Compositions Comprising Unsaturated Crystalline Polyesters for 3D Printing - Patent application

Unsaturated crystalline polyester resins address the limitations of SLS 3D printing by offering improved mechanical properties and finish quality, expanding the material range beyond crystalline polyamides, and reducing power requirements.

JP7556674B2Active Publication Date: 2024-09-26XEROX CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2019082683
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-05-17
Filing Date
2019-04-24
Publication Date
2024-09-26
Estimated Expiration
2039-04-24

AI Technical Summary

Technical Problem

The narrow range of applicable polymers in selective laser sintering (SLS) 3D printing limits the material properties of 3D parts, as only crystalline polyamides like PA-11 or PA-12 are successfully applied, while more flexible materials such as amorphous resins and high-performance materials are critical for broadening the scope.

Method used

Development of unsaturated crystalline polyester (CPE) resins derived from ethylenically unsaturated monomers and aliphatic diols, which can be crosslinked with thermal initiators to form thermosets, offering improved mechanical properties and a wider range of melting and crystallization temperatures suitable for SLS printing.

Benefits of technology

The unsaturated CPE resins provide improved mechanical properties and finish quality, eliminating the need for sanding or chemical treatments, and can be processed with lower power requirements, enhancing the versatility of SLS 3D printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556674000022
    Figure 0007556674000022
  • Figure 0007556674000014
    Figure 0007556674000014
  • Figure 0007556674000018
    Figure 0007556674000018
Patent Text Reader

Abstract

To provide polymeric materials for 3D printing which are more rigid or more flexible than the currently used polyamide and have lower Tc and Tm.SOLUTION: An unsaturated polyester resin includes an ethylenically unsaturated monomer, a first diol monomer, and a second diol monomer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to three-dimensional (3D) printing. In particular, the present disclosure relates to new materials for 3D printing based on unsaturated polyester resins.

[0002] Selective laser sintering (SLS) technology for additive manufacturing (3D printing) uses a rastering laser to "scan" over a bed of polymer powder and sinter it to form a solid shape in layers. Materials used for SLS are typically powdered polymers, either alone or in composite form. Selection of specifications and capabilities to meet the various needs of downstream applications drives the development of new materials for 3D printing via the SLS process.

[0003] Selective laser sintering (SLS) 3D printing technology produces plastic parts by using a laser as a power source to sinter successive layers of polymer powder. The problem that limits this technology from a wide industrial scope is the narrow variety of applicable polymers. To date, only a few commercial polymers, mainly consisting of crystalline polyamides (PA) such as PA-11 or PA-12, have been successfully applied to this technology, some limiting its use to other materials such as PA-6, thermoplastic polyurethanes (TPU), and polyetheramides (PEBA). Amorphous resins, elastomers, or other more flexible materials such as polypropylene (PP) and polyethylene (PE), as well as high-performance materials that are crucial to broaden the material properties of 3D parts, cannot be used. This is due to the limited requirement that the material must be crystalline and have a sharp melting and recrystallization point of approximately 30°C to 50°C temperature difference.

[0004] In SLS systems, a CO2 laser beam is used to selectively melt or sinter polymer particles deposited in thin layers. Localized complete coalescence of the polymer particles in the top powder layer as well as adhesion with previously sintered particles in the layer below is required. For crystalline or semi-crystalline polymers known for routine use in SLS processing, this implies that the crystallization temperature (Tc) should be suppressed as long as possible during processing, or at least for some sintered layers. The processing temperature must therefore be precisely controlled midway between melting (Tm) and crystallization (Tc) of a given polymer. This metastable thermodynamic region of the supercooled polymer melt is called the "sintering window" for a given polymer. The sintering window between the onset of Tc and Tm is approximately 30°C-40°C. Figure 1 shows the differential scanning calorimetry (DSC) spectrum of PA-12 SLS powder. (Source: Schmid et al., "Polymer Powders for Selective Laser Sintering (SLS)"; ETH-Zurich, 2014.)

[0005] There is a need for materials that are more rigid or flexible than the currently used polyamides (PA-6, PA-11, and PA-12). Additionally, there is a need for polymer materials that have lower temperatures (Tc and Tm) so that lower power requirements are needed for 3D printers.

[0006] The present disclosure provides an unsaturated polyester resin for use in three-dimensional (3D) printing, comprising: (1) an ethylenically unsaturated monomer having formula I,

[0007] [ka]

[0008] wherein each p and q is independently 0 to 8, and z is 1 to 5; (2) an ethylenically unsaturated monomer; and (3) a second diol monomer.

[0009] In some aspects, embodiments provide a composition comprising a crosslinked polyester resin prepared by contacting an unsaturated polyester with a thermal initiator, wherein the unsaturated polyester resin is a crosslinked polyester resin comprising at least one of: (1) an ethylenically unsaturated monomer derived from maleic acid, maleic anhydride, fumaric acid, chloromaleic acid, itaconic acid, 3-hexanedioic acid, 2-heptenedioic acid, 2-octenedioic acid, glutaconic acid, 2-decenedioic acid, traumatic acid, muconic acid, mesaconic acid, citraconic acid, and esters, and anhydrides, and mixtures thereof; , (2) a first diol monomer, and (3) a second diol monomer, and the thermal initiator is ammonium persulfate, sodium persulfate, potassium persulfate, an organic peroxide, 2,2'-azobis(2-methylpropanenitrile), 1,1'-azobis(cyanocyclohexane), 2-methyl 2-2'-azobispropanenitrile, 2-2'-azobisisobutylamide dehydrate, 2,2'-azobis(2-methyl-N-phenylpropionamidine) dihydrochloride, 2,2'-azobis[N-(4-chlorophenyl)-2-methylpropionamidine] ... 2,2'-azobis[N-(4-hydroxyphenyl)-2-methyl-propionamidine] dihydrochloride, 2,2'-azobis[N-(4-amino-phenyl)-2-methyl-propionamidine] tetrahydrochloride, 2,2'-azobis[2-methyl-N(phenylmethyl)propionamidine] dihydrochloride, 2,2'-azobis[2-methyl-N-2-propenylpropionamidine] dihydrochloride, 2,2'-azobis[N-(2-hydroxy-ethyl ... Azobis[2(5-methyl-2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(4,5,6,7-tetrahydro-1H-1,3-diazepin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(3,4,5,6-tetrahydropyrimidin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(5-hydroxy-3,4,5,6-tetrahydropyrimidin-2-yl)propane]dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride, and mixtures thereof. [Brief description of the drawings]

