Electrophotographic developer set including toner and powder adhesive, method for producing adhesive, and powder adhesive
The electrophotographic developer set with controlled wax properties in toner and powder adhesive addresses the issues of print transfer and adhesive strength, enabling effective simultaneous printing on paper bags and plain paper.
Patent Information
- Application Number
- JP2020130345
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-31
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-07-31
AI Technical Summary
Existing methods for printing on paper bags and plain paper simultaneously face challenges with adhesive toners that either fail to achieve strong adhesive strength or result in print transfer, as they either melt at inappropriate temperatures or do not provide sufficient adhesion.
An electrophotographic developer set comprising a toner with a thermoplastic resin and wax, and a powder adhesive with specific ester group concentrations and wax content ratios, designed to minimize print transfer and enhance adhesive strength by controlling the interaction between wax and paper components.
The developer set effectively prevents print transfer while achieving strong adhesive strength, allowing for the production of paper bags with reliable bonding and minimal image transfer.
Smart Images

Figure 0007555752000013 
Figure 0007555752000014 
Figure 0007555752000015
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an electrophotographic developer set including a toner and a powder adhesive, which develops an electrostatic latent image on a recording material by electrophotography to form a toner image and an adhesive part made of the powder adhesive having an adhesive function, and a method for producing an adhesive product using the electrophotographic developer set. [Background technology]
[0002] Conventionally, when using a printer or copier to create paper bags with different information printed on them for each individual, a pre-made paper bag would be set in the printer or copier and printed on. Therefore, when printing on paper bags and on plain paper at the same time, there was a problem that the paper used in the printer had to be changed from the paper bag to plain paper every time the printing target was changed, or the printing target was printed on the wrong target. In response to the above problems, a method has been proposed in which, in addition to forming an image with toner using an electrophotographic method, a bonding section is formed with a powder adhesive without pigment, and then the paper is bonded. In addition, a method has been proposed in which, by using this method, printing is performed on plain paper and the plain paper is simultaneously processed into a paper bag. In addition, a toner and a powder adhesive to be used in this method have been proposed. Patent Document 1 proposes an image forming method in which an image and an adhesive portion are formed using an adhesive toner having a lower limit of an appropriate fixing temperature than a toner for image formation. Patent Document 2 proposes a powder adhesive for electrophotography, which has a basic structure of a cyclic polyolefin resin. Patent Document 3 proposes an adhesive material for electrophotography using a styrene resin and a (meth)acrylic acid ester resin. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2006-171607 A [Patent Document 2] JP 2008-170659 A [Patent Document 3] JP 2019-167471 A Summary of the Invention [Problem to be solved by the invention]
[0004] The method described in Patent Document 1 discloses that by using an adhesive toner whose minimum optimum fixing temperature is lower than that of the image-forming toner, the adhesive toner can be melted at a temperature at which the image-forming toner does not melt. However, when this method is used to form an image area using toner and an adhesive area using powder adhesive on paper, and then the paper is stacked with the image area and adhesive area on the inside and the adhesive area is melted to make a paper bag, strong adhesive strength may not be obtained. Also, when the adhesive area is sufficiently heated and melted to obtain strong adhesive strength, the image area may melt and a phenomenon (print transfer) may occur in which part of the image area transfers to the opposing paper, and it was found that it is difficult to achieve both print transfer and strong adhesive strength. Furthermore, the powder adhesives described in Patent Documents 2 and 3 are intended for use in peeling off the adhesive portion, and therefore do not provide a strong adhesive strength sufficient for making paper bags. The present disclosure provides an electrophotographic developer set that is resistant to transfer of print and provides strong adhesive strength, and that includes a toner and a powder adhesive, and a method for producing an adhesive product using the electrophotographic developer set. [Means for solving the problem]
[0005] 1. An electrophotographic developer set comprising a toner containing a thermoplastic resin and a wax, and a powder adhesive containing a thermoplastic resin and a wax, When the ester group concentration of the wax contained in the toner is Ea (mmol / g), the content of the wax in the toner is Na (mass %), the ester group concentration of the wax contained in the powder adhesive is Eb (mmol / g), and the content of the wax in the powder adhesive is Nb (mass %), 0.00≦Ea≦2.45 2.50≦Eb≦3.60 0.80≦Nb / Na The electrophotographic developer set is Effect of the Invention
[0006] According to the present disclosure, it is possible to provide an electrophotographic developer set including a toner and a powder adhesive, which is resistant to print transfer and provides strong adhesive strength, and a method for producing an adhesive product using the electrophotographic developer set. [Brief description of the drawings]
[0007] [Figure 1] Schematic diagram of an image forming apparatus [Diagram 2] FIG. 2 is a diagram for explaining attachment of an adhesive unit to a main body of an image forming apparatus; [Diagram 3] FIG. 1 is a diagram showing a sheet transport path in an image forming apparatus; [Figure 4] A diagram to explain the folding process [Diagram 5] FIG. 1 is a perspective view showing an external appearance of an image forming apparatus; [Figure 6] FIG. 1 is a diagram illustrating an example of a product output by an image forming apparatus. [Figure 7] Schematic diagram of a process cartridge [Figure 8] Schematic diagram of evaluation sample [Figure 9] Schematic diagram of evaluation sample [Figure 10] Schematic diagram of adhesive strength evaluation DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] In the present disclosure, the expressions "XX or more and YY or less" and "XX to YY" representing a numerical range mean a numerical range including the endpoints, that is, the lower limit and the upper limit, unless otherwise specified. When numerical ranges are stated in stages, the upper and lower limits of each numerical range can be combined in any way. The methods for measuring the various physical properties will be described below.
[0009] First, an example of a method for producing a paper bag by an electrophotographic method using an electrophotographic developer set containing the above toner and powder adhesive will be described below. First, an image area made of toner and an adhesive area made of powder adhesive are developed on paper using an electrophotographic method (developing process). After that, the image area and adhesive area are fixed on the paper by heating (fixing process), and the paper is stacked so that the adhesive area is sandwiched between the sheets and further heated to melt the adhesive area and adhere it (adhesive process), thereby producing a paper bag. At this time, the paper can be stacked by folding the paper or by placing a different paper on top of it. Here, the inventors considered that it is important to reduce the adhesive strength between the toner and the paper in order to prevent the transfer of the image portion during the adhesion process, while it is important to increase the adhesive strength between the powder adhesive and the paper in order to obtain a strong adhesive force, and conducted extensive research to satisfy these two conflicting requirements.
[0010] The present disclosure relates to 1. An electrophotographic developer set comprising a toner containing a thermoplastic resin and a wax, and a powder adhesive containing a thermoplastic resin and a wax, When the ester group concentration of the wax contained in the toner is Ea (mmol / g), the content of the wax in the toner is Na (mass %), the ester group concentration of the wax contained in the powder adhesive is Eb (mmol / g), and the content of the wax in the powder adhesive is Nb (mass %), 0.00≦Ea≦2.45 2.50≦Eb≦3.60 0.80≦Nb / Na The present invention relates to an electrophotographic developer set comprising:
[0011] By controlling the physical properties of the developer set within the above ranges, it became possible to achieve both suppression of print transfer and strong adhesion. The inventors speculated that the reason for this was as follows, focusing on the interaction between the ester groups of the wax contained in the toner and powder adhesive and the hydroxyl groups of cellulose, the main material of paper. There are many hydroxyl groups on the surface of cellulose, and these hydroxyl groups bond with each other through hydrogen bonds to form paper. For this reason, if the powder adhesive contains many ester groups that can form hydrogen bonds with hydroxyl groups, the affinity between the powder adhesive and cellulose increases. This increased affinity improves the wettability of the powder adhesive with cellulose, and increases the rate at which the powder adhesive penetrates into the paper. As a result, the adhesive strength between the powder adhesive and paper improves.
[0012] In addition, since wax has a low viscosity when molten, the more ester groups introduced into the wax, the faster it will penetrate into the paper. Therefore, when wax with many ester groups introduced is added to a powder adhesive, the wax will penetrate into the paper quickly, and the entire powder adhesive will penetrate into the paper in a similar manner, greatly improving the adhesive strength between the powder adhesive and the paper. On the other hand, waxes generally have low polarity and low affinity for polar groups such as hydroxyl groups, etc. Therefore, when wax with a low amount of ester groups is added to a toner or powder adhesive, it actually inhibits the toner or powder adhesive from penetrating into the paper, reducing the adhesiveness to the paper.
[0013] Based on the above, in order to reduce the ester group concentration of the wax contained in the toner, when the ester group concentration of the wax contained in the toner is Ea (mmol / g), Ea must be 0.00 or more and 2.45 or less. By making Ea 2.45 or less, the adhesiveness between the toner and paper can be reduced, making it difficult for print transfer to occur. Furthermore, in order to increase the ester group concentration of the wax contained in the powder adhesive, when the ester group concentration of the wax contained in the powder adhesive is Eb (mmol / g), Eb must be 2.50 or more. By making Eb 2.50 or more, the adhesiveness between the powder adhesive and paper can be increased, and strong adhesive strength can be obtained. Furthermore, by making Eb 3.60 or less, excessive penetration of the powder adhesive into the paper can be prevented, and strong adhesive strength can be obtained. More preferably, Ea is 0.00 or more and 1.95 or less, and Eb is 2.60 or more and 3.40 or less.
[0014] Furthermore, in order to achieve both suppression of print transfer and strong adhesive strength, when the wax content in the toner is Na (mass %) and the wax content in the powder adhesive is Nb (mass %), the wax content ratio Nb / Na must be 0.80 or more. Setting the Nb / Na ratio to 0.80 or more means that the amount of wax contained in the powder adhesive is not too much or too little compared to the amount of wax contained in the toner. This makes it possible to make the amount of heat absorbed by the toner smaller than the amount of heat absorbed by the powder adhesive. Therefore, the heat provided by the fixing device in the adhesion process is not easily absorbed when the toner melts, and the amount of heat absorbed by the powder adhesive is not easily absorbed. It is unlikely to inhibit the melting of the material. As a result, the powder adhesive and paper can be strongly bonded. When the Nb / Na ratio is increased, heat is lost when the powder adhesive melts, which inhibits the toner from melting, and the adhesion between the toner and paper decreases, making it possible to achieve both print transfer prevention and strong adhesive strength. Nb / Na is preferably 1.00 or more and 6.00 or less, and more preferably 1.10 or more and 2.50 or less.
[0015] In the present disclosure, a compound having a molecular weight of 3000 or less and having an endothermic peak with an endothermic amount of 80 J / g or more as measured by differential scanning calorimetry (DSC) is defined as a wax.
[0016] The Ea and the Eb are 0.50≦Eb-Ea≦3.40 It is preferable that the difference between Ea and Eb is larger, and the effect of lowering the adhesiveness between the toner and the paper and the effect of increasing the adhesiveness between the powder adhesive and the paper can be achieved at a higher level. It is more preferable that Eb-Ea is 0.70 or more and 3.40 or less. The Ea and Eb can be controlled by the type and amount ratio of the wax contained in the toner and the powder adhesive, and the Na and Nb can be controlled by the amount of the wax contained in the toner and the powder adhesive.
[0017] The wax contained in the powder adhesive preferably contains at least one selected from the group consisting of ester waxes represented by the following formulas (1) and (2).
