Surface-treated infrared absorbing microparticles and their manufacturing method, infrared absorbing microparticle dispersion, and infrared absorbing microparticle dispersion
Surface-treated infrared absorbing fine particles with a metal oxide hydrate coating and controlled carbon concentration enhance heat and humidity resistance, ensuring sustained infrared absorption performance.
Patent Information
- Application Number
- JP2020177937
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-23
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-10-23
AI Technical Summary
Infrared absorbing fine particles require improved heat and humidity resistance to maintain high infrared absorption characteristics over extended periods, especially when exposed to moist heat atmospheres.
Surface-treated infrared absorbing fine particles are coated with a metal oxide hydrate formed from a metal chelate compound, with a carbon concentration of 5.0% by mass or less, using a heat treatment process to enhance moisture and heat resistance.
The surface-treated particles maintain excellent infrared absorption characteristics while demonstrating improved heat and humidity resistance, with minimal changes in transmittance and haze even after exposure to harsh conditions.
Smart Images

Figure 0007556262000006 
Figure 0007556262000002 
Figure 0007556262000001
Abstract
Description
[Technical field]
[0001] The present invention relates to surface-treated infrared absorbing nanoparticles and a method for producing the same, an infrared absorbing nanoparticle dispersion, and an infrared absorbing nanoparticle dispersion. [Background technology]
[0002] In recent years, the demand for infrared absorbers has been increasing rapidly, and many patents related to infrared absorbers have been proposed. Looking at these proposals from a functional perspective, for example, there are those that aim to block light in the near-infrared region (infrared rays) while allowing sufficient visible light in the fields of windows for various buildings and vehicles, thereby suppressing the rise in temperature inside the room while maintaining brightness.
[0003] The present inventors have disclosed, as such an infrared absorbing body, an infrared absorbing fine particle dispersion in which infrared absorbing fine particles are dispersed in a medium in Patent Document 1. Specifically, as the infrared absorbing fine particles, fine particles of tungsten oxide represented by the general formula WyOz (where W is tungsten, O is oxygen, 2.2≦z / y≦2.999) and / or fine particles of tungsten oxide represented by the general formula MxWyOz (where M is H, He, an alkali metal, an alkaline earth metal, a rare earth element, Mg, Zr, Cr, Mn, Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zn, Cd, Al, Ga, In, The present invention discloses an infrared absorbing microparticle dispersion comprising microparticles of a composite tungsten oxide represented by the formula: Tl, Si, Ge, Sn, Pb, Sb, B, F, P, S, Se, Br, Te, Ti, Nb, V, Mo, Ta, Re, Be, Hf, Os, Bi, and I, where W is tungsten and O is oxygen, and 0.001≦x / y≦1, 2.2≦z / y≦3.0), having a particle diameter of 1 nm or more and 800 nm or less.
[0004] In the infrared absorbing fine particles of Patent Document 1, the surface decomposes upon contact with moisture, causing the infrared transmittance to increase over time, and the infrared absorbing properties inherent to the infrared absorbing fine particles may not be maintained.
[0005] Therefore, in Patent Document 2, the present inventors disclose a technique for coating the surface of infrared absorbing particles with a tetrafunctional silane compound or a partial hydrolysis product thereof, and / or an organometallic compound in order to improve the water resistance of the infrared absorbing particles.
[0006] In addition, since the infrared absorber is used outdoors, the infrared absorbing fine particles are required to have excellent resistance to long-term exposure to a humid and hot atmosphere (humid and heat resistance) as well as water resistance. The humid and heat resistance means that even when the infrared absorber is exposed to a humid and hot atmosphere for a long period of time, the change in infrared transmittance before and after exposure is small, and the infrared absorbing properties can be maintained at a high level.
[0007] In this regard, the present inventors have disclosed in Patent Document 3 a technique for improving the moist heat resistance of the infrared absorbing fine particles of Patent Document 2. Specifically, the technique discloses coating the surface of the infrared absorbing fine particles with a hydrolysis product of a metal chelate compound or a cyclic metal oligomer compound or a polymer thereof. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] International Publication No. 2005 / 37932 [Patent Document 2] WO 2010 / 55570 [Patent Document 3] International Publication No. 2019 / 093524 Summary of the Invention [Problem to be solved by the invention]
[0009] However, the infrared absorbing fine particles are required to have higher resistance to moist heat, and further improvements are required. Specifically, it is required that the infrared absorbing fine particle dispersion can maintain high infrared absorbing properties for a longer period of time when exposed to a moist heat atmosphere.
[0010] An object of the present invention is to provide a technique for improving the moist heat resistance of infrared absorbing fine particles while maintaining excellent infrared absorbing properties. [Means for solving the problem]
[0011] The first aspect of the present invention is The present invention comprises infrared absorbing particles and a coating film containing a hydrate of a metal oxide formed so as to cover the surface of the particles, The carbon concentration is 5.0% by mass or less when measured by a combustion-infrared absorption method. These are surface-treated infrared absorbing particles.
[0012] A second aspect of the present invention is the first aspect, wherein the metal oxide contains one or more metal elements selected from Al, Zr, Ti, Si and Zn.
[0013] A third aspect of the present invention is the infrared absorbing nanoparticles according to the first or second aspect, wherein the infrared absorbing nanoparticles are selected from the group consisting of tungsten oxide nanoparticles represented by the general formula WyOz (wherein W is tungsten, O is oxygen, and 2.2≦z / y≦2.999), and tungsten oxide nanoparticles represented by the general formula MxWyOz (wherein M is H, He, an alkali metal, an alkaline earth metal, a rare earth element, Mg, Zr, Cr, Mn, Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, The component (A) is at least one of composite tungsten oxide nanoparticles represented by the formula: Cu, Ag, Au, Zn, Cd, Al, Ga, In, Tl, Si, Ge, Sn, Pb, Sb, B, F, P, S, Se, Br, Te, Ti, Nb, V, Mo, Ta, Re, Be, Hf, Os, Bi, I, and Yb, where W is tungsten and O is oxygen, and 0.001≦x / y≦1, 2.0≦z / y≦3.0).
[0014] A fourth aspect of the present invention is an infrared ray absorbing nanoparticle dispersion liquid comprising the surface-treated infrared ray absorbing nanoparticles of any one of the first to third aspects and a liquid medium.
[0015] A fifth aspect of the present invention is the liquid medium according to the fourth aspect, which is at least one of an organic solvent, an oil or fat, a liquid plasticizer, a compound that is polymerized by curing, and water.
[0016] A sixth aspect of the present invention is an infrared absorbing microparticle dispersion constituted by dispersing the surface-treated infrared absorbing microparticles according to any one of the first to third aspects in a solid resin.
[0017] A seventh aspect of the present invention is the sixth aspect, wherein the solid resin is at least one of a fluororesin, a PET resin, an acrylic resin, a polyamide resin, a vinyl chloride resin, a polycarbonate resin, an olefin resin, an epoxy resin, and a polyimide resin.
[0018] An eighth aspect of the present invention is a method for producing a composition comprising the steps of: A step of mixing infrared absorbing fine particles and water to obtain a dispersion for forming a coating film; adding a surface treatment agent containing a metal chelate compound to the coating film forming dispersion; and subjecting the dispersion liquid for forming a coating film to which the surface treatment agent has been added to a heat treatment, obtaining surface-treated infrared absorbing fine particles having a coating film containing a hydrate of a metal oxide derived from the metal chelate compound formed on the surface of the infrared absorbing fine particles; A method for producing surface-treated infrared absorbing particles.
[0019] A ninth aspect of the present invention is the eighth aspect, wherein the heat treatment is carried out at a temperature of 40° C. or more and 80° C. or less for 4 hours or more. Effect of the Invention
[0020] According to the present invention, it is possible to improve the moist heat resistance of infrared absorbing fine particles while maintaining excellent infrared absorbing properties. [Brief description of the drawings]
[0021] [Figure 1] FIG. 2 is a schematic plan view of a crystal structure in a composite tungsten oxide having a hexagonal crystal structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] <Findings of the present inventors> In order to solve the above-mentioned problems, the present inventors have investigated coating films for coating the surfaces of infrared absorbing fine particles, and have focused on metal chelate compounds as compounds for forming coating films. Metal chelate compounds generate hydrolysis products or their polymers by hydrolysis, and these products adhere to the surfaces of infrared absorbing fine particles to form coating films.
[0023] In addition to metal chelate compounds, compounds that form coating films include, for example, metal cyclic oligomer compounds. However, since metal cyclic oligomer compounds need to be dissolved in a low polarity solvent such as xylene or toluene, when water, which is a high polarity solvent, is added to hydrolyze the compound, the presence of the low polarity solvent may prevent the hydrolysis reaction from proceeding sufficiently. Therefore, carbon components derived from metal cyclic oligomer compounds may remain in the coating film. In contrast, metal chelate compounds do not need to use a low polarity solvent like metal cyclic oligomer compounds, and the hydrolysis reaction is easily promoted by adding water, so that the carbon components can be suppressed from remaining compared to metal cyclic oligomer compounds. Therefore, compared to metal cyclic oligomer compounds, metal chelate compounds have a higher affinity between the coating film and the infrared absorbing fine particles, and the coating film can be provided more uniformly on the surface of the infrared absorbing fine particles, so that a stronger coating film can be formed. As a result, metal chelate compounds can provide higher humidity and heat resistance.
[0024] However, it was confirmed that the coating film formed from the metal chelate compound increases in infrared transmittance over time when exposed to a moist heat atmosphere for a long period of time, and the desired infrared absorption characteristics cannot be maintained for a long period of time. In particular, it was confirmed that the transmittance of infrared rays with wavelengths of 800 nm to 1000 nm increases significantly. In other words, it was confirmed that there is room for improvement in the moist heat resistance of the coating film formed from the metal chelate compound.
[0025] According to the study by the present inventors, it was found that carbon components derived from hydrolysis products and their polymers remain in the coating film formed from the metal chelate compound, and the higher the concentration of these, the lower the moist heat resistance tends to be. Although the mechanism is unclear, it is speculated that the carbon components prevent the coating film from being dense or high-density, which results in a decrease in moist heat resistance.
[0026] For this reason, we have investigated methods for reducing the carbon content in the coating film, and have focused on a method in which a coating film made of a hydrolysis product or its polymer is formed and then subjected to a heat treatment.
[0027] According to the heat treatment, the hydrolysis products and polymers contained in the coating film can be further hydrolyzed to form metal oxide hydrates, and the coating film can be configured to contain metal oxide hydrates. In other words, the content of the hydrolysis products and polymers in the coating film can be reduced, and the carbon components derived therefrom can be reduced. As a result of further investigation, it was found that by configuring the coating film to have a predetermined concentration of carbon components, the surface-treated infrared-absorbing fine particles can maintain their inherent infrared absorbing properties while improving their moist heat resistance.
[0028] The present invention has been made based on the above findings.
[0029] <One embodiment> Hereinafter, one embodiment of the present invention will be described.
[0030] <1> Surface-treated infrared absorbing particles The surface-treated infrared absorbing particles of this embodiment include infrared absorbing particles and a coating film.
[0031] <1-1> Infrared absorbing particles Infrared absorbing particles include various materials containing free electrons, and are particles that show a reflection / absorption response to electromagnetic waves around the range of sunlight with wavelengths of 200 nm to 2600 nm due to plasma vibration (having infrared absorbing properties). For example, by having a particle diameter smaller than the wavelength of light, infrared absorbing particles can reduce geometric scattering in the visible light range (wavelengths of 380 nm to 780 nm), and can obtain particularly high transparency in the visible light range. Note that "transparency" here refers to "low scattering and high transmittance for light in the visible light range."
[0032] As the infrared absorbing particles, known particles can be used, but from the viewpoint of obtaining high infrared absorbing properties while ensuring transparency, it is preferable to use at least one of tungsten oxide particles and composite tungsten oxide particles. These infrared absorbing particles absorb a lot of light in the near infrared region, especially in the vicinity of 1000 nm in wavelength, so the transmitted color tone is often blue to green. Each particle will be described below.
