Method for producing titanosilicate zeolite without using raw materials containing alkoxy groups
A cost-effective method for producing titanosilicate zeolite with high Ti content by forming Ti-O-Si bonds in acidic and basic solutions, addressing the limitations of using alkoxy groups in zeolite synthesis.
Patent Information
- Application Number
- JP2019236375
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-12-26
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2039-12-26
AI Technical Summary
The production of titanosilicate zeolite using raw materials containing alkoxy groups is hindered by their flammability and high cost, making them unsuitable for large-scale synthesis.
A method involving the preparation of acidic and basic solutions without alkoxy groups, followed by neutralization to form Ti-O-Si bonds, and subsequent hydrothermal treatment with seed crystals and templates to produce titanosilicate zeolite.
This method enables the production of titanosilicate zeolite with a high Ti content without using expensive and flammable alkoxy groups, reducing production costs and enhancing Ti incorporation into the zeolite framework.
Smart Images

Figure 0007556686000002 
Figure 0007556686000005 
Figure 0007556686000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a titanosilicate zeolite without using a raw material containing an alkoxy group. [Background technology]
[0002] Zeolite is a general term for crystalline aluminosilicates, and is used in a wide range of fields, including catalysts, detergent builders, adsorbents, and soil conditioners. Zeolites contain Si and Al atoms in their frameworks and are known to have various crystal structures. These crystal structures are classified by a structural code using three letters of the alphabet. For example, the crystal structure of Y-type zeolite, which has long been used as an active species in fluid catalytic cracking catalysts, is classified as a FAU (faujasite) structure. In recent years, metallosilicate-type zeolites that contain metal atoms other than aluminum (Ga, Ti, V, Fe, Zn, Sb, etc.) in their frameworks instead of aluminum have also been known. These crystal structures are also classified by the same structural code as crystalline aluminosilicates. In metallosilicate-type zeolites, the metal ions in the framework are surrounded by SiO and are highly isolated. For this reason, metallosilicate-type zeolites are known to exhibit unusual catalytic functions.
[0003] In the synthesis of titanosilicate zeolite, which is one of the metallosilicate zeolites, alkali metal ions hinder the introduction of Ti atoms into the framework. In addition, alkali metal ions also promote the production of anatase-type titanium oxide (Non-Patent Document 1). Therefore, compounds containing alkoxy groups, such as tetraethoxysilane and tetrabutoxytitanium, which have an extremely low content of alkali metal ions, are widely used as raw materials for synthesizing titanosilicate zeolites that contain a large number of Ti atoms in the framework (Patent Document 1). However, compounds containing alkoxy groups are flammable and expensive compared to general inorganic compounds (e.g., water glass, etc.). For these reasons, compounds containing alkoxy groups have not necessarily been optimal as raw materials for mass production of titanosilicate zeolites. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2011-506241 [Non-patent literature]
[0005] [Non-Patent Document 1] Yoshio Ono and Takeaki Yashima (eds.), "Science and Engineering of Zeolite," Kodansha, 2000 Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a method for producing a titanosilicate zeolite containing a large amount of Ti without using raw materials containing alkoxy groups, which are expensive and flammable. [Means for solving the problem]
[0007] The method for producing titanosilicate zeolite using a raw material not containing an alkoxy group includes the steps of: preparing an acidic solution containing Ti; preparing a basic solution containing Si; mixing the acidic solution and the basic solution to neutralize them; preparing a precursor containing a product obtained in the neutralization step, a seed crystal, a template, and water; and hydrothermally treating the precursor to prepare titanosilicate zeolite. Effect of the Invention
[0008] According to the present invention, a titanosilicate zeolite containing a large amount of Ti can be produced without using raw materials containing alkoxy groups which are expensive and flammable. [Brief description of the drawings]
[0009] [Figure 1]1 shows XRD spectra of titanosilicate zeolites obtained in Example 1 and Comparative Examples 1 and 2. [Diagram 2] 1 shows UV spectra of titanosilicate zeolites obtained in Example 1, Example 3, and Reference Example 1. [Diagram 3] 1 is an electron microscope photograph of the titanosilicate zeolite obtained in Example 1. [Figure 4] 1 is an electron microscope photograph of the titanosilicate zeolite obtained in Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the method for producing titanosilicate zeolite of the present invention (hereinafter also referred to as "the production method of the present invention") will be described.
[0011] [Outline of the manufacturing method of the present invention] The manufacturing method of the present invention is a method for manufacturing titanosilicate zeolite without using raw materials containing alkoxy groups. Therefore, in the manufacturing method of the present invention, raw materials containing alkoxy groups such as tetraethyl orthosilicate and tetrabutoxy titanium are not used. The manufacturing method of the present invention is as follows. First, an acidic solution containing Ti and a basic solution containing Si are prepared from raw materials not containing alkoxy groups. Next, the acidic solution and the basic solution are mixed. At this time, a neutralization reaction occurs and a gel-like product is generated. This product is considered to be something like a hydrogel in which a hydroxide of titanium (e.g., titanium oxyhydroxide) and silicic acid (e.g., orthosilicic acid) are dehydrated and condensed. And, in this product, Ti-O-Si bonds formed by dehydration and condensation are considered to exist. Such a product is mixed with a template necessary for making the target zeolite and seed crystals for promoting the crystallization of the zeolite to prepare a precursor. By subjecting this precursor to hydrothermal treatment, a titanosilicate zeolite containing a large amount of Ti can be prepared.
