Wafer Processing Method
The wafer processing method with a post-rough polishing step using a secondary amine and water-soluble polymer composition effectively addresses the challenge of high polishing rate and defect reduction, enhancing productivity and surface quality.
Patent Information
- Application Number
- JP2021065422
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-07
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2041-04-07
AI Technical Summary
Existing wafer processing methods face challenges in achieving a high polishing rate while minimizing defects, particularly concave defects, due to the inefficiencies in the final polishing step, which are exacerbated by attempts to reduce polishing time.
A wafer processing method that includes a post-rough polishing step using a polishing composition containing a secondary amine with a molecular weight of 10,000 or more and a water-soluble polymer, at a concentration of 10-100 ppm, to enhance polishing rate and defect reduction.
The method achieves both a high polishing rate and significant defect reduction, particularly in concave defects, thereby improving productivity and surface quality of silicon wafers.
Smart Images

Figure 0007556318000004 
Figure 0007556318000005 
Figure 0007556318000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a wafer processing method. [Background technology]
[0002] As semiconductor device processes become increasingly miniaturized, the silicon wafers that serve as substrates are also required to be highly flat and have fewer defects.
[0003] Silicon wafers are generally made by slicing a single crystal silicon ingot into wafers, then removing any damaged layers that occur during the slicing process through a grinding process such as surface grinding or lapping, and further removing any damaged layers that occur during the surface grinding process or the like through multiple polishing processes to make the wafer defect-free.
[0004] In particular, in the polishing process, existing damaged layers and defects must be quickly removed. Generally, the polishing process consists of a rough polishing process and a finish polishing process. The purpose of the rough polishing process is to remove damage that occurs during surface grinding, etc., and the purpose of the finish polishing process is to remove damage that occurs in the rough polishing process.
[0005] In the rough polishing process, a relatively hard polishing cloth is used, and a strong base-based polishing composition is used to increase the pH, thereby increasing the polishing rate from both a mechanical and chemical standpoint.
[0006] On the other hand, for finish polishing, a relatively soft polishing cloth is used, a weak base-based polishing composition is used with a pH of about 9 to 10, and additives such as water-soluble polymers and surfactants are used to lower the polishing rate from both a mechanical and chemical standpoint.
[0007] Therefore, in order to remove the damage caused in the rough polishing step in the finish polishing step, a long polishing time is required, resulting in a decrease in productivity.
[0008] Furthermore, if the polishing time in the finish polishing step is shortened in order to prevent a decrease in productivity, there is a problem in that defects increase significantly.
[0009] Defects that occur when the finish polishing time is shortened, i.e., defects remaining from rough polishing, are specifically called pit defects, and are thought to be caused by the failure to remove damage that occurred in the rough polishing process.
[0010] In this context, attempts have been made in recent years to insert a "post-rough polishing process" between the rough polishing process and the finish polishing process.
[0011] By providing a post-rough polishing process specialized in removing damage that occurs during rough polishing, the number of processes increases, but the polishing time for finish polishing can be reduced, resulting in an overall improvement in productivity.
[0012] Here, in the post-rough polishing step, as described above, it is required to quickly remove damage caused by rough polishing at a high polishing rate, and it is also necessary to prevent defects from occurring in the post-rough polishing step itself.
[0013] In the post-rough polishing process, there has been a method of increasing the polishing rate, for example by increasing the load during polishing. However, increasing the load causes many defects in the post-rough polishing process itself, which actually extends the polishing time in the finish polishing process.
[0014] In addition, a method has been devised in which an alkali is added to the polishing composition to increase its pH value, but increasing the pH value increases the contribution of anisotropic etching, which further etches the damaged areas caused by rough polishing, resulting in the need for a large amount of polishing stock.