[0033] (Tungsten oxide particles) The tungsten oxide particles are composed of WO3 having oxygen deficiencies and are particles of tungsten oxide expressed by the general formula WyOz (where W is tungsten and O is oxygen).
[0034] In the tungsten oxide represented by the general formula WyOz, the composition range of tungsten and oxygen is preferably such that the composition ratio of oxygen to tungsten is less than 3, and further, when the infrared absorbing fine particles are described as WyOz, 2.2≦z / y≦2.999 is preferable. If the value of z / y is 2.2 or more, it is possible to avoid the appearance of the crystal phase of WO2, which is not the intended purpose, in the tungsten oxide, and it is possible to obtain chemical stability as a material, so that it is an effective infrared absorbing fine particle. On the other hand, if the value of z / y is 2.999 or less, the required amount of free electrons is generated, and it is an efficient infrared absorbing fine particle.
[0035] (Composite tungsten oxide particles) Composite tungsten oxide microparticles are composed of tungsten oxide (WO3) with the addition of an electropositive element (hereinafter also referred to as M element) that generates free electrons, and are composite tungsten oxide microparticles expressed by the general formula MxWyOz (where M is an electropositive element, W is tungsten, and O is oxygen). Composite tungsten oxide microparticles exhibit infrared absorption characteristics by controlling the amount of oxygen and adding element M, and show particularly strong absorption characteristics around 1000 nm.
[0036] In addition, in the composite tungsten oxide microparticles, element M is not particularly limited as long as it can generate free electrons, but is preferably one or more elements selected from H, He, alkali metals, alkaline earth metals, rare earth elements, Mg, Zr, Cr, Mn, Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zn, Cd, Al, Ga, In, Tl, Si, Ge, Sn, Pb, Sb, B, F, P, S, Se, Br, Te, Ti, Nb, V, Mo, Ta, Re, Be, Hf, Os, Bi, and I.
[0037] From the viewpoint of stability in MxWyOz, it is more preferable that the element M is one or more elements selected from alkali metals, alkaline earth metals, rare earth elements, Mg, Zr, Cr, Mn, Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zn, Cd, Al, Ga, In, Tl, Si, Ge, Sn, Pb, Sb, B, F, P, S, Se, Br, Te, Ti, Nb, V, Mo, Ta, and Re. Furthermore, from the viewpoint of improving the optical properties and weather resistance of the infrared absorbing fine particles, it is even more preferable that the element M belongs to an alkaline earth metal element, a transition metal element, a group 4B element, or a group 5B element.
[0038] In addition, in the composite tungsten oxide represented by the general formula MxWyOz, the composition ranges of the element M, tungsten, and oxygen are not particularly limited, but it is preferable that they satisfy the relationships of 0.001≦x / y≦1 and 2.0≦z / y≦3.
[0039] Regarding the above composition, first, the value of x / y, which indicates the amount of element M added, will be explained. If the value of x / y is 0.001 or more, a sufficient amount of free electrons is generated in the composite tungsten oxide, and the desired infrared absorption effect can be obtained. The more the amount of element M added, the more the supply of free electrons increases, and the infrared absorption efficiency also increases, but when the value of x / y is about 1, the effect also saturates. In addition, if the value of x / y is 1 or less, it is preferable because it is possible to avoid the generation of an impurity phase in the composite tungsten oxide microparticles.
[0040] Next, the value of z / y, which indicates the control of the amount of oxygen, will be described. Regarding the value of z / y, in the composite tungsten oxide represented by MxWyOz, the same mechanism as that of the tungsten oxide represented by WyOz described above works, and also in the case of z / y=3.0 or 2.0≦z / y≦2.2, the above-mentioned amount of added element M supplies free electrons. Therefore, 2.0≦z / y≦3.0 is preferable, 2.2≦z / y≦3.0 is more preferable, and 2.45≦z / y≦3.0 is even more preferable.
[0041] Moreover, from the viewpoint of improving the transmittance in the visible light region and the infrared absorption characteristics, it is preferable that the composite tungsten oxide particles have a hexagonal crystal structure. This point will be explained with reference to Fig. 1. Fig. 1 is a schematic plan view of the crystal structure of a composite tungsten oxide having a hexagonal crystal structure.
[0042] In Fig. 1, six octahedra formed of WO6 units, as shown by reference numeral 11, are assembled to form a hexagonal gap, and an element M, as shown by reference numeral 12, is arranged in the gap to form one unit, and a large number of such units are assembled to form a hexagonal crystal structure. In order to obtain the effect of improving the transmission of light in the visible light region and improving the absorption of light in the infrared region, it is sufficient that the composite tungsten oxide microparticles contain the unit structure described with reference to Fig. 1, and the composite tungsten oxide microparticles may be crystalline or amorphous.
[0043] When the cations of element M are added to the hexagonal gaps, the transmission of light in the visible light region is improved, and the absorption of light in the infrared region is improved. Generally, when an element M with a large ionic radius is added, the hexagonal crystal is easily formed. Specifically, when Cs, K, Rb, Tl, In, Ba, Li, Ca, Sr, Fe, or Sn is added, the hexagonal crystal is easily formed. Elements other than these may be used as long as the above-mentioned element M is present in the hexagonal gaps formed by the WO6 units, and the elements are not limited to the above-mentioned elements.
[0044] When the composite tungsten oxide microparticles having a hexagonal crystal structure have a uniform crystal structure, the amount of the added element M is preferably 0.2 or more and 0.5 or less, more preferably 0.33, in terms of the value of x / y. When the value of x / y is 0.33, it is considered that the above-mentioned element M is arranged in all of the hexagonal voids.
[0045] The crystal structure of the composite tungsten oxide is not limited to hexagonal, and may be tetragonal or cubic. The absorption position in the infrared region tends to change depending on the crystal structure, and the absorption position tends to move to the long wavelength side in the order of cubic crystal < tetragonal crystal < hexagonal crystal. In addition, the absorption in the visible light region is small in the order of hexagonal crystal, tetragonal crystal, and cubic crystal. Therefore, it is preferable to use a composite tungsten oxide of hexagonal crystal for applications that transmit more light in the visible light region and absorb more light in the infrared region. However, the tendency of the optical characteristics described here is only a rough tendency, and changes depending on the type and amount of added element and the amount of oxygen, and the present invention is not limited to this.
[0046] In addition, among the composite tungsten oxide microparticles and the above-mentioned tungsten oxide microparticles, the so-called "Magneli phase" having a composition ratio expressed as 2.45≦z / y≦2.999 is chemically stable and has good absorption characteristics in the infrared region, and is therefore preferable as an infrared absorbing microparticle.
[0047] (Crystallite size) The crystallite size of the infrared absorbing fine particles is not particularly limited, but from the viewpoint of obtaining higher infrared absorbing properties, it is preferably 1 nm or more and 200 nm or less, more preferably 1 nm or more and 100 nm or less, and even more preferably 10 nm or more and 70 nm or less. Here, the crystallite size is measured by measuring the X-ray diffraction pattern by powder X-ray diffraction method (θ-2θ method) and analyzing by the Rietveld method. The X-ray diffraction pattern can be measured, for example, by using a powder X-ray diffractometer "X'Pert-PRO / MPD" manufactured by PANalytical, Spectris Co., Ltd.
[0048] <1-2>Coating film The coating film is formed so as to cover the surface of the infrared absorbing fine particles, and improves the moist heat resistance of the infrared absorbing fine particles. As described above, the coating film is formed by heat-treating the hydrolysis product obtained by hydrolyzing the metal chelate compound or its polymer, and is composed of a metal oxide hydrate derived from the metal chelate compound. In addition to the metal oxide hydrate, the coating film may also contain a metal oxide from which water has been eliminated. In the following, the film formed on the surface of the infrared absorbing fine particles before heat treatment is called the attached film, and the attached film subjected to heat treatment is called the coated film.
[0049] The metal chelate compound has a metal and a hydrolyzed structure. The metal chelate compound becomes a hydrolyzed product in which a part or all of the hydrolyzed structure becomes a hydroxyl group or a carboxyl group through a hydrolysis reaction, or becomes a polymerized product through self-condensation through a hydrolysis reaction. The hydrolyzed product or polymerized product adheres to the surface of the infrared absorbing fine particles, thereby forming an attached film containing the hydrolyzed product or polymerized product. In this embodiment, the infrared absorbing fine particles covered with this attached film are subjected to a heat treatment. The heating promotes the hydrolysis reaction of the hydrolyzed product or polymerized product contained in the attached film, thereby generating a hydrate of a metal oxide derived from the metal chelate compound. This makes it possible to obtain a coating film containing a hydrate of a metal oxide.
[0050] The metal oxide hydrate contained in the coating film contains a metal element derived from a metal chelate compound. The metal element contained in the metal oxide hydrate is not particularly limited, but from the viewpoint of wet heat resistance, it is preferable that the metal oxide hydrate contains one of aluminum (Al), zirconium (Zr), titanium (Ti), silicon (Si) and zinc (Zn). Specifically, the metal oxide hydrate preferably contains one or more of alumina hydrate, zirconia hydrate, titania hydrate, silica hydrate and zinc oxide hydrate.
[0051] In the coating film, not only hydrates of metal oxides but also hydrolysis products and polymers may remain. Hydrolysis products and polymers contain carbon components, but in this embodiment, the amount of hydrolysis products and polymers can be reduced, so that the carbon concentration in the coating film can be reduced. Specifically, the carbon concentration in the coating film can be 5.0 mass% or less. It is preferably 3.5 mass% or less, more preferably 3.0 mass% or less, and even more preferably 2.5 mass% or less. By setting the carbon concentration within the above range, the coating film can be formed more densely and the desired moist heat resistance can be obtained. The lower limit is not particularly limited, but is 0.01 mass%. The carbon concentration in the coating film is measured using a carbon analyzer based on the principle of combustion-infrared absorption method. For example, a carbon analyzer "CS-600" manufactured by LECO Co., Ltd. can be used.
[0052] In addition, since the coating film mainly contains hydrates of metal oxides, the content of water derived from the hydrates is preferably 0.50% by mass or more and 10% by mass or less, and more preferably 1.0% by mass or more and 8.0% by mass or less.
[0053] Here, the content of water derived from hydrates will be described. The water contained in the coating film comes not only from hydrates, but also from hydrolysis products and polymers that remain after incomplete hydrolysis. Hydrolysis products contain, for example, hydroxyl groups, which may be detected as water in analysis using a thermal analyzer. Therefore, the water content h derived from hydrates is calculated by subtracting the water content derived from hydrolysis products having hydroxyl groups from the water content in the coating film. The content of water derived from the hydrolysis product is calculated as c / (x×12)×y×18 from the carbon concentration c [mass%] contained in the coating film, the number of carbon atoms x contained in the hydrolysis product, and the number of water molecules y generated when the hydrolysis product is thermally analyzed. x and y are appropriately changed according to the type of metal chelate compound used, that is, according to the type of hydrolysis product generated. Meanwhile, the content of water contained in the coating film is measured by thermally analyzing the surface infrared absorbing particles. Then, the content of water derived from the hydrate h can be calculated by subtracting the content of water derived from the hydrolysis product from the content of water contained in the coating film. The specific calculation will be described in detail in the examples described later.
[0054] The thickness of the coating film is not particularly limited, but is preferably 0.5 nm to 100 nm, more preferably 0.5 nm to 20 nm, and even more preferably 1 nm to 10 nm. By making it 0.5 nm or more, the desired moist heat resistance can be obtained in the surface-treated infrared absorbing fine particles. On the other hand, by making it 100 nm or less, the optical properties such as transparency and infrared absorbing properties can be ensured in the surface-treated infrared absorbing fine particles.