[0018] [ka]
[0019] In the formula, l represents a positive integer of 2 or more and 12 or less (preferably 2 or more and 4 or less), n and m each independently represent a positive integer of 12 or more and 20 or less (preferably 14 or more and 20 or less), p represents a positive integer of 2 or more and 10 or less (preferably 2 or more and 4 or less), and q and r each independently represent a positive integer of 11 or more and 21 or less (preferably 14 or more and 20 or less). The ester waxes shown in formulas (1) and (2) have a linear structure and are easily crystallized, and the degree of crystallization in the powder adhesive is high, making it possible to obtain a powder adhesive with superior durability. Therefore, even when a large amount of printing is performed, contamination of developing devices and the like is unlikely to occur. In addition, the ester waxes shown in formulas (1) and (2) have close ester groups, so they have a strong interaction with the hydroxyl groups of cellulose. Therefore, it is easy to promote the penetration of the powder adhesive into the paper, and a stronger adhesive strength can be obtained. The ester wax is more preferably a compound represented by the following formula (3): It is more preferable that the wax contained in the powder adhesive contains an ester wax represented by the following formula (3).
[0020] [ka]
[0021] (n and m each independently represent a positive integer of 14 or more and 20 or less.) The ester wax shown in formula (3) has two ester groups close to each other in the molecule, which makes it easier to crystallize, and it is possible to obtain a powder adhesive with better durability. It is more preferable that n and m in formula (3) are each independently 16 or more and 20 or less.
[0022] The wax contained in the powder adhesive preferably further contains a chain saturated hydrocarbon having a peak carbon number of 20 or more and 70 or less (preferably 30 or more and 60 or less). The chain saturated hydrocarbon crystallizes faster than the above-mentioned ester wax and acts as a crystal nucleating agent for the ester wax. Therefore, the crystallinity of the ester wax is increased, and a powder adhesive having even greater durability can be obtained. The peak value of the carbon number is the peak value of the molecular weight obtained by measuring the molecular weight of acyclic saturated hydrocarbons. 2 This is the value obtained by dividing the formula quantity by 14.
[0023] The content Nb1 of the ester wax in the powder adhesive is preferably 8.0 mass% or more and 20.0 mass% or less, more preferably 8.0 mass% or more and 15.0 mass% or less, and even more preferably 9.0 mass% or more and 12.0 mass% or less. The content Nb2 of chain saturated hydrocarbons having a peak value of the carbon number of 20 or more and 70 or less in the powder adhesive is preferably 0.1 mass % or more and 5.0 mass % or less, and more preferably 0.5 mass % or more and 3.0 mass % or less. The Nb1 and the Nb2 2.00≦Nb1 / Nb2≦25.00 It is more preferable that Nb1 / Nb2 is equal to or greater than 3.00 and equal to or less than 7.00. Such a powder adhesive can be suitably used in electrophotographic processes and can provide strong adhesive properties.
[0024] The wax content Nb in the powder adhesive is preferably 8.0% by mass or more and 20.0% by mass or less. By having Nb in the above range, the adhesive strength between the powder adhesive and paper can be increased while preventing the powder adhesive from penetrating too much into the paper. Therefore, stronger adhesive strength can be obtained. The Nb content is more preferably 10.0 mass % or more and 17.0 mass % or less, and further preferably 10.0 mass % or more and 15.0 mass % or less.
[0025] The wax content Na in the toner is preferably 2.0% by mass or more and 15.0% by mass or less. By having Na in the above range, the amount of heat absorbed by the toner can be suppressed while reducing the adhesiveness between the toner and paper. Therefore, it is possible to achieve both excellent levels of print transfer and strong adhesiveness. The Na content is more preferably 5.0% by mass or more and 13.0% by mass or less, and further preferably 5.0% by mass or more and 10.0% by mass or less.
[0026] There are no particular limitations on the wax used in the toner, so long as it satisfies the above ester group concentration. The wax may be any known wax. Specific examples of the wax include the following. Hydrocarbon waxes (for example, petroleum waxes such as paraffin wax, microcrystalline wax, petroleum waxes and derivatives thereof, montan wax and derivatives thereof, hydrocarbon waxes and derivatives thereof produced by the Fischer-Tropsch process, polyolefin waxes and derivatives thereof such as polyethylene and polypropylene), natural waxes and derivatives thereof such as carnauba wax and candelilla wax, ester waxes, etc. Here, the derivatives include oxides, block copolymers with vinyl monomers, and graft modified products.
[0027] The wax contained in the toner is preferably at least one selected from the group consisting of hydrocarbon waxes and ester waxes. In addition, examples of ester waxes that can be used include monoester compounds containing one ester bond per molecule, diester compounds containing two ester bonds per molecule, and polyfunctional ester compounds such as trifunctional ester compounds containing three ester bonds per molecule, tetrafunctional ester compounds containing four ester bonds per molecule, and hexafunctional ester compounds containing six ester bonds per molecule. Among these, it is preferable to contain at least one compound selected from the group consisting of monoester compounds and diester compounds.
[0028] Specific examples of monoester compounds include waxes mainly composed of fatty acid esters, such as carnauba wax and montan acid ester wax; fatty acid esters from which some or all of the acid components have been deoxidized, such as deoxidized carnauba wax; compounds obtained by hydrogenating vegetable fats and oils; methyl ester compounds having a hydroxy group; and saturated fatty acid monoesters, such as stearyl stearate and behenyl behenate. Specific examples of the diester compound include dibehenyl sebacate, nonanediol dibehenate, behenate terephthalate, and stearyl terephthalate. The wax may contain other known waxes other than the above compounds. The wax may be used alone or in combination of two or more kinds.
[0029] The wax contained in the toner is preferably a saturated fatty acid monoester. For example, the toner preferably contains an ester compound of a monoalcohol having 18 to 24 carbon atoms and a monocarboxylic acid having 18 to 24 carbon atoms. Behenyl behenate is more preferable.
[0030] Furthermore, it is preferable that both the powder adhesive and the toner contain at least one compound selected from the group consisting of monoester compounds and diester compounds. Monoester compounds and diester compounds tend to have a higher degree of crystallinity and a larger amount of heat absorption than hydrocarbon waxes and trifunctional or higher ester compounds. Therefore, if the powder adhesive and toner satisfy the above conditions, when the powder adhesive and toner melt in the adhesion process, the melting behavior of the wax is easily matched, and the effects of the above physical properties are easily obtained.
[0031] The thermoplastic resin contained in the toner and the powder adhesive is not particularly limited. For example, known thermoplastic resins such as polyester resins, vinyl resins, acrylic resins, styrene-acrylic resins, polyethylene, polypropylene, polyolefin, ethylene-vinyl acetate copolymer resins, and ethylene-acrylic acid copolymer resins can be used. A plurality of these resins may be contained. The thermoplastic resins contained in the toner and the powder adhesive may be the same or different.
[0032] The thermoplastic resin is preferably a polyester resin or a styrene-acrylic resin, more preferably a styrene-acrylic resin. It is preferable that the thermoplastic resin contains at least one selected from the group consisting of an ester resin and a styrene-acrylic resin, and more preferable that the thermoplastic resin contains a styrene-acrylic resin. The content of the styrene-acrylic resin in the thermoplastic resin is preferably 50% by mass to 100% by mass, more preferably 80% by mass to 100% by mass, and even more preferably 90% by mass to 100% by mass. As the polyester resin, a known polyester resin can be used. Specific examples include condensation polymers of dibasic acids and their derivatives (carboxylic acid halides, esters, acid anhydrides) and dihydric alcohols. If necessary, trivalent or higher polybasic acids and their derivatives (carboxylic acid halides, esters, acid anhydrides), monobasic acids, trivalent or higher alcohols, and monohydric alcohols may also be used.
[0033] Examples of dibasic acids include aliphatic dibasic acids such as maleic acid, fumaric acid, itaconic acid, oxalic acid, malonic acid, succinic acid, dodecylsuccinic acid, dodecenylsuccinic acid, adipic acid, azelaic acid, sebacic acid, and decane-1,10-dicarboxylic acid; and aromatic dibasic acids such as phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, tetrabromophthalic acid, tetrachlorophthalic acid, HET acid, himic acid, isophthalic acid, terephthalic acid, and 2,6-naphthalenedicarboxylic acid. Furthermore, examples of derivatives of dibasic acids include carboxylic acid halides, esters and acid anhydrides of the above aliphatic dibasic acids and aromatic dibasic acids.
[0034] On the other hand, examples of dihydric alcohols include acyclic aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, and neopentyl glycol; bisphenols such as bisphenol A and bisphenol F; alkylene oxide adducts of bisphenol A such as an ethylene oxide adduct of bisphenol A and a propylene oxide adduct of bisphenol A; and aralkylene glycols such as xylylenediglycol.
[0035] Examples of trivalent or higher polybasic acids and anhydrides thereof include trimellitic acid, trimellitic anhydride, pyromellitic acid, and pyromellitic anhydride.
[0036] Examples of polymerizable monomers capable of forming the styrene-acrylic resin include styrene-based monomers such as styrene, α-methylstyrene, and divinylbenzene; unsaturated carboxylic acid esters such as methyl acrylate, butyl acrylate, methyl methacrylate, 2-hydroxyethyl methacrylate, t-butyl methacrylate, and 2-ethylhexyl methacrylate; unsaturated carboxylic acids such as acrylic acid and methacrylic acid; unsaturated dicarboxylic acids such as maleic acid; unsaturated dicarboxylic anhydrides such as maleic anhydride; nitrile-based vinyl monomers such as acrylonitrile; halogen-containing vinyl monomers such as vinyl chloride; and nitro-based vinyl monomers such as nitrostyrene. These may be used alone or in combination.
[0037] The unsaturated carboxylate is preferably a (meth)acrylic acid alkyl ester having an alkyl group with 1 to 8 (more preferably 2 to 6) carbon atoms. The styrene-acrylic resin is preferably a copolymer of styrene and a (meth)acrylic acid alkyl ester having an alkyl group with 1 to 8 (more preferably 2 to 6) carbon atoms.
[0038] The content of the thermoplastic resin in the powder adhesive is preferably 75.0% by mass or more and 92.0% by mass or less, and more preferably 80.0% by mass or more and 90.0% by mass or less. The content of thermoplastic resin in the toner is 75.0% by mass or more and 92.0% by mass or less. is preferable, and the content is more preferably 80.0 mass % or more and 90.0 mass % or less.
[0039] The ester group concentration Ec1 of the thermoplastic resin contained in the toner and the ester group concentration Ec2 of the thermoplastic resin contained in the powder adhesive are preferably 0.00 mmol / g or more and 2.50 mmol / g or less, and more preferably 1.50 mmol / g or more and 2.20 mmol / g or less. The above range means that the concentration of ester groups in the thermoplastic resin is low. By setting the concentration in the above range, the ester groups in the thermoplastic resin are less likely to inhibit the interaction between the ester groups in the wax and the hydroxyl groups in the paper, so that the effects of suppressing print transfer and providing strong adhesive strength are more easily obtained.
[0040] Furthermore, the difference between the ester group concentration of the thermoplastic resin contained in the toner and the ester group concentration of the thermoplastic resin contained in the powder adhesive is preferably 0.00 mmol / g or more and 1.50 mmol / g or less, and more preferably 0.00 mmol / g or more and 0.50 mmol / g or less. When the ester group concentrations of the thermoplastic resins contained in the toner and the powder adhesive are close to each other, the effects of suppressing print transfer and strong adhesive strength are more easily obtained. The ester group concentration of the thermoplastic resin can be controlled by the types and amount ratios of the monomers used in the thermoplastic resin.
