Non-oriented electrical steel sheet and its manufacturing method

By optimizing composition and hot rolling conditions to control impurity precipitation and grain size uniformity, the invention addresses 'reverse skid marks' in non-oriented electrical steel sheets, achieving stable magnetic properties and reduced energy loss.

JP7557123B2Active Publication Date: 2024-09-27NIPPON STEEL CORPORATION
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020018935
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-02-06
Publication Date
2024-09-27
Estimated Expiration
2040-02-06

AI Technical Summary

Technical Problem

Non-oriented electrical steel sheets exhibit variations in magnetic properties along the coil length due to 'reverse skid marks', which are caused by non-uniform precipitation of impurities during hot rolling, leading to inconsistent iron loss characteristics.

Method used

Optimizing the composition and hot rolling conditions of non-oriented electrical steel sheets by reducing impurities like C, N, S, and Mn, controlling the precipitation behavior of MnS, and maintaining uniform grain size across the coil thickness, achieved through specific temperature and cooling rate controls during hot rolling and annealing.

Benefits of technology

Stabilizes magnetic properties and minimizes energy loss by ensuring uniform grain size and precipitation across the coil, thereby meeting the requirements for consistent magnetic performance and productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557123000004
    Figure 0007557123000004
  • Figure 0007557123000009
    Figure 0007557123000009
  • Figure 0007557123000008
    Figure 0007557123000008
Patent Text Reader

Abstract

To provide a non-oriented electromagnetic steel sheet capable of resolving the variation "skid mark" of magnetic properties in the longitudinal direction to improve the entire magnetic properties, and a method for manufacturing the same.SOLUTION: A non-oriented electromagnetic steel sheet includes, by mass%, C:0.005% or less, Si:2.0-3.5%, Al:0.3-1.0%, Mn:0.20% or less, S:0.0020% or less, N:0.0030% or less and the remainder consisting of Fe and inevitable impurities. When setting a plate thickness to t and setting a smaller circle equivalent average particle size to GS1 and a larger one to GS2 in a circle equivalent average particle size on a rolling direction cross section in a region at a 1 / 4t position in the plate thickness direction from one surface and a circle equivalent average particle size on a rolling direction cross section in a region at a 3 / 4t position in the plate thickness direction from the one surface, a circle equivalent average particle size ratio R=GS2 / GS1 is 1.5 or less.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a non-oriented electrical steel sheet that is free from in-coil magnetic property variations caused by hot rolling, and a manufacturing method thereof. [Background technology]

[0002] Non-oriented electrical steel sheets are widely used mainly as iron core materials for rotating equipment. In particular, in response to recent demands for energy conservation, stable and good magnetic properties, productivity, and even cost reduction are required. In addition, the demand for non-oriented electrical steel sheets is rapidly increasing due to the increase in consumption in the transportation equipment field and the rapid progress of electrification in developing countries.

[0003] Since electrical steel sheets are used in electrical equipment, their magnetic properties are important. In particular, non-oriented electrical steel sheets have good iron loss properties (low iron loss values), so high-grade non-oriented electrical steel sheets with good iron loss properties have traditionally contained the second largest amount of Al after Si.

[0004] In recent years, in high-grade non-oriented electrical steel sheets, the "addition of more Al" has come to be considered not only for the purpose of rendering C, N, S, etc. harmless, but also, like Si, for the purpose of improving resistivity and for the effect of improving costs and characteristics (cost performance).

[0005] The magnetic properties of non-oriented electrical steel sheets are developed through a process that begins with adjusting the composition during steelmaking, followed by hot rolling, hot-rolled sheet annealing, cold rolling, and final annealing. Final annealing is basically performed in a dry atmosphere using a mixture of nitrogen and hydrogen gas, with the annealing temperature and time changed continuously. At this time, the magnetic properties can vary significantly along the length of the coil, especially in high-grade steel.

[0006] This phenomenon is known to be caused by differences in temperature history during slab heating and soaking in hot rolling. In hot rolling, a "skid" is present in the heating furnace to hold the slab, and attempts are made to heat the slab uniformly. This skid is cooled with water and is in contact with the slab, so its temperature must be low. Temperature deviations at this slab heating stage can affect the properties of the product due to precipitation in subsequent processes. The variation in properties caused by this temperature deviation is called a "skid mark."