[0055] The thickness of the coating film can be calculated from the content of the coating film estimated from the amount of the metal chelate compound added, the specific gravity of the coating film, and the BET specific surface area of the infrared absorbing fine particles. For example, the content of the coating film per 100 parts by mass of the infrared absorbing fine particles calculated from the amount of the metal chelate compound added is x parts by mass, and the specific gravity of the coating film is d [g / cm 3 ], and the BET specific surface area of the infrared absorbing particles is S[m 2 / g], the thickness t [nm] of the coating film is calculated by t = (x × 10) / (S × d). Here, the specific gravity d of the coating film is measured by adding only the metal chelate compound to water, carrying out the same operations as the surface treatment and heat treatment described later, obtaining a hydrate powder consisting of a hydrate of a metal oxide, and using the obtained powder. For example, the specific gravity of alumina hydrate is 2.5 g / cm 3 , zirconia hydrate is 3.5 g / cm 3 , titania hydrate is 2.6 g / cm 3 , silica hydrate is 2.0 g / cm 3 , zinc oxide hydrate is 3.5g / cm 3 It is.
[0056] The metal chelate compound for forming the coating film has a metal and a hydrolysis structure, and forms a hydrolysis product that can be attached to the surface of the infrared absorbing fine particles by hydrolysis. The metal contained in the metal chelate compound preferably contains any one of Al, Zr, Ti, Si and Zn from the viewpoint of improving the wet heat resistance of the surface-treated infrared absorbing fine particles. In addition, the hydrolysis structure preferably has one or more selected from an ether bond, an ester bond, an alkoxy group and an acetyl group. Specifically, it is preferably any one of a metal alkoxide, a metal acetylacetonate and a metal carboxylate.
[0057] Specifically, the following metal chelate compounds can be used:
[0058] Examples of aluminum-based chelate compounds include aluminum alcoholates such as aluminum ethylate, aluminum isopropylate, aluminum sec-butylate, and mono-sec-butoxyaluminum diisopropylate, or polymers thereof, ethyl acetoacetate aluminum diisopropylate, aluminum tris(ethyl acetoacetate), octyl acetoacetate aluminum diisopropylate, stearyl acetoaluminum diisopropylate, aluminum monoacetylacetonate bis(ethyl acetoacetate), aluminum tris(acetylacetonate), and the like. These compounds are alkoxy-containing aluminum chelate compounds obtained by dissolving aluminum alcoholate in an aprotic solvent, a petroleum solvent, a hydrocarbon solvent, an ester solvent, a ketone solvent, an ether solvent, an amide solvent, or the like, adding a β-diketone, a β-ketoester, a monohydric or polyhydric alcohol, a fatty acid, or the like to the solution, heating under reflux, and subjecting the solution to a ligand substitution reaction.
[0059] Examples of zirconia-based chelate compounds include zirconium alcoholates such as zirconium ethylate and zirconium butyrate, or polymers thereof, zirconium tributoxystearate, zirconium tetraacetylacetonate, zirconium tributoxyacetylacetonate, zirconium dibutoxybis(acetylacetonate), zirconium tributoxyethylacetoacetate, zirconium butoxyacetylacetonate bis(ethylacetoacetate), and the like.
[0060] Examples of titanium-based chelate compounds include titanium alcoholates such as methyl titanate, ethyl titanate, isopropyl titanate, butyl titanate, and 2-ethylhexyl titanate, and polymers thereof, titanium acetylacetonate, titanium tetraacetylacetonate, titanium octylene glycolate, titanium ethylacetoacetate, titanium lactate, and titanium triethanolamine.
[0061] As the silicon-based chelate compound, a tetrafunctional silane compound represented by the general formula: Si(OR)4 (wherein R is the same or different monovalent hydrocarbon group having 1 to 6 carbon atoms) or a hydrolysis product thereof can be used. Specific examples of the tetrafunctional silane compound include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetrabutoxysilane, etc. Furthermore, it is also possible to apply silane monomers in which a part or all of the alkoxy groups of these alkoxysilane monomers are hydrolyzed to form silanol (Si-OH) groups, and polymers self-condensed through a hydrolysis reaction. Furthermore, the hydrolysis product of the tetrafunctional silane compound (there is no appropriate terminology to indicate the entire intermediate of the tetrafunctional silane compound) includes a silane monomer in which a part or all of the alkoxy groups are hydrolyzed to become a silanol (Si-OH) group. Note that not all of the alkoxysilyl groups (Si-OR) in the alkoxysilane monomer are hydrolyzed to become silanol (Si-OH) during the hydrolysis reaction.
[0062] Preferred examples of zinc-based chelate compounds include zinc salts of organic carboxylates such as zinc octylate, zinc laurate, and zinc stearate, zinc acetylacetone chelate, zinc benzoylacetone chelate, zinc dibenzoylmethane chelate, and zinc acetoacetate chelate.
[0063] Among the above metal chelate compounds, those containing Al are particularly preferred. With Al-based metal chelate compounds, the hydrolysis reaction is not as fast as Ti-based or Zn-based compounds, and is faster than Zr-based compounds, so the hydrolysis reaction is easy to control and it is easy to form a uniform coating film on the surface of the infrared absorbing fine particles. As a result, the coating film has higher moist heat resistance and can be formed stably. Moreover, the production cost can be reduced, and the safety is also excellent.
[0064] <2> Method for producing surface-treated infrared absorbing particles Next, a method for producing the above-mentioned surface-treated infrared absorbing fine particles will be described.
[0065] <2-1> Preparation of infrared absorbing nanoparticle dispersion for forming coating film First, a fine particle powder containing infrared absorbing fine particles is added to a liquid medium and dispersed to prepare an infrared absorbing fine particle dispersion for forming a coating film (hereinafter also referred to as a dispersion for forming a coating film). Here, it is preferable to finely grind the fine particle powder beforehand and then add it to the liquid medium. Alternatively, it is preferable to add the fine particle powder to the liquid medium and then subject it to a grinding and dispersion treatment. This makes it possible to suppress the aggregation of the infrared absorbing fine particles and to monodisperse the infrared absorbing fine particles in the liquid medium. As a result, when forming a coating film, a uniform coating film can be formed on each infrared absorbing fine particle.
[0066] Water is used as the liquid medium used in the dispersion for forming the coating film. When water is used, the hydrolysis reaction of the metal chelate compound can be immediately started when the metal chelate compound is added to the dispersion for forming the coating film. To be more specific, the hydrolysis structure in the metal chelate compound contains a substituent that is easily hydrolyzed with a small amount of water and a substituent that is hydrolyzed with a large amount of water. For example, in the case of aluminum ethyl acetoacetate diisopropylate, which is a metal chelate compound, the isopropoxy group can be hydrolyzed with a small amount of water to become aluminum ethyl acetoacetate dihydroxide, while the substituent containing ethyl acetoacetate tends to be hydrolyzed only with a large amount of water. When such a metal chelate compound is added to an organic solvent as a liquid medium and then hydrolyzed, only a part of the hydrolysis structure in the metal chelate compound may be hydrolyzed, and the entire structure may not be hydrolyzed. As a result, carbon components derived from the substituents that cannot be hydrolyzed remain in the coating film, and the carbon concentration in the coating film tends to be high. On the other hand, by using water as the liquid medium, the hydrolysis structure can be hydrolyzed more reliably, the carbon components remaining in the coating film can be reduced, and the carbon concentration can be lowered. As a result, the coating film can be formed with a high density and fineness.
[0067] In addition, the amount of the infrared absorbing particles added to the coating film-forming dispersion liquid is not particularly limited, but it is preferable to adjust the concentration of the infrared absorbing particles dispersed in the liquid medium to 0.01% by mass or more and 80% by mass or less. By adjusting the concentration, the pH of the coating film-forming dispersion liquid can be set to 8 or less, and the infrared absorbing particles can be easily maintained in a dispersed state in the liquid medium by electrostatic repulsion.
[0068] Specific methods for pulverizing and dispersing fine powders include, for example, pulverizing and dispersing methods using devices such as bead mills, ball mills, sand mills, paint shakers, ultrasonic homogenizers, etc. Among these, pulverizing and dispersing methods using media such as beads, balls, and Ottawa sand, such as media agitation mills such as bead mills, ball mills, sand mills, and paint shakers, are preferred because they allow the desired dispersed particle size to be reached in a short time.
[0069] <2-2> Preparation of surface treatment agent Next, a surface treatment agent containing a metal chelate compound is prepared.
[0070] As the surface treatment agent, the metal chelate compound may be used as it is, but when added to the dispersion liquid for forming a coating film, the metal chelate compound may be diluted with a solvent to adjust the amount added per time. The solvent used for dilution is preferably one that does not react with the metal chelate compound and has high compatibility with the liquid medium contained in the dispersion liquid for forming a coating film. Specifically, alcohol-based, ketone-based, glycol-based, etc. can be preferably used. The dilution ratio is not particularly limited, but from the viewpoint of ensuring productivity, the dilution ratio is preferably 100 times or less.
[0071] <2-3> Addition of surface treatment agent Next, a predetermined amount of a surface treatment agent containing a metal chelate compound is added to the dispersion for forming a coating film over a predetermined period of time. The metal chelate compound is added to the dispersion for forming a coating film and hydrolyzed to form a hydrolysis product or a polymer thereof. The hydrolysis product or polymer is attached to the surface of the infrared absorbing fine particles, thereby forming an attached film containing at least one of the hydrolysis product and the polymer thereof.
[0072] The surface treatment agent is preferably added while stirring and mixing the dispersion for forming the coating film. By stirring and mixing, the aggregation of the infrared absorbing fine particles can be suppressed and the monodispersed state can be maintained. This can suppress the formation of a coating film on the surface of the aggregate of the infrared absorbing fine particles, and can allow the hydrolysis product or polymer to adhere uniformly and firmly to the surface of each fine particle. As a result, the formation of coarse particles that reduce transparency can be suppressed, and a dense and high-density coating film can be formed.
[0073] The amount of the metal chelate compound added is preferably 0.1 parts by mass or more and 1000 parts by mass or less in terms of metal element relative to 100 parts by mass of infrared absorbing fine particles, more preferably 1 part by mass or more and 500 parts by mass or less, and even more preferably 10 parts by mass or more and 150 parts by mass or less. By making the amount added 0.1 parts by mass or more, the desired moist heat resistance can be obtained by the coating film. On the other hand, by making the amount added 1000 parts by mass or less, it is possible to avoid an excessive amount of metal oxide hydrate coating on the infrared absorbing fine particles. In addition, the improvement in moist heat resistance by the surface treatment does not saturate, and an improvement in the coating effect can be expected. Furthermore, by making the amount of metal oxide hydrate coating on the infrared absorbing fine particles excessive, it is possible to avoid the fine particles from easily granulating with each other through the metal oxide hydrate when the medium is removed. As a result, the decrease in transparency due to granulation can be suppressed, and good transparency can be ensured. Moreover, it is possible to avoid an increase in production cost due to an increase in the amount of addition and processing time caused by an excess of metal chelate compound.
[0074] When adding a metal chelate compound to the dispersion liquid for forming a coating film, the metal chelate compound may be decomposed into metal ions immediately after the addition starts, but as the addition time passes and the amount added increases to become a saturated aqueous solution, the decomposition into metal ions ends.
[0075] <2-4> Heat treatment Next, the dispersion liquid containing the infrared absorbing fine particles having the adhesion film formed on the surface is subjected to a heat treatment.
[0076] The heat treatment further hydrolyzes the hydrolysis products and polymers contained in the attached film to form metal oxide hydrates. The heat treatment increases the ratio of metal oxide hydrates in the coating film and reduces carbon components derived from hydrolysis products and the like. The heat treatment is performed so that the carbon concentration in the coating film is 5.0 mass% or less. This forms surface-treated infrared absorbing particles having a coating film containing metal oxide hydrates formed on the surface.
