Non-invasive repair and renovation of hardened cementitious materials
An aqueous composition of colloidal silica and polycarboxylic acid effectively addresses the limitations of existing materials by providing deep penetration and self-healing capabilities for concrete structures, enhancing their durability and impermeability.
Patent Information
- Application Number
- JP2021559166
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-29
- Filing Date
- 2020-05-25
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2040-05-25
AI Technical Summary
Existing repair and sealing materials for hardened cementitious materials, such as concrete structures, suffer from low penetration depth, high cost, and complex application processes, often lacking self-healing capabilities.
An aqueous composition comprising colloidal silica and polycarboxylic acid, which interacts with the existing concrete matrix to initiate secondary hydration, forming new hydrated cement products and enhancing crack healing, with a penetration depth of at least 10 mm.
The composition achieves rapid, cost-effective repair and sealing with improved penetration depth, promoting self-healing properties and enhancing the impermeability of concrete structures.
Smart Images

Figure 0007555348000005 
Figure 0007555348000004 
Figure 0007555348000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an aqueous composition for the repair and / or sealing of hardened cementitious materials, in particular concrete structures, to a method for the repair and / or sealing of hardened cementitious materials using said aqueous composition, and to corresponding uses of said aqueous composition. [Background technology]
[0002] Modern concrete is a very durable structural material and, if properly formulated and placed, will usually provide a very long service life. In any case, hardened cementitious materials, particularly concrete structures, are subject to damage that may be the result of, for example, improper manufacturing, or deterioration from weathering or other harsh conditions due to mechanical, physical or chemical attack. Therefore, repair and / or sealing of hardened cementitious materials may be required to improve the durability of the structure. The need for repair and restoration of cementitious materials, particularly concrete structures, is becoming increasingly important and is an important market due to the increasing possibility of long life cycles in structures in the future.
[0003] Apart from mineral binder based concrete repair materials suitable for the repair or restoration of damaged structures, there is a wide range of other materials that are used to repair and / or seal hardened cementitious materials.
[0004] For example, pure colloidal silica can be used for repairing and sealing hardened reinforced concrete structures, however with low effectiveness.
[0005] EP 3053901 (Sika AG) teaches aqueous compositions for repairing and / or sealing hardened concrete structures comprising colloidal silica and polycarboxylate ethers. However, the penetration depth of such compositions may be limited.
[0006] US 2013 / 281577 (WR Grace & Co) describes an aqueous additive composition for modifying cementitious compositions, comprising colloidal nanoparticles of silica and polycarboxylate ethers. However, no application for repair of hardened cementitious materials is disclosed, and the penetration depth of such compositions is not subsequently optimized.
[0007] EP 2251376 (Sika AG) teaches in a preferred embodiment an aqueous polymer dispersion comprising, inter alia, 5-15 wt. % comb polymer, 10-30 wt. % fumed or colloidal silica, and 30-70 wt. % water. However, no application in the repair of hardened cementitious materials is disclosed, and subsequently, the penetration depth of such compositions is not optimized.
[0008] JP 2014-177394 A describes a method for repairing a concrete structure in which a restoring material, which is a mortar composition comprising, inter alia, cement, a superplasticizer comprising a polycarboxylic acid-based copolymer, and an amorphous silica fine powder, is applied to the area where a portion of the concrete structure has been removed. However, the solution provided is a mortar that is unable to penetrate deep cracks.
[0009] US 2004 / 0077768 (Akzo Nobel) discloses co-dispersions of colloidal silica and organic binders such as poly(acrylic acid). However, these systems are used as coating materials and not for the repair of hardened cementitious materials.
[0010] A commercial example of a water-resistant crystalline waterproof concrete mixture is the Sika WT-200® series (Sika Schweiz AG), which is a crystalline mixture for self-healing concrete that provides crystalline-based self-healing and reacts with portlandite (calcium hydroxide) to produce water-insoluble crystals. Crystalline mixtures for waterproofing are also sold by Xypex Chemical Corp.
[0011] Other examples of agents used for the repair and / or sealing of concrete structures are the bacteria sphaericus, zinc sulfate, alumina-coated silica nanoparticles, blast furnace slag or fly ash.
