Aluminum alloys for heat exchanger fins
Aluminum alloys with specific compositions and production processes address the challenges of strength, sag resistance, and corrosion in heat exchanger fins, achieving improved performance and recyclability for lightweight automotive applications.
Patent Information
- Application Number
- JP2021533412
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-09-06
- Filing Date
- 2019-09-03
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2039-09-03
AI Technical Summary
The automotive heat exchanger industry faces challenges in balancing the need for high strength, sag resistance, and corrosion performance in aluminum fin materials, particularly during brazing, while also seeking to reduce weight and thickness for energy efficiency.
Development of aluminum alloys with specific compositions, including Cu, Fe, Mn, and Zn, and production processes involving direct chill casting, hot rolling, cold rolling, and intermediate annealing to achieve desired mechanical properties and corrosion resistance, suitable for producing lightweight heat exchanger fins.
The resulting aluminum alloy fins exhibit improved strength, sag resistance, and corrosion performance, suitable for high-performance automotive heat exchangers, with enhanced recyclability and reduced fin crushing during brazing.
Smart Images

Figure 0007555339000059 
Figure 0007555339000105 
Figure 0007555339000067
Abstract
Description
[Technical field]
[0001] Claiming priority This application claims priority to U.S. Provisional Application No. 62 / 727,806, filed September 6, 2018, the entirety of which is incorporated herein by reference.
[0002] The present invention relates to the fields of materials science, materials chemistry, metallurgy, aluminum alloys, aluminum fabrication, and related fields. The present invention provides novel aluminum alloys for use in the production of heat exchanger fins, which are used in various heat exchanger devices, such as automotive radiators, condensers, evaporators, and related devices. [Background technology]
[0003] The automotive heat exchanger industry presents several requirements for the aluminum material ("fin stock") used in the production of heat exchanger fins. Balancing these requirements can be difficult. There is a need for an aluminum alloy fin stock that has high strength in both pre-brazed and post-brazed conditions, improved sag resistance meaning good behavior during brazing, and reduced fin erosion. To reduce the weight of automobiles, it is desirable to reduce the size and weight of automotive heat exchangers to conserve resources and save energy. Various methods have been investigated to achieve this goal, and one of the desired solutions is to reduce the thickness of the aluminum fin stock. To reduce the thickness of the fin material, it is important to increase the strength after brazing and ensure sufficient brazeability. At the same time, the heat exchanger fins need to have high electrical conductivity and good corrosion performance compared to other heat exchanger components. For example, the heat exchanger fins can be more anodic than the heat exchanger tube stock, resulting in the fins acting sacrificially. A desirable aluminum fin stock would possess properties and parameters that balance the above requirements. Summary of the Invention
[0004] Embodiments of the present subject matter are defined by the claims, rather than this Summary. This Summary is a high-level overview of various aspects of the invention and introduces some of the concepts that are further described in the Detailed Description section below. This Summary is not intended to identify key features or important features of the claimed subject matter, nor is it intended to be used in isolation to determine the scope of the claimed subject matter. The subject matter should be understood by reference to the entire specification, any or all drawings, and appropriate portions of each claim.
[0005] It is desirable to produce an aluminum fin stock that has the required thickness (gauge) combination, can withstand brazing, and will exhibit suitable mechanical properties, strength and electrical conductivity properties, and suitable corrosion potential for high performance heat exchanger applications before, during, and after brazing. Additionally, it is desirable to produce the aluminum fin stock from an input metal that incorporates scrap aluminum to produce the fin stock in an environmentally friendly and cost-effective manner. Improved aluminum alloy fin stock is disclosed that possesses a combination of features and properties that make it suitable for the production of heat exchanger fins for use in, for example, heat exchangers, such as those used in the automotive industry. In one example, the improved aluminum alloy fin stock can be produced in sheet form at a desired thickness (gauge) that is suitable for the production of lightweight heat exchanger units. The aluminum alloy fin stock is brazable and exhibits strength characteristics before, during, and after brazing that make it attractive for automotive heat exchanger applications. More specifically, the disclosed improved aluminum alloy fin stock possesses pre-braze strength characteristics that reduce fin crushing issues during brazing. The disclosed aluminum alloy fin stock also possesses a sufficiently high thermal conductivity suitable for heat exchanger applications, and has a corrosion potential that is negative enough for the fins to act sacrificially during heat exchanger corrosion. In summary, the improved aluminum alloy fin stock possesses one or more of the following properties: high strength, desirable post-braze mechanical properties, desirable sag resistance, desirable corrosion resistance, and desirable electrical conductivity. At the same time, the aluminum alloy fin stock can be produced from input aluminum that is at least partially suitable for recycling. More specifically, the improved aluminum alloy fin stock contains levels of non-aluminum constituents, e.g., Cu, Fe, Mn, and Zn, which match the levels of these elements found in certain scrap aluminum as input metal.
[0006] The disclosed aluminum alloy fin stock is produced in sheet, plate, or shate form. Processes for producing the improved aluminum alloy fin stock are also disclosed that incorporate one or more of a casting, rolling, or annealing step. In some cases, the process steps employed during the production of the improved aluminum alloy fin stock impart beneficial properties and characteristics to the material. In one exemplary process, the improved aluminum alloy fin stock is produced by using one or more cold rolling steps. Each of the cold rolling steps may involve multiple cold rolling passes. The cold rolling steps may be characterized by an achieved "cold work %" or "CW %". To achieve a required strength range of the aluminum alloy fin stock, it may be desirable to achieve a specified range or value of CW %. In one example, the aluminum alloy fin stock may be produced by a process involving direct chill casting and cold working (cold rolling) to produce a desired pre-braze temper, e.g., H14 temper. In other examples, the improved fin aluminum alloy material can be produced in various other strain-hardened pre-braze tempers, such as H16, H18, or other H1X tempers. The process for producing aluminum alloy fin stock can also involve hot rolling after direct chill casting, and intermediate annealing before the final cold rolling step (e.g., between the intermediate and final cold rolling steps). The term "intermediate annealing (IA)" refers to a heat treatment applied between the cold rolling steps. The IA temperature can affect the properties of the aluminum fin stock. For example, reducing the IA temperature from 400°C to 350°C results in a coarser grain size after brazing. The combination of CW% and IA temperature used in this production, along with other factors such as aluminum alloy composition, results in the desired properties.
[0007] The disclosed aluminum alloy fin stock can be used in various applications, for example, in the manufacture of fins for heat exchangers. In some cases, the improved aluminum alloy fin stock is useful in automotive heat exchangers that are high performance and lightweight. As some non-limiting examples, the aluminum alloy fin stock can be used in automotive heat exchangers, such as radiators, condensers, and evaporators. However, the use and applications of the improved aluminum alloy fin stock are not limited to automotive heat exchangers, and other applications are envisioned, as the features and properties of the aluminum alloy fin stock may be beneficial for uses and applications other than the production of automotive heat exchanger fins. For example, the improved aluminum alloy fin stock can be used in the manufacture of various devices that use heat exchangers and are produced by brazing, such as devices used in heating, ventilation, air conditioning, and refrigeration (HVAC&R) systems.
[0008] As described above, the improved aluminum alloy fin stock compositions and processes result in materials that possess a combination of beneficial features and characteristics that make them suitable for the manufacture of heat exchanger fins. For example, the aluminum alloy fin stock exhibits a beneficial combination of one or more of the following characteristics: pre-braze and post-braze mechanical properties, such as tensile strength, post-braze sag resistance, thermal conductivity, and corrosion potential. One example is an aluminum alloy that includes about 0.9-1.4 wt.% Si, about 0.3-0.6 wt.% Fe, about 0.20-0.60 wt.% Cu, about 1.0-1.7 wt.% Mn, about 0.01-0.25 wt.% Mg, about 0.1-3.0 wt.% Zn, and up to about 0.10 wt.% Ti, with the balance being 0.15 wt.% or less of Al and impurities. Another example is an aluminum alloy containing about 0.9-1.35% Si, about 0.3-0.6% Fe, about 0.20-0.60% Cu, about 1.0-1.7% Mn, about 0.01-0.25% Mg, about 0.1-3.0% Zn, and up to about 0.10% Ti, with the remainder being 0.15% or less Al and impurities. Another example is an aluminum alloy containing about 0.9-1.4% Si, about 0.35-0.6% Fe, about 0.20-0.60% Cu, about 1.0-1.7% Mn, about 0.01-0.25% Mg, about 0.1-3.0% Zn, and up to about 0.10% Ti, with the remainder being 0.15% or less Al and impurities.Some other examples are as follows: aluminum alloys containing about 0.9-1.2 wt% Si, 0.3-0.6 wt% Fe, 0.40-0.55 wt% Cu, 1.0-1.7 wt% Mn, 0.01-0.1 wt% Mg, and 0.1-3.0 wt% Zn, with the balance of Al and impurities being less than 0.15 wt%; Aluminum alloys containing 0.60 wt% Cu, about 1.1-1.60 wt% Mn, about 0.01-0.25 wt% Mg, about 0.1-3.0 wt% Zn, and up to 0.10 wt% Ti, with the balance of Al and impurities being 0.15 wt% or less; about 0.9-1.4 wt% Si, about 0.3-0.6 wt% Fe, about 0.20-0.60 wt% Cu, about 1.0-1.7 wt% Mn, about 0.05-0.2 wt% Ti, and about 0.15 wt% or less of Al and impurities; % Mg, about 0.1-3.0 wt.% Zn, and up to about 0.10 wt.% Ti, with the balance of Al and impurities being 0.15 wt.% or less; about 0.9-1.4 wt.% Si, about 0.3-0.6 wt.% Fe, about 0.20-0.60 wt.% Cu, about 1.0-1.7 wt.% Mn, about 0.01-0.25 wt.% Mg, about 1-3.0 wt.% Zn, and up to about 0.10 wt.% Ti. and the remaining Al and impurities are 0.15% or less by weight; and the remaining Al and impurities are 0.15% or less by weight, and the remaining Al and impurities are about 0.9-1.4% by weight Si, about 0.3-0.6% by weight Fe, about 0.20-0.60% by weight Cu, about 1.0-1.7% by weight Mn, about 0.01-0.25% by weight Mg, about 1.5-2.75% by weight Zn, and about 0.10% by weight Ti. In the disclosed aluminum alloys, one or more of Zr, V, Cr, or Ni may be present at less than 0.05% by weight, less than 0.04% by weight, less than 0.03% by weight, less than 0.02% by weight, or less than 0.01% by weight. In some cases, one or more of Zr, V, Cr, or Ni is absent (i.e., 0% by weight).