[0077] The heating temperature and heating time of the heat treatment may be appropriately adjusted. From the viewpoint of promoting the hydrolysis of the hydrolysis products and polymers while suppressing the deterioration of the infrared absorbing particles, the heating temperature is preferably 40°C or more and 80°C or less, more preferably 50°C or more and 70°C or less, and even more preferably 50°C or more and 60°C or less. In addition, the heating time is preferably 4 hours or more and 24 hours or less. With such a heating temperature and heating time, the amount of the hydrolysis products and polymers remaining in the coating film can be further reduced, the ratio of the metal oxide hydrate can be further increased, and the deterioration of the infrared absorbing properties due to the deterioration of the infrared absorbing particles can be suppressed.
[0078] The heat treatment is preferably carried out while stirring and mixing the dispersion liquid, which allows the coating film of each fine particle to be uniformly heat-treated, thereby ensuring uniformity in the quality of the coating film.
[0079] Specific examples of the heating treatment method include a method using a stand with a built-in resistance heater such as a hot plate, a container or kiln wrapped around a resistance heater such as a rubber heater, a thermostatic bath such as a water bath or oil bath, or a container or kiln wrapped around a heating medium pipe such as hot water or heated oil.
[0080] <2-5> Drying process Next, the dispersion liquid containing the surface-treated infrared absorbing microparticles obtained by the heat treatment is dried. Specifically, the dispersion liquid is dried by heating or drying under conditions that can avoid strong aggregation of the surface-treated infrared absorbing microparticles, or by vacuum fluidized drying or spray drying at a temperature of less than 100° C., for example. This results in a microparticle powder containing the surface-treated infrared absorbing microparticles.
[0081] In the treatment by vacuum fluidized drying, the drying and disintegration treatments are performed simultaneously under a reduced pressure atmosphere, so that the drying speed is fast and aggregation of the surface-treated infrared absorbing microparticles can be avoided. In addition, since the drying is performed under a reduced pressure atmosphere, the volatile components can be removed even at a relatively low temperature, and the amount of the remaining volatile components can be reduced to an extremely small amount. In addition, in the treatment by spray drying, secondary aggregation due to the surface force of the volatile components is unlikely to occur, and surface-treated infrared absorbing microparticles that are relatively free of secondary aggregation can be obtained without disintegration treatment.
[0082] The drying temperature is not particularly limited as long as it can remove water contained in the dispersion, but is preferably from 40° C. to 80° C., more preferably from 50° C. to 70° C., and even more preferably from 50° C. to 60° C. By carrying out the drying treatment at such a temperature, the hydrolysis of the hydrolysis products remaining in the coating film (such as products that have not been completely hydrolyzed to hydrates) can be promoted even during the drying treatment, so that the time for the heat treatment can be reduced and the production efficiency of the surface-treated infrared-absorbing microparticles can be further improved.
[0083] In this embodiment, the heating treatment and the drying treatment are performed separately, but the present invention is not limited thereto. For example, the drying treatment may be performed simultaneously with the heating treatment. In this case, the heating treatment corresponds to the temperature increase or constant temperature stage in the drying treatment. When the heating treatment and the drying treatment are performed separately, the hydrolysis product can be hydrolyzed more stably, whereas when the heating treatment and the drying treatment are performed simultaneously, the production process can be simplified and the production efficiency can be improved.
[0084] <3> Applications of surface-treated infrared absorbing particles The surface-treated infrared absorbing particles of the present embodiment can be used in the form of particles, or dispersed in a liquid medium or a solid medium. Hereinafter, the uses of the surface-treated infrared absorbing particles will be specifically described using examples of an infrared absorbing particle dispersion, an infrared absorbing particle dispersion, an infrared absorbing substrate, and an article using the infrared absorbing particle dispersion or the infrared absorbing substrate.
[0085] <3-1> Infrared absorbing nanoparticle dispersion The infrared ray absorbing microparticle dispersion liquid contains a microparticle powder including the above-mentioned surface-treated infrared ray absorbing microparticles, and a liquid medium, and is obtained by dispersing the microparticle powder in the liquid medium.
[0086] The infrared ray absorbing nanoparticle dispersion liquid can be prepared, for example, by adding the nanoparticle powder to a liquid medium and redispersing it. Alternatively, the infrared ray absorbing nanoparticle dispersion liquid can be prepared by replacing the liquid medium and carrying out solvent substitution, for example, by separating the surface-treated infrared ray absorbing nanoparticles from the dispersion liquid containing the above-mentioned surface-treated infrared ray absorbing nanoparticles and adding them to a liquid medium.
[0087] (Dispersed particle size) The particle size of the surface-treated infrared absorbing particles when the fine particle powder is dispersed in a liquid medium can be appropriately changed depending on the application of the infrared absorbing fine particle dispersion. For example, if the application requires transparency, the particle size is preferably 800 nm or less. By making the particle size 800 nm or less, the light is not completely blocked by scattering, and the visibility in the visible light region is maintained, and at the same time, the transparency is efficiently maintained.
[0088] In addition, when transparency in the visible light region is particularly important, it is preferable to further consider scattering by fine particles. From the viewpoint of reducing scattering by fine particles, the dispersed particle diameter is preferably 200 nm or less, and more preferably 100 nm or less. The reason for this is that if the dispersed particle diameter of the particles is small, scattering of light in the visible light region with a wavelength of 400 nm to 780 nm due to geometric scattering or Mie scattering is reduced, and it is possible to avoid the infrared absorbing film becoming like cloudy glass and not being able to obtain clear transparency. That is, when the dispersed particle diameter is 200 nm or less, geometric scattering or Mie scattering is reduced, and the Rayleigh scattering region is reached. In the Rayleigh scattering region, scattered light is reduced in proportion to the sixth power of the particle diameter, so that scattering is reduced and transparency is improved as the dispersed particle diameter decreases.
[0089] Furthermore, if the dispersed particle size is 100 nm or less, the scattered light is very little, which is preferable. From the viewpoint of avoiding light scattering, the dispersed particle size is preferably small, and if the dispersed particle size is 1 nm or more, industrial production is easy.
[0090] By setting the dispersed particle diameter to 800 nm or less, the haze value of the infrared absorbing nanoparticle dispersion in which the infrared absorbing nanoparticles are dispersed in a liquid medium can be set to 30% or less with a visible light transmittance of 85% or less. If the haze value is greater than 30%, the product becomes like cloudy glass and clear transparency cannot be obtained.
[0091] The dispersed particle size can be measured using an instrument based on the dynamic light scattering method, such as ELS-8000 manufactured by Otsuka Electronics Co., Ltd.
[0092] (Liquid medium) The liquid medium may be one or more liquid media selected from organic solvents, oils and fats, liquid plasticizers, compounds that become polymerized by curing, and water.
[0093] As the organic solvent, an alcohol-based, ketone-based, hydrocarbon-based, glycol-based, water-based, etc., can be used. Specifically, alcohol-based solvents such as methanol, ethanol, 1-propanol, isopropanol, butanol, pentanol, benzyl alcohol, and diacetone alcohol; Ketone solvents such as acetone, methyl ethyl ketone, dimethyl ketone, methyl propyl ketone, methyl isobutyl ketone, cyclohexanone, and isophorone; Ester solvents such as 3-methyl-methoxy-propionate, n-butyl acetate; Glycol derivatives such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol isopropyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol methyl ether acetate, and propylene glycol ethyl ether acetate; Amides such as formamide, N-methylformamide, dimethylformamide, dimethylacetamide, and N-methyl-2-pyrrolidone; Aromatic hydrocarbons such as toluene and xylene; Ethylene chloride, chlorobenzene, etc. can be used. Among these organic solvents, dimethyl ketone, methyl ethyl ketone, methyl isobutyl ketone, toluene, propylene glycol monomethyl ether acetate, n-butyl acetate, and the like can be preferably used.
[0094] The oil is preferably a vegetable oil or a vegetable-derived oil. Examples of vegetable oils that can be used include drying oils such as linseed oil, sunflower oil, tung oil, and perilla oil; semi-drying oils such as sesame oil, cottonseed oil, rapeseed oil, soybean oil, rice bran oil, and poppy oil; and non-drying oils such as olive oil, coconut oil, palm oil, and dehydrated castor oil. As the compound derived from vegetable oil, fatty acid monoesters, ethers, etc., which are obtained by directly esterifying fatty acids of vegetable oil with monoalcohols, can be used. Commercially available petroleum-based solvents can also be used as the oil. Commercially available petroleum-based solvents that can be used include Isopar (registered trademark) E, Exxor (registered trademark) Hexane, Heptane, E, D30, D40, D60, D80, D95, D110, and D130 (all manufactured by ExxonMobil).
[0095] Examples of the liquid plasticizer that can be used include a plasticizer that is a compound of a monohydric alcohol and an organic acid ester, an ester-based plasticizer such as a polyhydric alcohol organic acid ester compound, a phosphoric acid-based plasticizer such as an organic phosphoric acid-based plasticizer, etc. It is preferable that any of these plasticizers is liquid at room temperature. Among them, the plasticizer that is an ester compound synthesized from polyhydric alcohol and fatty acid can be preferably used.The ester compound synthesized from the polyhydric alcohol and fatty acid is not particularly limited, but for example, the glycol-based ester compound obtained by reacting glycol such as triethylene glycol, tetraethylene glycol, tripropylene glycol with monobasic organic acid such as butyric acid, isobutyric acid, caproic acid, 2-ethylbutyric acid, heptyl acid, n-octylic acid, 2-ethylhexyl acid, pelargonic acid (n-nonylic acid), decyl acid, etc. can be used. Further examples include ester compounds of tetraethylene glycol or tripropylene glycol with the above-mentioned monobasic organic solvents. Among them, fatty acid esters of triethylene glycol such as triethylene glycol dihexanate, triethylene glycol di-2-ethylbutyrate, triethylene glycol di-octanate, triethylene glycol di-2-ethylhexanoate, etc. can be used. Furthermore, fatty acid esters of triethylene glycol can also be preferably used.
[0096] The compound to be polymerized by curing is a monomer or oligomer that forms a polymer by polymerization, etc. Specifically, a methyl methacrylate monomer, an acrylate monomer, a styrene resin monomer, etc. can be used.
[0097] The liquid mediums described above can be used in combination of two or more kinds. Furthermore, if necessary, an acid or an alkali may be added to these liquid media to adjust the pH.
[0098] (Other additives) If necessary, the infrared absorbing nanoparticle dispersion may contain additives other than those mentioned above, such as a dispersant, a surfactant, a coupling agent, etc. These additives can further improve the dispersion stability of the surface-treated infrared absorbing nanoparticles and prevent the dispersed particles from becoming coarse due to re-aggregation.
[0099] The dispersant, coupling agent, and surfactant can be selected according to the application, but it is preferable that they have an amine-containing group, a hydroxyl group, a carboxyl group, a sulfo group, or an epoxy group as a functional group. These functional groups adsorb to the surface of the surface-treated infrared absorbing particles, preventing agglomeration and dispersing them uniformly. Polymer dispersants having any of these functional groups in the molecule are more preferable.
[0100] In addition, acrylic-styrene copolymer-based dispersants having functional groups are also preferred. Among them, acrylic-styrene copolymer-based dispersants having a carboxyl group as a functional group and acrylic-based dispersants having an amine-containing group as a functional group are more preferred. Dispersants having an amine-containing group as a functional group preferably have a molecular weight Mw of 2000 to 200000 and an amine value of 5 to 100 mgKOH / g. In addition, dispersants having a carboxyl group preferably have a molecular weight Mw of 2000 to 200000 and an acid value of 1 to 50 mgKOH / g.
