reaction between the silane coupling agent and the glass is sufficiently carried out, and is preferably 300° C. or lower, more preferably 180° C. or lower, so as to prevent deterioration of the organic functional group of the silane coupling agent.

[0073] The process of reducing the silane coupling agent can have at least one of the following steps: a washing step of washing off the silane coupling agent that has not formed a chemical bond with the glass surface; a drying step of heating and drying the washed glass; and a finish washing step of reducing unnecessary components that have not been washed off and have not formed a chemical bond with the glass surface. This makes it easier to control the ignition loss value. The process of reducing the silane coupling agent can have, for example, a finish drying step after the finish washing step.

[0074] Among these, in the finish cleaning step, unnecessary components that have not been completely washed off with water in the cleaning step and have not formed a chemical bond with the surface of the glass can be reduced. In this finish cleaning step, for example, an organic solvent can be used as the cleaning liquid. By having the finish cleaning step, even if a low dielectric glass such as that of this embodiment is used, it becomes easy to adjust the difference between the dielectric tangent and the bulk dielectric tangent of the obtained glass cloth within the numerical range described above. As the organic solvent here, a highly hydrophobic organic solvent is preferable, and an organic solvent having a high affinity with the residue and modified product of the silane coupling agent having a hydroxyl group is also preferable. The cleaning method can be an immersion method, a shower spray, or the like, and may be heated or cooled as necessary. In order to prevent the glass dissolved in the cleaning liquid from reattaching, it is preferable to reduce excess solvent from the glass after cleaning by a squeeze roller or the like.

[0075] As the organic solvent usable as the washing liquid in the finish washing step, for example, the following solvents can be used alone or in combination. As the highly hydrophobic organic solvent, for example, Saturated chain aliphatic hydrocarbons such as n-pentane, i-pentane, n-hexane, i-hexane, n-heptane, i-heptane, n-octane, i-octane, 2,2,4-trimethylpentane (isooctane), n-nonane, i-nonane, n-decane, i-decane, and 2,2,4,6,6-pentamethylheptane (isododecane); Saturated cyclic aliphatic hydrocarbons such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, and ethylcyclohexane; Aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, diethylbenzene, trimethylbenzene, and triethylbenzene; Halogen-containing solvents such as chloroform, dichloromethane, and dichloroethane; Examples of organic solvents that have a high affinity with the residue or modified product of the silane coupling agent include: Alcohols such as methanol, ethanol, butanol, etc.; Ketones such as acetone and methyl ethyl ketone; Ethers such as methyl ethyl ether and diethyl ether; Amides such as N,N-dimethylformamide and N,N-dimethylacetamide; Dimethyl sulfoxide; Among them, aromatic hydrocarbons, alcohols, or ketones are preferred, and methanol is more preferred, from the viewpoint of efficiently reducing the silane coupling agent physically attached to the glass. Therefore, it is preferred to use a cleaning liquid in which methanol is the main component (50% by mass or more, or 60% by mass or more of methanol relative to 100% by mass of the cleaning liquid) as the cleaning liquid in the finish cleaning step.

[0076] In the finish drying step, the cleaning liquid used in the finish washing step can be reduced. From the viewpoint of easiness in reducing the amount of cleaning liquid by drying, the cleaning liquid used in the finish washing step preferably has a boiling point of 120°C or less. For drying, a method of heat drying or air blowing can be adopted. When an organic solvent is used as the cleaning liquid, it is preferable to perform heat drying by hot air drying using low pressure steam or heat transfer oil as a heat source from the viewpoint of safety. The drying temperature is preferably equal to or higher than the boiling point of the cleaning liquid, and is preferably equal to or lower than 180°C from the viewpoint of suppressing deterioration of the silane coupling agent.

[0077] As a method for opening the glass cloth in the opening process, for example, a method of opening the glass cloth with spray water (high pressure water opening), a vibro washer, ultrasonic water, a mangle, or the like can be adopted. In this opening process, there is a tendency that the air permeability can be reduced by lowering the tension applied to the glass cloth. In order to suppress the decrease in the tensile strength of the glass cloth due to the opening process, it is preferable to take measures such as reducing friction with the contact members when weaving the glass yarn, optimizing the bundling agent, and increasing the amount of adhesion. From the viewpoint of reducing the number of voids 5 minutes after impregnation with castor oil, it is effective to increase the processing pressure in the opening process. As a method for opening glass cloth composed of glass yarns with high glass hardness, dry ice blasting is preferable.