[0009] In some examples, the disclosed aluminum alloys may have an ultimate tensile strength of at least 200 MPa when measured in a pre-brazed state, or at least 150 MPa when measured after brazing, or both. In one example, the ultimate tensile strength of the aluminum alloy may be 200-230 MPa when measured in a pre-brazed state, or greater than 170 MPa when measured after brazing, or both. The aluminum alloys may have a corrosion potential of -760 mV or less when measured after brazing. The aluminum alloys may have a thermal conductivity of greater than 40% (International Annealed Copper Standard, assuming 100% pure copper conductivity) when measured after brazing.
[0010] The disclosed aluminum alloys can be produced by a process including: direct chill casting of the aluminum alloy into an ingot; hot rolling of the ingot after direct chill casting; cold rolling the aluminum alloy to an intermediate thickness after hot rolling; intermediate annealing of the aluminum alloy rolled to an intermediate thickness at a temperature between 200°C and 400°C (200-400°C) after cold rolling; cold rolling the aluminum alloy after intermediate annealing to achieve a cold work % (CW %) of 20-40% resulting in a sheet having a thickness of 45-100 μm, 45-90 μm, 47-85 μm, or 50-83 μm. In a further process, continuous casting can be used. The CW % achieved in the above process can be 30-40%. The intermediate annealing may be performed at a temperature between 320°C and 370°C (320-370°C), between 290°C and 360°C (290-360°C), or between 340°C and 360°C (340-360°C). The intermediate annealing time may be 30 minutes to 60 minutes. A heat exchanger comprising the improved aluminum alloy is also disclosed. The heat exchanger may be an automotive heat exchanger. The heat exchanger may be a radiator, a condenser, or an evaporator. A process for making objects and devices comprising the improved alloy is also disclosed. An example of such a process is a process for making a heat exchanger, the process comprising joining by brazing at least one first aluminum alloy form fabricated from the improved aluminum alloy with a second aluminum alloy form, the process comprising assembling and clamping the two or more aluminum forms together and heating the two or more aluminum forms to a brazing temperature until a joint is formed between the two or more aluminum forms by capillary action. The use of the improved aluminum alloys to fabricate heat exchanger fins and other objects and devices is also included within the scope of this description. Other objects, features, and advantages of the present invention will become apparent from the following detailed description. [Brief description of the drawings]
[0011] [Figure 1A]1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 1B] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 1C] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 1D] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 1E] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 1F] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 1G] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 1H] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 1I] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 2A] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 2B] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 2C] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 2D] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 2E] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 2F]1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 2G] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 2H] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 2I] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 3A] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 3B] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 3C] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 3D] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 3E] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 3F] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 3G] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 3H] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 3I] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 4A] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 4B] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 4C] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 4D] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 4E] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 4F] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 4G] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 4H] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 4I] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 5A] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 5B] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 5C] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 5D] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 5E] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 5F]1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 5G] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 5H] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 5I] 1 is a photograph showing the grain size of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 6A] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 6B] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 6C] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 6D] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 6E] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 6F] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 6G] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 6H] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 6I] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure before brazing. [Figure 7A] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 7B] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 7C] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 7D] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 7E] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 7F] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 7G] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 7H] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 7I] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after standard brazing; [Figure 8A] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 8B] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 8C] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 8D] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 8E] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 8F]1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 8G] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 8H] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 8I] 1 is a photograph showing the grain structure of an aluminum alloy sample prepared according to the present disclosure after high speed brazing; [Figure 9] 5A-D show the effect of % cold work and intermediate annealing on different properties of aluminum alloy samples prepared according to the present disclosure. [Figure 10] 5A-5D are photographs showing the grain structure of aluminum alloy samples prepared according to the present disclosure and subjected to standard brazing. [Figure 11] 5A-5D are photographs showing the grain structure of aluminum alloy samples prepared according to the present disclosure and subjected to standard brazing. [Figure 12] 5A-5D are photographs showing the grain structure of aluminum alloy samples prepared according to the present disclosure and subjected to high speed brazing. [Figure 13] 5A-5D are photographs showing the grain structure of aluminum alloy samples prepared according to the present disclosure and subjected to high speed brazing. [Figure 14A] 1 is a photograph showing corrosion test results of coupons including aluminum alloy samples prepared according to the present disclosure; [Figure 14B] 1 is a photograph showing corrosion test results of coupons including aluminum alloy samples prepared according to the present disclosure; [Figure 14C] 1 is a photograph showing corrosion test results of coupons including aluminum alloy samples prepared according to the present disclosure; [Figure 14D] 1 is a photograph showing corrosion test results of coupons including aluminum alloy samples prepared according to the present disclosure; [Figure 14E]1 is a photograph showing corrosion test results of coupons including aluminum alloy samples prepared according to the present disclosure; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Described herein are high strength, corrosion resistant aluminum alloys, as well as methods of making and processing them. The aluminum alloys described herein exhibit improved mechanical strength, corrosion resistance, and / or formability. The alloys provided herein contain increased silicon (Si), copper (Cu), manganese (Mn), and magnesium (Mg) compared to existing alloys. The alloys provided herein may have improved strength after brazing compared to existing alloys. The alloy material may be formed as a fin stock and used in automotive heat exchangers, such as radiators, condensers, evaporators, and the like. The aluminum fin stock may be used in other brazing applications, such as, but not limited to, HVAC&R applications. Additionally, the aluminum alloy fin stock is useful for high performance, lightweight automotive heat exchangers. The fin stock is designed to be less stable than the tubes, and therefore corrodes faster than the tubes. Heat exchangers are designed based on this sacrificial corrosion protection by the fin stock on the tubes. Thus, the fin stock described herein provides this sacrificial protection to the tubes.
[0013] Definitions and Explanations As used herein, the terms "invention," "the invention," "this invention," and "the present invention" are intended to refer broadly to all of the subject matter of this patent application and the claims that follow. Any specification containing these terms should be understood in no way to limit the subject matter described herein, nor to limit the meaning or scope of the claims that follow.
[0014] In this description, reference is made to alloys identified by aluminum industry designations such as "series" or "1xxx." For an understanding of the number designation systems most commonly used to name and identify aluminum and its alloys, see "International Alloy Designations and Chemical Composition Limits for Wrought Aluminum and Wrought Aluminum Alloys" or "Registration Record of Aluminum Association Alloy Designations and Chemical Composition Limits for Aluminum Alloys in the Form of Castings and Ingot" (both published by the Aluminum Association).
[0015] As used herein, the meanings of "a," "an," or "the" include singular as well as plural references unless the context clearly dictates otherwise.
[0016] As used herein, a plate generally has a thickness of greater than about 15 mm. For example, a plate can refer to an aluminum product having a thickness of greater than about 15 mm, greater than about 20 mm, greater than about 25 mm, greater than about 30 mm, greater than about 35 mm, greater than about 40 mm, greater than about 45 mm, greater than about 50 mm, or greater than about 100 mm.
[0017] As used herein, a shade (also referred to as a sheet plate) generally has a thickness of about 4 mm to about 15 mm. For example, the shade may have a thickness of about 4 mm, about 5 mm, about 6 mm, about 7 mm, about 8 mm, about 9 mm, about 10 mm, about 11 mm, about 12 mm, about 13 mm, about 14 mm, or about 15 mm.
[0018] As used herein, sheet generally refers to an aluminum product having a thickness of less than about 4 mm. For example, the sheet may have a thickness of less than about 4 mm, less than about 3 mm, less than about 2 mm, less than about 1 mm, less than about 0.5 mm, less than about 0.3 mm, or less than about 0.1 mm, less than about 0.05 mm.
[0019] In this application, reference is made to alloy tempers or tempers. For an understanding of the descriptions of the most commonly used alloy tempers, please refer to "American National Standards (ANSI) H35 on Alloy and Temper Designation Systems". The F temper or temper refers to the aluminum alloy as produced. The O temper or temper refers to the aluminum alloy after annealing. The Hxx temper or temper, also referred to herein as the H temper, refers to the aluminum alloy after cold rolling, with or without heat treatment (e.g., annealing). Suitable H tempers include HX1, HX2, HX3, HX4, HX5, HX6, HX7, HX8, or HX9 tempers. For example, an aluminum alloy can only be in the possible H19 temper if it is cold rolled. In a further example, an aluminum alloy can be cold rolled and annealed to be in the possible H23 temper.
[0020] The following aluminum alloys are described in terms of elemental composition in weight percent (wt%) based on the total weight of the alloy, with the balance being aluminum and the maximum total weight of impurities being 0.15 wt% in each particular example alloy.