[0015] Other attempts have been made to increase the size of the abrasive grains to increase the mechanical removal action, but if the grain size is made too large, damage will occur due to the abrasive grains, resulting in many defects in the post-coarse polishing process itself and extending the polishing time in the finish polishing process. [Prior art documents] [Patent documents]
[0016] [Patent Document 1] JP 2008-147651 A [Patent Document 2] JP 2016-124943 A [Patent Document 3] International Publication No. WO2011 / 093223 Brochure [Patent Document 4] JP 2017-11220 A [Patent Document 5] JP 2019-119854 A Summary of the Invention [Problem to be solved by the invention]
[0017] For these reasons, there is a demand for a polishing technique in the post-rough polishing step that can quickly remove damage caused by the rough polishing step at a high polishing rate while not creating defects in the post-rough polishing step itself.
[0018] The present invention has been made to solve the above problems, and has an object to provide a wafer processing method capable of achieving both a high polishing rate and a high defect reduction capability. [Means for solving the problem]
[0019] In order to solve the above problems, the present invention provides a method for manufacturing a wafer by a grinding process, a rough polishing step of roughly polishing the ground wafer; a post-rough polishing step of post-rough polishing the roughly polished wafer while supplying a polishing composition containing a compound having a secondary amine in its molecule and a water-soluble polymer having a weight-average molecular weight of 10,000 or more, the compound having a secondary amine being present at a concentration of 10 ppm to 100 ppm; a finish polishing step of finish-polishing the wafer after the post-rough polishing; The present invention provides a method for processing a wafer, comprising the steps of:
[0020] According to the wafer processing method of the present invention, the damage caused in the grinding step and the rough polishing step can be sufficiently removed at a high polishing rate, and therefore, according to the wafer processing method of the present invention, both a high polishing rate and a high defect reduction capability can be achieved.
[0021] In the post-rough polishing step, it is preferable to use the polishing composition containing at least a compound in which the secondary amine has a cyclic structure.
[0022] By using a polishing composition containing such a compound in the post-rough polishing step, a higher polishing rate can be achieved.
[0023] In the post-rough polishing step, it is more preferable to use the polishing composition containing at least a compound in which the secondary amine has a six-membered ring structure.
[0024] By using a polishing composition containing such a compound in the post-rough polishing step, a higher defect reduction capability can be realized and a higher polishing rate can be realized.
[0025] In the post-rough polishing step, it is preferable to use the polishing composition containing silicon dioxide (silica) as an abrasive.
[0026] From the viewpoint of purity, it is preferable to use such a polishing composition. Effect of the Invention
[0027] As described above, the wafer processing method of the present invention can sufficiently remove damage caused in the grinding step and the rough polishing step at a high polishing rate. Therefore, the wafer processing method of the present invention can achieve both a high polishing rate and a high defect reduction capability, and is a wafer processing method excellent in productivity and surface defect reduction. [Brief description of the drawings]
[0028] [Figure 1] FIG. 1 is a flow chart showing an example of a wafer processing method of the present invention. [Diagram 2] 1 is a diagram showing the polishing rates (relative values assuming that Comparative Example 1 is 1) in each of the wafer processing methods of Examples 1 to 5 and Comparative Examples 1 to 6. FIG. [Diagram 3] 1 is a diagram showing the total number of defects (relative values assuming that Comparative Example 1 is 1) in each of the wafer processing methods of Examples 1 to 5 and Comparative Examples 1 to 6. FIG. [Figure 4] 1 is a diagram showing the number of pit defects (a relative value with the total number of defects taken as 1) obtained by each of the wafer processing methods of Examples 1 to 5 and Comparative Examples 1 to 6. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] As described above, there has been a demand for the development of a wafer processing method that can achieve both a high polishing rate and a high defect reduction capability.
[0030] As a result of extensive research into the above-mentioned problems, the inventors have found that by using a polishing composition in the post-rough polishing process, which contains a compound having a secondary amine in its molecule and a water-soluble polymer having a weight-average molecular weight of 10,000 or more, and in which the concentration of the compound having a secondary amine is 10 ppm to 100 ppm, it is possible to achieve both a high polishing rate and a high defect reduction capability, and have completed the present invention.
