Monofilament and its manufacturing method

A two-step drawing process with controlled conditions enhances the tensile properties of PA4 monofilaments by minimizing voids and optimizing molecular orientation, addressing the limitations of conventional methods in maintaining strength when knotted.

JP7556148B2Active Publication Date: 2024-09-25KUREHA CORPORATION
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023527594
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-06-08
Filing Date
2022-05-20
Publication Date
2024-09-25
Estimated Expiration
2042-05-20

AI Technical Summary

Technical Problem

Conventional spinning methods for polyamide 4 (PA4) monofilaments fail to adequately suppress void generation and enhance tensile properties when knotted, which is crucial for applications requiring high tensile strength in a knotted state.

Method used

A two-step drawing process involving dry heat and wet heat stretching with specific temperature and ratio conditions to produce a PA4 monofilament with controlled scattering intensity and birefringence, ensuring minimal voids and optimal molecular orientation.

Benefits of technology

The method results in a PA4 monofilament with enhanced tensile strength and elongation when knotted, suitable for applications like fishing lines, by effectively suppressing void formation and improving molecular orientation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556148000003
    Figure 0007556148000003
  • Figure 0007556148000004
    Figure 0007556148000004
  • Figure 0007556148000001
    Figure 0007556148000001
Patent Text Reader

Abstract

Achieved is a polyamide 4 (PA4) monofilament which demonstrates high tensile properties even when knotted. In this PA4 monofilament, the average value of the ratio I2 / I1 of a normalized scattering intensity I2 in the equatorial direction to a normalized scattering intensity I1 in the meridional direction is 5 or less for a scattering vector in the range of 0.02 nm-1 to 0.04 nm-1, inclusive, as measured by small-angle X-ray scattering. Furthermore, the birefringence of the monofilament is 50×10−3 or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a monofilament and a method for producing the same. [Background technology]

[0002] Polyamide 4 (hereinafter, also referred to as "PA4") is expected to be put to practical use as a bioplastic, and many spinning methods thereof are being investigated. One of the properties required for PA4 monofilaments is that they have high tensile strength. Known spinning methods for producing PA4 monofilaments having such high tensile strength include a solution spinning method using formic acid or the like (see, for example, Patent Document 1), a gel spinning method using an ionic liquid, and a melt spinning method using an inorganic salt (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-137934 A [Patent Document 2] International Publication No. 2012 / 157576 Summary of the Invention [Problem to be solved by the invention]

[0004] It is considered that monofilaments are usually used in a knotted state. Therefore, monofilaments for such applications are required to exhibit high tensile properties when knotted. However, all of the above-mentioned conventional spinning methods have room for improvement in terms of suppressing the generation of voids in PA4 monofilaments and improving the tensile properties when knotted.

[0005] An object of one aspect of the present invention is to provide a PA4 monofilament that exhibits high tensile properties even when knotted. [Means for solving the problem]

[0006] In order to solve the above problems, a monofilament according to one aspect of the present invention is a polyamide 4 monofilament, and the scattering vector of the monofilament measured by small angle X-ray scattering is 0.02 nm -1 More than 0.04nm -1 The average ratio I2 / I1 of the normalized scattering intensity I2 in the equatorial direction to the normalized scattering intensity I1 in the meridian direction in the following range is 5 or less, and the birefringence of the monofilament is 50×10 -3 That's all.

[0007] In order to solve the above problems, a method for producing a monofilament according to one embodiment of the present invention is a method for producing a polyamide 4 monofilament by drawing an undrawn yarn of polyamide 4, the method comprising: a first drawing step in which the undrawn yarn of polyamide 4 is drawn by dry heat drawing under conditions of a drawing temperature of 40°C or higher and a draw ratio of 2.5 to 3.5 times; and a second drawing step in which the primarily drawn yarn of polyamide 4 produced in the first drawing step is drawn by wet heat drawing under conditions of a drawing temperature of 80°C or higher and 120°C or lower and a specific draw ratio, the specific draw ratio being a draw ratio for the undrawn yarn in both the first drawing step and the second drawing step that is 3.5 times or higher in total (however, when the total draw ratio is 3.5 times, the draw ratio in the first drawing step is less than 3.5 times). Effect of the Invention

[0008] According to one embodiment of the present invention, it is possible to realize a PA4 monofilament that exhibits high tensile properties even when knotted. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a photograph showing a two-dimensional small angle X-ray scattering (SAXS) image of the monofilament of Example 1 of the present invention. [Diagram 2]FIG. 2 is a photograph showing a two-dimensional small angle X-ray scattering (SAXS) image of the monofilament of Comparative Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [Monofilament] [Polyamide 4] The monofilament according to the embodiment of the present invention is substantially composed of polyamide 4 (PA4). PA4 is a polymer compound having a structural unit represented by the following formula (1). In the following formula, x is 4.

[0011] [ka]

[0012] In an embodiment of the present invention, the polymer compound that constitutes the fiber structure of the monofilament may be only PA4. In an embodiment of the present invention, other components other than PA4 may be further contained within a range in which the effects of the present embodiment can be obtained. The other components may be one or more, and examples thereof include reinforcing materials, plasticizers, lubricants, and stabilizers. The other components may include polymer compounds other than PA4. The other components are appropriately used in an amount that further exerts the effects of the other components. Thus, the monofilament of the embodiment of the present invention is a PA4 monofilament.