[0010] Various embodiments of the present disclosure are described herein below with reference to the drawings. [Figure 1] Differential Scanning Calorimetry (DSC) spectrum of PA-12 SLS powder reproduced from Schmid, M., Amado, A., Wegener, K., 30th International Conference of the Polymer Processing Society, Cleveland, OH, USA, June 8-12, 2014. [Diagram 2] FIG. 1 shows the Young's modulus (E) / temperature relationship for various types of polymers, reproduced from Wisanrakkit and Gilham, J. Appl. Poly. Sci, 42, 2453 (1991). [Diagram 3] 1 shows differential scanning calorimetry (DSC) data for crystalline polyester resin 1 according to certain embodiments of the present disclosure. [Figure 4A] 1 shows digital microscope images of emulsion aggregation particles prepared from crystalline polyester resins according to certain embodiments of the present disclosure. [Figure 4B] 1 shows digital microscope images of emulsion aggregation particles prepared from crystalline polyester resins according to certain embodiments of the present disclosure. [Figure 4C] 1 shows digital microscope images of emulsion aggregation particles prepared from crystalline polyester resins according to certain embodiments of the present disclosure. [Figure 4D] 1 shows digital microscope images of emulsion aggregation particles prepared from crystalline polyester resins according to certain embodiments of the present disclosure. [Figure 5A] 1 is a digital microscope image of a sintered unsaturated CPE powder according to certain embodiments of the present disclosure. [Figure 5B]1 is a digital microscope image of a sintered unsaturated CPE powder according to certain embodiments of the present disclosure. [Figure 5C] 1 is a digital microscope image of a sintered unsaturated CPE powder according to certain embodiments of the present disclosure. [Figure 5D] 1 is a digital microscope image of a sintered unsaturated CPE powder according to certain embodiments of the present disclosure. [Figure 5E] 1 is a digital microscope image of a sintered unsaturated CPE powder according to certain embodiments of the present disclosure. [Figure 5F] 1 is a digital microscope image of a sintered unsaturated CPE powder according to certain embodiments of the present disclosure. [Figure 5G] 1 is a digital microscope image of commercially available PA-12 powder. [Figure 5H] 1 is a digital microscope image of commercially available PA-12 powder.

[0011] Embodiments herein provide unsaturated polyester resins for use in selective laser sintering (SLS) 3-D printing technology.

[0012] The best materials for SLS printing are crystalline and have sharp melting points. The present disclosure provides unsaturated crystalline polyesters (CPEs) (used interchangeably as "unsaturated polyesters" or "unsaturated polyester resins") similar to commercially available PA-12 with very similar DSC profiles but shifted to lower temperatures. The lower viscosity of the CPEs allows for printed objects with improved finishes and eliminates sanding or chemical surface treatments. Unsaturated CPEs can be crosslinked with thermal initiators to form thermosets. Crosslinked unsaturated CPEs have greater strength and improved mechanical properties compared to their uncrosslinked counterparts. Figure 2 shows a schematic diagram of a typical Young's modulus (E) / temperature relationship for crosslinked and uncrosslinked polymers.

[0013] The unsaturated CPE of embodiments can be derived from a diacid (ethylenically unsaturated monomer) of Formula I, and at least two aliphatic diols of Formula II.

[0014] A general synthetic scheme for preparing the unsaturated polyesters of formula III is shown below.

[0015] [ka]

[0016] In embodiments, the unsaturated CPE of the embodiments may be derived from fumaric acid and at least two aliphatic diols of formula II.

[0017] In embodiments, the unsaturated CPE of the embodiments can be derived from fumaric acid and two aliphatic diols, such as 1,4-butanediol (1,4-BD) and 1,6-hexanediol (1,6-HD). A synthetic scheme for preparing an unsaturated polyester from fumaric acid, 1,4-BD and 1,6-HD is shown below.

[0018] [ka]

[0019] Examples of ethylenically unsaturated monomers include, but are not limited to, maleic acid, maleic anhydride, fumaric acid, chloromaleic acid, itaconic acid, 3-hexanedioic acid, 2-heptenedioic acid, 2-octenedioic acid, glutaconic acid, 2-decenedioic acid, traumatic acid, muconic acid mesaconic acid, citraconic acid, and esters and anhydrides thereof, and mixtures thereof.

[0020] The ethylenically unsaturated monomer is reacted with at least two different aliphatic diols (ie, a first diol monomer and a second diol monomer) to form an unsaturated polyester of Formula III.

[0021] The two aliphatic diols differ in the number of carbon atoms in the molecule, where the first diol monomer contains 2-5 carbon atoms (m1=2-5) and the second diol monomer contains 6-10 carbon atoms (m2=6-10). In an embodiment, the first diol monomer contains 2-4 carbon atoms, or 3-4 carbon atoms. In an embodiment, the second diol monomer contains 6-9 carbon atoms, or 6-8 carbon atoms. Examples of aliphatic diols include, but are not limited to, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 2,2-dimethylpropanediol, 2,2,3-trimethylhexanediol, 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, xylylene dimethanol, cyclohexanediol, diethylene glycol, bis(2-hydroxyethyl)oxide, dipropylene glycol, dibutylene glycol, 2,2-dimethylpropane-1,3-diol (neopentyl glycol), hexane-2,5-diol, hexane-1,6-diol, and combinations thereof.

[0022] In embodiments, the carbon chain of any aliphatic diol may be optionally substituted at any carbon atom. Such optional substitutions may include halogen, C1-C4 alkyl, C1-C4 alkoxy, and combinations thereof.

[0023] By varying the molar ratio of the first diol monomer (Formula II, where m1=2-5) and the second diol monomer (Formula II, where m2=6-10) and reacting these monomers with the ethylenically unsaturated monomer (Formula I), a series of unsaturated polyester resins (Formula III) with various melting and recrystallization temperatures can be made. The molar ratio of the first diol monomer to the second diol monomer can be 80:20 to about 60:50, 75:25 to 65:35, and preferably 70:30.

