Floor coating method and floor coating
The coating method addresses the inefficiencies of existing floor construction by using a water-based urethane concrete composition to form stable unevenness and anti-slip properties, enabling rapid and durable floor creation.
Patent Information
- Application Number
- JP2022064717
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-04-08
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2042-04-08
AI Technical Summary
Existing methods for constructing slip-resistant floors are lengthy and complicated due to the need for multiple repetitions of troweling and compaction processes, and they fail to provide durable anti-slip properties by forming physical irregularities on the surface.
A coating method involving a base conditioning step, undercoating with a first aggregate, rolling compaction, spreading a second aggregate, and applying a topcoat after the undercoat hardens, using a water-based hard urethane concrete composition that forms urethane and urea bonds through hydration reactions.
This method allows for the stable formation of irregularities, resulting in a durable and highly slip-resistant floor surface that can be constructed in a shorter time frame, maintaining anti-slip properties and aesthetic qualities.
Smart Images

Figure 0007556561000003 
Figure 0007556561000002 
Figure 0007556561000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating floor construction method and a coated floor that construct a floor surface with durable and highly slip-resistant properties in a short period of time. [Background technology]
[0002] Conventionally, floor surfaces such as concrete in factories and maintenance garages are not suitable for working environments because, as is, they generate dust, oil seep in, and chip when tools or other objects are dropped on them. To solve these problems, floor coatings have been applied to the floor surfaces.
[0003] Additionally, in environments where the floor surface is likely to be covered with liquids such as water or oil, for example in food factories and kitchens, floor coatings made from materials with excellent anti-slip properties can be applied, or floor coatings containing aggregate of a specified particle size can be applied to create physical irregularities on the floor surface.
[0004] In such a situation, for example, the technology described in Patent Document 1 discloses a method for forming a coated floor, in which an aqueous hard urethane concrete composition containing aggregate is applied to a base by troweling, the applied surface obtained by troweling is further compressed by a rolling means, and the aqueous hard urethane concrete composition is hardened to form a coated floor of aqueous hard urethane concrete.
[0005] This technology is said to be capable of improving the strength, abrasion resistance, and surface appearance of coated floors made of water-based hard urethane concrete that contains aggregate.
[0006] For example, in the technology disclosed in Patent Document 2, a primer is applied to the base, and then a A coating floor method has been disclosed in which aggregate is spread on the surface before the undercoat hardens, and the undercoat is hardened to fix the aggregate, after which the coating floor material is applied.
[0007] This technology is said to enable low-fluidity floor coating materials to be applied evenly to a smooth base without the material slipping. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2016-138385 A [Patent Document 2] JP 2001-207631 A Summary of the Invention [Problem to be solved by the invention]
[0009] Indeed, the technology described in Patent Document 1 is advantageous in that the inclusion of aggregate can improve the strength and abrasion resistance of the coated floor, and furthermore, the proportion of the expensive main component of the coated floor material can be kept low by using the aggregate.
[0010] However, because workers cannot walk on the coated surface obtained by troweling before it hardens, they must either compact the area they can compact with a compaction roller from an untreated area, or compact the area from scaffolding or the like that does not affect the coated surface.
[0011] In the former case, the area that can be compacted at one time is limited, so the troweling and compacting of the base must be repeated multiple times, resulting in a long construction time. In the latter case, scaffolding must be set up, making the work extremely complicated, and the scaffolding can only be removed after the painted surface has hardened, resulting in a long construction time.
[0012] In addition, this technology uses rolling compaction to cause the aggregate to settle and move downward, so it is not possible to provide anti-slip properties by forming physical unevenness on the surface with the aggregate.
[0013] Furthermore, the technology described in Patent Document 2 is indeed advantageous in that when a low-fluidity floor coating material is applied to a smooth base, if the surface of the undercoat is first made uneven with aggregate, this prevents the floor coating material from slipping against the undercoat.
[0014] However, because workers cannot walk on the coated surface before the primer hardens, in order to spread aggregate (and compact it to help the aggregate adhere) before the primer hardens, workers must either spread (or compact) the area from an untreated area, or compact it from scaffolding or the like that does not affect the coated surface.
[0015] In the former case, the area that can be sprayed (or compacted) at one time is limited, so the primer coat (and compaction) on the base must be repeated multiple times, resulting in a long construction time. In the latter case, scaffolding must be set up, making the work very complicated, and the scaffolding can only be removed after the primer has hardened, resulting in a long construction time.
