Hardener, anti-slip coating agent, method for forming anti-slip coating film, and anti-slip coating material

The anti-slip coating agent with polyamine and tertiary amine components addresses the inefficiencies of existing treatments by enabling rapid curing and high-performance anti-slip film formation on bridge joints and other surfaces.

JP7555073B2Active Publication Date: 2024-09-24SHUTOKO MAINTENANCE KANAGAWA +4

Patent Information

Application Number
JP2020534990
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-29
Filing Date
2020-03-30
Publication Date
2024-09-24
Estimated Expiration
2040-03-30

AI Technical Summary

Technical Problem

Existing anti-slip treatments for bridge joints require lengthy curing times and complex processes, limiting their applicability and efficiency.

Method used

An anti-slip coating agent comprising a curing agent with polyamine and tertiary amine components, combined with an epoxy resin and aggregate, allows for rapid curing and formation of a high-performance anti-slip coating film.

Benefits of technology

The coating agent enables easy and efficient anti-slip film formation in a shorter time, providing enhanced adhesion and slip resistance on various surfaces, including metal substrates, without the need for specialized equipment or lengthy curing times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555073000002
    Figure 0007555073000002
  • Figure 0007555073000001
    Figure 0007555073000001
Patent Text Reader

Abstract

Provided are an anti-slip coating agent, and the like, suited for curing and forming an anti-slip coating cover having high anti-slip capability, more simply and in a shorter time. The anti-slip coating agent has a hardener (A) and a main agent (B), wherein the hardener (A) contains a polyamine (A1) having an N-H bond, a tertiary amine (A2) having no N-H bond, and a non-reactive diluent (A3), and the main agent (B) contains an epoxy resin (B1), a silane coupling agent (B2), and an aggregate (B3). In the anti-slip coating agent, the tertiary amine (A2) content is 5 parts by mass to 30 parts by mass with respect to 100 parts by mass of the polyamine (A1). The polyamine (A1) contains first polyamine species (a1-1) comprising a polyamine having a carbocyclic ring or a modified product thereof, and a second polyamine species (a1-2) comprising piperazine or a derivative thereof, or a modified product of either or both.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curing agent used for curing an epoxy resin, an anti-slip coating agent containing the curing agent, a method for forming an anti-slip coating film, and an anti-slip covering material. [Background technology]

[0002] Finger joints are used on road bridges and elevated roads to deal with vibrations and expansion and contraction at the joints between bridge girders and between bridge girders and embankments, as well as to eliminate steps at the joints. Finger joints are components installed at the joints of bridge girders and between bridge girders and embankments, and are made of face plates made of steel or other materials, which are installed on the running surface on which vehicles such as automobiles and motorcycles travel, so that the comb teeth of a pair of fingers installed on both sides of the joints interlock with each other.

[0003] In such finger joints, vehicles tend to slip when the running surface is wet, such as during rainy weather, so it is necessary to impart a property (so-called anti-slip property) that makes it difficult for running vehicles to slip on the surface of the face plate constituting the running surface even when the running surface changes to a wet state, in order to ensure the running safety of the vehicle. For example, Patent Document 1 describes an anti-slip method in which a reactive hardening acrylic resin containing (meth)acrylate phosphate is applied as a primer to the surface of a bridge expansion device such as a finger joint, and then a resin mortar made by mixing the reactive hardening acrylic resin with aggregate is applied and hardened to form a surface layer. In addition, Non-Patent Document 1 describes an anti-slip method in which the surface of the face plate is covered with an amorphous (non-crystalline coating) film by performing blast processing and arc spray processing. In addition, Non-Patent Document 2 describes an anti-slip method in which a process of applying two types of primers, applying an adhesive, and then spraying friction elements is repeated twice. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2014-034838 A

[0005] [Non-Patent Document 1] “Steel telescopic joint face plate anti-slip treatment amorphous alloy spraying”, [online], Bridge accessories and related product search service, [Retrieved February 15, 2019], Internet〈URL:http: / / www.e-bridge.jp / eb / introacs / pro_120004 / summary.php〉 [Non-Patent Document 2] “NETIS Plus Friction Element Coating Method”, [online], Advanced Construction Technology Center, [Retrieved February 15, 2019], Internet〈URL:http: / / www.netisplus.net / NETISPLUSDB / NETISPLUSDB / detail?TECHID=125439〉 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the method described in Patent Document 1 required a long period of time, around 24 hours, for the primer and resin mortar to be cured after application until they hardened, so its use was limited to anti-slip treatment of driving surfaces in places where the road could be closed for such a long period of time.

[0007] In addition, in the method described in Non-Patent Document 1, in order to form an amorphous coating, it is necessary to perform blast processing and arc spray processing on the face plate, and the anti-slip treatment process is complicated. In addition, in the method described in Non-Patent Document 2, after applying a primer or a friction element to the application surface, it is necessary to heat it using a dedicated heater and adhere the friction element to the face plate, and the anti-slip treatment process is complicated. Therefore, there has been a demand for materials and methods that allow for more convenient anti-slip treatment.

[0008] An object of the present invention is to provide an anti-slip coating agent suitable for easily curing and forming an anti-slip coating film having high anti-slip performance in a short period of time, a curing agent suitable for use with this anti-slip coating agent, a method for forming an anti-slip coating film, and an anti-slip covering material. [Means for solving the problem]

[0009] The present inventors have found that by using a curing agent containing a polyamine having an NH bond, a tertiary amine having no NH bond, and a non-reactive diluent (A3), it is possible to cure the base agent of an anti-slip coating agent containing an epoxy resin in a shorter time and form an anti-slip coating film having high anti-slip performance, and have completed the present invention. More specifically, the present invention provides the following.

