Dopant fluid storage and distribution system utilizing high performance structurally modified particulate carbon sorbents - Patent Application 20070123633
A structurally modified particulate carbon adsorbent with optimized particle size and VSA addresses safety and capacity issues in storing and delivering toxic dopant gases, enhancing semiconductor industry safety and compliance.
Patent Information
- Application Number
- JP2022529717
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-12
- Filing Date
- 2020-11-10
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-11-10
AI Technical Summary
Existing carbon adsorption systems for storing and handling highly toxic dopant gases in the semiconductor industry face challenges such as high pressure storage risks, mechanical system failures, and insufficient loading and delivery capacity, posing safety and regulatory concerns.
A structurally modified particulate carbon adsorbent with a specific particle size range of 0.15 mm to 0.5 mm, optimized for volumetric surface area (VSA) and bulk density, allowing for high deliverable capacity and safe storage of dopant fluids.
The system provides enhanced dispensing capacity and safety by ensuring reliable and efficient delivery of toxic gases, reducing risks and compliance with regulatory standards.
Smart Images

Figure 0007556030000001 
Figure 0007556030000002 
Figure 0007556030000003
Abstract
Description
[Technical field]
[0001] The present invention relates generally to a carbon adsorption system for storing and dispensing a dopant fluid that is reversibly adsorbed onto a structurally modified particulate carbon adsorbent. In particular, the present invention relates to a carbon adsorption system having a structurally modified particulate carbon adsorbent having a specific particle size that has an optimal volumetric surface area when loaded into the interior volume of a vessel. [Background technology]
[0002] There is a need for reliable sources of dopant fluids for a wide variety of industrial applications. Many industrial processing and manufacturing applications require the use of highly toxic dopant gases. The production of semiconductor materials represents one such application in which the safe storage and handling of highly toxic hydride or halide gases and mixtures thereof is required. Examples of such gases include silane, germane, ammonia, phosphine, arsine, boron trifluoride, stilbene, hydrogen sulfide, hydrogen selenide, telluride, phosphorus trifluoride, arsenic pentafluoride, and other halides or hydrides, and gas mixtures thereof. As a result of toxicity and safety considerations, these gases must be carefully stored and handled in industrial process facilities.
[0003] The semiconductor industry relies on a variety of gaseous sources, such as arsine and phosphine, hydrogen selenide, boron trifluoride, diborane, silicon tetrafluoride, germanium tetrafluoride, selenium hexafluoride, carbon monoxide, and carbon dioxide, as sources of arsenic, phosphorus, boron, silicon, germanium, selenium, and carbon, among others, in ion implantation. Ion implantation systems typically require the use of pure gases, such as arsine and phosphine, stored as liquefied compressed gases at their respective vapor pressures, and boron trifluoride and silicon tetrafluoride, at high pressures of 1500 psig in delivery containers. Due to their extreme toxicity and high vapor pressures, their use, transportation, and storage raise significant safety concerns for the semiconductor industry.
[0004] To address various safety concerns, there are many systems that have been developed to deliver these hydrides and halides under subatmospheric conditions to ion implantation tools. The safety of the device requires that the gas be delivered at a pressure below atmospheric pressure so that the gas cannot escape from the cylinder if the valve opens to the atmosphere. A vacuum condition must be applied to the cylinder to obtain gas flow. Thus, a fail-safe vacuum-operated valve design is required. Many mechanical systems have been developed for atmospheric delivery of dopant gases. Some involve the use of a pressure regulator, while others require a valve device to control and deliver the product at subatmospheric pressure. These valve devices are set to deliver or open when subatmospheric pressure or vacuum conditions are applied to the delivery port of the cylinder. The exact location of these devices can be within the port body, within the neck cavity, or within the cylinder itself. In each case, the pressure regulator or valve device is located upstream of the cylinder valve seat for the flow of gas from the interior of the cylinder to the delivery port. The main drawback of the mechanical systems is that many toxic gases are stored at high pressure (e.g., 500 psi or higher) in the cylinder. For example, a mechanical system may fail due to a leak, etc., thereby defeating the safety design purpose of the mechanical system. Although the likelihood of a leak or other type of failure of a particular mechanical system is low, there are nonetheless end users who are unwilling to accept any risk when working with highly toxic gases. Additionally, certain regulatory agencies do not permit the use of high pressure storage systems in semiconductor manufacturing environments.
[0005] To eliminate higher pressure storage, an alternative approach involves deploying solid sorbents loaded into cylinders as part of a sorbent storage and distribution system. Currently, there are several commercially available sorbent storage and distribution systems. However, many of these systems are unable to demonstrate satisfactory performance. For example, many of the sorbent-based systems do not demonstrate sufficient deliverability of the gas between the storage conditions and the release operating conditions. Others are unable to demonstrate sufficient loading capacity of the particular gas used. However, other sorbent-based systems do not have sufficient loading capacity and sufficient deliverability.
[0006] In view of these shortcomings, there is an unmet need for higher performance carbon adsorption-based systems that operate in a safe and reliable manner. Summary of the Invention
[0007] In one aspect, a carbon sorbent storage and dispensing system includes a container and a structurally modified particulate carbon sorbent disposed within an interior volume of the container, the structurally modified particulate carbon sorbent comprising a synthetic polymer-based material, the structurally modified particulate carbon sorbent further comprising particles having a particle size of about 0.5 mm or less but about 0.15 mm or more, the structurally modified particulate carbon sorbent being capable of being loaded into the container as free-flowing particles to provide a carbon sorbent flow rate of about 800 m per cc of the loading volume of the container. 2 The structurally modified particulate carbon adsorbent has modified structural characteristics to produce a volumetric surface area (VSA) of greater than 100 nm, and is further configured to reversibly adsorb a dopant fluid stored at 20° C. and at a storage pressure of less than 1 bar.
[0008] In a second aspect, a carbon sorbent storage and dispensing system is provided that includes a container and a structurally modified particulate carbon sorbent disposed within an interior volume of the container, the structurally modified particulate carbon sorbent comprising a synthetic polymer-based material, the structurally modified particulate carbon sorbent further comprising particles having a particle size of about 0.5 mm or less but 0.15 mm or more, the structurally modified particulate carbon sorbent being capable of being loaded into the container as free-flowing particles to provide a carbon sorbent flow rate of about 800 m per cc of the loading volume of the container. 2 1. A carbon adsorbent storage and dispensing system comprising: a structurally modified particulate carbon adsorbent having modified structural characteristics to produce a volumetric surface area (VSA) of greater than 100 nm; and wherein the structurally modified particulate carbon adsorbent is further configured to reversibly adsorb a dopant fluid stored at 20° C. and at a storage pressure of less than 1 bar, wherein the structurally modified particulate carbon adsorbent is characterized by a dispensing capacity of greater than 210 grams per liter of structurally modified particulate carbon adsorbent when the dopant fluid is arsine. [Brief description of the drawings]
[0009] [Figure 1] 1 is a curve intended to illustrate the volumetric surface area, bulk density, and specific surface area as a function of activation degree for a particular range of particle sizes, further illustrating the optimal operating mode of the present invention as opposed to the operating mode of prior art systems.