[0078] Dry ice blasting is a method of spraying (blowing) dry ice particles having a particle size of 5 to 300 μm from a height of 5 to 1000 mm with an air pressure of 0.05 to 1 MPa. More preferably, dry ice particles having a particle size of 5 to 300 μm are sprayed from a height of 5 mm to 600 mm with an air pressure of 0.1 to 0.5 MPa. By keeping the spraying amount within this range, quality problems such as breakage of glass fibers are unlikely to occur, and therefore, the effect of improving impregnation is expected.

[0079] The above steps do not necessarily have to be performed separately, and a plurality of steps can be combined into one step. For example, when the cleaning step is performed after the weaving step, the cleaning step can also function as the fiber-spreading step by using a high-pressure water spray or the like. In most cases, the composition of the glass cloth does not usually change before and after fiber-spreading. In addition, the method for manufacturing glass cloth can have any step other than the above steps. For example, a slitting step can be performed after the fiber-spreading step. If possible, the order of the above steps can be changed.

[0080] According to the surface treatment method of the glass cloth according to the present embodiment described above, unnecessary components that are considered to increase the dielectric tangent are suitably reduced, and then the silane coupling agent can be easily applied to the surface of each of the glass filaments that constitute the glass yarn.

[0081] [Wrinkles and / or scratches on glass cloth] As defects in the appearance of the glass cloth, wrinkles occurring during the glass cloth transport and / or scratches occurring due to unexpected contact with equipment are known. It is preferable that wrinkles and / or scratches on the glass cloth do not occur because they become defective parts when a prepreg is produced. As a method for suppressing wrinkles and / or scratches, tension control during glass cloth transport is effective, and fluttering of the glass cloth can be suppressed by applying sufficient tension to the glass cloth, so that wrinkles and / or scratches can be made difficult to occur. However, if the tensile strength in the warp direction per thickness of the glass cloth is too low, sufficient tension cannot be applied to the glass cloth, making it difficult to suppress wrinkles and / or scratches. The range of the tensile strength in the warp direction per thickness is as described above. If the tensile strength in the warp direction per thickness of the glass cloth is less than 0.50, breakage is likely to occur during the glass cloth transport process, and sufficient tension cannot be applied. In particular, after the glass cloth is immersed in the surface treatment solution, the solution is squeezed out, and then the glass cloth is dried to fix the surface treatment agent to the glass cloth. If sufficient tension is not applied, the glass cloth may wrinkle at the squeezed out portion and / or may be scratched due to unexpected contact with the heating furnace. In even worse cases, the glass cloth may break at the squeezed out portion.

[0082] [Tearing of glass cloth] When the strength of the glass cloth is significantly reduced, the glass cloth is likely to break (tear). Such a significant reduction in the strength of the glass cloth is likely to occur when the glass cloth is subjected to a high-temperature heat treatment (for example, 700 to 1500° C.). Furthermore, if the uniformity of the tensile strength in the warp direction and / or the uniformity of the filament diameter in the glass cloth is low, the glass cloth is likely to break during transportation. At this time, the above-mentioned wrinkles and / or scratches are also likely to occur. Therefore, the glass cloth according to this embodiment has a coefficient of variation of the tensile strength in the warp direction in the range of 15% or less and / or a coefficient of variation of the filament diameter of the glass fibers constituting the glass cloth in the range of 10% or less. The glass cloth having a coefficient of variation in the above range has high uniformity and, therefore, has few appearance defects.

[0083] Here, it is assumed that the ratio (coefficient of variation of tensile strength in the warp direction / coefficient of variation of filament diameter) is in the range of 1.3 to 1.4 when the glass cloth is subjected to a high-temperature heat treatment (for example, 700 to 1500°C). In this case, in the glass cloth according to the present embodiment, the ratio (coefficient of variation of tensile strength in the warp direction / coefficient of variation of filament diameter) is preferably more than 0 and 5.0 or less (excluding the range of 1.3 to 1.4). This embodiment is one embodiment of a glass cloth with few appearance defects. Also, assume that the ratio (coefficient of variation of filament diameter / coefficient of variation of tensile strength in the warp direction) is in the range of 0.7 to 0.8 when the glass cloth is subjected to a high-temperature heat treatment (for example, 700 to 1500°C). In this case, in the glass cloth according to the present embodiment, the ratio (coefficient of variation of filament diameter / coefficient of variation of tensile strength in the warp direction) is preferably more than 0 and 4.5 or less (excluding the range of 0.7 to 0.8). This embodiment is also one embodiment of a glass cloth with few appearance defects.