[0041] The toners and powder adhesives may contain colorants, including black colorants, yellow colorants, magenta colorants, and cyan colorants. Examples of black colorants include carbon black. Examples of yellow colorants include yellow pigments such as monoazo compounds, disazo compounds, condensed azo compounds, isoindolinone compounds, isoindoline compounds, benzimidazolone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Specific examples include CI Pigment Yellow 74, 93, 95, 109, 111, 128, 155, 174, 180, and 185.
[0042] Magenta colorants include magenta pigments such as monoazo compounds, condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Specific examples include CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 150, 166, 169, 177, 184, 185, 202, 206, 220, 221, 238, 254, and 269, and CI Pigment Violet Red 19.
[0043] Examples of cyan colorants include cyan pigments such as copper phthalocyanine compounds and their derivatives, anthraquinone compounds, basic dye lake compounds, etc. Specific examples include CI Pigment Blue 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, and 66. In addition to the pigment, various dyes conventionally known as colorants can also be used. The content of the colorant in the toner is preferably from 1.0% by mass to 20.0% by mass. The content of the colorant in the powder adhesive is preferably 0.0% by mass or more and 1.0% by mass or less.
[0044] The toner and powder adhesive may contain known materials, such as charge control agents, charge control resins, pigment dispersants, etc., as necessary.
[0045] If necessary, an external additive may be mixed into the toner and powder adhesive and adhered to the surface thereof. The external additive may be an inorganic fine particle selected from silica fine particles, alumina fine particles, titania fine particles, or a composite oxide thereof, etc. The composite oxide may be, for example, silica aluminum fine particles, strontium titanate fine particles, etc. The content of the external additive in the toner is preferably from 0.01% by mass to 10.0% by mass, and more preferably from 0.1% by mass to 4.0% by mass. The content of the external additive in the powder adhesive is preferably 0.01% by mass or more and 10.0% by mass or less, and more preferably 0.1% by mass or more and 4.0% by mass or less. The difference between the content of the external additive in the toner and the content of the external additive in the powder adhesive is preferably 0.0% by mass or more and 2.5% by mass or less, and more preferably 0.0% by mass or more and 2.0% by mass or less. The ratio of the content of the external additive in the toner to the content of the external additive in the powder adhesive (content of the external additive in the toner:content of the external additive in the powder adhesive) is preferably 1.0:8.0 to 8.0:1.0, more preferably 1.0:4.0 to 4.0:1.0, and even more preferably 1.0:2.0 to 2.0:1.0.
[0046] The glass transition temperature (Tg) of the toner or powder adhesive is preferably 45° C. or more and 60° C. or less. When the glass transition temperature is within the above range, the toner or powder adhesive can be suitably used in electrophotographic processes, and the effects of suppressing print transfer and providing strong adhesive strength can be obtained at a higher level. Furthermore, the difference between the Tg of the toner and the Tg of the powder adhesive is preferably 0° C. or more and 10° C. or less, and more preferably 0° C. or more and 7° C. or less. By making the Tg of the toner and the powder adhesive similar, it is possible to make the melted states in the adhesion process similar, making it easier to obtain the effects of suppressing print transfer and strong adhesive strength. The Tg of the toner and the powder adhesive can be controlled by the types and quantitative ratios of monomers used in the thermoplastic resins of the toner and the powder adhesive, or the types and quantitative ratios of waxes used.
[0047] The weight average particle diameter (D4) of the toner is preferably 4.0 μm or more and 15.0 μm or less. By being in the above range, the melting state in the adhesion process can be made uniform, so that a toner that is more resistant to print transfer can be obtained. The powder adhesive preferably has a weight average particle size (D4) of 4.0 μm or more and 20.0 μm or less. By being in this range, the melted state in the bonding process can be made uniform, and the thickness of the bonded part can be made sufficiently thick, resulting in stronger adhesive strength. Furthermore, it is preferable that the difference between the weight average particle diameter (D4) of the toner and the weight average particle diameter (D4) of the powder adhesive is 0.0 μm or more and 5.0 μm or less. By making the weight average particle diameter (D4) of the toner and the powder adhesive similar, it is possible to make the melting states in the adhesion process similar, so that it is easy to obtain the effects of suppressing print transfer and strong adhesive strength. The weight average particle diameter (D4) of the toner and the powder adhesive can be controlled by the manufacturing method of the toner and the powder adhesive.
[0048] The toner and the powder adhesive each preferably have a peak molecular weight of the main peak of 10,000 or more and 40,000 or less. When the peak molecular weight is within the above range, the toner and the powder adhesive can be suitably used in an electrophotographic process, and the effects of suppressing print transfer and providing strong adhesive strength can be obtained at a higher level. Furthermore, the difference between the peak molecular weight of the toner and the peak molecular weight of the powder adhesive is preferably 0 to 15,000. By making the peak molecular weights of the toner and the powder adhesive similar, the melting states in the adhesion process can be made similar, making it easier to obtain the effects of suppressing print transfer and strong adhesive strength. The peak molecular weight can be controlled by the manufacturing conditions of the thermoplastic resins of the toner and the powder adhesive.
[0049] The toner or powder adhesive can be produced by a known method such as a pulverization method, a suspension polymerization method, an emulsion aggregation method, or a dissolution suspension method, and the production method is not particularly limited.
[0050] In addition, powder adhesives are A powder adhesive comprising a thermoplastic resin, a compound represented by the above formula (3), and a chain saturated hydrocarbon having a carbon number of 20 to 70, the thermoplastic resin is a styrene-acrylic resin, The content of the thermoplastic resin in the powder adhesive is 75.0% by mass or more and 92.0% by mass or less, The content Nb1 of the compound represented by formula (3) in the powder adhesive is 8.0% by mass or more and 20.0% by mass or less, The content Nb2 of chain saturated hydrocarbons having a carbon number of 20 to 70 in the powder adhesive is 0.1% by mass or more and 5.0% by mass or less, The Nb1 and the Nb2 2.00≦Nb1 / Nb2≦25.00 It is preferable that the powder adhesive satisfies the above requirement. Such a powder adhesive can be suitably used in an electrophotographic process and can provide strong adhesiveness.
[0051] The Nb1 is preferably 8.0% by mass or more and 15.0% by mass or less, and more preferably 9.0% by mass or more and 12.0% by mass or less. The Nb2 is more preferably 0.5% by mass or more and 3.0% by mass or less. The Nb1 / Nb2 is more preferably 3.00 or more and 7.00 or less.
[0052] An example of an image forming apparatus and a processing apparatus for performing adhesive processing on paper, in which an electrophotographic developer containing a toner and a powdery adhesive can be suitably used, will be specifically described below. (Overall device configuration) First, the overall configuration of the image forming apparatus will be described with reference to Figures 1, 2, and 5. Figure 1 is a schematic diagram showing the cross-sectional configuration of an image forming apparatus 1 that includes an image forming apparatus main body (hereinafter referred to as apparatus main body 10) and a post-processing unit 30 connected to the apparatus main body 10. The image forming apparatus 1 is an electrophotographic image forming apparatus (electrophotographic system) that includes the apparatus main body 10 that includes an electrophotographic printing mechanism and the post-processing unit 30 as a sheet processing device.
[0053] 5 is a perspective view showing the external appearance of the image forming apparatus 1. The post-processing unit 30 is attached to the upper part of the apparatus main body 10. The image forming apparatus 1 has a sheet cassette 8 at the bottom, an openable and closable tray 20 on the right side surface, and a first discharge tray 13 on the top surface. First, the internal configuration of the device main body 10 will be described. As shown in Fig. 1, the device main body 10 includes a sheet cassette 8 as a sheet storage section for storing sheets P as recording media, an image forming unit 1e as an image forming means, a first fixing device 6 as a fixing means, and a housing 19 for accommodating these. The device main body 10 has a printing function for forming a toner image on a sheet P fed from the sheet cassette 8 by the image forming unit 1e, and creating a printed matter by performing a fixing process by the first fixing device 6.
[0054] The sheet cassette 8 is inserted into the housing 19 at the bottom of the device main body 10 so as to be removable, and stores a large number of sheets P. The sheets P stored in the sheet cassette 8 are fed from the sheet cassette 8 by a feeding member such as a feeding roller, and are separated one by one by a pair of separation rollers and then transported by a transport roller 8a. It is also possible to feed sheets set in an open tray 20 (FIG. 5) one by one.
[0055] The image forming unit 1e includes four process cartridges 7n, 7y, 7m, and 7c, and a It is a tandem type electrophotographic unit equipped with a scanner unit 2 and a transfer unit 3. A process cartridge is a replaceable unit that integrates a plurality of parts that are responsible for an image forming process. The apparatus main body 10 is provided with a cartridge support part 9 supported by a housing 19, and the process cartridges 7n, 7y, 7m, 7c are detachably mounted in mounting parts 9n, 9y, 9m, 9c provided on the cartridge support part 9. The cartridge support part 9 may be a tray member that can be pulled out from the housing 19.
[0056] Each of the process cartridges 7n, 7y, 7m, and 7c has a substantially common configuration except for the type of powder contained in the four powder containers 104n, 104y, 104m, and 104c. That is, each of the process cartridges 7n, 7y, 7m, and 7c includes a photosensitive drum 101 as an image carrier, a charging roller 102 as a charger, a powder container 104n, 104y, 104m, and 104c that contains the powder, and a developing roller 105 that performs development using the powder.
[0057] Of the four powder containers, the three powder containers 104y, 104m, and 104c on the right side in the drawing contain yellow, magenta, and cyan printing toners Ty, Tm, and Tc, respectively, as toners (first powders) for forming a visible image on the sheet P. In contrast, the powder container 104n on the leftmost side in the drawing contains powder adhesive Tn, which is a powder (second powder) for performing an adhesion process after printing. The powder containers 104y, 104m, and 104c are all examples of a first container that contains printing toner, and the powder container 104n is an example of a second container that contains powder adhesive. The process cartridges 7y, 7m, and 7c are all examples of a first process unit that forms a toner image using printing toner, and the process cartridge 7n is an example of a second process unit that forms an image of powder adhesive in a predetermined application pattern.
[0058] When printing black images such as text, the process black is produced by superimposing yellow (Ty), magenta (Tm), and cyan (Tc) toners. However, for example, a fifth process cartridge using black printing toner may be added to the image forming unit 1e so that black images can be produced using black printing toner. However, the present invention is not limited to this, and the type and number of printing toners can be changed depending on the application of the image forming device 1. The scanner unit 2 is disposed below the process cartridges 7n, 7y, 7m, and 7c and above the sheet cassette 8. The scanner unit 2 is an exposure unit that irradiates the photosensitive drum 101 of each of the process cartridges 7n, 7y, 7m, and 7c with laser light G to write an electrostatic latent image thereon.
[0059] The transfer unit 3 includes a transfer belt 3a as an intermediate transfer body (secondary image carrier). The transfer belt 3a is a belt member wound around a secondary transfer inner roller 3b and a tension roller 3c, and its outer circumferential surface faces the photosensitive drums 101 of the process cartridges 7n, 7y, 7m, and 7c. On the inner circumferential side of the transfer belt 3a, a primary transfer roller 4 is disposed at a position corresponding to each photosensitive drum 101. In addition, a secondary transfer roller 5 as a transfer means is disposed at a position facing the secondary transfer inner roller 3b. A transfer nip 5n between the secondary transfer roller 5 and the transfer belt 3a is a transfer portion (secondary transfer portion) where a toner image is transferred from the transfer belt 3a to the sheet P.