[0024] The higher the molar ratio of the first monomer to the second monomer, the lower the melting point of the resulting unsaturated polyester resin.

[0025] In an embodiment, the unsaturated polyester resin has a crystallization temperature (Tc) of about 50°C to about 70°C.

[0026] In embodiments, the unsaturated polyester resin has a melting temperature (Tm) of from about 75°C to about 110°C.

[0027] A low melting point unsaturated polyester resin can be obtained by increasing the first monomer content, but the recrystallization temperature of the unsaturated polyester resin is desirably greater than 58°C. If the recrystallization temperature is less than 58°C, the toner particles will stick together when exposed to high temperatures, causing blocking (or agglomeration). Blocking is a phenomenon in which the toner exposed to high temperatures softens and the toner particles aggregate.

[0028] The unsaturated polyester resin is desirably derived from at least 25 mole percent (in embodiments, at least 30 mole percent, at least 35 mole percent, at least 40 mole percent, at least 45 mole percent, or at least 50 mole percent) of ethylenically unsaturated monomers (diacids) to render the unsaturated polyester resin capable of being thermally cured (crosslinked) in the presence of a thermal initiator. In embodiments, the unsaturated polyester resin is derived from 30 mole percent to 95 mole percent, 40 mole percent to 90 mole percent, 50 mole percent to 85 mole percent, 60 mole percent to 80 mole percent, 65 mole percent to 80 mole percent, or 70 mole percent to 80 mole percent of ethylenically unsaturated monomers.

[0029] In embodiments, the unsaturated polyester resin is derived from 10 mole percent to 50 mole percent, 20 mole percent to 45 mole percent, or 30 mole percent to 45 mole percent of a first monomer.

[0030] In embodiments, the unsaturated polyester resin is derived from 5 mole percent to 50 mole percent, 10 mole percent to 50 mole percent, or 25 mole percent to 40 mole percent of a second monomer.

[0031] The viscosity of the unsaturated CPE resin at 120° C. can be 100 to 600 poise, or 200 to 500 poise. The acid value of the unsaturated CPE resin can be 3 to 20, or 5 to 20 KOH / g.

[0032] In an embodiment, a composition for use in 3D printing is provided that includes an unsaturated polyester resin that includes (or is derived from) an ethylenically unsaturated monomer (e.g., fumaric acid), a first monomer (e.g., 1,4-butanediol), a second monomer (e.g., 1,6-hexanediol), and mixtures thereof. In a further embodiment, the unsaturated polyester resin can be derived from 49 mole percent to 51 mole percent of the ethylenically unsaturated monomer (e.g., fumaric acid), 25 mole percent to 45 mole percent of the first monomer (e.g., 1,4-butanediol), and 10 mole percent to 30 mole percent of the second monomer (e.g., 1,6-hexanediol). In a further embodiment, the unsaturated polyester resin can be derived from 49 mole percent to 51 mole percent of an ethylenically unsaturated monomer (e.g., fumaric acid), 30 mole percent to 40 mole percent of a first monomer (e.g., 1,4-butanediol), and 10 mole percent to 30 mole percent of a second monomer (e.g., 1,6-hexanediol).

[0033] When unsaturated polyester resins are combined with thermal initiators during the SLS process, they can be cured to form rigid cross-linked unsaturated CPEs. The cured unsaturated polyester resins can be made by emulsion aggregation (EA) methods, resulting in particles with spherical to potato-like morphology.

[0034] Emulsion aggregation (EA) is a bottom-up approach to "grow" uniformly sized particles from submicron sized components. The EA process can produce the desired size and narrow particle size distribution required for optimal print quality. Through the EA process, nano-sized particles can be manipulated and engineered into micron-sized materials in a variety of composite designs. See U.S. Patent Nos. 5,585,215, 5,650,256, 5,501,935, and 5,418,108, which are incorporated herein by reference in their entireties. The result is core particles as aggregates with a volume average diameter of about 3 microns to about 100 microns, or embodiments with a volume average diameter of about 4 microns to about 90 microns, or embodiments with a volume average diameter of about 10 microns to about 80 microns.

[0035] The unsaturated CPE particles can have a circularity of about 0.910 to about 0.940, about 0.950 to about 0.970, or about 0.975 to about 0.990 as measured by a Sysmex FPIA 3000 Flow Particle Image Analyzer. The average particle size ranges from 5 to 120 microns, 6 to 80 microns, or 10 to 60 microns with a narrow size distribution (both volume and number) as measured by a Coulter Counter (Multisizer III). Ideally, the thermal initiator has a half-life below the emulsion aggregation coalescence temperature used during the EA process. The unsaturated polyester resin can be cured with a thermal initiator at a cure temperature of about 20°C to about 30°C, about 10°C to about 15°C above the melting point of the unsaturated polyester resin.

[0036] Examples of suitable thermal initiators include water-soluble initiators such as ammonium persulfate, sodium persulfate, potassium persulfate, organic soluble initiators including organic peroxides, and azo compounds including Vazo peroxides such as VAZO 64™, [2,2'-azobis(2-methylpropanenitrile) or 2,2'-azobis(isobutyronitrile), also known as AIBN], VAZO 88™, [1,1'-azobis(cyclohexanecarbonitrile) or 1,1'-azobis(cyanocyclohexane)], 2,2'-azodi(2-methylbutyronitrile (Vazo™ 67 from Sigma-Aldrich), and combinations thereof. Other suitable water-soluble initiators that may be used include azoamidine compounds such as 2-methyl 2-2'-azobispropanenitrile, 2-2'-azobisisobutylazo, and combinations thereof. amide dehydrate, 2,2'-azobis(2-methyl-N-phenylpropionamidine) dihydrochloride, 2,2'-azobis[N-(4-chlorophenyl)-2-methylpropionamidine] dihydrochloride, 2,2'-azobis[N-(4-hydroxyphenyl)-2-methylpropionamidine] dihydrochloride, 2,2'-azobis[N-(4-aminophenyl)-2-methylpropionamidine] tetrahydrochloride, 2,2'-azobis[2-methyl-N(phenylmethyl) propionamidine] dihydrochloride, 2,2'-azobis[2-methyl-N-2-propenylpropionamidine] dihydrochloride, 2,2'-azobis[N-(2-hydroxyethyl)-2-methylpropionamidine] dihydrochloride, 2,2'-azobis[2(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(4,5,6,7-tetrahydrofuran] 2,2'-azobis[2-(3,4,5,6-tetrahydropyrimidin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(5-hydroxy-3,4,5,6-tetrahydropyrimidin-2-yl)propane] dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride, and combinations thereof.