[0031] That is, the present invention relates to a grinding step of surface grinding or lapping a wafer; a rough polishing step of roughly polishing the ground wafer; a post-rough polishing step of post-rough polishing the roughly polished wafer while supplying a polishing composition containing a compound having a secondary amine in its molecule and a water-soluble polymer having a weight-average molecular weight of 10,000 or more, the compound having a secondary amine being present at a concentration of 10 ppm to 100 ppm; a finish polishing step of finish-polishing the wafer after the post-rough polishing; The present invention relates to a wafer processing method.
[0032] Although Patent Documents 1 to 5 disclose a technique of incorporating an amine compound into a polishing composition, they do not describe or suggest that the polishing composition used in the post-rough polishing step contains a compound having a secondary amine in its molecule and a water-soluble polymer having a weight-average molecular weight of 10,000 or more.
[0033] The present invention will be described in detail below with reference to the drawings, but the present invention is not limited thereto.
[0034] FIG. 1 is a flow diagram showing an example of a wafer processing method of the present invention.
[0035] In the wafer processing method of the present invention, a grinding step of surface grinding or lapping a wafer and a step of roughly polishing the ground wafer are followed by a post-rough polishing step, as shown in Fig. 1. After the post-rough polishing step, a finish polishing step of finish-polishing the wafer is performed.
[0036] In the wafer processing method of the present invention, in the post-rough polishing step, the roughly polished wafer is post-rough polished while supplying a polishing composition containing a compound having a secondary amine in its molecule and a water-soluble polymer having a weight-average molecular weight of 10,000 or more, and the concentration of the compound having the secondary amine is 10 ppm to 100 ppm. The reason for carrying out such a post-rough polishing step will be described below.
[0037] In order to solve the above problems, the present inventors have investigated amines as additives to a polishing composition used in the post-rough polishing step.
[0038] As a result of the investigation, a significant increase in the polishing rate was observed, especially in secondary amines (compounds having a secondary amine).
[0039] The series of amines is determined by the number of alkyl groups bonded to the nitrogen atom. For example, if only one alkyl group is bonded and the rest are hydrogen atoms, it is called a primary amine; if two alkyl groups are bonded, it is called a secondary amine; and if three alkyl groups are bonded, it is called a tertiary amine.
[0040] Furthermore, among secondary amines, those having a cyclic structure and having a secondary amine group therein showed a particularly remarkable effect of increasing the polishing rate.
[0041] Generally, amines have high nucleophilicity, and as the amine series increases, the nucleophilicity increases. On the other hand, tertiary amines have reduced nucleophilicity due to steric hindrance, so secondary amines are the most nucleophilic.
[0042] In this case, it is believed that the high nucleophilicity of secondary amines promoted the chemical reaction on the silicon wafer surface.
[0043] In addition, the ring structure was able to achieve a higher polishing rate, which is thought to be because the two-dimensional molecular structure strengthens the interaction with the flat silicon wafer, resulting in a stronger chemical action.
[0044] It was found that the effect of increasing the polishing rate was remarkable when the amine concentration was increased to 10 ppm or more. However, if the concentration was increased too much, the pH of the post-coarse polishing composition would increase, which would increase the number of defects.
[0045] It is believed that the higher the pH, the stronger the chemical action during polishing, causing the damage that occurred during rough polishing to become apparent during polishing.
[0046] For this reason, the concentration of the compound having a secondary amine in the polishing composition was set to 10 ppm to 100 ppm.
[0047] It was also found that the addition of a water-soluble polymer as an additive other than amines reduced the number of defects that occurred in the post-rough polishing process.
[0048] The water-soluble polymer adsorbs to the polishing cloth and wafer in the polishing environment, and acts to reduce damage to the silicon wafer surface.
[0049] Among water-soluble polymers, the use of a water-soluble polymer having a weight-average molecular weight of 10,000 or more can particularly suppress the occurrence of defects.
[0050] In other words, by using a polishing composition in which a compound having a secondary amine that has the effect of increasing the polishing rate and a water-soluble polymer having a weight-average molecular weight of 10,000 or more are added together, and the concentration of the compound having a secondary amine is set to 10 ppm to 100 ppm, in a post-rough polishing process carried out between the rough polishing process and the finish polishing process, it is possible to achieve both a high polishing rate and suppression of defect occurrence.
