Directional electromagnetic steel sheet
By forming linear grooves with controlled surface roughness and geometry on grain-oriented electrical steel sheets, noise reduction is achieved without compromising iron loss, addressing the limitations of existing magnetic domain refining techniques.
Patent Information
- Application Number
- JP2020108705
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-24
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2040-06-24
AI Technical Summary
Grain-oriented electrical steel sheets used as base materials for winding transformers require lower core loss and noise reduction, with existing magnetic domain refining techniques failing to achieve sufficient noise reduction effects.
The formation of linear grooves on the steel sheet surface with controlled surface roughness and groove geometry, achieved through pickling treatment and laser irradiation, promotes unevenness at the groove bottom surface to enhance domain wall pinning and reduce noise without impairing iron loss reduction.
The solution effectively reduces noise while maintaining iron loss reduction effects by controlling the shape and surface roughness of the grooves, achieving a grain-oriented electrical steel sheet with low noise and low iron loss.
Smart Images

Figure 0007557126000003 
Figure 0007557126000002 
Figure 0007557126000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a grain-oriented electrical steel sheet. [Background technology]
[0002] Grain-oriented electrical steel generally contains 2% to 5% by mass of Si as a steel sheet component, and the grain orientation of the steel sheet is called the Goss orientation, {110} <001> Grain-oriented electrical steel has excellent magnetic properties and is used, for example, as the core material for static inductors in transformers and the like.
[0003] In order to improve the magnetic properties of such grain-oriented electrical steel sheets, various technological developments have been made. In particular, with the recent demand for energy saving, grain-oriented electrical steel sheets are required to have even lower iron loss. In order to reduce the iron loss of grain-oriented electrical steel sheets, it is effective to increase the concentration of the crystal grains in the Goss orientation of the steel sheet to improve the magnetic flux density and reduce the hysteresis loss.
[0004] Grain-oriented electrical steel sheets used as the base material for wound transformers are required to reduce noise as well as reduce iron loss. In electrical steel sheets, magnetic domain refinement is performed to reduce iron loss, but since winding transformers are annealed to relieve distortion during the manufacturing process, a heat-resistant magnetic domain refinement technology is required to refine the magnetic domains.
[0005] One method for heat-resistant magnetic domain refinement is to form periodic grooves in a steel sheet. For example, Patent Document 1 discloses that the iron loss of the resulting grain-oriented electrical steel sheet is reduced by suppressing the N content in the forsterite coating formed after final annealing to 3.0 mass% or less and performing a magnetic domain refinement process by laser irradiation. It also discloses that the iron loss improvement effect is further improved by suppressing the compositional variation of each forsterite by controlling the Al and Ti contents in the forsterite coating and setting the standard deviation of the forsterite grain size to 1.0 times or less of the average grain size.
[0006] Patent Document 2 describes that by imparting linear scratches with an interval of 5 mm or less, a width of 1 mm or less, and a depth of 0.3 to 5.0 μm in terms of Ra value and 10 μm or less in terms of Rmax value to the surface of a steel sheet before or after decarburization annealing, a grain-oriented electrical steel sheet with extremely excellent iron loss and coating adhesion can be obtained.
[0007] Patent Document 3 describes a grain-oriented electrical steel sheet having a surface on which grooves are formed that extend in a direction intersecting the rolling direction and whose groove depth direction is the sheet thickness direction. The formed grooves have an asymmetric shape in the groove width direction with respect to the groove width center. It is disclosed that an iron loss reduction effect can be obtained by setting the average depth of a groove having such a cross-sectional shape, the arithmetic mean height Ra of a roughness curve that forms the outline of the groove bottom region of the groove, and the average length RSm of the roughness curve elements that form the outline of the groove bottom region within specific ranges.
[0008] Patent Documents 1 to 3 propose various magnetic domain refining techniques for achieving the effect of reducing iron loss when magnetic domain refining is performed, but make no proposal regarding noise reduction. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2012-31512 A [Patent Document 2] Japanese Patent Application Publication No. Hei 1-198429 [Patent Document 3] International Publication No. 2016 / 171130 Summary of the Invention [Problem to be solved by the invention]
[0010] Grain-oriented electrical steel sheets used as the base material for wound transformers are required to reduce noise as well as reduce iron loss. Heat-resistant magnetic domain refinement is generally achieved by forming linear grooves, but at present this does not provide sufficient noise reduction effects. When the surface roughness of the linear grooves formed for magnetic domain refinement is large, the magnetic wall area changes due to magnetic wall movement, and the magnetic wall movement becomes slower due to a larger pinning effect than when there are no grooves. At this time, the magnetic flux leakage is reduced on the groove side surface due to the large surface roughness, and the iron loss reduction effect is greatly reduced. On the other hand, when the surface roughness of the groove bottom surface is large, the reduction in magnetic flux leakage is small, and the impact on the iron loss reduction effect is small.