[0037] In an embodiment, the composition consists essentially of the unsaturated polyester resin. In an embodiment, the composition consists of 75-100%, 80-100%, or 90-95% by weight of the composition of the unsaturated polyester resin.

[0038] In embodiments, the composition consists essentially of the unsaturated CPE resin. In embodiments, the composition consists of 75-100%, 80-100%, or 90-95% by weight of the composition of the unsaturated CPE resin.

[0039] In embodiments, the unsaturated polyester resin has a yield stress in the range of about 10 megapascals to about 100 megapascals.

[0040] In embodiments, the unsaturated polyester resin has a yield strain in the range of about 1% to about 10%.

[0041] In embodiments, the unsaturated polyester resin has a Young's modulus in the range of about 0.5 to about 5 gigapascals.

[0042] In embodiments, the unsaturated polyester resin has a break strain in the range of about 10% to about 100%.

[0043] In embodiments, the unsaturated polyester resin has a stress at break in the range of about 10 megapascals to about 100 megapascals.

[0044] In embodiments, the cured unsaturated polyester resin has a yield stress in the range of about 10 megapascals to about 100 megapascals.

[0045] In embodiments, the cured unsaturated polyester resin has a yield strain in the range of about 1% to about 10%.

[0046] In embodiments, the cured unsaturated polyester resin has a Young's modulus in the range of about 0.5 to about 5 gigapascals.

[0047] In embodiments, the cured unsaturated polyester resin has a break strain in the range of about 10% to about 100%.

[0048] In embodiments, the cured unsaturated polyester resin has a break stress in the range of about 10 megapascals to about 100 megapascals.

[0049] In embodiments, the catalyst is tin-based. Such catalysts may be based on the oxidation states of tin (II) or tin (IV). In embodiments, the tin-based catalyst is mono- or dialkyltin-based. The monoalkyltins may further include oxide and / or hydroxide groups at the tin atom. In embodiments, the tin-based catalyst comprises a mixture of monobutyltin oxide, monobutyltin hydroxide oxide, and butylstannoic acid, commercially available as FASCAT® 4100. Other tin-based catalysts used in transesterification chemistry are well known in the art and may be similarly used to prepare polyester resins, such as the octabutyltetrathiocyanate stannoxane herein.

[0050] In an embodiment, the method includes curing an unsaturated polyester with a thermal initiator to form a mechanically robust material, where the mechanically robust material is a cross-linked unsaturated polyester. Typically, the curing occurs when the 3D object is being built by selective laser sintering (SLS).

[0051] In an embodiment, the method includes contacting an unsaturated polyester resin in the absence of a solvent. In an embodiment, the method includes preparing a solvent-free phase inversion emulsion (SFPIE) latex using the unsaturated polyester resin. The latex can be prepared by dispersing an unsaturated polyester with a surfactant and a base. The latex particle size can be in the range of about 50 to about 500 nanometers, or about 80 to about 300 nanometers.

[0052] The selection of specific surfactant or combination thereof, and the amount of each used, are within the understanding of those skilled in the art.Suitable surfactants include ionic or nonionic surfactants.Additionally, one or more surfactants can be used in the polymerization process.

[0053] Suitable anionic surfactants include sulfates and sulfonates, sodium lauryl sulfate, sodium dodecylbenzenesulfonate, sodium dodecylnaphthalene sulfate, dialkylbenzene alkyl sulfates and sulfonates, acids such as abietic acid available from Aldrich, and NEOGEN R™ and NEOGEN SC™ available from Daiichi Kogyo Seiyaku Co., Ltd, combinations thereof, etc. Other suitable anionic surfactants include DOWFAX™ 2A1 from Dow Chemical Company, alkyl diphenyl oxide disulfonates, and / or TAYCA POWER BN2060 from Tayca Corporation (Japan), which are branched sodium dodecylbenzenesulfonates.

[0054] Suitable cationic surfactants include ammoniums such as alkylbenzyldimethylammonium chloride, dialkylbenzene alkylammonium chloride, lauryl trimethylammonium chloride, alkylbenzylmethylammonium chloride, alkylbenzyldimethylammonium bromide, benzalkonium chloride, C12, C15, C17-trimethylammonium bromide, combinations thereof, etc. Other suitable cationic surfactants include cetylpyridinium bromide, halide salts of quaternized polyoxyethyl alkylamines, odecylbenzyltriethylammonium chloride, MIRAPOL and ALKAQUAT available from Alkaril Chemical Company, SANISOL (benzalkonium chloride) available from Kao Chemicals, combinations thereof, etc. Suitable cationic surfactants include SANISOL B-50 available from Kao Corp., which is primarily benzyldimethylalkonium chloride.

[0055] Suitable nonionic surfactants include alcohols, acids, and ethers, such as polyvinyl alcohol, polyacrylic acid, methalose, methylcellulose, ethylcellulose, propylcellulose, hydroxyethylcellulose, carboxymethylcellulose, polyoxyethylene cetyl ether, polyoxyethylene lauryl ether, polyoxyethylene octyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene oleyl ether, polyoxyethylene sorbitan monolaurate, polyoxyethylene stearyl ether, polyoxyethylene nonylphenyl ether, dialkylphenoxypoly(ethyleneoxy)ethanol, combinations thereof, and the like. Commercially available surfactants from Rhone-Poulenc such as IGEPAL CA-210™, IGEPAL CA-520™, IGEPAL CA-720™, IGEPAL CO-890™, IGEPAL CO-720™, IGEPAL CO-290™, IGEPAL CA-210™, ANTAROX 890™, and ANTAROX 897™ can be used.

[0056] Examples of bases include, but are not limited to, ammonium hydroxide, potassium hydroxide, sodium hydroxide, sodium carbonate, sodium bicarbonate, lithium hydroxide, potassium carbonate, triethylamine, triethanolamine, pyridine and its derivatives, diphenylamine and its derivatives, poly(ethyleneamine) and its derivatives, and combinations thereof.

