LAMINATE, OPTICAL LAMINATE, METHOD FOR PRODUCING OPTICAL LAMINATE, AND OPTICAL DEVICE

An adhesive layer with controlled creep deformation and crosslinked structures addresses the issue of adhesive penetration into optical sheet recesses, maintaining functionality and enabling efficient roll-to-roll manufacturing of optical laminates.

JP7556935B2Active Publication Date: 2024-09-26NITTO DENKO CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022501090
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-21
Filing Date
2021-02-19
Publication Date
2024-09-26
Estimated Expiration
2041-02-19

AI Technical Summary

Technical Problem

The penetration of adhesive layers into the uneven structures of optical sheets affects the functionality of optical laminates over time, and existing manufacturing methods for optical laminates using roll-to-roll processes face challenges in maintaining consistent adhesive penetration.

Method used

The development of an adhesive layer with specific creep deformation rates and properties, such as a creep deformation rate of 10% or less after 1 second and 16% or less after 30 minutes, along with a thickness of 0.1 μm to 20 μm, using polymers like copolymers of nitrogen-containing (meth)acrylic monomers and crosslinked structures, and incorporating active energy ray-curable resins to form a stable adhesive layer.

Benefits of technology

The adhesive layer effectively suppresses penetration into recesses of optical sheets, maintaining optical laminate functionality over time and enabling efficient roll-to-roll manufacturing, ensuring high diffuse transmittance and stable adhesive strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556935000008
    Figure 0007556935000008
  • Figure 0007556935000003
    Figure 0007556935000003
  • Figure 0007556935000002
    Figure 0007556935000002
Patent Text Reader

Abstract

An adhesive layer (20) configured so that: in a creep test in which a rotary rheometer is used, the creep deformation rate when a reaction force of 10,000 Pa is applied for one second at 50°C is 10% or less, and the creep deformation rate when a reaction force of 10,000 Pa is applied for 30 minutes at 50°C is 16% or less; and the 180° peel adhesive force with respect to a PMMA film is 10 mN / 20 mm or greater.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive layer, a laminate having an adhesive layer, a laminate having an adhesive composition layer for forming an adhesive layer, an optical laminate having an adhesive layer and an optical sheet, a method for producing an optical laminate, and an optical device including such an optical laminate. [Background technology]

[0002] Optical sheets (e.g., microlens sheets, prism sheets, brightness enhancement films (e.g., Brightness Enhancement Film: BEF (registered trademark) manufactured by 3M)) are used in various optical devices (e.g., display devices and lighting devices). In this specification, the term "optical sheet" is not limited to the above-mentioned examples, but broadly includes sheet-like optical members, and further includes, for example, a diffusion plate and a light guide plate. The optical sheet is attached to another optical sheet or an optical device, for example, by using an adhesive layer. In this specification, the term "optical laminate" refers to a configuration including an optical sheet and an adhesive layer or a configuration including a plurality of optical sheets. In this specification, the term "adhesive" is used to include a pressure-sensitive adhesive (also called a "pressure-sensitive adhesive").

[0003] The present applicant has disclosed in Patent Document 1 an optical laminate (referred to as an "optical laminate sheet" in Patent Document 1) that can be used in display devices and lighting devices. The optical laminate of Patent Document 1 has an optical sheet (e.g., a microlens sheet) having a concave-convex structure on its surface, and an adhesive layer provided on the surface having the concave-convex structure. 5% to 90% of the height of the convex portions of the concave-convex structure is filled with the adhesive layer. The adhesive layer is formed from an adhesive composition containing a graft polymer obtained by graft polymerizing a chain containing a cyclic ether group-containing monomer onto a (meth)acrylic polymer, and a photocationic polymerization initiator or a thermosetting catalyst. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-007046 A (Patent No. 5658490 A) [Patent Document 2] International Publication No. 2019 / 087118 Summary of the Invention [Problem to be solved by the invention]

[0005] When an optical sheet having a concave-convex structure on its surface is attached using an adhesive layer, the degree to which the adhesive layer penetrates into (fills) the concaves of the concave-convex structure affects the function of the optical sheet. Therefore, it is preferable that the degree to which the adhesive layer penetrates into the concaves of the concave-convex structure does not change over time.

[0006] In addition, from the viewpoint of mass productivity, it is preferable that an optical laminate in which an optical sheet and an adhesive layer are laminated or an optical laminate in which a plurality of optical sheets are laminated, which is used in an optical device, can be manufactured by a roll-to-roll method.

[0007] The present invention has been made to solve at least one of the above problems, and aims to provide an adhesive layer in which the degree of penetration into the recesses of the uneven structure of an optical sheet is suppressed from changing over time, a laminate having such an adhesive layer, a laminate having an adhesive composition layer capable of forming such an adhesive layer, an optical laminate having such an adhesive layer and an optical sheet, or an optical laminate that can be manufactured by a roll-to-roll method, and a method for manufacturing such an optical laminate. Another aim of the present invention is to provide an optical device including such an optical laminate. [Means for solving the problem]

[0008] According to an embodiment of the present invention, there are provided solutions as described in the following items. [Item 1] In a creep test using a rotational rheometer, the creep deformation rate is 10% or less when a stress of 10,000 Pa is applied for 1 second at 50°C, and the creep deformation rate is 16% or less when a stress of 10,000 Pa is applied for 30 minutes at 50°C. An adhesive layer having a 180° peel adhesion to PMMA film of 10mN / 20mm or more. [Item 2] 2. The adhesive layer according to item 1, having a haze of 0.01% or more and 5% or less. [Item 3] 3. The adhesive layer according to item 1 or 2, having a thickness of 0.1 μm or more and 20 μm or less. The thickness is preferably 15 μm or less, or 10 μm or less. [Item 4] The adhesive layer according to any one of items 1 to 3, comprising at least one of the following polymers (1) to (3): (1) A copolymer of a nitrogen-containing (meth)acrylic monomer and at least one other monomer; (2) A copolymer of a carboxyl group-containing acrylic monomer and at least one other monomer (excluding nitrogen-containing (meth)acrylic monomers); (3) Polyester polymers. [Item 5] 5. The adhesive layer according to any one of items 1 to 4, comprising a polyester-based polymer. [Item 6] Contains a (meth)acrylic polymer, 6. The adhesive layer according to any one of items 1 to 5, wherein the (meth)acrylic polymer is a copolymer of a nitrogen-containing (meth)acrylic monomer and at least one other monomer. [Item 7] 7. The adhesive layer according to item 6, wherein the nitrogen-containing (meth)acrylic monomer has a nitrogen-containing cyclic structure. [Item 8] 8. The adhesive layer according to item 6 or 7, wherein the (meth)acrylic polymer is crosslinked. [Item 9] 9. The adhesive layer according to any one of items 6 to 8, which does not comprise a grafted polymer. [Item 10] 10. The adhesive layer according to any one of items 6 to 9, further comprising a cured product of an active energy ray-curable resin. [Item 11] Item 11. The adhesive layer according to item 10, which is formed by curing the active energy ray curable resin of an adhesive composition layer containing the (meth)acrylic polymer, the active energy ray curable resin, and a polymerization initiator. [Item 12] An adhesive layer according to any one of items 1 to 10, A substrate having a release-treated main surface; having A laminate, in which the release-treated main surface of the substrate is bonded to the adhesive layer. The laminate described in Item 12 may be referred to as an "adhesive sheet." The laminate according to Item 12 may further include, for example, another substrate having a release-treated main surface disposed on the opposite side of the adhesive layer from the substrate. In this case, the release-treated main surface of the other substrate is bonded to the adhesive. The release-treated surface (release-treated surface) refers to a surface treated with a release agent. The release-treated main surface of the substrate (support) is formed by applying (applying) a release agent to one main surface of the substrate, and further drying, etc., as necessary. The release agent is not particularly limited, but examples thereof include silicone-based release agents, fluorine-based release agents, long-chain alkyl-based release agents, and fatty acid amide-based release agents. [Item 13] Item 12. The adhesive composition layer forming the adhesive layer according to item 11; A substrate having a release-treated main surface; having A laminate, in which the release-treated main surface of the substrate is attached to the adhesive composition layer. The laminate described in Item 13 may be referred to as an "adhesive sheet." The laminate according to item 13 may further include, for example, another substrate having a release-treated main surface disposed on the opposite side of the adhesive composition layer from the substrate. In this case, the release-treated main surface of the other substrate is bonded to the adhesive composition layer. [Item 14] a first optical sheet having a first main surface having a concave-convex structure and a second main surface opposite to the first main surface; the adhesive layer according to any one of items 1 to 11, which is disposed on the first main surface side of the first optical sheet; The optical laminate has the following structure. [Item 15] Item 15. The optical laminate according to item 14, wherein the uneven structure includes a plurality of recesses, and the surface of the adhesive layer and the first main surface of the first optical sheet define a plurality of spaces in the plurality of recesses. [Item 16] Item 16. The optical laminate according to item 15, wherein the uneven structure includes a flat portion in contact with the adhesive layer. [Item 17] 17. A method for producing the optical laminate according to any one of items 14 to 16, comprising bonding the first optical sheet and the adhesive layer. [Item 18] Item 18. The method according to item 17, wherein the steps are carried out in a roll-to-roll process. [Item 19] Item 17. The optical laminate of any one of items 14 to 16, further comprising a second optical sheet arranged on the side of the adhesive layer opposite the first optical sheet. [Item 20] Item 19 is a method for producing an optical laminate according to item 19, A step A1 of bonding a first laminate in which the first optical sheet and the adhesive layer are laminated to the second optical sheet; or a step A2 of bonding the first optical sheet to a second laminate in which the adhesive layer and the second optical sheet are laminated; A manufacturing method comprising either one of the steps of: [Item 21] The step A1 includes a step of bonding the first laminate and the second optical sheet by a roll-to-roll method, or 21. The manufacturing method according to item 20, comprising the step A2, wherein the step A2 comprises a step of bonding the second laminate and the first optical sheet by a roll-to-roll method. [Item 22] 20. An optical device comprising an optical laminate according to any one of items 14 to 16 and 19. [Item 23] A method for producing an optical laminate according to any one of items 14 to 16, which directly or indirectly cites item 11, A step A of applying the adhesive composition layer onto the first main surface of the first optical sheet; a step B of curing the active energy ray curable resin of the adhesive composition layer in a state in which the adhesive composition layer is applied onto the first main surface of the first optical sheet; A manufacturing method comprising: [Item 24] Item 24. The manufacturing method according to item 23, wherein the step A includes a step of bonding the first optical sheet and the adhesive composition layer by a roll-to-roll method. [Item 25] A method for producing an optical laminate according to item 19, which indirectly cites item 11, A step A1 of bonding a first laminate in which the first optical sheet and the adhesive composition layer are laminated to the second optical sheet; or A step A2 of bonding the first optical sheet to a second laminate in which the adhesive composition layer and the second optical sheet are laminated. Either one of the following: a step B of curing the active energy ray curable resin contained in the adhesive composition layer after the step A1 or the step A2; A manufacturing method comprising: [Item 26] The step A1 includes a step of bonding the first laminate and the second optical sheet by a roll-to-roll method, or Item 26. The manufacturing method according to item 25, comprising the step A2, wherein the step A2 comprises a step of bonding the second laminate and the first optical sheet by a roll-to-roll method. Effect of the Invention