[0012] Materials used for repair and / or sealing are often rather expensive or exhibit poor performance, especially low penetration depth. Many approaches do not support self-healing processes. Application to cementitious materials can be complex and time-consuming. Summary of the Invention [Problem to be solved by the invention]
[0013] It is therefore an object of the present invention to provide a composition for repairing and / or sealing hardened cementitious materials, in particular concrete structures and reinforced concrete structures, that overcomes the disadvantages of the above-mentioned conventional approaches. In particular, the composition must be relatively inexpensive, must allow for easy and / or quick application to the hardened cementitious material, and must exhibit a high penetration depth. Furthermore, the composition must exhibit good performance by initiating the cement recovery process. [Means for solving the problem]
[0014] Surprisingly, this objective was achievable with an aqueous composition comprising a combination of colloidal silica and a polycarboxylic acid.
[0015] The present invention therefore relates to an aqueous composition for the repair and / or sealing of hardened cementitious materials, in particular concrete structures, which comprises colloidal silica and a polycarboxylic acid, wherein said polycarboxylic acid according to claim 1 is not a comb polymer.
[0016] The main advantages of this composition are its low cost compared to other approaches and its simplicity and / or rapidity of application. Surprisingly, improved performance is also achieved, the penetration depth of the composition is very high, preferably at least 10 mm, in particular at least 20 mm or more, and the growth of new hydrated cement products occurs especially along the sides of the crack, contributing to the crack "healing" process.
[0017] The aqueous composition allows for a non-invasive treatment of hardened cementitious materials, particularly concrete structures, which effectively interacts with the existing concrete matrix to form new hydration products in a second hydration process of cement and / or SCM, SCM being a common abbreviation for auxiliary cementitious materials such as fly ash or slag, e.g., blast furnace slag.
[0018] The present invention also relates to a method for repairing and / or sealing a hardened cementitious material, in particular a concrete structure, comprising the step of applying an aqueous composition according to the present invention to the hardened cementitious material or a part thereof and filling any cracks having a width of up to 10 mm, as well as to the use of the aqueous composition for repairing and / or sealing a hardened cementitious material. Preferred embodiments of the present invention are described in the dependent claims.
[0019] The details set out below apply equally to the aqueous compositions, methods and uses, where applicable. [Brief description of the drawings]
[0020] [Figure 1]Figure 1 is a schematic representation of how the aqueous composition according to the invention is applied by transfer. In Figure 1, the aqueous composition according to the invention is placed as catholyte 3 on one side of the hardened concrete structure 1 to be repaired or sealed. Water, in particular distilled water, is placed as anolyte 2 on the other side. Electrodes 4, 5 connected to a voltage source 6 (for example 12 V) are immersed in the anolyte and the catholyte, respectively. For example, the potential can be applied in three cycles, i.e. two days connected and one day disconnected. [Diagram 2] Figure 2 is a schematic diagram of the crack specimen used in the examples, in which a mortar prism 1 has a crack 2 that extends to a certain depth below the diameter of the prism. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The aqueous composition comprises colloidal silica. Colloidal silica refers to silica particles dispersed in a colloidal state in a liquid phase, typically water. A colloid is a stable dispersion of particles. A stable dispersion or colloid of silica particles is also called a silica sol. Colloidal silica is generally amorphous silica. Colloidal silica is commercially available from a number of companies, for example from Nouryon under the trade name Levasil. For example, commercial products of colloidal silica can differ with respect to pH value, particle size or concentration. It is possible to use one type of colloidal silica or a mixture of two or more types of colloidal silica, for example with different particle sizes.
[0022] Colloidal silica can be anionic colloidal silica or cationic colloidal silica. As known to those skilled in the art, colloidal silica dispersions usually contain cations or anions for stabilization. In the case of cationic colloidal silica, silica particles are usually coated with alumina. Colloidal silica can be non-surface-modified silica or surface-modified silica, for example, surface-modified with silane or siloxane.