[0051] On the other hand, even if the above polishing composition is used only in, for example, the rough polishing step or the finish polishing step without being used in the post-rough polishing step, it is not possible to achieve both a high polishing rate and a high defect reduction ability as in the present invention.
[0052] Each step in the wafer processing method of the present invention will now be described in detail.
[0053] 〇Grinding process In the grinding step, the wafer is subjected to surface grinding or lapping. Any commonly used surface grinding and lapping may be applied, and there is no particular limitation.
[0054] 〇Rough polishing process The rough polishing process is carried out to remove damage introduced in the grinding process. In order to remove damage, the rough polishing process polishes off 0.1 μm or more, preferably 0.3 μm or more, and more preferably 1 μm or more. On the other hand, to maintain flatness and productivity, it is preferable to polish off 30 μm or less, and more preferably 10 μm or less.
[0055] The rough polishing step may be either single-sided polishing or double-sided polishing.
[0056] In the rough polishing process, polishing is performed using hard polishing pads, such as urethane foam pads, nonwoven fabric pads made of resin-impregnated nonwoven fabric, or suede pads.
[0057] From the viewpoint of improving flatness, it is desirable to use a polishing pad that is as hard as possible, and it is desirable to use a polishing pad having a hardness of 70 or more on the A scale.
[0058] The polishing composition used in the rough polishing step preferably contains abrasive grains. Examples of the abrasive grains include metal oxides such as silicon dioxide, magnesium oxide, cerium oxide, aluminum oxide, and zirconium oxide, and silicon dioxide is particularly preferred from the viewpoint of purity.
[0059] From the viewpoint of ensuring the polishing rate, the silicon dioxide of the abrasive grains is preferably contained in the polishing composition used in the rough polishing step at 0.01 wt% or more, more preferably at 0.1 wt% or more. On the other hand, from the viewpoint of reducing damage in the rough polishing step, the content of silicon dioxide in the polishing composition used in the rough polishing step is preferably 30 wt% or less, more preferably 10 wt% or less.
[0060] The rough polishing composition may contain a basic compound in addition to the abrasive grains, such as lithium hydroxide, sodium hydroxide, potassium hydroxide, aluminum hydroxide, calcium hydroxide, sodium carbonate, potassium carbonate, calcium carbonate, ammonia, and tetramethylammonium hydroxide.
[0061] The pH of the polishing composition increases due to the basic compound, and from the viewpoint of accelerating the polishing rate, the pH of the polishing composition used in the rough polishing step is preferably 8.0 or more, more preferably 9.0 or more, and even more preferably 10.0 or more. Also, from the viewpoint of the stability of the abrasive grains, the pH is preferably 14.0 or less, more preferably 13.0 or less, and even more preferably 12.0 or less.
[0062] 〇Post rough polishing process The purpose of the post-rough polishing step is to remove the polishing damage generated in the rough polishing step and to reduce the removal amount required for the subsequent finish polishing step.
[0063] The removal amount in the post-rough polishing step strongly depends on the conditions of the rough polishing step, but is preferably 0.1 μm or more, more preferably 0.3 μm or more, whereas from the viewpoint of maintaining flatness, it is preferably 10 μm or less, more preferably 3 μm or less.
[0064] The post-rough polishing step may be either single-sided polishing or double-sided polishing.
[0065] In the post-rough polishing process, it is desirable to use a polishing pad that is softer than that used in the rough polishing process in order to reduce polishing damage. The polishing pad used should be a urethane foam pad, a nonwoven fabric pad made of resin-impregnated nonwoven fabric, or a suede pad.
[0066] Specifically, the hardness of the polishing cloth in the post-rough polishing step is smaller than the hardness of the polishing cloth in the rough polishing step and is desirably A-hardness 90 or less, more desirably A-hardness 80 or less. On the other hand, in order to improve flatness, the A-hardness is desirably A-hardness 40 or more, more desirably A-hardness 50 or more.