[0013] [Small angle X-ray scattering intensity ratio] The monofilament according to the embodiment of the present invention has a specific scattering intensity ratio measured by a small angle X-ray scattering (SAXS) method. That is, the scattering vector q of the monofilament measured by the small angle X-ray scattering method is 0.02 nm -1 More than 0.04nm -1 The average ratio I2 / I1 of the normalized scattering intensity I2 in the equatorial direction to the normalized scattering intensity I1 in the meridian direction is 5 or less in the following range:

[0014] The average value of I2 / I1 is 0.02 nm -1More than 0.04nm -1 This is the average value of the ratio I2 / I1 of the normalized scattering intensity I1 in the meridian direction to the normalized scattering intensity I2 in the equatorial direction, obtained for each scattering vector q in increments of 0.000241 in the following range.

[0015] The normalized scattering intensity I2 in the equatorial direction represents voids (tiny cavities in the monofilament). The larger the I2, the greater the amount of voids present in the monofilament. On the other hand, the normalized scattering intensity I1 in the meridian direction represents scattering other than voids in the monofilament. The average value of the above ratio I2 / I1 being 5 or less indicates that the voids in the monofilament are sufficiently suppressed, and that the monofilament exhibits the same tensile properties even when knotted as when not knotted. PA4 monofilaments with an average value of the above ratio I2 / I1 being 5 or less have sufficiently high tensile properties even when knotted.

[0016] From the viewpoint of improving the tensile properties of the PA4 monofilament when knotted, the lower the ratio I2 / I1, the more preferable. For this reason, the ratio I2 / I1 is more preferably within the range of 1 or more and 2 or less.

[0017] The above I2 and I1 can be measured using a known small angle X-ray scattering measuring device. The above ratio I2 / I1 can be realized by a manufacturing method including a first stretching step and a second stretching step, which will be described later. For example, I2 tends to be smaller by lowering the stretch ratio in the second stretching step.

[0018] [Birefringence] The monofilament of the present invention has a specific birefringence. That is, the birefringence of the monofilament is 50×10 -3 That's all.

[0019] The birefringence of a monofilament is a measure of the degree of orientation of the polymer chains of the polymer compound that constitutes the monofilament with respect to the fiber axis direction. The greater the absolute value of the birefringence, the greater the degree of orientation. -3 The fact that the above conditions are met means that the monofilament has been subjected to a drawing step.

[0020] The birefringence is set to 50×10 from the viewpoint of improving the tensile properties of the monofilament. -3 It is preferable that the value is 55×10 or more. -3 More preferably, it is 60×10 or more. -3 From the viewpoint of exhibiting sufficiently high tensile properties when the monofilament is knotted, the birefringence is preferably 90×10 -3 It may be the following:

[0021] The birefringence can be measured, for example, by retardation measurement using a polarizing microscope equipped with a Berek compensator and a sodium lamp as a light source. The birefringence tends to be higher by increasing the stretch ratio in the manufacturing method described later.

[0022] [Tensile properties at knot] The tensile strength of the monofilament of the embodiment of the present invention at the time of knotting is preferably 550 MPa or more from the viewpoint of realizing sufficient tensile strength in the application in which the monofilament can be used in the knotted state. The application in which the monofilament can be used in the knotted state is, for example, a fishing line. The tensile strength at the time of knotting can be appropriately determined depending on the application of the monofilament. The tensile strength at the time of knotting is preferably high from the viewpoint of preventing the monofilament from breaking at the knotted portion when pulled, and is more preferably, for example, 550 MPa or more, and even more preferably, 600 MPa or more. On the other hand, the tensile strength at the time of knotting may be within the range that can be realized by the PA4 monofilament, and from such a viewpoint, the tensile strength at the time of knotting may be 1000 MPa or less.

[0023] The tensile strength of the monofilament at the knot can be measured using a known device capable of performing a tensile test on fibers. The tensile strength of the monofilament at the knot can be achieved by a manufacturing method including a first drawing step and a second drawing step, which will be described later. The tensile strength at the knot tends to be increased by lowering the density of the undrawn yarn.

[0024] In the monofilament of the embodiment of the present invention, the tensile elongation at knotting is preferably 10% or more from the viewpoint of preventing breakage when used in a knotted state. The tensile elongation at knotting can be appropriately determined depending on the application of the monofilament, and from the above viewpoint, it is more preferably 15% or more, and even more preferably 20% or more. On the other hand, the tensile elongation at knotting may be within a range that can be realized with a PA4 monofilament, and from such a viewpoint, the tensile elongation at knotting may be 50% or less.

[0025] The tensile elongation of the monofilament at the knot can be measured using a known device capable of performing a tensile test on fibers. The tensile elongation of the monofilament at the knot can be achieved by a manufacturing method including a first drawing step and a second drawing step described later. The tensile elongation at the knot tends to be lowered by increasing the drawing ratio in the manufacturing method described later, and tends to be higher by decreasing the density of the undrawn yarn.

[0026] [Thread diameter] The thread diameter of the monofilament according to the embodiment of the present invention is preferably 400 μm or less from the viewpoint of sufficiently increasing the tensile properties of the monofilament when knotted. If the thread diameter exceeds 400 μm, moisture absorption in the second drawing step of the production method described later may be insufficient, and the tensile properties when knotted may be insufficient. From the viewpoint of achieving sufficient moisture absorption of the monofilament in the second drawing step, the thread diameter of the monofilament is more preferably 300 μm or less, and even more preferably 200 μm or less. On the other hand, the thread diameter of the monofilament may be within a range that can be achieved with a PA4 monofilament depending on the application of the monofilament, but may be 50 μm or more from the viewpoint of sufficiently performing the moisture absorption.