[0007] In non-oriented electrical steel sheets, generally, the iron loss performance is superior in the areas near the skid pipes where the temperature is relatively low, and inferior in the areas between the skid pipes where the temperature is high, as shown in Table 1. This is called a skid mark.

[0008] Patent Document 1 discloses a technology that enables stable production of non-oriented electrical steel sheets without simply adding large amounts of alloying elements such as Si and Al, and that enables the slab heating temperature to be raised to a high level to eliminate skid marks that become evident due to the influence of Ti that is inevitably mixed in by increasing the purity of the steel. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 5-140649 Summary of the Invention [Problem to be solved by the invention]

[0010] However, in the case of non-oriented electrical steel sheets, the reverse phenomenon can also occur, where the magnetic properties of the parts corresponding to the skids are poor and the magnetic properties of the parts corresponding to the gaps between the skids are good. This is called "reverse skid marks."

[0011] [Table 1]

[0012] There has been a demand for a solution to these exact opposite phenomena. However, because these exact opposite phenomena exist, there are no appropriate measures within a wide range of manufacturing conditions, and the magnetic properties have not been sufficiently improved.

[0013] Therefore, an object of the present invention is to provide a non-oriented electrical steel sheet and a manufacturing method thereof in which the crystal grain size in the coil thickness direction of the non-oriented electrical steel sheet is made uniform, this state is realized over the entire length of the coil, and fluctuations in magnetic properties in the longitudinal direction, known as "skid marks," are eliminated, resulting in good overall magnetic properties. [Means for solving the problem]

[0014] As a result of intensive research, the present inventors have found that the "reverse skid mark" can be dramatically improved by hot rolling in a range outside the conventional hot rolling conditions for non-oriented electrical steel sheets and optimizing the composition of the steel sheet. The present invention was made based on the above findings and through further research, and the gist of the present invention is as follows.

[0015] (1) A non-oriented electrical steel sheet containing, by mass%, C: 0.005% or less, Si: 2.0 to 3.5%, Al: 0.3 to 1.0%, Mn: 0.20% or less, S: 0.0020% or less, N: 0.0030% or less, with the balance being Fe and unavoidable impurities, characterized in that, when the sheet thickness is t, the smaller of the circle-equivalent average grain diameter in a rolling direction cross section in a region located at 1 / 4t in the sheet thickness direction from one surface and the circle-equivalent average grain diameter in a rolling direction cross section in a region located at 3 / 4t in the sheet thickness direction from the said surface is designated as GS1 and the larger of the circle-equivalent average grain diameters in the rolling direction cross section in a region located at 3 / 4t in the sheet thickness direction from the said surface is designated as GS2, and the circle-equivalent average grain diameter ratio R = GS2 / GS1 is 1.5 or less.

[0016] (2) A method for producing the non-oriented electrical steel sheet according to (1) above, comprising the steps of: heating a steel slab having the chemical composition according to (1) above; hot-rolling the heated steel slab, coiling it, and hot-rolling it. rolled steel a hot rolling step for obtaining a strip; rolled steela hot rolled steel strip annealing step of annealing a strip to obtain an annealed hot rolled steel strip, a cold rolling step of cold rolling the annealed hot rolled steel strip to obtain a cold rolled steel strip, and a finish annealing step of finish annealing the cold rolled steel strip to obtain a non-oriented electrical steel sheet, wherein in the slab heating step, the average cross-sectional temperature of the slab on the skid is 1150°C or higher, and in the hot rolling step, the average cooling rate of the coldest part of the slab located on the skid after the slab is removed from a heating furnace until the finish rolling start temperature is 1.0°C / sec or lower, and the finish rolling start temperature is 950°C or higher.

[0017] (3) The method for producing a non-oriented electrical steel sheet according to (2), wherein in the hot-rolled steel strip annealing step, the hot-rolled steel strip is continuously annealed at a temperature of 950°C or higher and 1000°C or lower for 30 seconds or more. Effect of the Invention