[0012] More specifically, the production method of the present invention is a method for producing titanosilicate zeolite using a raw material that does not contain an alkoxy group, and includes the steps of preparing an acidic solution containing Ti, preparing a basic solution containing Si, mixing the acidic solution and the basic solution to neutralize them, preparing a precursor containing the product obtained in the neutralization step, a seed crystal, a template, and water, and hydrothermally treating the precursor to prepare titanosilicate zeolite.
[0013] Each step of the production method of the present invention will be described in detail below.
[0014] In the synthesis of general zeolites, alkali metal ions such as sodium and potassium are used as structure-directing agents. However, in the synthesis of titanosilicate zeolites, it is known that if there are many alkali metal ions, Ti is difficult to insert into the framework of titanosilicate zeolites. Inorganic compounds such as water glass (sodium silicate) are known as general raw materials for the synthesis of zeolites. However, even if the alkali metal is removed from inorganic compounds such as water glass (sodium silicate) by washing or the like, a small amount of alkali metal remains. For this reason, it has been difficult to adopt them as raw materials for the synthesis of titanosilicate zeolites. Therefore, raw materials containing alkoxy groups with an extremely small content of alkali metal ions have been used so far for the production of titanosilicate zeolites. In contrast, in the production method of the present invention, it is possible to produce titanosilicate zeolites containing a large amount of Ti by using inorganic compounds such as water glass (sodium silicate) without using raw materials containing such alkoxy groups. The production method of the present invention includes a step of mixing and neutralizing an acidic solution containing Ti with a basic solution containing Si, which generates Ti-O-Si bonds in the product. It is believed that the use of such a product makes it easier for Ti to be incorporated into titanosilicate zeolite.
[0015] [Preparing an acidic solution containing Ti] The manufacturing method of the present invention includes a step of preparing an acidic solution containing Ti.
[0016] In this step, a soluble titanium salt can be dissolved in water to prepare an acidic solution containing Ti. As the soluble titanium salt, a trivalent titanium compound or a tetravalent titanium compound can be used. At this time, a titanium compound containing an alkoxy group is not used as a raw material. As the soluble titanium salt, for example, titanium sulfate, titanyl sulfate, titanium nitrate, titanyl nitrate, titanyl halide (titanyl chloride), titanium halide (titanium trichloride, titanium tetrachloride), etc. can be used. In the production method of the present invention, as the soluble titanium salt, a tetravalent titanium compound is preferable, and titanyl sulfate is more preferable. In addition, if these are difficult to dissolve in an aqueous solution, they can be dissolved in an aqueous solution to which an acid such as sulfuric acid or hydrochloric acid is added. Examples of the acid used here include sulfuric acid and hydrochloric acid, as well as inorganic acids such as hydrofluoric acid, hydrobromic acid, and hydroiodic acid. It is preferable that no floating matter or particles of a size that can be visually confirmed remain in this acidic solution. When such an acidic solution is used, the amount of Ti contained in the finally obtained titanosilicate zeolite tends to increase. In addition, an acidic solution (for example, a sol) containing particles of a size that cannot be visually confirmed can be preferably used. More specifically, an acidic solution that does not contain particles of 10 μm or more in particle size distribution (volume basis) measured by a laser diffraction method can be preferably used. The solvent in this acidic solution is not limited to water, and may contain one or more organic solvents that are miscible with water.
[0017] The pH of this acidic solution is preferably in the range of more than 0 and not more than 4, and more preferably in the range of more than 0 and not more than 2. The closer the pH of this acidic solution is to 0, the better Ti dissolves. The temperature of the sample for measuring the pH is 25°C ± 1°C.
[0018] The concentration of Ti contained in this acidic solution is preferably in the range of 0.1% by mass to 5% by mass, more preferably 0.5% by mass to 3% by mass, calculated as TiO2. If the Ti concentration of this acidic solution is too high, the Ti-O-Si bonds contained in the product obtained by mixing with the basic solution containing Si will be reduced. This may result in an increase in Ti-O-Ti bonds in the product. If the Ti-O-Ti bonds increase, they will be more likely to precipitate as TiO2, and the Ti contained in the final titanosilicate zeolite will be reduced.
[0019] [Preparing a basic solution containing Si] The manufacturing method of the present invention includes a step of preparing a basic solution containing Si.