[0027] The thread diameter of the monofilament can be measured by a known technique for measuring fiber diameter, for example, by a known method for measuring the thread diameter of the fiber by pinching the fiber. The thread diameter of the monofilament tends to become smaller by increasing the draw ratio in the production method described below.

[0028] [Other physical properties] The monofilament of the embodiment of the present invention is only required to have the above-mentioned physical properties, and may further have other physical properties in addition to those described above, as long as the effects of the embodiment described above are achieved.

[0029] For example, the weight average molecular weight of PA4 in this embodiment is not limited, but from the viewpoint of fully expressing physical properties specific to PA4, such as mechanical properties and heat resistance, in the monofilament, it is preferably 20,000 or more, more preferably 30,000 or more, and even more preferably 35,000 or more. The weight average molecular weight of PA4 may be within a range in which a PA4 monofilament can be obtained, and from such a viewpoint, for example, it is preferably 200,000 or less, or preferably 100,000 or less.

[0030] [Method of manufacturing monofilament] The monofilament according to the embodiment of the present invention can be produced by the production method described below. The monofilament according to the embodiment of the present invention is produced by drawing an undrawn polyamide 4 yarn by the first drawing step and the second drawing step described below. By carrying out such a two-step drawing step, it is possible to produce a PA4 monofilament having excellent tensile properties when knotted, as described above.

[0031] [Undrawn yarn] The undrawn yarn of polyamide 4 is a monofilament produced by spinning polyamide 4 as a material, and is a monofilament that is not substantially drawn. It is preferable that the undrawn yarn is amorphous from the viewpoint of further improving the tensile properties at knotting of the finally produced monofilament. From this viewpoint, it is preferable that the density of the undrawn yarn is low. From the viewpoint of realizing the tensile properties at knotting of the monofilament described above (tensile strength at knotting of 550 MPa or more and tensile elongation at knotting of 10% or more), the density of the undrawn yarn is 1.225 g / cm 3 It is preferable that the density is 1.223 g / cm or less. 3 It is more preferable that:

[0032] However, even if the density of the undrawn yarn is high, it is possible to obtain a monofilament having improved tensile properties when knotted by the manufacturing method of the embodiment of the present invention. The density of the undrawn yarn can be appropriately determined within a range that allows the monofilament to exhibit tensile properties when knotted according to its intended use. From this viewpoint, the density of the undrawn yarn is set to 1.240 g / cm 3 It may be less than or equal to 1.250 g / cm 3 The density of the monofilament is correlated with the crystallinity of the monofilament, and the lower the density, the lower the crystallinity tends to be. For example, if the density of the monofilament is 1.230 g / cm 3 corresponds to a crystallinity of about 10% for the monofilament.

[0033] The density of the undrawn yarn can be determined by a method also known as the "density gradient method." The density of the undrawn yarn can be adjusted by the cooling conditions of the fibrous molten extrudate of PA4 produced by melt spinning. The density of the undrawn yarn tends to be lower as the cooling temperature is lower or the cooling time is longer.

[0034] [First stretching step] The first drawing step is a step of drawing the undrawn yarn of polyamide 4 by dry heat drawing under the conditions of a drawing temperature of 40° C. or more and a draw ratio of 2.5 to 3.5 times. However, when the total draw ratio described below is 3.5 times, the draw ratio in the first drawing step is less than 3.5 times. The first drawing step can be carried out by a known technique capable of carrying out drawing under such conditions. By drawing the undrawn yarn to some extent under the above conditions prior to the second drawing step, it is possible to prevent breakage during wet heat drawing.

[0035] In the first drawing step, the drawing temperature is 40° C. or higher. If the drawing temperature in the first drawing step is too low, whitening of the monofilament may occur. From the viewpoint of preventing whitening of the monofilament, the drawing temperature in the first drawing step is preferably 40° C. or higher, more preferably 50° C. or higher.

[0036] If the drawing temperature in the first drawing step is high, crystallization of PA4 in the monofilament may progress, and the tensile properties at the time of knotting may decrease. From the viewpoint of suppressing the progress of crystallization and fully expressing the tensile properties at the time of knotting, the drawing temperature in the first drawing step is preferably 100° C. or less, and more preferably 80° C. or less. From the viewpoint of preventing whitening in the monofilament and expressing the expected tensile properties at the time of knotting, the drawing temperature in the first drawing step is more preferably within the range of 60±5° C., and most preferably 60° C.

[0037] In the first drawing step, the draw ratio is 2.5 times or more and 3.5 times or less. If the draw ratio in the first drawing step is too low, necking remains in the PA undrawn yarn that has been subjected to the first drawing step (first drawn yarn), and local deformation occurs in the subsequent second drawing step, which may result in a non-uniform yarn diameter of the monofilament. From the viewpoint of obtaining a monofilament having a uniform yarn diameter, the draw ratio in the first drawing step is preferably 2.5 times or more, and more preferably 2.8 times or more.