[0067] The polishing composition used in the post-polishing step contains a compound having a secondary amine in the molecule.
[0068] Examples of compounds having a secondary amine include piperazine derivatives and alcoholamine derivatives. Examples of piperazine derivatives include piperazine, 2-methylpiperazine, 2-pyrrolidinone, and 2-aminoethylpiperazine, and examples of alcoholamine derivatives include diethanolamine.
[0069] As the compound having a secondary amine, a compound having a cyclic structure is preferred for the reasons mentioned above, and a compound having a six-membered ring structure is more preferred.
[0070] The concentration of the compound having a secondary amine is set to 10 ppm to 100 ppm for the reasons mentioned above.
[0071] In order to reduce damage caused by polishing, a water-soluble polymer having a weight-average molecular weight of 10,000 or more is added to the polishing composition used in the post-rough polishing process. As the water-soluble polymer having a weight-average molecular weight of 10,000 or more, a cellulose derivative or polyvinyl alcohol is preferably used.
[0072] The average weight average molecular weight of the water-soluble polymer is preferably 10 million or less, more preferably 1 million or less, in order to reduce an increase in defects due to aggregation.
[0073] In order to reduce polishing damage, the water-soluble polymer having a weight-average molecular weight of 10,000 or more is preferably added to the polishing composition used in the post-rough polishing step at 1 ppm or more, more preferably 10 ppm or more. On the other hand, in order to prevent a decrease in the polishing rate, the amount is preferably 10,000 ppm or less, more preferably 1,000 ppm or less, and even more preferably 100 ppm or less.
[0074] The polishing composition used in the post-rough polishing step can further contain abrasive grains. Examples of abrasive grains include metal oxides such as silicon dioxide, magnesium oxide, cerium oxide, aluminum oxide, and zirconium oxide, and silicon dioxide is particularly preferred from the viewpoint of purity. That is, it is preferred to use a polishing composition containing silicon dioxide as abrasive grains in the post-rough polishing step.
[0075] The silicon dioxide of the abrasive grains contained in the post-coarse polishing composition is preferably contained in an amount of 0.01 wt% or more of the polishing composition from the viewpoint of ensuring the polishing rate, and more preferably 0.1 wt% or more. On the other hand, from the viewpoint of reducing damage in the post-coarse polishing step, it is preferably contained in an amount of 30 wt% or less, and more preferably 10 wt% or less.
[0076] The post-rough polishing composition may contain a basic compound other than the compound having a secondary amine. Examples of the basic compound include lithium hydroxide, sodium hydroxide, potassium hydroxide, aluminum hydroxide, calcium hydroxide, sodium carbonate, potassium carbonate, calcium carbonate, ammonia, and tetramethylammonium hydroxide.
[0077] The pH of the polishing composition is increased by the compound having secondary amine and the basic compound, and from the viewpoint of polishing rate acceleration, the pH is preferably 8.0 or more, more preferably 9.0 or more, and even more preferably 10.0 or more. Also, from the viewpoint of abrasive grain stability, the pH is preferably 14.0 or less, more preferably 13.0 or less, and even more preferably 12.0 or less.
[0078] 〇Final polishing process After the post-rough polishing process, the wafer is transferred to the final polishing process.
[0079] The purpose of the final polishing step is to remove micro-roughness.
[0080] The removal amount in the final finish polishing step is preferably 1 nm or more, more preferably 3 nm or more, although it depends strongly on the conditions in the rough polishing step and the post-rough polishing step, whereas from the viewpoint of maintaining flatness, it is preferably 100 nm or less, more preferably 30 nm or less.
[0081] The final polishing step may be either single-sided or double-sided polishing.
[0082] In the final finish polishing process, it is desirable to use a polishing pad that is softer than that used in the post-rough polishing process in order to reduce polishing damage. The polishing pad can be a urethane foam pad, a nonwoven fabric pad made of resin-impregnated nonwoven fabric, or a suede pad, with the suede pad being the most preferable.