[0020] In this step, for example, silica can be dissolved in a basic solution to prepare a basic solution containing Si. At this time, a silicon compound containing an alkoxy group is not used as a raw material. In the manufacturing method of the present invention, a basic compound containing Si can also be prepared by using a method of dissolving an alkali metal silicate (sodium silicate, potassium silicate, etc.) in water, or a method of dispersing fumed silica in a basic solution. In this step, it is preferable to use a method of dissolving sodium silicate in water. It is preferable that this basic solution does not contain any suspended matter or particles of a size that can be confirmed by the naked eye. When such a basic solution is used, the titanosilicate zeolite finally obtained tends to contain a large amount of Ti. In addition, a silicon compound (e.g., silica sol) containing solid matter of a size that cannot be visually confirmed can be used. More specifically, a silicon compound that does not contain particles of 10 μm or more in the particle size distribution (volume basis) measured by a laser diffraction method can be used. base Any neutral solution can be preferably used. The solvent in the basic solution is not limited to water, and may contain one or more organic solvents that are miscible with water.
[0021] The pH of this basic solution is preferably in the range of 10 to 14. The higher the pH, the easier it is for Si to dissolve. In order for SiO2 to be stably dispersed in the basic solution, the pH of the basic solution is preferably at least 10. To adjust the pH of this basic solution, a basic compound such as sodium hydroxide, potassium hydroxide, sodium carbonate, or ammonia can be used. In the production method of the present invention, even compounds containing sodium or potassium can be used to adjust the pH. As the basic compound used to adjust the pH of this basic solution, ammonia is more preferably used.
[0022] The concentration of Si contained in this basic solution is preferably in the range of 5% by mass to 15% by mass, more preferably in the range of 7% by mass to 10% by mass, calculated as SiO2. If the concentration of Si in this basic solution is too high, SiO2 particles are likely to be generated or grown in this solution, and the number of Si-O-Si bonds may increase. If the number of Si-O-Si bonds in this solution increases, the amount of Si required to create Ti-O-Si bonds in the product obtained in the neutralization step described below decreases. As a result, the amount of Ti contained in the finally obtained titanosilicate zeolite tends to decrease. If the concentration of Si is too low, productivity will decrease drastically. Therefore, it is preferable that the concentration of Si is in the above range.
[0023] [Neutralization process] In this step, the acidic solution and the basic solution are mixed and neutralized. At this time, a gel-like product is generated by the neutralization reaction. In this step, the pH of the mixed solution after mixing both solutions is preferably in the range of more than 5 and less than 9, more preferably in the range of more than 6 and less than 8. The pH and mixing ratio of the acidic solution and the basic solution may be appropriately adjusted so that the pH of this mixed solution falls within the above range. In addition, after adjusting the mixed solution as necessary, further pH adjustment may be performed. For this pH adjustment, a conventionally known acidic solution or basic solution can be used. For example, a solution containing an inorganic acid such as sulfuric acid listed in the step of preparing an acidic solution containing Ti can be used as the acidic solution. In addition, a solution containing a basic compound such as ammonia listed in the step of preparing a basic solution containing Si can be used as the basic solution.
[0024] The molar ratio of Si to Ti contained in the product obtained in this step is preferably in the range of 25 to 50, more preferably in the range of 30 to 40, in terms of Si / Ti ratio. If this molar ratio is too small (i.e., the Ti content is too high), the amount of Ti outside the framework of the finally obtained titanosilicate zeolite tends to increase, which is undesirable. The Ti concentration of the acidic solution and the Si concentration of the basic solution, as well as the mixing ratio, may be appropriately adjusted so that the molar ratio of Si to Ti contained in this hydrogel falls within such a range. In this way, a titanosilicate zeolite containing a lot of Ti in the framework and a little Ti outside the framework can be obtained.
[0025] In this step, it is preferable to add the basic solution to the acidic solution little by little and mix them. When this method is used, titanium hydroxide is precipitated little by little in the acidic solution. Then, the precipitated titanium hydroxide and the surface OH of silicic acid or SiO2 particles undergo dehydration condensation to obtain a product containing many Ti-O-Si bonds. If these are mixed at once, at least one of the Ti concentration and the Si concentration is locally biased in the mixed solution, and many Ti-O-Ti bonds are generated in the area where the Ti concentration is high. Then, the Ti-O-Si bonds in the product are reduced, so that the Ti contained in the finally obtained titanosilicate zeolite may be reduced. The rate at which the basic solution is added to the acidic solution is preferably a rate at which the entire amount of the basic solution is added over at least 0.5 hours. However, if this addition takes too long, the productivity drops significantly, so in reality, it is preferable to add the entire amount of the basic solution within 2 hours.
[0026] In this step, the temperatures of the acidic solution, the basic solution and the mixed solution obtained by mixing them are each preferably in the range of more than 0° C. and less than 50° C. In particular, if the temperature of the mixed solution is too high, gelation proceeds excessively and the fluidity decreases drastically, which is undesirable from the viewpoint of handleability.
[0027] In this step, the product may be separated from the mixture, if necessary, by a conventional method such as filtration, centrifugation, drying, etc.