[0038] If the draw ratio in the first drawing step is too high, the first drawn yarn may be stretched too much, voids may occur, and the expected tensile properties at the time of knotting may be insufficient. From the viewpoint of suppressing the occurrence of voids in the monofilament, the draw ratio in the first drawing step is preferably 3.5 times or less, and more preferably 3.2 times or less. From the viewpoint of having a uniform yarn diameter and suppressing the occurrence of voids, the draw ratio in the first drawing step is more preferably within the range of 3±0.1 times, and most preferably 3 times.

[0039] The form of drawing in the first drawing step is hot drawing. Hot drawing here means drawing the monofilament in a gas phase (e.g., air) whose temperature is controlled to the above-mentioned drawing temperature. The humidity in the first drawing step is not limited, and may be, for example, 80% or less in relative humidity.

[0040] [Second stretching step] The second drawing step is a step of drawing the first drawn polyamide 4 yarn produced in the first drawing step by wet heat drawing under conditions of a drawing temperature of 80°C to 120°C and a draw ratio of 4 times or more. The second drawing step can be carried out by a known technique capable of carrying out drawing under such conditions. By drawing the first drawn yarn in a softened state by absorbing moisture after the first drawing step, it is possible to produce a PA4 monofilament having excellent tensile properties at the time of knotting as described above.

[0041] The drawing temperature in the second drawing step is 80° C. or higher and 120° C. or lower. If the drawing temperature in the second drawing step is too low, the moisture absorption of the first drawn yarn may be insufficient, and the tensile properties of the resulting monofilament at the time of knotting may be insufficient. From the viewpoint of allowing the first drawn yarn to absorb moisture sufficiently, the drawing temperature in the second drawing step is preferably 85° C. or higher, and more preferably 90° C. or higher.

[0042] The drawing temperature in the second drawing step can be appropriately set within a range in which the drawing atmosphere can be realized with steam. From the viewpoint of being able to set the drawing atmosphere, the drawing temperature in the second drawing step is preferably 110°C or less, and more preferably 105°C or less. From the viewpoint of being able to easily configure the drawing device and allowing the first drawn yarn to absorb moisture sufficiently, the drawing temperature in the second drawing step is more preferably within the range of 100±3°C, and most preferably 100°C.

[0043] The draw ratio in the second drawing step is 3.5 times or more. The draw ratio in the second drawing step in the embodiment of the present invention is expressed as the final draw ratio of the undrawn yarn by both the first drawing step and the second drawing step (also referred to as the "total draw ratio"). The draw ratio in the second drawing step alone is appropriately determined according to the draw ratio in the first drawing step and the total draw ratio. The draw ratio in the second drawing step is usually larger than the draw ratio in the first drawing step, and in this case, if the drawing step is only two stages, the total draw ratio will be the same as the draw ratio in the second drawing step.

[0044] If the draw ratio in the second drawing step is too low, the tensile properties of the monofilament at the time of knotting may decrease, and the expected tensile properties at the time of knotting may not be obtained. From the viewpoint of imparting sufficient strength to the monofilament, the draw ratio in the second drawing step is preferably a draw ratio of 3.8 times or more in total, and more preferably a draw ratio of 4 times or more.

[0045] On the other hand, if the stretch ratio in the second drawing step is too high, voids may occur in the monofilament. From the viewpoint of sufficiently suppressing the occurrence of voids in the monofilament, the stretch ratio in the second drawing step is preferably a stretch ratio that results in a total stretch ratio of 5 times or less, and more preferably a stretch ratio that results in a total stretch ratio of 4.5 times or less. From the viewpoint of sufficiently expressing the tensile properties of the monofilament when knotted and sufficiently suppressing the occurrence of voids, the stretch ratio in the second drawing step is more preferably a stretch ratio that results in a total stretch ratio within the range of 4±0.3 times, and most preferably a stretch ratio that results in a total stretch ratio of 4 times.

[0046] The form of drawing in the second drawing step is wet heat drawing. The wet heat drawing here means drawing the monofilament in a steam atmosphere whose temperature is controlled to the drawing temperature described above. The humidity in the second drawing step is not limited, and may be, for example, 90% or more in relative humidity.

[0047] The stretching time in the second stretching step is preferably long from the viewpoint of more thoroughly wetting the first stretched yarn. From this viewpoint, the stretching time is preferably 5 seconds or more, more preferably 8 seconds or more, and even more preferably 10 seconds or more. On the other hand, the stretching time in the second stretching step is preferably short from the viewpoint of monofilament productivity. From this viewpoint, the stretching time is preferably 60 seconds or less, more preferably 45 seconds or less, and even more preferably 30 seconds or less.

[0048] In addition, the diameter of the first drawn yarn is preferably small from the viewpoint of more thoroughly wetting the first drawn yarn in the second drawing step. From the viewpoint of realizing the tensile properties at knotting of the monofilament described above (tensile strength at knotting of 550 MPa or more and tensile elongation at knotting of 10% or more), the diameter of the first drawn yarn is preferably 500 μm or less, more preferably 400 μm or less, and even more preferably 300 μm or less.

[0049] [Other processes] The method for producing the monofilament according to the embodiment of the present invention may further include other steps than the first drawing step and the second drawing step described above, within the scope of obtaining the effects of the embodiment of the present invention. For example, the method may further include a spinning step for producing an undrawn PA4 yarn. The form of the spinning step is so-called melt spinning, and the spinning step may include a melt extrusion step for extruding a molten kneaded product of PA4 by extrusion molding to produce a fibrous molten extrudate of PA4, and a cooling step for cooling the molten extrudate produced in the melt extrusion step in a refrigerant liquid. Such a spinning step can be carried out by a known melt spinning technique for producing an undrawn yarn by liquid cooling.