[0083] Specifically, the hardness of the polishing cloth in the finish polishing step is smaller than the hardness of the polishing cloth in the post-rough polishing step and is desirably A-hardness 80 or less, more desirably A-hardness 70 or less. On the other hand, in order to improve flatness, the A-hardness is desirably A-hardness 30 or more, more desirably A-hardness 40 or more.
[0084] Examples of abrasive grains used in the finish polishing step include metal oxides such as silicon dioxide, magnesium oxide, cerium oxide, aluminum oxide, and zirconium oxide, with silicon dioxide being particularly preferred from the standpoint of purity.
[0085] The silicon dioxide content of the abrasive grains contained in the final polishing composition is preferably 0.01 wt% or more, more preferably 0.1 wt% or more, of the polishing composition from the viewpoint of ensuring the polishing rate, while being preferably 30 wt% or less, more preferably 10 wt% or less, from the viewpoint of reducing damage during the rough polishing step.
[0086] The finish-polishing composition may contain a basic compound in addition to the abrasive grains, such as lithium hydroxide, sodium hydroxide, potassium hydroxide, aluminum hydroxide, calcium hydroxide, sodium carbonate, potassium carbonate, calcium carbonate, ammonia, or tetramethylammonium hydroxide.
[0087] The pH of the polishing composition is increased by the basic compound, and from the viewpoint of accelerating the polishing rate, the pH is preferably 7.0 or more, more preferably 8.0 or more. From the viewpoint of the stability of the abrasive grains, the pH is preferably 14.0 or less, more preferably 13.0 or less, and even more preferably 12.0 or less.
[0088] The final polishing composition may contain a water-soluble polymer to reduce polishing damage. As the water-soluble polymer, a cellulose derivative or polyvinyl alcohol is preferably used.
[0089] In order to reduce polishing damage, the water-soluble polymer preferably has a weight-average molecular weight of 100 or more, more preferably 1000 or more. On the other hand, in order to reduce an increase in defects due to aggregation, the weight-average molecular weight is preferably 10 million or less, more preferably 1 million or less.
[0090] In order to reduce polishing damage, the water-soluble polymer is preferably added in an amount of 1 ppm or more, more preferably 10 ppm or more, while in order to prevent a decrease in the polishing rate, the amount is preferably 10,000 ppm or less, more preferably 1,000 ppm or less, and even more preferably 100 ppm or less.
[0091] In addition to the abrasive grains, basic compounds, and water-soluble polymers, amines may be added to increase the polishing rate. Examples of amines include piperazine derivatives and alcoholamine derivatives. Examples of piperazine derivatives include piperazine, 2-methylpiperazine, 2-pyrrolidinone, and 2-aminoethylpiperazine, and examples of alcoholamine derivatives include monoethanolamine, diethanolamine, and triethanolamine.
[0092] The concentration of the amines is preferably 1 ppm or more, more preferably 10 ppm or more, from the viewpoint of the polishing rate, while being 10,000 ppm or less, more preferably 1,000 ppm or less, and even more preferably 100 ppm or less, in order to prevent deterioration of the surface roughness.
[0093] Cleaning process A cleaning step may be performed in which the wafer after the polishing step is cleaned with a chemical solution, which may be appropriately selected from, for example, ammonia, sodium hydroxide, potassium hydroxide, hydrogen peroxide, hydrochloric acid, sulfuric acid, citric acid, hydrofluoric acid, ozone water, and the like, as required.
[0094] Inspection process The wafer surface defects are determined by, for example, counting the number of defects with a grain size of 26 nm or more using a Surfscan SP3 manufactured by KLA-Tencor Corporation.
[0095] When investigating the actual state of the above defects, a defect review inspection may be performed using a confocal optical system, for example, a defect inspection and review device MAGICS (M5640) manufactured by Lasertec Corporation.
[0096] By analyzing the review image, it is possible to determine whether the defect is convex or concave. A concave shape generally indicates that damage from grinding or rough polishing remains.
[0097] The wafer to be processed by the wafer processing method of the present invention is not particularly limited, but for example, a silicon wafer can be used as the processing target. EXAMPLES
[0098] The present invention will be specifically described below using examples and comparative examples, but the present invention is not limited to these.