[0101] Specific examples of commercially available dispersants include SOLSPERSE (registered trademark) 3000, 5000, 9000, 11200, 12000, 13000, 13240, 13650, 13940, 16000, 17000, 18000, 20000, 21000, 24000SC, 24000GR, 26000, 27000, and 280 manufactured by Lubrizol Japan. 00, 31845, 32000, 32500, 32550, 32600, 33000, 33500, 34750, 35100, 35200, 36600, 37500, 38500, 39000, 41000, 41090, 53095, 55000, 56000, 71000, 76500, J180, J200, M387, etc.; SOLPLUS (registered trademark) (hereinafter the same) D5 10, D520, D530, D540, DP310, K500, L300, L400, R700, etc.; Disperbyk (registered trademark) manufactured by BYK Japan (hereinafter the same) -101, 102, 103, 106, 107, 108, 109, 110, 111, 112, 116, 130, 140, 142, 145, 154, 161, 162, 163, 164, 165, 16 6, 167, 168, 170, 171, 174, 180, 181, 182, 183, 184, 185, 190, 191, 192, 2000, 2001, 2009, 2020, 2025, 2050, 2070, 2095, 2096, 2150, 2151, 2152, 2155, 2163, 2164, Anti-Terra (registered trademark) (hereinafter the same)-U, 203, 204, etc.;BYK (registered trademark) (hereinafter the same)-P104, P104S, P105, P9050, P9051, P9060, P9065, P9080, 051, 052, 053, 054, 055, 057, 063, 065, 066N, 067A, 077, 088, 141, 220S, 300, 302, 306, 307, 310, 315, 320, 322, 323, 325, 330, 331, 333, 337, 340, 345, 346, 347, 348, 350, 354, 355, 358N, 361N, 370, 375, 377, 378, 380N, 381, 392, 410, 425, 430, 1752, 4510, 6919, 9076, 9077, W909, W935, W940, W961, W966, W969, W972, W980, W985, W995, W996, W9010, D ynwet800, Cyclean3700, UV3500, UV3510, UV3570, etc.; EFKA Additives' EFKA (registered trademark) (hereinafter the same) 2020, 2025, 3030, 3031, 3236, 4008, 4009, 4010, 4015, 4020, 4046, 4047, 4050, 4055, 4060, 4080, 4300, 4310, 4320, 4330, 43 40, 4400, 4401, 4402, 4403, 4500, 5066, 5220, 6220, 6225, 6230, 6700, 6780, 6782, 7462, 8503, etc.; JONCRYL (registered trademark) manufactured by BASF Japan Ltd. (hereinafter the same); 67, 678, 586, 611, 680, 682, 690, 819, -JDX5050, etc.; TERPLUS (registered trademark) manufactured by Otsuka Chemical Co., Ltd. (hereinafter the same) MD1000, D 1180, D 1130, etc.; Ajisper (registered trademark) (hereinafter the same) PB-711, PB-821, PB-822, etc., manufactured by Ajinomoto Fine-Techno Co., Ltd.; Disparlon (registered trademark) (hereinafter the same) 1751N, 1831, 1850, 1860, 1934, DA-400N, DA-703-50, DA-325, DA-375, DA-550, DA-705, DA-725, DA-1401, DA-7301, DN-900, NS-5210, NVI-8514L, etc., manufactured by Kusumoto Chemicals Co., Ltd.;Examples of such products include Arphon (registered trademark) (hereinafter the same) UH-2170, UC-3000, UC-3910, UC-3920, UF-5022, UG-4010, UG-4035, UG-4040, and UG-4070, and Reseda (registered trademark) (hereinafter the same) GS-1015, GP-301, and GP-301S, manufactured by Toagosei Co., Ltd.; and Dianale (registered trademark) (hereinafter the same) BR-50, BR-52, BR-60, BR-73, BR-77, BR80, BR-83, BR-85, BR-87, BR-88, BR-90, BR-96, BR-102, BR-113, and BR-116, manufactured by Mitsubishi Chemical Corporation.
[0102] (Method of using infrared absorbing nanoparticle dispersion liquid) The infrared ray absorbing nanoparticle dispersion liquid can be used as an infrared ray absorbing substrate by applying the infrared ray absorbing nanoparticle dispersion liquid to the surface of a suitable substrate to form a dispersion film thereon. In other words, the dispersion film is a kind of a dried solidified product of the infrared ray absorbing nanoparticle dispersion liquid.
[0103] Moreover, the infrared-absorbing microparticle dispersion liquid can be dried and pulverized to obtain a powdered infrared-absorbing microparticle dispersion (hereinafter also referred to as a dispersed powder). In other words, the dispersed powder is a type of dried solidified product of the infrared-absorbing microparticle dispersion liquid. The dispersed powder is a powdered dispersion in which surface-treated infrared-absorbing microparticles are dispersed in a solid medium (such as a dispersant), and is distinguished from the above-mentioned surface-treated infrared-absorbing microparticle powder. Since the dispersed powder contains a dispersant, it is possible to easily redisperse the surface-treated infrared-absorbing microparticles in the medium by mixing with an appropriate medium.
[0104] The dispersed powder can be used as a raw material for adding the surface-treated infrared-absorbing microparticles in a dispersed state to an infrared-absorbing product. That is, the dispersed powder in which the surface-treated infrared-absorbing microparticles are dispersed in a solid medium may be dispersed again in a liquid medium and used as a dispersion liquid for an infrared-absorbing product, or the dispersed powder may be kneaded into a resin as described below.
[0105] On the other hand, infrared absorbing nanoparticle dispersions are used in various applications that utilize light-to-heat conversion.
[0106] For example, the curable ink composition can be obtained by adding the surface-treated infrared absorbing particles to an uncured thermosetting resin, or by dispersing the surface-treated infrared absorbing particles in a suitable solvent and then adding the uncured thermosetting resin. The curable ink composition is provided on a predetermined substrate and has excellent adhesion to the substrate when it is cured by irradiating electromagnetic waves such as infrared rays. At this time, the surface-treated infrared absorbing particles act as an auxiliary agent that increases the amount of heat generated by infrared irradiation. In addition to the use as a conventional ink, the curable ink composition is also an optimal curable ink composition for a stereolithography method in which a predetermined amount is applied, irradiated with electromagnetic waves such as infrared rays, cured, and piled up to form a three-dimensional object.
[0107] For example, the thermoplastic resin-containing ink composition can be obtained by adding the surface-treated infrared absorbing fine particles to a thermoplastic resin that has been heated and melted, or by dispersing the surface-treated infrared absorbing fine particles in a suitable solvent and then adding a thermoplastic resin that is highly soluble in the solvent. The thermoplastic resin-containing ink composition is provided on a predetermined substrate, and adheres to the substrate through the removal of the solvent by irradiation with electromagnetic waves such as infrared rays and the heat fusion of the resin. At this time, the surface-treated infrared absorbing fine particles act as an auxiliary agent that increases the amount of heat generated by infrared irradiation. In addition to the use as a conventional ink, the thermoplastic resin-containing ink composition can be applied in a predetermined amount, and then repeatedly irradiated with electromagnetic waves such as infrared rays to remove the solvent and heat fusion of the resin, thereby forming a three-dimensional object, making it an optimal thermoplastic resin-containing ink composition for the stereolithography method.
[0108] <3-2> Infrared absorbing nanoparticle dispersion The infrared absorbing nanoparticle dispersion contains surface-treated infrared absorbing nanoparticles and a solid medium, and is obtained by dispersing the surface-treated infrared absorbing nanoparticles in the solid medium.
[0109] As the solid medium, for example, a solid medium such as resin or glass can be used. The type of resin is not particularly limited and can be appropriately selected depending on the application. For example, PET resin, acrylic resin, polyamide resin, vinyl chloride resin, polycarbonate resin, olefin resin, epoxy resin, polyimide resin, etc. can be used as a low-cost, highly transparent and versatile resin. Also, fluororesin can be used in consideration of weather resistance.
[0110] The amount of filler relative to the solid medium (i.e., the amount of surface-treated infrared-absorbing microparticles) can be appropriately changed depending on the thickness of the substrate and the required optical and mechanical properties, but is generally preferably 50% by mass or less relative to the solid medium. If it is 50% by mass or less, granulation between the microparticles in the solid medium can be suppressed, so good transparency can be maintained. In addition, the amount of surface-treated infrared-absorbing microparticles used can be controlled, which is advantageous in terms of cost.
[0111] The shape of the infrared absorbing nanoparticle dispersion is not particularly limited and can be changed appropriately depending on the application. For example, it can be changed to any shape such as a film shape or a board shape. In addition, the thickness of the film shape or the boat shape can be changed appropriately depending on the application, and can be, for example, 0.1 μm to 50 mm.
[0112] The infrared absorbing nanoparticle dispersion can be prepared as follows. For example, the surface-treated infrared absorbing particles, the infrared absorbing particle dispersion, or the powder dispersion in which the surface-treated infrared absorbing particles are dispersed in a solid medium is added to a liquid medium, and the mixture is directly kneaded into a resin and molded into an arbitrary shape. Specifically, the resin is heated to a temperature near the melting point (about 200 to 300°C) to melt it, and then the surface-treated infrared absorbing particles are mixed and kneaded into the resin. Then, the mixture is molded into a predetermined shape by, for example, an extrusion molding method, an inflation molding method, a solution casting method, a casting method, or the like. The kneaded mixture may be molded as it is, or may be pelletized and then molded into pellets by the above-mentioned method.
[0113] Also, for example, the infrared absorbing microparticle dispersion can be prepared by further pulverizing the surface-treated infrared absorbing microparticles dispersed in a solid medium to obtain a powder. In the powdered infrared absorbing microparticle dispersion, the surface-treated infrared absorbing microparticles are already sufficiently dispersed in the solid medium. Therefore, the powdered infrared absorbing microparticle dispersion can be dissolved in a suitable liquid medium as a so-called master batch, or kneaded with resin pellets, etc., to easily produce a liquid or solid infrared absorbing microparticle dispersion.
[0114] <3-3> Infrared absorbing substrate The infrared absorbing substrate is a substrate having a surface-treated infrared absorbing fine particle-containing film-like dispersion (dispersion film) formed on the surface thereof. The infrared absorbing substrate has excellent moist heat resistance and chemical stability due to the dispersion film provided on the surface thereof, and can be suitably used as an infrared absorbing material.
[0115] The material of the substrate is not particularly limited as long as it is transparent, but glass, a resin board, a resin sheet, or a resin film is preferably used.
[0116] Resins used for resin boards, resin sheets, and resin films are not particularly limited as long as they do not cause problems in the surface state or durability of the required boards, sheets, and films. For example, boards, sheets, and films made of transparent polymers such as polyester polymers such as polyethylene terephthalate and polyethylene naphthalate, cellulose polymers such as diacetyl cellulose and triacetyl cellulose, polycarbonate polymers, acrylic polymers such as polymethyl methacrylate, styrene polymers such as polystyrene and acrylonitrile-styrene copolymers, polyethylene, polypropylene, polyolefins having a cyclic or norbornene structure, olefin polymers such as ethylene-propylene copolymers, vinyl chloride polymers, amide polymers such as aromatic polyamides, imide polymers, sulfone polymers, polyethersulfone polymers, polyetheretherketone polymers, polyphenylene sulfide polymers, vinyl alcohol polymers, vinylidene chloride polymers, vinyl butyral polymers, arylate polymers, polyoxymethylene polymers, epoxy polymers, and further various binary and ternary copolymers, graft copolymers, and blends thereof can be mentioned. In particular, polyester-based biaxially oriented films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene-2,6-naphthalate are preferred in terms of mechanical properties, optical properties, heat resistance, and economic efficiency. The polyester-based biaxially oriented film may be a copolymer polyester-based film.
[0117] The infrared absorbing substrate can be prepared as follows: For example, an infrared absorbing substrate in which the infrared absorbing nanoparticle dispersion is directly laminated on the substrate surface can be obtained by applying an infrared absorbing nanoparticle dispersion liquid obtained by mixing the surface-treated infrared absorbing nanoparticles with an organic solvent such as alcohol or a liquid medium such as water, a resin binder, and optionally a dispersant, to a suitable substrate surface, and then removing the liquid medium or curing the mixture.
[0118] The resin binder component can be selected according to the application, and examples of the resin binder component include an ultraviolet curing resin, a heat curing resin, a room temperature curing resin, a thermoplastic resin, etc. On the other hand, an infrared absorbing microparticle dispersion liquid not containing a resin binder component may be laminated on the surface of a substrate with an infrared absorbing microparticle dispersion, or after lamination, a liquid medium containing a binder component may be applied on the layer of the infrared absorbing microparticle dispersion.