[0084] [Prepreg] The prepreg according to the present embodiment contains the above-mentioned glass cloth and a matrix resin impregnated into the glass cloth, thereby making it possible to provide a prepreg with few voids.

[0085] The matrix resin may be a thermosetting resin or a thermoplastic resin. If possible, both may be used in combination, or may further contain other resins.

[0086] Examples of thermosetting resins include: (a) an epoxy resin obtained by reacting and curing a compound having an epoxy group with a compound having at least one group reactive with the epoxy group selected from the group consisting of an amino group, a phenol group, an acid anhydride group, a hydrazide group, an isocyanate group, a cyanate group, and a hydroxyl group; (b) a radical polymerization type curable resin obtained by curing a compound having at least one group selected from the group consisting of an allyl group, a methacryl group, and an acrylic group; (c) a maleimide triazine resin obtained by reacting and curing a compound having a cyanate group with a compound having a maleimide group; (d) a thermosetting polyimide resin obtained by reacting and curing a maleimide compound with an amine compound; (e) a benzoxazine resin obtained by crosslinking and curing a compound having a benzoxazine ring through thermal polymerization; Examples include. In (a) obtaining an epoxy resin, the compounds can be reacted without a catalyst, or the compounds can be reacted by adding a catalyst having a reaction catalytic ability, such as an imidazole compound, a tertiary amine compound, a urea compound, or a phosphorus compound. In (b) obtaining a radical polymerization type cured resin, a thermal decomposition type catalyst or a photodecomposition type catalyst can be used as a reaction initiator.

[0087] Examples of thermoplastic resins include polyphenylene ether, modified polyphenylene ether, polyphenylene sulfide, polysulfone, polyether sulfone, polyarylate, aromatic polyamide, polyether ether ketone, thermoplastic polyimide, insoluble polyimide, polyamide imide, and fluororesin. As an insulating material for printed wiring boards for high-speed communication, polyphenylene ether or modified polyphenylene ether, which has high radical reactivity, is preferable.

[0088] When the matrix resin used in a printed wiring board for high-speed communication has a vinyl group or a methacryl group, a silane coupling agent that has a relatively high hydrophobicity and a functional group involved in a radical reaction, such as a methacryl group, is compatible with the matrix resin.

[0089] As described above, the thermosetting resin and the thermoplastic resin can be used in combination. The prepreg can further contain an inorganic filler. The inorganic filler is preferably used in combination with the thermosetting resin, and examples of the inorganic filler include aluminum hydroxide, zirconium oxide, calcium carbonate, alumina, mica, aluminum carbonate, magnesium silicate, aluminum silicate, silica, talc, short glass fibers, aluminum borate, and silicon carbide. The inorganic filler may be used alone or in combination of two or more kinds.

[0090] [Printed wiring board] The printed wiring board according to the present embodiment contains the above prepreg, which makes it possible to provide a printed wiring board with excellent insulation reliability.

[0091] [Integrated circuits and electronic devices] An integrated circuit and an electronic device including the printed wiring board according to the present embodiment are also an aspect of the present embodiment. The integrated circuit and the electronic device obtained by using the printed wiring board according to the present embodiment are excellent in various properties. EXAMPLES

[0092] Next, the present invention will be described with reference to examples and comparative examples.

[0093] [Method of measuring thickness of glass cloth] The thickness of the glass cloth was measured according to JIS R 3420, 7.10. Specifically, a micrometer was used to gently rotate the spindle and lightly contact the measurement surface of the sample parallel to it. The scale was read after the ratchet made three noises. JIS R 3420, 7.10, specifies the general test method for cloth products such as glass cloth.