[0010] [Diagram 2] The amount of arsine partitioned, expressed in g of arsine / L of sorbent, is shown from different structurally modified particulate carbon sorbent samples of different volumetric surface areas for a specified range of particle sizes.
[0011] [Diagram 3] 1 illustrates an exemplary carbon sorbent storage and distribution system in accordance with the principles of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention is a paradigm shift in the design of improved performance carbon sorbent distribution systems. As described, in one aspect, the present invention provides a carbon sorbent-based storage and distribution system with particulate carbon sorbents with a unique combination of structural features that allow for optimal volumetric surface area resulting in a relatively higher distribution capacity of dopant fluids than is already achievable with some commercially available systems. The improvements of the present invention are primarily due to a shift in the design criteria commonly used prior to the advent of the present invention.
[0013] The terms "tapped bulk density" and "packed density" and "bulk density" may be used interchangeably herein and may be used to mean the ratio of the mass of a material to the so-called "settled volume" of the material occupying a finite volume when a known weight of material is packed into a 250 mL graduated cylinder and the packed cylinder is placed in a RotoTap apparatus for 5000 cycles. Once the 5000 cycles are completed, the "settled volume" is measured and from this the tapped bulk density is determined.
[0014] As used herein, the term "counting-based method" refers to a laser-based technique known in the art for determining average particle size using dynamic range analysis. This technique can be performed using a variety of commercially available instruments, such as the Camsizer® P4 particle analyzer available from Retsch Technology.
[0015] As used herein, the term "vessel" means any storage, filling, delivery, or transportable vessel capable of receiving a carbon sorbent with a dopant fluid reversibly adsorbed thereon, including, but not limited to, cylinders, containers, dewars, bottles, tanks, barrels, bulk, and microbulk.
[0016] As used herein, the term "dopant fluid" refers to gas, vapor, liquid, multi-phase dopant fluids, including mixtures, as well as single component dopant fluids.
[0017] As used herein, the term "deliverable capacity" or "distribution capacity" refers to the amount of dopant fluid that can be desorbed from the porous structure of a particulate carbon adsorbent, expressed in units of weight of dopant fluid per unit volume of adsorbent, when the pressure is reduced from 650 Torr to 20 Torr at a temperature of 20°C + / - 1°C, unless otherwise indicated.
[0018] The term "specific surface area," as used herein, refers to the surface area of the micropores of a particulate carbon adsorbent per unit mass of the particulate carbon adsorbent, and is typically measured in m per gram of particulate carbon adsorbent, unless otherwise specified, when the specific area value is measured by ASTM 6556-04 (BET N2,77K). 2 It is expressed in units of.
[0019] As used herein, "conduit" or "conduit flow network" means tubes, pipes, hoses, manifolds, and any other suitable structures sufficient to create one or more flow paths and / or allow the passage of a dopant fluid.
[0020] As used herein, "connected" or "operably connected" means a direct or indirect connection between two or more components that allows fluid, mechanical, chemical, and / or electrical communication between the two or more components.
[0021] The term "size" or "particle size" is intended to mean the average diameter or average effective diameter as measured by counting-based methods, and the shape of the particles can be spherical or irregular.
[0022] The term "particulate" is intended to include any free-flowing form, including beads, pellets, extrudates, powders, and granules.
[0023] The embodiments as described below are merely examples, and the present invention is not limited to the embodiments illustrated in the drawings. It should also be understood that the drawings are not scaled and, in some cases, details that are not necessarily required for understanding the embodiments, such as conventional manufacturing and assembly details, have been omitted. It should also be understood that certain features have been intentionally omitted in each of the drawings to better illustrate various aspects of the principles of the present invention.
[0024] The embodiments are described with reference to the drawings, in which similar elements are referenced by like numerals. The relevance and function of the various elements of the embodiments will be better understood from the detailed description that follows. The detailed description contemplates various permutations and combinations of features, aspects, and embodiments as being within the scope of the present disclosure. Thus, the present disclosure may be specified to comprise, consist of, or consist essentially of any of such combinations and permutations of these specific features, aspects, and embodiments, or a selected one or more of them.
[0025] Prior to the advent of the present invention, the predominant design objective for carbon sorbent storage and distribution systems was to maximize the surface area per unit mass ("specific surface area") of the particulate carbon material. Maximizing the specific surface area exfoliates the carbon material to create numerous mesopores and micropores that are believed to be potentially available for capture of dopant fluids during storage, thereby increasing the loading capacity of the material.
[0026] Still others have focused on higher utilization materials with a low end where only a relatively small percentage of the original amount of dopant fluid remains adsorbed on the carbon adsorbent during the dispensing operation, while the majority of the dopant fluid is reversibly desorbed from the material during the dispensing operation. For example, U.S. Patent No. 6,592,653 describes carbon adsorbents with bulk densities of less than 0.5 g / cc as a means of maximizing the surface area of the carbon adsorbent.
[0027] The present invention has determined that many carbon sorbent storage and dispensing systems based on any of the above design criteria do not provide optimal performance. As used herein, "performance" is measured in terms of the deliverable capacity of dopant fluid reversibly adsorbed onto specifically tailored structurally modified carbon sorbent particles during dispensing operations. The present invention has determined that in order to optimize volumetric surface area (i.e., also referred to as "VSA"), bulk density and the competing variables of specific surface area must be balanced. However, the present invention further recognizes that VSA by itself is not sufficient to optimize the performance of a carbon sorbent storage and dispensing system. In this regard, the present inventors have discovered that the VSA of the sorbent must be optimized in combination with a particle size of about 0.5 mm or less but 0.15 mm or greater. VSA (e.g., m per cubic centimeter ("cc") of container volume) is a measure of the relative density of the sorbent. 2 The bulk density (e.g., expressed in grams of material per cc of container volume) and the specific surface area (e.g., m per gram of material) are 2 The VSA is determined from the product of the VSA and the porosity (units of material) of the carbon adsorbent. The relatively low VSAs are located to the left and right of the mode of operation of the present invention in FIG. 1 and are described in more detail below. The present invention recognizes that lower levels of VSA produce a poor performing carbon storage and distribution system for dopant fluids. VSA provides a numerical indicator of porosity per unit volume and can be more specifically expressed as porosity per unit packed vessel volume of particulate carbon adsorbent (e.g., beaded or granular material). Thus, the carbon adsorbent storage and distribution system of the present invention is distinguishable from the prior art at least on the basis that it is designed around an optimal VSA mode of operation for carbon adsorbent particles having a particle size of about 0.5 mm or less but about 0.15 mm or more, as clearly shown in FIG. 1.