[0060] The first fixing device 6 is disposed above the secondary transfer roller 5. The first fixing device 6 is a thermal fixing type fixing device having a heating roller 6a as a fixing member and a pressure roller 6b as a pressure member. The heating roller 6a is heated by a heating element such as a halogen lamp or a ceramic heater, or a heating mechanism of an induction heating type. The pressure roller 6b is pressed against the heating roller 6a by a biasing member such as a spring, and the nip portion (fixing nip) between the heating roller 6a and the pressure roller 6b is pressed against the heating roller 6a by a biasing member such as a spring. The pressure applying portion 6c applies pressure to the sheet P passing through the pressure applying portion 6n.
[0061] The housing 19 is provided with a discharge port 12 (first discharge port) which is an opening for discharging the sheet P from the device body 10, and a discharge unit 34 is disposed in the discharge port 12. The discharge unit 34 which is a discharge means uses a so-called triple roller set having a first discharge roller 34a, an intermediate roller 34b, and a second discharge roller 34c. In addition, a switching guide 33, which is a flap-shaped guide that switches the transport path of the sheet P, is provided between the first fixing device 6 and the discharge unit 34. The switching guide 33 is rotatable around a shaft portion 33a such that a tip end 33b reciprocates in the direction of the arrow c in the figure.
[0062] The device main body 10 is equipped with a mechanism for performing double-sided printing. A motor (not shown) is connected to the discharge unit 34, and the intermediate roller 34b can rotate in the forward and reverse directions. A double-sided conveying path 1r is provided as a conveying path connected in a loop to the main conveying path 1m. The sheet P having an image formed on its first side while passing through the main conveying path 1m is sandwiched and conveyed between the first discharge roller 34a and the intermediate roller 34b by the switching guide 33 which has rotated clockwise. After the trailing end of the sheet P in the traveling direction passes through the switching guide 33, the switching guide 33 rotates counterclockwise and the intermediate roller 34b rotates in the reverse direction, so that the sheet P is inverted and conveyed to the double-sided conveying path 1r. Then, while the sheet P passes through the main conveying path 1m again in an inverted state, an image is formed on the second side of the sheet P.
[0063] After double-sided printing, the sheet P is nipped and conveyed between the intermediate roller 34b and the second discharge roller 34c by the switching guide 33 which has rotated counterclockwise, and is discharged from the apparatus main body 10. In addition, the transport path passing through the transport roller 8a, the transfer nip 5n, and the fixing nip 6n in the apparatus body 10 constitutes a main transport path 1m along which an image is formed on the sheet P. When viewed from the main scanning direction during image formation (the width direction of the sheet perpendicular to the transport direction of the sheet transported along the main transport path 1m), the main transport path 1m extends from below to above, passing along one side in the horizontal direction with respect to the image forming unit 1e. In other words, the device body 10 is a so-called vertical transport type (vertical path type) printer in which the main transport path 1m extends in a substantially vertical direction. When viewed vertically, the first discharge tray 13, the intermediate path 15, and the sheet cassette 8 overlap one another. Therefore, the horizontal direction in which the sheet moves when the discharge unit 34 discharges the sheet P is opposite to the horizontal direction in which the sheet moves when the sheet P is fed from the sheet cassette 8.
[0064] 1 (when viewed in the main scanning direction during image formation), it is preferable that the horizontal occupancy area of the main body portion of the post-processing unit 30 excluding the second discharge tray 35 is within the occupancy area of the device main body 10. By accommodating the post-processing unit 30 in the space above the device main body 10 in this way, it becomes possible to install the image forming device 1 with adhesive printing function in an installation space approximately the same as that of a normal vertical pass printer.
[0065] (Gluing unit) 2, the post-processing unit 30 is attached to the upper part of the apparatus body 10. The post-processing unit 30 is a post-processing unit in which a folder 31 as a folding means and a second fixing device 32 as an adhesive means (second fixing means) are housed and integrated in a housing (second housing) 39. The post-processing unit 30 is provided with a first discharge tray 13 that rotatably holds a tray switching guide 13a, an intermediate path 15, and a second discharge tray 35. The first discharge tray 13 is provided on the upper surface of the post-processing unit 30 and is located on the upper surface (FIG. 1) of the entire image forming apparatus 1. The function of each part of the post-processing unit 30 will be described later.
[0066] The post-processing unit 30 is provided with a positioning portion (e.g., a convex shape that engages with a concave portion of the housing 19) for positioning the housing 39 relative to the housing 19 (first housing) of the device body 10. The post-processing unit 30 is also provided with a drive source and control unit separate from the device body 10, and is electrically connected to the device body 10 by coupling a connector 36 of the post-processing unit 30 with a connector 37 of the device body 10. This causes the post-processing unit 30 to enter a state in which it operates based on commands from the control unit provided in the device body 10, using power supplied via the device body 10.
[0067] (Process cartridge) As described above, each of the process cartridges 7n, 7y, 7m, and 7c has a substantially common configuration, except for the type of powder contained in each of the four powder containers 104n, 104y, 104m, and 104c. Here, the process cartridge 7n will be described as a representative. FIG. 7 is a schematic cross-sectional view of the process cartridge 7n. The process cartridge 7n is made up of a photosensitive unit CC including a photosensitive drum 101 and the like, and a developing unit DT including a developing roller 105 and the like.
[0068] A photosensitive drum 101 is rotatably attached to the photosensitive unit CC via a bearing (not shown). The photosensitive drum 101 is driven to rotate in a clockwise direction (arrow w) in the drawing in response to an image forming operation by receiving a driving force from a driving motor serving as a driving means (driving source) (not shown). Furthermore, a charging roller 102 for charging the photosensitive drum 101 and a cleaning member 103 are arranged around the photosensitive drum 101 in the photosensitive unit CC. The developing unit DT is provided with a developing roller 105 as a developer carrier that rotates in a counterclockwise direction (arrow d) in the figure in contact with the photosensitive drum 101. The developing roller 105 and the photosensitive drum 101 each rotate such that their surfaces move in the same direction at the opposing portion (contact portion).
[0069] The developing unit DT is also provided with a developer supply roller 106 (hereinafter simply referred to as the "supply roller") as a developer supply member that rotates in a clockwise direction (arrow e) in the figure. The supply roller 106 and the developing roller 105 each rotate so that their surfaces move in the same direction at the opposing portion (contact portion). The supply roller 106 supplies powder adhesive (printing toner in the case of the process cartridges 7y, 7m, and 7c) onto the developing roller 105, and also acts to peel off any powder adhesive (printing toner in the case of the process cartridges 7y, 7m, and 7c) remaining on the developing roller 105 from above the developing roller 105. In addition, the developing unit DT is provided with a developing blade 107 as a developer regulating member that regulates the layer thickness of the powder adhesive (printing toner in the case of the process cartridges 7y, 7m, and 7c) supplied onto the developing roller 105 by the supply roller 106.
[0070] The powder container 104n contains a powder adhesive (printing toner in the case of the process cartridges 7y, 7m, and 7c). A rotatably supported transport member 108 is provided in the powder container 104n. The stirring member 108 rotates in a clockwise direction (arrow f) in the drawing to stir the powder contained in the powder container 104n and transport the powder to a development chamber 109 in which the development roller 105 and the supply roller 106 are provided. Here, the photoconductor unit CC and the developing unit DT may be separately formed as a photoconductor unit cartridge and a developing unit cartridge, respectively, and may be configured to be detachable from the main body of the image forming apparatus. It is also possible to configure the device as a powder cartridge that has only the powder container 104 and the conveying member 108 and is detachable from the main body of the apparatus.
[0071] (Image formation operation) Next, the image forming operation performed by the image forming apparatus 1 will be described with reference to Figs. 1 to 7. Figs. 3(a) and 3(b) are diagrams showing the sheet transport path in the image forming apparatus 1. Figs. 4(a) to 4(f) are diagrams for explaining the contents of the folding process. Figs. 6(a) and 6(b) are diagrams showing examples of products output by the image forming apparatus 1. When data of an image to be printed and a command to execute printing are input to the image forming apparatus 1, the control unit of the image forming apparatus 1 starts a series of operations (image forming operations) of conveying a sheet P to form an image, and, if necessary, performing post-processing by the post-processing unit 30. In the image forming operation, first, as shown in Fig. 1, the sheets P are fed one by one from the sheet cassette 8 and conveyed toward the transfer nip 5n via the conveying roller 8a.
[0072] In parallel with the feeding of the sheet P, the process cartridges 7n, 7y, 7m, and 7c are sequentially driven, and the photosensitive drum 101 is rotated in the clockwise direction (arrow w) in the figure. At this time, the photosensitive drum 101 is uniformly charged on its surface by the charging roller 102. Further, the scanner unit 2 irradiates the photosensitive drum 101 of each of the process cartridges 7n, 7y, 7m, and 7c with laser light G modulated based on image data to form an electrostatic latent image on the surface of the photosensitive drum 101. Next, the electrostatic latent image on the photosensitive drum 101 is developed into a powder image by powder carried on the developing roller 105 of each of the process cartridges 7n, 7y, 7m, and 7c.
[0073] The powder adhesive layer formed on the photosensitive drum 101 by development with the powder adhesive Tn differs from a toner image (normal toner image) of printing toner for recording images such as figures and text on the sheet P in that it is not intended to transmit visual information. However, in the following description, in order to apply the powder adhesive Tn to the sheet P in a predetermined application pattern, the layer of powder adhesive Tn developed into a shape corresponding to the application pattern by the electrophotographic process will also be treated as one of the "toner images." The transfer belt 3a rotates in a counterclockwise direction (arrow v) in the figure. The toner images formed in the process cartridges 7n, 7y, 7m, and 7c are primarily transferred from the photosensitive drum 101 to the transfer belt 3a by an electric field formed between the photosensitive drum 101 and the primary transfer roller 4.
[0074] The toner image carried by the transfer belt 3a and reaching the transfer nip 5n is secondarily transferred onto the sheet P transported along the main transport path 1m by the electric field formed between the secondary transfer roller 5 and the secondary transfer inner roller 3b. Thereafter, the sheet P is conveyed to the first fixing device 6 and subjected to a thermal fixing process. That is, when the sheet P passes through the fixing nip 6n, the toner image on the sheet P is heated and pressurized, so that the printing toners Ty, Tm, Tc and the powder adhesive Tn melt and then solidify, thereby obtaining an image fixed on the sheet P.
[0075] Regardless of single-sided or double-sided printing, the sheet P discharged from the device body 10 is sandwiched between the intermediate roller 34b and the second discharge roller 34c, as shown in Figures 3(a) and 3(b), and is transported to the first path R1 or the second path R2 by the tray switching guide 13a. A first path R1 shown in FIG. 3(a) is a path along which the sheet P that has passed through the first fixing device 6 is discharged onto the first discharge tray 13 by the discharge unit 34 in a normal printing mode in which the post-processing unit 30 is not used. The second path R2 shown in Figure 3 (b) is a path along which, in the adhesive printing mode, the sheet P that has passed through the first fixing device 6 is discharged to the second discharge tray 35 via the discharge unit 34, the folder 31 and the second fixing device 32.