[0028] If the product obtained in this step contains a large amount of alkali metal, it may be removed by washing to 10,000 ppm or less. In the production method of the present invention, by forming Ti-O-Si bonds in advance in the product, it becomes possible to synthesize a titanosilicate containing a large amount of Ti even in a state in which alkali metal is contained. However, if the alkali metal content of the product is too high, the amount of Ti contained outside the framework of the titanosilicate may increase. Therefore, by reducing the amount of alkali metal contained in the product by washing, the amount of Ti outside the framework in the titanosilicate zeolite can be reduced. The Ti contained outside the skeleton can be confirmed by UV-VIS measurement described later. The method for washing the product is preferably a method using an aqueous solution containing ammonium ions. As the ammonium ion source, a water-soluble ammonium salt can be used. Examples of the ammonium salt include water-soluble inorganic salts such as ammonium chloride, ammonium sulfate, ammonium nitrate, ammonium bicarbonate (ammonium hydrogen carbonate) and ammonium carbonate. As the ammonium ion source, ammonium bicarbonate and ammonium carbonate are preferred because of their ease of availability, ease of handling, influence on subsequent processes, ease of decomposition in the firing process, and little influence on titanosilicate. A more preferred ammonium ion source is ammonium bicarbonate. However, even if this method is used, it is practically difficult to reduce the alkali metal content to the same level (less than 10 ppm) as when a raw material containing an alkoxy group is used. The alkali metal contained in the product obtained in this step is preferably in the range of 10 ppm to 10,000 ppm, more preferably in the range of 100 ppm to 1,000 ppm. Here, the alkali metal content (concentration) is the ratio obtained by converting the alkali metal (M) into the mass of alkali metal oxide (M2O) and dividing it by the mass of the sample (alkali metal content (concentration) = [M2O mass] / [sample mass]). If the alkali metal content of the product is within the above range, a titanosilicate zeolite containing a lot of Ti and little extraskeletal Ti can be produced.
[0029] The viscosity of the product obtained in this step (measured at 25°C as a mixture of ion-exchanged water and the product to a solids concentration of 5%) is preferably in the range of more than 50 mPa·s and less than 5000 mPa·s, and more preferably in the range of more than 100 mPa·s and less than 1000 mPa·s. The viscosity of the product is one of the indicators that can grasp the bonding state in the product. When at least one of the Ti-O-Si bonds and Si-O-Si bonds increases in the product, the viscosity of the hydrogel also increases. In the manufacturing method of the present invention, a titanosilicate zeolite containing a large amount of Ti can be synthesized by using a hydrogel having a viscosity in the above range. The viscosity of the product can be adjusted by the retention time or retention temperature of the mixed solution obtained by mixing the acidic solution and the basic solution. Specifically, it can be adjusted by a method of retaining the mixture at a temperature of 20°C or more and 50°C or less until the viscosity of the product falls within the above range.
[0030] [Preparing the precursor] The production method of the present invention includes a step of preparing a precursor containing the product obtained in the above step, a seed crystal, a template, and water.
[0031] The seed crystals used in this step have the function of promoting the crystallization of titanosilicate zeolite. Therefore, a zeolite having the same structure as the titanosilicate zeolite finally obtained is used as the seed crystal. For example, when synthesizing TS-1 as the titanosilicate zeolite, TS-1 is used as the seed crystal. The amount of seed crystals added is preferably in the range of 10% by mass to 30% by mass, more preferably in the range of 20% by mass to 30% by mass, based on the total mass of the seed crystals and the product contained in the precursor (seed crystals + product, hereinafter also referred to as the "total mass of the precursor"). Here, the mass of the seed crystals refers to the sum of the masses of Si and Ti contained in the seed crystals, converted into SiO2 and TiO2, respectively. Similarly, the total mass of the precursor refers to the sum of the masses of Si and Ti contained in the precursor, converted into SiO2 and TiO2, respectively. In the production method of the present invention, if the amount of seed crystals added is too small, the amount of titanosilicate zeolite produced may decrease. Also, if the amount of seed crystals added is too large, the productivity of titanosilicate decreases. Such titanosilicate zeolite as seed crystals may be purchased as a commercially available product, or a part of the titanosilicate zeolite obtained by the production method of the present invention may be reused as the seed crystals.
[0032] The template used in this step is a template necessary for synthesizing titanosilicate zeolite. Titanosilicate zeolites having various structures can be synthesized depending on the type of template. For example, TS-1 having an MFI structure can be synthesized using tetrapropylammonium hydroxide (TPAOH). In addition, not limited to TS-1, any conventionally known template can be used to synthesize titanosilicate zeolite. The amount of template added is preferably such that the molar ratio of the template to the Si contained in the precursor (template / Si ratio) is in the range of 0.04 to 0.3, more preferably in the range of 0.08 to 0.2. Such templates for zeolite synthesis are generally expensive. However, in the production method of the present invention, titanosilicate zeolites can be synthesized even if the amount of template added is small.
[0033] The amount of water added in this step is preferably such that the molar ratio of water to Si contained in the precursor (H2O / Si ratio) is in the range of 10 to 100, more preferably 20 to 50. The number of moles of H2O referred to here refers to the number of moles when the Si and Ti contained in the precursor are converted to SiO2 and TiO2, respectively, and the difference between the sum of the mass of both and the mass of the template and the total mass of the precursor is regarded as the mass of water. If the amount of water added is too large, the yield of titanosilicate zeolite obtained in the hydrothermal treatment step described below will decrease, whereas if the amount of water added is too small, impurities will be generated, resulting in a decrease in the yield of titanosilicate zeolite.