[0009] According to an embodiment of the present invention, there are provided an adhesive layer in which the degree of penetration (filling) into the recesses of the concave-convex structure of an optical sheet is suppressed from changing over time, a laminate having such an adhesive layer, a laminate having an adhesive composition layer capable of forming such an adhesive layer, an optical laminate having such an adhesive layer and an optical sheet, or an optical laminate that can be manufactured by a roll-to-roll method, and a method for manufacturing such an optical laminate. According to another embodiment of the present invention, there is provided an optical device including such an optical laminate. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic cross-sectional view of an optical laminate 100A according to an embodiment of the present invention. [Diagram 2] FIG. 11 is a schematic cross-sectional view of an optical laminate 101A according to another embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing a creep curve of an adhesive. [Figure 4] 10A and 10B are schematic cross-sectional views of an optical laminate 100B and an optical laminate 101B according to still another embodiment of the present invention. [Diagram 5] 1 is a schematic perspective view of a first optical sheet 10b included in an optical laminate 100B. [Figure 6] 1 is a schematic cross-sectional view of a lighting device 200 including an optical laminate 100B. [Figure 7A] 2 is a schematic plan view of a shaping film 70 of an optical laminate according to an embodiment of the present invention. FIG. [Figure 7B] 2 is a schematic cross-sectional view of a shaping film 70. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] First, an adhesive layer according to an embodiment of the present invention, a laminate having an adhesive layer, a laminate having an adhesive composition layer for forming an adhesive layer, and an optical laminate having an adhesive layer and an optical sheet, as well as a method for manufacturing an optical laminate will be described.

[0012] 1 and 2 are schematic cross-sectional views of optical laminates 100A and 101A according to an embodiment of the present invention, respectively. As shown in FIG. 1, the optical laminate 100A has an adhesive layer 20a on the uneven structure of the prism surface (first main surface) 12s of the prism sheet (first optical sheet) 10a. Other optical sheets (e.g., a microlens sheet) may be used instead of the prism sheet 10a. As shown in FIG. 2, the optical laminate 101A has the optical laminate 100A and a second optical sheet 30 arranged on the side opposite to the first optical sheet 10a side of the adhesive layer 20a. The description of the optical laminate 100A also applies to the optical laminate 101A unless otherwise specified, so the description may be omitted to avoid duplication.

[0013] In the manufacturing process of the optical laminate 100A (or the optical laminate 101A), when the adhesive layer 20a is attached to the prism sheet 10a by, for example, a roll-to-roll method, it is required that the adhesive layer 20a does not penetrate too much into the recesses of the uneven structure of the prism sheet 10a. In addition, after the adhesive layer 20a is attached to the prism sheet 10a, it is required that the degree to which the adhesive layer 20a penetrates into the recesses does not change easily over time.

[0014] The inventors have discovered that there is a correlation between the creep deformation rate of the adhesive layer 20a and the degree of penetration when the adhesive layer 20a is attached to the prism sheet 10a and the change in the degree of penetration over time, and that the creep deformation rate can be used to select a suitable adhesive layer.

[0015] Generally, when a certain amount of stress is applied to a polymeric material with viscoelasticity, a phenomenon called creep occurs in which strain (deformation rate) increases over time, as shown by the creep curve in Figure 3. The strain of a viscoelastic material when a certain amount of stress is applied contains an elastic component that occurs instantaneously when the stress is applied, a viscoelastic component that is expressed as an increasing function of time and reaches a constant value after a long time, and a viscous component that increases in proportion to time. Due to the viscous component, the strain continues to increase at a constant rate even after a long time has passed. After the stress is removed, the viscous component of the strain remains without recovering.

[0016] The degree to which the adhesive layer 20a penetrates into the recesses when the adhesive layer 20a is bonded is correlated with the creep strain of the adhesive layer 20a after 1 second (referred to as "creep deformation rate A"). In other words, the degree to which the adhesive layer 20a penetrates into the recesses when the adhesive layer 20a is bonded is mainly influenced by the elastic component of the adhesive layer 20a. On the other hand, the change over time in the degree of penetration of the adhesive layer 20a into the recesses is correlated with the creep strain of the adhesive layer 20a after 30 minutes (1800 seconds) (referred to as "creep deformation rate B"). In other words, the change over time in the degree of penetration of the adhesive layer 20a into the recesses is mainly influenced by the viscoelastic component and viscous component of the adhesive layer 20a. The degree to which the adhesive layer 20a penetrates into the recesses can be evaluated by the diffuse transmittance of the optical laminate 100A. The greater the degree to which the adhesive layer 20a penetrates into the recesses of the prism sheet 10a, the smaller the diffuse transmittance. Creep deformation consists of two stages: transient creep (primary creep), an early stage of deformation where the strain rate (slope of the creep curve) gradually decreases, and steady-state creep (secondary creep), where the strain rate becomes almost constant. As shown in Figure 3, 30 minutes (1800 seconds) after pressure application is the time that belongs to the steady-state creep region after transient creep.

[0017] As will be described later with reference to an experimental example, the adhesive layer 20a of the optical laminate 100A according to the embodiment of the present invention has a creep deformation rate A of 10% or less when a stress of 10,000 Pa is applied at 50° C. for 1 second in a creep test using a rotational rheometer, and a creep deformation rate B of 16% or less when a stress of 10,000 Pa is applied at 50° C. for 30 minutes in a creep test using a rotational rheometer. The experimental example also shows the evaluation results of the diffuse transmittance of the optical laminate. The creep deformation rates A and B of the adhesive layer and the diffuse transmittance of the optical laminate can be measured, for example, by the method described in the experimental example described later.

[0018] In the adhesive layer 20a having a creep deformation rate A of 10% or less, the degree of penetration of the adhesive layer 20a into the recesses during bonding is sufficiently suppressed. In the adhesive layer 20a having a creep deformation rate B of 16% or less, the change in the degree of penetration into the recesses over time is sufficiently suppressed. The creep deformation rate A of the adhesive layer 20a is, for example, 10% or less, 9% or less, 8% or less, 7% or less, 6% or less, or 5% or less, and the creep deformation rate B of the adhesive layer 20a is, for example, 16% or less, 15% or less, 14% or less, 13% or less, 12% or less, 11% or less, or 10% or less. The lower limits of the creep deformation rates A and B are not particularly limited, but are, for example, greater than 0. It is more preferable that the adhesive layer 20a has a creep deformation rate A of 8% or less and a creep deformation rate B of 14% or less, and it is even more preferable that the creep deformation rate A is 5% or less and the creep deformation rate B is 10% or less.

[0019] The second optical sheet 30 has a main surface 38s on the adhesive layer 20a side and a main surface 32s opposite to the main surface 38s. The main surface 38s is a flat surface. The second optical sheet 30 can be made of any suitable material depending on the purpose. Examples of materials for the second optical sheet 30 include thermoplastic resins having optical transparency, and more specifically, examples of materials include films formed of (meth)acrylic resins such as polymethyl methacrylate (PMMA) or polycarbonate (PC) resins. At least one other optical member (or optical sheet) may be disposed on the side opposite to the adhesive layer 20a of the second optical sheet 30 of the optical laminate 101A (i.e., on the main surface 32s). The other optical member (optical sheet) includes, for example, a diffusion plate, a light guide plate, etc., and is adhered to the main surface 32s of the optical sheet 30 via an adhesive layer. That is, an optical laminate of another embodiment of the present invention includes the optical laminate 101A and at least one other optical sheet arranged on the side opposite the adhesive layer 20a of the second optical sheet 30 of the optical laminate 101A. An optical device of another embodiment of the present invention includes the optical laminate 101A and another optical member arranged on the side opposite the adhesive layer 20a of the second optical sheet 30 of the optical laminate 101A.

[0020] The 180° peel adhesive strength of the adhesive layer 20a to the PMMA film is, for example, 10 mN / 20 mm or more. The upper limit is not particularly limited, but is, for example, 50 N / 20 mm or less, 40 N / 20 mm or less, 30 N / 20 mm or less, 20 N / 20 mm or less, 10 N / 20 mm or less, or 1 N / 20 mm or less. The haze of the adhesive layer 20a is, for example, 0.01% or more and 5% or less, 4% or less, 3% or less, 2% or less, or 1.5% or less. The thickness of the adhesive layer 20a is, for example, 0.1 μm or more, 0.5 μm or more, or 1.0 μm or more, and 20 μm or less, 15 μm or less, 10 μm or less, or 5 μm or less. The adhesive layer 20a is used to attach the optical laminate 100A to another optical sheet or optical device. The 180° peel adhesive strength of the adhesive layer to the PMMA film and the haze of the adhesive layer can be measured, for example, by the method described in the Experimental Examples below.

[0021] As will be explained later with reference to experimental examples, the adhesive for forming the adhesive layer 20a can suitably be any of the following adhesives.

[0022] The adhesive contains, for example, a (meth)acrylic polymer, and the (meth)acrylic polymer is, for example, a copolymer of a nitrogen-containing (meth)acrylic monomer and at least one other monomer. The nitrogen-containing (meth)acrylic monomer has, for example, a nitrogen-containing cyclic structure. When the (meth)acrylic polymer is prepared using the nitrogen-containing (meth)acrylic monomer, particularly when the nitrogen-containing (meth)acrylic monomer has a nitrogen-containing cyclic structure, the effect of improving the elastic properties of the (meth)acrylic polymer can be obtained.

[0023] When the adhesive contains a (meth)acrylic polymer, the (meth)acrylic polymer is preferably crosslinked. When the adhesive contains a (meth)acrylic polymer, the adhesive may further contain an active energy ray curable resin (e.g., an ultraviolet ray curable resin) and a curing agent (e.g., a photopolymerization initiator), or may further contain a cured product of the active energy ray curable resin. The active energy rays are, for example, visible light and ultraviolet light. By introducing a crosslinked structure into the adhesive, deformation during application of the adhesive and deformation over time are suppressed. In particular, by curing the active energy ray curable resin after applying an adhesive composition layer (to become the adhesive layer 20a) to the optical sheet 10a, deformation over time of the adhesive layer 20a can be suppressed, and the change over time in the extent to which the adhesive layer 20a penetrates into the recesses can be suppressed. When the active energy ray curable resin is cured, the adhesive layer 20a becomes hard. If the adhesive layer 20a is too hard, it may be difficult to bond the adhesive layer 20a to the optical sheet 10a by the roll-to-roll method; however, this problem can be avoided by curing the active energy ray-curable resin after applying the adhesive composition layer to the optical sheet 10a.