[0016] Thus, the technology according to Patent Document 2 also has the same problem as Patent Document 1 in that the construction time is lengthened.
[0017] Furthermore, the technology disclosed in Patent Document 2 is a technology for preventing the coated floor material from slipping during work, but since the coated floor material is simply applied on top of an undercoat, the aggregate itself in the coated floor material cannot be fixed to the undercoat, and therefore the anti-slip properties and abrasion resistance cannot be maintained over the long term.
[0018] The present invention has been made in consideration of the above circumstances, and has an object to provide a coating floor method and a coated floor that can construct a floor surface with durable and highly slip-resistant properties in a short period of time. [Means for solving the problem]
[0019] In order to achieve the above object, the present invention provides the following techniques.
[0020] In the invention according to claim 1, the method includes a surface preparation step of preparing a base, a basecoat step of applying a basecoat material containing a first aggregate to the surface of the basecoat that has been subjected to the surface preparation step, a first rolling step of compressing the surface of the basecoat material, a scattering step of scattering a second aggregate onto the surface of the basecoat material that has been subjected to the surface preparation step before the basecoat material hardens, a second rolling step of compressing the surface onto which the basecoat material has been scattered, and a topcoat step of applying a topcoat material after the basecoat material hardens. After the surface preparation process, the base is divided into a plurality of adjacent work areas, and the first work area is subjected to the undercoat process through the second rolling process. After that, the undercoat process through the second rolling process are repeated for the adjacent work areas in sequence until all work areas are completed. After the undercoat material has hardened, the topcoat process is performed for all work areas. The present invention aims to provide a floor coating method characterized by the above-mentioned.
[0022] Claim 2 In the invention according to the present invention, the undercoat material is an aqueous hard urethane-based concrete composition that contains the first aggregate, forms urethane bonds and urea bonds with polyol, isocyanate, and water, and forms concrete by a hydration reaction with cement and water. 1 to The purpose of this invention is to provide the floor coating method described above.
[0023] Claim 3 In the invention according to the present invention, the thickness of the undercoat material is about 4.0 mm to about 7.0 mm, the thickness of the topcoat material is about 0.1 mm to about 0.3 mm, the particle size of the first aggregate is about 2.0 mm to 3.0 mm, and the particle size of the second aggregate is about 0.5 mm to 2.0 mm. 2 The present invention aims to provide a floor coating method as described above. Effect of the Invention
[0025] According to the invention described in claim 1, the process comprises a base preparation step for preparing the base, an undercoat step for applying a basecoat containing a first aggregate to the surface of the prepared base, a first rolling step for compacting the surface of the basecoat, a spraying step for spraying a second aggregate onto the rolled surface of the basecoat before the basecoat hardens, a second rolling step for compacting the surface onto which the basecoat has been sprayed, and a topcoat step for applying a topcoat after the basecoat has hardened.As a result, the second aggregate can be adhered in a layered manner onto the first aggregate before the basecoat hardens, and the second aggregate can be used to stably form an uneven surface, allowing the construction of a durable floor surface with high anti-slip properties.
[0026] In addition, because a stable unevenness can already be formed before the topcoat process, the topcoat can be formed as a thin film, and topcoats with individual functions such as coloring to improve aesthetics, abrasion resistance, and chemical resistance can be used flexibly without compromising the anti-slip properties.
[0027] Furthermore After the surface preparation process, the base is divided into a number of adjacent work areas, and the first work area is subjected to the undercoat process through the second rolling process. The undercoat process through the second rolling process are then repeated for the adjacent work areas in sequence until all work areas are completed. After the undercoat material has hardened, the topcoat process is performed on all work areas. This allows all work areas up to the second rolling process to be completed in one go even if the work area is large, and furthermore, once the undercoat material in the work area that has completed the final rolling process has hardened, the topcoat process can be performed on all work areas in one go, allowing work to be completed in a short amount of time.
[0028] Claim 2According to the described invention, the undercoat material contains a first aggregate, and is an aqueous hard urethane concrete composition that forms urethane bonds and urea bonds with polyol, isocyanate, and water, and forms concrete through a hydration reaction with cement and water.As a result, it has excellent impact resistance and abrasion resistance, as well as heat resistance and chemical resistance, and therefore can be widely used as a floor material with excellent durability required for food factories, machine factories, and industrial floors, and the particle size and content of the first aggregate can be easily adjusted.