[0094] [Method of measuring basis weight (mass of cloth)] The cloth was cut to a predetermined size, and the mass was divided by the sample area. 2 The weight of each piece was measured 20 times. The average weight of each glass cloth was calculated using the measured values ​​(g / m2). 2 ) and coefficient of variation were calculated. Coefficient of variation of glass cloth basis weight (%) = (Standard deviation of the weight of glass cloth per unit area / Average weight of glass cloth per unit area) x 100

[0095] [Method of measuring converted thickness] Since the glass cloth is a discontinuous planar body with air present between the glass fibers, the converted thickness was calculated by dividing the basis weight (mass of the cloth) of each glass cloth by the density of the glass. Converted thickness (μm) = basis weight (g / m 2 )÷Density(g / cm 3 ) The converted thickness was calculated by the above method. This converted thickness was used for the measurement by the resonance method.

[0096] [Method of measuring dielectric tangent] The dielectric loss tangent of each glass cloth was determined in accordance with IEC 62562. Specifically, the glass cloth sample was sampled to a size required for measurement with a split cylinder resonator and stored in a thermo-hygrostatic oven at 23°C and 50% RH for 8 hours or more. The dielectric properties of the stored sample were measured using a split cylinder resonator (manufactured by EM Lab) and an impedance analyzer (manufactured by Agilent Technologies). The measurement was performed five times for each sample, and the average value was calculated. In addition, the thickness of each sample was measured using the above-mentioned converted thickness. Similarly, a glass plate having a thickness of 300 μm or less and having the same composition as each glass cloth was prepared, and the bulk dielectric loss tangent was also measured from the thickness value obtained by measuring the thickness of the glass plate. Note that IEC 62562 mainly specifies a method for measuring the dielectric properties of fine ceramic materials used in microwave circuits in the microwave band.

[0097] [Method for measuring ignition loss of glass cloth] The ignition loss value of the glass loss was determined in accordance with JIS R3420.

[0098] [Tensile strength and coefficient of variation of glass cloth] According to JIS R3420, the tensile test in the warp direction of the glass cloth was carried out five times, and the average value was taken as the tensile strength in the warp direction. The coefficient of variation of the tensile strength in the warp direction was calculated using the following formula. Coefficient of variation of tensile strength in the warp direction (%) = (Standard deviation of tensile strength in the warp direction / Average tensile strength in the warp direction) x 100

[0099] [Tensile strength in the warp direction per thickness of glass cloth] Using the thickness of the glass cloth and the tensile strength in the warp direction, the following formula (A): Tensile strength of glass cloth in the warp direction (N / 25mm) / thickness of glass cloth (μm) (A) From this, the tensile strength in the warp direction per thickness of the glass cloth was calculated.

[0100] [Coefficient of variation of filament diameter] The warp threads of the glass cloth were pulled out, and the diameter of the filaments constituting the arbitrary glass fiber was measured every 1 cm for 10 cm, and the average value was taken as the average filament diameter. The coefficient of variation of the filament diameter was calculated from the measurement results using the following formula. Coefficient of variation of filament diameter (%) = (Standard deviation of filament diameter / average filament diameter) x 100

[0101] [Measurement of the amount of sodium ions contained in water used for washing before deoiling] The amount of sodium ions contained in the water used to wash the glass cloth before thermal deoiling was measured using an ion chromatograph. <Pretreatment conditions> The samples were prepared by diluting appropriately with water. <Cation ion chromatography conditions> Equipment:Tosoh,IC-2010 Separation column: Tosoh, TSKgel-Super IC-Cation / P (4.6 mm x 150 mm) Separation solution: 2.5mM HNO3 + 0.5mM L-histidine Flow rate: 1.0mL / min Detection: Electrical conductivity Column temperature: 40℃ Injection volume: 30μL

[0102] [Method of measuring and evaluating resin impregnation] The glass cloth was sampled to a size of 50 mm x 50 mm. The sample was taken without bending or touching the measurement points. The sampled glass cloth was soaked in castor oil (Hayashi Pure Chemical Industries, Ltd., product number: 03001535) at a liquid temperature of 25°C for a specified time, and the number of voids was counted. A high-precision camera (frame size: 5120 x 5120 pixels) was installed at a position perpendicular to the glass cloth, and an LED light (CCS Corporation, power flash bar type lighting) was used as a light source, and it was irradiated from both sides of the glass cloth from a position directly to the side 15 cm away from the glass cloth. Then, the number of voids of 160 μm or more that existed between the glass filaments was counted in a 32 mm x 32 mm viewing angle, and the average value of three measurements was taken as the number of voids. In other words, "the number of voids in a glass cloth 5 minutes after it is impregnated with castor oil" is the number of voids observed when a glass cloth is impregnated with castor oil for 5 minutes under the above conditions. The voids correspond to areas that have not been impregnated with the matrix resin. Therefore, a glass cloth having a small number of voids means that the glass cloth has excellent impregnation ability with the matrix resin.