[0034] The pH of the precursor obtained in this step is preferably in the range of 10 to 14, more preferably in the range of 11 to 13. When the pH of the precursor is in this range, the yield of titanosilicate zeolite increases.
[0035] It is preferable to wet-pulverize the precursor obtained in this step. By wet-pulverizing the precursor, the product and the seed crystals are mixed uniformly. Furthermore, by finely pulverizing the seed crystals, a titanosilicate zeolite with a small particle size can be obtained by hydrothermal treatment. Titanosilicate zeolite with a small particle size has a large surface area and can be suitably used for catalytic reactions. Furthermore, by performing such treatment, titanosilicate can be synthesized even if the amount of seed crystals added or the amount of template added is small. The reason for this is not clear, but it is thought that it is because the seed crystals and the product are wet-pulverized together, and the product aggregates around the fine seed crystals. It is thought that when such aggregates are formed, titanosilicate zeolite is likely to grow with the seed crystals as nuclei. As a method for performing the wet-pulverization treatment, a conventionally known method can be used. For example, a method can be used in which the precursor is set in a ball mill or a bead mill and pulverized using beads with a size of 1 mmφ or less. The treatment time for wet grinding is preferably within the range of 0.5 to 3 hours, inclusive. If the treatment time is within this range, a titanosilicate zeolite with high crystallinity can be obtained.
[0036] [Step of hydrothermally treating the precursor] The production method of the present invention includes a step of hydrothermally treating the precursor to obtain a titanosilicate zeolite.
[0037] In this step, the precursor is hydrothermally treated in an autoclave. The temperature of the hydrothermal treatment is preferably in the range of 130°C to 220°C, more preferably in the range of 150°C to 200°C. The rate of temperature increase to the above-mentioned temperature range is preferably in the range of 10°C / hour to 50°C / hour, more preferably in the range of 20°C / hour to 40°C / hour. Furthermore, the holding time after the temperature increase to the above-mentioned temperature range is preferably in the range of 10 hours to 48 hours, more preferably in the range of 12 hours to 24 hours. When the hydrothermal treatment conditions are in the above-mentioned range, a titanosilicate zeolite with a high Ti content and high crystallinity can be obtained.
[0038] After the hydrothermal treatment, a slurry containing titanosilicate zeolite is produced in the autoclave. If a titanosilicate zeolite solid is to be obtained, it can be obtained by drying this slurry. As the drying method, a conventionally known method can be used. In addition, the titanosilicate zeolite may be separated by a method such as filtration.
[0039] The titanosilicate zeolite obtained as a solid can be washed to remove impurities, if necessary. For example, the titanosilicate zeolite can be washed by suspending it in warm water and removing the solvent. Note that this washing cannot remove the template contained in the structure of the titanosilicate zeolite. Therefore, when removing the template, it is preferable to calcinate the titanosilicate zeolite in an oxygen-containing atmosphere. When calcining the titanosilicate zeolite, the calcination temperature is preferably in the range of 400°C or more and 600°C or less. In addition, the retention (calcination) time is preferably in the range of 1 hour or more and 24 hours or less. By calcining the titanosilicate zeolite under such conditions, the template can be removed without destroying its crystal structure. EXAMPLES
[0040] Hereinafter, the manufacturing method of the present invention will be described in more detail by way of examples, but the present invention is not limited to these scopes of implementation.
[0041] [Measurement method] In this example, various samples were analyzed based on the following analysis methods.
[0042] [Content of alkali metal] The concentration of alkali metal (M) was calculated by the calibration curve method using atomic absorption spectrometry (apparatus name: Z-2310 manufactured by Hitachi, Ltd.) after preparing an aqueous solution in which the sample powder pulverized in a mortar was completely dissolved. The obtained concentration of alkali metal was converted as M2O.
[0043] [Viscosity] The sample solution was set in a viscometer (TBV10 type viscometer manufactured by Toki Sangyo Co., Ltd.), measured for 30 seconds at a rotor rotation speed of 60 rpm, and the viscosity value after 30 seconds was taken as the measured value.
[0044] [X-ray diffraction measurement] The sample powder pulverized in a mortar was set in an X-ray diffractometer (MiniFlex600 manufactured by Rigaku Corporation, radiation source: CuKα), scanned from 2θ = 5 to 50°, and subjected to X-ray diffraction measurement. From the X-ray diffraction pattern of the obtained sample powder, those in which peaks could be confirmed on the diffraction planes attributed to the MFI structure were judged to have the MFI structure. Specifically, the presence or absence of diffraction peaks attributed to the (101), (111), (102), (131), (022), (051), (313), (323), and (062) planes was confirmed. The positions of the peaks attributed to these diffraction planes can be confirmed from the technical literature (M. M. J. Treacy, J. B. Higgins, COLLECTION OF SIMULATED XRD POWDER PATTERNS FOR ZEOLITES, Fifth Revised Edition, Elsevier). Note that the positions of the peaks may vary slightly depending on measurement conditions and the like. Therefore, those having peaks derived from the MFI structure were regarded as being within the range of ±0.5° from the peak positions described in the above literature.