[0028] FIG. 1 illustrates a generalized graphical relationship of VSA, bulk density, and specific surface area as a function of degree of activation for a particular carbon adsorbent. The x-axis is intended to indicate increasing activation moving from left to right along the x-axis, and the y-axis is intended to indicate increasing magnitude of VSA, bulk density, and specific surface area moving from bottom to top along the y-axis. With reference to FIG. 1, for a given intermediate degree of activation of a particular carbon adsorbent particle, having a particle size of about 0.5 mm or less but 0.15 mm or more, as indicated by an "x" on the x-axis, the structurally modified particulate carbon adsorbent has a corresponding specific surface area value and a corresponding bulk density value such that the product of the bulk density value and the specific area value results in an optimal VSA value for distributing a dopant fluid. The respective relative magnitudes of the specific surface area, bulk density, and VSA are graphically illustrated on the y-axis. The "x" represents an example of a combination of bulk density, specific surface area, and VSA values for carbon adsorbent particles ranging from 0.15 mm to 0.5 mm. The bracketed "invention" format represents the complete range of bulk densities, specific surface areas, and optimum VSA values for particulate carbon adsorbents having particle sizes of about 0.5 mm or less but 0.15 mm or more.
[0029] As used herein, the term "intermediate degree of activation" is understood to mean a certain level of activation of the particulate carbon adsorbent material that decomposes a portion of the starting carbon material in an amount less than the maximum activation corresponding to the bracketed mode of operation entitled "Prior Art Utilizing Maximum Activation" but greater than the minimum activation corresponding to the bracketed mode of operation entitled "Prior Art Utilizing Minimum Activation". Activation may occur as described in U.S. Patent Nos. 6,309,446, 7,288,504, 8,147,589, and 9,234,628, each of which is incorporated herein by reference in its entirety. The present invention requires structurally modified particulate carbon adsorbent carbon that has undergone a controlled intermediate degree of activation in combination with a particle size of about 0.5 mm or less but about 0.15 mm or more, as shown in FIG. 1. Preferably, the present invention employs substantially spherical or non-spherical synthetic polymer-based carbon materials, although other types of carbon-based active materials may be employed. Figure 1 is intended to illustrate, among other aspects, the effect of activation degree on VSA. The inventors have recognized that bulk density decreases linearly with increasing activation degree, resulting in a VSA curve where the product of specific surface area and bulk density passes through a maximum value as shown in Figure 1. Utilizing an over-activated carbon adsorbent will produce an insufficient VSA as a result of the bulk density being excessively reduced by the maximum activation degree, thereby resulting in a material with properties corresponding to the specific surface area, bulk density, and VSA curves to the right of the inventive mode of operation of Figure 1. Conversely, utilizing an under-activated material will create an insufficient VSA as a result of the unacceptably low specific surface area produced by the minimum activation degree, thereby resulting in a material with properties corresponding to the specific surface area, bulk density, and VSA curves to the left of the inventive mode of operation of Figure 1.
[0030] A correlation to the deliverability of VSA in combination with a range of particle sizes for structurally modified carbon sorbents has been discovered by the inventors. Examples 1-5 and Comparative Examples 1-2 provided below verify that correlation. Specifically, the amount of arsine delivered, expressed in g / L of sorbent, from various different structurally modified particulate carbon sorbents, as discussed, is greater, as is the volumetric surface area of the sorbent for sorbents having particle sizes within a particular range.
[0031] In one embodiment, a carbon sorbent storage and distribution system is provided that includes a container and a structurally modified particulate carbon sorbent disposed within an interior volume of the container to distribute arsine to a downstream process, such as an ion implantation tool, as part of an arsine-containing ion implantation process. The structurally modified particulate carbon sorbent is configured to store up to about 800 ml of the structurally modified particulate carbon sorbent to realize the benefits of a higher distribution capacity of a dopant fluid that is reversibly adsorbed on the structurally modified carbon sorbent. 2 The carbon sorbent has a VSA of over 100 / cc and particle size ranging from 0.15 mm to 0.50 mm. A significant benefit achieved with higher deliverable capacity with arsine and other dopant gases utilized in ion implantation processes is extended carbon sorbent storage and dispensing life. Extended vessel life allows for longer on-tool time and reduces replacement frequency during the ion implantation process. In this manner, the risks associated with vessel replacement are significantly reduced.
[0032] The volumetric surface area, as shown in Figure 2, is at least 800 m 21. The curves in FIG. 2 show the deliverable capacity of arsine fluid versus volumetric surface area for different structurally modified particulate carbon sorbents. Applicants constructed the curves by conducting several different tests utilizing different structurally modified carbon particulate sorbent samples with different volumetric surface areas. In other words, each data point represents a test utilizing a different structurally modified particulate carbon sorbent. The test procedures are described below for Comparative Examples 1-2 and Examples 1-5. The curves in FIG. 2 show that for carbon sorbent particles having particle sizes in the range of 0.15-0.5 mm, the amount of arsine delivered per liter of sorbent (delivery capacity) is 800 m 2 The increase in surface area over 800 m2 / cc in Figure 2 shows that 2 Each of the five data points showing arsine deliverability at a VSA of more than 800 μg / cc corresponds to Examples 1, 2, 3, 4, and 5 described below. The captioned mode of operation in FIG. 2, labeled "Invention," shows that a structurally modified particulate sorbent having particle sizes ranging from 0.15 mm to 0.5 mm provides arsine deliverability at a VSA of 800 μg / cc. 2 It is intended to define one aspect of the present invention that the container is designed to effectively fill the interior volume of the container so as to substantially improve arsine dispensing capacity in excess of 100000 / cc.