[0050] In the above cooling step, the cooling temperature is preferably low from the viewpoint of reducing the density of the undrawn yarn, and more specifically, it is preferably −10° C. or lower, more preferably −15° C. or lower, and even more preferably −20° C. or lower. The cooling temperature can be appropriately determined depending on the type of refrigerant liquid and production costs, and when the refrigerant liquid is a nonpolar solvent described below, it may be −60° C. or higher from the viewpoint of costs.

[0051] In the above cooling step, the cooling time is preferably long from the viewpoint of reducing the density of the undrawn yarn, more specifically, it is preferably 0.1 seconds or more, more preferably 0.2 seconds or more, and even more preferably 0.3 seconds or more. From the viewpoint of productivity, the cooling time is preferably short, and from this viewpoint, it is preferably 5 seconds or less, more preferably 3 seconds or less, and even more preferably 2 seconds or less.

[0052] In the above cooling step, the refrigerant liquid is preferably substantially inert to the molten extrudate of PA4 from the viewpoint of preventing the occurrence of surface roughness or whitening of the undrawn yarn. "Substantially inert" means that it does not substantially act on the molten extrudate, and more specifically, it is difficult to dissolve or is insoluble in PA4, and does not have permeability into the molten extrudate of PA4. Such a refrigerant liquid is preferably a non-polar solvent. Examples of non-polar solvents include silicone oil, hexane, nonane, decane, ethylcyclohexane, isopropylcyclohexane, toluene, and p-cymene.

[0053] In the spinning process, the fibrous molten extrudate is usually cooled while being pulled at a speed faster than the discharge speed of the molten extrudate, and then supplied to a drawing device. In an embodiment of the present invention, the pulling of the molten extrudate from the melt extrusion process to be supplied to the cooling process and the subsequent drawing process is not included in the drawing process, and may be appropriately set within a range in which the effects of this embodiment can be obtained.

[0054] In addition, in the method for producing the monofilament according to the embodiment of the present invention, a further drawing step that does not substantially generate voids may be carried out after the second drawing step. Such a further drawing step can be carried out by dry-heat drawing at a higher temperature (e.g., 200°C) than other drawing steps and at a moderate draw ratio (e.g., a final draw ratio (total draw ratio) including the further drawing step is 5 times). The further drawing step is advantageous from the viewpoint of further improving the tensile properties of the monofilament.

[0055] [Action and Effect] The method for producing a monofilament according to an embodiment of the present invention includes the first and second drawing steps described above. The PA4 monofilament produced by the method for producing the monofilament according to the present embodiment including these drawing steps has higher tensile properties at knotting than the PA4 monofilament produced through drawing steps other than these drawing steps. Thus, according to the embodiment of the present invention, the generation of voids in the monofilament is suppressed, and as a result, a monofilament having improved tensile properties at knotting can be realized. More specifically, according to the embodiment of the present invention, a monofilament having high tensile strength and tensile elongation at knotting can be realized.

[0056] In an embodiment of the present invention, the moisture absorption amount of the primary drawn yarn is reduced by the first drawing step, and then wet heat drawing is performed by the second drawing step. As a result, the primary drawn yarn absorbs sufficient moisture, and is further drawn in that state, thereby sufficiently suppressing the generation of voids and crystallization. Note that in dry heat drawing, the stress generated in the monofilament by drawing is usually high, making it easy to form voids. In the voids, stress is likely to concentrate at the time of knotting of the monofilament, and the monofilament is likely to break from the knots. Therefore, if the second drawing step is performed by dry heat drawing, the tensile properties at the time of knotting tend to decrease.

[0057] In addition, in the embodiment of the present invention, in both the first drawing step and the second drawing step, drawing is performed at a draw ratio that is sufficiently high so that breakage does not occur. Thus, the strength of the monofilament is fully developed. The tensile strength at the knot is always smaller than the tensile strength in a straight line. Thus, if the draw ratio in the drawing step is lowered, the tensile strength of the resulting monofilament in a straight line will be lower. Thus, if the draw ratio is lowered, the tensile strength of the resulting monofilament at the knot will also be lower.

[0058] The PA4 monofilament produced by the production method of this embodiment can be identified by the substantial absence of voids and traces of stretching. The presence or absence of voids can be confirmed by small angle X-ray scattering, and the traces of stretching can be confirmed by the degree of molecular orientation of PA4.

[0059] In an embodiment of the present invention, when the yarn diameter of the monofilament is sufficiently small, the yarn diameter of the first drawn yarn to be subjected to the second drawing step is also sufficiently small according to the draw ratio in the second drawing step, and the first drawn yarn can be drawn in a sufficiently wet state in the second drawing step. For example, if the yarn diameter of the monofilament is 400 μm or less, it is advantageous to realize the tensile properties at the time of knotting of the monofilament described above (tensile strength at the time of knotting of 550 MPa or more and tensile elongation at the time of knotting of 10% or more).

[0060] In the embodiment of the present invention, a lower density of the monofilament is advantageous in terms of improving the tensile properties at the time of knotting, and a lower density of the undrawn yarn is advantageous in terms of lowering the density of the monofilament (drawn yarn). From this viewpoint, the density of the undrawn yarn is preferably 1.225 g / cm 3 It is advantageous from the viewpoint of expressing the tensile properties of the monofilament when knotted, that the length is equal to or less than 1 mm.