[0018] By applying this technology, the properties of non-oriented electrical steel sheets become highly stable, fluctuations in the magnetic properties of rotating equipment are minimized, and energy loss is dramatically reduced. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a diagram showing the concept of conventional purity. [Diagram 2] FIG. 2 is a diagram showing the concept of the present invention in the case of high purity steel. [Diagram 3] FIG. 1 is a diagram showing the temperature history and precipitation curve of a coil. [Figure 4] FIG. 1 is a diagram showing the iron loss of the entire coil measured by a continuous iron loss measuring device during final annealing. [Diagram 5] 1A and 1B are diagrams showing examples of cross-sectional structures of the final product corresponding to a conventional hot rolling technique and a skid according to the present invention, where (a) is by the conventional hot rolling technique and (b) is by the present invention. [Figure 6] FIG. 1 is a graph showing the relationship between the circle-equivalent average grain size ratio R and the relative iron loss value. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] As a result of extensive research, the inventors have found that the "reverse skid mark" phenomenon can be dramatically improved by optimizing the region and composition outside the conventional hot rolling conditions. The present invention proposes a method for reducing this phenomenon.

[0021] The occurrence of skid marks in a heating furnace during hot rolling is believed to be due to the following reasons.

[0022] Melted and continuously cast slabs contain unavoidable impurities such as C, N, S, and Ti. These impurities form compounds with Mn, Al, etc. The dissolution and precipitation of these compounds, AlN, MnS, Ti-(N,C), BN, Nb-(C,N), and Zr-(C,N), are functions of temperature. In other words, above a certain temperature, they form a solid solution.

[0023] These impurities have two effects on the properties of non-oriented electrical steel sheet. One is grain growth, and the other is hysteresis loss, which is one type of iron loss. This phenomenon depends mainly on the impurity content and the slab heating time and temperature. In this way, impurities not only hinder grain boundary migration, but also cause an increase in hysteresis loss, which is one type of iron loss. For this reason, there has been a demand and pursuit to reduce impurities as much as possible. The inventors of the present invention have reached a solution after extensive research.

[0024] The details are given below.

[0025] First, non-oriented electrical steel sheets are mainly used for rotating equipment, so the crystal orientation is along the rolled surface. <100> It is required to have a primary recrystallized structure consisting of randomly oriented, uniform grains not exceeding 200 μm throughout the coil.

[0026] When the scale is small, such as in the research stage, the evaluation of the properties of non-oriented electrical steel sheets is not affected by variations in the material parts such as coils, and uniformity is maintained. However, with the recent increase in mass production and production scale that contributes to improving productivity, the manufacturing units are becoming larger. Specifically, the unit weight of slabs and coils is becoming larger, and as a result, the non-uniformity within the coils inevitably becomes more noticeable. A typical example of the cause of this is the occurrence of skid marks.

[0027] As mentioned above, the non-uniformity in the coil was previously thought to be due to non-uniform grain growth caused by non-uniform thermal history along the length of the coil. However, it has been discovered recently that this non-uniformity along the length is also due to non-uniformity along the thickness direction, i.e., non-uniformity in the two-dimensional magnetic properties of the thin steel sheet.

[0028] The main feature of the present invention is that the precipitation behavior of MnS and the like is synchronized with the cooling during hot rolling. For this reason, it is important to reduce the amount of MnS that precipitates and reduce the cooling dependency of the precipitation. Although the temperature history of the coil does not change much from the previous one, the rolling is performed by threading through the gaps in the precipitation curve.

[0029] The precipitation phenomena that affect the grain growth during the final annealing of non-oriented electrical steel sheets are mainly divided into two categories: (X) the initial state during slab heating and soaking, and (Y) the dynamic behavior during hot rolling.

[0030] (X) In the initial state of slab heating and soaking, the temperature is low on the skids and high between the skids. Depending on this temperature and the amount of precipitate-forming elements, the precipitation state will be as follows.

[0031] The temperature range of the skid section and the dissolution and precipitation of precipitates are in a thermodynamic relationship, and the dissolution curve roughly draws a quadratic function if both compounds are linear mutual terms, and the dissolution curve becomes horizontal because there is no amount of precipitation above the dissolution temperature corresponding to the content. This limit point changes depending on the content. As before, if there were a lot of precipitate elements, they would already precipitate due to equilibrium conditions in the heating furnace. In other words, they precipitate in the low temperature area, and in the high temperature area, they precipitate finely from a solid solution state during hot rolling.

[0032] In contrast, in the case of high purity steel as in the present invention, the precipitation state in the heating furnace is almost the same on and between skids, and during hot rolling, precipitation is delayed in the high temperature area (between skids), and the low temperature area is close to the precipitation nose, so it becomes fine and inhibits grain growth during final annealing. In such a case, a reverse skid type state occurs.