[0024] The adhesive layer 20a containing the cured product of the active energy ray curable resin is formed, for example, by the following method. First, an adhesive composition solution layer is formed from an adhesive composition solution containing a (meth)acrylic polymer, a crosslinking agent, an active energy ray curable resin, a polymerization initiator, and a solvent. The adhesive composition solution layer is formed, for example, on a release-treated main surface of a substrate. Next, the solvent in the adhesive composition solution layer is removed, and the (meth)acrylic polymer in the adhesive composition solution layer is crosslinked with a crosslinking agent (for example, by heating) to obtain an adhesive composition layer having a crosslinked structure. When the adhesive composition solution layer is formed on the release-treated main surface of a substrate, an adhesive composition layer is formed on the release-treated main surface of the substrate, and a laminate having a substrate and an adhesive composition layer is obtained. Here, the crosslinked structure formed by the (meth)acrylic polymer and the crosslinking agent is referred to as a first crosslinked structure. It is to be distinguished from a crosslinked structure (second crosslinked structure) formed by curing an active energy ray curable resin, which will be described later. The polymer of the adhesive composition solution layer may be crosslinked in the step of removing the solvent of the adhesive composition solution layer, or a step of crosslinking the polymer of the adhesive composition solution layer may be performed after the step of removing the solvent of the adhesive composition solution layer, separately from the step of removing the solvent of the adhesive composition solution layer. Thereafter, the adhesive composition layer is attached to the first main surface 12s of the optical sheet 10a, and in a state in which the adhesive composition layer is disposed on the first main surface 12s of the optical sheet 10a, the adhesive composition layer is irradiated with active energy rays to cure the active energy ray curable resin, thereby forming the adhesive layer 20a having a second crosslinked structure in addition to the first crosslinked structure. It is considered that the first crosslinked structure and the second crosslinked structure of the adhesive layer 20a form a so-called interpenetrating network structure (IPN).

[0025] The adhesive layer 20a that does not contain a cured product of the active energy ray curable resin is formed, for example, by the following method. First, an adhesive composition solution layer is formed from an adhesive composition solution containing a polymer, a crosslinking agent, and a solvent. This adhesive composition solution does not contain an active energy ray curable resin and a polymerization initiator. The adhesive composition solution layer is formed, for example, on a release-treated main surface of a substrate. Next, the solvent of the adhesive composition solution layer is removed, and the polymer of the adhesive composition solution layer is crosslinked with a crosslinking agent (for example, by heating) to obtain an adhesive layer 20a having a crosslinked structure. When the adhesive composition solution layer is formed on the release-treated main surface of the substrate, an adhesive layer is formed on the release-treated main surface of the substrate, and a laminate having a substrate and an adhesive layer is obtained. The polymer of the adhesive composition solution layer may be crosslinked in the step of removing the solvent of the adhesive composition solution layer, or after the step of removing the solvent of the adhesive composition solution layer, a step of crosslinking the polymer of the adhesive composition solution layer may be further performed separately from the step of removing the solvent of the adhesive composition solution layer.

[0026] The adhesive preferably does not contain a graft polymer. If the adhesive layer is formed from an adhesive composition containing a graft polymer, as in the adhesive layer described in Patent Document 1, the number of design factors and control factors of the material increases, and mass productivity may be poor. The creep characteristics of an adhesive that does not contain a graft polymer can be adjusted by various factors (for example, the type and amount of the crosslinking agent, the type and amount of the actinic radiation curable resin).

[0027] Preferred specific examples of the adhesive will be described below.

[0028] The adhesive contains, for example, a (meth)acrylic polymer. The monomer used in the production of the (meth)acrylic polymer may be any (meth)acrylate, and is not particularly limited. For example, an alkyl (meth)acrylate having an alkyl group with 4 or more carbon atoms may be used. In this case, the ratio of the alkyl (meth)acrylate having an alkyl group with 4 or more carbon atoms to the total amount of monomers used in the production of the (meth)acrylic polymer is, for example, 50% by mass or more.

[0029] In this specification, "alkyl(meth)acrylate" refers to a (meth)acrylate having a linear or branched alkyl group. The number of carbon atoms in the alkyl group of the alkyl(meth)acrylate is preferably 4 or more, and more preferably 4 or more and 9 or less. Note that (meth)acrylate refers to acrylate and / or methacrylate.

[0030] Specific examples of alkyl (meth)acrylates include n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, isoamyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and n-octyl (meth)acrylate. acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate, isomyristyl (meth)acrylate, n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, etc. These can be used alone or in combination.

[0031] The adhesive may contain a (meth)acrylic polymer which is a copolymer of a nitrogen-containing (meth)acrylic monomer and at least one other monomer. In this case, the (meth)acrylic polymer is preferably a copolymer obtained by copolymerizing the following monomers in the following amounts, where the total amount of the monomers used in the copolymerization is 100 parts by mass. Nitrogen-containing (meth)acrylic monomer: 10.0 parts by mass or more, 15.0 parts by mass or more, 20.0 parts by mass or more, 25.0 parts by mass or more, 30.0 parts by mass or more, or 35.0 parts by mass or more, and 40.0 parts by mass or less, 35.0 parts by mass or less, 30.0 parts by mass or less, 25.0 parts by mass or less, 20.0 parts by mass or less, or 15.0 parts by mass or less. For example, 10.0 parts by mass or more and 40.0 parts by mass or less. Hydroxyl group-containing acrylic monomer: 0.05 parts by mass or more, 0.75 parts by mass or more, 1.0 parts by mass or more, 2.0 parts by mass or more, 3.0 parts by mass or more, 4.0 parts by mass or more, 5.0 parts by mass or more, 6.0 parts by mass or more, 7.0 parts by mass or more, 8.0 parts by mass or more, or 9.0 parts by mass or more, and 10.0 parts by mass or less, 9.0 parts by mass or less, 8.0 parts by mass or less, 7.0 parts by mass or less, 6.0 parts by mass or less, 5.0 parts by mass or less, 4.0 parts by mass or less, 3.0 parts by mass or less, 2.0 parts by mass or less, or 1.0 parts by mass or less. For example, 0.05 parts by mass or more and 10.0 parts by mass or less. Carboxyl group-containing acrylic monomer: 1.0 parts by mass or more, 2.0 parts by mass or more, 3.0 parts by mass or more, 4.0 parts by mass or more, 5.0 parts by mass or more, 6.0 parts by mass or more, 7.0 parts by mass or more, 8.0 parts by mass or more, or 9.0 parts by mass or more, and 10.0 parts by mass or less, 9.0 parts by mass or less, 8.0 parts by mass or less, 7.0 parts by mass or less, 6.0 parts by mass or less, 5.0 parts by mass or less, 4.0 parts by mass or less, 3.0 parts by mass or less, or 2.0 parts by mass or less. For example, 1.0 parts by mass or more and 10.0 parts by mass or less. Alkyl (meth)acrylate monomer: (100 parts by mass) - (total amount of monomers other than alkyl (meth)acrylate monomer used in copolymerization)

[0032] In this specification, the term "nitrogen-containing (meth)acrylic monomer" includes, without particular limitation, a monomer having a polymerizable functional group with an unsaturated double bond of a (meth)acryloyl group and having a nitrogen atom. The "nitrogen-containing (meth)acrylic monomer" has, for example, a nitrogen-containing cyclic structure. Examples of the nitrogen-containing (meth)acrylic monomer having a nitrogen-containing cyclic structure include, for example, N-vinyl-2-pyrrolidone (NVP), N-vinyl-ε-caprolactam (NVC), and 4-acryloylmorpholine (ACMO). These can be used alone or in combination.

[0033] In this specification, the term "hydroxyl group-containing acrylic monomer" includes, without particular limitation, monomers having a polymerizable functional group with an unsaturated double bond of a (meth)acryloyl group and having a hydroxyl group. For example, hydroxyalkyl (meth)acrylates such as 2-hydroxybutyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate; 4-hydroxymethylcyclohexyl (meth)acrylate, and 4-hydroxybutyl vinyl ether.

[0034] In this specification, the term "carboxyl group-containing acrylic monomer" includes, without particular limitation, a monomer having a polymerizable functional group having an unsaturated double bond such as a (meth)acryloyl group or a vinyl group, and also having a carboxyl group. Examples of unsaturated carboxylic acid-containing monomers include (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. These can be used alone or in combination.

[0035] The adhesive may contain a (meth)acrylic polymer which is a copolymer of a carboxyl group-containing acrylic monomer and at least one other monomer (excluding nitrogen-containing (meth)acrylic monomers). In this case, the (meth)acrylic polymer is preferably a copolymer obtained by copolymerizing the following monomers in the following amounts when the total amount of the monomers used in the copolymerization is taken as 100 parts by mass. Carboxyl group-containing acrylic monomer: 1.0 parts by mass or more, 2.0 parts by mass or more, 3.0 parts by mass or more, 4.0 parts by mass or more, 5.0 parts by mass or more, 6.0 parts by mass or more, 7.0 parts by mass or more, 8.0 parts by mass or more, or 9.0 parts by mass or more, and 10.0 parts by mass or less, 9.0 parts by mass or less, 8.0 parts by mass or less, 7.0 parts by mass or less, 6.0 parts by mass or less, 5.0 parts by mass or less, 4.0 parts by mass or less, 3.0 parts by mass or less, or 2.0 parts by mass or less. For example, 1.0 parts by mass or more and 10.0 parts by mass or less. Alkyl (meth)acrylate monomer: 90.0 parts by mass or more, 91.0 parts by mass or more, 92.0 parts by mass or more, 93.0 parts by mass or more, 94.0 parts by mass or more, 95.0 parts by mass or more, 96.0 parts by mass or more, 97.0 parts by mass or more, or 98.0 parts by mass or more, and 99.0 parts by mass or less, 98.0 parts by mass or less, 97.0 parts by mass or less, 96.0 parts by mass or less, 95.0 parts by mass or less, 94.0 parts by mass or less, 93.0 parts by mass or less, 92.0 parts by mass or less, or 91.0 parts by mass or less. For example, 90.0 parts by mass or more and 99.0 parts by mass or less.

[0036] Examples of crosslinking agents that introduce a crosslinked structure into the (meth)acrylic polymer include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, silicone-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, silane-based crosslinking agents, alkyl etherified melamine-based crosslinking agents, metal chelate-based crosslinking agents, peroxides, etc. The crosslinking agents can be used alone or in combination of two or more.