[0099] In each of the following Examples and Comparative Examples, after the rough polishing step, a post-rough polishing step was carried out by single-sided polishing. The processing flow was as shown in Figure 1, in the order of a grinding step (specifically, a surface grinding step), a rough polishing step, a post-rough polishing step, and a finish polishing step.
[0100] In the Examples and Comparative Examples, the polishing compositions used in the post-rough polishing step were prepared as follows.
[0101] (Comparative Examples 1 to 6) In Comparative Example 1, a post-rough polishing step was carried out using a polishing composition prepared by using colloidal silica as abrasive grains and potassium hydroxide as alkali, without adding a water-soluble polymer or amines.
[0102] In Comparative Example 2, a post-rough polishing process was carried out using a polishing composition prepared in the same manner as in Comparative Example 1, except that 100 ppm of hydroxyethyl cellulose (weight average molecular weight 250,000) was added as a water-soluble polymer.
[0103] In Comparative Example 3, a polishing composition was prepared in the same manner as in Comparative Example 1, except that in addition to the same hydroxyethyl cellulose as that added in Comparative Example 2, 30 ppm of monoethanolamine was added as an amine.
[0104] In Comparative Example 4, a polishing composition was prepared in the same manner as in Comparative Example 1 except that, instead of the monoethanolamine used in Comparative Example 3, 30 ppm of triethanolamine was added.
[0105] In Comparative Example 5, a polishing composition was prepared in the same manner as in Comparative Example 1 except that no hydroxyethyl cellulose was added and only piperazine was added as the amine in an amount of 30 ppm.
[0106] In Comparative Example 6, a polishing composition was prepared in the same manner as in Comparative Example 2, except that the amount of piperazine added was increased from 30 ppm in Comparative Example 5 to 300 ppm together with the hydroxyethyl cellulose.
[0107] (Examples 1 to 5) In Example 1, a polishing composition was prepared in the same manner as in Comparative Example 2, except that 30 ppm of piperazine was added together with hydroxyethyl cellulose.
[0108] In Example 2, a polishing composition was prepared in the same manner as in Example 1 except that 90 ppm of piperazine was added together with hydroxyethyl cellulose.
[0109] In Example 3, a polishing composition was prepared in the same manner as in Example 1 except that 30 ppm of 2-methylpiperazine was added together with hydroxyethyl cellulose.
[0110] In Example 4, a polishing composition was prepared in the same manner as in Example 1 except that 30 ppm of 2-pyrrolidinone was added together with hydroxyethyl cellulose.
[0111] In Example 5, a polishing composition was prepared in the same manner as in Example 1 except that 30 ppm of 2-aminoethylpiperazine was added together with hydroxyethyl cellulose.
[0112] In each of the Examples and Comparative Examples, these post-rough polishing compositions were prepared, and post-rough polishing was carried out while supplying the polishing composition so that the removal amount of the wafer after rough polishing was 1 μm.
[0113] After that, the wafers were subjected to finish polishing, the surfaces of the wafers were cleaned in a cleaning process, and various inspections were carried out.
[0114] 2 and 3 show the polishing rate and the total number of defects in each of the wafer processing methods of Examples 1 to 5 and Comparative Examples 1 to 6, as relative values with Comparative Example 1 being set to 1. Also, FIG. 4 shows the number of concave defects (relative values when the total number of defects in each method is set to 1) in each of the wafer processing methods of Examples 1 to 5 and Comparative Examples 1 to 6. Also, the following Table 1 shows the components of the polishing compositions used in the post-rough polishing step in Examples 1 to 5 and Comparative Examples 1 to 6, as well as the inspection results for each example.
[0115] [Table 1]
[0116] As a result, as can be seen from Fig. 2 and Table 1, it can be seen that the polishing rate is increased in Comparative Example 5, in which piperazines are added, compared to Comparative Example 1. However, in Comparative Example 5, the total number of defects and the number of concave defects are both larger than those in Comparative Example 1. This is considered to be because the polishing composition used in the post-rough polishing process of Comparative Example 5 does not contain a water-soluble polymer.