[0045] <Composition Analysis of Products in Neutralization Process> Aqueous solution in which the sample powder pulverized in a mortar was completely dissolved with an acid was prepared. The concentration of Ti contained in this aqueous solution was calculated by the calibration curve method using inductively coupled plasma optical emission spectrometry (ICPS-8100 manufactured by Shimadzu Corporation). The obtained concentration of Ti was converted to TiO2. Here, the ignition residue amount when 1 g of the sample powder was heated at 1000 °C for 1 hour was measured, and the components other than the ignition residue amount were regarded as H2O. Then, assuming that the components contained in the sample powder were TiO2, SiO2, alkali metal oxide (M2O), and H2O, the concentration of Si was calculated as SiO2.
[0046] <Zeolite Composition Analysis> An aqueous solution in which the sample powder pulverized in a mortar was completely dissolved was prepared. The concentration of Ti contained in this aqueous solution was calculated by the calibration curve method using inductively coupled plasma optical emission spectrometry (ICPS-8100 manufactured by Shimadzu Corporation). The obtained concentration of Ti was converted to TiO2. Here, the ignition residue amount when 1 g of the sample powder was heated at 1000 °C for 1 hour was measured, and the components other than the ignition residue amount were regarded as H2O. Then, assuming that the components contained in the sample powder were TiO2, SiO2, alkali metal oxide (M2O), and H2O, the concentration of Si was calculated as SiO2.
[0047] <UV-VIS Measurement> The sample powder pulverized in a mortar was placed on a slide glass and pressed with a cover glass. This was set in a manufactured ultraviolet-visible-near-infrared spectrophotometer (JASCO Corporation, V-670), and the UV spectrum in the range of 200 to 500 cm -1 with a resolution of 1 cm -1 was measured.
[0048] <Particle Size Distribution> The particle size distribution of the sample was measured using a laser diffraction particle size distribution measuring device (manufactured by HORIBA, LA950V2, refractive index: 1.46). The median diameter was calculated from the obtained particle size distribution (volume basis).
[0049] <Observation with Electron Microscope> The sample powder was observed using a scanning electron microscope (manufactured by JEOL Ltd.: JSM-6010LA, acceleration voltage: 15 kV). When observing, the magnification was appropriately adjusted to a magnification at which the size of the primary particles could be confirmed.
[0050] [Example 1] <Step of preparing an acidic solution containing Ti> 12.5 g of titanyl sulfate with a concentration of 33.2 mass% (in terms of TiO2) was added to 180 g of sulfuric acid with a concentration of 25 mass%, and the titanyl sulfate was completely dissolved. 540 g of pure water was added thereto to prepare an acidic solution containing Ti. At this time, the pH of the acidic solution containing Ti was 0.2, and the concentration of Ti (in terms of TiO2) was 0.6 mass%. <Step of preparing a basic solution containing Si> 800 g of pure water was added to 420 g of sodium silicate with a concentration of 24.2 mass% (in terms of SiO2) to prepare a basic solution containing Si. At this time, the pH of the basic solution containing Si was 11.1, and the concentration of Si (in terms of SiO2) was 8.3 mass%. <Neutralization step> After heating the acidic solution containing Ti to 40°C, the basic solution containing Si was added at the same rate over 90 minutes to obtain a mixed solution. After the addition was completed, the mixed solution was stirred at 40°C for 40 minutes. Next, aqueous ammonia with a concentration of 15 mass% was added to this mixed solution to adjust the pH to 7.4, and then it was stirred for another 40 minutes. During the stirring, when the slurry thickened, pure water was appropriately added to the extent that it could be stirred. The obtained mixed solution was filtered to separate the product. This separated product was washed using a solution containing ammonium bicarbonate, and 1040.6 g (Si concentration 8.80 mass% (in terms of SiO2) and Ti concentration 0.35 mass% (in terms of TiO2)) was obtained. The Si / Ti ratio of this product was 33 (molar ratio), and the alkali metal content was 200 ppm.
[0051] <Step of preparing a precursor> 235 g of the product obtained in the above step was added to a container containing 105 g of pure water and stirred for 1 hour. Next, 40 g of a 40 mass% aqueous solution of tetrapropylammonium hydroxide (TPAOH) was added as a template and stirred for 1 hour. Furthermore, 20 g of an aqueous suspension of TS-1 zeolite obtained by the method of Reference Example 1 described later was added as seed crystals and stirred for 1 hour to obtain a precursor. The Si concentration in the aqueous suspension was 33.8 mass% (SiO2 equivalent), and the Ti concentration was 1.4 mass% (TiO2 equivalent). This precursor had Si / Ti=33 (molar ratio), TPAOH / Si=0.172 (molar ratio), H2O / Si=43 (molar ratio), and pH 12.7, and the content of seed crystals was 25 mass% of the total mass of the precursor. <Step of Hydrothermally Treating Precursor> The entire amount of the obtained precursor was placed in a 500 ml autoclave, heated to 160°C at a rate of 32°C / hour, and hydrothermally treated at 160°C for 18 hours. After the treatment, it was cooled to room temperature. The solid content contained in the solution in the autoclave was separated by filtration. The solid content was washed with pure water and dried to obtain 25.7 g of white powder. <Analysis> When the white powder was subjected to X-ray diffraction measurement, the diffraction pattern derived from the MFI structure was confirmed. In addition, the white powder was subjected to composition analysis and UV-Vis measurement. The results are shown in Table 1. In Table 1, "Ti content" represents the percentage (mass %) obtained by converting the Si and Ti in the zeolite into the masses of SiO2 and TiO2, respectively, and dividing the mass converted into TiO2 by the sum of the two.