[0033] It should be understood that the present invention can be used with other dopant fluids. For example, other dopant gases such as arsine, phosphine, boron trifluoride, hydrogen selenide, diborane, silicon tetrafluoride, germanium tetrafluoride, and any other suitable dopant fluids that can be adsorbed and desorbed from the structurally modified particulate carbon adsorbent described herein can be used with the structurally modified carbon adsorbent storage and dispensing system of the present invention. The dispensing capacity of such other dopant fluids is expected to behave similarly to that of FIG. 2, whereby the deliverable capacity during the dispensing operation increases when utilizing a higher level of VSA and a structurally modified particulate carbon adsorbent having a particle size of about 0.5 mm or less but about 0.15 mm or more. In one embodiment, the dopant fluid, such as phosphine, boron trifluoride, hydrogen selenide, diborane, silicon tetrafluoride, germanium tetrafluoride, germane, or any other suitable dopant fluid, is preferably at a concentration of greater than 800 but not greater than 900 m3 per cc of the fill volume of the container, with a particle size ranging from 0.15 mm to 0.5 mm, or more preferably 0.2 to 0.475 mm. 2 In another embodiment, the VSA is reversibly adsorbed onto a structurally modified carbon adsorbent having a porous surface area of 875-900 m with a particle size ranging from 0.15 mm to 0.5 mm, or more preferably 0.2-0.475 mm. 2 / cc or more, preferably 850-875m 2 / cc, most preferably 800-850m 2 / cc range. The compatibility of the present invention with other dopant fluids (e.g., dopant gases) provides a wide range of benefits in a variety of process applications requiring a consistent supply of dopant fluid with minimal process downtime disruption, thereby significantly increasing throughput and reducing the associated risks of vessel replacement. The present inventors have determined that structurally modified particulate carbon sorbents designed with such VSA values have a microporous structure that produces a relatively high delivery capacity when incorporated as part of a carbon storage and delivery system.
[0034] The present invention also provides a method for producing a sorbent having a particle size of 0.15 mm to 0.5 mm, or 0.20 mm to 0.45 m, or 0.25 mm to 0.40 mm, in combination with a structurally modified carbon sorbent having a particle size of 900 m per cc of the packed volume of the container. 2 Also contemplated are distribution systems having structurally modified particulate carbon adsorbents having VSA's of the above porous surface areas.
[0035] Surprisingly, the present invention can generate higher deliverable capacities for dopant fluids even if the specific surface area of the structurally modified carbon sorbent is not maximized. Some prior art systems have focused on maximizing the specific surface area to maximize loading capacity. However, for a particular particle size of 0.15 mm to 0.5 mm, the optimal VSA range within the present invention's format as shown in FIG. 1 allows for deliverable capacities that can be higher than those achieved in prior art systems, even if the specific surface area of the structurally modified particulate carbon sorbent is not maximized as was done in many prior art systems. The present invention has an optimal VSA with a wide range of microporous structures with appropriate pore volumes structurally configured to reversibly adsorb dopant fluids during adsorption. In one embodiment, the structurally modified particulate carbon sorbent can exhibit a deliverable capacity of 200 g / cc or more, 220 g / cc or more, 230 g / cc or more, or 240 g / cc or more of dopant fluid. The structural features of the sorbents of the present invention (i.e., optimized VSA and specific particle size range) result in a high performance carbon sorbent delivery system, thereby potentially increasing throughput in a variety of end-use and intermediate applications.
[0036] We now discuss the characteristics that yield optimal VSA values for a particular particle size range used as part of a carbon sorbent storage and distribution system. First, the tapped bulk density as used in the present invention is equal to at least 0.45 g / cc to avoid carbon sorbent storage and distribution systems with over-activated carbon sorbents, as shown in the right hand portion of FIG. 1 entitled "Prior Art Utilizing Maximum Activation". In one embodiment, the bulk density can be up to 0.5 g / cc or more, or up to 0.6 g / cc or more. In another embodiment, the bulk density ranges from greater than 0.45 g / cc up to 0.7 g / cc, or from 0.45 to 0.6 g / cc, or from 0.5 to 0.70 g / cc. While maintaining a sufficient level of bulk density is important, it should be understood that there is an upper limit to the bulk density avoided by the present invention to avoid carbon sorbent storage and distribution systems with over-activated carbon sorbents, as shown in the left hand portion of FIG. 1 entitled "Prior Art Utilizing Minimum Activation". Thus, it is preferred that the bulk density be 0.7 g / cc or less.
[0037] In addition to bulk density, an optimal VSA also has a specific surface area in a particular range. The specific surface area of a structurally modified granular carbon adsorbent is typically in the range of 1000 m. 2 / g, 1300m 2 / g or more, or 1400m 2 In another embodiment, the specific surface area of the structurally modified particulate carbon adsorbent is 1300 m 2 / g~maximum 1800m 2 / g, or 1400m 2 / g~1800m 2 / g, or 1500m 2 / g~1800m 2 / g. Such ranges are intended to fall along the bracketed specific surface area curves within the mode of operation of the present invention in FIG.
[0038] As shown in FIG. 1, the combination of high specific surface area with sufficient bulk density for particle sizes in the range of 0.15 mm to 0.5 mm ensures that the VSA of a given carbon adsorbent particle is optimized, thereby ensuring that the carbon adsorbent storage and distribution system can be configured to operate with improved distribution capabilities for a variety of dopant fluids. Prior to the present invention, many conventional systems have focused on maximizing surface area per unit mass at the expense of losing an excessive amount of bulk density because bulk density was considered merely a secondary design consideration. However, the present invention recognizes that (i) both specific surface area and bulk density are competing variables that must be balanced to optimize the VSA, and further, (ii) such balance must occur within the context of carbon adsorbent particle sizes in the range of 0.15 mm to 0.5 mm. Thus, the exact bulk density combined with the specific surface area of a given structurally modified particulate carbon adsorbent of the required particle size may depend on the ability to create and impart the required intermediate activation degree to the carbon adsorbent. The ability for a material to have a relatively high specific surface area without excessive loss of bulk density is only possible with an intermediate degree of activation for a certain range of particle sizes, as shown in FIG.