[0117] On the other hand, from Fig. 3 and Table 1, in Examples 1 to 5 in which a water-soluble polymer having a weight average molecular weight of 10,000 or more was added together with a compound having a secondary amine such as piperazines at a concentration of 10 ppm to 100 ppm to the polishing composition used in the post-rough polishing step, the polishing rate was equal to or higher than that of Comparative Example 1, as shown in Fig. 2 and Table 1, while the total number of defects after the finish polishing was reduced compared to Comparative Example 1. In particular, in Examples 1 to 3 and 5 in which a water-soluble polymer having a weight average molecular weight of 10,000 or more was added together with piperazines at a concentration of 10 ppm to 100 ppm to the polishing composition used in the post-rough polishing step, as shown in Fig. 2 and Table 1, an increase in the polishing rate was observed compared to Comparative Example 1, and the total number of defects after the finish polishing was reduced compared to Comparative Example 1.
[0118] In addition, by reviewing the above defects and comparing the number of pit defects, it is found that, as shown in FIG. 4 and Table 1, the number of pit defects in Examples 1 to 5 all tended to decrease.
[0119] That is, in Examples 1 to 5, both a high polishing rate and a high defect reduction capability were achieved.
[0120] This result is believed to be due to the fact that the addition of a compound having a secondary amine, such as piperazines, at a concentration of 10 ppm to 100 ppm increased the polishing rate in the post-rough polishing process, reduced polishing damage before the rough polishing process, and reduced concave defects.
[0121] It is also believed that the addition of hydroxyethyl cellulose having a weight-average molecular weight of 10,000 or more as a water-soluble polymer to the polishing composition used in the post-rough polishing process has also contributed greatly to the reduction in defects that occur in the post-rough polishing process.
[0122] On the other hand, in Comparative Examples 2 to 4 in which a compound having a secondary amine was not added to the polishing composition used in the post-rough polishing step, the polishing rate was lower and the total number of defects and the number of concave defects were larger than those in Examples 1 to 5, as is clear from Figures 2 to 4 and Table 1. In particular, a comparison of Examples 1, 3 to 5 and Comparative Examples 3 and 4 in which the amount of amines added was about the same shows that a high polishing rate and a high defect reduction ability cannot be achieved at the same time when a compound having a primary amine or a tertiary amine is used.
[0123] 2 to 4, the total number of defects and the number of concave defects were also large in Comparative Example 6. This is believed to be because the content of piperazine in the polishing composition used in the post-rough polishing step in Comparative Example 6 was too high, resulting in an increase in defects.
[0124] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.
Claims
1. a grinding step of surface grinding or lapping the wafer; a rough polishing step of roughly polishing the ground wafer; a post-rough polishing step of post-rough polishing the roughly polished wafer while supplying a polishing composition containing a compound having a secondary amine in its molecule and a water-soluble polymer having a weight-average molecular weight of 10,000 or more, the compound having the secondary amine being present at a concentration of 10 ppm to 100 ppm; a finish polishing step of finish-polishing the wafer after the post-rough polishing; A wafer processing method comprising the steps of:
2. 2. The method for processing a wafer according to claim 1, wherein the polishing composition contains at least a compound in which the secondary amine has a cyclic structure in the post-rough polishing step.
3. 3. The method for processing a wafer according to claim 2, wherein the polishing composition contains at least a compound in which the secondary amine has a six-membered ring structure in the post-rough polishing step.
4. 4. The wafer processing method according to claim 1, wherein the polishing composition contains silicon dioxide as an abrasive in the post-rough polishing step.
Citation Information
Patent Citations
Slurry composition for final polishing of silicon wafer, and method for final polishing of silicon wafer using the same
JP2008147651A
Polishing composition
JP2016124943A
Polishing liquid composition for silicon wafer
JP2017011220A
Polishing composition
JP2019119854A
Method for reclaiming semiconductor wafer and polishing composition
WO2011093223A1