[0057] The crosslinked unsaturated polyester (or cured unsaturated polyester) disclosed herein can be used as a support material that is generally removable and serves as a temporary support when making complex three-dimensional objects. Suitable support materials are well known in the art. For example, U.S. Patent No. 8,460,451 describes a support material for SLA (stereolithography) printers, which is incorporated herein by reference in its entirety. The invention disclosed herein can be used in SLA (stereolithography) printers, but it is specifically designed for use with SLS (selective laser sintering) printing, which eliminates the need for additional support materials.

[0058] The support material may be delivered through the same or a different printhead as the polyester resin material. The support material is often supplied as a liquid and typically contains a hydrophobic chemical that is solid at ambient temperature and liquid at elevated application temperatures. However, unlike the polyester resin material, the support material is subsequently removed to provide the completed three-dimensional part.

[0059] Removal of the support material can be accomplished by several processes including heating the support material above its melting point along with the use of a suitable organic carrier to sufficiently remove the support material from the polyester resin material.

[0060] In an embodiment, the method of printing a three-dimensional article includes utilizing a laser to sinter successive layers of an unsaturated crystalline polyester as disclosed herein as a build material to form a three-dimensional article. In an embodiment, the unsaturated crystalline polyester is in particulate form. In an embodiment, the particulates of the unsaturated crystalline polyester can be prepared by controlled aggregation of latex nanoparticles of the unsaturated crystalline polyester using an aggregating agent. This process is known as emulsion aggregation. In an embodiment, the method of printing a three-dimensional article further includes supporting at least one layer of the build material with a support material. Furthermore, in an embodiment of the method described herein, the build material and / or the support material are selectively deposited according to an image of the three-dimensional article, the image being in a computer-readable format.

[0061] The following examples are presented to illustrate embodiments of the present disclosure. These examples are intended for illustrative purposes only and are not intended to limit the scope of the present disclosure. Also, parts and percentages are by weight unless otherwise indicated. As used herein, "room temperature" refers to a temperature of about 20°C to about 25°C.

[0062] General resin synthesis Examples 1 and 2 describe the preparation and characterization of polyester resins according to embodiments disclosed herein.

[0063] Example 1 (Crystalline Unsaturated Polyester (CPE) - Resin 1) A 2-liter Buchi reactor equipped with a mechanical stirrer, distillation apparatus, and bottom discharge valve was charged with fumaric acid (5.00 moles), 1,4-butanediol (1.27 moles), and 1,6-hexanediol (3.83 moles). The mixture was heated to 165° C. under nitrogen for 1 hour. When the batch temperature reached 120° C., stirring was started. The reaction temperature was then increased at 0.5° C. per minute until the batch temperature reached 191° C. Viscosity measurements were taken at 120° C. (100 rpm) using a Brookfield viscometer and then sampled periodically until the viscosity reached 315 Pa. The reaction mixture was discharged into a metal container and allowed to cool to room temperature overnight.

[0064] Example 2 (Crystalline Unsaturated Polyester (CPE) - Resin 2) Crystalline unsaturated polyester (CPE) resin 2 was prepared by the procedure of Example 1 using the conditions discussed herein, except that the warm resin was left in the reactor overnight and the latex conversion was started in the same reactor the next day (see Example 5 for latex synthesis procedure).

[0065] FIG. 2 shows differential scanning calorimetry (DSC) data for Crystalline Polyester Resin 1 confirming the unsaturated polyester resin properties according to the present embodiments (DSC data was obtained on a Q2500 Differential Scanning Calorimeter (TA Instruments) from 0° C. to 150° C. to 0° C. at a rate of 10° C. / min.

[0066] Additional crystalline unsaturated polyester resins were prepared according to the above method, except that the amounts of 1,6-hexanediol (1,6-HD) and 1,4-butanediol (1,4-BD) were different. Table 2 shows the properties of the unsaturated polyester resins obtained from different molar ratios of 1,4-butanediol (1,4-BD) and 1,6-hexanediol (1,6-HD). The variation in viscosity and acid number in the resins shown in Table 2 is due to the experimental equipment and experimental error, as well as slight differences in conditions in each batch (e.g., equipment variation, heating time, reaction rate, measurement error, etc.).

[0067] [Table 2]

[0068] Examples 3-5 describe the preparation of unsaturated crystalline polyester (CPE) latexes from Resins 1 and 2 (Examples 1 and 2). Latexes 1-3 are latex emulsions consisting of polymer particles produced from the solvent-free emulsion polymerization of unsaturated crystalline polyesters.

[0069] Example 3 (Latex 1 prepared from Resin 1) To a 1 L glass reactor, 10.03 g of TAYCA POWER BN2060 surfactant (branched sodium dodecylbenzene sulfonate), 6.93 g of trimethylamine (TEA), and 200.00 g of crystalline unsaturated polyester resin 1 (prepared according to Example 1) were added. The reactor was heated to 105° C. at a controlled rate. Once the resin began to melt, mixing was started at a low speed (<50 RPM). With the reactor temperature at 100° C., DI water was fed to the reactor at a rate of 1.0 g / min. As the viscosity increased, the mixing speed was gradually increased to 165 RPM and then 200 RPM. Once the latex was formed, DI water was fed to the reactor at an increased rate of 2.0 g / min, which was gradually increased to 3.0 g / min and 250 RPM. A total of 300 g of DI water was added. It was then thoroughly cooled and the reactor temperature was reduced to 25° C. The product was collected in a storage tank and sieved through a 25 μm screen. The particle size was then measured by a Nanotrac® U2275E particle size analyzer. A narrow particle size of 72.5 nm±19.9 nm was achieved.

[0070] Example 4 (Latex 2 prepared from Resin 1) Example 4 was prepared according to the procedure of Example 3, except that 10.04 g of TAYCA POWER BN2060 surfactant (branched sodium dodecylbenzene sulfonate), 4.52 g of trimethylamine (TEA) and 200.00 g of crystalline unsaturated polyester resin 1 (prepared according to Example 1) were added to a 1 L glass reactor. A total of 320 g of DI water was added. The particle size was then measured by a Nanotrac® U2275E particle size analyzer. A narrow particle size of 171.1 nm ± 59.3 nm was achieved.