[0010] (1) The present invention relates to an anti-slip coating agent having a curing agent (A) and a main agent (B), wherein the curing agent (A) contains a polyamine (A1) having an NH bond, a tertiary amine (A2) having no NH bond, and a non-reactive diluent (A3); the main agent (B) contains an epoxy resin (B1), a silane coupling agent (B2), and an aggregate (B3); the content of the tertiary amine (A2) is 5 to 30 parts by mass per 100 parts by mass of the polyamine (A1); and the polyamine (A1) contains first polyamines (a1-1) consisting of a polyamine having a carbon ring or a modified product thereof, and second polyamines (a1-2) consisting of piperazine or a derivative thereof, or a modified product of either or both of them.

[0011] (2) The present invention also relates to the anti-slip coating agent according to (1), in which the content of the silane coupling agent (B2) is 2 to 7 parts by mass and the content of the aggregate (B3) is 300 to 1,200 parts by mass, relative to 100 parts by mass of the epoxy resin (B1).

[0012] (3) The present invention also relates to the anti-slip coating agent according to (1) or (2), in which the aggregate (B3) contains silica sand (b3-1) and alumina (b3-2).

[0013] (4) The present invention also relates to the anti-slip coating agent according to (3), wherein the alumina (b3-2) has a particle size distribution having two peaks, a first peak and a second peak, the first peak being within the range of more than 63 μm and not more than 150 μm, and the second peak being within the range of more than 355 μm and not more than 1700 μm.

[0014] (5) The present invention also relates to a curing agent for an anti-slip coating agent, which comprises a polyamine (A1) having an NH bond, a tertiary amine (A2) having no NH bond, and a non-reactive diluent (A3), in which the content of the tertiary amine (A2) is 5 to 30 parts by mass per 100 parts by mass of the polyamine (A1), and the polyamine (A1) comprises first polyamines (a1-1) consisting of a polyamine having a carbon ring or a modified product thereof, and second polyamines (a1-2) consisting of piperazine or a derivative thereof, or a modified product of either or both of them.

[0015] (6) The present invention also relates to the curing agent according to (5), wherein the polyamine (A1) contains an aliphatic polyamine.

[0016] (7) The present invention also relates to the curing agent according to (5) or (6), in which the content of the first polyamines (a1-1) is 70% by mass to 95% by mass and the content of the second polyamines (a1-2) is 5% by mass to 30% by mass, when the total content of the polyamines (A1) is 100% by mass.

[0017] (8) The present invention also relates to the curing agent according to any one of (5) to (7), wherein the content of the non-reactive diluent (A3) is 5 parts by mass to 60 parts by mass per 100 parts by mass of the polyamine (A1).

[0018] (9) The present invention also provides a method for forming an anti-slip coating film, comprising: a mixing step of mixing the curing agent (A) according to any one of (5) to (8) with a base material (B) containing an epoxy resin (B1), a silane coupling agent (B2) and an aggregate (B3) to prepare an anti-slip coating agent; and a coating / drying step of applying the anti-slip coating agent to a surface of a substrate, and then leaving the anti-slip coating agent to dry at room temperature for a short period of time within 4 hours to harden the agent, thereby forming an anti-slip coating film.

[0019] (10) The present invention also provides the method for forming an anti-slip coating film according to (9), wherein at least a portion of the surface of the substrate is made of metal.

[0020] (11) The present invention also relates to the method for forming an anti-slip coating film according to (9) or (10), wherein the mixing step comprises mixing the curing agent (A) and the main agent (B) in a mass ratio of 1:5 to 1:15 to prepare the anti-slip coating agent.

[0021] (12) The present invention also provides an anti-slip coating material having a substrate and an anti-slip coating film on a surface of the substrate, the anti-slip coating film comprising a polyamine (A1) having an NH bond, a tertiary amine (A2) having no NH bond, and a non-reactive diluent (A3), the content of the tertiary amine (A2) being 5 to 30 parts by mass per 100 parts by mass of the polyamine (A1), the polyamine (A1) being a cured product of an anti-slip coating agent obtained by mixing a curing agent (A) containing a first polyamine (a1-1) consisting of a polyamine having a carbon ring or a modified product thereof, and a second polyamine (a1-2) consisting of piperazine or a derivative thereof, or a modified product of either or both of them, and a main agent (B) containing an epoxy resin (B1), a silane coupling agent (B2) and an aggregate (B3).

[0022] (13) The present invention also provides the anti-slip coating material according to (12), in which at least a portion of the surface of the substrate is made of metal. Effect of the Invention

[0023] According to the present invention, it is possible to obtain an anti-slip coating agent suitable for easily curing and forming an anti-slip coating film having high anti-slip performance in a short period of time, a curing agent suitable for use in this anti-slip coating agent, a method for forming an anti-slip coating film, and an anti-slip covering material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Specific embodiments of the present invention will be described in detail below. Note that the present invention is not limited to the following embodiments, and various modifications are possible without departing from the gist of the present invention.

[0025] <Hardening agent> The curing agent (A) according to the present embodiment is a curing agent used in an anti-slip coating agent, and contains a polyamine (A1) having an NH bond, a tertiary amine (A2) having no NH bond, and a non-reactive diluent (A3), and the content of the tertiary amine (A2) is 5 to 30 parts by mass, more preferably 5 to 20 parts by mass, per 100 parts by mass of the polyamine (A1).

[0026] The curing agent (A) according to this embodiment makes it possible to cure the base material (B) containing the epoxy resin (B1) in a shorter time to form an anti-slip coating film, and also makes it possible to easily form an anti-slip coating film by simply mixing the curing agent (A) and the base material (B) and applying the mixture to a substrate.