[0011] In the present invention, a special pickling solution is used to perform pickling before groove formation, which causes the heat transfer coefficient of the precipitates on the steel sheet surface to deviate from the specific heat and heat transfer coefficient of the base steel.Then, the unevenness of the groove bottom surface due to the difference in heat transfer when the grooves are formed by laser irradiation is promoted, and the noise reduction effect is obtained without compromising the iron loss reduction effect.
[0012] The present invention has been made in view of the above problems, and aims to reduce the iron loss of the resulting grain-oriented electrical steel sheet and achieve further noise reduction by controlling the shape of the linear grooves formed for magnetic domain refinement and the Ra value of the surface roughness of the groove bottom and side surfaces within a certain range. [Means for solving the problem]
[0013] The gist of the present invention is that, in terms of mass %, 、S i: 2.50-4.50%, Mn: 0.01-0.15% , C: 0.085% or less, acid-soluble Al: 0.065% or less, N: 0.012% or less, Cr: 0.3% or less, Cu: 0.4% or less, P: 0.5% or less, Sn: 0.3% or less, Sb: 0.3% or less, Ni: 1% or less, S: 0.015% or less, Se: 0.015% or less, Bi: 0.02% or less. and the balance being Fe and impurities, the steel sheet having a steel sheet surface on which linear grooves extending in a direction forming an angle of 0 to 30° with a rolling direction perpendicular thereto are formed at intervals of 1 to 20 mm, the grooves having a depth D of 10 to 50 μm and a groove width W of 20 to 200 μm, and a surface roughness Ra value of the bottom surface of the grooves exceeding 5.0 μm. , 10.0μm or less MnS at the bottom of the groove is not replaced with one or more sulfides selected from the group consisting of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni, AndThe grain-oriented electrical steel sheet is not coated with one or more elements selected from the group consisting of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni, and the surface roughness Ra value of the groove side surface is 0.1 to 5.0 μm. Hereinafter, in this specification, "one or more selected from the group consisting of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni" will be referred to simply as "Cu, etc.", and "one or more sulfides selected from the group consisting of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni" will be referred to simply as "sulfides of Cu, etc.". Effect of the Invention
[0014] According to the present invention, the grooves formed by laser irradiation have uneven bottom surfaces, which increases the pinning effect of the magnetic domain walls while maintaining the effect of reducing iron loss, thereby reducing noise. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a cross-sectional view of a groove in a grain-oriented electrical steel sheet according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Preferred embodiments of the present invention will be described in detail below. Unless otherwise specified, the expression "A to B" for numerical values A and B means "A or more and B or less." In such an expression, when a unit is added only to numerical value B, the unit is also applied to numerical value A.
[0017] [Steel plate composition] First, the chemical composition of the steel sheet used in the grain-oriented electrical steel sheet according to the present invention will be described. In the following, unless otherwise specified, the notation "%" represents "mass%." The balance of the steel sheet other than the elements described below is Fe and impurities.
[0018] The composition of the steel sheet used in the grain-oriented electrical steel sheet of the present invention is {110} <001> It has a favorable composition for controlling the Goss texture accumulated in the orientation. 、S Contains i: 2.50 to 4.50%, Mn: 0.01 to 0.15%.
[0019] (Si: 2.50~4.50%) The content of Si (silicon) is 2.50 to 4.50%. Si increases the electrical resistance of the steel sheet, thereby reducing eddy current loss, which is one of the causes of iron loss. If the content of Si is less than 2.50%, it is not preferable because it becomes difficult to sufficiently suppress the eddy current loss of the final grain-oriented electrical steel sheet. If the content of Si is more than 4.50%, it is not preferable because the workability of the grain-oriented electrical steel sheet decreases. Therefore, the content of Si is 2.50 to 4.50%, and preferably 2.70 to 4.00%.