[0033] The present invention does not merely reduce the amount of impurity elements, but also controls the hot rolling conditions of (Y) to realize an intermediate state between the reverse skid type and the forward skid type.

[0034] As shown in FIG. 1, in the forward skid type, the high temperature portion is in solid solution, and due to the high temperature during hot rolling, precipitates such as MnS are finely precipitated.

[0035] In addition, in the case of high purity steel, the amount of solid solution in the initial state does not differ in the precipitation state (solid solution state) in the temperature range of the skid section, but if the hot rolling conditions are not controlled, the precipitates will precipitate later in the high temperature section during hot rolling, resulting in a non-uniform precipitation state.

[0036] Although the temperatures on the skids and between the skids are the same, comparing Figures 1 and 2, as the purity of the steel plate components increases (Figure 2), the temperature of point A (solid solubility limit) thermodynamically decreases.

[0037] Comparing Figure 1 and Figure 2, the area to the right of point A (high temperature region) expands due to high purification, and this expansion is utilized to cause uniform precipitation. However, if left in this state, uniform fine precipitation will occur, so active precipitation is performed by hot-rolled sheet annealing to make the entire area harmless.

[0038] The temperature history and precipitation curve of the coil are shown in Figure 3. The solid line in Figure 3 represents the prior art, and the dashed line represents the present invention. The arrows represent the overall length of the coil.

[0039] As shown in Figure 3, in the reverse skid type (Y), in the dynamic behavior during hot rolling, in the case of high purity steel, when heated, the precipitation state is almost the same in both the high temperature and low temperature areas. When a slab in this state is hot rolled, the start of precipitation is delayed and the precipitation rate is slower than when the slab contains a large amount of impurity elements as described below, and the width of the precipitation curve is wider. By performing hot rolling in the gaps, the precipitation behavior becomes uniform. The solid line is steel containing a large amount of impurity elements. Also, the dashed lines are on the low temperature side, the long time side, and the intervals are wider.

[0040] In the present invention, the amount of Mn and S is small, so the start of MnS precipitation is delayed, the interval between the isoprecipitation curves is widened, and the entire length of the coil is placed between them, realizing uniform precipitation. In the conventional condition, the amount of Mn and S is high, so the start of MnS precipitation is early, and the interval is widened, resulting in non-uniform precipitation.

[0041] <Circle equivalent average particle size ratio R> Figure 4 shows a chart of iron loss measured over the entire coil length using a continuous iron loss measuring device during final annealing.

[0042] An example of the nonuniformity of crystal grains in the thickness direction in the cross section at the (1) position in Figure 4 is shown in Figure 5(a). The top side of the page corresponds to the top surface of the slab when it is heated in the hot rolling furnace, and the rolling direction is from left to right on the page. The sheet thickness is 0.5 mm. It was found that the grain size changes almost continuously in the thickness direction from the bottom surface to the top surface when the slab is heated. To quantify this, the smaller circle-equivalent average grain size in the rolling direction cross section at the 1 / 4t position and the 3 / 4t position (1 / 4t position from the other surface) of the total sheet thickness from one side of the steel sheet is defined as GS1, and the larger circle-equivalent average grain size ratio RGS2 / GS1 is defined. When GS1=GS2, R=1. Incidentally, non-oriented electrical steel sheets are coiled and uncoiled in many processes after hot rolling (coiling, uncoiling), so the top and bottom surfaces are switched when the slab is heated. For this reason, in the present invention, "one side" and "the other side" are relativized.

[0043] As a result of the study by the inventors, it was found that if the circle equivalent average particle diameter ratio R is ≦ 1.5, reverse skid marks do not occur. Normally, this R is estimated to be a small value (more uniform), but in reality, 1.5 is the boundary. This is considered as follows.

[0044] In high-grade non-oriented electrical steel sheets, the grain size in the final product is relatively large, exceeding 100 μm. As a result, the grain shape changes from polyhedral to polyhedral. In the case of polyhedral grains (large grains), there is a large deviation from a sphere. For this reason, in the case of large grains, the grain size is overestimated as a representative value indicating the grain size. In other words, the above circle-equivalent average grain size ratio R≦1.5 is estimated to be smaller than 1.5 in an ideal three-dimensional grain size evaluation. Figure 5(b) shows an example of a cross-sectional structure corresponding to a skid of the final product obtained by the present invention.