[0052] [Example 2: Wet grinding process] The steps up to the neutralization step were carried out under the same conditions as in Example 1. <Precursor preparation process: Addition of wet grinding process> 235 g of the product obtained in the above step and 20 g of an aqueous suspension of TS-1 zeolite obtained as seed crystals by the method of Reference Example 1 described later were added to a container containing 105 g of pure water to prepare a slurry. The Si concentration in the aqueous suspension was 33.8 mass% (SiO2 equivalent), and the Ti concentration was 1.4 mass% (TiO2 equivalent). The slurry was subjected to a wet grinding process using a bead mill filled with zirconia beads of 1 mmφ. During this process, the median diameter of the slurry was confirmed every 30 minutes using a particle size distribution measuring device (laser diffraction type). The process was terminated when there was no change in the median diameter of the slurry. At this time, the time required for the process was 2 hours. The slurry after the process was collected, and 40 g of a TPAOH aqueous solution with a concentration of 40 mass% was added and stirred for 1 hour to obtain a precursor. This precursor had a molar ratio of Si / Ti=33, a molar ratio of TPAOH / Si=0.172, and a molar ratio of H2O / Si=43, and the content of seed crystals was 25 mass% of the total mass of the precursor (same as in Example 1). The subsequent steps and analyses were carried out in the same manner as in Example 1.
[0053] [Example 3: High alkali metal concentration] The same method as in Example 1 was used, except that the step of washing the product obtained in the neutralization step with a solution containing ammonium bicarbonate was not performed. The alkali metal content of the product obtained in the neutralization step in Example 3 was 10.57 mass %. The viscosity of the precursor was 632 mPa s.
[0054] [Comparative Example 1: No neutralization step, no seed crystals] 12 g of basic titania sol (pH: 8.87, Ti content: 8.9 mass% (TiO2 equivalent), Si content: 1.2 mass% (SiO2 equivalent)) was added to a container containing 280 g of pure water and stirred for 15 minutes. 69 g of basic silica sol (pH 9.22, Si content: 40 mass% (SiO2 equivalent)) was added to this and stirred for 1 hour. 40 g of tetrapropylammonium hydroxide (TPAOH) aqueous solution (concentration 40 mass%) was added as a template and stirred for 1 hour to obtain a precursor. This precursor had a Si / Ti=35 (molar ratio), TPAOH / Si=0.170 (molar ratio), and H2O / Si=43 (molar ratio). Subsequent steps and analysis were performed in the same manner as in Example 1.
[0055] [Comparative Example 2: No neutralization process] 9 g of basic titania sol (pH: 8.87, Ti content: 8.9 mass% (TiO2 equivalent), Si content: 1.2 mass% (SiO2 equivalent)) was added to a container containing 270 g of pure water and stirred for 15 minutes. 51.6 g of basic silica sol (pH 9.22, Si content: 40 mass% (SiO2 equivalent)) was added to this and stirred for 1 hour. 40 g of tetrapropylammonium hydroxide (TPAOH) aqueous solution (concentration 40 mass%) was added as a template and stirred for 1 hour. Furthermore, 30 g of an aqueous suspension of TS-1 zeolite (Si / Ti (molar ratio) = 33) produced by the same method as the method of Reference Example 1 described later was added as seed crystals to obtain a precursor. This aqueous suspension had a Si concentration of 22.8 mass% (SiO2 equivalent) and a Ti concentration of 0.9 mass% (TiO2 equivalent). The precursor had a molar ratio of Si / Ti=34, a molar ratio of TPAOH / Si=0.171, and a molar ratio of H2O / Si=43. The subsequent steps and analyses were carried out in the same manner as in Example 1.
[0056] [Reference Example 1: Using raw materials containing alkoxy groups] 70 g of TPAOH solution (concentration 40% by mass) was added as a template to a container containing 148 g of pure water and stirred for 15 minutes. 8 g of tetrabutoxytitanium (TBOT) (Ti concentration 23.5% by mass (TiO2 equivalent)) was added to the mixture and stirred for 1 hour. Then, 174 g of tetraethoxysilane (TEOS) (Si concentration 27.4 mass% (SiO2 equivalent)) was added at once and stirred for 1 hour. This was heated to 80°C, and the process of evaporating a certain amount of ethanol and adding pure water was repeated to perform solvent replacement. It was confirmed that the conductivity of the slurry after solvent replacement was 6.4 mS / cm, and this was placed in a 500 ml autoclave and hydrothermally treated at 160°C for 18 hours. The slurry had Si / Ti = 34 and TPAOH / Si = 0.174. After treatment, it was cooled, and the product was filtered and washed with pure water to obtain a white powder. When X-ray diffraction measurement was performed on this white powder, a diffraction pattern derived from the MFI structure was confirmed. In addition, composition analysis and UV-Vis measurement were performed on this white powder. The results are shown in Table 1.