[0076] An intermediate path 15 is provided between the first fixing device 6 and the folding device 31 in the second route R2. The intermediate path 15 is a sheet conveying path that passes through the upper surface (top surface) of the image forming apparatus 1. , and extends substantially parallel to the first discharge tray 13 below the first discharge tray 13. The intermediate path 15 and the first discharge tray 13 are inclined vertically upward toward the folder 31 with respect to the horizontal direction. Therefore, the entrance of the folder 31 (the guide roller pair (31c, 31d) described below) is located vertically above the exit of the device main body 10 (the nip between the intermediate roller 34b and the second discharge tray 34c). The folder 31 has four rollers, namely, a first guide roller 31c, a second guide roller 31d, a first folding roller 31a, and a second folding roller 31b, and a lead-in portion 31e. The first guide roller 31c and the second guide roller 31d are a pair of guide rollers that sandwich and transport the sheet P received from a transport path (intermediate path 15 in this embodiment) on the upstream side of the folder 31. The first folding roller 31a and the second folding roller 31b are a pair of folding rollers that feed the sheet P while folding it.
[0077] Note that the distance M (FIG. 1) between the second discharge roller 34c and the first guide roller 31c in the sheet transport direction along the second path R2 is configured to be shorter than the overall length L (FIG. 4(a)) in the transport direction of the sheet P before folding. In other words, the distance M between the second discharge roller 34c and the first guide roller 31c determines the lower limit of the length in the transport direction of the sheet that can be processed by the post-processing unit 30. With this configuration, the sheet P is smoothly delivered from the discharge unit 34 to the pair of guide rollers.
[0078] The folding process by folder 31 will be described with reference to Figures 4(a) to 4(f). When performing the folding process, first guide roller 31c and first folding roller 31a rotate clockwise in the figure, and second guide roller 31d and second folding roller 31b rotate counterclockwise in the figure. First, the leading edge q of the sheet P sent out from the discharge unit 34 is pulled into the pair of guide rollers (31c, 31d) as shown in Fig. 4(a). As shown in Fig. 4(b), the leading edge q of the sheet P is guided downward by the guide wall 31f, contacts the first folding roller 31a, is pulled into the mutually opposing first folding roller 31a and second guide roller 31d, and abuts against the wall 31g of the pull-in portion 31e.
[0079] As the sheet P is pulled in by the guide roller pair (31c, 31d), the leading edge q slides against the wall 31g and advances toward the back of the pull-in section 31e. Eventually, the leading edge q hits the end 31h of the pull-in section 31e as shown in Fig. 4(c). The pull-in section 31e forms a space below the intermediate path 15 and extending substantially parallel to the intermediate path 15. At the stage shown in Fig. 4(c), the sheet P is wrapped around the second guide roller 31d and bent into a U-shape. When the sheet P is further drawn in by the guide roller pair (31c, 31d) from the state shown in Fig. 4(c), bending begins to occur at the middle portion r as shown in Fig. 4(d). Eventually, as shown in Fig. 4(e), the middle portion r comes into contact with the second folding roller 31b, and the sheet P is drawn into the nip portion of the folding roller pair (31a, 31b) by the frictional force received from the second folding roller 31b. Then, as shown in Fig. 4(f), the sheet P is folded with the middle portion r as the crease, and is discharged by the folding roller pair (31a, 31b) with the middle portion r at the front.
[0080] Here, the depth N of the retraction portion 31e (FIG. 4(e)), i.e., the distance from the nip portion of the pair of folding rollers (31a, 31b) to the end portion 31h of the retraction portion 31e, is set to half the total length L of the sheet P. This enables the folder 31 to fold the sheet P in half (center folding). Note that by changing the depth N of the retraction portion 31e, the position of the fold can be changed as desired. The folder 31 described above is an example of a folding means, and a folding mechanism may be used, for example, by pressing a blade against the sheet P and forcing it into a nip between a pair of rollers to form a crease. In addition, the folding process is not limited to folding in half, and a folding mechanism that performs, for example, a Z-fold or a triple fold may be used. In addition, the folding device 31 is composed of a rotating roller and a fixed drawing part 31e. The drive mechanism can be simplified compared to a folding mechanism that uses a reciprocating blade. In addition, the folder 31 only needs to be provided with a retraction section 31e having a depth N that is half the sheet length, in addition to the four rollers, so the post-processing unit 30 can be made compact.
[0081] The sheet P that has passed through the folder 31 is conveyed to the second fixing device 32 as shown in Fig. 3(b). The second fixing device 32 has a thermal fixing type configuration similar to the first fixing device 6. That is, the second fixing device 32 has a heating roller 32b as a heating member and a pressure roller 32a as a pressure member. The heating roller 32b is heated by a heating element such as a halogen lamp or a ceramic heater, or a heating mechanism of an induction heating type. The pressure roller 32a is pressed against the heating roller 32b by a biasing member such as a spring, and generates a pressure force for applying pressure to the sheet P passing through a nip portion (adhesion nip) between the heating roller 32b and the pressure roller 32a.
[0082] The sheet P folded by the folder 31 is subjected to a bonding process (a second thermal fixing to the image surface to which the powder adhesive Tn has been applied) by the second fixer 32, so that the sheet P is bonded in the folded state. That is, when the sheet P passes through the bonding nip, the powder adhesive Tn on the sheet P is heated and remelted, and is then pressurized, so that the powder adhesive Tn adheres to the opposing surface (the surface opposing the image surface of the sheet P to which the toner image of the powder adhesive Tn has been transferred in the folded state). Then, the powder adhesive Tn cools and hardens, so that the image surface and the opposing surface of the sheet P are bonded (bonded) together using the powder adhesive Tn as an adhesive.
[0083] The sheet P that has been subjected to the adhesion process by the second fixing device 32 is discharged to the left side in the figure from a discharge outlet 32c (second discharge outlet) provided in a housing 39 of the post-processing unit 30, as shown in Fig. 3(b). Then, the sheet P is stored in a second discharge tray 35 (see Fig. 1) provided on the left side surface of the apparatus main body 10. This completes the image formation operation when the sheet P is transported along the second path R2.
[0084] It is possible to change the bonding locations of the folded sheet P by changing the application pattern of the powder adhesive Tn on the sheet P. Figures 6(a) and 6(b) show examples of deliverables (output products of the image forming apparatus) with different application patterns of the powder adhesive Tn. Fig. 6(a) is an example of a deliverable (semi-adhesive deliverable) intended to be opened by the recipient. In the case of a pay slip 51 in Fig. 6(a), powder adhesive Tn is applied to the entire circumference 51a of the outer periphery on one side of a sheet P, and the sheet is folded and adhered at a central crease 51b. Fig. 6(b) shows a bag (medicine bag) as an example of a product (fully bonded product) that is not intended to be opened. In this case, powder adhesive Tn is applied to a U-shaped area 52a so that three sides, including crease 52b, of the folded sheet P are joined. Although no image is formed on the inside of the bag in Fig. 6(b), an image can be formed if necessary.
[0085] 6(a) and 6(b), the image forming apparatus 1 can output any of the products exemplified in Fig. 6(a) and 6(b) in one stop without preparing preprinted paper. That is, in parallel with the operation of recording an image on one or both sides of the sheet P using printing toner, it is possible to apply the powder adhesive Tn in a predetermined application pattern and output a product in a state in which the sheet has been subjected to folding and adhesive processing. 6(a) and 6(b), one side of the sheet P used as the base paper becomes the outside of the product, and the other side becomes the inside of the product. Therefore, in the image forming operation for the first side in double-sided printing, an image for the outside surface is formed with printing toner, and in the image forming operation for the second side, an image for the inside surface is formed with printing toner and powder adhesive Tn is applied in a predetermined application pattern.
[0086] The image recorded by the image forming device 1 using printing toner can include the format (unchanging portion) when preprinted paper is used, and variable portions such as personal information. Therefore, as described above, it is possible to output a product that is bonded by a gluing process from base paper such as blank paper that is not preprinted paper. However, the image forming device 1 can also be used for purposes in which preprinted paper is used as a recording medium and printing and gluing processes for variable portions are performed.
[0087] (Method of manufacturing adhesive (finished product)) A method for producing an adhesive product in which at least one piece of paper is bonded to the adhesive using the electrophotographic developer set, comprising the steps of: In the adhesive article, when a surface of the paper on which the adhesive portion exists is designated as surface A, the adhesive article has an image portion formed by the toner on at least one surface A, The method for producing the bonded product includes the following steps (A) or (B): (A) a step of forming an image portion and an adhesive portion by developing an image portion using the toner and an adhesive portion using the powder adhesive on at least one of the surfaces of the paper, which will become the surface A, and fixing the image portion and the adhesive portion by heating; (B) a step of forming an adhesive portion by developing the adhesive portion by the powder adhesive on one side of the surface of the paper that will become surface A and fixing the adhesive portion by heating, and a step of forming an image portion by developing an image portion by the toner on at least the other side of the paper that will become surface A and fixing the image portion by heating; The method for producing the adhesive product includes the steps of: After the image area and the adhesive area are formed, the paper is stacked so as to sandwich the formed adhesive area, and heated to melt the adhesive area to bond the papers together, thereby obtaining the bonded product.
[0088] The bonded product may be in the form of a single piece of paper that is folded and bonded together via an adhesive joint, or in the form of two pieces of paper that are bonded together via an adhesive joint. The bonded product may have, for example, a bag-like or tubular shape. When papers are bonded together via an adhesive joint, there will be two surfaces A in the bonded object where the adhesive joint is present, and the adhesive joint made of powder adhesive need only be formed on at least one of the two surfaces.
[0089] For example, as in step (A), an image area and an adhesive area are formed on at least one side of the surface that will become surface A of the paper. Also, as in step (B), an adhesive area is formed on one side of the surface that will become surface A of the paper, and an image area is formed on the other side. When manufacturing an adhesive product using a single sheet of paper, the toner image and the powder adhesive may be formed on at least one side of the paper, and the image may or may not be formed on the other side of the paper.
[0090] When two sheets of paper are bonded together to produce a bonded product, in step (A), an image area and an adhesive area are formed on one of the sheets, which will become surface A. An image area or an adhesive area may or may not be formed on the other sheet. Furthermore, when two sheets of paper are bonded together to produce a bonded product, in step (B) an adhesive portion is formed on the surface that will become side A of one of the sheets, and an image portion is formed on the surface that will become side A of the other sheet.
[0091] The formation of the image portion and the formation of the adhesive portion may be performed in either order, or both may be performed simultaneously. The development and fixation of the image portion and the development and fixation of the adhesive portion may be performed, for example, by the above-mentioned image forming apparatus. Also, a known electrophotographic method may be adopted.
[0092] After forming the image area and adhesive area, if it is one piece of paper, the paper is folded to sandwich the adhesive area, and if it is two pieces of paper, they are stacked and the adhesive area is sandwiched. Then, the adhesive area is melted by heating to bond the papers together, and a bonded product (delivered product) is obtained. This type of bonding process is carried out, for example, in the image forming apparatus described above. This can be done using a sheet processing device or a sheet handling device.
[0093] The measurement methods for each physical property are described below. <Identification of the molecular structures of thermoplastic resin and wax, measurement method for the content Na of wax contained in toner and the content Nb of wax contained in powder adhesive, and the content of thermoplastic resin contained in powder adhesive or toner> A pyrolysis gas chromatography mass spectrometer (hereinafter referred to as pyrolysis GC / MS) and NMR are used to identify the molecular structures of the thermoplastic resin and wax, and to measure the wax content Na in the toner and the wax content Nb in the powder adhesive. Pyrolysis GC / MS can determine the constituent monomers of the entire resin sample and calculate the peak area of each monomer, but quantification requires normalization of peak intensity using a reference sample of known concentration.On the other hand, NMR makes it possible to determine and quantify the constituent monomers without using a sample of known concentration. Therefore, depending on the circumstances, the constituent monomers are determined by comparing the spectra obtained by both NMR and pyrolysis GC / MS.
