Process for preparing stabilized aliphatic polyesters and compositions obtained therefrom
The stabilization of aliphatic polyesters through ring-opening polymerization with specific stabilizers addresses melt instability, ensuring stability and suitability for food contact applications while preserving biodegradability.
Patent Information
- Application Number
- JP2021566522
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-03
- Filing Date
- 2020-05-29
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-05-29
AI Technical Summary
Aliphatic polyesters, particularly polylactides, are unstable during melt processing due to backbiting reactions, leading to degradation and the need for stabilization to maintain biodegradability and suitability for food contact applications.
A process involving ring-opening polymerization of cyclic ester monomers with a stabilizer of formula (I) to inhibit depolymerization, followed by optional removal of residual monomers, resulting in a melt-stable aliphatic polyester composition.
The process produces a melt-stable aliphatic polyester with reduced degradation, maintaining biodegradability and suitability for food contact applications, with effective stabilization achieved by compounds like L-cysteine, L-cystine, and glutathione.
Smart Images

Figure 0007555532000033 
Figure 0007555532000034 
Figure 0007555532000035
Abstract
Description
[Technical field]
[0001] The present invention relates to a process for the preparation of stabilized aliphatic polyesters and to compositions obtained therefrom. [Background technology]
[0002] Aliphatic polyesters based on cyclic ester monomers, such as lactide, glycolide, trimethylene carbonate (TMC), epsilon-caprolactone, and p-dioxanone, and combinations thereof, have many attractive properties. They often have high biocompatibility and attractive resorbability, making them suitable for the fabrication of scaffolds and implants for use in the human or animal body. Moreover, in particular, polylactide, also called polylactic acid, is a promising material in the field of technical applications, for example, packaging materials.
[0003] The use of lactic acid and lactide to produce biodegradable polymers is well known. Such polymers have been used extensively in food contact applications and the medical industry. Processes developed for the production of polymers utilized in the food and / or medical industries have incorporated techniques dictated by the need for high purity of the final product.
[0004] Typically, manufacturers of such polymers will convert the monomers into polymer beads, resins, or other pelletized or powdered products with as little residual monomer as possible. The polymer in these forms is then sold to end users who extrude, blow mold, cast film, blow film, thermoform, injection mold, or fiber spin the polymer at elevated temperatures to form useful articles. These processes generally proceed via melt processing.
[0005] It is generally known that natural lactide polymers or polylactides are unstable during elevated temperature processing, such as melt processing by end-user purchasers of polymer resins. One proposed reaction pathway includes a "backbiting" reaction in which terminal hydroxyl groups form lactides. Other proposed reaction pathways include "backbiting" reactions in which hydroxyl end groups form cyclic oligomers, chain scission via hydrolysis of ester bonds, intramolecular beta-elimination reactions that generate new acid end groups and unsaturated carbon-carbon bonds, and radical chain decomposition reactions. It is clear that the degradation of the polymer during melt processing must be reduced to a commercially acceptable rate while maintaining the biodegradable or compostable qualities that make them so desirable. This is accomplished through deactivation of the catalyst used in the polymerization, since uncatalyzed lactide reformation is slow enough to be of no practical relevance.
[0006] Moreover, the melt polymerization of lactide will result in a thermodynamic equilibrium amount of residual lactide that needs to be removed, typically well below 1%. It is precisely the backbiting reactions that counter this removal, and it is desirable to re-establish this equilibrium. Therefore, already during the production of polylactide and before the removal of the residual lactide, the catalytic backbiting reactions must be prevented by stabilization.
[0007] Stabilizers have been used to counteract the catalytic lactide reformation. Many different additives have been proposed, but the majority are either not acceptable at all in food contact applications (because of the health risks associated with the additive) or are acceptable only with very low migration limits. Summary of the Invention [Problem to be solved by the invention]
[0008] Therefore, a need exists for lactide polymer compositions that are melt stable at the elevated temperatures common in melt processing and are suitable for food contact applications.
[0009] The present disclosure addresses these needs. [Means for solving the problem]
[0010] In a first aspect, the present invention provides a process for preparing a composition comprising an aliphatic polyester by ring-opening polymerization of a cyclic ester monomer, the process comprising: (a) providing a cyclic ester monomer and a polymerization catalyst to a reactor; (b) melt polymerizing the cyclic ester monomer to form a composition comprising an aliphatic polyester; (c) stabilizing the composition against aliphatic polyester depolymerization by incorporating therein or applying thereto at least one stabilizer to obtain a melt-stable composition; (d) optionally removing at least a portion of the residual cyclic ester monomer; Including, The stabilizer is represented by the formula (I) [ka] [In the formula, R 1 is hydrogen or C 1~6 is alkyl, R 2 is hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR 7 )-(CH2) n -C(=O)- and C 1~6 selected from the group including alkylcarbonyl, R 3 is hydroxyl, C 1~6 Alkoxy, and -NH-(CH2) p -C(=O)-OH, m is an integer selected from 0, 1, or 2; n is an integer selected from 1 or 2; and p is an integer selected from 1 or 2; Each R 4 are independently hydrogen or C 1~6 alkyl, Each R 5are independently hydrogen or C 1~6 alkyl, R 6 is hydrogen or the formula [ka] (where: * represents the attachment point to S in formula (I) and R 7 is hydrogen, C 1~6 Alkyl, and C 1~6 alkylcarbonyl] The present invention provides a process for producing a compound of formula (I).
[0011] In a second aspect, the present invention provides a composition directly obtainable by the process according to the first aspect of the present invention. The present invention also relates to uses of such compositions, for example for making shaped articles. The compositions of the present invention are particularly suitable for food contact applications.
[0012] In a third aspect, the present invention provides a process for stabilizing an aliphatic polyester against depolymerization, comprising the steps of: (a) forming an aliphatic polyester; and (b) stabilizing the polyester against depolymerization by incorporating therein or applying thereto at least one stabilizer to obtain a melt-stable polyester, the stabilizer being represented by formula (I): [ka] [In the formula, R 1 is hydrogen or C 1~6 is alkyl, R 2 is hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR 7 )-(CH2) n -C(=O)- and C 1~6 selected from the group including alkylcarbonyl, R 3 is hydroxyl, C 1~6 Alkoxy, and -NH-(CH2)p -C(=O)-OH, m is an integer selected from 0, 1, or 2; n is an integer selected from 1 or 2; p is an integer selected from 1 or 2; Each R 4 are independently hydrogen or C 1~6 alkyl, Each R 5 are independently hydrogen or C 1~6 alkyl, R 6 is hydrogen or the formula [ka] (where: * represents the attachment point to S in formula (I) and R 7 are independently hydrogen, C 1~6 Alkyl, and C 1~6 alkylcarbonyl] The present invention provides a process for producing a compound of formula (I).
[0013] In a fourth aspect, the present invention also provides a compound of formula (I) as a stabilizer against depolymerization of aliphatic polyesters. [ka] [In the formula, R 1 is hydrogen or C 1~6 is alkyl, R 2 is hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR 7 )-(CH2) n -C(=O)- and C 1~6 selected from the group including alkylcarbonyl, R 3 is hydroxyl, C 1~6 Alkoxy, and -NH-(CH2) p -C(=O)-OH, m is an integer selected from 0, 1, or 2; n is an integer selected from 1 or 2; p is an integer selected from 1 or 2; Each R 4 are independently hydrogen or C 1~6 alkyl, Each R 5 are independently hydrogen or C 1~6 alkyl, R 6 is hydrogen or the formula [ka] (where: * represents the attachment point to S in formula (I) and R 7 is hydrogen, C 1~6 Alkyl, and C 1~6 alkylcarbonyl] The present invention provides the use of the compound of the formula:
[0014] According to the present invention, when said polyester composition, preferably a polylactide composition, is stabilized with at least one compound of formula (I), preferably in an amount sufficient to inhibit the generation of lactide in the melt, a melt-stable aliphatic polyester composition, preferably a melt-stable polylactide composition, is obtained.