[0027] [Polyamine (A1)] As the polyamine (A1), a polyamine having an NH bond or a modified product thereof can be used, which can react with the epoxy group contained in the epoxy resin (B1) to cure. As such a polyamine, it is preferable to contain a first polyamine (a1-1) consisting of a polyamine having a carbon ring or a modified product thereof, and a second polyamine (a1-2) consisting of piperazine or a derivative thereof, or a modified product of either or both of them. By using a first polyamine (a1-1) having a carbon ring as the polyamine (A1), the mechanical and thermal durability of the cured product can be improved, and the steric hindrance of the carbon ring can suppress heat generation during mixing with the main agent (B), making it easier to apply. At the same time, by using a second polyamine (a1-2) such as piperazine, which has a relatively high reactivity among cyclic compounds, the main agent (B) containing the epoxy resin (B1) can be cured in a shorter time.

[0028] Among these, specific examples of the first polyamines (a1-1) include alicyclic polyamines such as 1,3-bisaminomethylcyclohexane, menthene diamine, isophorone diamine, bis(4-amino 3-methylcyclohexyl)methane, and diaminocyclohexylmethane, aliphatic polyamines containing aromatic rings such as m-xylylene diamine, and aromatic polyamines such as m-phenylenediamine, diaminodiphenylmethane, and diaminodiphenylsulfone, but are not limited thereto. Modified products of these polyamines, such as Mannich compounds, amine adducts with epoxy compounds, ketimine compounds, polyamidoamines, Michael addition compounds, aldimine compounds, and urea adducts with isocyanate compounds may also be used.

[0029] In particular, as the first polyamines (a1-1), it is preferable to use diamines from the viewpoint of making the curing reaction milder and facilitating mixing with the base agent (B) and coating, and it is particularly preferable to use 1,3-bisaminomethylcyclohexane or m-xylylenediamine.

[0030] As the first polyamines (a1-1), one or a combination of two or more of these compounds can be used.

[0031] The mixing ratio of the first polyamines (a1-1) is preferably 70 mass% or more, and more preferably 80 mass% or more, when the total content of the polyamines (A1) is 100 mass%, On the other hand, the mixing ratio of the first polyamines (a1-1) is preferably 95% by mass or less, and more preferably 90% by mass or less, when the total content of the polyamines (A1) is taken as 100% by mass.

[0032] Specific examples of the second polyamines (a1-2) include, but are not limited to, N-2-aminoethylpiperazine, piperazine, N-methylpiperazine, 1,4-bis-(8-aminopropyl)-piperazine, piperazine-1,4-diazacycloheptane, 1-(2'-aminoethylpiperazine), 1-[2'-(2"-aminoethylamino)ethyl]piperazine, and the like. Modified polyamines may also be used as the second polyamines (a1-2).

[0033] As the second polyamines (a1-2), one or a combination of two or more of these compounds can be used.

[0034] The mixing ratio of the second polyamines (a1-2) is preferably 5% by mass or more, more preferably 10% by mass or more, based on the total content of the polyamines (A1) being 100% by mass. On the other hand, the mixing ratio of the second polyamines (a1-2) is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, based on the total content of the polyamines (A1) being 100% by mass.

[0035] As the polyamine (A1), a polyamine not included in the first polyamines (a1-1) and the second polyamines (a1-2), such as a chain aliphatic polyamine, may be used. However, the blending ratio of the chain aliphatic polyamine is preferably 10% by mass or less, more preferably 5% by mass or less, when the total content of the polyamine (A1) is taken as 100% by mass.

[0036] [Tertiary amine (A2)] Tertiary amines (A2) that do not have an NH bond can be used, and since they promote the reaction between the polyamine (A1) and the epoxy group, the curing time of the base agent (B) containing the epoxy resin (B1) can be shortened. Note that tertiary amines that have an NH bond have multiple nitrogen atoms and are reactive with the epoxy group contained in the epoxy resin (B1), and therefore are included in the polyamine (A1) in the present invention.

[0037] Specific examples of the tertiary amine (A2) include 2,4,6-tri(dimethylaminomethyl)phenol, triethanolamine, dialkylaminoethanol, triethylenediamine[1,4-diazacyclo(2,2,2)octane], and the like.

[0038] The blending ratio of the tertiary amine (A2) is preferably more than 0 mass%, more preferably 5 mass% or more, and even more preferably 10 mass% or more, based on 100 parts by mass of the polyamine (A1). On the other hand, the blending ratio of the tertiary amine (A2) is preferably 30 mass% or less, more preferably 20 mass% or less, and even more preferably 15 mass% or less, based on 100 parts by mass of the polyamine (A1).

[0039] [Non-reactive diluent (A3)] The non-reactive diluent (A3) is necessary to be contained in the curing agent in order to adjust the physical properties such as viscosity in the mixture of the curing agent (A) and the main agent (B) and to improve the workability. Specific examples of the non-reactive diluent (A3) include aromatic alcohols such as benzyl alcohol, phenol, phenethyl alcohol, nonylphenol, and dinonylphenol, xylene resin, coumarone-indene resin, isoparaffin mixture, high boiling point aromatic hydrocarbon compounds, and white tar, but are not limited thereto.

[0040] The blending ratio of the non-reactive diluent (A3) is preferably 5% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, based on 100 parts by mass of the polyamine (A1). On the other hand, from the viewpoint of ensuring practical hardness of the anti-slip coating film, the blending ratio of the non-reactive diluent (A3) is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less, based on 100 parts by mass of the polyamine (A1).