[0039] The particles of the structurally modified particulate carbon adsorbent can have a size ranging from 0.5 mm to about 0.15 mm. In another embodiment, the particle size ranges from 0.4 mm to 0.15 mm. In yet another embodiment, the particle size ranges from 0.35 mm to a minimum of 0.2 mm, or from 0.3 to 0.2 mm, or from 0.15 to 0.2 mm. Surprisingly, for a given degree of activation, as can be reflected in gravimetric surface area measurements (i.e., traditional BET surface area measurements), the inventors have discovered that the tradeoff between specific surface area and bulk density is reduced or minimized for particle sizes in the range of 0.15 mm to 0.5 mm, more preferably 0.2 mm to 0.475 mm, since the bulk density does not appear to drop off significantly for a given amount of activation of the material. However, applicants have found that as particle sizes drop below 0.15mm handling problems arise, thereby establishing the criticality remaining at 0.15mm and above, and applicants have observed that larger particle sizes above 0.5mm do not achieve optimal VSA, thereby establishing the criticality remaining at 0.5mm and below.
[0040] Additionally, the pore size distribution is substantially composed of micropores with minimal amounts of mesopores and macropores as measured by mercury porosimetry. The mercury porosimetry analysis technique utilizes the uptake of mercury into the pores of a structurally modified particulate carbon adsorbent under controlled pressure. The uptake of mercury into the pores is indicative of the volume percent ("vol %) of mesopores and macropores, which in their aggregates have sizes ranging from 0.0035 micrometers to 12.5 micrometers, and the volume percent is based on the total volume of the solid pieces of the adsorbent. An AutoPoreIV 9500 porosimeter, commercially available from Micrometrics Instruments Corporation, was utilized by the inventors to generate the mesopore and macropore size data.
[0041] The inventors have conducted extensive testing based on the above mercury porosimetry analysis technique and concluded that the performance benefits of the resulting activated structure are substantially or entirely attributable to the presence of a microporous structure having mesopores and macropores, preferably less than 10% by volume, based on the total volume of the solid piece of particulate sorbent. The presence of mesopores and macropores does not impart any beneficial properties to the performance of the carbon sorbent storage and distribution system, as measured in terms of distribution capacity. Thus, the present invention contemplates a substantially microporous structure having less than 10% by volume, mesopores and macropores, based on the total volume of the solid piece of particulate sorbent, where a substantially microporous structure can be defined as a micropore size of less than about 2 nm (i.e., 20 Angstroms). Without being bound by theory, it is believed that the increased presence of a combination of mesopores or macropores can be formed as a result of overactivating the material or activating the material in a non-selective manner, such that a number of pores in the particle may tend to agglomerate into larger pores under certain conditions.
[0042] In one embodiment of the present invention, the particulate morphology is substantially spherical. Substantially spherical particles may tend to be more or less uniformly activated throughout the volume of the particle, with the structurally modified particulate carbon sorbent containing a balanced distribution and uniformly sized micropores throughout the particle with less than 10 volume percent mesopores and macropores, based on the total volume of the solid piece of particulate sorbent. In contrast, particles of other shapes, particularly substantially non-spherical particles that are substantially irregularly shaped, may have greater variations in their activation such that structural characteristics that result in optimal VSA values for use as part of the carbon sorbent storage and distribution system of the present invention are not obtained. Furthermore, substantially spherical particles allow the bulk densities described herein above to be achieved by substantially spherical particles having a structure that can be effectively packed within the internal volume of the storage and distribution system vessel.
[0043] The substantially spherical particles have sizes that may range as described herein above, with other narrower ranges of sizes contemplated falling within the broader range of 0.15 mm to 0.5 mm.
[0044] The activated carbon adsorbents are preferably non-carbohydrate synthetic polymeric materials such as those based on styrene and divinylbenzene. Other examples include any of the synthetic polymeric materials described in U.S. Patents 6,309,446, 7,288,504, 8,147,589, and 9,234,628.
[0045] An exemplary carbon sorbent storage and dispensing system according to the principles of the present invention is shown in FIG. 3. FIG. 3 shows a carbon sorbent storage and dispensing system having a structurally modified particulate carbon sorbent (2) loaded within the interior volume of a vessel (1). A cylinder valve (3) has threads that can be connected to the top of the vessel (1) along with corresponding threads on the neck (6) of the vessel (1). The cylinder valve (3) includes a valve opening and closing handle (5) that allows for the dispensing of a dopant fluid that is reversibly adsorbed onto the structurally modified particulate carbon sorbent (2). A single port valve assembly is shown connected to the vessel (1). An outlet port (4) is shown along which the desorbed dopant fluid can flow out of the interior volume of the vessel (1). The outlet port (4) also serves as a loading inlet port through which a dopant fluid can be introduced during adsorption of the dopant fluid onto the structurally modified particulate carbon sorbent (2).
[0046] The carbon sorbent storage and distribution system may be coupled to any suitable downstream process. In one example, the carbon sorbent storage and distribution system may be coupled to a downstream ion implanter to allow arsine or phosphine to be distributed to the downstream ion implanter, where the arsine or phosphine is delivered at a controlled flow rate to the ion implanter and ionized under appropriate ion implantation conditions to obtain arsine- or phosphorus-containing ions for subsequent implantation into wafers. Other downstream processes include, but are not limited to, semiconductor processing plants, flat panel display manufacturing facilities, organic synthesis facilities, pharmaceutical manufacturing facilities, anesthesia gas distribution masks, air treatment or water pollution abatement facilities, combustion gas processes, or any other suitable downstream process facilities for intermediate or end use of gases distributed from the carbon sorbent storage and distribution system of the present invention.
[0047] One or more of the carbon sorbent storage and distribution systems may be disposed within the gas cabinet. In such a gas cabinet arrangement with multiple carbon sorbent storage and distribution systems, each of the systems may be manifolded to one another for selective delivery of dopant fluid desorbed from the structurally modified particulate carbon sorbent from one or more of such carbon sorbent storage and distribution systems. The cabinet may further include independent thermocouples, or other temperature sensing / monitoring devices and components, to prevent overheating of the systems and / or other internal components of the gas cabinet.
[0048] In another embodiment, the use of structurally modified particulate carbon sorbents can be efficiently loaded into containers for dopant gases that may be applied for storage at pressures substantially subatmospheric to above atmospheric pressures in conjunction with a storage and dispensing system incorporating an UpTime® valve designed to ensure that downstream vacuum conditions are required to trigger the release of the product. UpTime® style valves are described in U.S. Patent Nos. 7,905,247, 5,937,895, 6,007,609, 6,045,115, 7,708,028, and 9,909,670, each of which is incorporated herein by reference in its entirety.
[0049] It is understood that modifications to the above-described embodiments may be made without departing from the scope of the present invention. For example, a mixture of different sorbents may be used, each of which falls within the contemplated particle size and VSA criteria. Additionally, it is understood that any commercially available synthetic polymeric particulate carbon sorbent may be modified to meet the required attributes of the present invention with respect to VSA and particle size, and then loaded into the dispensing vessel.