[0015] Exemplary compounds in this group are L-cysteine, L-cystine, glutathione, and N-acetyl-L-cysteine, which are known food additives and therefore provide preferred chemical stabilization strategies for food contact applications.
[0016] These and other characteristics, features and advantages of the present invention will become apparent from the following detailed description, which illustrates, by way of example, the principles of the invention. [Brief description of the drawings]
[0017] [Figure 1]1 depicts a graph plotting complex viscosity as a function of time for unstabilized and L-cysteine stabilized PLA samples. [Diagram 2] 1 depicts a graph plotting complex viscosity as a function of time for unstabilized and L-cystine stabilized PLA samples. [Diagram 3] 1 depicts a graph plotting complex viscosity as a function of time for unstabilized and N-acetyl-L-cysteine stabilized PLA samples. [Figure 4] 1 depicts a graph plotting complex viscosity as a function of time for unstabilized and glutathione-stabilized PLA samples. [Diagram 5] 1 depicts a graph plotting the complex viscosity of several comparative PLA samples as a function of time. [Figure 6] 1 depicts a graph plotting the complex viscosity of several comparative PLA samples as a function of time. [Figure 7] 1 depicts a graph plotting the complex viscosity of several comparative PLA samples as a function of time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The terms used in describing the present invention shall be construed in accordance with the following definitions, unless the context indicates otherwise.
[0019] Unless otherwise defined, all terms used in disclosing the present invention, including scientific and technical terms, have the meanings commonly understood by one of ordinary skill in the art to which the invention belongs. For further guidance, definitions of terms are included to better appreciate the teachings of the present invention.
[0020] In the following passages, various aspects of the invention are defined in more detail. Each aspect so defined may be combined with any other aspect or aspects, unless expressly specified to the contrary. In particular, any feature indicated as being preferred or advantageous may be combined with any other feature or features indicated as being preferred or advantageous.
[0021] References throughout this specification to "one embodiment" or "an embodiment" mean that a particular feature, structure, or characteristic described in connection with this embodiment is included in at least one embodiment of the invention. Thus, the appearances of the phrase "in one embodiment" or "in an embodiment" in various places throughout this specification are not necessarily all referring to the same embodiment, but may be. Moreover, as will be apparent to one of ordinary skill in the art from this disclosure, particular features, structures, or characteristics may be combined in any suitable manner in one or more embodiments. Furthermore, although some embodiments described herein include some features that are not included in other embodiments, combinations of features of different embodiments are considered to be within the scope of the invention and form different embodiments, as will be understood by one of ordinary skill in the art.
[0022] The terms "comprising," "comprises," and "comprised of," as used herein, are synonymous with "including," "includes," or "containing," or "contains," and are inclusive or open-ended and do not exclude additional, unrecited members, elements, or method steps. It will be understood that the terms "comprising," "comprises," and "comprised of," as used herein, include the terms "consisting of," "consists," and "consists of."
[0023] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise. By way of example, "a step" means one step or more than one step.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. All publications referenced herein are incorporated by reference.
[0025] The recitation of numerical ranges by endpoints includes all integers and, where appropriate, decimals subsumed within the range (e.g., 1 to 5 can include 1, 2, 3, 4, e.g., when referring to several elements, as well as 1.5, 2, 2.75, and 3.80, e.g., when referring to measurements). The recitation of endpoints also includes the endpoint values themselves (e.g., 1.0 to 5.0 includes both 1.0 and 5.0). Any numerical range recited herein is intended to include all subranges subsumed therein.
[0026] Whenever the term "substituted" is used in the present invention, it is understood to mean that one or more hydrogens on the indicated atom in the expression "substituted" are replaced with a selection from the indicated group, provided that the normal valence of the indicated atom is not exceeded and the substitution results in a chemically stable compound. When a group is substitutable, such a group can be substituted with one or more, preferably 1, 2, or 3, substituents.
[0027] The term “alkyl” as a group or part of a group refers to a group of formula C n H 2n+1where n is a number of at least 1. The alkyl group may be linear or branched and may be substituted as indicated herein. Preferably, the alkyl group contains 1 to 6 carbon atoms, preferably 1 to 5 carbon atoms, preferably 1 to 4 carbon atoms, preferably 1 to 3 carbon atoms, preferably 1 to 2 carbon atoms. When a subscript is used herein following a carbon atom, the subscript refers to the number of carbon atoms that the specified group may contain. For example, "C 1~6 The term "alkyl" refers to a group of the formula C n H 2n+1 (wherein n is a number ranging from 1 to 6). For example, C 1~6 Alkyl includes all linear or branched alkyl groups having 1 to 6 carbon atoms, and thus includes, for example, methyl, ethyl, n-propyl, i-propyl, 2-methylethyl, butyl and its isomers (e.g., n-butyl, i-butyl, and t-butyl), pentyl and its isomers, hexyl and its isomers, etc. For example, C 1~4 Alkyl includes all linear or branched alkyl groups having 1 to 4 carbon atoms, and thus includes, for example, methyl, ethyl, n-propyl, i-propyl, 2-methyl-ethyl, butyl and its isomers (e.g., n-butyl, i-butyl, and t-butyl).
[0028] "C 1~6 The term "alkylcarbonyl" refers to a carbonyl group linked to an alkyl group, i.e., -C(=O)R a (In the formula, R a is C 1~6 The term "alkyl" refers to a group that forms a cyclic or cyclic alkyl group, as defined above for alkyl.
[0029] "C 1~6 The term "alkoxy" refers to a group of the formula -OR a (wherein R a is C 1~6 As defined above for alkyl.
[0030] The terms set forth above and other terms used herein are well understood by those of skill in the art.
[0031] Preferred descriptions (features) and embodiments of the process, composition, and use of the present invention are defined hereinafter. Each description and embodiment of the present invention so defined may be combined with any other description and / or embodiment, unless clearly indicated to the contrary. In particular, any feature indicated as being preferred or advantageous may be combined with any other feature or description indicated as being preferred or advantageous. In this regard, the present invention is particularly grasped by any one or any combination of one or more of the following numbered descriptions and embodiments together with any other aspects and / or embodiments.
[0032] 1. A process for preparing a composition comprising an aliphatic polyester by ring-opening polymerization of a cyclic ester monomer, said process comprising the steps of: (a) providing a cyclic ester monomer and a polymerization catalyst to a reactor; (b) melt polymerizing the cyclic ester monomer to form a composition comprising an aliphatic polyester; (c) incorporating therein or applying thereto at least one compound of formula (I); and (d) optionally removing at least a portion of the residual (unreacted) cyclic ester monomer; [ka] [In the formula, R 1 is hydrogen or C 1~6 is alkyl, R 2 is hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR 7 )-(CH2) n -C(=O)- and C 1~6 selected from the group including alkylcarbonyl, R 3 is hydroxyl, C 1~6 Alkoxy, and -NH-(CH2) p -C(=O)-OH, m is an integer selected from 0, 1, or 2; n is an integer selected from 1 or 2; p is an integer selected from 1 or 2; Each R 4 are independently hydrogen or C 1~6 alkyl, Each R 5 are independently hydrogen or C 1~6 alkyl, R 6 is hydrogen or the formula [ka] (where: * represents the attachment point to S in formula (I) and R 7 is hydrogen, C 1~6 Alkyl, and C 1~6 alkylcarbonyl] process.