[0021] As used herein, "electrochemical potential" refers to the susceptibility of a material to oxidation-reduction reactions. Electrochemical potential can be used to evaluate the corrosion resistance of the aluminum alloys described herein. Negative values can describe materials that oxidize easily (e.g., lose electrons or increase oxidation state) when compared to materials with positive electrochemical potentials. Positive values can describe materials that reduce easily (e.g., gain electrons or decrease oxidation state) when compared to materials with negative electrochemical potentials. Electrochemical potential, as used herein, is a vector quantity that represents magnitude and direction.
[0022] As used herein, the meaning of "room temperature" can include a temperature of about 15°C to about 30°C, such as about 15°C, about 16°C, about 17°C, about 18°C, about 19°C, about 20°C, about 21°C, about 22°C, about 23°C, about 24°C, about 25°C, about 26°C, about 27°C, about 28°C, about 29°C, or about 30°C.
[0023] All ranges disclosed herein should be understood to encompass any and all subranges subsumed therein. For example, the stated range "1 to 10" should be considered to encompass any and all subranges between (and including) the minimum value of 1 and the maximum value of 10, i.e., all subranges beginning with a minimum value of 1 or more, e.g., 1 to 6.1, and ending with a maximum value of 10 or less, e.g., 5.5 to 10.
[0024] Alloy composition The novel aluminum alloys are described below. The properties of the aluminum alloy fin stock vary depending on its composition. The aluminum alloy fin stock disclosed herein possesses several advantageous properties. The aluminum alloy fin stock can be produced in the form of a sheet, a sheet, or a plate, and possesses desirable strength before, during, and after brazing, even at gauges of 200 μm or less than 100 μm, making it suitable for the manufacture of fins for heat exchanger applications. The aluminum alloy material also possesses thermal conductivity and corrosion potential that are suitable for the production of fin stock.
[0025] The aluminum alloy fin stock disclosed herein may include higher contents of one or more of Cu, Si, and Mg compared to known fin stock alloys. The aluminum alloy fin stock composition and / or its production process results in improved material properties such as reduced fin crushing during brazing, increased strength after brazing, improved thermal conductivity, improved sagging resistance, and increased anodic corrosion potential. The aluminum alloy fin stock possesses improved strength, thermal conductivity, and / or corrosion potential compared to known alloys used to produce the fin stock. The relatively high levels of non-aluminum components in the aluminum alloy fin stock allow for a variety of metal inputs, as it can be produced from input metals incorporating aluminum that are easily recycled.
[0026] In some examples, the aluminum alloy fin stock is produced by a process that includes a heat treatment (intermediate annealing) step prior to the final cold rolling step. The intermediate annealing is performed at a temperature between 200° C. and 400° C. for about 30 minutes to 2 hours (e.g., about 1 hour to 2 hours). The intermediate annealing is followed by a cold rolling step resulting in a specified reduction in thickness ("% cold work", as defined later in this specification). In some examples, the combination of the above process steps (intermediate annealing and subsequent cold rolling) increases the pre-braze strength and improves the post-braze coarse grain structure, thereby improving the sag resistance of the improved aluminum fin stock, and also affects the thermal conductivity and corrosion potential, resulting in a material with a favorable combination of characteristics and properties.
[0027] In some examples, the alloy may have the following elemental composition provided in Table 1. Table 1 TIFF0007555339000001.tif72122
[0028] In some examples, the alloy may have the following elemental composition provided in Table 2. Table 2 TIFF0007555339000002.tif72122
[0029] In some examples, the alloy may have the following elemental composition as provided in Table 3. Table 3 TIFF0007555339000003.tif72122
[0030] In some examples, the alloy may have the following elemental composition as provided in Table 4. Table 4 TIFF0007555339000004.tif71121
[0031] In some examples, the alloy may have the following elemental composition as provided in Table 5. Table 5 TIFF0007555339000005.tif74121
[0032] In some examples, the alloy may have the following elemental composition as provided in Table 6. Table 6 TIFF0007555339000006.tif70120
[0033] In some examples, the alloy may have the following elemental composition as provided in Table 7. Table 7 TIFF0007555339000007.tif72120
[0034] In some examples, the alloy may have the following elemental composition as provided in Table 8. Table 8 TIFF0007555339000008.tif70120
[0035] In some examples, the alloy may have the following elemental composition as provided in Table 9. Table 9 TIFF0007555339000009.tif69122
[0036] In some examples, the alloy may have the following elemental composition as provided in Table 10. Table 10 TIFF0007555339000010.tif72121
[0037] In some examples, the alloy comprises silicon (Si) in an amount of about 0.9 wt.% to about 1.4 wt.% (e.g., about 0.95 wt.% to about 0.35 wt.%, about 1.0 wt.% to about 1.30 wt.%, about 1.10 wt.% to 1.2 wt.%, 0.8 wt.% to 1.30 wt.%) based on the total weight of the alloy. For example, the alloy may be about 0.90 wt%, about 0.91 wt%, about 0.92 wt%, about 0.93 wt%, about 0.94 wt%, about 0.95 wt%, about 0.96 wt%, about 0.97 wt%, about 0.98 wt%, about 0.99 wt%, about 1.00 wt%, about 1.01 wt%, about 1.02 wt%, about 1.03 wt%, about 1.04 wt%, about 1.05 wt%, about 1.06 wt%, about 1.07 wt%, about 1.08 wt%, about 1.09 wt%, about 1.10 wt%, about 1.11 wt%, about 1.12 wt%, about 1.13 wt%, about 1.14 wt%, about 1.15 wt%, about 1.16 wt%, about 1.17 wt%, about 1.18 wt%, about 1.19 wt%, about 2.2 wt%, about 2.23 wt%, about 2.24 wt%, about 2.25 wt%, about 2.26 wt%, about 2.27 wt%, about 2.28 wt%, about 2.29 wt%, about 2.30 wt%, about 2.31 wt%, about 2.32 wt%, about 2.33 wt%, about 2.34 wt%, about 2.35 wt%, about 2.36 wt%, about 2.37 wt%, about 2.38 wt%, about 2.39 wt%, about 2.40 wt%, about 2.41 wt%, about 2.42 wt%, about 2.43 wt%, about 2.44 wt%, about 2.45 wt%, about 2.46 wt%, about 2.47 wt%, about The aluminum alloy may contain about 1.16 wt%, about 1.17 wt%, about 1.18 wt%, about 1.19 wt%, about 1.20 wt%, about 1.21 wt%, about 1.22 wt%, about 1.23 wt%, about 1.24 wt%, about 1.25 wt%, about 1.26 wt%, about 1.27 wt%, about 1.28 wt%, about 1.29 wt%, about 1.30 wt%, about 1.31 wt%, about 1.32 wt%, about 1.33 wt%, about 1.34 wt%, about 1.35 wt%, about 1.36 wt%, about 1.37 wt%, about 1.38 wt%, about 1.39 wt%, or about 1.40 wt% Si. All percentages are expressed in weight percent. In particular, the Si content affects the melting temperature of the aluminum alloy. Increasing the Si content reduces the melting point of the aluminum alloy. Therefore, for an aluminum alloy fin stock to be brazable, the Si content of the alloy must be low enough so that the alloy does not melt during the brazing cycle. On the other hand, a relatively high Si content in the alloy leads to the formation of AlMnSi dispersoids, which results in beneficial dispersoid strengthening of the matrix and improved strength properties of the alloy. The Si content used in the disclosed fin stock alloy balances the above factors.
[0038] In some examples, the alloy also includes iron (Fe) in an amount of about 0.30 wt % to about 0.60 wt % (e.g., about 0.35 wt % to about 0.60 wt %, about 0.40 wt % to about 0.60 wt %, or about 0.41 wt % to about 0.47 wt %) based on the total weight of the alloy. For example, the alloy may include about 0.30 wt %, about 0.31 wt %, about 0.32 wt %, about 0.33 wt %, about 0.34 wt %, about 0.35 wt %, about 0.36 wt %, about 0.37 wt %, about 0.38 wt %, about 0.39 wt %, about 0.40 wt %, about 0.41 wt %, about 0.42 wt %, about 0.43 wt %, about 0.44 wt %, about 0.45 wt % , about 0.46 wt%, about 0.47 wt%, about 0.48 wt%, about 0.49 wt%, about 0.50 wt%, about 0.51 wt%, about 0.52 wt%, about 0.53 wt%, about 0.54 wt%, about 0.55 wt%, about 0.56 wt%, about 0.57 wt%, about 0.58 wt%, about 0.59 wt%, or about 0.60 wt% Fe. All percentages are expressed in weight percent. In aluminum alloys, Fe can be part of the intermetallic components, which can include Mn, Si, and other elements. It is often beneficial to control the Fe content of aluminum alloys to affect the content of the crude intermetallic components.