[0029] Claim 3 According to the described invention, the thickness of the undercoat material is approximately 4.0 mm to approximately 7.0 mm, the thickness of the topcoat material is approximately 0.1 mm to approximately 0.3 mm, the particle size of the first aggregate is approximately 2.0 mm to 3.0 mm, and the particle size of the second aggregate is approximately 0.5 mm to 2.0 mm. This allows the second aggregate to be stably layered on top of the first aggregate, and therefore the second aggregate can be used to stably form an uneven surface, allowing the construction of a floor surface with high slip resistance. [Brief description of the drawings]
[0031] [Figure 1] FIG. 1 is a flow diagram of a floor coating method according to an embodiment of the present invention. [Diagram 2] FIG. 11 is a plan view showing the state of the undercoat application area in the floor coating method according to this embodiment, where (a) is before the undercoat process, (b) is a diagram of the divided work areas, (c) is a diagram of the first work area after construction, (d) is a diagram of the fifth work area after construction, (e) is a diagram of the tenth work area after construction, and (f) is a diagram of the completion of the undercoat application for all work areas. [Diagram 3] FIG. 2 is a simplified cross-sectional view of a coated floor constructed by the coating floor construction method according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] The gist of the floor coating method according to the embodiment of the present invention is characterized by comprising a base preparation step of preparing the base, a base coating step of applying a base coating material containing a first aggregate to the surface of the base coating, a first rolling step of compressing the surface of the base coating material, a scattering step of scattering a second aggregate on the surface of the base coating material before the base coating material hardens, a second rolling step of compressing the surface on which the base coating material has been scattered, and a top coating step of applying a top coating material after the base coating material hardens. In other words, the present invention aims to provide a floor coating method that constructs a floor surface with high anti-slip properties and durability in a short time.
[0033] As shown in Figs. 1 and 2, the floor coating method according to the embodiment of the present invention includes a surface preparation step S1 for preparing a surface of a base G, a base coating step S2 for applying a base coating material 2 containing a first aggregate 1 to the surface of the base coating material G, a first rolling step S3 for rolling the surface of the base coating material 2, a spraying step S4 for spraying a second aggregate 3 on the rolled surface of the base coating material 2 before the base coating material 2 hardens, a second rolling step S5 for rolling the surface on which the base coating material 2 has been sprayed, and a top coating step for applying a top coating material 4 after the base coating material 2 has hardened. S6 It consists of:
[0034] In addition, after the base preparation process S1, the base G is divided into a number of adjacent work areas, and the first work area g1, which serves as the starting point, is subjected to the undercoat process S2 through the second rolling process S5. After that, the undercoat process S2 through the second rolling process S5 are repeated for the adjacent work areas (g2 and onwards) in sequence until all work areas have been completed. After the undercoat material 2 has hardened, the topcoat process S6 is performed on all work areas.
[0035] The undercoat material 2 is an aqueous hard urethane concrete composition that contains the first aggregate 1, forms urethane bonds and urea bonds with polyol, isocyanate, and water, and forms concrete through a hydration reaction with cement and water.
[0036] In addition, the coated floor is formed using materials in which the thickness of the undercoat material 2 is approximately 4.0 mm, the thickness of the topcoat material 4 is approximately 0.15 mm, the particle size of the first aggregate 1 is approximately 2.5 mm, and the particle size of the second aggregate 3 is approximately 1.0 mm; however, it is also possible to use materials in which the thickness of the undercoat material 2 is approximately 4.0 mm to approximately 7.0 mm, the thickness of the topcoat material 4 is in the range of approximately 0.1 mm to approximately 0.3 mm, and the particle size of the first aggregate 1 is approximately 2.0 mm to approximately 3.0 mm, and the particle size of the second aggregate 3 is approximately 0.5 mm to 2.0 mm.
[0037] Furthermore, the topcoat step S6 is carried out approximately two hours after the undercoat step S2 is completed.
[0038] The floor coating method according to this embodiment will be described in detail below.
[0039] The base G may be concrete, mortar, a painted floor, etc., and is not particularly limited, but in this embodiment, a painted floor construction method will be described as being intended for concrete.