[0061] 〔summary〕 As is clear from the above description, the monofilament according to the embodiment of the present invention is a polyamide 4 monofilament, and the scattering vector of the monofilament measured by small angle X-ray scattering is 0.02 nm. -1 More than 0.04nm -1 In the following range, the ratio I2 / I1 of the normalized scattering intensity I2 in the equatorial direction to the normalized scattering intensity I1 in the meridian direction is 5 or less, and the average birefringence of the monofilament is 50×10 -3 That's all.

[0062] The method for producing a monofilament according to an embodiment of the present invention is a method for producing a polyamide 4 monofilament by drawing an undrawn polyamide 4 yarn, and includes a first drawing step in which the undrawn polyamide 4 yarn is drawn by dry heat drawing under conditions of a drawing temperature of 40° C. or higher and a draw ratio of 2.5 to 3.5 times, and a second drawing step in which the first drawn polyamide 4 yarn produced in the first drawing step is drawn by wet heat drawing under conditions of a drawing temperature of 80° C. or higher and 120° C. or lower and a specific draw ratio. The specific draw ratio is a draw ratio that results in a total draw ratio of 3.5 times or higher, which is the final draw ratio for the undrawn yarn in both the first and second drawing steps. However, when the total draw ratio is 3.5 times, the draw ratio in the first drawing step is less than 3.5 times.

[0063] Therefore, according to an embodiment of the present invention, it is possible to realize a PA4 monofilament that exhibits high tensile properties even when knotted.

[0064] In an embodiment of the present invention, the tensile strength of the monofilament when knotted may be 550 MPa or more, and the tensile elongation of the monofilament when knotted may be 10% or more. This configuration is even more effective from the viewpoint of realizing a monofilament having sufficient tensile strength in applications where it may be used in a knotted state.

[0065] In an embodiment of the present invention, the monofilament may have a thread diameter of 400 μm or less, which is more effective in terms of sufficiently increasing the tensile properties of the monofilament when knotted.

[0066] In an embodiment of the present invention, the density of the undrawn yarn is 1.225 g / cm 3 This configuration is even more effective from the viewpoint of realizing the above-mentioned tensile properties of the monofilament when knotted (tensile strength when knotted of 550 MPa or more and tensile elongation when knotted of 10% or more).

[0067] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in the different embodiments are also included in the technical scope of the present invention. EXAMPLES

[0068] Example 1 At room temperature, 2 mol% of potassium tert-butoxide was added to α-pyrrolidone in a polymerization vessel and stirred. After dissolving the potassium tert-butoxide, 2 mol% of tetramethylammonium chloride was added as a polymerization aid and 0.1 mol% of N,N'-adipyldipyrrolidone was added as an initiator. After the addition, the system became cloudy and stirring soon became difficult. 72 hours after stirring was stopped, the lumps formed in the flask were removed and crushed. Unreacted materials and low molecular weight substances were washed with acetone. Powdered PA4 was obtained by drying the washed crushed material. The weight average molecular weight (Mw) of the obtained PA4 was 140,000.

[0069] The Mw of PA4 was measured by the following procedure, analytical equipment and conditions. [Measurement procedure] 10 mg of the PA4 sample obtained as described above was dissolved in hexafluoroisopropanol (HFIP) containing 5 mM sodium trifluoroacetate, and 10 cm 3 After that, the mixture was filtered through a membrane filter to obtain a sample solution. 10 μL of this sample solution was injected into an analyzer described below, and the weight-average molecular weight of PA4 was measured under the measurement conditions described below. In this specification, the symbol "to" indicates a range including both ends. [Analyzer] GPC equipment: Tosoh HLC-8420GPC [Measurement conditions] A) Column: Shoko Science GPC HFIP806M x 2 (connected in series) B) Eluent: 5mM CF3COONa / HFIP C) MALS: Wyatt DAWN HELEOS 2 D) Sample 10-11mg / 5mM CF3COONa / HFIP 10mL E) Flow rate: 1.0 mL / min F)dn / dc:0.240

[0070] PA4 was formed into a fiber shape by melt extrusion at a temperature of 265°C, and the obtained fibrous molten extrudate was passed through a volatile silicone oil ("KF-995", Shin-Etsu Silicone Co., Ltd.) bath at -20°C for 0.3 seconds immediately after forming to cool and solidify. In this way, an undrawn yarn of PA4 was produced. The density of the undrawn yarn was determined by the following method, and it was found to be 1.220 g / cm. 3 It was.

[0071] [Method of measuring density] The density of the undrawn yarn was determined by the density gradient method. The density was adjusted to 1.20-1.30 g / cm by changing the mixture ratio of heptane and carbon tetrachloride. 3 Six mixed solvents were used, adjusted in increments of 0.02 between 0.01 and 0.1.

[0072] Next, the produced undrawn yarn was drawn by dry heat drawing at a drawing temperature of 60°C and a draw ratio of 3.0 times. The humidity of the atmosphere during the dry heat drawing was 10% RH or less. Next, as the second stage drawing (secondary drawing), the produced first drawn yarn was drawn by wet heat drawing at a drawing temperature of 100°C and a total draw ratio of 4.0 times. The humidity of the atmosphere during the wet heat drawing was 100% RH. In this way, a monofilament of drawn yarn of PA4 was produced.