[0050] The features and characteristics of the carbon sorbent storage and distribution system are more fully illustrated by the following non-limiting comparative examples and examples. Example 1
[0051] A sample of the synthetic polymer derived structurally modified particulate carbon adsorbent was weighed and loaded into a sample container at a packing density of 0.5851 g / cc. The structurally modified particulate carbon adsorbent was preconditioned via heat and vacuum to remove aggregated moisture and air from the pores to levels below 1 ppm. The final vacuum conditions associated with preconditioning the container with the loaded adsorbent were 50 mTorr or less than 0.05 Torr. The structurally modified particulate carbon adsorbent had a size of 0.475 mm and a specific surface area of 1486 m. 2 / g, resulting in a volumetric surface area of 869 m 2 / cc.
[0052] The arsine gas from the source cylinder was regulated through a mass flow controller to control the amount of arsine gas adsorbed into the sample vessel. The temperature of the adsorption process was maintained at 20°C ± -1°C. The pressure in the sample vessel was measured to determine the end point of the filling. The filling was stopped when a storage pressure of approximately 650 Torr was achieved and maintained (stable) in the sample vessel.
[0053] After the adsorption process was completed, a distribution process was performed. The flow of arsine dopant fluid from the sample vessel was performed utilizing a pressure differential between the pressure within the interior volume of the sample vessel and a lower pressure outside the sample vessel, thereby desorbing the dopant fluid from the modified particulate carbon sorbent in the sample vessel and recovering it from the sample vessel. As a result of the pressure differential, the arsine dopant fluid was desorbed from the modified particulate carbon sorbent as arsine gas, which was then recovered from the interior of the sample vessel and flowed through the distribution assembly. The arsine gas flowed through a mass flow controller which maintained a substantially constant flow rate through the distribution conduit during the distribution operation. The distribution of arsine gas occurred in the sample vessel from a starting pressure of 650 Torr to a final pressure of 20 Torr in a temperature controlled system where the temperature was maintained at 20°C + / - 1°C. The pressure in the sample vessel was measured during the distribution operation. Desorption was stopped when a pressure of approximately 20 Torr was achieved and maintained (stable) in the sample vessel. The flows through the mass flow controllers were summed to determine the grams of gas removed from the sample vessel from 650 Torr down to 20 Torr. The summator showed a delivery capacity of 228.73 grams of arsine per liter of structurally modified particulate carbon adsorbent. This example was run at 800 m for particle sizes ranging from 0.15 to 0.5 mm. 2 It was determined that a sufficiently high VSA of more than 1 / cc resulted in acceptable performance. Example 2
[0054] A sample of the synthetic polymer derived structurally modified particulate carbon adsorbent was weighed and loaded into a sample container at a packing density of 0.4853 g / cc. The structurally modified particulate carbon adsorbent was preconditioned via heat and vacuum to remove aggregated moisture and air from the pores to levels below 1 ppm. The final vacuum conditions associated with preconditioning the container with the loaded adsorbent were 50 mTorr or less than 0.05 Torr. The structurally modified particulate carbon adsorbent had a size of 0.457 mm and a specific surface area of 1736 m. 2 / g, resulting in a volumetric surface area of 842 m 2 / cc.
[0055] The arsine gas from the source cylinder was regulated through a mass flow controller to control the amount of arsine gas adsorbed into the sample vessel. The temperature of the adsorption process was maintained at 20°C ± -1°C. The pressure in the sample vessel was measured to determine the end point of the filling. The filling was stopped when a storage pressure of approximately 650 Torr was achieved and maintained (stable) in the sample vessel.
[0056] After the adsorption process was completed, a distribution process was performed. The flow of arsine dopant fluid from the sample vessel was performed utilizing a pressure differential between the pressure within the interior volume of the sample vessel and a lower pressure outside the sample vessel, thereby desorbing the dopant fluid from the modified particulate carbon sorbent in the sample vessel and recovering it from the sample vessel. As a result of the pressure differential, the arsine dopant fluid was desorbed from the modified particulate carbon sorbent as arsine gas, which was then recovered from the interior of the sample vessel and flowed through the distribution assembly. The arsine gas flowed through a mass flow controller which maintained a substantially constant flow rate through the distribution conduit during the distribution operation. The distribution of arsine gas occurred in the sample vessel from a starting pressure of 650 Torr to a final pressure of 20 Torr in a temperature controlled system where the temperature was maintained at 20°C + / - 1°C. The pressure in the sample vessel was measured during the distribution operation. Desorption was stopped when a pressure of approximately 20 Torr was achieved and maintained (stable) in the sample vessel. The flows through the mass flow controllers were summed to determine the grams of gas removed from the sample vessel from a full vacuum of 650 Torr down to 20 Torr. The summator showed a delivery capacity of 213.57 grams of arsine per liter of structurally modified particulate carbon adsorbent. This example was run at 800 ml for particle sizes ranging from 0.15 mm to 0.5 mm. 2 It was determined that a sufficiently high VSA of more than 1 / cc resulted in acceptable performance. Example 3
[0057] A sample of the synthetic polymer derived structurally modified particulate carbon adsorbent was weighed and loaded into a sample container at a packing density of 0.6908 g / cc. The structurally modified particulate carbon adsorbent was preconditioned via heat and vacuum to remove aggregated moisture and atmospheric impurities from the pores to levels below 1 ppm. The final vacuum conditions associated with preconditioning the container with the loaded adsorbent were 50 mTorr or less than 0.05 Torr. The structurally modified particulate carbon adsorbent had a size of 0.202 mm and a specific surface area of 1300 m. 2 / g, resulting in a volumetric surface area of 898 m 2 / cc.
[0058] The arsine gas from the source cylinder was regulated through a mass flow controller to control the amount of arsine gas adsorbed into the sample vessel. The temperature of the adsorption process was maintained at 20°C ± -1°C. The pressure in the sample vessel was measured to determine the end point of the filling. The filling was stopped when a pressure of approximately 650 Torr was achieved and maintained (stable) in the sample vessel.