[0071] Example 5 (Latex 3 prepared from Resin 2) The resin was first synthesized by adding 479.55g of fumaric acid, 94.57g of 1,4-butanediol (BD) and 373.54g of 1,6-hexane-diol (HD) to a 2L butiglass reactor (prepared according to Example 2). The warm resin was left in the reactor overnight and the latex conversion was started the next day in the same reactor. To 800g of resin (expected yield), 40g of TAYCA POWER BN2060 surfactant (branched sodium dodecylbenzene sulfonate) and 18g of trimethylamine (TEA) were added. The reactor was heated to 115°C at a controlled rate. Once the resin started to melt at 74°C, mixing was started at a slow speed. At a reactor temperature of 100.8°C, DI water was fed to the reactor at a rate of 4.0g / min. The addition of DI water was stopped and restarted at a rate of 2.5 g / min, stopped again, then gradually increased in increments of 0.2 g / min from 2.0 g / min to 5.0 g / min to a final rate of 8 g / min. A total of 1200 g of DI water was added. It was then thoroughly cooled and the reactor temperature was reduced to 25° C. The product was then discharged and sieved through a 25 μm screen. The particle size was then measured by a Nanotrac® U2275E particle size analyzer. A narrow particle size of 120.1 nm±31.5 nm was achieved.

[0072] Table 3 summarizes the amounts of reagents used in the preparation of Latexes 1-3 and the particle size of the resulting latexes.

[0073] [Table 3]

[0074] Microparticle formation Example 6 (Preparation of Emulsion Aggregation (EA) Particles (CPE Microspheres 1) from Latex 1 (Example 3)) To a 2L glass reactor, 230.29g of CPE latex 1 from Example 3 and 456.07g of DI water were added. The pH was then adjusted to 6.42-3.04 with 53.67g of 0.3M nitric acid and 1.44g of ALS (aluminum sulfate) was added to the slurry while homogenizing at 3,000-4,000 RPM. The reactor was set at 131 RPM with one P4 shaft and heated to 66°C to agglomerate the CPE particles. Particle size was sampled periodically with a Coulter (small bore size). The slurry was gradually lowered to pH 1.6 with 0.3M nitric acid. When the particle size reached approximately 9.6 microns, freezing of the particles was initiated by pH adjusting the slurry with 27.08g of 4% NaOH until the pH reached 3.0. The reactor temperature was then increased to 84°C over 1 hour and the RPM was reduced to 90. Once the coalescence temperature of 84°C was reached, the slurry was allowed to coalesce for 4 hours. The slurry was then cooled to room temperature, washed 3 times with DI water, isolated by centrifugation and freeze dried. The final dried powder was subjected to moisture analysis, digital microscopy, SEM, DSC and TGA. The final particle size measured by SEM was 30-80 μm.

[0075] Example 7 (Preparation of Emulsion Aggregation (EA) Particles (CPE Microspheres 2) from Latex 2 (Example 4)) To a 2L glass reactor, 209.39g of CPE latex 2 from Example 4 and 477.00g of DI water were added. The pH was then adjusted to 5.87-3.02 with 35.72g of 0.3M nitric acid and 1.44g of ALS (aluminum sulfate) was added to the slurry while homogenizing at 3,000-4,000 RPM. The reactor was set at 125 RPM with one P4 shaft and heated to 70°C to agglomerate the CPE particles. Particle size was sampled periodically with a Coulter (large bore size). The slurry was gradually reduced to pH 1.62 with 0.3M nitric acid. The reactor temperature was then increased to 84°C over 1 hour and the RPM reduced to 80. The pH of the slurry was gradually reduced to pH 0.89 with 66.92g of 0.3M nitric acid. The slurry was allowed to coalesce at 84° C. for 5 hours. The slurry was then cooled to room temperature, washed three times with DI water, isolated by centrifugation, and freeze-dried. The final dry powder was subjected to moisture analysis and digital microscopy. The final particle size measured by digital microscopy was 47-75 μm.

[0076] Example 8 (Preparation of EA particles (CPE microspheres 3) from latex 3 (Example 5)) To a 2L glass reactor was added 184.99g of CPE latex 3 from Example 5 and 431.00g of DI water. The pH was then adjusted to 5.91-3.00 with 40.98g of 0.3M nitric acid and 1.44g of ALS (aluminum sulfate) was added to the slurry while homogenizing at 3,000-4,000 RPM. The reactor was set at 135 RPM with one P4 shaft and heated to 70°C to agglomerate the CPE particles. Particle size was sampled periodically with a Coulter (large bore size). The slurry was gradually reduced to pH 1.52 with 0.3M nitric acid. The RPM was increased to 150. With a reactor temperature of 75°C and a particle size of approximately 8 microns, a 10% EP33 (19.34g) shell was added and the pH was adjusted to 2.34 with 0.3M nitric acid. When the particle size reached approximately 8.8 microns, the reactor temperature was increased to 84° C. over one hour. At 84° C., 3.08 g of a chelating agent (Versene 100) was added to the reactor. The pH of the slurry was gradually lowered to pH 1.01 with 80.92 g of 1 M nitric acid. The slurry was allowed to coalesce at 84° C. for four hours. The slurry was then cooled to room temperature, washed three times with DI water, isolated by centrifugation, and freeze-dried. The final dried powder was subjected to moisture analysis and digital microscopy.

[0077] Example 9 (Preparation of EA particles (CPE microspheres 4) from latex 3 (Example 5)) To a 2L glass reactor, 206.14g of CPE latex 3 from Example 5 and 484.00g of DI water were added. The pH was then adjusted to 5.88-3.06 with 35.01g of 0.3M nitric acid and 1.44g of ALS (aluminum sulfate) was added to the slurry while homogenizing at 3,000-4,000 RPM. The reactor was set at 135 RPM with one P4 shaft and heated to 70°C to agglomerate the CPE particles. Particle size was sampled periodically with a Coulter (large bore size). The slurry was gradually reduced to pH 1.30 with 1M nitric acid. The RPM was increased to 140. With a reactor temperature of 75°C and a particle size of approximately 8.3 microns, 3.08g of chelating agent (Versene 100) was added. The reactor temperature was then increased to 84° C. over 1 hour and the RPM was reduced to 96. The pH of the slurry was gradually reduced to pH 1.12 with 46.43 g of 1 M nitric acid. The slurry was allowed to coalesce at 84° C. for 4 hours. The slurry was then cooled to room temperature, washed three times with DI water, isolated by centrifugation, and freeze-dried. The final dried powder was submitted for moisture analysis and digital microscopy. The final particle size measured by digital microscopy was 74-115 μm.