[0041] [Other ingredients] To the curing agent (A) according to the present embodiment, various additives such as a plasticizer, a moisture absorbent, a physical property adjusting agent, a colorant, an anti-sagging agent, an antioxidant, an anti-aging agent, a solvent, a pigment, a dye, and a fluorescent material may be added as necessary.

[0042] <Anti-slip coating agent> The anti-slip coating agent according to this embodiment comprises the above-mentioned curing agent (A) and a main agent (B), and the main agent (B) contains an epoxy resin (B1), a silane coupling agent (B2), and an aggregate (B3).

[0043] In the anti-slip coating agent according to this embodiment, the epoxy resin (B1) hardens in a shorter time and the aggregate (B3) and the epoxy resin (B1) are firmly bonded to each other, so that an anti-slip coating film having high anti-slip performance can be easily formed in a shorter time.

[0044] [Epoxy resin (B1)] The epoxy resin (B1) is a polymer or oligomer having two or more epoxy groups in one molecule and capable of crosslinking by reacting with an amine-based curing agent. Examples of the epoxy resin (B1) include bisphenol A type epoxy resin obtained by condensation reaction of bisphenol A and epichlorohydrin, bisphenol F type epoxy resin, bisphenol AD ​​type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, glycidyl ester type epoxy resin, biphenyl type epoxy resin, polymer type epoxy resin, and other modified epoxy resins. As the epoxy resin (B1), one or more of these resins can be used in combination.

[0045] The epoxy resin (B1) has a viscosity (25°C) of preferably 20 Pa·s or less, more preferably 15 Pa·s or less. The epoxy resin (B1) has a mass average molecular weight of preferably 200 to 4000, more preferably 300 to 2000. The epoxy resin (B1) has an epoxy equivalent (based on JIS K7236) of preferably 150 to 1000 g / eq, more preferably 150 to 700 g / eq.

[0046] When two or more epoxy resins are used in combination, the mass average molecular weight and epoxy equivalent of the epoxy resin (B1) are the mass average molecular weight and epoxy equivalent of the two or more epoxy resins as a whole.

[0047] [Silane coupling agent (B2)] As the silane coupling agent (B2), a compound having a functional group that bonds to an organic material and a functional group that bonds to an inorganic material in one molecule can be used. Among them, it is preferable to use a compound that is reactive with organic materials such as epoxy resin (B1) and also reactive with inorganic materials such as aggregate (B3) and substrate (described below). This chemically bonds the reaction product of epoxy resin (B1) and polyamine (A1) with aggregate (B3) and substrate, making the anti-slip coating film more durable.

[0048] The silane coupling agent (B2) is represented by the general formula X-Si(OR)3, for example. Here, X is a functional group that can react with an organic material, more specifically, an amino group, a vinyl group, an epoxy group, a mercapto group, a halogen group, and a hydrocarbon group having these groups. OR is a hydrolyzable group, more specifically, a methoxy group, an ethoxy group, and the like.

[0049] Specific examples of the silane coupling agent (B2) include epoxy silanes such as γ-glycidoxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, β-(3,4-epoxycyclohexyl)methyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltriethoxysilane, β-(3,4-epoxycyclohexyl)methyltriethoxysilane, and γ-glycidoxypropyltriethoxysilane; N-β(aminoethyl)γ-aminopropyltrimethoxysilane; and N- Examples of the silanes include aminosilanes such as β(aminoethyl)γ-aminopropyltriethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldiethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, and N-phenyl-γ-aminopropyltriethoxysilane; and vinylsilanes such as vinyltris(β-methoxyethoxy)silane, vinylethoxysilane, and vinyltrimethoxysilane, but are not limited to these.

[0050] The blending ratio of the silane coupling agent (B2) is preferably 2 parts by mass or more, more preferably 3 parts by mass or more, per 100 parts by mass of the epoxy resin (B1) in order to increase the adhesion of the anti-slip coating film to the substrate and to form a harder film. On the other hand, the blending ratio of the silane coupling agent (B2) is preferably 7 parts by mass or less, more preferably 5 parts by mass or less, in order to reduce the viscosity during application and further improve workability.

[0051] [Aggregate (B3)] The anti-slip coating agent of the present invention contains an aggregate (B3), which imparts anti-slip properties to the coating film made of the cured product of the anti-slip coating agent and imparts toughness to the coating film.

[0052] The aggregate (B3) may be any commonly used aggregate, and is not particularly limited. Examples of the aggregate include silica sand, alumina, silicon carbide, glass balloons, fly ash balloons, and shirasu balloons.

[0053] The content of aggregate (B3) in the anti-slip coating agent is preferably 300 parts by mass or more, more preferably 500 parts by mass or more, and even more preferably 600 parts by mass or more, per 100 parts by mass of epoxy resin (B1), from the viewpoint of imparting anti-slip performance to the coating film. On the other hand, the content of aggregate (B3) in the anti-slip coating agent may be preferably 1200 parts by mass or less, more preferably 1000 parts by mass or less, and even more preferably 800 parts by mass or less, per 100 parts by mass of epoxy resin (B1), from the viewpoint of improving the tensile properties of the coating film and facilitating application to a substrate.

[0054] Among the aggregates (B3), it is preferable to contain silica sand (b3-1) and alumina (b3-2), and in particular, it is preferable that the alumina (b3-2) has a particle size distribution with two peaks, a first peak and a second peak.

[0055] (Silica sand (b3-1)) Of these, the silica sand (b3-1) preferably has a peak in the range of 300 μm to 850 μm in mass-based particle size distribution, and more preferably has a peak in the range of 425 μm to 600 μm. Furthermore, the silica sand (b3-1) is preferably one in which the majority of the silica sand is left on a sieve with a nominal size of 300 μm, 425 μm, or 600 μm when a particle size test is conducted on the silica sand based on JIS Z2601 (test method for foundry sand), and more preferably one in which the majority of the silica sand is left on a sieve with a nominal size of 425 μm.