[0094] Specifically, when the amount of resin components that are insoluble in deuterated chloroform, which is the extraction solvent used in NMR measurement, is less than 5.0% by mass, quantification is performed by NMR measurement. On the other hand, when 5.0% by mass or more of resin components that are insoluble in deuterated chloroform, which is the extraction solvent used in NMR measurement, are present, both NMR and pyrolysis GC / MS measurements are performed on the deuterated chloroform soluble fraction, and pyrolysis GC / MS measurement is performed on the deuterated chloroform insoluble fraction. In this case, first, NMR measurement is performed on the deuterated chloroform soluble fraction to determine and quantify the constituent monomers (quantitative result 1). Next, pyrolysis GC / MS measurement is performed on the deuterated chloroform soluble fraction to determine the peak area of the peak attributable to each constituent monomer. Using quantitative result 1 obtained by NMR measurement, the relationship between the amount of each constituent monomer and the pyrolysis GC / MS peak area is determined. Next, the deuterated chloroform insoluble fraction is subjected to pyrolysis GC / MS measurement to determine the peak area of the peak attributable to each constituent monomer. From the relationship between the amount of each constituent monomer obtained by the measurement of the deuterated chloroform soluble fraction and the peak area of the pyrolysis GC / MS, the constituent monomers in the deuterated chloroform insoluble fraction are quantified (quantitative result 2). Then, the quantitative result 1 and the quantitative result 2 are combined to obtain the final quantitative result of each constituent monomer. Specifically, the following operations are carried out.
[0095] (1) 50 mg of toner or powder adhesive is precisely weighed into an 8 mL glass sample bottle, 1 mL of deuterated chloroform is added, the bottle is capped, and the bottle is dispersed and dissolved for 1 hour using an ultrasonic disperser. The bottle is then filtered through a 0.4 μm membrane filter, and the filtrate is collected. At this time, the deuterated chloroform insoluble matter remains on the membrane filter. (2) Regarding the filtrate: 1 H-NMR measurement is performed, and the spectrum is assigned to each constituent monomer in the resin to obtain a quantitative value. (3) If analysis of deuterium chloroform insoluble matter is required, perform pyrolysis GC / MS analysis. If necessary, perform derivatization such as methylation.
[0096] (NMR measurement conditions) Bruker AVANCE 500 manufactured by Bruker Biospin Co., Ltd. Measurement nuclei: 1 H Measurement frequency: 500.1MHz Number of times: 16 Measurement temperature: room temperature
[0097] (Measurement conditions for pyrolysis GC / MS) Pyrolysis equipment: Japan Analytical Industry Co., Ltd. TPS-700 Thermal decomposition temperature: Optimum value between 400℃ and 600℃ GC / MS equipment: ISQ manufactured by Thermo Fisher Scientific Co., Ltd. Column: "HP5-MS" (Agilent / 19091S-433), length 30 m, inner diameter 0.25 mm, film thickness 0.25 μm GC / MS conditions Filler requirements: InletTemp:250℃ Split Flow: 50mL / min GC heating conditions: 40℃ (5min) → 10℃ / min (300℃) → 300℃ (20min)
[0098] <How to calculate the ester group concentration of wax> In this disclosure, the ester group concentration is defined as the number of ester groups contained per molecular weight (mmol / g). The ester group concentrations Ea and Eb of the wax are calculated from the molecular structure of the wax obtained by the above measurement, and the content of the wax contained in the toner and the powder adhesive. The molecular weight obtained from the molecular structure of the wax contained in the toner is na (g / mol), and the number of ester groups contained in one molecule of the wax contained in the toner is aa and When I did that, Ea = 1000 x aa / na (mmol / g) The ester group concentration Ea of the wax contained in the toner is calculated as follows. Similarly, the molecular weight obtained from the molecular structure of the wax contained in the powder adhesive is nb (g / mol), and the number of ester groups contained in one molecule of the wax contained in the powder adhesive is ab and When I did that, Eb = 1000 × ab / nb (mmol / g) The ester group concentration Eb of the wax contained in the powder adhesive is calculated as Furthermore, when a plurality of waxes are contained, Ea and Eb are calculated as average values multiplied by the content (mass%) as a coefficient as follows. For example, if a toner contains three types of wax, Wax 1 to 3, and the ester group concentration of Wax 1 is Ea1 and the content is Na1, the ester group concentration of Wax 2 is Ea2 and the content is Na2, and the ester group concentration of Wax 3 is Ea3 and the content is Na3, then Ea is calculated using the following formula. Ea=Ea1×(Na1 / (Na1+Na2+Na3))+Ea2×(Na2 / (Na1+Na2+Na3))+Ea3×(Na3 / (Na1+Na2+Na3)) In this case, there is no limit to the number of waxes that may be used at the same time. Eb is also calculated in the same manner as above.
[0099] <How to calculate the ester group concentration of thermoplastic resin> When the ester group concentration of the thermoplastic resin is taken as Ec, it is calculated from the molecular structure and mass ratio of the constituent monomers of the thermoplastic resin obtained by the above measurement. When the molecular weight of the monomer from which the structure constituting the thermoplastic resin is derived is nc (g / mol) and the number of ester groups contained in one molecule of the monomer is ac (mol), Ec = 1000 × ac / nc (mmol / g) The ester group concentration of the thermoplastic resin is defined as Ec. Furthermore, when the thermoplastic resin is composed of a plurality of monomers, the ester group concentration of each monomer is determined in the same manner. From the ester group concentration of each monomer thus determined and the content (mass%) of the structure derived from each monomer in the thermoplastic resin, the average value is multiplied by the content as a coefficient as follows: For example, in the case of a thermoplastic resin composed of three types of monomers, monomers 1 to 3, the ester group concentration of monomer 1 is Ec1, the constituent ratio (mass % in the thermoplastic resin) is Nc1, the ester group concentration of monomer 2 is Ec2, the constituent ratio is Nc2, and the ester group concentration of monomer 3 is Ec3, the constituent ratio is Nc3, then Ec is calculated using the following formula. Ec=Ec1×(Nc1 / (Nc1+Nc2+Nc3))+Ec2×(Nc2 / (Nc1+Nc2+Nc3))+Ec3×(Nc3 / (Nc1+Nc2+Nc3)) In this case, there is no limit to the number of monomers that may be used simultaneously. When the thermoplastic resin contains a plurality of resins, the concentration is calculated as an average value multiplied by the content (mass%) as a coefficient in the same manner as in the calculation example of the ester group concentration of the wax.
[0100] <Method of measuring glass transition temperature (Tg)> The glass transition temperature (Tg) of thermoplastic resins and the like is measured using a differential scanning calorimeter "Q1000" (manufactured by TA Instruments). The melting points of indium and zinc are used for temperature correction of the detector, and the heat of fusion of indium is used for heat correction. Specifically, 1 mg of sample is weighed out and placed in an aluminum pan, and an empty aluminum pan is used as a reference. Using the modulation measurement mode, measurements are performed in the range of 0°C to 100°C with a temperature rise rate of 1°C / min and temperature modulation conditions of ±0.6°C / 60 seconds. Since the specific heat change is obtained during the temperature rise process, the intersection point between the line midway between the baseline before and after the specific heat change and the differential heat curve is taken as the glass transition temperature (Tg).
[0101] <Method for measuring weight-average particle size (D4) of powder adhesives and toners> The weight average particle diameter (D4) is calculated as follows. The measurement device used is a precision particle size distribution measurement device using the pore electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.). The measurement is performed with an effective measurement channel count of 25,000. The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of 1.0%, for example, "ISOTON II" (manufactured by Beckman Coulter, Inc.). Before performing measurements and analysis, the dedicated software is set up as follows. In the "Change standard measurement method (SOMME)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard particle 10.0 μm" (Beckman Coulter, Inc.). Press the "Threshold / Noise level measurement button" to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement." In the "Pulse to particle size conversion setting" screen of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range from 2 μm to 60 μm.
[0102] The specific measurement method is as follows. (1) Pour 200.0 mL of the electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "Aperture tube flush" function of the dedicated software to remove dirt and air bubbles from inside the aperture tube. (2) Place 30.0 mL of the electrolyte solution in a 100 mL flat-bottom glass beaker. Add 0.3 mL of a solution of "Contaminon N" (a 10% aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted 3 times by mass with ion-exchanged water as a dispersant. (3) Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetra150" (manufactured by Nikkaki Bios Co., Ltd.) that has two built-in oscillators with an oscillation frequency of 50 kHz and a phase shift of 180 degrees and an electrical output of 120 W. Place 3.3 L of ion-exchanged water in the ultrasonic disperser's water tank and add 2.0 mL of Contaminon N to this tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, 10 mg of the measurement sample is added little by little to the electrolyte solution and dispersed. Then, the ultrasonic dispersion process is continued for another 60 seconds. During the ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, the electrolyte solution (5) in which the toner particles are dispersed is dropped into the round-bottom beaker (1) placed in the sample stand, and the measurement concentration is adjusted to 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) Analyze the measurement data using the dedicated software that comes with the device to calculate the weight-average particle size (D4). Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight-average particle size (D4).
[0103] <Method of measuring molecular weight distribution and peak molecular weight> The molecular weight distribution and the peak molecular weight are measured by gel permeation chromatography (GPC) as follows. First, the measurement sample is dissolved in tetrahydrofuran (THF). The obtained solution is then filtered through a solvent-resistant membrane filter "Myshoridisc" (manufactured by Tosoh Corporation) with a pore size of 0.2 μm to obtain a sample solution. The sample solution is adjusted so that the concentration of components soluble in THF is 0.8 mass%. This sample solution is used to perform measurements under the following conditions. Equipment: High-speed GPC equipment "HLC-8220GPC" [Tosoh Corporation] Column: 2 columns of LF-604 [Showa Denko Co., Ltd.] Eluent:THF Flow rate: 0.6ml / min Oven temperature: 40℃ Sample injection volume: 0.020 ml In calculating the molecular weight of the sample, a molecular weight calibration curve prepared using a standard polystyrene resin (for example, trade names "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500" manufactured by Tosoh Corporation) is used. From the obtained molecular weight distribution, the largest peak is taken as the main peak, and the molecular weight value of this peak is taken as the peak molecular weight. EXAMPLES
[0104] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples, the parts are by weight unless otherwise specified.
[0105] The compositions and physical properties of the waxes used in the examples and comparative examples are shown in Table 1.
[0106] [Table 1] In the table, HNP-9 is a hydrocarbon wax (peak carbon number 33) manufactured by Nippon Seiro.
[0107] <Production example of polyester resin> A molar ratio of 1.00 mol of terephthalic acid, 0.65 mol of a 2 mol propylene oxide adduct of bisphenol A, and 0.35 mol of ethylene glycol was added to a reaction vessel equipped with a stirrer, a thermometer, a nitrogen inlet tube, a dehydration tube, and a pressure reducing device, and the mixture was heated to a temperature of 130° C. with stirring. Then, 0.52 parts of tin di(2-ethylhexanoate) was added as an esterification catalyst relative to 100.00 parts of the monomer, and the mixture was heated to 200° C. and condensation polymerization was carried out until the desired molecular weight was reached. Further, 3.00 parts of trimellitic anhydride was added to 100.00 parts of the above monomer to obtain a polyester resin. The resulting polyester resin had a peak molecular weight of 12,000, a glass transition temperature (Tg) of 75° C., an acid value of 8.2 mg KOH / g, and an ester group concentration of 5.41 mmol / g.