[0119] Specifically, the infrared absorbing substrate is prepared by applying a liquid infrared absorbing microparticle dispersion in which surface-treated infrared absorbing microparticles are dispersed in one or more liquid media selected from organic solvents, organic solvents in which resins are dissolved, organic solvents in which resins are dispersed, and water to the surface of the substrate, and solidifying the resulting coating film by an appropriate method. In addition, the infrared absorbing substrate is prepared by applying a liquid infrared absorbing microparticle dispersion containing a resin binder component to the surface of the substrate, and solidifying the resulting coating film by an appropriate method. In addition, the infrared absorbing substrate is prepared by applying a liquid infrared absorbing microparticle dispersion in which surface-treated infrared absorbing microparticles are dispersed in a powdery solid medium to a predetermined medium, to the surface of the substrate, and solidifying the resulting coating film by an appropriate method. Of course, the infrared absorbing substrate is prepared by applying an infrared absorbing microparticle dispersion in which two or more of the various liquid infrared absorbing microparticle dispersions are mixed to the surface of the substrate, and solidifying the resulting coating film by an appropriate method.
[0120] <3-4>Goods The above-mentioned infrared absorbing microparticle dispersions and infrared absorbing articles such as films and boards which are infrared absorbing base materials can be suitably used, for example, in window materials in various buildings and vehicles that aim to block light in the infrared region while allowing sufficient visible light in and suppressing an increase in temperature inside the room while maintaining brightness, and in filters used in PDPs (plasma display panels) that block infrared rays emitted forward from the PDP.
[0121] In addition, since the surface-treated infrared absorbing particles have absorption in the infrared region, when an infrared laser is irradiated onto a printed surface containing the surface-treated infrared absorbing particles, the surface-treated infrared absorbing particles absorb infrared rays having a specific wavelength. Therefore, the counterfeit prevention printed matter obtained by printing the counterfeit prevention ink containing the surface-treated infrared absorbing particles onto one or both sides of a printed substrate can be judged for authenticity from the difference in the amount of reflection or transmission by irradiating infrared rays having a specific wavelength and reading the reflection or transmission. The counterfeit prevention printed matter is an example of the infrared absorbing particle dispersion according to the present invention.
[0122] In addition, an ink can be prepared by mixing an infrared absorbing fine particle dispersion liquid and a binder component, and the ink can be applied to a substrate, dried, and then cured to form a light-to-heat conversion layer. The light-to-heat conversion layer can generate heat only at a desired location with high positional accuracy by irradiation with an electromagnetic wave laser such as infrared, and can be applied in a wide range of fields such as electronics, medicine, agriculture, and machinery. For example, it can be suitably used as a donor sheet used when forming an organic electroluminescence element by a laser transfer method, thermal paper for a thermal printer, or an ink ribbon for a thermal transfer printer. The light-to-heat conversion layer is an example of an infrared absorbing fine particle dispersion according to the present invention.
[0123] In addition, infrared absorbing fibers can be obtained by dispersing surface-treated infrared absorbing particles in a suitable medium and incorporating the dispersion on the surface and / or inside of fibers. The infrared absorbing fibers efficiently absorb near-infrared rays from sunlight and the like due to the inclusion of surface-treated infrared absorbing particles, and become infrared absorbing fibers with excellent heat retention, while at the same time transmitting light in the visible light range, resulting in infrared absorbing fibers with excellent design. As a result, they can be used for various applications such as textile products that require heat retention, such as cold weather clothing, sports clothing, stockings, curtains, and other industrial textile products. The infrared absorbing fibers are an example of the infrared absorbing particle dispersion according to the present invention.
[0124] Furthermore, the film- or board-shaped infrared absorbing microparticle dispersion can be applied to materials used for roofs and exterior walls of agricultural and horticultural greenhouses. The film- or board-shaped infrared absorbing microparticle dispersion can be used as a heat insulating material for agricultural and horticultural facilities, which transmits visible light to ensure the light necessary for photosynthesis of plants in the agricultural and horticultural greenhouses, while efficiently absorbing other light such as near-infrared light contained in sunlight. The heat insulating material for agricultural and horticultural facilities is one example of the infrared absorbing microparticle dispersion according to the present invention.
[0125] <Effects of this embodiment> According to this embodiment, one or more of the following advantages are achieved.
[0126] The surface-treated infrared absorbing particles of this embodiment are produced by attaching a hydrolysis product or a polymer thereof of a metal chelate compound to the surface of the infrared absorbing particles, and then subjecting the attached film to a heat treatment. The heat treatment can further hydrolyze the hydrolysis product or the polymer thereof contained in the attached film to a metal oxide hydrate. The coating film obtained by heat treating the attached film contains a metal oxide hydrate and is configured to have a carbon concentration of 5.0 mass% or less. Such a coating film contains a small amount of the hydrolysis product or the polymer thereof of the metal chelate compound, and the carbon component derived from these is small. Therefore, the surface-treated infrared absorbing particles can achieve high moisture and heat resistance compared to the case where the coating film is composed of a hydrolysis product while maintaining high infrared absorbing properties.
[0127] The metal oxide hydrate forming the coating film preferably contains one or more metal elements selected from Al, Zr, Ti, Si, and Zn. By containing such metal elements, the moist heat resistance of the surface-treated infrared absorbing nanoparticles can be further improved.
[0128] The heat treatment is preferably carried out at a heating temperature of 40° C. to 80° C. for 4 hours or more. By carrying out the heat treatment under such conditions, the hydrolysis products in the deposited film can be further hydrolyzed. Therefore, the carbon concentration in the obtained coating film can be reduced and the ratio of metal oxide hydrates can be increased, thereby further improving the moist heat resistance.
[0129] Furthermore, in the surface-treated infrared absorbing microparticles of this embodiment, the coating film is formed into a dense, high-density film with a low carbon concentration by a specified heat treatment, so that heat treatment at 100°C or higher to improve adhesion to the infrared absorbing microparticles and chemical stability is not required. Generally, when heat treatment is performed at 100°C or higher, the surface-treated infrared-absorbing particles tend to aggregate and form coarse aggregates. Since the coarse aggregates impair the transparency of the infrared-absorbing particle dispersion, etc., they need to be crushed and redispersed. However, crushing the surface-treated infrared-absorbing particles may damage the coating film, and in some cases, part of the coating film may peel off. This makes it difficult to achieve both transparency and moisture and heat resistance. In this regard, the surface-treated infrared absorbing nanoparticles of the present embodiment do not require a heat treatment at 100° C. or higher, and therefore can avoid aggregation due to high-temperature heat treatment and disintegration to redisperse the aggregates, thereby preventing a decrease in moist heat resistance due to damage to the coating film and achieving high transparency.
[0130] By using the surface-treated infrared absorbing nanoparticles of this embodiment or an infrared absorbing nanoparticle dispersion liquid containing the same, it is possible to prepare an infrared absorbing nanoparticle dispersion or an infrared absorbing substrate having excellent infrared absorbing properties, moist heat resistance and transparency.
[0131] Specifically, when an infrared absorbing microparticle dispersion or an infrared absorbing base material is prepared so as to have a visible light transmittance of 80%, the transmittance of light with a wavelength of 800 nm to 1000 nm is 32% or more and 55% or less, thereby realizing high infrared absorbing properties.
[0132] Furthermore, when an infrared absorbing microparticle dispersion or an infrared absorbing base material prepared so as to have a visible light transmittance of 80% is exposed to a moist and hot atmosphere at a temperature of 85°C and a relative humidity of 90% for 1000 hours, the change in the average transmittance at wavelengths of 800 nm to 1000 nm before and after exposure is 1.5% or less, thereby achieving excellent moist and heat resistance.
[0133] Furthermore, when an infrared absorbing nanoparticle dispersion or an infrared absorbing base material is prepared so as to have a visible light transmittance of 80%, the haze value is 1.2% or less, and excellent transparency can be achieved. EXAMPLES
[0134] The present invention will be specifically described below with reference to examples, although the present invention is not limited to the following examples.
[0135] First, the evaluation methods in the examples and comparative examples are described. In this example, the surface-treated infrared absorbing fine particles are measured for dispersed particle size, crystallite size, BET specific surface area, and carbon concentration. The infrared absorbing sheet as the infrared absorbing substrate is evaluated for optical properties, haze value, and moist heat resistance. Each evaluation method is described below.
[0136] (Dispersed particle size) The dispersed particle size is shown as an average value measured by a particle size measuring device (ELS-8000 manufactured by Otsuka Electronics Co., Ltd.) based on the dynamic light scattering method.
[0137] (Crystallite size) The crystallite size was measured by powder X-ray diffraction (θ-2θ method) using a powder X-ray diffractometer (X'Pert-PRO / MPD manufactured by PANalytical, Spectris Co., Ltd.), and calculated by the Rietveld method.
[0138] (BET specific surface area) The BET specific surface area was measured using a BET specific surface area measuring device (Macsorb-1208 manufactured by Mountec Co., Ltd.).
[0139] (carbon concentration) The carbon concentration of the surface-treated infrared absorbing fine particle powder was measured using a carbon analyzer (CS-600 manufactured by LECO Co.) based on the principle of the combustion-infrared absorption method.
[0140] (Optical properties) The optical properties of the infrared absorbing sheet were measured at 5 nm intervals in the wavelength range of 200 nm to 2600 nm using a spectrophotometer (U-4100 manufactured by Hitachi, Ltd.), and the visible light transmittance was calculated according to JIS R 3106. The average transmittance in the wavelength range of 800 nm to 1000 nm was also calculated. Note that the optical property values (visible light transmittance, haze value) of the infrared absorbing sheet referred to here include the optical property values of the resin sheet, which is the substrate.
[0141] (Haze value) The haze value of the infrared absorbing sheet was measured using a haze meter (HM-150 manufactured by Murakami Color Co., Ltd.) and calculated in accordance with JIS K7105.
[0142] (Moisture and heat resistance) The method for evaluating the moist heat resistance of an infrared absorbing sheet is to expose the infrared absorbing sheet with a visible light transmittance of about 80% to a moist heat atmosphere at a temperature of 85°C and a relative humidity of 90% for 1000 hours. If the change in solar radiation transmittance before and after the exposure was 1.5% or less, the sheet was judged to have good moist heat resistance, and if the change was more than 1.5%, the sheet was judged to have insufficient moist heat resistance.
[0143] [Example 1] (Preparation of surface-treated infrared absorbing fine particles) Hexagonal cesium tungsten bronze (Cs) with Cs / W (molar ratio) = 0.33 0.33 WO z A mixture of 25% by mass of powdered CWO (registered trademark) (YM-01 manufactured by Sumitomo Metal Mining Co., Ltd.) and 75% by mass of pure water was loaded into a paint shaker containing 0.3 mm diameter ZrO2 beads and ground and dispersed for 10 hours to obtain the Cs 0.33 WO z A dispersion of fine particles was obtained.
[0144] Cs in the obtained dispersion 0.33 WO z The dispersed particle diameter of the fine particles was measured to be 100 nm. The particle diameter measurement was set to a particle refractive index of 1.81 and a non-spherical particle shape. The background was measured using pure water, and the solvent refractive index was set to 1.33. After removing the solvent from the obtained dispersion, the crystallite diameter was measured to be 32 nm. After removing the solvent from the obtained dispersion, the dried product was crushed in a mortar and Cs 0.33 WO z The BET specific surface area of the particles was measured to be 38 m 2 / g.
[0145] The obtained Cs 0.33 WO z The dispersion of fine particles was mixed with pure water, and Cs 0.33 WO z A coating film-forming dispersion A having a fine particle concentration of 2 mass % was obtained.
[0146] The above is shown in Table 1 below.
[0147] [Table 1]
[0148] Next, as shown in Table 2 below, 2.5 mass % of aluminum ethyl acetoacetate diisopropylate as an aluminum-based chelate compound and 97.5 mass % of isopropyl alcohol (IPA) were mixed to obtain a surface treatment agent a.