[0056] From the viewpoint of imparting anti-slip performance to the coating film, the content of the silica sand (b3-1) in the anti-slip coating agent is preferably 80 parts by mass or more, more preferably 100 parts by mass or more, and even more preferably 130 parts by mass or more, per 100 parts by mass of the epoxy resin (B1). On the other hand, the content of the silica sand (b3-1) in the anti-slip coating agent may be preferably 300 parts by mass or less, more preferably 250 parts by mass or less, and even more preferably 200 parts by mass or less, per 100 parts by mass of the epoxy resin (B1).

[0057] (Alumina (b3-2)) Alumina (b3-2) preferably has two peaks, a first peak and a second peak, in the particle size distribution based on mass. Of these, the first peak is preferably in the range of more than 63 μm and not more than 150 μm, and more preferably in the range of more than 75 μm and not more than 125 μm. The second peak is preferably in the range of more than 355 μm and not more than 1700 μm, more preferably in the range of more than 425 μm and not more than 1000 μm, and even more preferably in the range of more than 500 μm and not more than 600 μm. By using granular alumina (b3-2) having such two peaks in the particle size distribution, the anti-slip performance of the coating film can be further improved.

[0058] Furthermore, when a grain size test is conducted on alumina based on JIS R6001 (grain size of abrasives for grinding wheels), the alumina (b3-2) is preferably a mixture of one or more selected from F150, F120, F100, and F90 and one or more selected from F46, F40, F36, F30, F24, F22, F20, F16, and F14, and more preferably a mixture of one or both of F120 and F100 and one or more selected from F40, F36, F30, F24, and F22.

[0059] From the viewpoint of imparting anti-slip performance to the coating film, the content of alumina (b3-2) in the anti-slip coating agent is preferably 300 parts by mass or more, more preferably 400 parts by mass or more, and even more preferably 500 parts by mass or more, per 100 parts by mass of epoxy resin (B1). On the other hand, the content of alumina (b3-2) in the anti-slip coating agent may be preferably 1000 parts by mass or less, more preferably 800 parts by mass or less, and even more preferably 700 parts by mass or less, per 100 parts by mass of epoxy resin (B1).

[0060] [Other ingredients (B4)] The base resin (B) used in this embodiment may contain other components (B4) such as an epoxy-based reactive diluent, a non-reactive diluent, an organic solvent, a plasticizer, etc., for the purpose of improving workability, etc.

[0061] Among these, the epoxy-based reactive diluent is not particularly limited as long as it is a mono-, di-, or triepoxide that is generally commercially available, such as o-cresyl glycidyl ether, trimethylolpropane triglycidyl ether, phenyl glycidyl ether, alkyl glycidyl ether, glycidyl ester, α-olefin epoxide, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, cyclohexane dimethanol glycidyl ether, cyclohexane dimethanol diglycidyl ether, alkyl phenyl glycidyl ether, and alkyl phenol glycidyl ether.

[0062] Examples of non-reactive diluents include benzyl alcohol, nonylphenol, dinonylphenol, xylene resin, coumarone-indene resin, isoparaffin mixture, high boiling aromatic hydrocarbon compounds, white tar, etc. Examples of plasticizers include various esters of phthalic acid, phosphoric acid, and fatty acid. Examples of organic solvents include acetone, methyl ethyl ketone, methyl butyl ketone, methyl isobutyl ketone, cyclohexanone, toluene, xylene, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, cellosolve, methyl cellosolve, n-propanol, and isopropanol.

[0063] The base material (B) used in this embodiment may contain a thickener for the purpose of preventing dripping during application, etc. Examples of the thickener include fumed silica, anhydrous silicic acid, hydrous silicic acid, diatomaceous earth, calcined clay, clay, talc, kaolin, bentonite, and organic bentonite.

[0064] The base material (B) used in this embodiment may contain a colorant such as a pigment, dye, or fluorescent material for the purpose of adjusting the visibility of the anti-slip coating film, etc. Examples of the colorant include carbon black, titanium oxide, ferric oxide, and active zinc oxide.

[0065] <Method of forming anti-slip coating film> The method for forming the anti-slip coating film according to this embodiment includes a mixing step of mixing the above-mentioned curing agent (A) and main agent (B) to prepare an anti-slip coating agent, and a coating / drying step of applying the anti-slip coating agent to the surface of a substrate and then leaving the anti-slip coating agent to dry at room temperature for a short period of time, for example, within 4 hours, to harden the anti-slip coating film.

[0066] [Mixing process] In the mixing step, the above-mentioned hardener (A) and base agent (B) are mixed to prepare an anti-slip coating agent. The above-mentioned hardener (A) is often in liquid form, and the base agent (B) is often in paste form. There are no particular limitations on the mixing means, as long as it is possible to mix the liquid hardener (A) with the paste-like base agent (B).

[0067] The mixing ratio of the curing agent (A) and the base agent (B) (ratio of curing agent (A) to base agent (B)) is preferably 1:5 to 1:15 by mass. By keeping the ratio of the curing agent (A) to the base agent (B) within this range, it is possible to promote curing of the coating film in the coating and drying process described below.

[0068] In order to obtain a homogeneous anti-slip coating agent, the mixing time of the curing agent (A) and the base agent (B) in the mixing step is preferably 1 minute or more, more preferably 2 minutes or more. On the other hand, the upper limit of the mixing time can be determined according to the pot life, but is preferably less than 10 minutes, more preferably 5 minutes or less. Note that the "pot life" here refers to the (maximum) time during which the anti-slip coating agent can be spread over the substrate after starting to mix the curing agent (A) and the base agent (B).