[0020] (Mn: 0.01 to 0.15%) The content of Mn (manganese) is 0.01 to 0.15%. Mn forms MnS and MnSe, which are inhibitors that affect secondary recrystallization. If the content of Mn is less than 0.01%, the absolute amount of MnS and MnSe that cause secondary recrystallization is insufficient, which is not preferable. If the content of Mn is more than 0.15%, it is not preferable because it becomes difficult to dissolve Mn during slab heating. In addition, if the content of Mn is more than 0.15%, it is not preferable because the precipitate size of MnS and MnSe, which are inhibitors, tends to become coarse, and the optimal size distribution as an inhibitor is impaired. Therefore, the content of Mn is 0.01 to 0.15%, preferably 0.03 to 0.13%.
[0021] The components other than Si and Mn may be the components contained in ordinary grain-oriented electrical steel sheets. For example, the components other than Si and Mn are, by mass%, C :0 .085% or less, acid soluble Al :0 .065% or less, N :0 .012% or less, Cr :0 .3% or less, Cu:0 .4% or less, P :0 .5% or less, Sn :0 .3% or less, Sb :0 .3% or less, Ni :1 % or less, S :0 .015% or less, Se :0 .015% or less, Bi :0 It may contain up to .02%.
[0022] The balance of the steel sheet other than the above-mentioned components is Fe and impurities. Here, the impurity elements refer to components contained in raw materials or components mixed in during the manufacturing process, but not intentionally contained in the steel sheet.
[0023] In order to refine the magnetic domains, grooves are formed on the surface of the steel sheet, which extend in a direction intersecting the rolling direction and whose depth direction is the sheet thickness direction. The grooves need only be provided so as to intersect with the rolling direction, and the groove extension direction does not necessarily have to be perpendicular to the rolling direction, but are provided in a direction that forms an angle of 0 to 30° with the direction perpendicular to the rolling direction. Furthermore, when viewed from the sheet thickness direction (when the grooves are viewed from above), the grooves do not necessarily have to have a linear shape, and may have an arched shape. The groove shape measurement described below is performed after removing the insulating coating from the final product by pickling or the like.
[0024] The grooves are formed on the surface of the steel sheet at intervals of 1 to 20 mm. If the groove interval is less than 1 mm, the magnetic domain refining effect is saturated and the effect of reducing eddy current loss is hardly obtained, while hysteresis loss increases due to distortion, resulting in increased iron loss, which is not preferable. If the groove interval exceeds 20 mm, the magnetic domain refining effect decreases, resulting in insufficient iron loss improvement, which is not preferable. The preferable groove interval is 2 to 10 mm.
[0025] FIG. 1 is a cross-sectional view of a groove in an electrical steel sheet of the present invention. In this figure, the groove is shaped like a trapezoid, but the groove shape may be arched. In one embodiment of the electrical steel sheet of the present invention, the depth D of the groove is in the range of 10 μm to 50 μm. If the depth D is less than 10 μm, the amount of magnetic poles generated from the side surface of the groove is small, and a sufficient iron loss reduction effect cannot be obtained. If the depth D exceeds 50 μm, the magnetic domains are subdivided, but the decrease in magnetic flux density due to the formation of the groove becomes large, and a sufficient iron loss reduction effect cannot be obtained. The preferred depth is 15 μm to 30 μm.
[0026] (Measurement of groove depth D) The method for measuring the "depth D" according to the present invention is as follows. An arbitrary location on the electrical steel sheet was selected, and the maximum depths of two arbitrary grooves (A) and (B) spaced 3 mm apart as shown in the groove cross-section of Figure 1 were measured using a laser microscope (a 3D laser microscope using a pinhole confocal optical system), with the deeper being depth d and the shallower being depth d'. Depth D was the average of these values.
[0027] The "groove width W" in the present invention is the portion indicated by w and w' in FIG. 1. The groove width W is in the range of 20 μm to 200 μm. If the width W is less than 20 μm, the magnetic flux leaking from the groove side enters the opposite groove side, the amount of magnetic pole generated is reduced, and sufficient iron loss reduction effect cannot be obtained. If the width W exceeds 200 μm, the iron loss reduction effect is saturated, and the laser power required to form the groove becomes large, which simply increases the manufacturing cost. The preferred width W is 30 to 100 mm.