[0045] The relationship between the circle-equivalent average grain size ratio R and the relative iron loss value (W15 / 50 ratio) is shown in Figure 6. The relative iron loss value (W15 / 50 ratio) is calculated by dividing the maximum iron loss value by the minimum iron loss value in the longitudinal direction of the steel plate.

[0046] FIG. 6 shows the results of the circle equivalent average grain size ratio R and the relative iron loss value for the case of non-oriented electrical steel sheet produced to obtain 50A290 according to JIS C 2552 by heating and soaking a non-oriented electrical steel sheet slab containing Si=2.6%, Mn=0.20%, Al=0.45%, C=0.0015%, S=0.00018%, N=0.0015%, Ti=0.0019%, and the balance being unavoidable impurities, at 1050-1180°C for 350-400 minutes using a method according to the conventional technology.

[0047] The characteristics are good in the area where the circle equivalent average particle diameter ratio R is small, but when the circle equivalent average particle diameter ratio R exceeds 1.5, the iron loss deteriorates significantly and W15 / 50 does not meet the 2.9W / kg. This is the result obtained from various parts of the coil where reverse skid marks occurred, and as shown here, the best point is 2.4W / kg, but the worst point is 3.2W / kg, and a deterioration of the iron loss fluctuation of 30% or more is recognized, which deviates from the 50A290 standard.

[0048] <Component composition> The composition of the components will be described below. In the following, % means % by mass.

[0049] Si: 2.00~3.50% Silicon: 2.00 to 3.50%. Silicon is an element that increases resistivity and contributes to improving iron loss characteristics. If it is less than 2.00%, γ-α transformation occurs during hot rolling, and forward skid marks may occur instead of reverse skid marks. If it is more than 3.50%, breaks occur frequently during the manufacturing process, especially during rolling, making commercial production impossible.

[0050] Al: 0.30-1.00% Al is also added to ensure resistivity. If the Al content exceeds 1.00%, roll wear in various rolling mills occurs significantly, hindering production. If the Al content is below 0.30%, the effect of improving iron loss is small.

[0051] Mn: 0.20% or less Mn combines with S to exist as MnS, which deteriorates magnetic properties, so a small amount is preferred, but achieving low Mn content will increase costs. With regard to the main purpose of controlling the morphology of MnS, a small amount will delay the precipitation of MnS and reduce fluctuations in the precipitation state of MnS in hot-rolled steel strips.

[0052] S: 0.0020% or less Reducing the S content is the backbone of this technology, and it must be 0.0020% or less. If it is more than this, skid marks will occur (forward, not backward). As with Mn, a lower S content will delay the precipitation of MnS in terms of morphology control, and reduce fluctuations in the precipitation state of MnS in hot-rolled steel strips.

[0053] C: 0.0050% or less As inevitable impurities, C, N, Ti, etc. are well known elements that form precipitates. Although it is better to have less of these elements that form precipitates, it is necessary to consider the cost.

[0054] If C is not below 0.0050%, magnetic aging will occur, which will be fatal to the quality, so it should be below 0.0050%. Of course, this value is not a regulation at the steelmaking stage, but a regulation value for the final product, non-oriented electrical steel sheet. It is more preferable to have it below 0.0030%.

[0055] N: 0.0030% or less N not only hinders grain boundary migration but also causes an increase in hysteresis loss among iron losses, so the content must be small. Since the non-oriented electrical steel sheet of the present invention contains a large amount of Al, N precipitates by forming AlN, and the N content may be 0.0030% or less. Furthermore, compared to MnS, the precipitation of AlN during hot rolling is slower, so its effect in the present invention is extremely weak.

[0056] Other elements that are inevitably contained in the final steel sheet are Se, Nb, and Cu. 、 These include P, Sn, Sb, and B. The amount of unavoidable elements should be kept small, preferably 0.005% or less. 。S N, Sb, and P are up to about 0.05% 、 Also, B teeth, In the high-grade non-oriented electrical steel sheet of the present invention, its addition is not preferred, and the content is preferably 0.0010% or less.

[0057] <Manufacturing method> This is the core process of this technology, and compared to previous technologies, its distinctive feature is that high-purity non-oriented electrical steel sheet slabs are heated at low temperatures and then hot-rolled at high temperatures.