[0033] 2. A process for preparing a composition comprising an aliphatic polyester by ring-opening polymerization of a cyclic ester monomer, said process comprising: (a) providing a cyclic ester monomer and a polymerization catalyst to a reactor; (b) melt polymerizing the cyclic ester monomer to form a composition comprising an aliphatic polyester; (c) stabilizing the composition against aliphatic polyester depolymerization by incorporating therein or applying thereto at least one stabilizer to obtain a melt-stable composition; (d) optionally removing at least a portion of the residual cyclic ester monomer; and the stabilizer comprises a compound represented by formula (I) [ka] [In the formula, R 1 is hydrogen or C 1~6 is alkyl, R2 is hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR 7 )-(CH2) n -C(=O)- and C 1~6 selected from the group including alkylcarbonyl, R 3 is hydroxyl, C 1~6 Alkoxy, and -NH-(CH2) p -C(=O)-OH, m is an integer selected from 0, 1, or 2; n is an integer selected from 1 or 2; p is an integer selected from 1 or 2; Each R 4 are independently hydrogen or C 1~6 alkyl, Each R 5 are independently hydrogen or C 1~6 alkyl, R 6 is hydrogen or the formula [ka] (where: * represents the attachment point to S in formula (I) and R 7 is hydrogen, C 1~6 Alkyl, and C 1~6 alkylcarbonyl] The process is a compound of.
[0034] 3. The process of statements 1 or 2, wherein the aliphatic polyester is a polylactide prepared by ring-opening polymerization of lactide, the process comprising the steps of: (a) providing lactide and a polymerization catalyst to a reactor; (b) melt polymerizing the lactide to form a composition comprising polylactide; (c) incorporating therein or applying thereto at least one compound of formula (I); and (d) optionally removing at least a portion of the residual (unreacted) lactide.
[0035] 4. The process of any one of statements 1-3, wherein the aliphatic polyester is a polylactide prepared by ring-opening polymerization of lactide, the process comprising the steps of: (a) providing lactide and a polymerization catalyst to a reactor; (b) melt polymerizing the lactide to form a composition comprising polylactide; (c) stabilizing the composition against polylactide depolymerization by incorporating therein or applying thereto at least one stabilizer, wherein said stabilizer is at least one compound of Formula (I), to obtain a melt-stable composition; and (d) optionally removing at least a portion of the residual lactide.
[0036] 5. The process of any one of statements 1 to 4, wherein the compound of formula (I) inhibits the generation of lactide in a melt of the polylactide composition.
[0037] 6. R 1 is hydrogen, R 2 But hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR 7 )-(CH2) n -C(=O)- and C 1~6 selected from the group including alkylcarbonyl, R 3 is hydroxyl or -NH-CH2-C(=O)-OH; m is an integer selected from 1 or 2; n is an integer selected from 1 or 2; p is an integer selected from 1 or 2; Each R 4 and R 5 is hydrogen, R 6 is hydrogen or the formula [ka] and R 7 is hydrogen, 6. The process according to any one of claims 1 to 5.
[0038] 7. The process according to any one of statements 1 to 6, wherein the compound of formula (I) is selected from the group comprising cysteine, cystine, N-acetyl-cysteine, N-acetyl-cystine, glutathione, stereoisomers thereof, and mixtures thereof.
[0039] 8. The process according to any one of statements 1 to 7, wherein the compound of formula (I) is present in an amount of at least 0.010 wt%, preferably at least 0.025 wt%, based on the total weight of the polylactide. For example, the compound of formula (I) can be incorporated into or applied to the aliphatic polyester composition, preferably the polylactide composition, in an amount of at least 0.010 wt%, such as at least 0.020 wt%, such as at least 0.050 wt%, such as at least 0.075 wt%, such as at least 0.090 wt%, such as at least 0.10 wt%, based on the total weight of the polylactide composition. For example, the compound of formula (I) can be incorporated into or applied to the aliphatic polyester composition, preferably the polylactide composition, in an amount of at most 0.50 wt%, based on the total weight of the polylactide composition. For example, the compound of formula (I) can be incorporated into or applied to the aliphatic polyester composition, preferably the polylactide composition, in an amount of at most 0.30 wt%, such as at most 0.20 wt%, such as at most 0.18 wt%, such as at most 0.15 wt%, based on the total weight of the composition.
[0040] 9. The process according to any one of statements 1 to 8, wherein the compound of formula (I) is incorporated therein or applied thereto in an amount in the range of 0.010% to 0.5% by weight, such as 0.025% to 0.5% by weight, preferably 0.050% to 0.40% by weight, such as 0.075% to 0.30% by weight, for example at least 0.090% to 0.20% by weight, such as 0.095% to 0.15% by weight, based on the total weight of the aliphatic polyester composition, preferably the polylactide composition.
[0041] 10. The process of any one of statements 1-9, comprising adding at least one antioxidant prior to or simultaneously with step (c).
[0042] 11. The process of any one of statements 1 to 10, further comprising additives such as UV absorbers and / or light stabilizers.
[0043] 12. The process of any one of statements 1 to 11, wherein simultaneously with or after step (c) the composition is subjected to one or more devolatilization steps (d).
[0044] 13. The process of any one of statements 1 to 12, wherein step (c) is carried out after the polymerization has reached its lactide equilibrium.
[0045] 14. The process of any one of statements 1 to 13, wherein the polymerization process is a batch melt process or a continuous melt process.
[0046] 15. The process of any one of statements 1-14, comprising: i) continuously providing lactide and a polymerization catalyst to a continuous mixing reactor for a first polymerization; ii) continuously removing said first polymerization reaction mixture from the continuous mixing reactor and continuously providing said first polymerization reaction mixture to a plug flow reactor; iii) continuously removing a composition from the plug flow reactor; and (iv) incorporating or applying at least one compound of formula (I) thereto.
[0047] 16. The process of statement 15, wherein the first reactor is a loop reactor.
[0048] 17. The process of statement 15, wherein the first reactor is a continuous stirred tank reactor.
[0049] 18. The process of statement 15, wherein the continuous mixing reactor and / or plug flow reactor is a static mixer reactor.
[0050] 19. The process of any one of statements 1-18, wherein the polymerization is carried out at at least 100°C, such as at least 110°C, such as at least 120°C, for example at least 130°C.
[0051] 20. A composition obtainable directly by the process according to any one of statements 1 to 19, wherein said composition comprises a polylactide and at least one stabilizer, said stabilizer being a compound of formula (I).
[0052] 21. A process for stabilizing an aliphatic polyester against depolymerization, comprising the step of: [ka] [In the formula, R 1 is hydrogen or C 1~6 is alkyl, R 2 is hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR 7 )-(CH2) n -C(=O)- and C 1~6 selected from the group including alkylcarbonyl, R 3 is hydroxyl, C 1~6 Alkoxy, and -NH-(CH2) p -C(=O)-OH, m is an integer selected from 0, 1, or 2; n is an integer selected from 1 or 2; p is an integer selected from 1 or 2; Each R 4 are independently hydrogen or C 1~6 alkyl, Each R 5 are independently hydrogen or C 1~6 alkyl, R 6 is hydrogen or the formula [ka] (where: * represents the attachment point to S in formula (I) and R 7 is hydrogen, C 1~6 Alkyl, and C 1~6 alkylcarbonyl] The process comprises incorporating therein or applying thereto a compound of formula (I).