[0040] The construction area G described in the floor coating method according to this embodiment is, as shown in the plan view of FIG. 2(a), approximately L-shaped in plan view and has a construction area of 49.0 mm 2 (T1=5.0m, T2=8.0m, T3=3.0m, T4=3.0m), and all spaces except T4 are described as being surrounded by walls.
[0041] As shown in Fig. 2(b), the construction area G is divided into eight work areas g1 to g15 (t1, t2, t3 = 1.0 m), and the work areas are divided into the first work area g1 on the north side, which is the starting point, and the work areas g1,..., g8 to g12 on the south side, and east Construction will then proceed sequentially to work areas g13 to g15 on the side.
[0042] Regarding the division of the work area G, it goes without saying that the size of the work area and the number of divisions can be changed appropriately depending on the situation, so long as the second compaction process S5 can be completed in one go.
[0043] The undercoat material 2 described in the floor coating method according to this embodiment is prepared by mixing a first liquid (Yutak Complete CPM A liquid by Nippon Tokushu Toryo Co., Ltd.) whose main components are polyol and water, a second liquid (Yutak Complete CPM B liquid by Nippon Tokushu Toryo Co., Ltd.) whose main component is isocyanate, and a first aggregate 1 made of cement consisting of powder with a particle size of approximately 0.1 mm to 0.3 mm and the above-mentioned ceramic aggregate.
[0044] In addition, the resin produced by the reaction between the first liquid and the second liquid exhibits flexibility, impact resistance, and abrasion resistance due to the urethane bonds, and exhibits chemical resistance, abrasion resistance, toughness, and adhesion due to the urea bonds, and concrete, which is made of cement and water, can achieve improved heat resistance, adhesion, and strength due to the hydration reaction.
[0045] In addition, the undercoat material 2 may be mixed with a hardening accelerator or a coloring agent that acts as a pigment to exhibit hardening acceleration properties and aesthetic appearance.
[0046] Specifically, the construction area shown in Figure 2(a) is 49.0 mm 2 For the application area G, approximately 36 kg of the first liquid, approximately 36 kg of the second liquid, and approximately 324 kg of a mixture of cement and the first aggregate 1 are used, and a coating film approximately 4.0 mm thick is formed using the primer 2 obtained by mixing and stirring these.
[0047] Next, in the base material adjustment process S1, after removing dust and foreign matter from the surface, any remaining laitance, efflorescence, and oils are thoroughly removed. On the flat parts, U-shaped groove joints 10 mm wide and 10 mm deep are formed at intervals of up to 5 m, and similar U-shaped grooves are also formed at the boundaries with the edges of walls, etc.
[0048] In the surface preparation step S1, it is necessary that the substrate is sufficiently dry and free of floating water.
[0049] Furthermore, it is sufficient if the work area is large enough to allow all work areas to be completed at once for the subsequent processes, but if it is necessary to divide the work area into multiple work areas for construction, it is desirable to clearly mark the work areas on the floor with masking tape or the like so that they can be identified in advance, as shown in Figure 2(b).
[0050] In the undercoating step S2, a topcoat material 4 containing a first aggregate 1 is applied to the base by a trowel such as a metal trowel, and in this embodiment, this is performed within 15 minutes for one work area.
[0051] The first rolling process S3 is carried out immediately after the undercoating process S2. The rolling process is carried out by rolling the sand roller without pressing the coating surface. Come Repeat multiple times to the extent necessary.
[0052] In this embodiment, a sand and bone roller is used for compaction, but other rollers such as a wool roller, a mastic roller, or a head cut roller may also be used, and the present invention is not limited to this embodiment.
[0053] The spreading step S4 is carried out immediately after the first compaction step S3. In this embodiment, as described above, the alumina aggregate having a particle size of approximately 1.0 mm is spread uniformly by hand spreading. When spreading by hand, the distance at which the hand can be stretched out from the untreated area and the spread can be carried out stably is set to approximately 1.0 m. Therefore, in this embodiment, all the working areas g1 to g15 are divided taking into consideration the length at which hand spreading is possible.
[0054] In this embodiment, alumina aggregate is used as the second aggregate 3, and in a broader sense, ceramic aggregate can also be used. However, since ceramic aggregate has poor uniformity in particle size, it is preferable to use a material with a particle size in the range of approximately 0.5 mm to 2.0 mm. Silica sand (No. 4: 0.6 mm to 1.12 mm) can also be used.