[0028] (Measurement of groove width W) The method for measuring the "groove width W" according to the present invention is as follows. An arbitrary location on the electrical steel sheet was selected, and the widths at which the groove depth of two arbitrary points (A) and (B) separated by 3 mm, which are shown in the groove cross-section diagram in Figure 1, are halved were measured using a laser microscope (a 3D laser microscope using a pinhole confocal optical system), with the wider one being w and the narrower one being w'. The groove width W is the average of these values.
[0029] In the present invention, the "surface roughness Ra value of the groove bottom surface and groove side surface" refers to the value of the arithmetic mean height Ra of the roughness curve of the groove bottom surface and groove side surface between two points (A) and (B) in Figure 1. The definition of the arithmetic mean height Ra of the roughness curve is in accordance with Japanese Industrial Standard JIS B 0601 (2013). "Groove bottom surface" refers to the deepest part of the bottom of the groove. "Groove side surface" refers to the side surface part of the groove whose depth is half the maximum groove depth in cross section.
[0030] In the grain-oriented electrical steel sheet of the present invention, Ra of the groove bottom surface is more than 5.0 μm, preferably 6.0 μm or more. The upper limit is 10.0 μm or less, preferably 8.0 μm or less. If Ra is less than 5.0 μm, the noise reduction effect cannot be obtained. If Ra exceeds 10.0 μm, the effect of increasing hysteresis loss becomes large, and a grain-oriented electrical steel sheet with low noise and low iron loss cannot be obtained. In addition, in the grain-oriented electrical steel sheet of the present invention, MnS on the groove bottom surface is not replaced with sulfides such as Cu, and is not coated with Cu, etc. Here, "MnS on the groove bottom surface is not replaced with sulfides such as Cu, and is not coated with Cu, etc." means that the substitution rate of MnS replaced with sulfides such as Cu is 0%, and the coverage rate of MnS covered with Cu, etc. is 0%.
[0031] In the grain-oriented electrical steel sheet of the present invention, the Ra of the groove side surface is 0.1 to 5.0 μm, preferably 0.1 to 3.0 μm, and more preferably 0.1 to 1.0 μm. If Ra is less than 0.1 μm, there is no problem with the magnetic properties, but it is difficult to realize from the viewpoint of manufacturing technology. If Ra exceeds 5.0 μm, the pinning effect of the domain wall becomes large, the hysteresis loss increases, and a sufficient iron loss reduction effect cannot be obtained.
[0032] In the grain-oriented electrical steel sheet of the present invention, MnS at the bottom of the groove is not replaced with sulfides such as Cu, and no coating such as Cu is applied, and the Ra of the bottom of the groove is more than 5.0 μm. , 10.0μm or lessThe reason why low iron loss and low noise can be achieved by setting the surface roughness Ra of the groove side surface within the range of 0.1 to 5.0 μm is believed to be because controlling the surface roughness Ra of the groove side surface provides an iron loss reduction effect, and controlling the surface roughness Ra of the groove bottom surface provides a noise reduction effect.
[0033] (Method for measuring surface roughness Ra of groove bottom and side surfaces) Each Ra was measured using a laser microscope (a 3D laser microscope using a pinhole confocal optical system). An arbitrary location on the electromagnetic steel sheet was selected, and the unevenness of the groove bottom surface of a straight line connecting the maximum depth points d and d' of two groove parts (A) and (B) that are 3 mm apart as shown in the groove cross-sectional view of FIG. 1 was taken as the surface roughness Ra of the groove bottom surface of the present invention. In addition, of the points (d / 2, d' / 2) that are half the maximum depths d and d' of both groove parts, which are on the same side of the maximum depth, the unevenness Ra and Ra' of the groove side surface of a straight line connecting the points (d / 2, d' / 2) on the same side of the maximum depth were derived, and the average value of these values was taken as the Ra of the groove side surface.
[0034] [Method of manufacturing grain-oriented electrical steel sheets] The manufacturing process of the grain-oriented electrical steel sheet of the present invention will be described below by dividing it into a process for obtaining a cold-rolled steel sheet and a subsequent magnetic domain control process.