[0103] [Production of Q1035 (gray cloth)] A cloth was woven using an air jet loom with a weaving density of 66 warp threads / 25 mm and 68 weft threads / 25 mm using glass yarns with a SiO2 content of more than 99.9% by mass. The cloth was woven to a width of 1300 mm. As the warp threads, silica glass yarns with an average filament diameter of 5.0 μm, 100 filaments, and 1.0Z twist were used. As the weft threads, silica glass yarns with an average filament diameter of 5.0 μm, 100 filaments, and 1.0Z twist were used.

[0104] [Q1078 (grey cloth) manufacturing] A cloth was woven using an air jet loom with a weaving density of 54 warp threads / 25 mm and 54 weft threads / 25 mm using glass yarns with a SiO2 content of more than 99.9% by mass. The cloth was woven to a width of 1300 mm. As the warp threads, silica glass yarns with an average filament diameter of 5.0 μm, 200 filaments, and 1.0Z twist were used. As the weft threads, silica glass yarns with an average filament diameter of 5.0 μm, 200 filaments, and 1.0Z twist were used.

[0105] [Q1017 (grey cloth) manufacturing] A cloth was woven using an air jet loom with a weaving density of 95 warp threads / 25 mm and 95 weft threads / 25 mm using glass yarns with a SiO2 content of more than 99.9% by mass. The cloth was woven to a width of 1300 mm. As the warp threads, silica glass yarns with an average filament diameter of 4.0 μm, 50 filaments, and 1.0Z twist were used. As the weft threads, silica glass yarns with an average filament diameter of 4.0 μm, 50 filaments, and 1.0Z twist were used.

[0106] Example 1 The obtained Q1035 greige cloth was conveyed at a line speed where it was immersed in a water tank containing washing water 1 (sodium ion content = 2 ppm) for 20 seconds, while the sodium ions adhering to the glass surface were washed off (pre-de-oiling washing process). After that, it was heated at 800 ° C for 15 seconds in a heating furnace installed on the same line to perform de-oiling (thermal de-oiling process). Next, a treatment liquid was prepared by dispersing 0.3 mass % of 3-methacryloxypropyltrimethoxysilane (silane coupling agent A); Z6030 (manufactured by Dow Toray Co., Ltd.) in pure water adjusted to pH = 3 with acetic acid. The cloth was immersed in the treatment liquid at a line tension of 200 N and a line speed of 30 m / min (surface treatment agent application process), and after squeezing, it was heated and dried at 130 ° C for 60 seconds to fix the silane coupling agent (fixing process). The dried cloth was then immersed in water at a frequency of 25 kHz and an output of 0.50 W / cm 2The excess silane coupling agent that had physically adhered to the cloth was reduced by irradiating it with ultrasonic waves (cleaning process), and then the cloth was dried at 130°C for 1 minute (drying process) to obtain glass cloth.

[0107] Example 2 A glass cloth was obtained in the same manner as in Example 1, except that the glass cloth was washed with washing water 2 (sodium ion content=10 ppm) and heated at 900° C. for 15 seconds to deoil it.

[0108] Example 3 A glass cloth was obtained in the same manner as in Example 1, except that the glass cloth was heated at 1000° C. for 15 seconds to remove the oil.

[0109] Example 4 A glass cloth was obtained in the same manner as in Example 3, except that a treatment liquid was used in which 0.15 mass % of 3-methacryloxypropyltrimethoxysilane (silane coupling agent A); Z6030 (manufactured by Dow Toray Industries, Inc.) and 0.40 mass % of 5-hexenyltrimethoxysilane (silane coupling agent B); Z6161 (manufactured by Dow Toray Industries, Inc.) were dispersed in pure water adjusted to pH = 3 with acetic acid.