[0055] In addition, in this embodiment, the spraying is performed by hand, but other devices such as a lysine gun or a blower may also be used, and the method is not limited to this embodiment.
[0056] In addition, it is desirable for the second aggregate 3 to be scattered to have a similar color to that of the undercoat material 2 in terms of aesthetic appeal.
[0057] The second rolling step S5 is carried out immediately after the spreading step S4, and is carried out by rolling the sand roller in a stroking manner rather than pressing against the application surface. In this case, it is necessary to carry out the work with an even weaker force than the second rolling step S5.
[0058] In this embodiment, a sand and bone roller is used for compaction, but other rollers such as a wool roller, a mastic roller, or a head cut roller may also be used, and the present invention is not limited to this embodiment.
[0059] The base G thus prepared is then subjected to the undercoat process S2 through the second compaction process S5. However, if the work is divided into multiple work areas, for example, as shown in Figures 2(b) to (f), the undercoat process S2 through the second compaction process S5 are carried out on the first work area g1, which serves as the starting point, and then the undercoat process S2 through the second compaction process S5 are repeated for adjacent work areas in sequence until all work areas are completed.
[0060] Once the second compaction step S5 has been completed for all work areas, the topcoat step S6 can be carried out using a roller or brush approximately two hours after the final application of the undercoat material 2 has been completed.
[0061] In this embodiment, after 2 hours or more have passed since application of the above-mentioned undercoat material 2, it is possible to walk on the coated surface without any damage, and the topcoat step S6 can be carried out.
[0062] The topcoat material 4 used in the topcoat process S6 is not particularly limited, but in this embodiment, since stable unevenness can already be formed in the previous process, the topcoat material 4 is applied using the following material, which is a thin film and emphasizes anti-slip properties.
[0063] The topcoat material 4 described in the floor coating method according to this embodiment is prepared by mixing a third liquid whose main components are polyol and water (Nihon Tokushu Toryo Co., Ltd.: U-TAC Complete GA Liquid), a fourth liquid whose main component is isocyanate (Nihon Tokushu Toryo Co., Ltd.: U-TAC Complete GB Liquid), and cement consisting of powder (Nihon Tokushu Toryo Co., Ltd.: U-TAC Complete T Powder).
[0064] Specifically, the construction area shown in Figure 2(a) is 49.0 mm 2 For the application area G, approximately 2 kg of the third liquid, approximately 2 kg of the fourth liquid, and approximately 3 kg of cement are used, and these are mixed and stirred to obtain the topcoat material 4, which is used to form a coating film approximately 0.15 mm thick.
[0065] Therefore, in this embodiment, by forming a top coat material 4 on a base coat material 2 having a thickness of approximately 4.0 mm, a coated floor having a thickness of approximately 4.15 mm is formed from the base G, and the area where the second aggregate 3 emerges has a maximum thickness of approximately 5.15 mm, forming a well-defined uneven surface.
[0066] In the topcoat process S6, the prepared topcoat material 4 is applied to the surface of the undercoat material 2 by a roller. In this case, the work can be performed on all application areas G in one go, and in this embodiment, this is completed within 7 minutes, forming a coating film as shown in Figure 3.
[0067] In this embodiment, a wool roller is used for top coating, but a mastic roller, a head cut roller, a brush, etc. may also be used, and the present invention is not limited to this embodiment.
[0068] As described above, the floor coating method according to this embodiment includes a base preparation step S1 for preparing the base of the base G, a base coating step S2 for applying the base coating material 2 containing the first aggregate 1 to the surface of the base coating material G that has been prepared, a first rolling step S3 for compacting the surface of the base coating material 2, a spraying step S4 for spraying the second aggregate 3 on the rolled surface of the base coating material 2 before the base coating material 2 hardens, a second rolling step S5 for compacting the surface on which the base coating material 2 has been sprayed, and a top coating step S6 for applying the top coating material 4 after the base coating material 2 hardens. Therefore, the second aggregate 3 can be laminated and fixed on the first aggregate 1 before the base coating material 2 hardens, so that the surface can be stably formed with the second aggregate 3, and a floor surface with high durability and high slip resistance can be constructed.