[0037] An isocyanate-based crosslinking agent is a compound having two or more isocyanate groups (including isocyanate regenerating functional groups in which the isocyanate groups are temporarily protected by a blocking agent or oligomerization) in one molecule.

[0038] Examples of the isocyanate crosslinking agent include aromatic isocyanates such as tolylene diisocyanate and xylylene diisocyanate, alicyclic isocyanates such as isophorone diisocyanate, and aliphatic isocyanates such as hexamethylene diisocyanate.

[0039] More specifically, for example, lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate, alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate, aromatic diisocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate and polymethylene polyphenyl isocyanate, trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, product name: Coronate L), trimethylolpropane / hexamethylene diisocyanate trimer adduct ( Examples of such polyisocyanates include isocyanate adducts such as isocyanurate of hexamethylene diisocyanate (manufactured by Tosoh Corporation, product name: Coronate HL) and isocyanurate of hexamethylene diisocyanate (manufactured by Tosoh Corporation, product name: Coronate HX), trimethylolpropane adduct of xylylene diisocyanate (manufactured by Mitsui Chemicals, Inc., product name: D110N), trimethylolpropane adduct of hexamethylene diisocyanate (manufactured by Mitsui Chemicals, Inc., product name: D160N); polyether polyisocyanates, polyester polyisocyanates, and adducts of these with various polyols, and polyisocyanates multifunctionalized with isocyanurate bonds, biuret bonds, allophanate bonds, etc.

[0040] The isocyanate crosslinking agent may be used alone or in combination of two or more. The amount of the isocyanate crosslinking agent is, for example, 0.01 parts by mass or more, 0.02 parts by mass or more, 0.05 parts by mass or more, or 0.1 parts by mass or more, and 10 parts by mass or less, 9 parts by mass or less, 8 parts by mass or less, 7 parts by mass or less, 6 parts by mass or less, or 5 parts by mass or less, and preferably 0.01 parts by mass or more and 10 parts by mass or less, 0.02 parts by mass or more and 9 parts by mass or less, or 0.05 parts by mass or more and 8 parts by mass or less. The amount of the isocyanate crosslinking agent may be appropriately adjusted in consideration of the cohesive force, prevention of peeling in a durability test, and the like.

[0041] In addition, in the aqueous dispersion of the modified (meth)acrylic polymer prepared by emulsion polymerization, it is not necessary to use an isocyanate-based crosslinking agent. However, if necessary, a blocked isocyanate-based crosslinking agent can be used since it easily reacts with water.

[0042] The epoxy crosslinking agent is a multifunctional epoxy compound having two or more epoxy groups in one molecule. Examples of the epoxy crosslinking agent include bisphenol A, epichlorohydrin type epoxy resin, ethylene glycidyl ether, N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, diamine glycidylamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, sorbitol, and the like. Examples of the epoxy crosslinking agent include polyglycidyl ether, glycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, polyglycerol polyglycidyl ether, sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl-tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. Examples of the epoxy crosslinking agent include Mitsubishi Gas Chemical Company, Inc.'s product names "Tetrad C" and "Tetrad X".

[0043] The epoxy crosslinking agent may be used alone or in combination of two or more. The amount of the epoxy crosslinking agent is, for example, 0.01 parts by mass or more, 0.02 parts by mass or more, 0.05 parts by mass or more, or 0.1 parts by mass or more, and 10 parts by mass or less, 9 parts by mass or less, 8 parts by mass or less, 7 parts by mass or less, 6 parts by mass or less, or 5 parts by mass or less, and preferably 0.01 parts by mass or more and 10 parts by mass or less, 0.02 parts by mass or more and 9 parts by mass or less, or 0.05 parts by mass or more and 8 parts by mass or less. The amount of the epoxy crosslinking agent may be appropriately adjusted in consideration of the cohesive force, prevention of peeling in a durability test, and the like.

[0044] Any peroxide crosslinking agent can be used as long as it generates radical active species when heated and promotes crosslinking of the base polymer of the adhesive. Taking into account workability and stability, it is preferable to use a peroxide whose 1-minute half-life temperature is 80°C or higher and 160°C or lower, and it is even more preferable to use a peroxide whose 1-minute half-life temperature is 90°C or higher and 140°C or lower.

[0045] Examples of peroxides include di(2-ethylhexyl)peroxydicarbonate (1-minute half-life temperature: 90.6° C.), di(4-t-butylcyclohexyl)peroxydicarbonate (1-minute half-life temperature: 92.1° C.), di-sec-butylperoxydicarbonate (1-minute half-life temperature: 92.4° C.), t-butylperoxyneodecanoate (1-minute half-life temperature: 103.5° C.), t-hexylperoxypivalate (1-minute half-life temperature: 109.1° C.), t-butylperoxypivalate (1-minute half-life temperature: 110.3° C.), dilauroylperoxide (1 1-minute half-life temperature: 116.4°C), di-n-octanoyl peroxide (1-minute half-life temperature: 117.4°C), 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate (1-minute half-life temperature: 124.3°C), di(4-methylbenzoyl)peroxide (1-minute half-life temperature: 128.2°C), dibenzoyl peroxide (1-minute half-life temperature: 130.0°C), t-butylperoxyisobutyrate (1-minute half-life temperature: 136.1°C), 1,1-di(t-hexylperoxy)cyclohexane (1-minute half-life temperature: 149.2°C), and the like. Among these, di(4-t-butylcyclohexyl) peroxydicarbonate (1-minute half-life temperature: 92.1°C), dilauroyl peroxide (1-minute half-life temperature: 116.4°C), dibenzoyl peroxide (1-minute half-life temperature: 130.0°C), etc. are preferably used because of their excellent crosslinking reaction efficiency.

[0046] The half-life of a peroxide is an index showing the decomposition rate of the peroxide, and refers to the time it takes for the remaining amount of peroxide to be reduced to half. The decomposition temperature for obtaining the half-life at any time and the half-life time at any temperature are listed in manufacturer catalogs, for example, NOF Corporation's "Organic Peroxide Catalog 9th Edition (May 2003)."

[0047] The peroxide may be used alone or in combination of two or more. The amount of the peroxide is 0.02 to 2 parts by mass, preferably 0.05 to 1 part by mass, based on 100 parts by mass of the (meth)acrylic polymer. The amount is appropriately adjusted within this range to adjust processability, reworkability, crosslinking stability, peelability, etc.

[0048] The amount of decomposed peroxide remaining after the reaction treatment can be measured, for example, by HPLC (high performance liquid chromatography).

[0049] More specifically, for example, about 0.2 g of the adhesive after the reaction treatment is taken out, immersed in 10 ml of ethyl acetate, and extracted by shaking at 120 rpm at 25°C for 3 hours in a shaker, and then allowed to stand at room temperature for 3 days. Next, 10 ml of acetonitrile is added, and the mixture is shaken at 120 rpm at 25°C for 30 minutes, and about 10 μl of the extract obtained by filtering through a membrane filter (0.45 μm) is injected into HPLC for analysis, and the amount of peroxide after the reaction treatment can be determined.

[0050] In addition, an organic crosslinking agent or a polyfunctional metal chelate may be used as the crosslinking agent. The polyfunctional metal chelate is a compound in which a polyvalent metal is covalently or coordinately bonded to an organic compound. Examples of polyvalent metal atoms include Al, Cr, Zr, Co, Cu, Fe, Ni, V, Zn, In, Ca, Mg, Mn, Y, Ce, Sr, Ba, Mo, La, Sn, and Ti. Examples of atoms in the organic compound that are covalently or coordinately bonded include oxygen atoms, and examples of the organic compound include alkyl esters, alcohol compounds, carboxylic acid compounds, ether compounds, and ketone compounds.

[0051] The amount of active energy ray curable resin is, for example, 3 parts by mass or more and 60 parts by mass or less with respect to 100 parts by mass of the (meth)acrylic polymer. The mass average molecular weight (Mw) before curing is 4000 or more and 50000 or less. As the active energy ray curable resin, for example, an acrylate-based, epoxy-based, urethane-based, or ene-thiol-based ultraviolet curable resin can be suitably used.

[0052] As the active energy ray-curable resin, a monomer and / or oligomer that undergoes radical polymerization or cationic polymerization by active energy rays is used.

[0053] Examples of monomers that undergo radical polymerization by active energy rays include monomers having an unsaturated double bond such as a (meth)acryloyl group or a vinyl group, and monomers having a (meth)acryloyl group are preferably used because of their excellent reactivity.

[0054] Specific examples of monomers having a (meth)acryloyl group include allyl (meth)acrylate, caprolactone (meth)acrylate, cyclohexyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, glycidyl (meth)acrylate, caprolactone-modified 2-hydroxyethyl (meth)acrylate, isobornyl (meth)acrylate, morpholine (meth)acrylate, phenoxyethyl (meth)acrylate, tripropylene glycol di( Examples of the polyvinyl chloride di(meth)acrylate include tert-butyl ether di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane ethoxy tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and caprolactone-modified dipentaerythritol hexa(meth)acrylate.

[0055] Examples of oligomers that undergo radical polymerization by active energy rays include polyester (meth)acrylates, epoxy (meth)acrylates, and urethane (meth)acrylates, which have two or more unsaturated double bonds, such as (meth)acryloyl groups and vinyl groups, added to the backbone of polyester, epoxy, or urethane as functional groups similar to those of monomers.

[0056] Polyester (meth)acrylates are obtained by reacting a polyester having terminal hydroxyl groups, obtained from a polyhydric alcohol and a polycarboxylic acid, with (meth)acrylic acid. Specific examples include the Aronix M-6000, 7000, 8000, and 9000 series manufactured by Toa Gosei Co., Ltd.

[0057] Epoxy (meth)acrylates are obtained by reacting epoxy resins with (meth)acrylic acid, and specific examples include Lipoxy SP and VR series manufactured by Showa Polymer Co., Ltd. and Epoxy Ester series manufactured by Kyoeisha Chemical Co., Ltd.

[0058] Urethane (meth)acrylates are obtained by reacting polyols, isocyanates, and hydroxy (meth)acrylates. Specific examples include the Art Resin UN series manufactured by Negami Chemical Industrial Co., Ltd., the NK Oligo U series manufactured by Shin-Nakamura Chemical Co., Ltd., and the Shikoh UV series manufactured by Mitsubishi Chemical Corporation.