[0039] In some examples, the disclosed alloys include copper (Cu) in an amount of about 0.2 wt.% to about 0.60 wt.% (e.g., about 0.20 wt.% to about 0.40 wt.% or about 0.40 wt.% to about 0.55 wt.%) based on the total weight of the alloy. For example, the alloys may include about 0.20 wt.%, about 0.21 wt.%, about 0.22 wt.%, about 0.23 wt.%, about 0.24 wt.%, about 0.25 wt.%, about 0.26 wt.%, about 0.27 wt.%, about 0.28 wt.%, about 0.29 wt.%, about 0.30 wt.%, about 0.31 wt.%, about 0.32 wt.%, about 0.33 wt.%, about 0.34 wt.%, about 0.35 wt.%, about 0.36 wt.%, about 0.37 wt.%, about 0.38 wt.%, about 0.39 wt.%, about 0.40 wt.%, about 0.45 wt.%, about 0.46 wt.%, about 0.47 wt.%, about 0.48 wt.%, about 0.49 wt.%, about 0.50 wt.%, about 0.51 wt.%, about 0.52 wt.%, about 0.53 wt.%, about 0.54 wt.%, about 0.55 wt.%, about 0.56 wt.%, about 0.57 wt.%, about 0.58 wt.%, about 0.59 wt.%, about 0.60 wt.%, about 0.61 wt.%, about 0.62 wt.%, about 0.63 wt.%, about 0.64 w The aluminum alloy may contain about 0.41 wt%, about 0.42 wt%, about 0.43 wt%, about 0.44 wt%, about 0.45 wt%, about 0.46 wt%, about 0.47 wt%, about 0.48 wt%, about 0.49 wt%, about 0.50 wt%, about 0.51 wt%, about 0.52 wt%, about 0.53 wt%, about 0.54 wt%, about 0.55 wt%, about 0.56 wt%, about 0.57 wt%, about 0.58 wt%, about 0.59 wt%, or about 0.60 wt% Cu. All percentages are expressed in weight percent. Cu in solid solution increases the strength of the aluminum alloy. An increase in Cu content may also lead to the formation of Cu-containing AlMnCu dispersoids, which store Mn and dissolve during brazing, resulting in the release of Mn into solid solution. This process improves post-braze strength, and the relatively high Cu content of the fin stock alloy allows for cost savings and improved recyclability.
[0040] In some examples, the alloy includes manganese (Mg) in an amount of about 1.0 wt % to about 1.7 wt % (e.g., about 1.10 wt % to about 1.65 wt %, about 1.15 wt % to about 1.35 wt %, or about 1.2 wt % to about 1.35 wt %) based on the total weight of the alloy. For example, the alloy includes manganese (Mg) in an amount of about 1.0 wt %, about 1.01 wt %, about 1.02 wt %, about 1.03 wt %, about 1.04 wt %, about 1.05 wt %, about 1.06 wt %, about 1.07 wt %, about 1.08 wt %, about 1.09 wt %, about 1.1 wt %, about 1.11 wt %, about 1.12 wt %, about 1.13 wt %, about 1.14 wt %, about 1.15 wt %, about 1.16 wt %, about 1.1 7% by weight, approximately 1.18% by weight, approximately 1.19% by weight, approximately 1.2% by weight, approximately 1.21% by weight, approximately 1.22% by weight, approximately 1.23% by weight, approximately 1.24% by weight, approximately 1.25% by weight, approximately 1.26 Weight%, about 1.27 weight%, about 1.28 weight%, about 1.29 weight%, about 1.3 weight%, about 1.31 weight%, about 1.32 weight%, about 1.33 weight%, about 1.34 weight%, about 1.35 weight% %, about 1.36% by weight, about 1.37% by weight, about 1.38% by weight, about 1.39% by weight, about 1.4% by weight, about 1.41% by weight, about 1.42% by weight, about 1.43% by weight, about 1.44% by weight , about 1.45% by weight, about 1.46% by weight, about 1.47% by weight, about 1.48% by weight, about 1.49% by weight, about 1.50% by weight, about 1.51% by weight, about 1.52% by weight, about 1.53% by weight, The alloy may contain about 1.54%, about 1.55%, about 1.56%, about 1.57%, about 1.58%, about 1.59%, about 1.60%, about 1.61%, about 1.62%, about 1.63%, about 1.64%, about 1.65%, about 1.66%, about 1.67%, about 1.68%, about 1.69%, or about 1.7% Mn by weight. All percentages are expressed as weight percent. Mn in solid solution increases the strength of the aluminum alloy and shifts the corrosion potential to more cathodic conditions. When present, (FeMn)-Al in fine and dense dispersions. 6 Or Al 15 Mn 3 S 2 Dispersoids of Fe, Mn, Al, and Si, to name a few, can strengthen aluminum alloys by strengthening the particles.15 (FeMn) 3 S 2 , Al 5 FeSi or Al 8 FeMg 3 S 6 These combine during solidification to form various intermetallic constituents, i.e. grains, within the microstructure such as Mn. Higher Mn contents, especially in combination with higher Fe contents, can lead to the formation of coarse Mn-Fe intermetallic constituents.
[0041] In some examples, the alloy comprises zinc (Zn) in an amount of about 0.1 wt % to about 3.0 wt % (e.g., about 0.5 wt % to about 2.8 wt %, about 1.0 wt % to about 2.5 wt %, about 1.5 wt % to about 3.0 wt %, about 1.5 wt % to about 2.75 wt %, or about 1.9 wt % to about 2.6 wt %) based on the total weight of the alloy. For example, the alloy may be about 0.1 wt%, about 0.11 wt%, about 0.12 wt%, about 0.13 wt%, about 0.14 wt%, about 0.15 wt%, about 0.16 wt%, about 0.17 wt%, about 0.18 wt%, about 0.19 wt%, about 0.2 wt%, about 0.21 wt%, about 0.22 wt%, about 0.23 wt%, about 0.24 wt%, about 0.25 wt%, about 0.26 wt%, about 0.27 wt%, about 0.28 wt%, about 0.29 wt%, about 0.3 wt%, about 0.31 wt%, about 0.32 wt%, about 0.33 wt%, about 0.34 wt%, about 0.35 wt%, about 0.36 wt%, about 0.37 wt%, about 0.38 wt%, about 0.39 wt%, about 0.40 wt%, about 0.41 wt%, about 0.42 wt%, about 0.43 wt%, about 0.44 wt%, about 0.45 wt%, about 0.46 wt%, about 0.47 wt%, about 0.48 wt%, about 0.49 wt%, about 0.50 wt%, about 0.51 wt%, about 0.52 wt%, about 0.53 wt%, about 0.54 wt%, about 0.55 wt%, about 0.56 wt%, about 0.57 wt%, about 0.58 wt%, about 0.59 wt%, about 0.60 wt%, about 0.61 wt%, about 0.62 wt%, about 0.63 wt%, about 0.64 wt%, about 0.65 wt%, about 0 .33% by weight, approximately 0.34% by weight, approximately 0.35% by weight, approximately 0.36% by weight, approximately 0.37% by weight, approximately 0.38% by weight, approximately 0.39% by weight, approximately 0.4% by weight, approximately 0.41% by weight, approximately 0.42% by weight, approximately 0.43% by weight, approximately 0.44% by weight, approximately 0 .45% by weight, approximately 0.46% by weight, approximately 0.47% by weight, approximately 0.48% by weight, approximately 0.49% by weight, approximately 0.5% by weight, approximately 0.51% by weight, approximately 0.52% by weight, approximately 0.53% by weight, approximately 0.54% by weight, approximately 0.55% by weight, approximately 0.56% by weight, approximately 0 .57% by weight, approximately 0.58% by weight, approximately 0.59% by weight, approximately 0.6% by weight, approximately 0.61% by weight, approximately 0.62% by weight, approximately 0.63% by weight, approximately 0.64% by weight, approximately 0.65% by weight, approximately 0.66% by weight, approximately 0.67% by weight, approximately 0.68% by weight, approximately 0 .69% by weight, approximately 0.7% by weight, approximately 0.71% by weight, approximately 0.72% by weight, approximately 0.73% by weight, approximately 0.74% by weight, approximately 0.75% by weight, approximately 0.76% by weight, approximately 0.77% by weight, approximately 0.78% by weight, approximately 0.79% by weight, approximately 0.8% by weight, approximately 0. 81% by weight, approximately 0.82% by weight, approximately 0.83% by weight, approximately 0.84% by weight, approximately 0.85% by weight, approximately 0.86% by weight, approximately 0.87% by weight, approximately 0.88% by weight, approximately 0.89% by weight, approximately 0.9% by weight, approximately 0.91% by weight, approximately 0.92% by weight, approximately 0. 