[0057] [Table 1]
[0058] It was confirmed from the X-ray diffraction patterns that the white powders obtained by the methods of Examples 1 to 3 and Comparative Examples 1 and 2 all have an MFI structure. Among them, the X-ray diffraction patterns obtained by the methods of Example 1, Comparative Example 1, and Comparative Example 2 are shown in FIG. 1. Considering this together with the results of the composition analysis, the white powders obtained by the methods of Examples 1 to 3 including the neutralization step have an MFI structure. In addition, since the white powders obtained by the methods of Examples 1 to 3 have a high Ti content, they are considered to be titanosilicate zeolite. Furthermore, this Ti content is close to the Ti content of the titanosilicate synthesized from the conventional raw material containing an alkoxy group shown in Reference Example 1. On the other hand, the white powder obtained by the method of Comparative Example 1, which does not include a neutralization step, has an MFI structure but contains almost no Ti. For this reason, the white powder obtained by the method of Comparative Example 1 is considered to be silicalite. In addition, the white powder obtained by the method of Comparative Example 2, which does not include a neutralization step, has an MFI structure and contains a small amount of Ti, so at first glance it looks like a titanosilicate zeolite. However, since this Ti is almost the same as the Ti content derived from the TS-1 zeolite used as the seed crystal, it is considered that the method of Comparative Example 2 cannot synthesize titanosilicate zeolite.
[0059] The UV spectra of Example 1, Example 3, and Reference Example 1 are shown in FIG. -1 The shoulder appearing near the center is derived from extra-skeletal Ti. The titanosilicate zeolite obtained by the method of Example 3 has a higher shoulder than that of Example 1 or Reference Example 1, confirming that it contains extra-skeletal Ti. On the other hand, the titanosilicate zeolite obtained by the method of Example 1 has a lower shoulder, confirming that it contains almost no extra-skeletal Ti. This is at approximately the same level as the titanosilicate zeolite synthesized using a raw material containing an alkoxy group as shown in the method of Reference Example 1. The titanosilicate zeolite obtained by the method of Example 1 has a low alkali metal content (200 ppm) in the product obtained in the neutralization step. In contrast, the titanosilicate zeolite obtained by the method of Example 3 has a high alkali metal content (10.57 mass%) in the product obtained in the neutralization step. Therefore, the shoulder originating from extraframework Ti is believed to depend on the alkali metal content of the product obtained in the neutralization step.
[0060] An electron microscope photograph of Example 1 is shown in Figure 3. An electron microscope photograph of Example 2 is shown in Figure 4. From these electron microscope photographs, it was confirmed that the titanosilicate zeolite of Example 2, in which the precursor was subjected to wet-pulverization treatment, had produced smaller primary particles than the titanosilicate zeolite of Example 1, in which the precursor was not subjected to wet-pulverization treatment.
Claims
1. A method for producing a titanosilicate zeolite having an MFI structure using a raw material that does not contain an alkoxy group, comprising the steps of: preparing an acidic solution containing Ti; Providing a basic solution containing Si; mixing the acidic solution with the basic solution to neutralize; The method includes the steps of: preparing a precursor containing the product obtained in the neutralization step, a seed crystal, a template, and water; and hydrothermally treating the precursor to prepare a titanosilicate zeolite. A method for producing titanosilicate zeolite.
2. 2. A method for producing the titanosilicate zeolite according to claim 1, comprising the step of wet-grinding the precursor.
3. 3. The method for producing titanosilicate zeolite according to claim 2, wherein the precursor is wet-ground using beads having a size of 1 mmφ or less for a treatment time of 0.5 hours or more and 3 hours or less.
4. The method for producing a titanosilicate zeolite according to any one of claims 1 to 3, wherein the precursor is hydrothermally treated by maintaining it at a temperature in the range of 130°C or higher and 220°C or lower for a period of 10 hours or higher and 48 hours or lower.
5. 5. The method for producing titanosilicate zeolite according to claim 4, wherein the rate at which the temperature is raised to the temperature range is in the range of 10° C. / hour or more and 50° C. / hour or less.
Citation Information
Patent Citations
Synthesis method of titanium silicalite TS-1
CN102320619A
Large porous crystalline titanium molecular sieve zeolite
JP1990184516A
Method for synthesizing halide-free titanium-containing zeolites
JP1998500654A
Method of manufacturing titanium / silicon molecular sieve of large particle diameter and method of manufacturing cyclohexanone oxime using the same
JP2011121860A
Preparation process for TS-1 zeolite
JP2011506241A