[0023] The weight average particle size of the colloidal silica is usually in the range of 1 to 150 nm, preferably 2 nm to 35 nm, more preferably 5 nm to 10 nm. Small particle size distributions, for example a weight average particle size of about 5 nm, are particularly preferred. The weight average particle size, as used herein, can be determined by the dynamic light scattering method described in ISO 22412:2017.
[0024] The aqueous composition further comprises at least one polycarboxylic acid. The aqueous composition may comprise one or more polycarboxylic acids. The polycarboxylic acid in the context of the present invention is a homo- or copolymer of at least one ethylenically unsaturated carboxylic or dicarboxylic acid. Suitable ethylenically unsaturated carboxylic or dicarboxylic acids are selected from the group consisting of acrylic acid, methacrylic acid, 3,3-dimethylacrylic acid, crotonic acid, isocrotonic acid, angelic acid, tiglic acid, maleic acid, fumaric acid, itaconic acid and sorbic acid, preferably acrylic acid and / or methacrylic acid.
[0025] Said ethylenically unsaturated carboxylic or dicarboxylic homo- or copolymers may contain small amounts of further comonomers such as ethylene, propylene, butadiene, isoprene, styrene, alkyl esters of acrylic or methacrylic acid, acrylonitrile, acrylamide, vinyl esters, preferably vinyl acetate, vinyl chloride and vinylpyrrolidone, etc. However, it is preferred that the polycarboxylic acids of the invention consist of at least 85 mol %, preferably at least 90 mol %, more preferably at least 95 mol %, in particular at least 99 mol %, of monomers selected from the above list of ethylenically unsaturated carboxylic or dicarboxylic acids, each based on the total composition of the polycarboxylic acid.
[0026] The homo- and copolymers can be linear or branched and they may additionally be crosslinked. The copolymers may be random, block or gradient.
[0027] According to one embodiment, the polycarboxylic acid is a homopolymer, preferably a homopolymer of acrylic acid or methacrylic acid.
[0028] The polycarboxylic acids of the present invention may be used in their protonated form or in their partially or fully neutralized form.
[0029] According to a preferred embodiment, at least a portion of the carboxyl groups of the polycarboxylic acids of the invention are neutralized with an oxide or hydroxide of an alkali or alkaline earth metal or with ammonia.
[0030] According to a particularly preferred embodiment, the polycarboxylic acids are polyacrylates or polymethacrylates, especially in the form of their sodium salts.
[0031] The weight average molecular weight (Mw) of the polycarboxylic acid is preferably 1,000 to 150,000 g / mol, more preferably 5,000 to 100,000 g / mol, and especially 5,000 to 10,000 g / mol. The weight average molecular weight can be determined by gel permeation chromatography (GPC).
[0032] According to an embodiment, the polycarboxylic acid may be in the form of a solid, preferably fine powder having a particle size of 20 to 3000 μm, preferably 50 to 1000 μm, more preferably 90 to 850 μm. The particle size distribution may be determined by the methods described in ASTM C136 and ASTM C117.
[0033] According to a further embodiment, the polycarboxylic acid can be in the form of an aqueous preparation, in particular a solution or a dispersion, which has a solids content of at least 25% by weight, preferably at least 30% by weight, in particular at least 40% by weight, each based on the total weight of the aqueous preparation.
[0034] The polycarboxylic acids of the present invention do not contain any polyalkylene oxide groups attached to the polycarboxylic acid backbone, and therefore are not comb polymers, also known as PCE fluidizers.
[0035] According to the most preferred embodiment of the invention, the polycarboxylic acid is a homopolymer of acrylic acid or methacrylic acid, in particular in the form of their sodium salts, having an average molecular weight Mw, measured by GPC, of 1,000 to 150,000 g / mol, preferably 5,000 to 100,000 g / mol, in particular 5,000 to 10,000 g / mol.
[0036] The aqueous composition of the present invention contains water. As mentioned above, many aqueous dispersions or silica sols of colloidal silica and polycarboxylic acids are commercially available. Also, commercially available polycarboxylic acid products can be a mixture with water. The aqueous composition can be easily prepared by mixing the aqueous dispersions or silica sols of colloidal silica and polycarboxylic acids, for example, as aqueous solutions or dispersions. If necessary, the water content can be adjusted by adding more water. If necessary, the pH value can be adjusted by adding an acid or base.