[0110] Example 5 Glass cloth was obtained in the same manner as in Example 1, except that the glass cloth was heated at 1100°C for 15 seconds to deoil the glass cloth, the line tension was changed to 130N, and the silane coupling agent was fixed using a treatment liquid in which 0.50 mass% of 5-hexenyltrimethoxysilane (silane coupling agent B); Z6161 (manufactured by Dow Toray Industries, Inc.) was dispersed.

[0111] Example 6 The obtained Q1078 grey cloth was conveyed at a line speed so that it was immersed in a water tank containing washing water 1 (sodium ion content = 2 ppm) for 20 seconds, while the sodium ions adhering to the glass surface were washed off (pre-de-oiling washing process). After that, it was heated at 800 ° C for 15 seconds in a heating furnace installed on the same line to perform de-oiling (thermal de-oiling process). Next, a treatment liquid was prepared by dispersing 0.3 mass % of 3-methacryloxypropyltrimethoxysilane (silane coupling agent A); Z6030 (manufactured by Dow Toray Co., Ltd.) in pure water adjusted to pH = 3 with acetic acid. The cloth was immersed in the treatment liquid at a line tension of 260 N and a line speed of 30 m / min (surface treatment agent application process), and after squeezing, it was heated and dried at 130 ° C for 60 seconds to fix the silane coupling agent (fixing process). The dried cloth was then immersed in water at a frequency of 25 kHz and an output of 0.50 W / cm 2 The excess silane coupling agent that had physically adhered to the cloth was reduced by irradiating it with ultrasonic waves (cleaning process), and then the cloth was dried at 130°C for 1 minute (drying process) to obtain glass cloth.

[0112] Example 7 A glass cloth was obtained in the same manner as in Example 6, except that the glass cloth was washed with washing water 2 (sodium ion content=10 ppm) and heated at 1000° C. for 15 seconds to deoil it.

[0113] Example 8 A glass cloth was obtained in the same manner as in Example 7, except that the silane coupling agents were fixed using a treatment solution prepared by dispersing 0.15 mass% of 3-methacryloxypropyltrimethoxysilane (silane coupling agent A); Z6030 (manufactured by Dow Toray Industries, Inc.) and 0.3 mass% of 5-hexenyltrimethoxysilane (silane coupling agent B); Z6161 (manufactured by Dow Toray Industries, Inc.) in pure water adjusted to pH = 3 with acetic acid.

[0114] Example 9 A glass cloth was obtained in the same manner as in Example 6, except that the glass cloth was heated at 1100° C. for 15 seconds to remove the oil.

[0115] Example 10 A glass cloth was obtained in the same manner as in Example 6, except that the glass cloth was heated at 1200° C. for 15 seconds for deoiling and that the line tension was changed to 150 N.

[0116] Example 11 The obtained Q1017 greige cloth was conveyed at a line speed so that it was immersed in a water tank containing wash water 1 (sodium ion content = 2 ppm) for 20 seconds, while the sodium ions adhering to the glass surface were washed off (pre-de-oiling washing process). After that, it was heated at 1000°C for 15 seconds in a heating furnace installed on the same line to perform de-oiling (thermal de-oiling process). Next, a treatment liquid was prepared by dispersing 0.15 mass% of 3-methacryloxypropyltrimethoxysilane (silane coupling agent A); Z6030 (manufactured by Dow Toray Co., Ltd.) and 0.3 mass% of 5-hexenyltrimethoxysilane (silane coupling agent B); Z6161 (manufactured by Dow Toray Co., Ltd.) in pure water adjusted to pH = 3 with acetic acid. The cloth was immersed in the treatment liquid with a line tension of 150 N and a line speed of 30 m / min (surface treatment agent application process), and after squeezing out the liquid, it was heated and dried at 130°C for 60 seconds to fix the silane coupling agent (fixing process). The dried cloth was then immersed in water at a frequency of 25 kHz and an output of 0.50 W / cm 2 The excess silane coupling agent that had physically adhered to the cloth was reduced by irradiating it with ultrasonic waves (cleaning process), and then the cloth was dried at 130°C for 1 minute (drying process) to obtain glass cloth.