[0053] 22. A process for stabilizing an aliphatic polyester against depolymerization, comprising: (a) forming an aliphatic polyester; and (b) stabilizing the polyester against depolymerization by incorporating therein or applying thereto at least one stabilizer to obtain a melt-stable polyester, the stabilizer being represented by formula (I): [ka] [In the formula, R 1 is hydrogen or C 1~6 is alkyl, R 2 is hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR 7 )-(CH2) n -C(=O)- and C 1~6 selected from the group including alkylcarbonyl, R 3 is hydroxyl, C 1~6 Alkoxy, and -NH-(CH2) p -C(=O)-OH, m is an integer selected from 0, 1, or 2; n is an integer selected from 1 or 2; p is an integer selected from 1 or 2; Each R 4 are independently hydrogen or C 1~6 alkyl, Each R 5 are independently hydrogen or C 1~6 alkyl, R6 is hydrogen or the formula [ka] (where * represents the point of attachment to S in formula (I)) is selected from the group R 7 is hydrogen, C 1~6 Alkyl, and C 1~6 alkylcarbonyl] The process is a compound of.
[0054] 23. The process according to any one of statements 21 to 22, wherein the aliphatic polyester is a lactic acid-based polyester, preferably polylactic acid.
[0055] 24. The process according to any one of statements 21 to 23, wherein the compound of formula (I) is selected from the group consisting of cysteine, cystine, N-acetyl-cysteine, N-acetyl-cystine, glutathione, stereoisomers thereof, and mixtures thereof.
[0056] 25. The process of any one of statements 21 to 24, wherein the compound of formula (I) is incorporated into or applied to the aliphatic polyester in an amount of at least 0.025 wt.%, based on the total weight of the aliphatic polyester.
[0057] 26. The process of any one of statements 21 to 25, comprising incorporating or applying at least one antioxidant.
[0058] 27. As a stabilizer against depolymerization of aliphatic polyesters, [ka] [In the formula, R 1 is hydrogen or C 1~6 is alkyl, R 2 is hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR7 )-(CH2) n -C(=O)- and C 1~6 selected from the group including alkylcarbonyl, R 3 is hydroxyl, C 1~6 Alkoxy, and -NH-(CH2) p -C(=O)-OH, m is an integer selected from 0, 1, or 2; n is an integer selected from 1 or 2; p is an integer selected from 1 or 2; Each R 4 are independently hydrogen or C 1~6 alkyl, Each R 5 are independently hydrogen or C 1~6 alkyl, R 6 is hydrogen or the formula [ka] (where: * represents the attachment point to S in formula (I) and R 7 is hydrogen, C 1~6 Alkyl, and C 1~6 alkylcarbonyl] Use of compounds.
[0059] 28. The use according to statement 27, wherein the aliphatic polyester is a polylactide.
[0060] 29. Use of at least one compound of formula (I) in a polylactide composition to inhibit the evolution of lactide in a melt of the polylactide composition.
[0061] 30. The use according to any one of statements 27 to 29, wherein the compound of formula (I) is selected from the group comprising cysteine, cystine, N-acetyl-cysteine, N-acetyl-cystine, glutathione, stereoisomers thereof, and mixtures thereof.
[0062] 31. The use of any one of statements 29-30, wherein the composition further comprises at least one antioxidant, such as a vitamin or an organophosphite antioxidant.
[0063] According to the present invention, there is provided a process for preparing a stabilized composition comprising an aliphatic polyester by ring-opening polymerization of a cyclic ester monomer, the process comprising the steps of: (a) providing a cyclic ester monomer and a polymerization catalyst to a reactor, (b) melt polymerizing the cyclic ester monomer to form a composition comprising an aliphatic polyester, (c) stabilizing the composition against aliphatic polyester depolymerization by incorporating therein or applying thereto at least one stabilizer that is a compound of formula (I) to obtain a melt-stable composition, and (d) optionally removing at least a portion of the residual cyclic ester monomer.
[0064] Preferably, said process makes it possible to obtain a melt-stable polyester composition, preferably a polylactide composition, when a composition comprising polylactide is stabilized with a compound of formula (I), preferably said compound being used in an amount sufficient to inhibit the evolution of lactide in the melt.
[0065] Preferably, a melt-stable polylactide is a polymer that has a stable viscosity at the melt processing temperatures at which it is processed in existing or commercially available melt processing equipment, and has a rate of lactide reformation that is low enough that the amount of degradation upon processing at the same temperatures does not substantially affect the physical properties of the final polymer article or cause significant plating or fouling of the processing equipment, including molecular weight and viscosity, as well as others as disclosed herein.
[0066] Testing for melt stability may involve heating a devolatilized sample of polylactide to 250° C. at atmospheric pressure for 20 minutes and determining the weight percent of lactide evolved.
[0067] The present invention relates to the preparation of compositions using polymerization carried out in the substantial absence of solvent, i.e. melt polymerization. Optionally, minor amounts of solvent may be present during the process, for example, added as a solvent for catalyst or additional reaction components. The process is preferably intended to encompass situations in which the reaction mixture contains less than 5% by weight of solvent, preferably less than 2% by weight, more preferably less than 1% by weight, even more preferably less than 0.5% by weight of solvent, based on the total weight of the reaction mixture.
[0068] The polymerization process can be a batch melt process or a continuous melt process.
[0069] The polymerization is preferably carried out under inert conditions, such as under dry nitrogen or an argon gas blanket.
[0070] The ring-opening polymerization can be carried out at a temperature of at least 100° C. For example, the polymerization can be carried out at a temperature in the range of 100° C. to 240° C., preferably 100° C. to 220° C., and even more preferably 100° C. to 200° C.
[0071] The main reactants provided to the reactor include lactide and a polymerization catalyst. Optionally, additional components, such as cocatalysts, initiators for molecular weight control, and / or additives, may also be added. The components can be added directly to the reactor, either pure or in a solvent, or (some of) the reactants may be combined prior to addition to the reactor. The addition point of the additive will depend on the function of the additive. For example, antioxidants may be added prior to the first polymerization, while catalyst deactivators are generally added after the polymerization is complete.
[0072] Suitable cyclic ester monomers are those which contain 5 to 7 covalently bonded carbon atoms in the ring, at least one, typically one or two, oxygen atoms in the ring, and a carbonyl oxygen atom substituted on the carbon atom adjacent to the oxygen atom in the ring (together forming an ester bond). When there is more than one oxygen atom in the ring, an oxygen atom may be substituted on the carbon atom adjacent to all or just one of the oxygen atoms. The carbon atoms in the ring may be C 1~4 The monomers may be substituted with alkyl groups. Suitable monomers include lactide, glycolide, trimethylene carbonate, epsilon-caprolactone, p-dioxanone, and mixtures thereof. If more than one type of monomer is used, a polyester copolymer will result.
[0073] Lactide, whether in combination with one or more of glycolide, trimethylene carbonate, and epsilon-caprolactone, is the preferred cyclic ester monomer used as the starting material. The lactide used in the present invention may be L-lactide (derived from two L-lactic acid molecules), D-lactide (derived from two D-lactic acid molecules), meso-lactide (derived from an L-lactic acid molecule and a D-lactic acid molecule), or a mixture of two or more of the above. A 50 / 50 mixture of L-lactide and D-lactide, having a melting point of about 126° C., is often referred to in the literature as D,L-lactide or rac-lactide. Mixtures of the above-mentioned lactides are also suitable for use in the present process.