[0059] After the adsorption process was completed, a distribution process was performed. The flow of arsine dopant fluid from the sample vessel was performed utilizing a pressure differential between the pressure within the interior volume of the sample vessel and a lower pressure outside the sample vessel, thereby desorbing the dopant fluid from the modified particulate carbon sorbent in the sample vessel and recovering it from the sample vessel. As a result of the pressure differential, the arsine dopant fluid was desorbed from the modified particulate carbon sorbent as arsine gas, which was then recovered from the interior of the sample vessel and flowed through the distribution assembly. The arsine gas flowed through a mass flow controller which maintained a substantially constant flow rate through the distribution conduit during the distribution operation. The distribution of arsine gas occurred in the sample vessel from a starting pressure of 650 Torr to a final pressure of 20 Torr in a temperature controlled system where the temperature was maintained at 20°C + / - 1°C. The pressure in the sample vessel was measured during the distribution operation. Desorption was stopped when a pressure of approximately 20 Torr was achieved and maintained (stable) in the sample vessel. The flows through the mass flow controllers were summed to determine the grams of gas removed from the sample vessel from a full vacuum of 650 Torr down to 20 Torr. The summator showed a delivery capacity of 243.21 grams of arsine per liter of structurally particulate modified carbon adsorbent. This example was run at 800 ml for particle sizes ranging from 0.15 mm to 0.5 mm. 2 It was determined that a sufficiently high VSA of more than 1 / cc resulted in acceptable performance. Example 4
[0060] A sample of the synthetic polymer derived structurally modified particulate carbon adsorbent was weighed and loaded into a sample container at a packing density of 0.6098 g / cc. The structurally modified particulate carbon adsorbent was preconditioned via heat and vacuum to remove aggregated moisture and atmospheric impurities from the pores to levels below 1 ppm. The final vacuum conditions associated with preconditioning the container with the loaded adsorbent were 50 mTorr or less than 0.05 Torr. The structurally modified particulate carbon adsorbent had a size of 0.195 mm and a specific surface area of 1470 m 2 / g, resulting in a volumetric surface area of 896 m 2 / cc.
[0061] The arsine gas from the source cylinder was regulated through a mass flow controller to control the amount of arsine gas adsorbed into the sample vessel. The temperature of the adsorption process was maintained at 20°C ± -1°C. The pressure in the sample vessel was measured to determine the end point of the filling. The filling was stopped when a pressure of approximately 650 Torr was achieved and maintained (stable) in the sample vessel.
[0062] After the adsorption process was completed, a distribution process was performed. The flow of arsine dopant fluid from the sample vessel was performed utilizing a pressure differential between the pressure within the interior volume of the sample vessel and a lower pressure outside the sample vessel, thereby desorbing the dopant fluid from the modified particulate carbon sorbent in the sample vessel and recovering it from the sample vessel. As a result of the pressure differential, the arsine dopant fluid was desorbed from the modified particulate carbon sorbent as arsine gas, which was then recovered from the interior of the sample vessel and flowed through the distribution assembly. The arsine gas flowed through a mass flow controller which maintained a substantially constant flow rate through the distribution conduit during the distribution operation. The distribution of arsine gas occurred in the sample vessel from a starting pressure of 650 Torr to a final pressure of 20 Torr in a temperature controlled system where the temperature was maintained at 20°C + / - 1°C. The pressure in the sample vessel was measured during the distribution operation. Desorption was stopped when a pressure of approximately 20 Torr was achieved and maintained (stable) in the sample vessel. The flows through the mass flow controllers were summed to determine the grams of gas removed from the sample vessel from a full vacuum of 650 Torr down to 20 Torr. The summator showed a delivery capacity of 247.39 grams of arsine per liter of structurally particulate modified carbon adsorbent. This example was run at 800 ml for particle sizes ranging from 0.15 to 0.5 mm. 2 It was determined that a sufficiently high VSA of more than 1 / cc. resulted in acceptable performance. Example 5
[0063] A sample of the synthetic polymer derived structurally modified particulate carbon adsorbent was weighed and loaded into a sample container at a packing density of 0.5232 g / cc. The structurally modified particulate carbon adsorbent was preconditioned via heat and vacuum to remove coagulated moisture and atmospheric impurities from the pores to levels below 1 ppm. The final vacuum conditions associated with preconditioning the container with the loaded adsorbent were 50 mTorr or less than 0.05 Torr. The structurally modified particulate carbon adsorbent had a size of 0.191 mm and a specific surface area of 1796 m. 2 / g, resulting in a volumetric surface area of 940 m 2 / cc.
[0064] The arsine gas from the source cylinder was regulated through a mass flow controller to control the amount of arsine gas adsorbed into the sample vessel. The temperature of the adsorption process was maintained at 20°C ± -1°C. The pressure in the sample vessel was measured to determine the end point of the filling. The filling was stopped when a pressure of approximately 650 Torr was achieved and maintained (stable) in the sample vessel.
[0065] After the adsorption process was completed, a distribution process was performed. The flow of arsine dopant fluid from the sample vessel was performed utilizing a pressure differential between the pressure within the interior volume of the sample vessel and a lower pressure outside the sample vessel, thereby desorbing the dopant fluid from the modified particulate carbon sorbent in the sample vessel and recovering it from the sample vessel. As a result of the pressure differential, the arsine dopant fluid was desorbed from the modified particulate carbon sorbent as arsine gas, which was then recovered from the interior of the sample vessel and flowed through the distribution assembly. The arsine gas flowed through a mass flow controller which maintained a substantially constant flow rate through the distribution conduit during the distribution operation. The distribution of arsine gas occurred in the sample vessel from a starting pressure of 650 Torr to a final pressure of 20 Torr in a temperature controlled system where the temperature was maintained at 20°C + / - 1°C. The pressure in the sample vessel was measured during the distribution operation. Desorption was stopped when a pressure of approximately 20 Torr was achieved and maintained (stable) in the sample vessel. The flows through the mass flow controllers were summed to determine the grams of gas removed from the sample vessel from a full vacuum of 650 Torr down to 20 Torr. The summator showed a delivery capacity of 263.56 grams of arsine per liter of structurally particulate modified carbon adsorbent. This example was run at 800 ml for particle sizes ranging from 0.15 to 0.5 mm. 2 It was determined that a sufficiently high VSA of more than 1 / cc. resulted in acceptable performance. Comparative Example 1
[0066] A sample of the carbon adsorbent was weighed and packed into a sample container with a packing density of 0.3794 g / cc. The carbon adsorbent was preconditioned via heat and vacuum to remove coagulated moisture and atmospheric impurities from the pores to 1 ppm levels. The final vacuum conditions associated with preconditioning the container with the packed adsorbent were 50 mTorr or less than 0.05 Torr. The carbon adsorbent had a size of 0.434 mm and a specific surface area of 1920 m. 2 / g, resulting in a volumetric surface area of 728 m 2 / cc.