[0059] The photopolymerization initiator is excited and activated by irradiation with ultraviolet light to generate radicals, and has the effect of curing the polyfunctional oligomer through radical polymerization. For example, acetophenone-based photopolymerization initiators such as 4-phenoxydichloroacetophenone, 4-t-butyldichloroacetophenone, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 1-(4-dodecylphenyl)-2-hydroxy-2-methylpropan-1-one, 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexylphenylketone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1; benzoin-based photopolymerization initiators such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, and 2,2-dimethoxy-2-phenylacetophenone; benzophenone, benzoylbenzoic acid, benzoylbenzoic acid methyl; 4-phenoxyphenyl; Examples of the photopolymerization initiator include benzophenone-based photopolymerization initiators such as nylbenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, and 3,3'-dimethyl-4-methoxybenzophenone; thioxanthone-based photopolymerization initiators such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone; and special photopolymerization initiators such as α-acyloxime ester, acylphosphine oxide, methylphenyl glyoxylate, benzil, camphorquinone, dibenzosuberone, 2-ethylanthraquinone, and 4',4"-diethylisophthalophenone. Examples of the photopolymerization initiator include allylsulfonium hexafluorophosphate salts, sulfonium hexafluorophosphate salts, and bis(alkylphenyl) A photocationic polymerization initiator such as iodonium hexafluorophosphate can also be used.

[0060] The photopolymerization initiator may be used in combination of two or more kinds. The polymerization initiator is preferably blended in an amount of 0.5 to 30 parts by mass, more preferably 1 to 20 parts by mass, per 100 parts by mass of the active energy ray curable resin. If the amount is less than 0.5 parts by mass, the polymerization does not proceed sufficiently, and the curing speed becomes slow, whereas if the amount is more than 30 parts by mass, the hardness of the cured sheet may decrease.

[0061] The active energy rays are not particularly limited, but are preferably ultraviolet rays, visible light, and electron beams. The crosslinking treatment by ultraviolet irradiation can be carried out using an appropriate ultraviolet light source such as a high pressure mercury lamp, a low pressure mercury lamp, an excimer laser, a metal halide lamp, or an LED lamp. In this case, the amount of ultraviolet irradiation can be appropriately selected depending on the required degree of crosslinking, but usually, for ultraviolet rays, it is 0.2 J / cm. 2 More than 10J / cm 2 It is desirable to select from the following ranges: The temperature during irradiation is not particularly limited, but is preferably up to about 140° C. in consideration of the heat resistance of the support.

[0062] When the adhesive contains a polyester-based polymer instead of or together with the (meth)acrylic polymer, for example, a polyester-based polymer having the following characteristics is preferred.

[0063] The type of carboxylic acid component (or the characteristics of the skeleton, etc.): At least a dicarboxylic acid containing two carboxyl groups is contained, specifically, a dicarboxylic acid. The dicarboxylic acid is not particularly limited, but examples thereof include dimer acids derived from sebacic acid, oleic acid, and erucic acid. Other examples include aliphatic or alicyclic dicarboxylic acids such as glutaric acid, suberic acid, adipic acid, azelaic acid, 1,4-cyclohexanedicarboxylic acid, 4-methyl-1,2-cyclohexanedicarboxylic acid, dodecenylsuccinic anhydride, fumaric acid, succinic acid, dodecanedioic acid, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, maleic acid, maleic anhydride, itaconic acid, and citraconic acid, as well as terephthalic acid, isophthalic acid, orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 2,2'-diphenyldicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid. In addition to the dicarboxylic acids mentioned above, tricarboxylic acids containing three or more carboxyl groups can also be used.

[0064] Type of diol component (or skeletal characteristics, etc.): Contains at least one having two hydroxyl groups in the molecule, specifically diol. Fatty acid esters, dimer diols derived from oleic acid, erucic acid, etc., glycerol monostearate, etc. Others include aliphatic glycols such as ethylene glycol and 1,2-propylene glycol, and as non-aliphatic glycols, ethylene oxide adducts and propylene oxide adducts of bisphenol A, ethylene oxide adducts and propylene oxide adducts of hydrogenated bisphenol A, etc.

[0065] As a crosslinking agent for introducing a crosslinked structure into the polyester polymer, an isocyanate crosslinking agent, an oxazoline crosslinking agent, an aziridine crosslinking agent, a silane crosslinking agent, an alkyl etherified melamine crosslinking agent, or a metal chelate crosslinking agent can be used. The blending amount is, for example, 2.0 parts by mass or more and 10.0 parts by mass or less per 100 parts by mass of the polyester polymer.

[0066] Next, optical laminates 100B and 101B according to other embodiments of the present invention will be described with reference to Figs. 4 to 6. For components having substantially the same functions as those of the previous embodiment, the description of the previous embodiment applies unless otherwise specified. The optical laminate 100B functions as a light distribution control element described in Patent Document 2, and can be manufactured using a roll-to-roll method. The entire disclosure of Patent Document 2 is incorporated herein by reference.

[0067] Fig. 4 is a schematic cross-sectional view of the optical laminates 100B and 101B, showing a state in which the first optical sheet 10b is bonded to the surface 38s of the second optical sheet 30 via an adhesive layer 20b. Fig. 5 is a schematic perspective view of the optical sheet 10b of the optical laminate 100B. Fig. 6 is a schematic cross-sectional view of an illumination device 200 including the optical laminate 102B and a light source 60, showing the trajectory of a light ray.

[0068] Please refer to FIG. 4 and FIG. 5. The optical laminate 100B has a first optical sheet 10b having a first main surface 12s having a concave-convex structure and a second main surface 18s opposite to the first main surface 12s, and an adhesive layer 20b arranged on the first main surface 12s side of the first optical sheet 10b. The optical laminate 101B has the optical laminate 100B and a second optical sheet 30 arranged on the side opposite to the first optical sheet 10b side of the adhesive layer 20a. Here, the concave-convex structure of the first main surface 12s of the optical sheet 10b includes a plurality of recesses 14, and the surface of the adhesive layer 20b and the first main surface 12s of the optical sheet 10b define a plurality of spaces 14 (indicated by the same reference numerals as the recesses) in the plurality of recesses 14. The adhesive layer 20b is an essential component for defining the spaces 14 of the optical laminate 100B, and is a part of the optical laminate 100B.

[0069] The uneven structure of the optical sheet 10b includes a flat portion 10s in contact with the adhesive layer 20b. The uneven structure includes, for example, a plurality of convex portions 15 each having a trapezoidal cross section. Since the uneven structure has the flat portion 10s in contact with the adhesive layer 20b, the uneven structure of the optical sheet 10b is less susceptible to the adhesive layer 20b penetrating into the concave portions than the uneven structure of the prism surface of the prism sheet 10a shown in FIG. 1. Therefore, by using the above adhesive, an optical laminate 100B can be obtained in which the adhesive layer 20b does not penetrate into the plurality of spaces 14 and does not change over time.

[0070] The optical sheet 10b can be manufactured by the same method and using the same material as the known prism sheet or microlens sheet. The size and shape of the uneven structure of the optical sheet 10b can be changed as appropriate (Patent Document 2). However, as described above, the optical sheet 10b differs from the known prism sheet or microlens sheet in that the optical sheet 10b functions as the optical laminate 100B in which the space 14 is defined only after it is bonded to the adhesive layer 20.

[0071] 4, in the optical laminate 101B, the second optical sheet 30 is disposed so that its surface 38s is adhered to the surface 22s of the adhesive layer 20b. Any appropriate material can be used as the material constituting the second optical sheet 30 depending on the purpose. Examples of materials for the second optical sheet 30 include light-transmitting thermoplastic resins, and more specifically, examples of materials include films formed of (meth)acrylic resins such as polymethyl methacrylate (PMMA) and polycarbonate (PC) resins.

[0072] The space 14 of the optical laminate 100B is defined by surfaces 16s and 17s, which are parts of the first main surface 12s of the first optical sheet 10b, and a surface 28s of the adhesive layer 20b. Here, an example is shown in which the surface 16s is inclined (more than 0° and less than 90°) with respect to the sheet surface (the horizontal direction in the figure), and the surface 17s is approximately perpendicular to the sheet surface, but this is not limiting and various modifications may be made (see Patent Document 2).

[0073] The optical laminate 100B is used in a lighting device 200, for example, as shown in FIG. 6. A light guide plate 50 is provided on the side of the adhesive layer 20b of the optical laminate 100B opposite to the first optical sheet 10b side. The optical laminate 100B and the light guide plate 50 are collectively referred to as an optical laminate 102B. The optical laminate 102B is bonded to the light guide plate 50 at the surface 22s of the adhesive layer 20b of the optical laminate 100B. The light guide plate 50 is disposed so that light from a light source (e.g., an LED) 60 is incident on the light receiving surface of the light guide plate 50, and the light guided into the light guide plate 50 is totally reflected (TIR) ​​at the interface 16s and the interface 14s formed by the space 14, as shown by the arrows in FIG. 6. The light beam totally reflected at the interface 14s (surface 28s of the adhesive layer 20b) is guided through the light guide plate 50 and the adhesive layer 20b, and the light beam totally reflected at the inclined surface 16s is emitted to the outside from the surface 18s of the optical laminate 100B. The distribution (light distribution) of the light beam emitted from the optical laminate 100B can be adjusted by adjusting the shape, size, arrangement density, etc. of the space 14. Here, it is preferable that the refractive indexes of the light guide plate 50, the adhesive layer 20b, and the optical sheet 10b are equal to each other.

[0074] 4 to 6 show an example in which the cross-sectional shape of the protrusion 15 is a trapezoid, but the shape of the protrusion 15 is not limited to that shown in the drawings and can be modified in various ways. By adjusting the shape, size, etc. of the protrusion 15, the shape, size, arrangement density, etc. of the space 14 can be adjusted. For example, WO 2011 / 124765 describes an example of a laminate having a plurality of spaces therein. The entire disclosure of WO 2011 / 124765 is incorporated herein by reference.

[0075] Experimental examples (Examples and Comparative Examples) will be described below.

[0076] [Example 1] (Preparation of Adhesive Composition Solution) First, an acrylic polymer was prepared. In a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a cooler, 62.9 parts by mass of n-butyl acrylate (BA), 33.9 parts by mass of 4-acryloylmorpholine (ACMO), 2.9 parts by mass of acrylic acid (AA), 0.3 parts by mass of 4-hydroxybutyl acrylate (4HBA), and 0.1 parts by mass of 2,2'-azobisisobutyronitrile as a polymerization initiator were charged into the flask together with ethyl acetate so that the total monomer amount was 50% by mass, and nitrogen gas was introduced while gently stirring to replace the nitrogen gas for 1 hour, and then the liquid temperature in the flask was kept at around 58 ° C. and a polymerization reaction was carried out for 8 hours to obtain an acrylic polymer. Here, after 2 hours had passed since the start of the polymerization reaction, ethyl acetate was dropped over 3 hours so that the solid content was 35% by mass. That is, the acrylic polymer was obtained as an acrylic polymer solution having a solid content of 35% by mass.