[0074] In some embodiments, the lactide used as the starting material is L-lactide containing up to 50% by weight of other lactides. For example, the lactide used as the starting material can be L-lactide containing 50-10% D-lactide. In other embodiments, the lactide is substantially pure L-lactide, where substantially pure means that it may contain up to 10% by weight, e.g., up to 5% by weight or up to 1% by weight, of other lactides. In other embodiments, the lactide is substantially pure D-lactide, where substantially pure means that it may contain up to 10% by weight, e.g., up to 5% by weight or up to 1% by weight, of other lactides.
[0075] The polymerization catalyst utilized in this process has the general formula M(Y 1 ,Y 2 ,…Y p ) q where M is a metal selected from the group consisting of elements from columns 3 to 12 of the Periodic Table of the Elements, furthermore the elements Al, Ga, In, Tl, Ge, Sn, Pb, Sb, Ca, Mg, and Bi; 1 , Y 2 , … Y p are each a substituent selected from the group consisting of linear or branched alkyl having 1 to 20 carbon atoms, aryl having 6 to 30 carbon atoms, alkoxy having 1 to 20 carbon atoms, aryloxy having 6 to 30 carbon atoms, and other oxide groups, carboxylate groups, and halide groups, as well as elements of Groups 15 and / or 16 of the Periodic Table, and p and q are integers from 1 to 6. Examples of suitable catalysts may include, inter alia, Sn, Ti, Zr, Zn, and Bi catalysts, preferably alkoxides or carboxylates, more preferably Sn(Oct)2, Ti(OiPr)4, Ti(2-ethylhexanoate)4, Ti(2-ethylhexyloxide)4, Zr(OiPr)4, zirconium tris(phenolate), (2,4-di-tert-butyl-6-(((2-(dimethylamino)ethyl(methyl)amino)methyl)phenoxy)(ethoxy)zinc, or Zn(lactate)2, as mentioned in WO 2014 / 177543.
[0076] The catalyst concentration, calculated as metal weight, can generally be at least 5 ppm, more particularly at least 10 ppm, such as at least 30 ppm, for example at least 40 ppm. The catalyst concentration can generally be at most 300 ppm, particularly at most 150 ppm.
[0077] Optionally, a cocatalyst, i.e., a compound that further increases the rate of polymerization, can be added to the lactide and catalyst. Suitable cocatalysts are known in the art. See, for example, U.S. Patent No. 6,166,169.
[0078] The process is represented by the formula R 9 This can be carried out in the presence of a coinitiator of -OH, 9 is halogen, hydroxyl, and C 1~6 C, optionally substituted with one or more substituents selected from the group consisting of alkyl 1~20 Alkyl, C 6~30 Aryl and C 6~30 Aryl C 1~20 Preferably, R is selected from the group consisting of alkyl. 9 is halogen, hydroxyl, and C 1~6 C, optionally substituted with one or more substituents each independently selected from the group consisting of alkyl 3~12 Alkyl, C 6~10 Aryl and C 6~10 aryl C alkyl, preferably R 9 is halogen, hydroxyl, and C 1~4 C, optionally substituted with one or more substituents each independently selected from the group consisting of alkyl 3~12 Alkyl, C 6~10 Aryl and C 6~10The initiator may be a monoalcohol. The alcohol may be a polyol, such as a diol, triol, or higher functional polyhydric alcohol. The alcohol, such as glycerol or propanediol or any other sugar-based alcohol, such as erythritol, may be derived from biomass. The alcohol may be used alone or in combination with other alcohols. In an embodiment, non-limiting examples of initiators include 1-octanol, 1-decanol, isopropanol, propanediol, trimethylolpropane, 2-butanol, 3-buten-2-ol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, 1,7-heptanediol, benzyl alcohol, 4-bromophenol, 1,4-benzenedimethanol, and (4-trifluoromethyl)benzyl alcohol, preferably the compound is selected from 1-octanol, isopropanol, and 1,4-butanediol. It is understood that similar initiators further having other nucleophilic groups, such as amine groups, may also be used. Macromolecules may also be used as initiators, so long as they contain suitable end groups, such as hydroxyl or amine end groups.
[0079] Selection of appropriate cocatalysts, initiators, and optional additives such as antioxidants, phosphates, epoxidized vegetable oils, plasticizers, catalyst killers, etc. is within the purview of one skilled in the art.
[0080] Preferably, the polymerization reaction is allowed to proceed to lactide equilibrium. The conversion can be determined immediately after polymerization or by online techniques such as mid-IR, near-IR, Raman spectroscopy, for example, in real time online by Raman spectroscopy and offline by gas chromatography.
[0081] In one embodiment, the composition thus obtained is subjected to a devolatilization step in order to reduce the monomer content of the composition. Prior to or simultaneously with the devolatilization step, the composition is subjected to a stabilization step using at least one compound of formula (I).
[0082] Thus, the present invention also encompasses a process for stabilizing an aliphatic polyester composition against depolymerization, comprising incorporating therein or applying thereto at least one compound of formula (I).Preferably, said process for stabilizing an aliphatic polyester against depolymerization comprises the steps of (a) forming an aliphatic polyester, and (b) stabilizing the polyester against depolymerization by incorporating therein or applying thereto at least one stabilizer to obtain a melt-stable polyester, said stabilizer being a compound of formula (I).
[0083] The present invention also includes the use of a compound of formula (I) as a stabilizer against aliphatic polyester depolymerization, preferably against polylactide depolymerization.The present invention also includes the use of at least one compound of formula (I) in a polylactide composition to inhibit the evolution of lactide in a melt of the polylactide composition.
[0084] The compound of formula (I) can be incorporated or applied in an amount of at least 0.010% by weight based on the total weight of the aliphatic polyester composition, for example, at least 0.025% by weight based on the total weight of the aliphatic polyester composition, preferably the polylactide composition. For example, the compound of formula (I) can be incorporated or applied in an amount of at least 0.050% by weight, for example, at least 0.075% by weight, for example, at least 0.090% by weight, for example, at least 0.10% by weight based on the total weight of the aliphatic polyester composition, preferably the polylactide composition. For example, the compound of formula (I) can be incorporated or applied in an amount of at most 0.50% by weight based on the total weight of the aliphatic polyester composition, preferably the polylactide composition. For example, the compound of formula (I) can be incorporated into or applied to the aliphatic polyester composition, preferably the polylactide composition, in an amount of at most 0.30 wt%, such as at most 0.20 wt%, such as at most 0.18 wt%, such as at most 0.15 wt%, based on the total weight of the composition.