[0149] [Table 2]
[0150] Next, 890 g of the obtained coating film forming dispersion A was placed in a beaker, and while strongly stirring with a stirrer with blades, 360 g of surface treatment agent a was added dropwise over 3 hours as shown in Table 2 above. Here, as shown in Table 2, the surface treatment agent a was added so that the content of Al element derived from the Al-based chelate compound was 5 parts by mass relative to 100 parts by mass of infrared absorbing fine particles. As a result, the Al-based chelate compound contained in the surface treatment agent a was hydrolyzed, and the hydrolysis product or its polymer was attached to the surface of the infrared absorbing fine particles to form an attached film. Next, as shown in Table 3 below, after the dropwise addition of the surface treatment agent a, stirring was further performed at a temperature of 55 ° C for 5 hours to prepare the aged liquid according to Example 1. As a result, the hydrolysis product or polymer in the attached film was further hydrolyzed to a hydrate of metal oxide, and a coating film containing the hydrate of metal oxide was formed. Next, the medium was evaporated from the aged liquid by vacuum flow drying at a temperature of 55 ° C for 3 hours to obtain a powder containing the surface-treated infrared absorbing fine particles according to Example 1 (surface-treated infrared absorbing fine particle powder).
[0151] [Table 3]
[0152] (Carbon concentration in surface infrared absorbing fine powder) The carbon concentration of the surface-treated infrared absorbing fine particles according to Example 1 was measured and found to be 1.9 mass %, as shown in Table 4 below.
[0153] [Table 4]
[0154] (Preparation of infrared absorbing nanoparticle dispersion) 8% by mass of the surface-treated infrared absorbing fine particle powder according to Example 1, 24% by mass of a polyacrylate-based dispersant, and 68% by mass of toluene were mixed together. The resulting mixture was placed in a paint shaker containing 0.3 mmφZrO2 beads, and pulverized and dispersed for 1 hour to obtain an infrared absorbing fine particle dispersion according to Example 1.
[0155] (Production and evaluation of infrared absorbing sheets) Next, the medium was evaporated from the above-mentioned infrared absorbing fine particle dispersion liquid by vacuum fluidized drying, and an infrared absorbing fine particle dispersion powder according to Example 1 was obtained. This dispersion powder and polycarbonate resin were dry blended so that the visible light transmittance of the infrared absorbing sheet obtained later would be around 80%. Here, the surface-treated infrared absorbing fine particles were blended so that the concentration was 0.09 wt%. The obtained blend was kneaded at 290°C using a twin-screw extruder, extruded from a T-die, and formed into a sheet material with a thickness of 0.75 mm by a calendar roll method, and an infrared absorbing sheet according to Example 1 was obtained. The infrared absorbing sheet is an example of an infrared absorbing fine particle dispersion according to the present invention.
[0156] The optical properties of the obtained infrared absorbing sheet of Example 1 were measured, and as shown in Table 5 below, the visible light transmittance was 79.7%, the average transmittance at wavelengths of 800 nm to 1000 nm was 32.5%, and the haze was 0.9%.
[0157] The obtained infrared absorbing sheet according to Example 1 was exposed to a humid and hot atmosphere at a temperature of 85°C and a relative humidity of 90% for 1000 hours, and then its optical properties were measured. As shown in the following Table 5, the visible light transmittance was 80.4%, the average transmittance at wavelengths of 800nm to 1000nm was 33.7%, and the haze was 0.9%. It was found that the amount of change in the visible light transmittance due to exposure to the humid and hot atmosphere was small, 0.7%, and the amount of change in the average transmittance at wavelengths of 800nm to 1000nm was 1.2%, and that the haze did not change.
[0158] [Table 5]
[0159] (Evaluation of surface-treated infrared absorbing particles) Finally, the characteristics of the surface-treated infrared absorbing fine particles contained in the infrared absorbing sheet according to Example 1 were investigated. The infrared absorbing sheet according to Example 1 was immersed in chloroform to dissolve all organic components. Then, a centrifuge (H-9R manufactured by Kokusan Co., Ltd.) was used to separate the chloroform and a cake of aggregates of surface-treated infrared absorbing fine particles at a rotation speed of 22,000 rpm. Then, the cake was washed with toluene, acetone, and ethanol in this order, and only the surface-treated infrared absorbing fine particles were taken out.
[0160] The components of the surface-treated infrared absorbing particles were analyzed using an ICP emission spectrometer (Shimadzu Corporation, Model: ICPE9000), and it was found to contain 56% by mass of tungsten and 4.2% by mass of aluminum, as shown in Table 4. Tungsten was Cs 0.33 WO z Since it is an element caused by fine particles, 84 mass% of Cs was found in the surface-treated infrared absorbing fine particles. 0.33 WO z It was found that the particles contained Cs 0.33 WO z The Z was calculated as 3.0. Furthermore, when the sample was analyzed using a thermal analyzer consisting of a thermobalance (Bruker AXS) and a mass analyzer (Q-MS, Bruker AXS), it was found that the sample contained 2.4% by mass of water. The content of water derived from hydrates was calculated from this and found to be 1.5% by mass. In other words, the coating film contained a high proportion of water derived from metal oxide hydrates, and it was found that the coating film was mainly composed of hydrates. Here, the analysis using the thermal analyzer was performed by heating the film from room temperature to 500°C at a heating rate of 20°C / min and flowing carrier gas at a He flow rate of 150cc / min. The gas components with mass-to-charge ratios m / z=17 and 18 were all considered to be water, and the amount of water generated was evaluated.
[0161] The content of water derived from hydrates was specifically calculated as follows. When aluminum ethyl acetoacetate diisopropylate is used as the metal chelate compound, aluminum ethyl acetoacetate dihydroxide is not completely hydrolyzed and remains in the coating film as a hydrolysis product. When one aluminum ethyl acetoacetate dihydroxide is thermally analyzed, two water molecules (molecular weight 18) are generated, and the amount of water minus this amount is the amount of water derived from the hydrate. Since there are six carbon atoms (atomic weight 12) in aluminum ethyl acetoacetate dihydroxide, when the carbon concentration of the surface-treated infrared absorbing particles is c [mass %], the content h3 of water derived from the hydrolysis product (aluminum ethyl acetoacetate dihydroxide) is c / (12×6)×18×2, which is c×0.5. Therefore, when the content of water in the coating film is h2 [mass %], the content h1 [mass %] of water derived from the hydrate is h2-c×0.5. Specifically, since h2 is 2.4 mass% and c is 1.9 mass%, in Example 1, the content h3 of water derived from the hydrolysis product is 0.95 (= 1.9 × 0.5) mass%, and the content h1 [mass%] of water derived from the hydrate is 1.5 mass%.
[0162] From the above results, the surface-treated infrared absorbing particles are 0.33 WO z It was determined that the microparticles were coated with a coating film containing alumina hydrate (Al2O3·nH2O).
[0163] [Examples 2 and 3] In Examples 2 and 3, as shown in Table 2, the amount of surface treatment agent a and the dropwise addition time were changed as surface treatment conditions, and the same operation as in Example 1 was performed. Specifically, the dropwise addition amount of surface treatment agent a was changed from 300 g in Example 1 to 1800 g in Example 2 and 3600 g in Example 3. The dropwise addition time was changed from 3 hours in Example 1 to 15 hours in Example 2 and 30 hours in Example 3. The rest of the operations were performed in the same manner as in Example 1 to obtain a surface-treated infrared absorbing fine particle powder, an infrared absorbing fine particle dispersion, an infrared absorbing fine particle dispersion powder, and an infrared absorbing sheet, and the same evaluations were performed as in Example 1. The content of water derived from the hydrate was calculated by the same method as in Example 1.
[0164] [Examples 4 to 7] In Examples 4 to 7, the same operations as in Example 1 were carried out except that surface treatment agents b to e were used instead of surface treatment agent a, as shown in Table 2, to obtain surface-treated infrared absorbing microparticle powders, infrared absorbing microparticle dispersions, infrared absorbing microparticle dispersion powders, and infrared absorbing sheets, and the same evaluations as in Example 1 were carried out. Surface treatment agent b was prepared by mixing 2.4 mass % of zirconium tributoxyacetylacetonate and 97.6 mass % of isopropyl alcohol. Surface treatment agent c was prepared by mixing 2.6 mass % of diisopropoxytitanium bisethylacetoacetate and 97.4 mass % of isopropyl alcohol. Surface treatment agent d was prepared so as to contain only 309 g of tetraethoxysilane without adding isopropyl alcohol. Surface treatment agent e was prepared by mixing 4.4 mass % of zinc acetylacetonate and 95.6 mass % of isopropyl alcohol.
[0165] In the same manner as in Example 1, the characteristics of the surface-treated infrared absorbing fine particles contained in the infrared absorbing sheet of Examples 4 to 7 were investigated. As a result, as shown in Table 4, in Example 4, Cs 0.33 WO zThe particles were identified as surface-treated infrared absorbing particles having a coating film containing zirconia hydrate formed on the surface of the particles. In Example 5, Cs 0.33 WO z The particles were identified as surface-treated infrared absorbing particles having a coating film containing titania hydrate formed on the surface of the particles. In Example 6, Cs 0.33 WO z The particles were identified as surface-treated infrared absorbing particles having a coating film containing silica hydrate formed on the surface of the particles. In Example 7, Cs 0.33 WO z The particles were identified as surface-treated infrared absorbing particles having a coating film containing zinc oxide hydrate formed on the surface of the particles.
[0166] In Examples 4 to 7, the content of water derived from hydrates was calculated by the following method. In Example 4, zirconium tributoxy acetylacetonate was used as the metal chelate compound, so the component that was not completely hydrolyzed and remained was zirconium trihydroxide acetylacetonate. This hydrolysis product contains 5 carbon atoms, and 3 water molecules are generated by thermal analysis. From this, the content of water derived from the hydrolysis product is c×0.9, and the content of water derived from the hydrate is hc×0.9, which is calculated to be 1.3 mass%. In addition, in Example 5, diisopropoxytitanium bisethylacetoacetate was used as the metal chelate compound, so the component that was not completely hydrolyzed and remained was dihydroxytitanium bisethylacetoacetate. This hydrolysis product contains 10 carbon atoms, and two water molecules are generated by thermal analysis. From this, the content of water derived from the hydrolysis product is c×0.3, and the content of water derived from the hydrate is hc×0.3, which is calculated to be 1.8% by mass. In Example 6, tetraethoxysilane was used as the metal chelate compound, and the component that was not completely hydrolyzed and remained was tetraethoxysilane. Since tetraethoxysilane does not generate water molecules in thermal analysis, the content of water derived from the hydrate was h, which was 4.5% by mass. In addition, in Example 7, zinc acetylacetonate was used as the metal chelate compound, so the component that was not completely hydrolyzed and remained was zinc monohydroxymonoacetylacetonate. This hydrolysis product contains 5 carbon atoms, and one water molecule is generated by thermal analysis. From this, the content of water derived from the hydrolysis product is c×0.3, and the content of water derived from the hydrate is hc×0.3, which is calculated to be 1.5 mass%.
[0167] [Examples 8 and 9] In Examples 8 and 9, the same procedure as in Example 1 was carried out, except that the type of infrared absorbing particles was changed as shown in Table 1. Specifically, the infrared absorbing particles were changed from the hexagonal cesium tungsten bronze powder in Example 1 to a hexagonal rubidium tungsten bronze powder with Rb / W (molar ratio) = 0.33 in Example 8, and from the Magneli phase W powder in Example 9. 18 O 49 to prepare coating film-forming dispersions B and C. Thereafter, the same operations as in Example 1 were carried out on these coating film-forming dispersions B and C to obtain a surface-treated infrared absorbing microparticle powder, an infrared absorbing microparticle dispersion, an infrared absorbing microparticle dispersion powder, and an infrared absorbing sheet, and the same evaluations were carried out as in Example 1. The content of water derived from the hydrate was calculated by the same method as in Example 1.