[0108] <Production example of powder adhesive 1> Styrene: 75.0 parts n-Butyl acrylate: 25.0 parts Polyester resin: 4.0 parts Wax 1: 14.0 parts Wax 7: 2.0 parts Divinylbenzene: 0.5 parts The mixture of the above materials was kept at 60° C. and stirred at 500 rpm using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) to dissolve uniformly, thereby preparing a polymerizable monomer composition. Meanwhile, 0.10 mol / L-Na was added to a vessel equipped with a high-speed stirring device Clearmix (M Technique Co., Ltd.). 3 PO 4 850.0 parts of the aqueous solution and 8.0 parts of 10% hydrochloric acid were added, the rotation speed was adjusted to 15,000 rpm, and the mixture was heated to 70°C. 2 127.5 parts of the aqueous solution was added to prepare an aqueous medium containing a calcium phosphate compound. After the polymerizable monomer composition was added to the aqueous medium, 7.0 parts of t-butyl peroxypivalate, a polymerization initiator, was added, and the mixture was granulated for 10 minutes while maintaining a rotation speed of 15,000 rpm. After that, the high-speed agitator was replaced with a propeller agitator, and the mixture was stirred at 70° C. for 5 minutes while refluxing. After reacting for 2 hours, the liquid temperature was increased to 85° C. and the reaction was continued for another 2 hours. After the polymerization reaction was completed, the resulting slurry was cooled, and then hydrochloric acid was added to the slurry to adjust the pH to 1.4 and stirred for 1 hour to dissolve the calcium phosphate salt. The slurry was then washed with three times the amount of water, filtered, dried, and classified to obtain powder adhesive particles. Then, silica fine particles (number-average particle size of primary particles: 10 nm, BET specific surface area: 170 m) that had been hydrophobized using dimethyl silicone oil (20% by mass) were added as an external additive to 100.0 parts of the powder adhesive particles. 2 The mixture was mixed for 15 minutes at 3000 rpm using a Mitsui Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) to obtain powder adhesive 1.
[0109] <Production examples of powder adhesives 2-13, 15-18> As shown in Table 2, powder adhesives 2 to 13 and 15 to 18 were obtained in the same manner as in the production example of powder adhesive 1, except that the type and amount of wax added were changed.
[0110] [Table 2] The EVA in the table is an ethylene-vinyl acetate copolymer resin (Ultrathene 685, manufactured by Tosoh).
[0111] <Production example of powder adhesive 14> Polyester resin: 100.0 parts Wax 1: 14.0 parts Wax 7: 2.0 parts The above materials were premixed in a Henschel mixer (manufactured by Nippon Coke Company), and then melt-kneaded using a twin-screw kneading extruder (manufactured by Ikegai Iron Works Co., Ltd.: PCM-30 type). The resulting kneaded product was cooled, coarsely pulverized in a hammer mill, and then pulverized in a mechanical pulverizer (Turbo Kogyo Co., Ltd.: T-250). The resulting finely pulverized powder was classified using a multi-division classifier utilizing the Coanda effect to obtain powder adhesive particles with a weight average particle size (D4) of 5.8 μm. Then, silica fine particles (number-average particle size of primary particles: 10 nm, BET specific surface area: 170 m) that had been hydrophobized using dimethyl silicone oil (20% by mass) were added as an external additive to 100.0 parts of the powder adhesive particles. 2 The mixture was mixed at 3,000 rpm for 15 minutes using a Mitsui Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) to obtain Powder Adhesive 14.
[0112] <Production example of powder adhesive 19> TopasTM (Tikona, cyclic polyolefin resin) 39.8 parts TopasTB (Tikona, cyclic polyolefin resin) 18.5 parts 30.0 parts of Alcon P-100 (Arakawa Chemical Co., Ltd., alicyclic saturated hydrocarbon resin) 6.5 parts QuintacSL-125 (Zeon Corporation, thermoplastic elastomer) The above materials were premixed in a Henschel mixer (manufactured by Nippon Coke Company), and then melt-kneaded using a twin-screw kneading extruder (manufactured by Ikegai Iron Works Co., Ltd.: PCM-30 type). The resulting kneaded product was cooled, coarsely pulverized in a hammer mill, and then pulverized in a mechanical pulverizer (Turbo Kogyo Co., Ltd.: T-250). The resulting finely pulverized powder was classified using a multi-division classifier utilizing the Coanda effect to obtain powder adhesive particles with a weight average particle size (D4) of 9.0 μm. Then, silica fine particles (number-average particle size of primary particles: 10 nm, BET specific surface area: 170 m) that had been hydrophobized using dimethyl silicone oil (20% by mass) were added as an external additive to 100.0 parts of the powder adhesive particles. 2 The mixture was mixed at 3,000 rpm for 15 minutes using a Mitsui Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) to obtain powder adhesive 19.
[0113] <Production example of powder adhesive 20> (Preparation of Core Resin Particle Dispersion) Styrene: 450 parts 2-Ethylhexyl acrylate: 135 parts Acrylic acid: 12 parts Dodecanethiol: 9 parts The above components were mixed and dissolved to prepare a solution. On the other hand, 10 parts of an anionic surfactant (DOWFAX2A1, manufactured by The Dow Chemical Company) was dissolved in 250 parts of ion-exchanged water, and the above solution was added thereto, and the mixture was dispersed and emulsified in a flask (monomer emulsion A). Furthermore, 1 part of anionic surfactant (DOWFAX2A1, manufactured by Dow Chemical Company) was dissolved in 555 parts of ion-exchanged water and charged into the polymerization flask. A reflux condenser was attached to the polymerization flask, and while injecting nitrogen, the polymerization flask was heated to 75° C. in a water bath with slow stirring and maintained at that temperature. 9 parts of ammonium persulfate was dissolved in 43 parts of ion-exchanged water and added dropwise to the polymerization flask via a metering pump over 20 minutes, and then the monomer emulsion A was added dropwise via a metering pump over 200 minutes. Thereafter, the polymerization flask was kept at 75°C for 3 hours while continuing to stir, and the first stage of polymerization was completed. As a result, a core resin particle dispersion precursor having a volume average particle size of 190 nm, a glass transition temperature of 53°C, and a weight average molecular weight of 33,000 was obtained. Next, after the temperature was lowered to room temperature, 600 parts of 2-ethylhexyl acrylate and 850 parts of ion-exchanged water were added to the polymerization flask and slowly stirred for 2 hours. Then, the temperature was raised to 70°C while continuing to stir, and 4.5 parts of ammonium persulfate and 110 parts of ion-exchanged water were dropped over 20 minutes via a metering pump. Then, the mixture was maintained for 3 hours while continuing to stir to complete the polymerization. Through the above steps, a core resin particle dispersion liquid having a volume average particle size of 260 nm, a weight average molecular weight of 200,000, and a solid content of 33 mass % was obtained.
[0114] (Preparation of Shell Resin Particle Dispersion) Styrene: 450 parts n-Butyl acrylate: 135 parts Allyl methacrylate: 18 parts Acrylic acid: 12 parts Dodecanethiol: 9 parts The above components were mixed and dissolved to prepare a solution. On the other hand, 10 parts of an anionic surfactant (DOWFAX2A1, manufactured by The Dow Chemical Company) was dissolved in 250 parts of ion-exchanged water, and the above solution was added thereto, and the mixture was dispersed and emulsified in a flask (monomer emulsion A). Furthermore, 1 part of anionic surfactant (DOWFAX2A1, manufactured by Dow Chemical Company) was dissolved in 555 parts of ion-exchanged water and charged into the polymerization flask. A reflux condenser was attached to the polymerization flask, and while injecting nitrogen, the polymerization flask was heated to 75° C. in a water bath with slow stirring and maintained at that temperature. 9 parts of ammonium persulfate was dissolved in 43 parts of ion-exchanged water and added dropwise to the polymerization flask via a metering pump over 20 minutes, and then the monomer emulsion A was added dropwise via a metering pump over 200 minutes. Thereafter, the polymerization flask was kept at 75° C. for 3 hours while continuing stirring to complete the first stage polymerization, thereby obtaining a shell resin particle dispersion having a volume average particle size of 190 nm, a glass transition temperature of 53° C., a weight average molecular weight of 33,000, and a solid content of 42% by mass.
[0115] (Powder adhesive manufacturing) Core resin particle dispersion: 504 parts Ion-exchanged water: 710 parts Anionic surfactant: 1 part (Dow Chemical Company, Dowfax2A1) The above components as the core-forming material were placed in a 3-liter reaction vessel equipped with a thermometer, pH meter, and stirrer, and 1.0% nitric acid was added at 25°C to adjust the pH to 3.0. The mixture was then dispersed at 5,000 rpm with a homogenizer (IKA Japan Co., Ltd.: Ultra Turrax T50) while adding 23 parts of the prepared aluminum sulfate aqueous solution, and dispersed for 6 minutes. Then, a stirrer and a mantle heater were placed in the reaction vessel, and the mixture was heated while being stirred. When the volume average particle size reached 5.0 μm, the temperature was maintained, and 170 parts of the shell resin particle dispersion liquid was added as the shell forming material. After maintaining the temperature for 30 minutes, the pH was adjusted to 9.0 using a 1% aqueous sodium hydroxide solution. Then, the temperature was raised to 90°C, and maintained at 98°C. After maintaining the temperature for 10.0 hours, the vessel was cooled to 30°C with cooling water. Then, the mixture was washed with water three times the amount of the slurry, filtered, dried, and classified to obtain powder adhesive particles having a weight average particle size (D4) of 5.9 μm. Then, silica fine particles (number-average particle size of primary particles: 10 nm, BET specific surface area: 170 m) that had been hydrophobized using dimethyl silicone oil (20% by mass) were added as an external additive to 100.0 parts of the powder adhesive particles. 2 The mixture was mixed at 3,000 rpm for 15 minutes using a Mitsui Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) to obtain powder adhesive 20.
[0116] The physical properties of the resulting powder adhesives 1 to 20 were measured using the methods described above. The results are shown in Table 3.
[0117] [Table 3]
[0118] <Toner 1 Manufacturing Example> Styrene: 60.0 parts Colorant: 6.5 parts (CI Pigment Blue 15:3, Dainichi Seika Chemicals Co., Ltd.) The above materials were placed in an attritor (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and further dispersed using zirconia particles having a diameter of 1.7 mm at 220 rpm for 5 hours to obtain a pigment dispersion liquid. Styrene: 15.0 parts n-Butyl acrylate: 25.0 parts Polyester resin: 4.0 parts Wax 8: 12.0 parts Divinylbenzene: 0.5 parts The above materials were mixed and added to the pigment dispersion liquid. The resulting mixture was kept at 60° C. and stirred at 500 rpm using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) to dissolve and disperse uniformly, thereby preparing a polymerizable monomer composition. Meanwhile, 0.10 mol / L-Na was added to a vessel equipped with a high-speed stirring device Clearmix (M Technique Co., Ltd.). 3 PO 4 850.0 parts of the aqueous solution and 8.0 parts of 10% hydrochloric acid were added, the rotation speed was adjusted to 15,000 rpm, and the mixture was heated to 70°C. 2 127.5 parts of the aqueous solution was added to prepare an aqueous medium containing a calcium phosphate compound. After the polymerizable monomer composition was added to the aqueous medium, 7.0 parts of t-butyl peroxypivalate, a polymerization initiator, was added, and the mixture was granulated for 10 minutes while maintaining a rotation speed of 15,000 rpm. After that, the high-speed agitator was replaced with a propeller agitator, and the mixture was reacted at 70°C for 5 hours under reflux, and then the liquid temperature was increased to 85°C and the mixture was reacted for another 2 hours. After the polymerization reaction was completed, the resulting slurry was cooled, and then hydrochloric acid was added to the slurry to adjust the pH to 1.4 and the slurry was stirred for 1 hour to dissolve the calcium phosphate salt.The slurry was then washed with three times the amount of water, filtered, dried, and classified to obtain toner particles. Thereafter, silica fine particles (number average particle diameter of primary particles: 10 nm, BET specific surface area: 170 m) that had been hydrophobized using dimethyl silicone oil (20% by mass) were added to 100.0 parts of the toner particles as an external additive. 2 The mixture was mixed for 15 minutes at 3000 rpm using a Mitsui Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) to obtain toner 1.