[0085] Suitable compounds of formula (I) are R 1 is hydrogen or C 1~6 is alkyl, preferably R 1 is hydrogen or C 1~4 is alkyl, preferably R 1 is hydrogen or C 1~2 is alkyl, preferably R 1 is hydrogen or methyl, preferably R 1 is hydrogen, R 2 But hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR 7 )-(CH2) n -C(=O)- and C 1~6 alkylcarbonyl, preferably R 2 But hydrogen, C 1~4 Alkyl, HO-C(=O)-CH(NH2)-(CH2)2-C(=O)-, and C1~4 alkylcarbonyl, preferably R 2 is selected from the group consisting of hydrogen, C1-2 alkyl, HO-C(=O)-CH(NH2)-(CH2)2-C(=O)-, and C1-2 alkylcarbonyl, preferably R 2 is selected from the group consisting of hydrogen, methyl, ethyl, HO-C(=O)-CH(NH2)-(CH2)2-C(=O)-, and methylcarbonyl; R 3 But hydroxyl, C 1~6 Alkoxy, and -NH-(CH2) p -C(=O)-OH, preferably R 3 But hydroxyl, C 1~4 Alkoxy, and -NH-(CH2) p -C(=O)-OH containing groups, preferably R 3 is selected from the group including hydroxyl, C1-2 alkoxy, and -NH-CH2-C(=O)-OH, preferably R 3 is selected from the group comprising hydroxyl, methoxy, and -NH-CH2-C(=O)-OH, preferably R 3 is hydroxyl or -NH-(CH2) p -C(=O)-OH, m is an integer selected from 0, 1, or 2, preferably m is an integer selected from 1 or 2, preferably m is 1; n is an integer selected from 1 or 2, preferably n is 2; p is an integer selected from 1 or 2, preferably p is 1; Each R 4 are independently hydrogen or C 1~6 alkyl, preferably each R 4 are independently hydrogen or C 1~4 alkyl, preferably each R 4 are independently hydrogen or C 1~2 alkyl, preferably each R 4 is independently selected from hydrogen or methyl, preferably each R 4 is hydrogen, Each R 5 are independently hydrogen or C 1~6 alkyl, preferably each R 5 are independently hydrogen or C 1~4 alkyl, preferably each R 5 are independently hydrogen or C 1~2 alkyl, preferably each R 5 is independently selected from hydrogen or methyl, preferably each R 5 is hydrogen, R 6 is hydrogen or the formula [ka] (where: * represents the attachment point to S in formula (I) and R 7 But hydrogen, C 1~6 Alkyl, and C 1~6 alkylcarbonyl-containing groups, preferably R 7 is hydrogen or C 1~4 alkyl, preferably R 7 is hydrogen or C 1~2 alkyl, preferably R 7 is selected from hydrogen or methyl, preferably R 7 is hydrogen, It is a compound.
[0086] Preferred compounds of formula (I) are those in which R 1 is hydrogen and R 2 But hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR 7 )-(CH2) n -C(=O)- and C 1~6 alkylcarbonyl; R 3 is hydroxyl or -NH-CH-C(=O)-OH, m is an integer selected from 1 or 2, n is 2, p is 1, and each R 4 and R 5 is hydrogen and R6 is hydrogen or the formula [ka] and R 7 is a compound in which H is hydrogen.
[0087] Preferred compounds of formula (I) are those in which R 1 is hydrogen and R 2 is selected from the group consisting of hydrogen, HO-C(=O)-CH(NH2)-(CH2)2-C(=O)-, and methylcarbonyl; R 3 is hydroxyl or -NH-CH2-C(=O)-OH, m is 1, n is 2, p is 1, and each R 4 and R 5 is hydrogen and R 6 is hydrogen or the formula [ka] is a compound selected from the group consisting of:
[0088] Preferably, said compound of formula (I) is selected from the group comprising cysteine, cystine, N-acetyl-cysteine, N-acetyl-cystine, glutathione, their stereoisomers and mixtures thereof. Most preferred compounds are L-cysteine, L-cystine, N-acetyl-L-cysteine, N-acetyl-L-cystine, glutathione, D-cysteine, D-cystine, N-acetyl-D-cysteine, N-acetyl-D-cystine and mixtures thereof.
[0089] Unless otherwise specified, the chemical designation of a compound represents a mixture of all possible stereochemical isomeric forms, said mixture including all diastereomers and enantiomers of the basic molecular structure (since the compound of formula (I) has at least one chiral center) as well as stereochemically pure or enriched compounds. As used herein, unless otherwise specified, the term "enantiomer" refers to each individual optically active form of a compound having an optical purity or enantiomeric excess (as determined by standard methods in the art) of at least 80% (i.e., at least 90% of one enantiomer and at most 10% of the other enantiomer), preferably at least 90%, more preferably at least 98%.
[0090] In addition to adding the compounds of formula (I), further additives such as antioxidants and other stabilizers can be added to the composition.
[0091] Non-limiting examples of additional compounds suitable for stabilization include antioxidants such as vitamins, phosphite-containing compounds, polyfunctional carboxylic acids, hindered phenolic compounds, organic peroxides, catalyst deactivators such as hindered alkyl, aryl, and phenolic hydrazides, amides of aliphatic and aromatic mono- and dicarboxylic acids, cyclic amides, hydrazones and bishydrazones of aliphatic and aromatic aldehydes, hydrazides of aliphatic and aromatic mono- and dicarboxylic acids, bisacylated hydrazine derivatives, heterocyclic compounds, endcapping with anhydrides, and mixtures thereof.
[0092] Preferred antioxidants are phosphite-containing compounds, hindered phenolic compounds, or other phenolic compounds, including compounds such as trialkyl phosphites, mixed alkyl / aryl phosphites, alkylated aryl phosphites, sterically hindered aryl phosphites, aliphatic spirocyclic phosphites, sterically hindered phenyl spirocyclic compounds, sterically hindered bisphosphonites, vitamins, hydroxyphenylpropionates, hydroxybenzyls, alkylidene bisphenols, alkylphenols, aromatic amines, thioethers, hindered amines, hydroquinones, and mixtures thereof.
[0093] Preferably, the antioxidant has formula (II) or (III): [ka] (In the formula, R 40 , R 41 , R 42 , and R 43 is independently 1~8 alkyl, or R 40 and R 42 may each independently be hydrogen; R 44 , R 45 , and R 46 are independently hydrogen or C 1~8 (It is alkyl) The phosphite may be a compound of the formula:
[0094] Suitable phosphites include, but are not limited to, [ka] Examples include:
[0095] Most of the additives and stabilizers listed herein are commercially available.
[0096] The polymer is treated with the stabilizing compound by mixing the stabilizing compound and the composition, for example at a temperature similar to the polymerization temperature, which can be done using a static mixer, an extruder, or any other conventional method of mixing at least one highly viscous material.
[0097] The composition may also be subjected to a devolatilization step (d), which is carried out to remove volatile materials, particularly unreacted monomers, from the molten or solid polymer. Volatiles are removed by increasing the temperature under reduced pressure, e.g., under vacuum.
[0098] Examples of devolatilizers include extruders, especially twin-screw extruders, wiped film evaporators, falling film evaporators, rotary devolatilizers, rotary disk devolatilizers, centrifugal devolatilizers, flat plate devolatilizers, and static expansion chambers, e.g. those involving special distributors such as the Sulzer devolatilization technology described in EP 1 800 724.
[0099] Devolatilization in various stages and / or combinations of various types of equipment may also be possible, with the use of static expansion chambers being considered. A stripping gas such as nitrogen may be applied in one or more stages to facilitate devolatilization. Devolatilization may also be performed via the solid state after polymerization or by drying the solid pelletized material under vacuum or inert gas flow, for example in a tumble dryer. Optionally, a crystallization step may be performed prior to the drying step.
[0100] The composition can then be further processed directly for end use by extrusion, blow molding, film casting, film blowing, thermoforming, foaming, or elevated temperature fiber spinning to form a useful article. Optionally, the polymer can be compounded with additives such as antioxidants, nucleating agents, mineral fillers, glass or natural fibers, processing aids, UV stabilizers, or other polymer additives known to those skilled in the art.
[0101] The compositions may also be processed into particles such as beads, chips, or other pellets or powders in a manner known in the art and then sold to end users.