[0069] The pot life of an anti-slip coating agent varies depending on environmental conditions such as the temperature of use, but some examples of approximate pot life are as follows: 35 to 45 minutes at temperatures between 0°C and 10°C, 25 to 35 minutes at temperatures between 10°C and 20°C, 17 to 20 minutes at room temperature (between 20°C and 30°C), and 10 to 12 minutes at temperatures between 30°C and 40°C.

[0070] [Coating and drying process] In the coating and drying process, an anti-slip coating agent consisting of a mixture of a curing agent (A) and a base material (B) is applied to a substrate, and then the applied film is dried and cured to form an anti-slip coating film.

[0071] The substrate to which the anti-slip coating agent is applied is not particularly limited, and the agent can be applied to a substrate having at least a part of its surface made of metal. The resulting anti-slip coating film is firmly bonded to the metal surface of the substrate and exhibits anti-slip performance, so that when a vehicle runs on the anti-slip coating film formed on the metal surface, the vehicle is less likely to slip.

[0072] The substrate may be subjected to surface preparation as necessary. The anti-slip coating agent of the present invention can provide an anti-slip coating film with desired properties even when applied to a substrate that has only been subjected to relatively minor surface preparation such as grade 3 scraping (surface preparation to the extent of removing rusted areas).

[0073] The anti-slip coating agent can be applied to the substrate by any conventional means, such as a brush, a roller, etc. The anti-slip coating agent of the present invention does not require any special equipment or skills to form an anti-slip coating film, and can impart the desired anti-slip performance with a single application, so that anti-slip processing can be performed over a wider range at once.

[0074] The thickness of the anti-slip coating agent is determined according to the particle size of the aggregate (B3), and can be, for example, 0.5 mm to 5.0 mm. In the anti-slip coating agent of the present invention, an anti-slip coating film is formed by hardening the epoxy resin (B1) and bonding the epoxy resin (B1) with the aggregate (B3) or the base material, so that the thicker the anti-slip coating agent is applied, the higher the anti-slip performance can be obtained.

[0075] The time required for drying and curing the coating film varies depending on environmental conditions such as the temperature of use, but can be, for example, 5 to 10 hours under temperature conditions of 0° C. or higher and lower than 10° C., 3 to 6 hours under temperature conditions of 10° C. or higher and lower than 20° C., 2 to 4 hours under temperature conditions of normal temperature (20° C. or higher and lower than 30° C.), and 1 to 3 hours under temperature conditions of 30° C. or higher and lower than 40° C. In particular, when an anti-slip coating agent is applied to a road joint and dried at normal temperature, a long period of curing of about 24 hours was required when a conventional anti-slip coating agent was used, but when the anti-slip coating agent of the present invention is used, it is possible to dry and cure the applied anti-slip coating agent at normal temperature in a short period of time of within 4 hours to form an anti-slip coating film.

[0076] Furthermore, the anti-slip coating agent of the present invention can provide an anti-slip coating film by drying and curing even in low-temperature environments of 5°C or less, where curing was difficult with conventional epoxy resins, without the need for heating using special equipment.

[0077] In addition, the anti-slip coating agent of the present invention can harden the coating film in a short time, as described above, especially under warm conditions, and impart anti-slip properties to the substrate. Therefore, even in a limited time, such as during nighttime construction work on a highway, anti-slip treatment can be performed on a wider range of substrates.

[0078] As described above, the anti-slip coating agent of the present invention is capable of easily forming a coating film having high anti-slip performance in a wide temperature range in a short period of time, and therefore can be suitably used to impart anti-slip performance to slippery areas of road surfaces and floors, such as roadways, sidewalks, parking lots, and parks.

[0079] <Anti-slip covering material> The anti-slip coating material of the present invention has a substrate having an anti-slip coating film on its surface, and the anti-slip coating film contains a curing agent (A) containing a polyamine (A1) having an NH bond and a tertiary amine (A2) not having an NH bond, an epoxy resin (B1), and a base material (B) containing a silane coupling agent (B2) and an aggregate (B3). Here, the polyamine (A1), the tertiary amine (A2), the epoxy resin (B1), the silane coupling agent (B2), and the aggregate (B3) are as described above. The anti-slip coating material may also contain the above-mentioned non-reactive diluent (A3).

[0080] Such anti-slip coating materials include finger joints provided at the joints between bridge girders of road bridges and elevated roads, and at the joints between bridge girders and embankments, and it is preferable that at least the running surface of the finger joints on which vehicles run has an anti-slip coating film.Other examples of anti-slip coating materials include members that become slippery in a wet state, such as drainage outlets, manhole covers, pedestrian walkways, stairs, slopes, inspection walkways, and scaffolding. EXAMPLES

[0081] Next, in order to clarify the effects of the present invention, examples of the present invention will be described, but the present invention is not limited to these.

[0082] <Preparation of curing agent and anti-slip coating agent> The curing agent (A) and the base agent (B) were prepared in the mixing ratios shown in Tables 1 and 2, respectively, and then the curing agent (A) and the base agent (B) were mixed to obtain an anti-slip coating agent.

[0083] [Table 1]

[0084] [Table 2]

[0085] Details of each component used in the preparation of the curing agent (A) and the base agent (B) shown in Table 1 are as follows. Note that, for the polyamine (A1) and the tertiary amine (A2), a composition containing the components shown in Table 1 may be used, but the curing agent (A) was prepared so that the content of the components shown in Table 1, not the content of the composition, would be the value shown in Table 1.