[0119] <Production Examples of Toners 2 to 11> As shown in Table 4, toners 2 to 11 were obtained in the same manner as in the production example of toner 1, except that the type and amount of wax added were changed.
[0120] [Table 4]
[0121] The physical properties of the obtained toners 1 to 11 were measured using the methods described above. The results are shown in Table 5.
[0122] [Table 5]
[0123] Developer sets were prepared using the obtained powder adhesives and toners in the combinations shown in Table 6. Developer sets 1 to 22 were used as examples, and developer sets 23 to 29 were used as comparative examples.
[0124] [Table 6]
[0125] The obtained developer sets 1 to 29 were subjected to performance evaluation according to the following method. The evaluations were all performed in a room temperature and humidity (25°C / 50% RH) environment, and the paper used was GFC-081 (81.0 g / m 2 ) (Canon Marketing Japan) was used. The results are shown in Table 7.
[0126] <Evaluation of adhesive strength and print transfer> (Preparation of sample images for evaluation) A commercially available Canon laser beam printer LBP712Ci was used to create the sample images for evaluation. The software was modified so that the printer could operate even if all cartridges were not set. The amount of powder adhesive and toner applied (mg / cm2) was also measured. 2 ) can be adjusted arbitrarily. The toner in the cyan cartridge of the LBP712Ci was removed, and 150 g of the toner of each developer set was refilled and set in the cyan station. The toner in the black cartridge was removed, and 150 g of the powder adhesive of each developer set was refilled and set in the black station. Using this printer, as shown in Figure 8, a powder adhesive was applied in an area of 4 cm with a margin of 8 cm at the tip, with a quantity of 0.5 mg / cm. 2 Print with a margin of 2 cm and apply 0.08 mg / cm2 of toner to an area of 4 cm. 2 (Image A). In addition, leave a margin of 8 cm at the tip of another piece of paper and apply powder adhesive to an area of 4 cm at a rate of 0.5 mg / cm. 2 (Image B). The obtained image A was cut to a width of 3 cm to obtain sample A. Similarly, image B was cut to obtain sample B.
[0127] (Sample images for evaluation) As shown in FIG. 9, Sample A and Sample B were placed facing each other with the image surfaces facing inward, and were laminated together by passing Sample A through the external fixing unit removed from the LBP712Ci with the side of Sample A facing up.
[0128] (Adhesive strength evaluation) A Tensilon universal testing machine RTG-1225 (manufactured by A&D Co., Ltd.) was used to evaluate the adhesive strength. A parallel clamping jaw was used as the jig, and the bonded sample was set as shown in Figure 10. The horizontal axis indicates the distance (mm) obtained when the sample image for evaluation was peeled off at a speed of 50 mm / min, and the vertical axis indicates the stress (N / cm 2 The maximum value in the graph is multiplied by 1 / 3 to obtain the stress per 1 cm of width, which is the adhesive strength (N / cm 2 The larger this value, the better the adhesive strength.
[0129] (Evaluation of print transfer) After peeling the sample as described above, the density of the toner transferred to the paper side that was not originally printed with toner was measured and used to evaluate the print transfer. A reflectometer (Tokyo Denshoku Co., Ltd.'s "REFLECTOMETER MODEL TC-6DS") was used to measure the density. The reflectance Dr (%) of the part with the transferred print and the reflectance Ds (%) of the white part of the paper were measured, and the reflectance was calculated using the following formula. Print transfer density (%) = Dr (%) - Ds (%) The smaller this value, the more effectively print transfer is suppressed.
[0130] <Durability evaluation> Using a printer equipped with the above toner and powder adhesive, 15,000 images with a print rate of 1% were printed. After printing, the cartridge filled with the powder adhesive was removed and disassembled, and the number of vertical streaks that appeared on the developing roller was confirmed using an optical microscope. The fewer the number of vertical streaks, the less likely the parts were to be contaminated and the better the durability.
[0131] [Table 7] [Explanation of symbols]
[0132] 1...image forming apparatus, 1e...image forming means (image forming unit), 1m...main transport path, 2...scanner unit, 3...transfer unit, 3a...transfer belt, 3b...secondary transfer inner roller, 3c...tension roller, 4...primary transfer roller, 5...transfer means (secondary transfer roller), 5n...transfer nip, 6...fixing means (first fixing device), 6a...heating roller, 6b...pressure roller, 6n...fixing nip, 7n...second process unit (process cartridge), 7y, 7m, 7c...first process unit (process cartridge), 8...sheet cassette, 8a...transport roller, 9...cartridge support section, 10...apparatus main body, 12...discharge port (first discharge port), 13...guide member (first discharge tray), 13...a tray switching guide, 15...intermediate path, 19...first housing, 20...openable tray, 30...sheet processing device (post-processing unit), 31...folding means (folder), 31a...first folding roller, 31b...second folding roller, 31c...first guide roller, 31d...second guide roller, 31e...pulling section, 31f...guide wall, 31g...wall, 31h...end section, 32...adhesive means (second fixing device), 33...switching guide, 33a...switching guide shaft section, 33b...switching guide tip, 34...discharge unit, 34a...first discharge roller, 34b...intermediate roller, 34c...second discharge roller, 35...second discharge tray, 36, 37...connector, 39...second housing, 51...adhesive postcard, 52...medicine bag, 51a...periphery of outer periphery, 51b, 52b...central fold, 52a...U-shaped area, 101...photosensitive drum, 102...charging roller, 103...cleaning member, 104n, 104y, 104m, 104c...powder container, 105...developing roller, 106...developer supply port roller, 107...developing blade, 108...agitating member, 109...developing chamber, P...sheet, R1...first path, R2...second path, Tn...powder adhesive, Ty, Tm, Tc...printing toner, CC...photoconductor unit, DT...developing unit, q...leading edge of sheet P, r...middle part, L...total length of sheet P, M...spacing, N...depth of retraction part
Claims
1. 1. An electrophotographic developer set comprising a toner containing a thermoplastic resin and a wax, and a powder adhesive containing a thermoplastic resin and a wax, When the amount of substance (mmol) of the ester group in 1 g of the wax contained in the toner is Ea (mmol / g), the content of the wax in the toner is Na (mass %), the amount of substance (mmol) of the ester group in 1 g of the wax contained in the powder adhesive is Eb (mmol / g), and the content of the wax in the powder adhesive is Nb (mass %), 0.00≦Ea≦2.45 2.50≦Eb≦3.60 0.80≦Nb / Na 13. An electrophotographic developer set comprising:
2. The Ea and the Eb are 0.50≦Eb−Ea≦3.40 2. The electrophotographic developer set according to claim 1, which satisfies the above formula:
3. 3. The electrophotographic developer set according to claim 1, wherein the wax contained in the powder adhesive contains at least one selected from the group consisting of ester waxes represented by the following formulas (1) and (2): (In formula (1), l represents a positive integer of 2 or more and 12 or less, and n and m each independently represent 1. In formula (2), p represents a positive integer of 2 or more and 10 or less, and q and r each independently represent a positive integer of 11 or more and 21 or less.
4. 4. The electrophotographic developer set according to claim 1, wherein the wax contained in the powder adhesive contains an ester wax represented by the following formula (3): (In formula (3), n and m each independently represent a positive integer of 14 or more and 20 or less.)
5. 5. The electrophotographic developer set according to claim 3, wherein a content Nb1 of the ester wax in the powder adhesive is 8.0% by mass or more and 20.0% by mass or less.
6. 6. The electrophotographic developer set according to claim 3, wherein the wax contained in the powder adhesive further contains a chain saturated hydrocarbon having a peak value of 20 or more and 70 or less carbon atoms.
7. 7. The electrophotographic developer set according to claim 1, wherein a content Nb of the wax in the powder adhesive is 8.0% by mass or more and 20.0% by mass or less.
8. 8. The electrophotographic developer set according to claim 1, wherein the content of the wax in the toner is from 2.0% by mass to 15.0% by mass.
9. 9. The electrophotographic developer set according to claim 1, wherein the wax contained in the toner comprises an ester compound of a monoalcohol having 18 to 24 carbon atoms and a monocarboxylic acid having 18 to 24 carbon atoms.
10. 10. The electrophotographic developer set according to claim 1, wherein the thermoplastic resin contained in the toner and the powder adhesive comprises at least one selected from the group consisting of a polyester resin and a styrene-acrylic resin.
11. A method for producing an adhesive product in which at least one paper is bonded via an adhesive portion, using the electrophotographic developer set according to any one of claims 1 to 10, comprising the steps of: In the adhesive article, when a surface of the paper on which the adhesive portion exists is designated as surface A, the adhesive article has an image portion formed by the toner on at least one surface A, The method for producing the bonded product includes the following steps (A) or (B): (A) a step of forming an image portion and an adhesive portion by developing an image portion using the toner and an adhesive portion using the powder adhesive on at least one of the surfaces of the paper that will become the surface A, and fixing the image portion and the adhesive portion by heating; (B) a step of forming an adhesive portion by developing the adhesive portion by the powder adhesive on one side of the surface of the paper that will become surface A and fixing the adhesive portion by heating, and a step of forming an image portion by developing an image portion by the toner on at least the other side of the paper that will become surface A and fixing the image portion by heating; The method for producing the adhesive product includes the steps of: After the image area and the adhesive area are formed, the paper is stacked so as to sandwich the formed adhesive area, and heated to melt the adhesive area to bond the papers together, thereby obtaining the bonded product.
12. A thermoplastic resin, a compound represented by the following formula (3), and a peak value of the carbon number being 20 or more and 70 or less.
1. A powder adhesive containing a linear saturated hydrocarbon wax, comprising: the thermoplastic resin is a styrene-acrylic resin, The content of the thermoplastic resin in the powder adhesive is 75.0% by mass or more and 92.0% by mass or less, The content Nb1 of the compound represented by formula (3) in the powder adhesive is 8.0% by mass or more and 20.0% by mass or less, the content Nb2 of the chain saturated hydrocarbon wax having a peak value of the carbon number of 20 or more and 70 or less in the powder adhesive is 0.1% by mass or more and 5.0% by mass or less; The Nb1 and the Nb2 2.00≦Nb1 / Nb2≦25.00 A powder adhesive characterized by satisfying the above. (In formula (3), n and m each independently represent a positive integer of 14 or more and 20 or less.)
Citation Information
Patent Citations
Image forming method
JP2006171607A
Powder adhesive
JP2008170659A
Adhesive material, sheet for producing press-bonding printed matter, method for producing sheet for producing press-bonding printed matter, press-bonding printed matter, method for producing press-bonding printed matter, and apparatus for producing press-bonding printed matter
JP2019167471A