93% by weight, approximately 0.94% by weight, approximately 0.95% by weight, approximately 0.96% by weight, approximately 0.97% by weight, approximately 0.98% by weight, approximately 0.99% by weight, approximately 1.0% by weight, approximately 1.01% by weight, approximately 1.02% by weight, approximately 1.03% by weight, approximately 1.04% by weight, approximately 1.05 wt%, about 1.06 wt%, about 1.07 wt%, about 1.08 wt%, about 1.09 wt%, about 1.1 wt%, about 1.11 wt%, about 1.12 wt%, about 1.13 wt%, about 1.14 wt%, about 1.15 wt%, about 1.16 wt%, about 1.17 wt%, about 1.18 wt%, about 1.19 wt%, about 1.2 wt%, about 1.21 wt%, about 1.22 wt%, about 1.23 wt%, about 1.24 wt%, about 1.25 wt%, about 1.26 wt%, about 1.27 wt%, about 1.28 wt%, about 1.29 wt%, about 1.3 wt%, about 1.31 wt%, about 1.32 wt%, about 1.33 wt%, about 1.34 wt%, about 1.35 wt%, about 1.36 wt%, about 1.37 wt%, about 1.38 wt%, about 1.39 wt%, about 1.4 wt%, about 1.41 wt%, about 1.42 wt%, about 1.43 wt%, about 1.44 wt%, about 1.45 wt%, about 1.46 wt%, about 1.47 wt%, about 1.48 wt%, about 1.49 wt%, about 1.5 wt%, about 1.51 wt%, about 1.52 wt%, about 1.53 wt%, about 1.54 wt%, about 1.55 wt%, about 1.56 wt%, about 1.57 wt%, about 1.58 wt%, about 1.59 wt%, about 1.6 wt%, about 1.61 wt%, about 1.62 wt%, about 1.63 wt%, about 1.64 wt%, about 1.65 wt%, about 1.66 wt%, about 1.67 wt%, about 1.68 wt%, about 1.69 wt%, about 1.7 wt%, about 1.71 wt%, about 1.72 wt%, about 1.73 wt%, about 1.74 wt%, about 1.75 wt%, about 1.76 wt%, about 1.77 wt%, about 1.78 wt%, about 1.79 wt%, about 1.8 wt%, about 1.81 wt%, about 1.82 wt%, about 1.83 wt%, about 1.84 wt%, about 1.85 wt%, about 1.86 wt%, about 1.87 wt%, about 1.88 wt%, about 1.89 wt%, about 1.9 wt%, about 1.91 wt%, about 1.92 wt%, about 1.93 wt%, about 1.94 wt%, about 1.95 wt%, about 1.96 wt%, about 1.97 wt%, about 1.98 wt%, about 1.99 wt%, about 2.0 wt%, about 2.01 wt%, about 2.02 wt%, about 2.03 wt%, about 2.04 wt%, about 2.05 wt%, about 2.06 wt%, about 2.07 wt%, about 2.08 wt%, about 2.09 wt%, about 2.1 wt%, about 2.11 wt%, about 2.12 wt%, about 2.13 wt%, about 2.14 wt%, about 2.15 wt%, about 2.16 wt%, about 2.17% by weight, approximately 2.18% by weight, approximately 2.19% by weight, approximately 2.2% by weight, approximately 2.21% by weight, approximately 2.22% by weight, approximately 2.23% by weight, approximately 2.24% by weight, approximately 2.25% by weight, approximately 2.26% by weight, approximately 2.27% by weight , about 2.28% by weight, about 2.29% by weight, about 2.3% by weight, about 2.31% by weight, about 2.32% by weight, about 2.33% by weight, about 2.34% by weight, about 2.35% by weight, about 2.36% by weight, about 2.37% by weight, about 2.3 8% by weight, about 2.39% by weight, about 2.4% by weight, about 2.41% by weight, about 2.42% by weight, about 2.43% by weight, about 2.44% by weight, about 2.45% by weight, about 2.46% by weight, about 2.47% by weight, about 2.48% by weight, About 2.49 weight%, about 2.5 weight%, about 2.51 weight%, about 2.52 weight%, about 2.53 weight%, about 2.54 weight%, about 2.55 weight%, about 2.56 weight%, about 2.57 weight%, about 2.58 weight%, about 2.59 weight% Amount %, about 2.6% by weight, about 2.61% by weight, about 2.62% by weight, about 2.63% by weight, about 2.64% by weight, about 2.65% by weight, about 2.66% by weight, about 2.67% by weight, about 2.68% by weight, about 2.69% by weight, about 2 .7% by weight, approximately 2.71% by weight, approximately 2.72% by weight, approximately 2.73% by weight, approximately 2.74% by weight, approximately 2.75% by weight, approximately 2.76% by weight, approximately 2.77% by weight, approximately 2.78% by weight, approximately 2.79% by weight, approximately 2.8% by weight, The fin stock aluminum alloy may contain about 2.81 wt%, about 2.82 wt%, about 2.83 wt%, about 2.84 wt%, about 2.85 wt%, about 2.86 wt%, about 2.87 wt%, about 2.88 wt%, about 2.89 wt%, about 2.9 wt%, about 2.9 wt%, about 2.91 wt%, about 2.92 wt%, about 2.93 wt%, about 2.94 wt%, about 2.95 wt%, about 2.96 wt%, about 2.97 wt%, about 2.98 wt%, about 2.99 wt%, or about 3.0 wt% Zn. All percentages are expressed in weight percent. Zn is typically added to aluminum alloys to shift the corrosion potential toward the anodic end of the scale. In the disclosed fin stock aluminum alloy, the relatively high Zn content of up to 3 wt% compensates for the shift in corrosion potential due to the increased Si and Cu content, thus resulting in more anodic corrosion potential. More anodic corrosion potential allows the fins made from the alloy to act sacrificially to protect the heat exchanger tubes, thus improving the overall corrosion resistance of the heat exchanger.
[0042] In certain examples, the alloy may include Mg in an amount of about 0.01 wt.% to about 0.25 wt.% (e.g., about 0.05 wt.% to about 0.20 wt.% or about 0.10 wt.% to about 0.20 wt.%) based on the total weight of the alloy. For example, the alloy may include about 0.01 wt%, about 0.02 wt%, about 0.03 wt%, about 0.04 wt%, about 0.05 wt%, about 0.06 wt%, about 0.07 wt%, about 0.08 wt%, about 0.09 wt%, about 0.1 wt%, about 0.11 wt%, about 0.12 wt%, about 0.13 wt%, about 0.14 wt%, about 0.15 wt%, about 0.16 wt%, about 0.17 wt%, about 0.18 wt%, about 0.19 wt%, about 0.2 wt%, about 0.21 wt%, about 0.22 wt%, about 0.23 wt%, about 0.24 wt%, or about 0.25 wt% Mg. All percentages are expressed in weight percent. Mg contributes to the strength of the aluminum alloys described herein through solid solution strengthening.
[0043] In some examples, the ratio of Cu to Zn is 2:1 to 1:15, e.g., 1:1 to 1:10, or 1:5 to 1:10. The ratio of Cu to Zn is 2:1, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, or 1:15.
[0044] The aluminum alloys described herein may include titanium (Ti) in an amount of up to about 0.10 wt% (e.g., 0 to about 0.05 wt%, about 0.001 to about 0.04 wt%, or about 0.01 to about 0.03 wt%) based on the total weight of the alloy. For example, the alloy may include about 0.001 wt%, about 0.002 wt%, about 0.003 wt%, about 0.004 wt%, about 0.005 wt%, about 0.006 wt%, about 0.007 wt%, about 0.008 wt%, about 0.009 wt%, about 0.01 wt%, about 0.02 wt%, about 0.03 wt%, about 0.04 wt%, about 0.05 wt%, about 0.06 wt%, about 0.07 wt%, about 0.08 wt%, about 0.09 wt%, or about 0.1 wt% Ti. In some cases, Ti is absent in the alloy (i.e., 0 wt.%). All percentages are expressed in wt.%.
[0045] Optionally, the alloy composition may further include other trace elements, sometimes referred to as impurities, in amounts of about 0.05% by weight or less, 0.04% by weight or less, 0.03% by weight or less, 0.02% by weight or less, or 0.01% by weight or less, respectively. These impurities may include, but are not limited to, Ga, V, Ni, Sc, Ag, B, Bi, Zr, Li, Pb, Sn, Ca, Hf, Sr, or combinations thereof. Thus, Ga, V, Ni, Sc, Ag, B, Bi, Zr, Li, Pb, Sn, Ca, Hf, or Sr may be present in the alloy in amounts of 0.05% by weight or less, 0.04% by weight or less, 0.03% by weight or less, 0.02% by weight or less, or 0.01% by weight or less. In certain embodiments, the sum of all impurities does not exceed 0.15% by weight (e.g., 0.1% by weight). All percentages are expressed in weight percent. In certain embodiments, the remaining percentage of the alloy is aluminum.
[0046] Process for making aluminum alloy fin stock In certain embodiments, the disclosed alloy compositions are products of the disclosed methods. Without intending to limit the disclosure, the properties of aluminum alloys are determined in part by the formation of the microstructure during preparation of the alloy. In certain embodiments, the method of preparation of the alloy composition can affect or even determine that the alloy has suitable properties for a desired application.
[0047] The process for producing aluminum alloy fin stock can involve direct chill (DC) casting of the aluminum alloy into an ingot. After DC casting, the process includes preheating the ingot for hot rolling. Preheat temperature and hot rolling time are closely controlled to low levels to retain large grain size and high strength after the finished fin stock is brazed. In some examples, prior to hot rolling, the ingot can be preheated in a furnace at a suitable heating rate, e.g., 50°C / hour, for up to about 12 hours, up to about 500°C, e.g., 450-480°C, and then the temperature can be held at about 450-500°C, e.g., about 470-480°C, for 5-7 hours ("soak" or "soaking"). After preheating and soaking, the ingot is hot rolled to a gauge between 2 and 10 mm, for example, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, or 10 mm. This may be called the "exit gauge" after hot rolling.
[0048] The process for producing the aluminum alloy fin stock then includes a cold rolling step to create the desired thickness (gauge) and other properties of the material. For example, after the hot rolling step, the hot rolled aluminum alloy is cold rolled to reduce the thickness of the material to a thickness or gauge of 1-2 mm, e.g., 1 mm (first cold roll gauge) during the first cold rolling step. This may include multiple cold rolling passes. It is then further cold rolled to a thickness or gauge of 100-200 μm (intermediate cold roll gauge) during an intermediate cold rolling step. This may also involve multiple passes. Depending on the hot rolling gauge, the desired final thickness, and other properties described below, the aluminum alloy may require more or fewer cold rolling passes to achieve the desired gauge. The number of cold rolling passes is not limited and can be suitably adjusted depending, for example, on the desired thickness of the final sheet and other properties of the material.