[0086] [Hardening agent (A)] [Polyamine (A1)] (First polyamines (a1-1)) Mannich modification of m-xylylenediamine (manufactured by Chori GLEX Co., Ltd., model number: KA-861, m-xylylenediamine content: 10% by mass, amine value: 375) m-Xylylenediamine (amine value: 825) 1,3-bisaminomethylcyclohexane (manufactured by Yun Teh Industries, model number: JOINTMINE989, 1,3-bisaminomethylcyclohexane content: 40-50% by mass, amine value: 380) (Secondary polyamines (a1-2)) N-2-aminoethylpiperazine (manufactured by Chori GLEX Co., Ltd., model number: PH-770, N-2-aminoethylpiperazine content: 50-60% by mass, amine value: 580) [Tertiary amine (A2)] 2,4,6-Tri(dimethylaminomethyl)phenol (Sigma-Aldrich, model number: DMP-30) [Non-reactive diluent (A3)] Benzyl alcohol (LANXESS)

[0087] [Main ingredient (B)] [Epoxy resin (B1)] Bisphenol A epoxy resin (Mitsui Petrochemical Industries, Ltd., Model: Epomic R140, Mass average molecular weight: 350-400, Epoxy equivalent: 189g / eq, Viscosity: 13 Pa·s / 25°C) [Silane coupling agent (B2)] γ-Glycidoxypropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd., model number: KBM-403) [Aggregate (B3)] (Silica sand (b3-1)) Silica sand No. 5 (manufactured by JFE Mineral Co., Ltd., model number: Silica Sand Iide Silica Sand No. 5, mass-based particle size distribution peak: 500 μm) (Alumina (b3-2)) Alumina #120 (manufactured by Nippon Carlit Co., Ltd., model number: Sakurandam WA F120, mass-based particle size distribution peak: 100 μm) Alumina #36 (manufactured by Nippon Carlit Co., Ltd., model number: Sakurandam WA F36, mass-based particle size distribution peak: 500 μm) Alumina #14 (manufactured by Nippon Carlit Co., Ltd., model number: Sakurandam WA F14, mass-based particle size distribution peak: 1400 μm) [Other ingredients (B4)] (Reactive diluent) o-Cresyl glycidyl ether ·Trimethylpropane triglycidyl ether (Thickener) Hydrophobic fumed silica (manufactured by Nippon Aerosil Co., Ltd., model number: RY200S) (Coloring agent) Carbon black (manufactured by Mitsubishi Chemical Corporation, model number: MA100)

[0088] The obtained anti-slip coating agent was applied to a substrate consisting of a steel plate (SS400 general structural rolled steel material specified in JIS G 3101) measuring 300 mm in length, 300 mm in width, and 4.5 mm in thickness using a nap roller to a uniform thickness of 3 mm, and then left to stand at an air temperature of 20°C for 4 hours to dry and harden the applied film, thereby obtaining an anti-slip coating film.

[0089] At this time, the workability was evaluated by visual inspection for the presence or absence of stickiness when applying the anti-slip coating agent to the substrate and the presence or absence of dripping from the coating film. Coating agents that could maintain their shape when applied to the wooden board and were easy to spread when applied were deemed to have good workability and were marked with an "O". Coating agents that had difficulty maintaining their shape when applied to the wooden board or were difficult to spread when applied were deemed to have poor workability (unacceptable) and were marked with an "X".

[0090] In addition, the hardening of the film when drying and hardening the coating film was evaluated 30 minutes, 1 hour, 2 hours, 3 hours, and 4 hours after coating, based on JIS K7215, using a D-type durometer (rubber hardness tester, manufactured by Asker Corporation). At this time, if the hardness of the surface of the film could be measured and the value was 60 or more, the film was deemed to have hardened well and was marked as "◯". If the hardness of the surface of the film could be measured and the value was less than 60, the film was deemed to have hardened poorly but was at a pass level (passable) and marked as "△". If the hardness of the surface of the film could not be measured, the film was deemed to have hardened poorly (failable) and marked as "X".

[0091] The adhesion strength [MPa] of the obtained anti-slip coating film to the substrate was measured based on JIS K 5600-5. In addition, the slip resistance value (BPN) of the anti-slip coating film was measured based on ASTM E 303. The adhesion strength to the substrate and the slip resistance value were measured at five different points on the same anti-slip coating film, and the average value was used as the measurement result. These measurement results are shown in Table 1.

[0092] The evaluation results in Table 1 show that in Inventive Examples 1 to 13, the anti-slip coating film can be formed more easily in a shorter time.

[0093] Furthermore, it was found that the anti-slip coating films obtained in Inventive Examples 1 to 13 had high adhesion to the substrate of 12 MPa or more, and the anti-slip coating films also had high slip resistance values ​​(BPN) of 60 or more.

[0094] The above results show that the curing agents used in Inventive Examples 1 to 13 and the anti-slip coating agents using them were able to easily form anti-slip coating films with high anti-slip performance in a short period of time.

[0095] In contrast, the anti-slip coating film formed using the curing agent of Comparative Example 1 did not contain either the secondary polyamines (a1-2) or the tertiary amine (A2), and therefore was inferior in terms of workability. In addition, the surface hardness of the film could not be measured even 4 hours after application, and the film was also inferior in terms of hardening.

[0096] In addition, the anti-slip coating film formed using the curing agent of Comparative Example 2 did not contain secondary polyamines (a1-2) and had a low content of tertiary amine (A2), so it was inferior in terms of workability. Furthermore, the surface hardness of the film could not be measured even 4 hours after application, and the film was also inferior in terms of hardening.