[0035] [Process from slab to cold-rolled steel sheet] A slab containing, by mass%, at least 2.50% to 4.50% Si, 0.01% to 0.15% Mn, and the balance being Fe and impurities, is hot-rolled to obtain a hot-rolled steel sheet. Next, the hot-rolled steel sheet is pickled to obtain a pickled sheet, or the hot-rolled steel sheet is annealed to obtain a hot-rolled annealed sheet, and then the hot-rolled annealed sheet is pickled to obtain a pickled sheet. The pickling solution used here contains one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni (also referred to as "Cu, etc."), the total concentration of each element is 0.0001 to 0.1000%, and the pH is -1 to 5. The temperature of the pickling solution is 15°C to 100°C, and the steel sheet is immersed in the pickling solution for 5 to 200 seconds. A pickled sheet is obtained by this pickling process, and the pickled sheet is cold-rolled to obtain a cold-rolled steel sheet.
[0036] [Slab composition] The components of the slab used in the production of the grain-oriented electrical steel sheet according to the present invention contain at least Si: 2.50 to 4.50%, and Mn: 0.01 to 0.15%.
[0037] The Si (silicon) content is 2.5 to 4.5%. Si increases the electrical resistance of the steel sheet, thereby reducing eddy current loss, which is one of the causes of iron loss. If the Si content is less than 2.5%, it is not preferable because it becomes difficult to sufficiently suppress the eddy current loss of the final grain-oriented electrical steel sheet. If the Si content exceeds 4.5%, it is not preferable because the workability of the grain-oriented electrical steel sheet decreases. Therefore, the Si content is 2.5% to 4.5%, and preferably 2.7 to 4.0%.
[0038] The content of Mn (manganese) is 0.01 to 0.15%. Mn forms MnS and MnSe, which are inhibitors that affect secondary recrystallization. If the content of Mn is less than 0.01%, the absolute amount of MnS and MnSe that cause secondary recrystallization is insufficient, which is not preferable. If the content of Mn is more than 0.15%, it is not preferable because it becomes difficult to dissolve Mn during slab heating. In addition, if the content of Mn is more than 0.15%, it is not preferable because the precipitate size of MnS and MnSe, which are inhibitors, tends to become coarse, and the optimal size distribution as an inhibitor is impaired. Therefore, the content of Mn is 0.01 to 0.15%, preferably 0.03 to 0.13%.
[0039] The components other than Si and Mn can be the following components: For example, the components other than Si and Mn are, by mass%, C: 0.020-0.100%, S and Se: 0.001-0.050%, acid-soluble Al: 0.010-0.050%, N: 0.002-0.015%, Cr: 0.020-0.100%, S and Se: 0.001-0.050%, Cr: 0.020-0.015 ... :0 .300% or less, Cu :0 .400% or less, P :0 .500% or less, Sn :0 .300% or less, Sb :0 .300% or less, Ni :1 .000% or less, S :0 .015% or less, Se :0 .015% or less, Bi :0 It may contain up to .020%.
[0040] The C (carbon) content is 0.02 to 0.10%. C has various roles, but if the C content is less than 0.02%, the grain size becomes excessively large when the slab is heated, which increases the iron loss value of the final grain-oriented electrical steel sheet, which is not preferable. If the C content exceeds 0.10%, the decarburization time becomes long during decarburization after cold rolling, which increases the manufacturing cost, which is not preferable. Also, if the C content exceeds 0.10%, decarburization is likely to be incomplete, which is not preferable because it may cause magnetic aging in the final grain-oriented electrical steel sheet. Therefore, the C content is 0.02 to 0.10%, and preferably 0.05 to 0.09%.
[0041] The total content of S (sulfur) and Se (selenium) is 0.001 to 0.050%. S and Se form an inhibitor together with the above-mentioned Mn. Both S and Se may be contained in the slab, but at least one of them should be contained in the slab. If the total content of S and Se is outside the above range, it is not preferable because a sufficient inhibitor effect cannot be obtained. Therefore, the total content of S and Se is 0.001 to 0.050%, preferably 0.001 to 0.040%.
[0042] The content of acid-soluble Al (acid-soluble aluminum) is 0.01 to 0.05%. Acid-soluble Al constitutes an inhibitor necessary for producing a grain-oriented electrical steel sheet with high magnetic flux density. If the content of acid-soluble Al is less than 0.01%, the amount of acid-soluble Al is insufficient, and the inhibitor strength is insufficient, which is not preferable. If the content of acid-soluble Al is more than 0.05%, the AlN precipitated as an inhibitor becomes coarse, which is not preferable, and therefore the inhibitor strength is reduced. Therefore, the content of acid-soluble Al is 0.01 to 0.05%, and preferably 0.01 to 0.04%.