[0078] Table 4 summarizes the emulsion aggregation process for preparing CPE microspheres from the CPE latexes. Digital microscope images of Example 6 Latex 1, Example 7 Latex 2, Example 8 Latex 3, and Example 9 Latex 3 are shown in Figures 4A-D, respectively.

[0079] [Table 4] EXAMPLES

[0080] SLS printing Dry powder materials CPE Microsphere 1, CPE Microsphere 3, CPE Microsphere 4 (Examples 6, 8, and 9, respectively) were subjected to pre-sintering tests on a Sharebot SnowWhite SLS printer ("SnowWhite"), which determined the baseline performance of the dry powders. The SnowWhite is a specialized 3D printer that uses a CO2 laser to sinter thermoplastic powders layer by layer. The laser selectively melts the material by scanning a cross-section of the desired object, which was generated using a computer-aided design (CAD) model. After the first layer is scanned, the powder bed is lowered, new powder material is rolled on top of it, and the next layer is scanned until the part is complete. The main advantages of powder-based systems compared to other additive manufacturing techniques are the elimination of the printing support and the reusability of the material.

[0081] The procedure for printing with SnowWhite was as follows: A 30mm x 30mm x 0.1mm square was printed as a pre-screening object. 1. 0.5 wt% R812 silica with particles is blended into the CPE to improve flow at 12,000 RPM for 10 seconds. (Note this step was only done for Example 6). 2. The particles were sieved through a 150 micron screen. 3. The sieved particles were coated onto an aluminum plate using a bar coater (40 mil gap / approximately 1 mm thick powder layer). 4. The samples were placed in the SnowWhite chamber. The motor was disabled since no multilayer objects were printed. The temperature control of the build chamber was also disabled. The powder bed temperature was adjusted to be approximately 5°C below the Tm for each material. The laser speed and laser power were varied to determine the optimal printing conditions. 5. The chamber and powder bed were allowed to cool to room temperature before removing the part.

[0082] Table 5 shows the laser power and laser speed levels tested for each unsaturated CPE powder sample (Examples 6, 8, and 9) and the commercial PA-12 powder (AdSint PA12 obtained from ADVANC3D Materials® GmbH). The CO2 laser is a 14 watt laser with a temperature range of <190° C. This temperature is the temperature of the laser used in the Sharebot SnowWhite printer. The set temperature is not associated with each laser power setting. Partial shrinkage was measured by averaging the length and width of the printed squares and dividing this value by 30 mm to determine the percentage difference. For CPE Microsphere 3 and CPE Microsphere 4, the negative shrinkage values ​​are due to unsintered powder adhering to the part. In comparison, the commercial PA-12 powder showed the least partial shrinkage, indicating that the CPE particles just stuck together when exposed to the laser. Print quality was measured on an arbitrary scale of 1-5, with 5 being the best print quality and 1 being the worst print quality.

[0083] [Table 5]

[0084] Example 11 Digital microscope images of sintered unsaturated CPE powder and commercial PA-12 powder are shown in FIG. 5. Images labeled as a-h correspond to the examples shown in Table 5. CPE Microsphere 1 (Example 6) powder was low density, it was cohesive and difficult to flatten. The voids on the surface of the sintered parts were the result of insufficient powder coating (FIG. 5A). At higher laser powers, the particles melted instead of sintering (FIG. 5B). CPE Microsphere 3 (Example 8) had very poor flowability, with agglomerated particles sticking together and not coating well. This was expected based on the grainy surface observed in the optical micrographs (Table 3). CPE Microsphere 4 (Example 9) shows improved flowability compared to sintered unsaturated CPE powder Examples 6 and 8. The sintered bodies of CPE Microsphere 4 were fragile and broke into pieces (FIG. 5E) or had significant voids at higher laser powers due to non-uniform coating (FIG. 5F). In comparison, the commercially available PA-12 powder flowed well and sintered to form a uniform part with no voids (FIG. 5G). FIG. 5H shows a digital microscope image of the sintered PA-12, demonstrating uniform particle packing. These results are promising and demonstrate that unsaturated crystalline polyester EA particles can be sintered. Although the examples printed from the embodiments of the present invention did not exactly match the print quality of the commercial standard (PA-12), the examples show that the compositions of the present embodiments can be used to print and form objects of satisfactory quality.

[0085] Improvements in particle distribution and shape improve print quality.

Claims

1. 1. An unsaturated polyester resin for use in three-dimensional (3D) printing, comprising: an ethylenically unsaturated monomer which is fumaric acid; a first diol monomer represented by formula II and m is 2 to 5; a second diol monomer represented by formula II and m is 6 to 10, [Case 1] the acid component contained in the unsaturated polyester resin is only the fumaric acid, the ethylenically unsaturated monomer is present at 49 to 51 mole percent (mol %) of the unsaturated polyester resin; The unsaturated polyester resin has a molar ratio of the first diol monomer to the second diol monomer of 75:25 to 50:

50.

2. 2. The unsaturated polyester resin of claim 1, wherein the first diol monomer is present at 30 to 45 mole percent (mol %) of the unsaturated polyester resin.

3. 10. The unsaturated polyester resin of claim 1, wherein the second diol monomer is present at 25 to 40 mole percent (mol %) of the unsaturated polyester resin.

4. The unsaturated polyester resin according to claim 1, wherein the unsaturated polyester resin has a crystallization temperature (Tc) of 50°C to 70°C.

5. 2. The unsaturated polyester resin of claim 1, wherein the unsaturated polyester resin has a melting temperature (Tm) of 75°C to 110°C.

6. 2. The unsaturated polyester resin of claim 1, wherein the unsaturated polyester resin has a viscosity of 200 to 600 poise at 120°C.

7. The unsaturated polyester resin according to claim 1, wherein the acid value of the unsaturated polyester resin is 3 to 20 mg KOH / g.