[0117] Example 12 Glass cloth was obtained in the same manner as in Example 1, except that the glass cloth, from which excess silane coupling agent had been reduced by ultrasonic cleaning, was subjected to an opening treatment by uniformly spraying 5 to 50 μm dry ice particles over the entire glass cloth at an air pressure of 0.4 MPa.

[0118] (Example 13) Glass cloth was obtained in the same manner as in Example 6, except that the glass cloth, from which excess silane coupling agent had been reduced by ultrasonic cleaning, was subjected to an opening treatment by uniformly spraying 5 to 50 μm dry ice particles over the entire glass cloth at an air pressure of 0.45 MPa.

[0119] Comparative Example 1 Glass cloth was obtained in the same manner as in Example 1, except that washing water 3 (sodium ion content = 24 ppm) was used in the pre-deoiling washing step, and the line tension was changed to 60 N. Because the tension was low, the glass cloth fluttered significantly during transportation, and wrinkles and scratches due to contact with the drying furnace were visually confirmed on the glass cloth during the treatment liquid fixing step.

[0120] Comparative Example 2 A glass cloth was obtained in the same manner as in Comparative Example 1, except that the glass cloth was heated at 1000°C for 15 seconds for deoiling and the line tension was changed to 90 N. Because the tension was low, the glass cloth fluttered significantly during transportation, and wrinkles and scratches due to contact with the drying furnace were visually confirmed on the glass cloth during the treatment liquid fixing process.

[0121] Comparative Example 3 Except for changing the line tension to 130 N, an attempt was made to process the glass cloth in the same manner as in Comparative Example 2. However, since the ratio of the tensile strength of the glass cloth to the line tension (tensile strength of the glass cloth (warp direction) / line tension) was low, the glass cloth was broken in the fixing step of the silane coupling agent, and the glass cloth could not be obtained.

[0122] Comparative Example 4 Glass cloth was obtained in the same manner as in Example 7, except that washing water 3 (sodium ion content = 24 ppm) was used in the pre-deoiling washing step, and the line tension was changed to 80 N. Because the tension was low, the glass cloth fluttered significantly during transportation, and wrinkles and scratches due to contact with the drying furnace were visually confirmed on the glass cloth during the treatment liquid fixing step.

[0123] Comparative Example 5 Except for changing the line tension to 150 N, an attempt was made to process glass cloth in the same manner as in Comparative Example 4. However, since the ratio of the tensile strength of the glass cloth to the line tension (tensile strength of the glass cloth (warp direction) / line tension) was low, the glass cloth was broken in the fixing step of the silane coupling agent, and the glass cloth could not be obtained.

[0124] Comparative Example 6 A glass cloth was obtained in the same manner as in Example 4, except that the glass cloth was deoiled by heating at 350°C for 10 hours, the line tension was set to 200 N, and the cleaning water was changed to 2. No wrinkles or scratches were found in the obtained glass cloth, but the dielectric tangent of the glass cloth was high because the temperature of the deoiling by heating was low.

[0125] [Method for visual inspection of glass cloth] The glass cloths of the above-mentioned Examples and Comparative Examples were visually inspected for wrinkles, scratches, and tears on the glass cloth, every 1 m of the product, while irradiating a halogen lamp with a tension of 100 N / 1300 mm on a roll-to-roll inspection table. The number of defective products per 2000 m of product was counted, with the number of defective products being defined as product parts with one or more appearance defects per 1 m of product, and the number of non-defective products being defined as product parts with no appearance defects per 1 m of product. From the inspection results, the glass cloths of the Examples and Comparative Examples were graded according to the following index. Wrinkles A: The total area of ​​the product with wrinkles is less than 101m (= the defective quantity rate is less than 5%) B: The total number of wrinkled product parts is between 101 and 200 m (= the defective quantity rate is between 5% and 10%) C: The total length of the product with wrinkles is 200m or more (= the defective quantity occurrence rate is 10% or more) scratch A: The total area of ​​the product with scratches is less than 101m (= the defective quantity occurrence rate is less than 5%) B: The total number of damaged product parts is between 101 and 200 m (= the defective quantity rate is between 5% and 10%) C: The total length of the damaged product is 200m or more (= the defective quantity occurrence rate is 10% or more) Tear A: The total length of the torn cloth is less than 7m (the defective quantity rate is less than 0.3%) B: The total length of the torn cloth is between 7m and 12m (the defective quantity rate is between 0.3% and 0.6%) C: The total length of the torn cloth product is 12m or more (the defective quantity occurrence rate is 0.6% or more)

[0126] The manufacturing conditions and evaluation results of the examples and comparative examples are shown in the table below. Note that, by using the glass cloth of the examples, prepregs, printed wiring boards, integrated circuits, and electronic devices could be manufactured by ordinary methods.