[0073] The diameter of the produced monofilament was measured by pinching the monofilament with a micrometer. The diameter of each of five randomly selected monofilaments was measured at one arbitrary point in the length direction, and the average value of the obtained measurements was calculated and used as the diameter of the monofilament. The diameter of the monofilament was 168 μm.

[0074] Example 2 A monofilament was produced in the same manner as in Example 1, except that the draw ratio of the first drawn yarn in the wet heat drawing of the second drawing was changed to a total draw ratio of 4.8 times. The yarn diameter of the monofilament was 147 μm.

[0075] Example 3 A monofilament was produced in the same manner as in Example 1, except that the temperature of the silicone oil bath for cooling the fibrous molten extrudate was changed to 40° C. The density of the undrawn yarn was 1.239 g / cm 3 It was.

[0076] Example 4 A monofilament was produced in the same manner as in Example 1, except that the primary draw ratio of the undrawn yarn was changed to 2.5 times.

[0077] Example 5 A monofilament was produced in the same manner as in Example 1, except that the primary draw ratio of the undrawn yarn was changed to 3.5 times.

[0078] Example 6 A monofilament was produced in the same manner as in Example 1, except that the primary drawing temperature of the undrawn yarn was changed to 50°C.

[0079] Example 7 A monofilament was produced in the same manner as in Example 1, except that the first drawing temperature of the undrawn yarn was changed to 100°C.

[0080] Comparative Example 1 Monofilaments were produced in the same manner as in Example 1, except that the drawing temperature (secondary drawing temperature) in the second drawing of the first-drawn yarn was changed to 200°C, and the first-drawn yarn was drawn by dry heat drawing instead of wet heat drawing.

[0081] Comparative Example 2 Monofilaments were produced in the same manner as in Example 3, except that the secondary drawing temperature was changed to 200° C., and the primarily drawn yarn was secondarily drawn by dry heat drawing instead of wet heat drawing.

[0082] Comparative Example 3 Monofilaments were produced in the same manner as in Example 3, except that the secondary drawing temperature was changed to 200°C, the draw ratio was changed to a total draw ratio of 4.6 times, and the primarily drawn yarn was secondarily drawn by dry heat drawing instead of wet heat drawing.

[0083] Comparative Example 4 An attempt was made to produce a monofilament in the same manner as in Example 3, except that the secondary drawing temperature was changed to 200°C, the draw ratio was changed to 4.8 times in total, and the primarily drawn yarn was secondarily drawn by dry heat drawing instead of wet heat drawing. Stretching breakage occurred during the secondary drawing, and drawing could not be performed.

[0084] Comparative Example 5 An attempt was made to produce a PA4 monofilament by stretching the undrawn yarn at a temperature of 100° C. and a stretch ratio of 3.0 times using wet heat drawing. Stretch breakage occurred during wet heat drawing, and drawing could not be carried out.

[0085] Comparative Example 6 A monofilament was produced in the same manner as in Comparative Example 1, except that the primary draw ratio of the undrawn yarn was changed to 2.5 times.

[0086] Comparative Example 7 A monofilament was produced in the same manner as in Comparative Example 1, except that the primary draw ratio of the undrawn yarn was changed to 3.5 times.

[0087] Comparative Example 8 A monofilament was produced in the same manner as in Comparative Example 1, except that the primary drawing temperature of the undrawn yarn was changed to 50°C.

[0088] Comparative Example 9 A monofilament was produced in the same manner as in Comparative Example 1, except that the first drawing temperature of the undrawn yarn was changed to 100°C.

[0089] Comparative Example 10 A monofilament was produced in the same manner as in Comparative Example 1, except that the second drawing was not carried out.

[0090] 〔evaluation〕 [Scattering vectors by small angle X-ray scattering (SAXS)] For each of the monofilaments in the above examples and comparative examples, the normalized scattering intensity I1 in the meridian direction and the normalized scattering intensity I2 in the equatorial direction were measured by the following measurement method, and their ratio I2 / I1 was calculated. -1 More than 0.04nm -1 This is the average value of all the ratios I2 / I1 obtained for each scattering vector q in increments of 0.000241 in the following range. <Method of measuring normalized scattering intensity> A fiber sample consisting of 16 bundled monofilaments was placed in a cell and immersed in tetradecane, and X-ray scattering measurements were performed under the following conditions. Equipment: Nano-Viewer, manufactured by Rigaku Corporation X-ray source: CuKα Current-Voltage: 40kV-20mA Irradiation time: 45 min Camera length: 830mm (small angle) Slit: 0.7mmΦ-0.6mmΦ-0.8mmΦ

[0091] [Birefringence of monofilament] The birefringence of each of the monofilaments in the above Examples and Comparative Examples was measured by the following measurement method. <Method of measuring birefringence> The birefringence of the monofilament was determined by retardation measurement using a polarizing microscope equipped with a Berek compensator and a sodium lamp as a light source.

[0092] [Tensile properties of monofilament at knots] For each of the monofilaments in the above examples and comparative examples, the tensile strength and tensile elongation of the monofilament at the knot were measured by the following measurement method. If the tensile strength at the knot is 550 MPa or more and the tensile elongation at the knot is 10% or more, it can be judged that there is no practical problem even when used in applications where it is knotted like fishing line. <Method of measuring tensile strength and tensile elongation> The tester was a Tensilon RTF-1210, and the tensile measurements were performed at 23°C, 50% RH, with the chuck distance set to 150 mm and the tensile speed set to 150 mm / min. When knotting, the knot was placed in the center between the chucks.