[0037] The aqueous composition is a liquid. The aqueous composition is preferably an aqueous dispersion or sol. The pH value of the aqueous composition can vary in a wide range depending on the type of components used and the desired application. According to an embodiment, the pH value of the aqueous composition can vary from 1 to 13, preferably from 6 to 12, in particular from 7.5 to 11.
[0038] The content of colloidal silica in the aqueous composition is preferably 1-50% by weight, more preferably 5-50% by weight or 10-50% by weight, even more preferably 5-45% by weight or 10-45% by weight, based on the total weight of the aqueous composition. The weight of colloidal silica in this specification refers, as usual, to the solid content of SiO2 (i.e. not including water).
[0039] The content of the polycarboxylic acid in the aqueous composition is preferably 1 to 50% by weight, more preferably 2 to 50% by weight or 4 to 50% by weight, and even more preferably 2 to 25% by weight or 4 to 25% by weight, based on the total weight of the aqueous composition.
[0040] In a preferred embodiment, the content of colloidal silica in the aqueous composition is 10 to 20% by weight, based on the total weight of the aqueous composition, and / or the content of polycarboxylic acid in the aqueous composition is 2 to 10% by weight, in particular 2 to 5% by weight, based on the total weight of the aqueous composition.
[0041] According to a particularly preferred embodiment, the weight ratio of colloidal silica to polycarboxylic acid on a dry basis is at least 4, preferably 4.5.
[0042] The content of water in the aqueous composition is, for example, at least 15% by weight, preferably at least 25% by weight, more preferably at least 40% by weight or at least 60% by weight, based on the total weight of the aqueous composition.
[0043] The aqueous composition may optionally further comprise one or more additives. The additives may be those commonly used in the art.
[0044] In particular, it is generally suitable that the aqueous composition does not comprise a hydraulic mineral binder, such as, for example, cement, since mineral binders are reactive with water. According to a particularly preferred embodiment, the composition of the invention does not comprise a hydraulic mineral binder, in particular cement.
[0045] The total amount of colloidal silica, polycarboxylic acid and water, based on the total weight of the aqueous composition, may vary depending on requirements, for example being at least 80% by weight, preferably at least 90% by weight, more preferably at least 95% by weight.
[0046] Thus, according to an embodiment, the aqueous composition of the present invention comprises (in each case based on the total weight of the aqueous composition): - 1 to 50% by weight, preferably 5 to 50% by weight, of colloidal silica, - 1 to 50% by weight, preferably 2 to 50% by weight and in particular 2 to 25% by weight of polycarboxylic acids, at least 15% by weight, preferably at least 25% by weight, more preferably at least 40% by weight of water wherein the weight ratio of colloidal silica to polycarboxylic acid on a dry basis is at least 4, preferably 4.5, and the total amount of colloidal silica, polycarboxylic acid and water is at least 80% by weight, preferably at least 90% by weight.
[0047] According to a further embodiment, the aqueous composition of the present invention comprises (in each case based on the total weight of the aqueous composition): - 1 to 50% by weight, preferably 5 to 50% by weight, of colloidal silica, - 1 to 50% by weight, preferably 2 to 50% by weight and in particular 2 to 25% by weight of polycarboxylic acids, at least 15% by weight, preferably at least 25% by weight, more preferably at least 40% by weight of water and the weight ratio of colloidal silica to polycarboxylic acid on a dry basis is at least 4, preferably 4.5.
[0048] In particular, the aqueous composition of the present invention is free of comb polymers or polycarboxylate ethers (PCE), which means that the content of such comb polymers or polycarboxylate ethers (PCE) is less than 0.1% by weight, preferably less than 0.01% by weight.
[0049] The aqueous composition according to the invention is suitable for a method of repairing and / or sealing hardened cementitious materials, in particular hardened concrete structures, which are preferably hardened reinforced concrete structures.