[0127] [Method of manufacturing laminate] 45 parts by mass of polyphenylene ether (SABIC, Noryl SA9000), 10 parts by mass of triallyl isocyanurate, 45 parts by mass of toluene, and 0.6 parts by mass of 1,3-di(tert-butylisopropylbenzene) were added to a stainless steel container and stirred at room temperature for 1 hour to prepare a varnish. The glass cloth obtained in Examples 1, 6, 12, and 13 was impregnated with the prepared varnish, and then dried at 115°C for 1 minute to obtain a prepreg. The obtained prepreg was layered, and copper foil with a thickness of 12 μm was further layered on top and bottom, and the resulting mixture was heated at 200°C and 40 kg / cm 2 Each laminate was heated and pressed at 400° C. for 120 minutes to obtain a laminate having a thickness of 1 mm.

[0128] [Method of evaluating the insulation reliability of laminates] A wiring pattern with through holes spaced 0.30 mm apart was prepared on the copper foil on both sides of the laminate obtained as described above to obtain a sample for evaluating insulation reliability. A voltage of 50 V was applied to the obtained sample in an atmosphere of 85°C temperature and 85% RH humidity, and the change in resistance value was measured. In this case, a resistance of less than 1 MΩ within 500 hours after the start of the test was counted as an insulation failure. The same measurement was performed on 10 samples, and the number of samples that did not have an insulation failure was calculated.

[0129]

Table 1

Table 2

Table 3

Table 4

Claims

1. washing the glass cloth with water having a sodium ion content of 20 ppm or less; A step of heating and degreasing the glass cloth after cleaning the glass cloth; A method for producing a glass cloth by weaving glass yarn having a bulk dielectric tangent of 0.0010 or less, comprising the steps of: (a) preparing a glass cloth from a glass yarn having a bulk dielectric tangent of 0.0010 or less; and (b) preparing a glass cloth from a glass yarn having a bulk dielectric tangent of 0.0010 or less;

2. The method for producing glass cloth according to claim 1 , wherein the step of thermally deoiling includes a step of thermally deoiling at 700° C. or higher.

3. 3. The method for producing a glass cloth according to claim 1, wherein the step of washing the glass cloth includes a step of immersing the glass cloth in water having a sodium ion content of 20 ppm or less.

4. 3. The method for producing a glass cloth according to claim 1, wherein the step of washing the glass cloth includes a step of washing the glass cloth by using ultrasonic waves while immersing the glass cloth in water having a sodium ion content of 20 ppm or less.

5. 3. The method for producing a glass cloth according to claim 1, wherein the step of washing the glass cloth includes a step of washing the glass cloth with water having a sodium ion content of 20 ppm or less by using a spray.

6. 3. The method for producing a glass cloth according to claim 1, wherein the step of washing the glass cloth includes a step of washing the glass cloth with water having a sodium ion content of 20 ppm or less while conveying the glass cloth.

7. 3. The method for producing a glass cloth according to claim 1, further comprising: washing the glass cloth with water having a sodium ion content of 20 ppm or less while conveying the glass cloth; and heating the glass cloth at a temperature of 700° C. or more.

8. The silicon (Si) content in the glass yarn constituting the glass cloth is silicon dioxide (SiO 2 3. The method for producing a glass cloth according to claim 1, wherein the content of the glass fiber composite material is 95.0 to 100 mass % in terms of the total mass of the fiber.

Citation Information

Patent Citations

  • JP1974080394A

  • Production of glass fiber fabric

    JP1984130365A

  • Warp sizing agent for glass woven fabric

    JP1995279055A

  • Glass cloth and laminated sheet of glass cloth-reinforced synthetic resin

    JP2001073253A

  • Method for washing inorganic fiber fabric

    JP2003096659A