[0077] Next, the obtained acrylic polymer solution was mixed with 7 parts by mass of ultraviolet-curable urethane acrylate resin A (mass average molecular weight Mw: 5,500) in terms of solid content, 0.7 parts by mass of 2,2-dimethoxy-1,2-diphenylethan-1-one (product name "Omnirad651", manufactured by IGM Japan LLC) as a photopolymerization initiator, and 0.1 parts by mass of 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane (product name "TETRAD-C", manufactured by Mitsubishi Gas Chemical Co., Inc.) as a crosslinking agent, per 100 parts by mass of the polymer, to prepare an adhesive composition solution.

[0078] (Preparation of adhesive sheet) An adhesive composition solution was applied to one side of a silicone release-treated 38 μm-thick polyethylene terephthalate (PET) film (trade name "MRF38", manufactured by Mitsubishi Chemical Corporation) to form an adhesive composition solution layer. At this time, the adhesive composition solution layer was applied so that the thickness after drying (i.e., the thickness of the adhesive composition layer) was 1 μm. The adhesive composition solution layer was dried at 150° C. for 3 minutes to remove the solvent from the adhesive composition solution layer and crosslink the acrylic polymer with a crosslinking agent to obtain an adhesive composition layer having a first crosslinked structure. Next, the adhesive composition layer was bonded to the release-treated surface of a silicone release-treated 38 μm-thick polyethylene terephthalate (PET) film (trade name "MRE38", manufactured by Mitsubishi Chemical Corporation) to produce an adhesive sheet (first laminate) having a laminated structure of PET film / adhesive composition layer / PET film.

[0079] (Preparation of optical laminate) One of the release-treated PET films was peeled off from the obtained adhesive sheet (first laminate) and the exposed adhesive composition layer was bonded to an acrylic resin film (thickness: 20 μm). The other separator (PET film) was then peeled off and the layer was bonded to the prism surface of a prism sheet (manufactured by Nippon Tokushu Kogaku Jushi Co., Ltd., product number "LPV90-0.01S") having irregularities with a pitch P of 10 μm, a height H of 5.0 μm, and an apex angle θ of 90° (see Figure 1), to obtain a laminate (second laminate) having a laminate structure of acrylic resin film / adhesive composition layer / prism sheet.

[0080] Next, this second laminate was irradiated with ultraviolet light from the upper surface (acrylic resin film side) of the second laminate to cure the ultraviolet curable resin in the adhesive composition layer, thereby forming an adhesive layer having a second crosslinked structure in addition to the first crosslinked structure, and an optical laminate (third laminate) of Example 1 having a laminated structure of acrylic resin film / adhesive layer / prism sheet (optical sheet) was obtained. The optical laminate (third laminate) of Example 1 has a first optical sheet (prism sheet) 10a, an adhesive layer 20a, and a second optical sheet (acrylic resin film) 30, as in the optical laminate 101A shown in FIG. 2. The ultraviolet light irradiation was performed using an LED lamp (manufactured by Quark Technology Co., Ltd., peak illuminance: 200 mW / cm2). 2 , cumulative light intensity 1500mJ / cm 2 (wavelength 345-365 nm) was used, and the UV illuminance was measured using a UV Power Puck (manufactured by Fusion UV Systems Japan, Inc.).

[0081] [Example 2] (Preparation of Adhesive Composition Solution) Example 2 differs from Example 1 in that in the preparation of the acrylic polymer, n-butyl acrylate, 4-acryloylmorpholine, acrylic acid, and 4-hydroxybutyl acrylate were used in amounts of 67.8 parts by mass, 29.0 parts by mass, 2.9 parts by mass, and 0.3 parts by mass, respectively. 0.1 parts by mass of 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane (product name "TETRAD-C", manufactured by Mitsubishi Gas Chemical Co., Ltd.) was added as a crosslinking agent to the obtained acrylic polymer solution per 100 parts by mass of the solid content of the polymer to prepare an adhesive composition solution. That is, the adhesive composition solution of Example 2 does not contain an ultraviolet curable resin and a photopolymerization initiator.

[0082] (Preparation of adhesive sheet) An adhesive composition solution was applied to one side of a 38 μm thick polyethylene terephthalate (PET) film (product name "MRF38", manufactured by Mitsubishi Chemical Corporation) that had been subjected to a silicone release treatment to form an adhesive composition solution layer. At this time, the adhesive composition solution layer was applied so that the thickness after drying (i.e., the thickness of the adhesive layer) would be 1 μm. The adhesive composition solution layer was dried at 150° C. for 3 minutes to remove the solvent from the adhesive composition solution layer, and the acrylic polymer was crosslinked with a crosslinking agent to obtain an adhesive layer having a crosslinked structure.

[0083] In the above-mentioned Example 1, the adhesive composition solution contains an acrylic polymer, a crosslinking agent, an ultraviolet curing resin, a photopolymerization initiator, and a solvent. In Example 1, an adhesive composition solution layer formed from the adhesive composition solution is dried at 150°C for 3 minutes, and an adhesive composition layer having a first crosslinked structure is formed by crosslinking the acrylic polymer with a crosslinking agent, and then an adhesive layer having a second crosslinked structure in addition to the first crosslinked structure is formed by curing the ultraviolet curing resin of the adhesive composition layer. In contrast, in Example 2, the adhesive composition solution does not contain an ultraviolet curing resin and a photopolymerization initiator. In Example 2, an adhesive composition solution layer formed from the adhesive composition solution is dried at 150°C for 3 minutes, and an adhesive layer having a crosslinked structure is formed by crosslinking the acrylic polymer with a crosslinking agent.

[0084] Next, an adhesive layer was bonded to the release-treated surface of a 38 μm thick polyethylene terephthalate (PET) film (product name "MRE38", manufactured by Mitsubishi Chemical Corporation) that had been silicone release-treated to produce an adhesive sheet (first laminate) having a laminated structure of PET film / adhesive layer / PET film.

[0085] (Preparation of optical laminate) One of the release-treated PET films was peeled off from the obtained adhesive sheet (first laminate), and the exposed adhesive layer was attached to an acrylic resin film (thickness: 20 μm), and the other separator (PET film) was peeled off and attached to the prism surface of a prism sheet (manufactured by Nippon Tokushu Kogaku Jushi Co., Ltd., product number "LPV90-0.01S") having irregularities with a pitch of 10 μm and a height of 5.0 μm, thereby obtaining an optical laminate (second laminate) of Example 2. The optical laminate of Example 2 has a first optical sheet (prism sheet) 10a, an adhesive layer 20a, and a second optical sheet (acrylic resin film) 30, as in the optical laminate 101A shown in FIG.

[0086] [Example 3] (Preparation of Adhesive Composition Solution) In Example 3, in the preparation of an acrylic polymer, 95.0 parts by mass of n-butyl acrylate, 5.0 parts by mass of acrylic acid, and 0.2 parts by mass of 2,2'-azobisisobutyronitrile as a polymerization initiator were charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas introduction tube, and a cooler together with ethyl acetate so that the total monomer amount was 40.0% by mass. After introducing nitrogen gas while gently stirring to replace with nitrogen for 1 hour, the liquid temperature in the flask was kept at about 63°C and a polymerization reaction was carried out for 6 hours. Thereafter, ethyl acetate was added so that the solid content was 40% by mass, and an acrylic polymer was obtained. An adhesive composition solution was prepared by blending 6.0 parts by mass of 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane (trade name "TETRAD-C", manufactured by Mitsubishi Gas Chemical Co., Ltd.) as a crosslinking agent with respect to 100 parts by mass of the solid content of the polymer into the obtained acrylic polymer solution.

[0087] (Preparation of adhesive sheet) The same procedure as in Example 2 was followed.

[0088] (Preparation of optical laminate) The same procedure as in Example 2 was followed.

[0089] [Example 4] (Preparation of Adhesive Composition Solution) First, a polyester polymer was prepared. A three-necked separable flask was equipped with a stirrer, a thermometer, and a vacuum pump, and 48.9 g of dimer acid (trade name "Pripol 1009", molecular weight 567, manufactured by Croda Japan Co., Ltd.), 51.1 g of dimer diol (trade name "Pripol 2033", molecular weight 537, manufactured by Croda Japan Co., Ltd.), and 0.1 g of dibutyltin oxide (manufactured by Kanto Chemical Co., Ltd.) as a catalyst were charged therein, and the temperature was raised to 200°C while stirring in a reduced pressure atmosphere (2.0 kPa or less), and this temperature was maintained. The reaction was continued for about 5 hours to obtain a polyester polymer.

[0090] The obtained polyester polymer solution was mixed with 4.0 parts by mass of an isocyanurate of hexamethylene diisocyanate (product name "Coronate HX", manufactured by Tosoh Corporation) as a crosslinking agent per 100 parts by mass of the solid content of the polymer to prepare an adhesive composition solution.

[0091] (Preparation of adhesive sheet) An adhesive composition solution was applied to one side of a silicone release-treated 38 μm-thick polyethylene terephthalate (PET) film (trade name "MRF38", manufactured by Mitsubishi Chemical Corporation) to form an adhesive composition solution layer. At this time, the adhesive composition solution layer was applied so that the thickness after drying (i.e., the thickness of the adhesive layer) would be 3 μm. The adhesive composition solution layer was dried at 120° C. for 3 minutes to remove the solvent and obtain an adhesive composition layer. Next, the adhesive composition layer was attached to the release-treated surface of a silicone release-treated 38 μm-thick polyethylene terephthalate (PET) film (trade name "MRE38", manufactured by Mitsubishi Chemical Corporation) and left at 40° C. for 3 days to produce an adhesive sheet (first laminate) having a laminated structure of PET film / adhesive layer / PET film. By treating at 40° C. for 3 days, the polyester polymer of the adhesive composition layer is crosslinked with the crosslinking agent, and an adhesive layer having a crosslinked structure is obtained. Note that a crosslinking reaction may also occur partially in the process of drying at 120° C. for 3 minutes.

[0092] (Preparation of optical laminate) The same procedure as in Example 2 was followed.

[0093] [Example 5] (Preparation of Adhesive Composition Solution) Example 5 differs from Example 1 in that in the preparation of the acrylic polymer, n-butyl acrylate, 4-acryloylmorpholine, acrylic acid, and 4-hydroxybutyl acrylate were used in amounts of 74.6 parts by mass, 18.6 parts by mass, 6.5 parts by mass, and 0.3 parts by mass, respectively. Furthermore, in the preparation of the adhesive composition solution, the obtained acrylic polymer solution was mixed with 10 parts by mass of ultraviolet-curable urethane acrylate resin A in solid form as an ultraviolet-curable resin, 1.0 part by mass of 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone (trade name "Omnirad2959", manufactured by IGM Japan LLC) as a photopolymerization initiator, and 0.6 parts by mass of 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane (trade name "TETRAD-C", manufactured by Mitsubishi Gas Chemical Co., Ltd.) as a crosslinking agent, relative to 100 parts by mass of the polymer. The rest was the same as in Example 1.