[0050] For example, the hardened concrete structure or hardened reinforced concrete structure can be any civil engineering structure or part thereof. Examples of civil engineering structures are buildings, bridges, pipelines, dams, reservoirs, underground structures such as tunnels, stock underpasses and monuments. The hardened concrete structure or hardened reinforced concrete structure can be, for example, a wall, slab, beam, column, pier, post, parapet, parapet, foundation, flooring, frame, curb, sill, sub-beam, coping, cornice or corner.
[0051] The degree of impermeability of concrete to water is determined by the impermeability of the binder matrix. Hardened concrete is a porous material that allows the passage of water or other media through a structure of capillary pores. These capillaries are voids created by the excess amount of water in the concrete that is not needed for the chemical reaction for hardening known as hydration.
[0052] In addition, hardened cementitious materials, especially concrete structures, may have damage or defects caused by, for example, thermal, mechanical, chemical and / or physical attacks. Typical damage or defects in cementitious materials are, for example, cracks, voids or crevices. Of course, the impermeability is further reduced by such damage or defects.
[0053] Cracks having a width of up to several millimeters, for example cracks having a width of up to 2 mm, 5 mm or 10 mm, can be repaired or sealed with the aqueous composition of the present invention. Although cracks having a width of less than 0.4 mm or 0.2 mm are usually not considered problematic with respect to the structural integrity of cementitious materials, especially hardened concrete, such cracks may be repaired or sealed with the aqueous composition of the present invention, for example to improve or restore the aesthetics of the concrete surface.
[0054] The method for repairing or sealing a hardened cementitious material, particularly a hardened concrete structure, comprises the step of applying the aqueous composition of the present invention to the hardened cementitious material, particularly a concrete structure, or to a portion thereof. Depending on the purpose, the aqueous composition may be applied to the entire hardened cementitious material, or to only a portion thereof. For example, only a portion of the hardened concrete structure that contains damage or defects or may be exposed to harsher conditions than other portions, e.g., may come into contact with water, may be treated.
[0055] Application of the aqueous composition to a hardened cementitious material, particularly a concrete structure or part thereof, may be carried out by conventional means. The aqueous composition may be applied onto the surface of the cementitious material or part thereof, for example by roller, brush, trowel, or by spray, for example by air gun spray or airless spray, so that the material can penetrate the surface. Transport is primarily by capillary suction. This can also be considered as infiltration or saturation.
[0056] Alternatively, the aqueous composition may be applied to the hardened cementitious material, particularly the concrete structure, or a part thereof, by injection. A common injection device, such as a manual injection device or an injection pump, may be used. Injection is particularly suitable for filling cracks, although this can also be achieved by the other methods described.
[0057] Alternatively, the aqueous composition may be applied to the hardened cementitious material, in particular the concrete structure or a part thereof, by migration (see FIG. 1). The migration method is a method known to those skilled in the art, in which anolyte (anolyte) is placed on one side of the hardened concrete structure to be repaired or sealed, and catholyte (catholyte) is placed on the other side. An external potential is then applied across the hardened cementitious material so that ions can migrate into the structure. In the migration method according to the invention, the aqueous composition of the invention is used as one electrolyte, preferably as catholyte. The other electrolyte, preferably anolyte, is for example water, in particular distilled water. Migration can occur with the application of an external potential for one or more cycles.
[0058] Thus, the aqueous composition is preferably applied to the hardened cementitious material, in particular the concrete structure or part thereof, by injection, transfer or capillary suction. Injection and capillary suction are very simple application methods. Transfer methods are quick and time-saving.
[0059] The method of the present invention is a non-invasive method. By non-invasive is meant a non-destructive method, i.e. the cementitious material to be repaired and / or sealed, in particular concrete, e.g. cracked concrete, is not removed.
[0060] The method of the present invention is particularly suitable in relation to hardened or reinforced concrete structures which contain cracks.
[0061] The sealing of cementitious materials is the protection against ingress, i.e. reducing or preventing the ingress of adverse agents, such as water, other liquids, vapours, gases, chemicals and biological agents. Sealing is a procedure that improves the impermeability of concrete.
[0062] The amount of the aqueous composition of the present invention that is applied to a hardened cementitious material, particularly a concrete structure, or portion thereof, is not particularly limited.