[0049] After intermediate cold rolling, the process for producing the aluminum alloy fin stock may include an intermediate annealing step to develop desired properties of the aluminum alloy fin stock. The term "intermediate annealing" refers to a heat treatment applied between the cold rolling steps. As described herein, intermediate annealing is applied between the intermediate cold rolling step and the final cold rolling step. Intermediate annealing involves heating the aluminum alloy to a temperature of about 200°C to about 400°C, e.g., about 225°C to about 400°C, about 225°C to about 375°C, about 225°C to about 350°C, about 225°C to about 325°C, about 300°C to about 375°C, about 325°C to about 350°C, about 340°C to about 360°C, about 290°C to about 360°C, or about 345°C to about 350°C, maintaining the intermediate annealing temperature for 3 to 5 hours, e.g., about 4 hours, and then cooling. The temperature maintenance period of about 200°C to about 400°C can be called "soak" or "soaking". A constant rate of 40°C / hour to 50°C / hour, for example 50°C / hour, can be applied for heating and cooling the material before and after soaking. The intermediate annealing conditions affect the structure and properties of the aluminum alloy fin stock in various ways. For example, a higher intermediate annealing temperature can reduce the strength after brazing. Therefore, the intermediate annealing conditions are selected within the ranges specified herein to provide the desired properties of the aluminum alloy fin stock.
[0050] After the intermediate annealing, a final cold rolling is performed to achieve a cold work % (CW%) during the final cold rolling step (which may include multiple cold rolling passes) of 20%-45%, 25%-40%, 20%-40%, 20%-35%, 25%-35%, or 5%-45%. In some embodiments, the CW% is less than or equal to 35%, while in other embodiments, the CW% is greater than 35%. After the final cold rolling step, the aluminum alloy fin blank of the present invention possesses a thickness (gauge) of about 45-100 μm, 45-90 μm, 47-85 μm, or 50-83 μm.
[0051] The final cold rolling step affects the structure and properties of the aluminum alloy fin stock. For example, increasing the CW% increases the pre-braze strength of the aluminum material (ultimate tensile strength (UTS), yield strength (YS), or both measured in the pre-braze state). Therefore, the CW% used is adjusted within the ranges specified herein to achieve the desired properties of the aluminum alloy fin stock.
[0052] The process for producing the aluminum alloy fin stock disclosed herein can be carried out in a manner that results in an aluminum material having a desired temper. For example, the process can be carried out to provide an aluminum material that may be described as having or being "strain hardened," "cold worked," and / or an "H1X" temper (e.g., H14 temper). In some examples, the improved fin stock aluminum alloy material described herein may be produced in H14, H16, or H18 tempers. It is understood that the particular property ranges are related to the temper designation. It is also understood that the temper designation refers to the pre-braze properties of the material.
[0053] characteristics The aluminum alloy fin stocks disclosed herein possess a number of advantageous properties, characteristics, or parameters that, individually or in various combinations, allow the aluminum alloy materials described herein to be used in the production of fins for heat exchangers. However, it should be understood that the scope of the invention is not limited to any particular use or application, and that the properties of the aluminum alloy fin stocks may be advantageous in a variety of other applications. Some of these properties are described below. Some other properties, which may not be specifically described, may result from the composition and / or production process used to fabricate the aluminum alloy fin stocks described herein.
[0054] Some embodiments of the aluminum alloy materials described herein are produced as sheets, e.g., less than 4 mm thick, e.g., 45-100 μm thick. The aluminum alloy sheets may be produced in H1X tempers (e.g., H14, H16, or H18 tempers). The aluminum alloy materials described herein may possess one or more of the following properties in any combination: a UTS of 210 MPa or more (i.e., at least 210 MPa) or between 210 and 230 MPa, measured in the pre-braze state, a UTS of 150 MPa or more (i.e., at least 150 MPa) or between 150 and 170 MPa, measured after brazing, a sag resistance of 25 to 33 mm, measured after brazing; a thermal conductivity of 40 to 48, 43 to 47, or 44 to 45 IACS, measured after brazing; an open circuit potential corrosion value (vs. Standard Calomel Electrode (SCE), also referred to as "corrosion potential") of -740 mV or less (e.g., -750 mV), and / or a coarse post-braze grain microstructure of 80 to 400 μm. Parameters measured "after brazing" or "post-brazing" (also called "post-braze") are measured after a simulated brazing cycle during which an aluminum alloy sample is heated to a temperature of 595°C to 610°C and then cooled to room temperature in about 20 minutes. Parameters measured before brazing (the "pre-brazing" or "pre-brazed" condition), also called "pre-braze" parameters, are measured before or without subjecting the material to any brazing cycle.
[0055] The disclosed aluminum alloy fin stock has improved strength and electrical conductivity and exhibits lower corrosion potential values. The disclosed aluminum alloy fin stock can also withstand a copper accelerated salt spray (CASS) test according to ASTM B368(2014) for at least 20 days without separation from the brazed joint. CASS testing is generally performed by forming a coupon of the fin and tube, brazing to form the joint, and subjecting the brazed coupon to testing. Due to the above characteristics and advantages, the aluminum alloy fin stock of the present invention can be advantageously used in a variety of uses and applications, which are described in more detail below.
[0056] Use and applications The aluminum alloy fin stock described herein can be used in a variety of applications, including, but not limited to, heat exchangers. In one example, the aluminum alloy fin stock can be used in automotive heat exchangers, such as, but not limited to, radiators, condensers, and evaporators. For example, the improved aluminum alloy fin stock can be used in the manufacture of various devices that use heat exchangers and are produced by brazing, such as devices used in heating, ventilation, air conditioning, and refrigeration (HVAC&R). The uses and applications of the aluminum alloy fin stock described herein are within the scope of the present invention, as are objects, forms, devices, and the like made of or including the aluminum alloys described herein. Processes for making, producing, or manufacturing such objects, forms, devices, and the like are also within the scope of the present invention.
[0057] The aluminum alloys described herein are suitable for fabrication or manufacturing processes requiring the joining of metal surfaces by brazing. Brazing is a metal joining process in which a filler metal is heated above its melting point and dispersed between two or more mating parts by capillary action. The use of aluminum alloys in brazing and related processes, and the results, such as objects produced according to manufacturing processes involving brazing, are commonly referred to as "brazing applications." The components of the heat exchanger described herein are joined by brazing during the manufacturing process. The filler metal melts during brazing and becomes the filler metal available to flow to the contact points between the components being brazed by capillary action.
[0058] One exemplary object that can be fabricated using the aluminum alloy fin stock described herein is a heat exchanger. Heat exchangers are produced by assembly of parts with tubes, plates, fins, headers, and side supports, to name a few. For example, a radiator is constructed with tubes, fins, headers, and side supports. Except for the fins, which are typically bare, meaning they are not covered with Al-Si alloy, all other parts of the heat exchanger are typically covered with braze cladding on one or both sides. Once assembled, the heat exchanger unit is secured by bands or such devices, holding the unit together with flux and brazing. Brazing is usually done by passing the unit through a tunnel furnace. Brazing can also be done by dipping in molten salt or in a batch or semi-batch process. The unit is heated to a brazing temperature of 590°C to 610°C, a joint is created by capillary action, and then dipped at the appropriate temperature until it cools below the solidus temperature of the filler metal. Heating rates vary depending on the type of furnace and the size of the heat exchanger being produced. Some other examples of objects that can be fabricated using the aluminum alloy fin stock described herein are evaporators, radiators, heaters or condensers.
[0059] The first embodiment is an aluminum alloy containing about 0.9-1.4 wt.% Si, about 0.3-0.6 wt.% Fe, about 0.20-0.60 wt.% Cu, about 1.0-1.7 wt.% Mn, about 0.01-0.25 wt.% Mg, about 0.1-3.0 wt.% Zn, and up to about 0.10 wt.% Ti, with the remainder being Al and impurities of 0.15 wt.% or less.
[0060] Embodiment 2 is the aluminum alloy of any preceding or subsequent embodiment, wherein the aluminum alloy includes about 0.95-1.35 wt.% Si, about 0.3-0.6 wt.% Fe, about 0.20-0.60 wt.% Cu, about 1.0-1.7 wt.% Mn, about 0.01-0.25 wt.% Mg, about 0.1-3.0 wt.% Zn, up to about 0.10 wt.% Ti, with the balance being less than or equal to 0.15 wt.% Al and impurities.
[0061] Embodiment 3 is the aluminum alloy of any preceding or subsequent embodiment, wherein the aluminum alloy includes about 0.9-1.4 wt.% Si, about 0.35-0.6 wt.% Fe, about 0.20-0.60 wt.% Cu, about 1.0-1.7 wt.% Mn, about 0.01-0.25 wt.% Mg, about 0.1-3.0 wt.% Zn, up to about 0.10 wt.% Ti, with the balance being 0.15 wt.% or less of Al and impurities.
[0062] Embodiment 4 is the aluminum alloy of any preceding or subsequent embodiment, wherein the aluminum alloy includes about 0.9-1.4 wt.% Si, about 0.3-0.6 wt.% Fe, about 0.20-0.40 wt.% Cu, about 1.0-1.7 wt.% Mn, about 0.01-0.25 wt.% Mg, about 0.1-3.0 wt.% Zn, up to about 0.10 wt.% Ti, with the balance being less than or equal to 0.15 wt.% Al and impurities.
[0063] Embodiment 5 is the aluminum alloy of any preceding or subsequent embodiment, wherein the aluminum alloy includes about 0.9-1.4 wt.% Si, about 0.3-0.6 wt.% Fe, about 0.40-0.55 wt.% Cu, about 1.0-1.7 wt.% Mn, about 0.01-0.25 wt.% Mg, about 0.1-3.0 wt.% Zn, up to about 0.10 wt.% Ti, with the balance being less than or equal to 0.15 wt.% Al and impurities.
[0064] Embodiment 6 is the aluminum alloy of any preceding or subsequent embodiment, wherein the aluminum alloy includes about 0.9-1.4 wt.% Si, about 0.3-0.6 wt.% Fe, about 0.20-0.60 wt.% Cu, about 1.1-1.65 wt.% Mn, about 0.01-0.25 wt.% Mg, about 0.1-3.0 wt.% Zn, up to about 0.10 wt.% Ti, with the balance being less than or equal to 0.15 wt.% Al and impurities.