[0097] In addition, the anti-slip coating films formed using the curing agents of Comparative Examples 3 to 5 did not contain the secondary polyamines (a1-2), and therefore were inferior in terms of workability. In addition, the surface hardness of the film could not be measured even 4 hours after application, and the film was also inferior in terms of hardening.

[0098] In addition, the anti-slip coating film formed using the curing agent of Comparative Example 6 did not contain the non-reactive diluent (A3), and therefore was inferior in terms of workability and had a low slip resistance value of less than 60.

[0099] Although the embodiments and examples of the present invention have been described above, the above-described embodiments and examples do not limit the invention according to the claims. It should be noted that not all of the combinations of features described in the embodiments and examples are essential to the means for solving the problems of the invention.

Claims

1. An anti-slip coating agent having a curing agent (A) and a base agent (B), The curing agent (A) is A polyamine (A1) having an N—H bond; A tertiary amine (A2) having no N—H bond; A non-reactive diluent (A3), Contains The main component (B) is An epoxy resin (B1), A silane coupling agent (B2), Aggregate (B3); Contains the content of the tertiary amine (A2) is 5 parts by mass to 30 parts by mass relative to 100 parts by mass of the polyamine (A1); the polyamine (A1) comprises a first polyamine (a1-1) consisting of a polyamine having a carbon ring or a modified product thereof, and a second polyamine (a1-2) consisting of piperazine or a derivative thereof, or a modified product of either or both of them; The anti-slip coating agent has a content of the first polyamines (a1-1) of 70% by mass to 95% by mass and a content of the second polyamines (a1-2) of 5% by mass to 30% by mass, when the total content of the polyamines (A1) is 100% by mass.

2. 2. The anti-slip coating agent according to claim 1, wherein the content of the silane coupling agent (B2) is 2 to 7 parts by mass and the content of the aggregate (B3) is 300 to 1,200 parts by mass, relative to 100 parts by mass of the epoxy resin (B1).

3. The anti-slip coating agent according to claim 1 or 2, wherein the aggregate (B3) contains silica sand (b3-1) and alumina (b3-2).

4. The anti-slip coating agent according to claim 3, wherein the alumina (b3-2) has a particle size distribution having two peaks, a first peak and a second peak, the first peak being within a range of more than 63 μm and not more than 150 μm, and the second peak being within a range of more than 355 μm and not more than 1700 μm.

5. A polyamine (A1) having an N—H bond; A tertiary amine (A2) having no N—H bond; A non-reactive diluent (A3); Contains the content of the tertiary amine (A2) is 5 parts by mass to 30 parts by mass relative to 100 parts by mass of the polyamine (A1); the polyamine (A1) comprises a first polyamine (a1-1) consisting of a polyamine having a carbon ring or a modified product thereof, and a second polyamine (a1-2) consisting of piperazine or a derivative thereof, or a modified product of either or both of them; The curing agent for an anti-slip coating agent, wherein the content of the first polyamines (a1-1) is 70% by mass to 95% by mass, and the content of the second polyamines (a1-2) is 5% by mass to 30% by mass, when the total content of the polyamines (A1) is 100% by mass.

6. The curing agent according to claim 5 , wherein the polyamine (A1) contains an aliphatic polyamine.

7. The curing agent according to claim 5 or 6, wherein the content of the non-reactive diluent (A3) is 5 parts by mass to 60 parts by mass relative to 100 parts by mass of the polyamine (A1).

8. A curing agent (A) according to any one of claims 5 to 7, a mixing step of mixing an epoxy resin (B1), a silane coupling agent (B2), and a base material (B) containing an aggregate (B3) to prepare an anti-slip coating agent; a coating / drying step of applying the anti-slip coating agent to the surface of a substrate, and then leaving the anti-slip coating agent to dry at room temperature for a short period of time of up to 4 hours to harden the anti-slip coating film; The method for forming an anti-slip coating film comprises the steps of:

9. The method for forming an anti-slip coating film according to claim 8, wherein at least a part of the surface of the substrate is made of metal.

10. 10. The method for forming an anti-slip coating film according to claim 8, wherein the mixing step comprises mixing the curing agent (A) and the base agent (B) in a mass ratio of 1:5 to 1:15 to prepare the anti-slip coating agent.

11. An anti-slip coating material having a substrate and an anti-slip coating film on a surface of the substrate, The anti-slip coating film is a curing agent (A) containing a polyamine (A1) having an N-H bond, a tertiary amine (A2) not having an N-H bond, and a non-reactive diluent (A3), the content of the tertiary amine (A2) being 5 parts by mass to 30 parts by mass per 100 parts by mass of the polyamine (A1), the polyamine (A1) containing a first polyamine (a1-1) consisting of a polyamine having a carbon ring or a modified product thereof, and a second polyamine (a1-2) consisting of piperazine or a derivative thereof, or a modified product of either or both of them, the content of the first polyamine (a1-1) being 70% by mass to 95% by mass and the content of the second polyamine (a1-2) being 5% by mass to 30% by mass when the total content of the polyamine (A1) is taken as 100% by mass; A base material (B) containing an epoxy resin (B1), a silane coupling agent (B2) and an aggregate (B3); The anti-slip coating material is a hardened product of the anti-slip coating agent obtained by mixing the above.

12. The anti-slip coating according to claim 11, wherein at least a portion of the surface of the substrate is made of metal.

Citation Information

Patent Citations

  • Cementing material for durable colored pavement and preparation method thereof

    CN103627140A

  • Colored anti-skid thin layer and preparation method thereof

    CN109233566A

  • JP1974114699A

  • Polymer concrete composition for repair and top coating of cement-like road

    JP1990274722A

  • Binder for paving material and paving material using the same

    JP2003040977A

Cited By

  • A low irritant composition for non-slip coating

    KR102793568B1