[0058] The idea of ​​the present invention is to realize a uniform state of impurities that have a large effect on the grain growth of non-oriented electrical steel sheets, and in particular, in the case of the present technology, it is suitable for coils with a thickness of 1.6 to 2.8 mm, a width of 1000 mm to 1300 mm, and a length of about 2000 m, and to realize a uniform state of unavoidable impurities of Mn-S(-Cu) compounds over the entire length of the coil. To achieve this, the precipitation curve during hot rolling and the cooling conditions of the coil must be aligned.

[0059] To achieve this, first, the S content is reduced as described above, and then the hot rolling heating temperature is lowered to promote the precipitation of MnS as much as possible, and the decrease in the hot rolling temperature is slowed as much as possible.

[0060] <Slab heating> (Average temperature of slab section on skid ≧ 1150℃ If the average cross-sectional temperature of the slab on the skid is less than 1150°C, even high purity steel such as that of the present invention will approach the nose of the precipitation curve shown in Figure 3 during hot rolling and cause non-uniform precipitation across it. For this reason, the average cross-sectional temperature of the slab on the skid is set to 1150°C or higher. The cross-sectional temperature of the slab on the skid can be obtained from the measured values ​​of parts that can be measured with a radiation thermometer and from heat transfer calculations.

[0061] <Hot rolling> (Average cooling rate of the coldest part of the slab ≦1.0℃ / sec) If the average cooling rate of the coldest part of the slab exceeds 1.0°C / sec, non-uniform precipitation will occur approaching and crossing the nose of the precipitation curve shown in Figure 3 during hot rolling, as in the case of slab heating, even in high purity steel such as that of the present invention. For this reason, the average cooling rate of the coldest part of the slab is set to 1.0°C / sec or less. Here, the "coldest part of the slab" corresponds to the part of the slab located on the skid in the heating furnace.

[0062] (Finish rolling start temperature TF0≧950℃) If the finish rolling start temperature TF0 is less than 950°C, similar to the slab heating and cooling rate of the coldest part of the slab, non-uniform precipitation will occur during hot rolling, approaching and crossing the nose of the precipitation curve shown in Figure 3, even in high purity steel such as that of the present invention. For this reason, the finish rolling start temperature TF0 is set to 950°C or higher.

[0063] The idea behind achieving this high-temperature hot rolling is the opposite of the conventional hot rolling conditions for non-oriented electrical steel sheets.

[0064] <Hot-rolled sheet annealing> In this technology, it is preferable to perform hot-rolled sheet annealing between the hot rolling and the final cold rolling. This heat treatment is also effective in controlling precipitates. This is to cause recrystallization of the pre-cold rolling structure and to cause MnS precipitation more completely. The former recrystallization is to improve and secure the magnetic properties, and the latter is to obtain a complete precipitation state of the remaining MnS. The temperature is preferably 950℃ to 1000℃. If it is lower than this, the recrystallization in the pre-cold rolling structure is insufficient and the magnetic properties are inferior. Also, if it is high, the recrystallization is sufficient, but the MnS re-solidifies and causes reverse skid marks. The above effects can be obtained if the time is 30 seconds or more. It is possible to exceed 60 seconds, but productivity is poor.

[0065] <Product thickness> In actual production, the minimum product thickness is 0.18 mm. It is possible to produce products thinner than 0.18 mm, but if the roll diameter is large, it is not possible to roll satisfactorily while meeting the thickness precision (thickness variation of 5% or less). As the absolute value of iron loss of the grain-oriented electrical steel sheet increases with thickness, the upper limit of 0.50 mm according to the Japanese Industrial Standards is set. EXAMPLES

[0066] The present invention is a technology to prevent non-uniformity in the magnetic properties of non-oriented electrical steel sheets in the coil length direction. Since the absolute value of the magnetic properties depends on the components, etc., in this embodiment, the evaluation was done not by the absolute iron loss value but by the fluctuation value (circle-equivalent average grain size ratio R).