[0065] Embodiment 7 is the aluminum alloy of any preceding or subsequent embodiment, wherein the aluminum alloy includes about 0.9-1.4 wt.% Si, about 0.3-0.6 wt.% Fe, about 0.20-0.60 wt.% Cu, about 1.0-1.7 wt.% Mn, about 0.05-0.2 wt.% Mg, about 0.1-3.0 wt.% Zn, up to about 0.10 wt.% Ti, with the balance being less than or equal to 0.15 wt.% Al and impurities.
[0066] Embodiment 8 is an aluminum alloy containing about 0.9-1.4 wt.% Si, about 0.3-0.6 wt.% Fe, about 0.20-0.60 wt.% Cu, about 1.0-1.7 wt.% Mn, about 0.01-0.25 wt.% Mg, about 1-3.0 wt.% Zn, up to about 0.10 wt.% Ti, with the remainder being Al and impurities of 0.15 wt.% or less.
[0067] Embodiment 9 is an aluminum alloy containing about 0.9-1.4 wt.% Si, about 0.3-0.6 wt.% Fe, about 0.20-0.60 wt.% Cu, about 1.0-1.7 wt.% Mn, about 0.01-0.25 wt.% Mg, about 1.5-2.75 wt.% Zn, up to about 0.10 wt.% Ti, with the remainder being Al and impurities of 0.15 wt.% or less.
[0068] A tenth embodiment is an aluminum alloy comprising about 0.9-1.4 wt.% Si, about 0.3-0.6 wt.% Fe, about 0.20-0.60 wt.% Cu, about 1.0-1.7 wt.% Mn, about 0.01-0.25 wt.% Mg, about 0.1-3.0 wt.% Zn, up to about 0.05 wt.% Ti, with the remainder being Al and impurities up to 0.15 wt.%.
[0069]
[0023] Embodiment 11 is an aluminum alloy according to any preceding or subsequent embodiment, wherein the alloy is produced by a process including: direct chill casting the aluminum alloy into an ingot; hot rolling the ingot after direct chill casting; cold rolling the aluminum alloy to an intermediate thickness after hot rolling; intermediate annealing the aluminum alloy rolled to an intermediate thickness at 200-400°C after cold rolling; cold rolling the aluminum alloy after intermediate annealing to achieve a cold work % (CW %) of 20-40% to obtain a sheet having a thickness of 45-100 μm, 45-90 μm, 47-85 μm, or 50-83 μm.
[0070] Embodiment 12 is the aluminum alloy of the preceding or subsequent embodiments, wherein the intermediate annealing is performed at 250-360°C or 290-360°C.
[0071] Embodiment 13 is an aluminum alloy according to any preceding or subsequent embodiment, wherein the intermediate annealing time is 30-60 minutes.
[0072] Embodiment 14 is an aluminum alloy according to any preceding or subsequent embodiment, wherein the CW% is 30-40%.
[0073] Embodiment 15 is an aluminum alloy according to any preceding or subsequent embodiment, wherein the aluminum alloy has one or both of an ultimate tensile strength of at least 200 MPA when measured in the pre-brazed condition, or at least 150 MPA when measured after brazing.
[0074] Embodiment 16 is an aluminum alloy according to any preceding or subsequent embodiment, wherein the aluminum alloy has a corrosion potential of −740 mV or less, measured after brazing.
[0075] Embodiment 17 is an aluminum alloy according to any preceding or subsequent embodiment, wherein the aluminum alloy has a thermal conductivity of greater than 40% IACS, as measured after brazing.
[0076] An eighteenth embodiment is a heat exchanger comprising an aluminum alloy according to any preceding or subsequent embodiment.
[0077] Embodiment 19 is a process for making a heat exchanger comprising joining by brazing at least one first aluminum alloy form fabricated from the aluminum alloy of any preceding or subsequent embodiment with a second aluminum alloy form, the process comprising assembling and clamping two or more aluminum forms together and heating the two or more aluminum forms to a brazing temperature until a bond is created between the two or more aluminum forms by capillary action.
[0078] Example 20 is the process of example 19, wherein the first aluminum alloy can withstand a CASS test according to ASTM B368(2014) for at least 20 days without coming off the joint.
[0079] Embodiment 21 is the use of an aluminum alloy in the fabrication of the heat exchanger fins of any of the preceding or subsequent embodiments.
[0080] The following examples serve to further illustrate the invention but at the same time do not constitute any limitation thereof, whereas it should be clearly understood that various embodiments, modifications thereof and equivalents, which may suggest themselves to those skilled in the art after reading the description herein, may be used without departing from the spirit of the invention.
[0081] Example 1 Nine aluminum alloy samples were prepared with the compositions shown in Table 11 below. Each sample contained up to 0.15 wt% impurities with the remainder being Al. Each sample was prepared by direct chill casting of the aluminum alloy into an ingot and then hot rolling. The ingots produced by DC casting were preheated for hot rolling. The ingots were then hot rolled to the exit gauge and then cold rolled to the first cold roll gauge. The ingots were then further cold rolled to an intermediate cold roll gauge. The ingots were then intermediate annealed. After the intermediate anneal, a final cold roll was performed to a CW% of 20-40% resulting in each sample having a thickness of 45μm-100μm. Table 11 TIFF0007555339000012.tif130170
[0082] Each of the samples in Table 11 was then tested for mechanical properties, electrical conductivity, corrosion potential, and solidus temperature in the pre-brazing state, after standard brazing, and after high-speed brazing. During standard brazing, the samples were heated to a temperature of 605°C and cooled to room temperature in approximately 45 minutes to simulate the temperature-time profile of a commercial brazing process. High-speed brazing was performed at a much faster heating and cooling rate compared to the standard brazing cycle. The material was heated to a temperature of 600-605°C and cooled to room temperature in approximately 20 minutes. Yield strength, ultimate tensile strength, and uniform elongation were measured for all samples. Testing was performed according to ASTM B557 standard. Three samples of each alloy variant were tested and average values in both the pre-brazing and post-brazing states were reported. Electrical conductivity was reported as IACS% (International Annealed Copper Standard, assuming 100% pure copper conductivity). Yield strength, ultimate tensile strength, and elongation results are shown in Table 12 below. The solidus temperatures are also reported in Table 12. The thermal conductivity and corrosion potential measured after brazing are reported in Table 13. The experimental alloys had a minimum braze-resistant yield strength of 55 MPa and a higher ultimate tensile strength than the alloy of Comparative Example 1.
[0083] The open circuit potential corrosion value vs. standard calomel electrode (SCE) of -764 mV for Comparative Example 1 compared to -735 mV for Alloy H indicated that fin deformation would act sacrificially on any tube alloy if the corrosion potential difference was maintained between the tube and fin alloys at about 30-150 mV. Table 12 TIFF0007555339000013.tif101169Table 13 TIFF0007555339000014.tif86168
[0084] Each of the samples Comparative Example 1 and A-H were photographed using an optical microscope. Microstructural characterization was performed to examine the dispersoids, intermetallic size and distribution, and grain structure before and after brazing. The microstructures were characterized using HNO 3After removing smut by 2.5% HBF for 60 seconds, the sample was 4 The microstructures were examined by etching with a Barker etch. Figures 1A-I show the microstructure before brazing, Figures 2A-I show the microstructure after standard brazing, and Figures 3A-I show the microstructure after high speed cycle brazing. A Barker etch was used to reveal the grain structure. Figures 4A-I show plan views of the grain structure after standard brazing, and Figures 5A-I show plan views of the grain structure after high speed cycle brazing. Each of samples Comparative Example 1 and A-H was also photographed to show the cross-sectional grain structure before brazing (Figures 6A-I), after standard brazing (Figures 7A-I), and after high speed brazing (Figures 8A-I). For each set of micrographs, Figure A corresponds to Comparative Example 1, Figure B corresponds to Sample A, Figure C corresponds to Sample B, and so on.
[0085] Example 2 Alloy samples C, E, G, and H were prepared as in Example 1, except that the CW% was varied during the intermediate anneal at 350°C (prior to brazing). The results are shown in Table 14 below and in Figure 9A. As shown below and in Figure 9A, yield strength was improved when greater than 35% CW was performed compared to when 35% CW or less was performed. Ultimate tensile strength was also increased above 35% CW compared to when less than 35% CW was performed, except for sample E. Elongation% was decreased when greater than 35% CW was performed compared to when less than 35% CW was performed, except for sample H. Table 14 TIFF0007555339000015.tif56168
[0086] Example 3 Alloy samples C, E, G, and H were prepared as in Example 1, except that the CW% was changed after the intermediate anneal at 350°C (post-braze). The results are shown in Table 15 below and in Figure 9B. As shown below and in Figure 9B, with the exception of sample G, the yield strength improved when more than 35% CW was performed compared to when 35% CW or less was performed. With the exception of sample H, the ultimate tensile strength decreased when more than 35% CW was performed compared to when less than 35% CW was performed. In general, the elongation% remained about the same or decreased when more than 35% CW was performed compared to when 35% CW or less was performed. Table 15 TIFF0007555339000016.tif57168
[0087] Example 4 Alloy samples C, E, G and H were prepared as in Example 1, except that the intermediate annealing temperature was varied above 35% CW (before brazing). The results are shown in Table 16 below and in Figure 9C. As shown below and in Figure 9C, the yield strength, ultimate tensile strength, and % elongation all decreased at higher intermediate annealing temperatures. Table 16 TIFF0007555339000017.tif57166
[0088] Example 5 Alloy samples C, E, G and H were prepared as in Example 1, except that the effect of intermediate annealing temperature above 35% CW (post-braze) was varied. The results are shown in Table 17 below and in Figure 9D. As shown below and in Figure 9D, at higher intermediate annealing temperatures, yield strength decreased, elongation increased, and ultimate tensile strength stayed the same (sample C) or decreased (samples E, G and H). Table 17 TIFF0007555339000018.tif56168
[0089] Alloy samples C, E, G, and H were then subjected to either standard cycle or rapid cycle brazing and photographed as above. For samples subjected to standard brazing cycle with intermediate annealing at 250°C, the top view grain size after brazing is shown in Figures 10A-D, where Figure 10A corresponds to sample C, Figure 10B corresponds to sample E, Figure 10C corresponds to sample G, and Figure 10D corresponds to sample H. Similarly, for samples subjected to standard brazing cycle with intermediate annealing at 350°C, the top view grain size after brazing is shown in Figures 11A-D, where Figure 11A corresponds to sample C, Figure 11B corresponds to sample E, Figure 11C corresponds to sample G, and Figure 11D corresponds to sample H.