[0063] The aqueous composition of the present invention is typically applied in one coat, layer or step.However, it is also possible, and in certain cases is preferred, to apply the aqueous composition of the present invention in multiple coats, layers or steps, for example 2 or 3 coats, layers or steps, each of which is applied afterwards with a waiting period between them.The application of multiple coats, layers or steps can further increase the penetration depth of the aqueous composition of the present invention.
[0064] The components of the aqueous composition according to the present invention can form an insoluble material throughout the pores and capillary structures of the concrete, sealing the concrete and thus improving protection against the intrusion of water and other liquids such that the impermeability is enhanced.
[0065] In addition, the aqueous composition may also repair damage or defects in hardened cementitious materials, particularly concrete structures, by enhancing the self-healing properties of the cementitious material and by improving its ability to repair damage or defects such as cracks.
[0066] The components of the aqueous composition, especially the colloidal silica, effectively interact with the existing cementitious matrix of the cementitious material, especially the concrete, to form new hydrated cementitious products in the second hydration process of the cement and / or SCM. The growth of new hydrated cementitious products also occurs especially on the crack flanks involved in the crack healing process. Thus, restoration of the cementitious material can occur.
[0067] The aqueous composition of the invention, comprising colloidal silica and polycarboxylic acid, has significantly improved performance, especially improved penetration depth, compared to the use of colloidal silica alone or the combined use of colloidal silica and PCE. Thus, the aqueous composition applied by the method of the invention allows the formation of new hydration products at the sides of the crack, in some cases with Ca / Si ratios below 1.0, demonstrating the effectiveness of the method. The usual value for Portland CSH phase is Ca / Si=1.4-2.0 in SEM characterization, but the new chemical and physical recovery is based on a different phase (not portlandite) with a Ca / Si ratio of 0.5-1.
[0068] The method of the present invention is suitable for sealing hardened cementitious materials, especially concrete structures. The method is particularly suitable for filling cracks with a width of up to 10 mm in said hardened cementitious materials, especially concrete. This treatment can improve the impermeability of the cementitious material. The method of the present invention is therefore suitable for renovating cementitious materials, especially concrete structures. The method of the present invention is also suitable for repairing hardened cementitious materials, especially concrete structures, since it induces the growth of new hydrated cement products so that recovery or restoration can be achieved. Of course, the method is also suitable for simultaneously repairing and sealing hardened cementitious materials, especially concrete structures.
[0069] The method of the invention may optionally comprise further steps, in particular the preparation of the surface to be treated, for example cleaning, dusting, drying, wetting and / or application of a primer.
[0070] The method of the invention may optionally be combined with at least one additional treatment of the cementitious material, which may be selected from at least one of the conventional treatments of hardened cementitious materials, in particular concrete structures, such as protection of the reinforcement of reinforced concrete by application of corrosion inhibitors, crack sealing with reactive agents, such as epoxy or polyurethane resins, or waterproofing of the surface of the concrete structure with a hydrophobic material (hydrophobic saturation).
[0071] The aqueous composition of the present invention is therefore suitable for repairing and / or sealing hardened cementitious materials, in particular concrete structures, preferably hardened reinforced concrete structures. In particular, the aqueous composition of the present invention is suitable for filling cracks having a width of up to 10 mm in hardened cementitious materials, in particular concrete. EXAMPLES
[0072] Penetration depth and crack filling capacity testing
[0073] [Table 1]
[0074] Ex.1 is an aqueous composition of the present invention. Ref.1 and Ref.2 are reference examples.
[0075] Compositions Ref.1, Ref.2 and Ex.1 were applied on 4x4x16 cm mortar prisms made from mortar based on ordinary Portland cement (CEM IR / SR) and quartz sand with a cement / sand ratio of 0.33 and a water / cement ratio of 0.5. 600 g / m of monofilament polypropylene fibres of 12 mm length were applied. 3 The addition of fibers was necessary to prevent complete fracture of the specimens upon the introduction of cracks. The mortar prisms were fully cured at 21 °C / 95% relative humidity. Then, one crack with a width of 229–326 μm was introduced per mortar prism by three-point bending.