[0102] The present invention will be illustrated by the following examples without being limited thereto or by them. EXAMPLES
[0103] material If used, the following chemicals Lactide: Puralact L B3 resin grade, Corbion Thailand, ≥99% (w / w) Initiator: 2-Ethyl-1-hexanol, Acros, 99% Catalysts and solvents: TinOctoate, Sigma, 92.5-100.0%, Toluene, Fisher, 99.8+%, analytical grade Test stabilizers listed in Table A:
[0104] [Table 1]
[0105] analysis Absolute molecular weight Absolute molecular weight parameter M n , M w The molecular weight, molecular weight, and polydispersity index (PDI) were determined using gel permeation chromatography (GPC) with light scattering detection unless otherwise stated. Specifically, a Viscotek GPC Mx VE2001 system was used with 1,1,1,3,3,3-hexafluoro-2-propanol (also known as hexafluoroisopropanol or HFiP) in 0.02M CF3COOK as the solvent at a flow rate of 0.7 mL / min. The size exclusion columns used were two PSS PFG analytical linear columns (M, 300 × 8.00 mm, 7 μm) connected in series. 20-25 mg of polymerization mixture sample was weighed into a 20 ml crimp-capped vial, to which 17 grams of HFiP was added. The resulting suspension was shaken at room temperature for at least 16 hours. After 16 hours, 1 ml of sample was filtered through a PVDF 0.45 μm filter, transferred to a 2 ml vial, and injected into the GPC system for analysis.
[0106] Residual lactide content The amount of residual lactide in the polylactide samples was determined by a precipitation method to separate monomeric lactide from polymeric lactide in the polymerization mixture. A sample of the first polymerization mixture (containing polylactide and lactide monomer) was dissolved in a known amount of dichloromethane (containing an internal standard). The polylactide fraction of the polymerization mixture was then removed by precipitation by introducing the dichloromethane solution into an excess amount of a 5 / 95 acetone / hexane solvent mixture. After half an hour of precipitation, the polymeric fraction was removed by filtration through a 0.45 μm filter. The remaining solution was then analyzed using gas-liquid chromatography to determine the amount of lactide monomer in the sample.
[0107] Stereochemical purity After destructive methylation, the stereochemical purity of PLA was evaluated. For that purpose, 0.1 g of PLA was placed in a crimp-cap vial, followed by the addition of 2.0 g of dichloromethane (pure, Acros Organics) and 5.0 g of methanol (JT Baker), and the sample was dissolved at 70 °C for 2 h. After cooling to room temperature, 3.0 g of Amberlyst 15 (ion exchange resin, dry, Acros Organics) was added, and the saponification reaction was allowed to proceed at 80 °C for 22 h. After cooling to room temperature, the sample was subjected to chiral gas chromatographic separation on a Thermo Focus GC equipped with a CP-Chirasil-dex CB separation column. This achieved the separation of R- and S-methyl lactates, the ratio of which allowed the final determination of the stereochemical purity of the sample.
[0108] ring-opening polymerization Ring-opening polymerizations of lactide were carried out in a 2-liter batch reactor. All polymerizations were carried out with 150 ppm tin octoate and 20 Meq / kg 1-ethyl-2-hexanol.
[0109] Before feeding lactide to the batch reactor, the reactor was subjected to a vacuum of 3 mbar. The vacuum was then released by adding nitrogen to the reactor. This vacuum / nitrogen cycle was performed three times to remove any residual ambient atmosphere. For the dry reactor, 750 grams of Puralact L polymer grade was added to the reactor. A vacuum / nitrogen cycle was then performed on the lactide flakes in the cold reactor. After melting the L-lactide to 130°C under nitrogen, initiator: 1.97g 2-ethyl-1-hexanol and catalyst: 1.13gr 10% (w / w) tin octoate / toluene solution were added to start the polymerization. To better control the amount of tin octoate added, it was first dissolved in toluene and injected into the reactor. The temperature of the melt was increased to 180°C. The temperature was held at 180°C for 120 minutes and the melt was stirred at 50 rpm.
[0110] All stabilizers were then tested by adding them to the reactor after lactide equilibrium was reached. 0.1 wt% of stabilizer was added to the polymerization mixture in a batch reactor, which was then mixed at 180°C for 15 minutes. Immediately after, the reactor contents were offloaded into a steel bucket cooled with ice water, which was then chopped into millimeter-sized chips. The chips were spread in a Petri dish, which was then placed in a vacuum oven at 130°C. A small nitrogen bleed was applied to a vacuum of 5 mbar, and the degassing process was allowed to proceed under these conditions for 16 hours.
[0111] Samples of the original PLA and the corresponding stabilized PLA were analyzed for molecular weight and residual lactide monomer content as well as lactide reformation and rheological behavior.
[0112] The effectiveness of the stabilizers was evaluated using a lactide reformation experiment. During this test, a melt flow indexer is heated to 250°C and filled with 5 grams of sample. The sample is kept stationary at normal atmosphere and 250°C for 20 minutes. The heat aged sample is offloaded and analyzed for lactide content. The lactide content of the heat aged sample is compared to that of the non-heat aged sample. To be determined as a heat stable sample, the sample should have less than 0.3% lactide increase compared to the non-heat aged sample. The results are shown in Table 1.
[0113] [Table 2]
[0114] Comparative Examples 1 to 8 As can be seen in Table 1, except for the compounds used in this invention, all other compounds tested show lactide reformation above 0.3 wt %. Therefore, these additives are not effective catalyst deactivators.
[0115] Examples 1 to 6 Also shown in Table 1 are Examples 1-6 of the present invention, where L-cysteine, L-cystine, n-acetyl-L-cysteine, and glutathione all perform well in inhibiting lactide reformation. These compounds effectively prevent the backbiting reaction, demonstrating their effectiveness as catalyst deactivators. The compounds used in the present invention consistently showed less than 0.3 wt. % reformed lactide when exposed to 250° C. for 20 minutes. These compounds are effectively good stabilizers.
[0116] It can also be concluded from Example 6 that the combination of antioxidant Irgafos126 with L-cysteine results in a heat-stable PLA. Moreover, the incorporation of Irgafos126 into the polymerization of lactide equilibria improved the color of the stabilized PLA compared to Example 5.
[0117] Samples of PLA containing L-cysteine, n-acetyl-L-cysteine, L-cystine, and glutathione were subjected to a rheological time sweep (30 min, 10% amplitude, 1 s) at 250 °C. -1 The non-stabilized PLA samples were exposed to a 1000 Hz angular frequency (1000 Hz) and compared against the stabilized samples. All samples were dried in a dry air oven prior to measurement to reduce moisture content below 100 ppm. An Anton Paar MCR301 rotational rheometer with a 25 mm plate-plate geometry was used to heat the top plate and air to 250 °C with the bottom plate heated by an electric oven. Approximately 2 g of sample was added to the bottom plate at 250 °C and the top plate was lowered to a gap distance of 5 mm. The sample was allowed to melt at this setting for 5 min, after which the top plate was lowered to a gap distance of 0.5 mm to remove excess sample. The electric oven was then returned to the plate and sample and the measurement was started. The top plate was heated at 250 °C for 1 s for 30 min. -1 The mixture was then vibrated at a speed of 100 rpm and an amplitude of 10%. During this 30 minute period, the resistance to vibration was measured by the rheometer, which is a measurement for the complex viscosity.
[0118] The stabilized PLA should have a higher complex viscosity at the beginning of the measurement and should maintain a higher level for a longer period of time. These results are presented in Figures 1-4. Comparative example results are presented in Figures 5-7.