[0094] (Preparation of adhesive sheet) The same procedure as in Example 1 was followed.

[0095] (Preparation of optical laminate) The same procedure as in Example 1 was followed.

[0096] [Example 5a] An optical laminate of Example 5a having a laminated structure of acrylic resin film / adhesive layer / optical sheet (textured film) was prepared in the same manner as in Example 5, except that the following textured film 70 was used as the optical sheet.

[0097] (Manufacturing of textured film) A concave-convex film was produced according to the method described in JP-A-2013-524288. Specifically, the surface of a polymethyl methacrylate (PMMA) film was coated with lacquer (Finecure RM-64, manufactured by Sanyo Chemical Industries, Ltd.), an optical pattern was embossed on the film surface containing the lacquer, and then the lacquer was cured to produce the desired concave-convex film. The total thickness of the concave-convex film was 130 μm, and the haze was 0.8%. FIG. 7A shows a plan view of a part of the produced concave-convex film 70 seen from the concave-convex surface side. FIG. 7B shows a 7B-7B' cross-sectional view of the concave-convex film of FIG. 7A. A plurality of recesses 74 having a length L of 80 μm, a width W of 14 μm, and a depth H of 10 μm and a triangular cross section were arranged at intervals of width E (155 μm) in the X-axis direction. Furthermore, such a pattern of recesses 74 was arranged at intervals of width D (100 μm) in the Y-axis direction. The density of the recesses 74 on the surface of the unevenly shaped film was 3612 pieces / cm 2 7B, θa and θb were both 41°, and the occupied area ratio of the recesses 74 when the film was viewed in plan from the uneven surface side was 4.05%.

[0098] [Example 6] Example 6 differs from Example 5 in that, in the preparation of the adhesive sheet (first laminate), the thickness of the adhesive composition solution layer after drying (i.e., the thickness of the adhesive composition layer) was 5 μm. The rest of the procedure was the same as in Example 5.

[0099] [Example 6a] An optical laminate of Example 6a having a laminated structure of acrylic resin film / adhesive layer / optical sheet (texture-imparting film) was prepared in the same manner as in Example 6, except that a texture-imparting film 70 was used as the optical sheet.

[0100] [Example 7] Example 7 differs from Example 5 in that, in the preparation of the adhesive sheet (first laminate), the thickness of the adhesive composition solution layer after drying (i.e., the thickness of the adhesive composition layer) was 10 μm. The rest of the procedure was the same as in Example 5.

[0101] [Example 7a] An optical laminate of Example 7a having a laminated structure of acrylic resin film / adhesive layer / optical sheet (textured film) was prepared in the same manner as in Example 7, except that a textured film 70 was used as the optical sheet.

[0102] [Comparative Example 1] Comparative Example 1 differs from Example 2 in that in the preparation of the acrylic polymer, n-butyl acrylate, 4-acryloylmorpholine, acrylic acid, and 4-hydroxybutyl acrylate were used in amounts of 77.4 parts by mass, 19.4 parts by mass, 2.9 parts by mass, and 0.3 parts by mass, respectively. The rest of the procedure was the same as in Example 2.

[0103] [Comparative Example 2] Comparative Example 2 differs from Example 2 in that in the preparation of the acrylic polymer, n-butyl acrylate, 4-acryloylmorpholine, acrylic acid, and 4-hydroxybutyl acrylate were used in amounts of 92.0 parts by mass, 4.8 parts by mass, 2.9 parts by mass, and 0.3 parts by mass, respectively. The rest of the procedure was the same as in Example 2.

[0104] The following evaluations were carried out for the optical laminates of Examples 1 to 7 and Comparative Examples 1 and 2. The evaluation results are shown in Table 1.

[0105] <Evaluation of creep deformation rate> An adhesive layer laminate (1 mm thick) was prepared as follows. Examples 1 and 5-7: Four adhesive sheets (fifth laminates) having a laminated structure of PET film / adhesive composition layer (thickness 10 μm) / PET film were prepared in the same manner as the above adhesive sheet (first laminate), except that the thickness of the adhesive composition layer was 10 μm, with a width of 20 cm and a length of 30 cm. Then, each of the fifth laminates was irradiated with ultraviolet light to cure the ultraviolet curable resin of the adhesive composition layer, thereby obtaining an adhesive sheet (sixth laminate) having a laminated structure of PET film / adhesive layer (thickness 10 μm) / PET film. By repeating the process of laminating the adhesive layers of the obtained adhesive sheet (sixth laminate) in multiple layers and the process of dividing the adhesive layer laminate into multiple test pieces (cutting out multiple test pieces), a laminate of adhesive layers (thickness 1 mm, size 4 cm × 6 cm) in which a total of 100 adhesive layers (thickness 10 μm) were laminated was obtained. The ultraviolet light irradiation to the fifth laminate was performed using an LED lamp (manufactured by Quark Technology Co., Ltd., peak illuminance: 200 mW / cm 2 , cumulative light intensity 1500mJ / cm 2 (wavelength 345-365 nm) was used, and the UV illuminance was measured using a UV Power Puck (manufactured by Fusion UV Systems Japan, Inc.). Examples 2 to 4 and Comparative Examples 1 and 2: Four adhesive sheets (sixth laminates) having a laminated structure of PET film / adhesive layer (thickness 10 μm) / PET film were produced in the same manner as the above adhesive sheet (first laminate), except that the thickness of the adhesive layer was 10 μm. The process of laminating the adhesive layers of the obtained adhesive sheet (sixth laminate) in multiple layers and the process of dividing the adhesive layer laminate into multiple test pieces (cutting out multiple test pieces) were repeated to obtain an adhesive layer laminate (thickness 1 mm, size 4 cm × 6 cm) in which a total of 100 adhesive layers (thickness 10 μm) were laminated.

[0106] A cylinder with a diameter of 8 mm (height of 1 mm) was punched out from the laminate (thickness of 1 mm) of the adhesive layer obtained as described above to prepare a test specimen. A stress of 10,000 Pa was applied to the test specimen for 30 minutes at a measurement temperature of 50°C using a viscoelasticity measuring device (device name "ARES G-2", manufactured by TA Instruments Japan Co., Ltd.), and the deformation rate was measured after 1 second and 30 minutes.

[0107] In this specification, the "creep deformation rate" of the adhesive layer is the "creep deformation rate" obtained by the above method using a laminate (thickness 1 mm) of the adhesive layer. According to the experiment by the present inventor, the creep deformation rate of a laminate having a thickness of 1 mm was not significantly different between a laminate formed by laminating 20 adhesive layers having a thickness of 50 μm, a laminate formed by laminating 100 adhesive layers having a thickness of 10 μm, and a laminate formed by laminating 200 adhesive layers having a thickness of 5 μm. That is, the creep deformation rate of a laminate having a thickness of 1 mm does not depend on the thickness of the adhesive layers, as long as the thickness of each adhesive layer constituting the laminate is at least in the range of 5 μm to 50 μm. According to the study by the present inventor, if the thickness of each adhesive layer is 0.1 μm or more, the creep deformation rate of a laminate having a thickness of 1 mm is considered to be almost constant.

[0108] <180° peel adhesion to polymethyl methacrylate (PMMA)> For Examples 2 to 4 and Comparative Examples 1 and 2, one of the release-treated PET films was peeled off from the obtained adhesive sheet (first laminate), and the exposed surface of the adhesive layer was bonded to a 25 μm thick polyethylene terephthalate (PET) film (product name "Lumirror S-10", manufactured by Toray Industries, Inc.) to obtain a test specimen.

[0109] The test piece was cut to a width of 20 mm, the other release-treated PET film was peeled off, and the exposed surface of the adhesive layer was attached to a polymethyl methacrylate (PMMA) plate (thickness 2 mm, product name "Acrylite", manufactured by Mitsubishi Chemical Corporation) to prepare a test piece, and the adhesive strength (mN / 20 mm) to the PMMA plate was measured. The pressure bonding when attaching to the PMMA plate was performed by rolling a 2 kg roller back and forth once, and 30 minutes after bonding, the 180° peel adhesive strength was measured using a tension and compression tester (device name "AGS-50NX", manufactured by Shimadzu Corporation) under the following conditions. Peeling speed: 300mm / min Measurement conditions: Temperature: 23±2℃, Humidity: 65±5%RH

[0110] For Examples 1 and 5 to 7, test specimens were prepared in the same manner as in Examples 2 to 4 and Comparative Examples 1 and 2 using the adhesive sheet (first laminate), and after bonding with a PMMA plate (i.e., after obtaining a laminate of PET film (Lumirror S-10) / adhesive composition layer / PMMA plate), the test specimens were prepared by irradiating ultraviolet light from the PET film side. The ultraviolet light irradiation was performed using an LED lamp (manufactured by Quark Technology Co., Ltd., peak illuminance: 200 mW / cm 2 , cumulative light intensity 1500mJ / cm 2 (wavelength 345-365 nm) was used, and the UV illuminance was measured using a UV Power Puck (manufactured by Fusion UV Systems Japan, Inc.).

[0111] <Haze evaluation> An adhesive layer laminate (thickness 80 μm) was prepared as follows. Examples 1 and 5-7: In the same manner as in the above <Evaluation of creep deformation rate>, an adhesive sheet (sixth laminate) having a laminated structure of PET film / adhesive layer (thickness 10 μm) / PET film was produced in a size of 20 cm width and 30 cm length. Eight test pieces were cut out from the obtained adhesive sheet (sixth laminate), and eight adhesive layers (thickness 10 μm) were laminated to obtain an adhesive layer laminate (thickness 80 μm). Examples 2 to 4 and Comparative Examples 1 and 2: Using the same method as in the above <Evaluation of creep deformation rate>, an adhesive sheet (sixth laminate) having a laminated structure of PET film / adhesive layer (thickness 10 μm) / PET film was produced with a size of 20 cm width and 30 cm length. Eight test pieces were cut out from the obtained adhesive sheet (sixth laminate), and eight adhesive layers (thickness 10 μm) were laminated to obtain an adhesive layer laminate (thickness 80 μm).

[0112] A laminate having a laminated structure of PET film / adhesive layer laminate (thickness 80 μm) / PET film was obtained by bonding the adhesive layer laminate (thickness 80 μm) with a PET film that had been subjected to a silicone release treatment. One separator (PET film) was peeled off from the laminate having a laminated structure of PET film / adhesive layer laminate (thickness 80 μm) / PET film, and the adhesive layer laminate was bonded to a glass plate (trade name "EAGLE XG", Corning, thickness 0.7 mm), and the other separator was peeled off to prepare a test piece having a laminated structure of adhesive layer laminate / glass plate. The haze of the test piece was measured with a haze meter (device name "HZ-1", Suga Test Instruments Co., Ltd.) under D65 light.