[0093] The manufacturing conditions and properties of the monofilaments in the above Examples and Comparative Examples are shown in Table 1. Two-dimensional SAXS images of the monofilament of Example 1 are shown in Fig. 1, and two-dimensional SAXS images of the monofilament of Comparative Example 1 are shown in Fig. 2. In Fig. 1 and Fig. 2, arrow I1 indicates the meridian direction in the two-dimensional SAXS images, and arrow I2 indicates the equator direction in the two-dimensional SAXS images.

[0094] [Table 1]

[0095] [Consideration of Examples and Comparative Examples] As is clear from Fig. 1, the monofilaments of the examples have small void scattering (scattering due to voids) in the central equatorial direction in the two-dimensional SAXS image. Also, as is clear from Table 1, the I2 / I1 ratios of the monofilaments of the examples are all 5 or less, and the birefringence is 50 × 10 -3 The monofilaments of the examples have improved tensile properties when knotted compared to the monofilaments of the comparative examples. Furthermore, the tensile strength when knotted is higher in Examples 1, 2, and 4 to 7, which have a lower density of the undrawn yarn, compared to Example 3.

[0096] On the other hand, in Comparative Examples 1 to 3 and 7 to 9, the tensile properties at the time of knotting are substantially decreased compared to those in the Examples. As is clear from Fig. 2, in the monofilament of Comparative Example 1, a strong streak is observed in the central equatorial direction in the two-dimensional SAXS image, and thus void scattering is confirmed. This is considered to be due to the formation of voids inside the monofilament as a result of the second drawing step being performed at a high drawing temperature and a high draw ratio.

[0097] In Comparative Example 4, breakage occurred during drawing of the first-drawn yarn, and in Comparative Example 5, breakage occurred during drawing of the undrawn yarn. This is thought to be because, in Comparative Example 4, the undrawn yarn was drawn without being wet, which caused voids to form and break the yarn. In Comparative Example 5, this is thought to be because the effect of the decrease in strength due to wetting of the undrawn yarn outweighed the effect of the improvement in strength due to drawing of the undrawn yarn.

[0098] Comparing Comparative Example 1 and Comparative Example 10 with the Examples, the monofilaments of the Examples tend to have higher tensile strength due to the secondary wet heat drawing, among the tensile properties exhibited by the dry heat drawing of the undrawn yarn. In addition, the secondary wet heat drawing tends to reduce the tensile elongation less than the secondary dry heat drawing. Furthermore, according to Examples 1 to 7, it is expected that the balance between tensile strength and tensile elongation can be appropriately adjusted by adjusting the conditions of the primary dry heat drawing and the secondary wet heat drawing.

[0099] In addition, since PA4 has a relatively high hydrophilicity, it is believed that the strength of the monofilament will decrease in the presence of water. Therefore, dry heat drawing is believed to be advantageous for developing the strength of PA4 monofilaments. Therefore, polyamides with higher hydrophobicity than PA4, such as PA6, are believed to be less susceptible to the effects of moisture absorption during drawing. Therefore, it is believed that the strength of undrawn PA6 yarn will be sufficiently improved even if it is drawn by wet heat drawing. [Industrial Applicability]

[0100] The PA4 monofilament of the present invention can be used as a synthetic fiber having excellent tensile properties, and the present invention is expected to further reduce the environmental burden caused by the use of the synthetic fiber.

Claims

1. A monofilament of polyamide 4, The scattering vector of the monofilament measured by small angle X-ray scattering is 0.02 nm -1 0.04nm or more -1 The average ratio I2 / I1 of the normalized scattering intensity I2 in the equatorial direction to the normalized scattering intensity I1 in the meridian direction is 5 or less in the following range: The birefringence of the monofilament is 50×10 -3 That's all. Monofilament.

2. 2. The monofilament according to claim 1, which has a tensile strength at knot of 550 MPa or more and a tensile elongation at knot of 10% or more.

3. 3. The monofilament according to claim 1 or 2, having a yarn diameter of 400 μm or less.

4. A method for producing a polyamide 4 monofilament by drawing an undrawn polyamide 4 yarn, comprising the steps of: A first drawing step of drawing the undrawn yarn of polyamide 4 by dry heat drawing under conditions of a drawing temperature of 40° C. or higher and a draw ratio of 2.5 times or more and 3.5 times or less; A second drawing step of drawing the first drawn yarn of polyamide 4 produced in the first drawing step by wet heat drawing at a drawing temperature of 80° C. or more and 120° C. or less at a specific draw ratio; The specific draw ratio is a draw ratio such that a total draw ratio, which is the draw ratio for the undrawn yarn in both the first drawing step and the second drawing step, is 3.5 times or more (however, when the total draw ratio is 3.5 times, the draw ratio in the first drawing step is less than 3.5 times).

5. The density of the undrawn yarn is 1.225 g / cm 3 The method for producing the monofilament according to claim 4, wherein:

Citation Information

Patent Citations

  • Metal vapor discharge lamp

    JP1980006726A

  • Silk gut

    JP1988056238A

  • Melt spinning of nylon-4

    JP1992136215A

  • Method for producing nylon 4 fiber, nylon 4 fiber and tire

    JP2019137934A

  • Method for producing nylon 4 fiber and nylon 4 fiber

    JP2021031790A