[0067] The arsine gas from the source cylinder was regulated through a mass flow controller to control the amount of arsine gas adsorbed into the sample vessel. The temperature of the adsorption process was maintained at 20°C ± -1°C. The pressure in the sample vessel was measured to determine the end point of the filling. The filling was stopped when a pressure of approximately 650 Torr was achieved and maintained (i.e., stabilized) in the sample vessel.
[0068] After the adsorption process was completed, a distribution process was performed. The flow of arsine dopant fluid from the sample vessel was performed utilizing a pressure differential between the pressure within the interior volume of the sample vessel and a lower pressure outside the sample vessel, thereby desorbing the dopant fluid from the carbon adsorbent in the sample vessel and recovering it from the sample vessel. As a result of the pressure differential, the arsine dopant fluid was desorbed from the carbon adsorbent as arsine gas, which was then recovered from the interior of the sample vessel and flowed through the distribution assembly. The arsine gas flowed through a mass flow controller that maintained a substantially constant flow rate through the distribution conduit during the distribution operation. The distribution of arsine gas occurred in the sample vessel from a starting pressure of 650 Torr to a final pressure of 20 Torr in a temperature controlled system where the temperature was maintained at 20°C + / - 1°C. The pressure in the sample vessel was measured during the distribution operation. Desorption was stopped when a pressure of approximately 20 Torr was achieved and maintained (stable) in the sample vessel. The flows through the mass flow controllers were totaled to determine the grams of gas removed from the sample vessel from a full vacuum of 650 Torr down to 20 Torr. The totalizer indicated a delivery capacity of 187.41 grams of arsine per liter of carbon sorbent.
[0069] Test results showed significantly lower arsine deliverability from Examples 1-5. It was concluded that particle sizes within the required range of (0.15-0.5) mm were not sufficient in themselves to produce acceptable performance. A sufficiently high VSA was also required. This example was run at 800 m 2 The requirements of both VSA above 1 / cc and particle size within (0.15-0.5) mm range were verified. Comparative Example 2
[0070] A sample of the carbon adsorbent was weighed and packed into a sample container with a packing density of 0.59 g / cc. The carbon adsorbent was preconditioned via heat and vacuum to remove aggregated moisture and air from the pores to levels below 1 ppm. The final vacuum conditions associated with preconditioning the container with the packed adsorbent were 50 mTorr or less than 0.05 Torr. The carbon adsorbent had a size of 0.7 mm and a specific surface area of 1200 m2 / g, resulting in a volumetric surface area of 708 m 2 / cc.
[0071] The arsine gas from the source cylinder was regulated through a mass flow controller to control the amount of arsine gas adsorbed into the sample vessel. The temperature of the adsorption process was maintained at 20°C ± -1°C. The pressure in the sample vessel was measured to determine the end point of the filling. The filling was stopped when a pressure of approximately 650 Torr was achieved and maintained (stable) in the sample vessel.
[0072] After the adsorption process was completed, a distribution process was performed. The flow of arsine dopant fluid from the sample vessel was performed utilizing a pressure differential between the pressure within the interior volume of the sample vessel and a lower pressure outside the sample vessel, thereby desorbing the dopant fluid from the carbon adsorbent in the sample vessel and recovering it from the sample vessel. As a result of the pressure differential, the arsine dopant fluid was desorbed from the carbon adsorbent as arsine gas, which was then recovered from the interior of the sample vessel and flowed through the distribution assembly. The arsine gas flowed through a mass flow controller that maintained a substantially constant flow rate through the distribution conduit during the distribution operation. The distribution of arsine gas occurred in the sample vessel from a starting pressure of 650 Torr to a final pressure of 20 Torr in a temperature controlled system where the temperature was maintained at 20°C + / - 1°C. The pressure in the sample vessel was measured during the distribution operation. Desorption was stopped when a pressure of approximately 20 Torr was achieved and maintained (stable) in the sample vessel. The flows through the mass flow controllers were totalized to determine the grams of gas removed from the sample vessel down to a full vacuum of 650 Torr and then 20 Torr. The totalizer indicated a delivery capacity of 190.64 grams of arsine per liter of carbon sorbent. Test results were consistent over a 800m 2 As a result of the relatively low VSA, less than 1 / cc, and particle size above the upper limit of 0.5 mm, Examples 1-5 show significantly lower arsine deliverability. 2 The requirements of both VSA above 1 / cc and particle size within the range of (0.15-0.5) mm were further verified.
[0073] Collectively, the tests showed that the specific range of particle size and optimal VSA combination in Examples 1, 2, 3, 4 and 5 produced significantly higher arsine deliverable capacity than those in Comparative Examples 1 and 2.
[0074] While what are considered to be particular embodiments of the invention have been shown and described, it will of course be understood that various modifications and changes in form or detail can be readily made without departing from the spirit and scope of the invention. It is therefore intended that the invention not be limited to the exact forms and details shown and described herein, nor be limited to anything less than the full scope of the invention disclosed herein and claimed below.
Claims
【Claim 1】 1. A carbon sorbent storage and dispensing system comprising: a container; and a structurally modified particulate carbon sorbent disposed within an interior volume of the container, the structurally modified particulate carbon sorbent being made of a synthetic polymer-based material, the structurally modified particulate carbon sorbent further comprising particles having a particle size ranging from about 0.15 mm to about 0.2 mm, the structurally modified particulate carbon sorbent being capable of being loaded into the container as free-flowing particles to provide a carbon sorbent flow rate of about 800 m per cc of loading volume of the container. 2 1. A carbon adsorbent storage and distribution system comprising: a carbon adsorbent having modified structural characteristics to produce a volumetric surface area (VSA) of greater than 100 nm; and wherein the structurally modified particulate carbon adsorbent is further configured to reversibly adsorb a dopant fluid stored at 20° C. and at a storage pressure of less than 1 bar, the dopant fluid being arsine, phosphine, boron trifluoride, hydrogen selenide, diborane, silicon tetrafluoride, germanium tetrafluoride, or germane.
Citation Information
Patent Citations
Gas storage-delivery method and gas storage-delivery device
JP1999082891A
Method of depositing dielectric film
JP2002190522A
Fluid storage and delivery system comprising high work capacity physical sorbent
JP2008196689A
Vertical type light-emitting diode, and crystal growth method
JP2015005534A
Spherical phenol resin activated carbon for methane occlusion and method for producing the same, and methane occlusion material using activated carbon and methane occlusion method using activated carbon
JP2018047453A