[0113] In this specification, the "haze" of the adhesive layer refers to the "haze" determined by the above method using a laminate (thickness 80 μm) of the adhesive layer. The haze of the 80 μm-thick laminate does not depend on the thickness of each adhesive layer constituting the laminate.

[0114] <Evaluation of diffuse transmittance> The acrylic resin film of the optical laminate of each Example or Comparative Example was set in a haze meter (device name "HZ-1", manufactured by Suga Test Instruments Co., Ltd.) so that it faced the light source, and the diffuse transmittance was measured using D65 light. The diffuse transmittance was measured immediately after lamination (within 5 minutes) (referred to as "Diffuse transmittance (immediately)" in Table 1) and 10 days after lamination (storage at temperature: 23±2°C, humidity: 65±5% RH) (referred to as "Diffuse transmittance (after 10 days)" in Table 1). The obtained diffuse transmittance was judged according to the following criteria. Diffuse transmittance immediately after lamination (within 5 minutes) ◎: 96% or more ○: 95% or more but less than 96% △: 94% or more but less than 95% ×: Less than 94% Diffuse transmittance 10 days after lamination ◎: 90% or more ○: 85% or more but less than 90% △: 84% or more but less than 85% ×: Less than 84%

[0115] [Table 1]

[0116] The optical laminates of Examples 1 to 7 all had a diffuse transmittance of 95% or more immediately after lamination (within 5 minutes), and a diffuse transmittance of 85% or more 10 days after lamination. In contrast, the optical laminates of Comparative Examples 1 and 2 had a diffuse transmittance of less than 95% immediately after lamination (within 5 minutes), and a diffuse transmittance of less than 85% 10 days after lamination. From these results, it can be said that the adhesive layers of Examples 1 to 7 are suppressed from penetrating into the recesses of the optical sheet when the adhesive layer is bonded to the optical sheet, and are suppressed from changing over time in the degree of penetration of the adhesive layer into the recesses.

[0117] For the optical laminates of Examples 5a, 6a and 7a using a concave-convex film having a plurality of recesses on the surface as the optical sheet, 10 days after the optical sheet and the adhesive composition layer were bonded together, the cross sections of the optical laminates of Examples 5a, 6a and 7a (cross sections including the cross section of FIG. 7B of the concave-convex film 70) were observed at a magnification of 1500 times using an optical microscope (Nikon Solutions Co., Ltd., ECLIPSE LV100). For all of Examples 5a, 6a and 7a, it was confirmed from the observation images that the adhesive layer did not substantially penetrate into the recesses 74 of the concave-convex film 70, and it was confirmed that the change over time in the degree of penetration of the adhesive layer into the recesses was suppressed.

[0118] The adhesive layers of the optical laminates of Examples 1 to 7 all have a creep deformation rate after 1 second (creep deformation rate A) of 10% or less, and a creep deformation rate after 30 minutes (creep deformation rate B) of 16% or less. In contrast, the adhesive layers of the optical laminates of Comparative Examples 1 and 2 have a creep deformation rate A of more than 10% or a creep deformation rate B of more than 16%. It can be said that the creep deformation rate of the adhesive layer has a certain correlation with the diffuse transmittance of the optical laminate. From the results of Examples 1 to 7, it can be seen that from the viewpoint of suppressing the penetration of the adhesive layer into the recesses of the optical sheet when the adhesive layer is bonded to the optical sheet and the change over time in the degree of penetration of the adhesive layer into the recesses, an adhesive layer having a creep deformation rate after 1 second (creep deformation rate A) of 10% or less and a creep deformation rate after 30 minutes (creep deformation rate B) of 16% or less is preferable.

[0119] Example 2 and Comparative Examples 1 and 2 differ only in the mass ratio of n-butyl acrylate (BA) and 4-acryloylmorpholine (ACMO) in the preparation of the (meth)acrylic polymer. In Example 2, BA:ACMO=70:30, in Comparative Example 1, BA:ACMO=80:20, and in Comparative Example 2, BA:ACMO=95:5. The ratio of the ACMO-derived component to the entire adhesive is 29.0 mass% in Example 2, 19.4 mass% in Comparative Example 1, and 4.8 mass% in Comparative Example 2. However, this is not limited to this example, and as can be seen from, for example, Example 3, the (meth)acrylic polymer may be prepared without using a nitrogen-containing (meth)acrylic monomer. The adhesives of Examples 1 and 5 to 7 further contain a cured product of an ultraviolet-curable resin in addition to a component derived from a nitrogen-containing (meth)acrylic monomer having a nitrogen-containing cyclic structure (Example 1: 31.4 mass% of the entire adhesive, Examples 5 to 7: 16.7 mass% of the entire adhesive). When the cured product of the ultraviolet curable resin is further included, the preferred ratio of the nitrogen-containing (meth)acrylic monomer having a nitrogen-containing cyclic structure may change. Furthermore, as in Example 4, it is understood that an adhesive containing a polyester polymer instead of a (meth)acrylic polymer can be used. [Industrial Applicability]

[0120] The optical laminate of the present invention is widely used in optical devices such as display devices and lighting devices. [Explanation of symbols]

[0121] 10a, 10b First optical sheet 12s, 18s main surface (front) 20a, 20b adhesive layer 30 Second optical sheet 32s, 38s main surface (front) 50 Light guide plate 60 light source 100A, 100B, 101A, 101B, 102B Optical laminate 200 Lighting Equipment

Claims

1. A first optical sheet having a first main surface having a concave-convex structure and a second main surface opposite the first main surface; an adhesive layer disposed on the first main surface side of the first optical sheet; having the concave-convex structure includes a plurality of concave portions, and a surface of the adhesive layer and the first main surface of the first optical sheet define a plurality of spaces in the plurality of concave portions; The uneven structure includes a flat portion in contact with the adhesive layer, the adhesive layer has a creep deformation rate of 10% or less when a stress of 10,000 Pa is applied to it at 50° C. for 1 second in a creep test using a rotational rheometer, and a creep deformation rate of 16% or less when a stress of 10,000 Pa is applied to it at 50° C. for 30 minutes; The adhesive layer has a 180° peel adhesive strength to a PMMA film of 10 mN / 20 mm or more, The adhesive layer does not include a graft polymer, The adhesive layer comprises at least one of the following polymers (1) or (2): (1) A (meth)acrylic polymer of a nitrogen-containing (meth)acrylic monomer having a nitrogen-containing cyclic structure and at least one other monomer; (2) Polyester-based polymers.

2. An optical laminate as described in claim 1, wherein the haze of the adhesive layer is 0.01% or more and 5% or less.

3. An optical laminate as described in claim 1 or 2, wherein the thickness of the adhesive layer is 0.1 μm or more and 20 μm or less.

4. An optical laminate described in any one of claims 1 to 3, wherein the adhesive layer further contains a copolymer of a carboxyl group-containing acrylic monomer and at least one other monomer (excluding a nitrogen-containing (meth)acrylic monomer).

5. An optical laminate described in any one of claims 1 to 4, wherein the adhesive layer contains a polyester-based polymer.

6. An optical laminate described in any one of claims 1 to 5, wherein the adhesive layer contains the (meth)acrylic polymer.

7. The optical laminate according to claim 6 , wherein the (meth)acrylic polymer is crosslinked.

8. An optical laminate as described in claim 6 or 7, wherein the adhesive layer further contains a cured product of an active energy ray-curable resin.

9. The optical laminate described in claim 8, wherein the adhesive layer is formed by curing the active energy ray curable resin of an adhesive composition layer containing the (meth)acrylic polymer, the active energy ray curable resin, and a polymerization initiator.

10. The adhesive layer of any one of claims 1 to 8, A substrate having a release-treated main surface; having A laminate, in which the release-treated main surface of the substrate is bonded to the adhesive layer.

11. The adhesive composition layer forming the adhesive layer of the optical laminate according to claim 9; A substrate having a release-treated main surface; having A laminate, in which the release-treated main surface of the substrate is attached to the adhesive composition layer.

12. A method for producing the optical laminate according to claim 1 , comprising the step of bonding the first optical sheet and the adhesive layer together.

13. The method of claim 12 , wherein the process is performed in a roll-to-roll process.

14. The optical laminate according to claim 1 , further comprising a second optical sheet arranged on the side of the adhesive layer opposite to the first optical sheet side.

15. A method for producing the optical laminate according to claim 14, A step A1 of bonding a first laminate in which the first optical sheet and the adhesive layer are laminated to the second optical sheet; or A process A2 of bonding the first optical sheet to a second laminate in which the adhesive layer and the second optical sheet are laminated. A manufacturing method comprising either one of the steps of:

16. The method includes the step A1, and the step A1 includes a step of bonding the first laminate and the second optical sheet by a roll-to-roll method, or The manufacturing method according to claim 15 , further comprising the step A2, wherein the step A2 includes a step of bonding the second laminate and the first optical sheet by a roll-to-roll method.

17. An optical device comprising the optical laminate according to any one of claims 1 to 9 and 14.

18. A method for producing the optical laminate according to claim 9, A step A of applying the adhesive composition layer onto the first main surface of the first optical sheet; a step B of curing the active energy ray curable resin of the adhesive composition layer in a state in which the adhesive composition layer is applied onto the first main surface of the first optical sheet; A manufacturing method comprising:

19. The method according to claim 18 , wherein the step A includes a step of bonding the first optical sheet and the adhesive composition layer by a roll-to-roll method.

20. A method for producing an optical laminate according to claim 14, which recites claim 9, A step A1 of bonding a first laminate in which the first optical sheet and the adhesive composition layer are laminated to the second optical sheet; or A process A2 of bonding the first optical sheet to a second laminate in which the adhesive composition layer and the second optical sheet are laminated. Either one of the following: a step B of curing the active energy ray curable resin contained in the adhesive composition layer after the step A1 or the step A2; A manufacturing method comprising:

21. The method includes the step A1, and the step A1 includes a step of bonding the first laminate and the second optical sheet by a roll-to-roll method, or The manufacturing method according to claim 20 , further comprising the step A2, wherein the step A2 includes a step of bonding the second laminate and the first optical sheet by a roll-to-roll method.

Citation Information

Patent Citations

  • Method and apparatus for culturing animal cell

    JP1981058490A

  • Radiation-curing pressure-sensitive adhesive sheet

    JP2005112966A

  • Adhesive sheet and liquid crystal display

    JP2011026361A

  • Optical sheet with adhesive layer, method for producing optical sheet with adhesive layer, light source using optical sheet with adhesive layer, and image display device using optical sheet with adhesive layer

    JP2011215601A

  • Optical laminated sheet, method of manufacturing optical laminated sheet, light source with optical laminated sheet, and image display device with optical laminated sheet

    JP2012007046A