[0168] [Comparative Example 1] In Comparative Example 1, an infrared absorbing fine particle dispersion, an infrared absorbing fine particle dispersion powder, and an infrared absorbing sheet were prepared without performing a surface treatment on the infrared absorbing fine particles as in Examples 1 to 9. Specifically, as shown in Table 1, 7% by mass of hexagonal cesium tungsten bronze powder, 24% by mass of a polyacrylate-based dispersant, and 69% by mass of toluene were mixed, and the resulting mixture was loaded into a paint shaker containing 0.3 mmφZrO2 beads and ground and dispersed for 4 hours to obtain a coating film forming dispersion D according to Comparative Example 1. The dispersed particle diameter of the infrared absorbing fine particles in the obtained coating film forming dispersion D was measured to be 100 nm. The particle diameter measurement settings were a particle refractive index of 1.81, and a particle shape of asphericity. The background was measured using toluene, and the solvent refractive index was 1.50. After removing the solvent from the obtained dispersion, the crystallite diameter was measured to be 32 nm.
[0169] Next, without adding a surface treatment agent to this coating film-forming dispersion D, this was used as an infrared absorbing microparticle dispersion according to Comparative Example 1. The medium was evaporated from the infrared absorbing microparticle dispersion according to Comparative Example 1 by vacuum fluidized drying, to obtain an infrared absorbing microparticle dispersion powder according to Comparative Example 1.
[0170] The infrared absorbing fine particle dispersion powder according to Comparative Example 1 and polycarbonate resin were dry blended so that the concentration of the infrared absorbing fine particles was 0.075 wt%. The obtained blend was kneaded at 290°C using a twin-screw extruder, extruded from a T-die, and made into a sheet material with a thickness of 0.75 mm by a calendar roll method, thereby obtaining an infrared absorbing sheet according to Comparative Example 1.
[0171] The optical properties of the obtained infrared absorbing sheet according to Comparative Example 1 were measured, and as shown in Table 4, the visible light transmittance was 79.2%, the average transmittance at wavelengths of 800 nm to 1000 nm was 32.6%, and the haze was 1.0%.
[0172] The obtained infrared absorbing sheet according to Comparative Example 1 was exposed to a humid heat atmosphere of 85°C and 90% for 1000 hours, and then the optical properties were measured. The visible light transmittance was 81.2%, the average transmittance at wavelengths of 800nm to 1000nm was 40.3%, and the haze was 1.2%. The change in the visible light transmittance due to exposure to a humid heat atmosphere was 2.0%, and the change in the average transmittance at wavelengths of 800nm to 1000nm was 7.7%, which was found to be larger than that of the Examples. The change in the haze was 0.2%.
[0173] In addition, since no coating film was formed in Comparative Example 1, the components contained in the infrared absorbing fine particles were not analyzed by ICP emission spectrometry, and the carbon concentration was not measured.
[0174] [Comparative Examples 2 and 3] In Comparative Examples 2 and 3, the same operation as in Comparative Example 1 was performed except that the type of infrared absorbing particles was changed as shown in Table 1. Specifically, the type of infrared absorbing particles was changed from the hexagonal cesium tungsten bronze powder in Comparative Example 1 to a hexagonal rubidium tungsten bronze powder with Rb / W (molar ratio) = 0.33 in Comparative Example 2, and from the Magneli phase W powder in Comparative Example 3. 18 O 49 The composition was changed to the above, respectively, to prepare coating film-forming dispersions E and F. Subsequently, infrared absorbing fine particle dispersion powder and infrared absorbing sheet were obtained using these dispersions E and F, and the same evaluation as in Example 1 was carried out. In addition, since no coating film was formed in Comparative Examples 2 and 3, ICP emission analysis was not carried out on the components contained in the infrared absorbing fine particles. Carbon concentration was also not measured.
[0175] [Comparative Example 4] In Comparative Example 4, the same operation as in Example 1 was performed except that the heat treatment conditions after the addition of the surface treatment agent were changed as shown in Table 3. Specifically, 890 g of the dispersion liquid A for forming a coating film obtained in the same manner as in Example 1 was placed in a beaker, and 360 g of the surface treatment agent a was added dropwise thereto over 3 hours while stirring vigorously with a stirrer with a blade. In Comparative Example 4, after the dropwise addition of the surface treatment agent a, stirring was performed at a temperature of 20°C for 24 hours to prepare an aged liquid. Next, the medium was evaporated from the aged liquid by vacuum flow drying at a temperature of 30°C for 72 hours to obtain a powder containing surface-treated infrared absorbing fine particles according to Comparative Example 4. When the carbon concentration of the surface-treated infrared absorbing fine particle powder according to Comparative Example 4 was measured, it was 5.6 mass% as shown in Table 4. Using the obtained powder, the same operation as in Example 1 was performed to obtain an infrared absorbing fine particle dispersion liquid, an infrared absorbing fine particle dispersion powder, and an infrared absorbing sheet according to Comparative Example 4, and the same evaluation as in Example 1 was performed.
[0176] In Comparative Example 4, the characteristics of the surface-treated infrared absorbing particles contained in the infrared absorbing sheet were investigated in the same manner as in Example 1. As a result, as shown in Table 4, it was found that the infrared absorbing sheet contained 55 mass % of tungsten and 4.1 mass % of aluminum. Tungsten was Cs 0.33 WO z Since it is an element caused by fine particles, 83 mass% of Cs was found in the surface-treated infrared absorbing fine particles. 0.33 WO z It was found that the particles contained Cs 0.33 WO z The Z was calculated as 3.0. Furthermore, it was found that the water content was 3.1 mass%. From this, the content of water derived from hydrates was calculated in the same manner as in Example 1, and was found to be 0.30 mass%. Furthermore, as shown in Table 4, it was found that the carbon concentration was 5.6 mass%, exceeding 5.0%. From this, it was confirmed that the ratio of water derived from metal oxide hydrates was small in the coating film of Comparative Example 4, and that more hydrolysis products that were not completely hydrolyzed to hydrates remained in the coating film than the hydrates.
[0177] <Evaluation Results> As shown in Tables 4 and 5, in Examples 1 to 9, by forming a coating film containing a metal oxide hydrate and having a low carbon concentration of 5.0 mass% or less, it was confirmed that the change in transmittance of light with wavelengths of 800 nm to 1000 nm before and after exposure was 1.5% or less, and high moist heat resistance could be realized. In addition, the initial value of the transmittance of light with wavelengths of 800 nm to 1000 nm before exposure was 32% or more and 55% or less, and high infrared absorption characteristics could be realized. In addition, the haze value was small at 1.2% or less, and it was confirmed that the transparency was excellent.
[0178] In contrast, in Comparative Examples 1 to 3, the initial transmittance of light with wavelengths of 800 nm to 1000 nm before exposure was low, but the value after exposure increased, confirming low moist heat resistance, as shown in Table 5. This is believed to be because no coating film was provided on the surface of the infrared absorbing spherical particles, and the surface of the infrared absorbing particles was decomposed by moisture, resulting in a decrease in the infrared absorbing properties.
[0179] In Comparative Example 4, the carbon concentration in the surface-treated infrared absorbing microparticles was 5.6% by mass, which was confirmed to exceed 5.0% by mass, as shown in Table 4. This is believed to be because, although a heat treatment was performed after the deposition film containing the hydrolysis product was formed in Comparative Example 4, the heat treatment was insufficient, and hydrolysis of the hydrolysis product did not progress much, resulting in the hydrolysis product remaining in the coating film.
[0180] As described above, according to this embodiment, it was confirmed that by configuring the coating film of the surface-treated infrared absorbing microparticles so that it contains a predetermined amount of metal oxide hydrate and has a carbon concentration below a predetermined value, it is possible to improve moist heat resistance while maintaining the desired high infrared absorption characteristics.
Claims
1. The present invention comprises infrared absorbing particles and a coating film containing a hydrate of a metal oxide formed so as to cover the surface of the particles, The carbon concentration as measured by a combustion-infrared absorption method is 5.0% by mass or less; The content of water derived from the hydrate of the metal oxide is 1.0% by mass or more and 8.0% by mass or less. Surface treated infrared absorbing particles.
2. 2. The surface-treated infrared absorbing nanoparticles according to claim 1, wherein the metal oxide contains one or more metal elements selected from the group consisting of Al, Zr, Ti, Si and Zn.
3. The infrared absorbing fine particles include tungsten oxide fine particles represented by the general formula WyOz (wherein W is tungsten, O is oxygen, and 2.2≦z / y≦2.999), and fine particles of a general formula MxWyOz (wherein M is H, He, an alkali metal, an alkaline earth metal, a rare earth element, Mg, Zr, Cr, Mn, Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zn, C tungsten oxide fine particles represented by the formula: 0.001≦x / y≦1, 2.0≦z / y≦3.0; d, Al, Ga, In, Tl, Si, Ge, Sn, Pb, Sb, B, F, P, S, Se, Br, Te, Ti, Nb, V, Mo, Ta, Re, Be, Hf, Os, Bi, I, Yb; W is tungsten; O is oxygen; and 0.001≦x / y≦1, 2.0≦z / y≦3.
0.
3. The surface-treated infrared absorbing particles according to claim 1 or 2.
4. The coating film contains a metal element constituting the metal oxide hydrate in an amount of 10 parts by mass or more and 500 parts by mass or less per 100 parts by mass of the infrared absorbing nanoparticles. The surface-treated infrared absorbing nanoparticles according to claim 1 .
5. An infrared absorbing nanoparticle dispersion comprising the surface-treated infrared absorbing nanoparticles according to claim 1 and a liquid medium.
6. 6. The infrared absorbing nanoparticle dispersion according to claim 5, wherein the liquid medium is at least one of an organic solvent, an oil or fat, a liquid plasticizer, a compound that is polymerized by curing, and water.
7. 5. An infrared absorbing nanoparticle dispersion comprising the surface-treated infrared absorbing nanoparticles according to claim 1 dispersed in a solid resin.
8. 8. The infrared absorbing nanoparticle dispersion according to claim 7, wherein the solid resin is at least one of a fluororesin, a PET resin, an acrylic resin, a polyamide resin, a vinyl chloride resin, a polycarbonate resin, an olefin resin, an epoxy resin, and a polyimide resin.
9. A step of mixing infrared absorbing fine particles and water to obtain a dispersion for forming a coating film; adding a surface treatment agent containing a metal chelate compound to the dispersion for forming a coating film; and subjecting the dispersion liquid for forming a coating film to which the surface treatment agent has been added to a heat treatment, a coating film containing a hydrate of a metal oxide derived from the metal chelate compound is formed on the surface of the infrared absorbing fine particles, and surface-treated infrared absorbing fine particles are obtained, the carbon concentration being 5.0 mass% or less when measured by a combustion-infrared absorption method, and the content of water derived from the hydrate of the metal oxide being 1.0 mass% or more and 8.0 mass% or less. A method for producing surface-treated infrared absorbing particles.
10. The heat treatment is carried out at a temperature of 40° C. or higher and 80° C. or lower for 4 hours or longer. The method for producing the surface-treated infrared absorbing fine particles according to claim 9.
11. In the step of adding the surface treatment agent, the surface treatment agent is added so that the content of the metal element constituting the metal oxide is 10 parts by mass or more and 500 parts by mass or less per 100 parts by mass of the infrared absorbing fine particles. The method for producing the surface-treated infrared absorbing fine particles according to claim 9 or 10.
Citation Information
Patent Citations
Infrared shielding material microparticle dispersion, infrared shield, process for producing infrared shielding material microparticle, and infrared shielding material microparticle
WO2005037932A1
Infrared blocking particle, method for producing the same, infrared blocking particle dispersion using the same, and infrared blocking base
WO2010055570A1
Surface-treated infrared-absorbing fine particles, surface-treated infrared-absorbing fine particle powder, infrared-absorbing fine particle dispersion in which said surface-treated infrared-absorbing fine particles are used, infrared-absorbing fine particle dispersoid, and methods for producing these
WO2019093524A1