[0076] The application of compositions Ref.1, Ref.2 and Ex.1 was carried out at 21°C / 60% relative humidity by a two-step procedure: in the first step, the respective composition was allowed to penetrate freely into the entire area of the crack for 24 hours, then the surface was allowed to dry for 2 days, then the free penetration was repeated for another 24 hours. In the second step, an electric field (12V) was applied across the specimen for 24 hours.
[0077] The penetration depth was measured along the crack side by scanning electron microscopy (SEM) in backscattering mode, by energy dispersive X-ray spectroscopy (EDX) and by analysis of the material composition in the crack. The relative abundances of SiO2, CaO, Al2O3, K2O and SO3 were determined at various depths along the crack on the cross-sections of treated specimens after 28 days of curing at 23 °C / 50% relative humidity. As the applied compositions form gels of calcium silicate hydrates (CSH-gels), the CaO / SiO2 ratios of these gels were then calculated to assess the penetration depth. CSH-phases with CaO / SiO2 ratios < 1 are CSH-gels derived from one of the compositions Ref. 1, Ref. 2, Ex. 1, whereas CSH-phases with CaO / SiO2 > 1 are the phases of the surrounding mortar.
[0078] The respective CaO / SiO2 ratios and therefore the associated penetration depths are given in Table 2 below: As can be seen, the penetration of the inventive sample Ex.1 is significantly higher than either reference.
[0079] The degree of crack filling was determined visually by stereomicroscope and relies on the growth of new hydrated cement phases.
[0080] The crack filling is shown in Table 2 below. It can be seen that the inventive example Ex.1 has a higher crack filling near the surface and up to a depth of 1 mm.
[0081] [Table 2]
[0082] To demonstrate effective filling or repair of the cracks, further tests were performed. The tests were based on measuring the resistance across the filled cracks, which means the resistance across the repaired mortar. The lower the resistance, the more the cracks were filled with conductive material, indicating an effective treatment.
[0083] As can be seen from Table 3 below, this resistance is lower for the inventive example Ex.1 compared to Ref.2, meaning that the repair was more effective with Ex.1.
[0084] [Table 3] The present disclosure includes the following inventive aspects: <Aspect 1> 1. An aqueous composition for the repair and / or sealing of hardened cementitious materials, in particular hardened concrete structures, comprising colloidal silica and at least one polycarboxylic acid, said at least one polycarboxylic acid being not a comb polymer. <Aspect 2> 2. The aqueous composition according to aspect 1, wherein the colloidal silica has a weight average particle size in the range of 1 nm to 150 nm, preferably 2 nm to 35 nm, and more preferably 5 nm to 10 nm. <Aspect 3> 3. The aqueous composition according to aspect 1 or 2, wherein the content of the colloidal silica is in the range of 1 to 50% by weight, preferably 5 to 50% by weight, and the content of the polycarboxylic acid is in the range of 1 to 50% by weight, preferably 2 to 50% by weight, in particular 2 to 25% by weight, based on the total weight of the aqueous composition. <Aspect 4> Aspect 4. The aqueous composition according to any one of aspects 1 to 3, wherein the weight ratio of colloidal silica to polycarboxylic acid on a dry basis is at least 4, preferably 4.5. <Aspect 5> Aqueous composition according to any of aspects 1 to 4, wherein the at least one polycarboxylic acid consists of at least 85 mol %, preferably at least 90 mol %, more preferably at least 95 mol %, in particular at least 99 mol %, of monomers selected from acrylic acid, methacrylic acid, 3,3-dimethylacrylic acid, crotonic acid, isocrotonic acid, angelic acid, tiglic acid, maleic acid, fumaric acid, itaconic acid and sorbic acid, preferably acrylic acid and / or methacrylic acid, each based on the total composition of the polycarboxylic acid. <Aspect 6> 6. The aqueous composition of embodiment 5, wherein the at least one polycarboxylic acid is a homopolymer, preferably a homopolymer of acrylic acid or methacrylic acid. <Aspect 7> Aspect 7. The aqueous composition according to any one of aspects 1 to 6, wherein the total amount of colloidal silica, polycarboxylic acid and water is at least 80% by weight, preferably at least 90% by weight, based on the total weight of the aqueous composition. <Aspect 8> Aspect 8. The aqueous composition according to