[0090] For samples with intermediate annealing at 250°C and subjected to high speed brazing cycles, the plan view grain size after brazing is shown in Figures 12A-D, where Figure 12A corresponds to Sample C, Figure 12B corresponds to Sample E, Figure 12C corresponds to Sample G, and Figure 12D corresponds to Sample H. Similarly, for samples with intermediate annealing at 350°C and subjected to high speed brazing cycles, the plan view grain size after brazing is shown in Figures 13A-D, where Figure 13A corresponds to Sample C, Figure 13B corresponds to Sample E, Figure 13C corresponds to Sample G, and Figure 13D corresponds to Sample H. Based on the grain structure images, it is observed that increasing the CW% above 35% reduces the grain size after brazing due to the increased driving force for recrystallization, but this effect does not appear to have a detrimental effect on sag resistance. Similarly, decreasing the intermediate annealing temperature from 350°C to 250°C and decreasing the CW% results in coarse grain size after brazing. The combination of intermediate annealing temperature and CW% was carefully selected based on the desired properties required. For example, different combinations of IA and CW% may be required to obtain shatter resistance and coarse grain size of the fins.
[0091] Example 6 The comparative sample and samples C, E, G and H were prepared and brazed as in Example 1. Fin and tube coupons were joined for each sample and each coupon was subjected to CASS testing according to ASTM B368 (2014). CASS testing was performed for 40 days. Corrosion activity was characterized by examining the brazed joints and the fins at 10, 20 and 40 days. At the end of the 40 days, each fin acted sacrificially to protect the tube.
[0092] The results shown for Examples 2-5 confirm that some elements such as Mg and Cu play a role in contributing to the yield strength and ultimate tensile strength of the alloy. However, increased Mg and Cu would typically also be expected to lead to increased corrosion when compared to samples with lower amounts of Mg and Cu. The images shown in Figures 14A-E are metallographic cross-sections taken at 100x magnification. Surprisingly and unexpectedly, as shown in Figures 14A-E, samples with increased amounts of Mg and Cu did not exhibit increased corrosion compared to samples with lower amounts of Mg and Cu. Thus, each of Samples C, E, G and H performed similarly to the comparative sample with respect to corrosion, but had other superior properties.
[0093] All patents, patent specifications, publications, and abstracts cited above are incorporated herein by reference in their entirety. Various embodiments of the invention have been described to achieve various objects of the invention. It should be recognized that these embodiments are merely illustrative of the principles of the invention. Numerous modifications and adaptations thereof will be readily apparent to those skilled in the art without departing from the spirit and scope of the invention as defined in the following claims.
Claims
1. An aluminum alloy for fins comprising 0.9-1.4 wt.% Si, 0.35-0.6 wt.% Fe, 0.20-0.60 wt.% Cu, 1.0-1.4 wt.% Mn, 0.11-0.25 wt.% Mg, 0.1-3.0 wt.% Zn, 0.001-0.10 wt.% Ti, the balance being Al and 0.15 wt.% or less of impurities.
2. % by weight of Si, 0.35 to 0.6 by weight of Fe, 0.20 to 0.60 by weight of Cu, 1.0 to 1.4 by weight of Mn, 0.11 to 0.25 by weight of Mg, 0.1 to 3.0 by weight of Zn, 0.001 to 0.10 by weight of Ti, the balance being Al and 0.15% or less by weight of impurities. The aluminum alloy for fins according to claim 1.
3. % of Si, 0.35 to 0.6 wt.% of Fe, 0.20 to 0.40 wt.% of Cu, 1.0 to 1.4 wt.% of Mn, 0.11 to 0.25 wt.% of Mg, 0.1 to 3.0 wt.% of Zn, 0.001 to 0.10 wt.% of Ti, the balance being Al and 0.15 wt.% or less of impurities. The aluminum alloy for fins according to claim 1.
4. % of Si, 0.35 to 0.6 wt.% of Fe, 0.40 to 0.55 wt.% of Cu, 1.0 to 1.4 wt.% of Mn, 0.11 to 0.25 wt.% of Mg, 0.1 to 3.0 wt.% of Zn, 0.001 to 0.10 wt.% of Ti, the balance being Al and 0.15 wt.% or less of impurities. The aluminum alloy for fins according to claim 1.
5. % of Si, 0.35 to 0.6 wt.% of Fe, 0.20 to 0.60 wt.% of Cu, 1.1 to 1.4 wt.% of Mn, 0.11 to 0.25 wt.% of Mg, 0.1 to 3.0 wt.% of Zn, 0.001 to 0.10 wt.% of Ti, the balance being Al and 0.15 wt.% or less of impurities. The aluminum alloy for fins according to claim 1.
6. % of Si, 0.35 to 0.6 wt.% of Fe, 0.20 to 0.60 wt.% of Cu, 1.0 to 1.4 wt.% of Mn, 0.11 to 0.2 wt.% of Mg, 0.1 to 3.0 wt.% of Zn, 0.001 to 0.10 wt.% of Ti, the balance being Al and 0.15 wt.% or less of impurities. The aluminum alloy for fins according to claim 1.
7. % of Si, 0.35 to 0.6 wt.% of Fe, 0.20 to 0.60 wt.% of Cu, 1.0 to 1.4 wt.% of Mn, 0.11 to 0.25 wt.% of Mg, 1.5 to 2.75 wt.% of Zn, 0.001 to 0.10 wt.% of Ti, the balance being Al and 0.15 wt.% or less of impurities. The aluminum alloy for fins according to claim 1.
8. % of Si, 0.35 to 0.6 wt.% of Fe, 0.20 to 0.60 wt.% of Cu, 1.0 to 1.4 wt.% of Mn, 0.11 to 0.25 wt.% of Mg, 0.1 to 3.0 wt.% of Zn, 0.001 to 0.05 wt.% of Ti, the balance being Al and 0.15 wt.% or less of impurities. The aluminum alloy for fins according to claim 1.
9. A method for manufacturing an aluminum alloy fin material, the method comprising: Direct chill casting the aluminum alloy for fins according to any one of claims 1 to 8 into an ingot; hot rolling the ingot after the direct chill casting; cold rolling the aluminum alloy to an intermediate gauge after the hot rolling; After the cold rolling, intermediate annealing the aluminum alloy rolled to the intermediate thickness at 200 to 400°C; cold rolling the aluminum alloy after the intermediate annealing to achieve a cold working percent (CW%) of 20-40% to obtain a sheet; wherein the sheet has a thickness of 45 to 100 μm, 45 to 90 μm, 47 to 85 μm, or 50 to 83 μm.
10. 10. The method of claim 9, wherein the intermediate annealing is at 250-360°C or 290-360°C.
11. The method according to claim 9 or 10, wherein the intermediate annealing time is between 30 and 60 minutes.
12. The method according to any one of claims 9 to 11, wherein the CW% is 30 to 40%.
13. 13. The method of any one of claims 9 to 12, wherein the sheet has an ultimate tensile strength of at least 200 MPa when measured in a pre-brazed state, or at least 150 MPa when measured after brazing by heating to a brazing temperature of 590°C to 610°C and cooling to below the solidus temperature of the filler metal, or both.
14. 14. The method according to any one of claims 9 to 13, wherein the sheet has a corrosion potential vs. Standard Calomel Electrode (SCE) of -740mV or less when measured after brazing by heating to a brazing temperature of 590°C to 610°C and cooling to below the solidus temperature of the filler metal.
15. 15. The method according to any one of claims 9 to 14, wherein the sheet has a thermal conductivity of greater than 40% IACS when measured after brazing by heating to a brazing temperature of 590°C to 610°C and cooling to below the solidus temperature of the filler metal.
16. A heat exchanger comprising the aluminum alloy for fins according to any one of claims 1 to 8.
17. A process for making a heat exchanger, comprising joining by brazing at least one first aluminium alloy form made from an aluminium alloy for fins according to any one of claims 1 to 8, assembling and securing two or more of said aluminum alloy forms together; heating two or more of said aluminum alloy forms to a brazing temperature until a bond is formed between the two or more of said aluminum alloy forms by capillary action; The process comprising:
18. 20. The process of claim 17, wherein the first aluminum alloy form is capable of withstanding at least 20 days of CASS testing according to ASTM B368(2014) without removal from the joint.
19. Use of the aluminium alloy for fins according to any one of claims 1 to 8 for making fins of a heat exchanger.
Citation Information
Patent Citations
High strength aluminum alloy fin material for heat exchanger
JP1996041573A
aluminum brazing alloy
JP2003514989A
Aluminum alloy for heat exchanger fins
JP2017528605A