[0119] Figures 1-7 show that the results of the time sweep experiment are comparable to the lactide reforming experiment. The compound used in the present invention showed the best stabilization effect (Figures 1-4) compared to other agents tested (Figures 5-7). The time sweep at 250°C shows the increased and stabilized viscosity of the stabilized samples of the compound used in the present invention versus the original PLA. This confirms the stabilization effect of L-cysteine, n-acetyl-L-cysteine, L-cystine, and glutathione. From the rheological data shown in Figures 1-4, it can be observed that higher and more stable viscosity levels are achieved with the stabilized PLA.
[0120] The molecular weight retention and racemization of PLA containing L-cysteine and L-cystine were also investigated, and the results are shown in Table 2.
[0121] [Table 3]
[0122] The molecular weight results (Mw) shown in Table 2 indicate that the addition of the test compounds used in the present invention does not adversely affect the molecular weight at all. The results in Table 2 also show that there is no increase in racemization caused by one of the test compounds.
[0123] From the experimental results, L-cysteine, n-acetyl-L-cysteine, L-cystine, and glutathione all stabilize PLA against thermal degradation; Racemization after addition of the test compound does not occur in the compound of formula I; You can see that.
[0124] PLA exhibits high viscosity retention through the use of L-cysteine, n-acetyl-L-cysteine, L-cystine, and glutathione as stabilizers.
Claims
1. 1. A process for preparing a composition comprising an aliphatic polyester by ring-opening polymerization of a cyclic ester monomer, said process comprising: (a) providing a cyclic ester monomer and a polymerization catalyst to a reactor; (b) melt polymerizing the cyclic ester monomer to form a composition comprising an aliphatic polyester; (c) stabilizing said composition against aliphatic polyester depolymerization by incorporating therein or applying thereto at least one stabilizer to obtain a melt-stable composition; (d) optionally removing at least a portion of the residual cyclic ester monomer; and the stabilizer comprises a compound represented by formula (I): 【Chemistry 1】 [In the formula, R 1 is hydrogen or C 1~6 is alkyl, R 2 is hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR 7 )-(CH 2 ) n -C(=O)- and C 1~6 selected from the group including alkylcarbonyl; R 3 is hydroxyl, C 1~6 Alkoxy, and -NH-(CH 2 ) p -C(=O)-OH; m is an integer selected from 0, 1, or 2; n is an integer selected from 1 or 2; p is an integer selected from 1 or 2; Each R 4 are independently hydrogen or C 1~6 alkyl, Each R 5 are independently hydrogen or C 1~6 alkyl, R 6 is hydrogen or the formula 【Chemistry 2】 (where: * represents the attachment point to S in formula (I). and R 7 is hydrogen, C 1~6 Alkyl, and C 1~6 alkylcarbonyl] The process is a compound of.
2. 2. The process of claim 1, wherein the aliphatic polyester is a polylactide prepared by ring-opening polymerization of lactide, the process comprising the steps of: (a) providing lactide and a polymerization catalyst to a reactor; (b) melt polymerizing the lactide to form a composition comprising polylactide; (c) stabilizing the composition against polylactide depolymerization by incorporating therein or applying thereto at least one stabilizer, wherein said stabilizer is at least one compound of Formula (I), to obtain a melt-stable composition; and (d) optionally removing at least a portion of the residual lactide.
3. R 1 is hydrogen, R 2 is hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR 7 )-(CH 2 ) n -C(=O)- and C 1~6 selected from the group including alkylcarbonyl; R 3 is hydroxyl or -NH-CH 2 -C(=O)-OH, m is an integer selected from 1 or 2; n is 2; p is 1, Each R 4 and R 5 is hydrogen, R 6 is hydrogen or the formula 【Chemistry 3】 and R 7 is hydrogen, 3. The process according to claim 1 or 2.
4. 4. The process according to any one of claims 1 to 3, wherein the compound of formula (I) is selected from the group comprising cysteine, cystine, N-acetyl-cysteine, N-acetyl-cystine, glutathione, stereoisomers thereof, and mixtures thereof.
5. The process of any one of claims 1 to 4, wherein the compound of formula (I) is present in an amount of at least 0.010 wt%, based on the total weight of the composition of the aliphatic polyester.
6. 6. The process of any one of claims 1 to 5, comprising adding at least one antioxidant prior to or simultaneously with step (c).
7. 7. The process of any one of claims 1 to 6, wherein simultaneously with or after step (c) the composition is subjected to one or more steps (d), which step (d) is a devolatilization step (d).
8. A composition directly obtainable by the process according to any one of claims 1 to 7, said composition comprising a polylactide and at least one compound of formula (I).
9. 1. A process for stabilizing an aliphatic polyester against depolymerization, comprising: (a) forming an aliphatic polyester; and (b) stabilizing said polyester against depolymerization by incorporating therein or applying thereto at least one stabilizer to obtain a melt-stable polyester, said stabilizer being represented by formula (I): 【Chemistry 4】 [In the formula, R 1 is hydrogen or C 1~6 is alkyl, R 2 is hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR 7 )-(CH 2 ) n -C(=O)- and C 1~6 selected from the group including alkylcarbonyl; R 3 is hydroxyl, C 1~6 Alkoxy, and -NH-(CH 2 ) p -C(=O)-OH; m is an integer selected from 0, 1, or 2; n is an integer selected from 1 or 2; p is an integer selected from 1 or 2; Each R 4 are independently hydrogen or C 1~6 alkyl, Each R 5 are independently hydrogen or C 1~6 alkyl, R 6 is hydrogen or the formula 【Chemistry 5】 (where: * represents the attachment point to S in formula (I). is selected from the group R 7 is hydrogen, C 1~6 Alkyl, and C 1~6 alkylcarbonyl] The process is a compound of.
10. 10. The process of claim 9, wherein the aliphatic polyester is a lactic acid based polyester, preferably polylactic acid.
11. 11. The process according to claim 9 or 10, wherein the compound of formula (I) is selected from the group comprising cysteine, cystine, N-acetyl-cysteine, N-acetyl-cystine, glutathione, stereoisomers thereof, and mixtures thereof.
12. The process of any one of claims 9 to 11, further comprising incorporating or applying at least an antioxidant.
13. As stabilizers against depolymerization of aliphatic polyesters, 【Chemistry 6】 [In the formula, R 1 is hydrogen or C 1~6 is alkyl, R 2 is hydrogen, C 1~6 Alkyl, HO-C(=O)-CH(NHR 7 )-(CH 2 ) n -C(=O)- and C 1~6 selected from the group including alkylcarbonyl; R 3 is hydroxyl, C 1~6 Alkoxy, and -NH-(CH 2 ) p -C(=O)-OH; m is an integer selected from 0, 1, or 2; n is an integer selected from 1 or 2; p is an integer selected from 1 or 2; Each R 4 are independently hydrogen or C 1~6 alkyl, Each R 5 are independently hydrogen or C 1~6 alkyl, R 6 is hydrogen or the formula 【Chemistry 7】 (where: * represents the attachment point to S in formula (I). and R 7 is hydrogen, C 1~6 Alkyl, and C 1~6 alkylcarbonyl] Use of compounds.
14. The use according to claim 13, wherein the aliphatic polyester is a polylactide.
15. 15. The use according to claim 13 or 14, wherein the compound of formula (I) is selected from the group comprising cysteine, cystine, N-acetyl-cysteine, N-acetyl-cystine, glutathione, stereoisomers thereof, and mixtures thereof.
Citation Information
Patent Citations
Production of lactic acid polyester
JP1997077863A
Production of polylactic acid resin excellent in heat stability
JP1997110967A
Aliphatic polyester and / or copolyester and method for producing same
JP2000514483A