[0069] In addition, since a stable unevenness can already be formed before the topcoat process S6, the topcoat material 4 can be formed as a thin film, and topcoat materials with individual functions such as coloring to improve aesthetics, abrasion resistance, and chemical resistance can be used flexibly without compromising the anti-slip properties.
[0070] In addition, after the base preparation step S1, the base G is divided into a number of adjacent work areas, and the first work area g1, which serves as the starting point, is subjected to the undercoat step S2 through the second rolling step S5. Then, the undercoat step S2 through the second rolling step S5 are repeated for the adjacent work areas (g2 and onwards) in sequence until all work areas are completed. After the undercoat material 2 has hardened, the topcoat step S6 is performed on all work areas. This allows all work areas up to the second rolling step S5 to be worked on at once, even if the work area is large. Moreover, once the undercoat material 2 in the work area where the final second rolling step S5 has been completed has hardened, the topcoat step S6 can be performed on all work areas at once, allowing work to be completed in a short time.
[0071] In addition, the undercoat material 2 contains the first aggregate 1 and is an aqueous hard urethane concrete composition that forms urethane bonds and urea bonds with polyol, isocyanate, and water, and forms concrete through a hydration reaction with cement and water. Therefore, it has excellent impact resistance and abrasion resistance, as well as heat resistance and chemical resistance, and can be widely used as a floor material with excellent durability required for food factories, machine factories, and industrial floors. The particle size and content of the first aggregate 1 can also be easily adjusted.
[0072] Furthermore, by setting the thickness of the undercoat material to approximately 4.0 mm to approximately 7.0 mm, the thickness of the topcoat material to approximately 0.1 mm to approximately 0.3 mm, the particle size of the first aggregate to approximately 2.0 mm to 3.0 mm, and the particle size of the second aggregate to approximately 0.5 mm to 2.0 mm, the second aggregate 3 can be stably layered on top of the first aggregate 1, so that the surface can be stably formed with the second aggregate 3, and a floor surface with high slip resistance can be constructed.
[0073] Furthermore, by using the floor coating method according to the present invention, a floor surface with high anti-slip properties can be provided.
[0074] Although a preferred embodiment of the present invention has been described above, the present invention is not limited to such a specific embodiment, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]
[0075] G. Base g1 working area (first) g2 work area g3 work area g4 work area g5 work area g6 work area g7 work area g8 work area g9 work area g10 work area g11 work area g12 work area g13 working area g14 work area g15 Work area (last) S1 Base material preparation process S2 Undercoating process S3 First rolling process S4 Spraying process S5 Second rolling process S6 Top coating process 1. First aggregate 2. Undercoat 3 Secondary aggregate 4 Topcoat
Claims
1. The method comprises a surface preparation step of preparing a base, a base coating step of applying a base coating material containing a first aggregate to the surface of the base coating that has been prepared, a first rolling step of compressing the surface of the base coating material, a scattering step of scattering a second aggregate onto the surface of the base coating material that has been compressed before the base coating material hardens, a second rolling step of compressing the surface onto which the base coating material has been scattered, and a top coating step of applying a top coating material after the base coating material hardens, This floor coating method is characterized in that after the base preparation process, the base is divided into a number of adjacent work areas, and the undercoat process through the second rolling process are carried out on a first work area that serves as a starting point, and then the undercoat process through the second rolling process are repeated for adjacent work areas in sequence until all work areas have been completed, and then the topcoat process is carried out on all work areas after the undercoat material has hardened.
2. The method for applying the coating to a floor according to claim 1, characterized in that the undercoat material is an aqueous hard urethane-based concrete composition that contains the first aggregate, forms urethane bonds and urea bonds with polyol, isocyanate, and water, and forms concrete through a hydration reaction with cement and water.
3. The coating method according to claim 2, characterized in that the thickness of the undercoat material is approximately 4.0 mm to approximately 7.0 mm, the thickness of the topcoat material is approximately 0.1 mm to approximately 0.3 mm, the particle size of the first aggregate is approximately 2.0 mm to 3.0 mm, and the particle size of the second aggregate is approximately 0.5 mm to approximately 2.0 mm.
Citation Information
Patent Citations
Method for forming floor panel
JP1988315762A
Formation of light-transmitting nonslip resin coating
JP1989027668A
Wet substrate paving structure and construction method therefor
JP1996120607A
Coated floor surface forming method
JP1999131776A
Plastered floor construction method
JP2001207631A