any one of aspects 1 to 7, wherein the water content is at least 15% by weight, preferably at least 25% by weight, and more preferably at least 40% by weight, based on the total weight of the aqueous composition. <Aspect 9> A method of repairing and / or sealing a hardened cementitious material comprising the step of applying an aqueous composition according to any of aspects 1 to 8 to the hardened cementitious material, or a part thereof, and filling any cracks having a width up to 10 mm. <Aspect 10> 10. The method of embodiment 9, wherein the hardened cementitious material is a hardened concrete structure, particularly a hardened reinforced concrete structure. <Aspect 11> 11. The method according to any one of claims 9 to 10, wherein the aqueous composition is applied by pouring, moving, dipping or spreading, for example by brush, spray or roller, onto the surface of the structure. <Aspect 12> 12. The method of any one of aspects 9-11, wherein the hardened cementitious material comprises cracks. <Aspect 13> 13. The method of any of aspects 9-12, wherein application of the aqueous composition to the hardened cementitious material is non-invasive. <Aspect 14> 14. The method of any of aspects 9-13, comprising at least one additional treatment of the hardened cementitious material selected from protecting the reinforcement by application of a corrosion inhibitor, crack sealing with a reactive agent, or waterproofing the surface of the hardened cementitious material with a hydrophobic material. <Aspect 15> Use of the aqueous composition according to any of the aspects 1 to 7 for repairing and / or sealing hardened cementitious materials, preferably hardened concrete structures, in particular hardened reinforced concrete structures.
Claims
1. A method of repairing and / or sealing a hardened cementitious material, comprising the steps of applying an aqueous composition to the hardened cementitious material, or a portion thereof, to fill any cracks having a width up to 10 mm, said aqueous composition comprising colloidal silica and at least one polycarboxylic acid, said at least one polycarboxylic acid being not a comb polymer; The colloidal silica has a weight average particle size in the range of 2 nm to 35 nm, the content of the colloidal silica is in the range of 5 to 50 wt % based on the total weight of the aqueous composition, and the content of the polycarboxylic acid is in the range of 1 to 50 wt %.
2. 2. The method of claim 1, wherein the weight ratio of colloidal silica to polycarboxylic acid on a dry basis is at least 4.
3. 3. The method of claim 1 or 2, wherein the at least one polycarboxylic acid consists of at least 85 mole %, based on the total composition of the polycarboxylic acid, of monomers selected from acrylic acid, methacrylic acid, 3,3-dimethylacrylic acid, crotonic acid, isocrotonic acid, angelic acid, tiglic acid, maleic acid, fumaric acid, itaconic acid, and sorbic acid.
4. The method of claim 3 , wherein the at least one polycarboxylic acid is a homopolymer.
5. The method according to any one of claims 1 to 4, wherein the total amount of colloidal silica, polycarboxylic acid and water is at least 80% by weight, based on the total weight of the aqueous composition.
6. The method according to any one of claims 1 to 5, wherein the water content is at least 15% by weight, based on the total weight of the aqueous composition.
7. The method of claim 1 , wherein the hardened cementitious material is a hardened concrete structure.
8. The method of claim 7 , wherein the aqueous composition is applied by pouring, transferring, soaking or painting onto the surface of the structure.
9. The method of any one of claims 1 to 8, wherein the hardened cementitious material comprises cracks.
10. 10. The method of any one of claims 1 to 9, wherein application of the aqueous composition to the hardened cementitious material is non-invasive.
11. 11. The method of any one of claims 1 to 10, comprising at least one additional treatment of the hardened cementitious material selected from protecting the reinforcement by application of a corrosion inhibitor, crack sealing with a reactive agent, or waterproofing the surface of the hardened cementitious material with a hydrophobic material.
Citation Information
Patent Citations
Special interface treating agent of cement-based materials for repair and use method of special interface treating agent
CN108101581A
JP1974039620A
Production of aqueous silicone emulsion composition
JP1986246255A
Water leakage preventing composition