[0067] A non-oriented electrical steel sheet slab having the composition shown in Table 2 was hot-rolled under the conditions shown in Table 3 to obtain a hot-rolled sheet having a thickness of 2.0 mm. The hot-rolled sheet was annealed under the conditions shown in Table 3, pickled, and then cold-rolled steel sheet having a thickness of 0.5 mm was obtained. Then, a final annealing was performed at 975 to 1050°C for about 60 seconds. After that, the circle-equivalent average grain size was obtained at the 1 / 4t position and the 3 / 4t position in the thickness direction of the steel sheet, and the circle-equivalent average grain size ratio R was obtained. In addition, the maximum and minimum values ​​of the iron loss in the length direction of the steel sheet were obtained, and a relative iron loss value of 1.03 or less was considered to be acceptable.

[0068] By applying the present invention in this manner, the variation in grain size over the entire length of the coil is greatly reduced, resulting in a uniform product.

[0069] [Table 2]

[0070] [Table 3] [Industrial Applicability]

[0071] The present invention realizes uniformity of the properties of non-oriented electrical steel sheets. In general, non-oriented electrical steel sheets are produced in coil form, and the larger the size, the better the productivity. For example, thickness (0.35 mm, 0.50 mm, etc.) x width (about 1200 mm) x length (over 5000 m). With the conventional technology, within this length of over 5000 m, there was a fluctuation in magnetic properties due to temperature deviation caused by skids in the hot rolling heating furnace. Furthermore, the grading (certification of representative values ​​of properties) performed for each coil is performed using the worst value in the coil, so if there is a fluctuation in the coil, the worst value is applied, which results in over-specification or failure to build in the desired product properties, resulting in reduced productivity. Application of the present technology can greatly contribute to the production of non-oriented electrical steel sheets that do not suffer from such phenomena.

Claims

1. In mass percent, C: 0.005% or less, Si: 2.0 to 3.5%, Al: 0.3-1.0%, Mn: 0.20% or less, S: 0.0020% or less, N: 0.0030% or less and the remainder being Fe and unavoidable impurities, When the thickness is t, the smaller of the circle-equivalent average grain diameter in the rolling direction cross section of a region at 1 / 4t in the thickness direction from one surface and the circle-equivalent average grain diameter in the rolling direction cross section of a region at 3 / 4t in the thickness direction from the surface is designated as GS1 and the larger of the circle-equivalent average grain diameters is designated as GS2, and the circle-equivalent average grain diameter ratio R=GS2 / GS1 is 1.5 or less. A non-oriented electrical steel sheet.

2. A non-oriented electrical steel sheet as described in claim 1, characterized in that the iron loss relative value W15 / 50 ratio, calculated by dividing the maximum value of iron loss W15 / 50 in the longitudinal direction of the non-oriented electrical steel sheet by the minimum value, is 1.03 or less.

3. A method for producing the non-oriented electrical steel sheet according to claim 1 or 2, A slab heating step for heating a steel slab having the chemical composition according to claim 1; a hot rolling step of hot rolling the heated steel slab and coiling it to obtain a hot rolled steel strip; A hot-rolled steel strip annealing process in which the hot-rolled steel strip is annealed to obtain an annealed hot-rolled steel strip; A cold rolling step of cold rolling the annealed hot rolled steel strip to obtain a cold rolled steel strip; a finish annealing step of finish annealing the cold rolled steel strip to obtain a non-oriented electrical steel sheet; A method for producing a non-oriented electrical steel sheet comprising: In the slab heating step, the cross-sectional average temperature of the slab on the skid is 1150° C. or more; In the hot rolling process, after the slab is extracted from the heating furnace, the average cooling rate of the coldest part of the slab located on the skid during the period up to the finish rolling start temperature is 1.0 ° C. / sec or less, and the finish rolling start temperature is 950 ° C. or more. A method for producing a non-oriented electrical steel sheet comprising the steps of:

4. The method for producing a non-oriented electrical steel sheet according to claim 3, characterized in that in the hot-rolled steel strip annealing step, the hot-rolled steel strip is continuously annealed at a temperature of 950°C or higher and 1000°C or lower for 30 seconds or longer.

Citation Information

Patent Citations

  • Preparation method for low-iron loss high-magnetic strength non-oriented silicon steel ultra-thin strip

    CN108330397A

  • Nondirectional silicon steel plate with small iron loss

    JP1984074258A

  • Laminated film, manufacture thereof and utility

    JP1992033852A

  • Manufacture of now-oriented silicon steel sheet excellent in magnetic property

    JP1993140649A

  • High-grade non-oriented electromagnetic steel sheet having stable magnetic property, and manufacturing method therefor

    JP2006131963A