8. 1. A composition comprising: a crosslinked polyester resin prepared by contacting an unsaturated polyester resin with a thermal initiator; The unsaturated polyester resin is an ethylenically unsaturated monomer which is fumaric acid; a first diol monomer represented by formula II and m is 2 to 5; a second diol monomer represented by formula II and m is 6 to 10; [chemical 2] the acid component contained in the unsaturated polyester resin is only the fumaric acid, The thermal initiator may be ammonium persulfate, sodium persulfate, potassium persulfate, organic peroxides, 2,2'-azobis(2-methylpropanenitrile), 1,1'-azobis(cyanocyclohexane), 2-methyl 2-2'-azobispropanenitrile, 2,2'-azobisisobutylamide dehydrate, 2,2'-azobis(2-methyl-N-phenylpropionamidine) dihydrochloride, 2,2'-azobis[N-(4-chlorophenyl)propionamidine]di ... 2,2'-azobis[N-(4-hydroxyphenyl)-2-methyl-propionamidine] dihydrochloride, 2,2'-azobis[N-(4-amino-phenyl)-2-methylpropionamidine] tetrahydrochloride, 2,2'-azobis[2-methyl-N(phenylmethyl)propionamidine] dihydrochloride, 2,2'-azobis[2-methyl-N-2-propenylpropionamidine] dihydrochloride, amidine] dihydrochloride, 2,2'-azobis[N-(2-hydroxy-ethyl)-2-methylpropionamidine] dihydrochloride, 2,2'-azobis[2(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(4,5,6,7-tetrahydro-1H-1,3-diazepin-2-yl)propane] dihydrochloride, hydrochloride, 2,2'-azobis[2-(3,4,5,6-tetrahydropyrimidin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(5-hydroxy-3,4,5,6-tetrahydropyrimidin-2-yl)propane]dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}dihydrochloride, and mixtures thereof. the ethylenically unsaturated monomer is present at 49 to 51 mole percent (mol %) of the unsaturated polyester resin; A composition, wherein a molar ratio of said first diol monomer to said second diol monomer is from 75:25 to 50:

50.

9. The thermal initiator may be ammonium persulfate, sodium persulfate, potassium persulfate, organic peroxides, 2,2'-azobis(2-methylpropanenitrile), 1,1'-azobis(cyanocyclohexane), 2-methyl 2-2'-azobispropanenitrile, 2,2'-azobisisobutylamide dehydrate, 2,2'-azobis(2-methyl-N-phenylpropionamidine) dihydrochloride, 2,2'-azobis[N-(4-chlorophenyl)-2-methylpropionamidine] dihydrochloride, 2,2'-azobis[N-(4- 2,2'-azobis[N-(4-aminophenyl)-2-methylpropionamidine] tetrahydrochloride, 2,2'-azobis[2-methyl-N(phenylmethyl)propionamidine] dihydrochloride, 2,2'-azobis[2-methyl-N-2-propenylpropionamidine] dihydrochloride, 2,2'-azobis[N-(2-hydroxyethyl)-2-methylpropionamidine] dihydrochloride, 2,2'-azobis[2(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(2-imidazo 10. The composition of claim 8, wherein the azobis(2-(4,5,6,7-tetrahydro-1H-1,3-diazepin-2-yl)propane) dihydrochloride is selected from the group consisting of 2,2'-azobis[2-(3,4,5,6-tetrahydropyrimidin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(5-hydroxy-3,4,5,6-tetrahydropyrimidin-2-yl)propane] dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride, and mixtures thereof.

10. The composition of claim 8, wherein the first diol monomer is present at 30 to 45 mole percent (mol %) of the crosslinked polyester resin.

11. The composition of claim 8, wherein the second diol monomer is present at 25 to 40 mole percent (mol %) of the crosslinked polyester resin.

12. 1. A method of making a resin emulsion, comprising: copolymerizing a mixture comprising an ethylenically unsaturated dicarboxylic acid, which is fumaric acid, a first diol represented by formula II and m is 2-5, and a second diol represented by formula II and m is 6-10, thereby forming an unsaturated polyester resin, conducted at a temperature in the range of 150° C. to 205° C.; dispersing the unsaturated polyester resin in a solution containing a surfactant to form the resin emulsion; [C3] The method according to claim 1, wherein the only acid component contained in the unsaturated polyester resin is fumaric acid.

13. The method of claim 12 , wherein the method further comprises contacting the resin emulsion with a thermal initiator.

14. 14. The method of claim 13, wherein contacting the unsaturated polyester resin with the thermal initiator is conducted in the absence of a solvent.

15. The thermal initiator may be ammonium persulfate, sodium persulfate, potassium persulfate, organic peroxides, 2,2'-azobis(2-methylpropanenitrile), 1,1'-azobis(cyanocyclohexane), 2-methyl 2-2'-azobispropanenitrile, 2,2'-azobisisobutylamide dehydrate, 2,2'-azobis(2-methyl-N-phenylpropionamidine) dihydrochloride, 2,2'-azobis[N-(4-chlorophenyl)propionamidine] dihydrochloride, 2,2'-azobis[N-(4-hydroxyphenyl)-2-methyl-propionamidine] dihydrochloride, 2,2'-azobis[N-(4-aminophenyl)-2-methylpropionamidine] tetrahydrochloride, 2,2'-azobis[2-methyl-N(phenylmethyl)propionamidine] dihydrochloride, 2,2'-azobis[2-methyl-N-2-propenylpropionamidine] 2,2'-azobis[N-(2-hydroxyethyl)-2-methylpropionamidine] dihydrochloride, 2,2'-azobis[2(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(4,5,6,7-tetrahydro-1H-1,3-diazepin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(4,5,6,7-tetrahydro-1H-1,3-diazepin-2-yl)propane] dihydrochloride, 14. The method of claim 13, wherein the compound is selected from the group consisting of 2,2'-azobis[2-(3,4,5,6-tetrahydropyrimidin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(5-hydroxy-3,4,5,6-tetrahydropyrimidin-2-yl)propane]dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}dihydrochloride, and mixtures thereof.

Citation Information

Patent Citations

  • JP1972039187Y1

  • Unsaturated polyester esin compositions

    JP1977052989A

  • Production of air-drying unsaturated polyester of good pigment dispersibility

    JP1986097325A

  • Crystalline polyester

    JP2004226569A

  • Active energy ray-curable composition, storage body, inkjet recording device, recorded matter, and stereoscopic cured product

    JP2016117807A