[0043] The N (nitrogen) content is 0.002 to 0.015%. N forms AlN, which is an inhibitor, together with the above-mentioned acid-soluble Al. If the N content is outside the above range, it is not preferable because a sufficient inhibitor effect cannot be obtained. Therefore, the N content is 0.002 to 0.015%, and preferably 0.002 to 0.012%.
[0044] In addition, in order to improve magnetic properties, the slab used in the manufacture of the grain-oriented electrical steel sheet according to the present embodiment may contain, in mass%, one or more selected from the group consisting of Cu: 0.4% or less, P: 0.5% or less, Sn: 0.3% or less, Sb: 0.3% or less, Ni: 1.0% or less, S: 0.015% or less, Se: 0.015% or less, and Bi: 0.02% or less, in place of a portion of the remaining Fe, in addition to the above-mentioned elements. In the slab according to one embodiment, the Cr content may be 0.02% or more, the Bi content may be 0.0005% or more, the Sb content may be 0.005% or more, the Se content may be 0.001% or more, and the Mo content may be 0.005% or more, in mass%.
[0045] A slab is formed by casting molten steel adjusted to the above-described composition. The method for casting the slab is not particularly limited. In research and development, even if a steel ingot is formed in a vacuum melting furnace or the like, the same effects as when a slab is formed can be confirmed for the above-described components.
[0046] [Process to make hot-rolled steel sheet] The cast slab is heated at a predetermined temperature, and the heated slab is hot-rolled to be processed into a hot-rolled steel sheet. The thickness of the hot-rolled steel sheet after processing may be, for example, 1.8 mm to 3.5 mm. If the thickness of the hot-rolled steel sheet is less than 1.8 mm, the temperature of the steel sheet after hot rolling becomes low, and the amount of AlN precipitated in the steel sheet increases, making secondary recrystallization unstable, and the magnetic properties of the grain-oriented electrical steel sheet having a final thickness of 0.23 mm or less are degraded, which is not preferable. If the thickness of the hot-rolled steel sheet is more than 3.5 mm, the rolling load in the cold rolling process becomes large, which is not preferable.
[0047] [Annealing process] After performing normal hot-rolled sheet annealing to obtain a hot-rolled annealed sheet, the hot-rolled annealed sheet is subjected to a cold rolling process.
[0048] [Process to make cold-rolled steel sheet] After the hot-rolled steel sheet is pickled, it is processed into cold-rolled steel sheet by rolling it in one cold rolling process or multiple cold rolling processes with intermediate annealing in between. In addition, the steel sheet may be heat-treated at about 300°C or less between passes of cold rolling, between rolling roll stands, or during rolling. In such a case, the magnetic properties of the final grain-oriented electrical steel sheet can be improved. The hot-rolled steel sheet may be rolled by three or more cold rolling passes, but since multiple cold rolling passes increase the manufacturing cost, it is preferable to roll the hot-rolled steel sheet by one or two cold rolling passes. When cold rolling is performed by reverse rolling such as a Sendzimir mill, the number of passes in each cold rolling pass is not particularly limited, but is preferably 9 passes or less from the viewpoint of manufacturing cost. The steps from the slab to obtaining a cold-rolled steel sheet have been described above.
[0049] Next, decarburization annealing is performed. The cold-rolled steel sheet is subjected to heat treatment (i.e., decarburization annealing) under a predetermined temperature condition (for example, heating at 700 to 900°C for 1 to 3 minutes). When the decarburization annealing is performed, the carbon in the cold-rolled steel sheet is reduced to a predetermined amount or less, and a primary recrystallization structure is formed. In addition, in the decarburization annealing, an oxide layer containing silica (SiO2) as a main component is formed on the surface of the cold-rolled steel sheet.
[0050] Next, an annealing separator is applied. In this process, an annealing separator containing magnesia (MgO) as a main component is applied to the surface of the cold-rolled steel sheet (the surface of the oxide layer). Next, the cold-rolled steel sheet coated with the annealing separator is subjected to heat treatment (i.e., finish annealing) under a predetermined temperature condition (for example, heating at 1100 to 1300°C for 20 to 24 hours). When the finish annealing is performed, secondary recrystallization occurs in the cold-rolled steel sheet, and the cold-rolled steel sheet is purified. As a result, a cold-rolled steel sheet is obtained that has the above-mentioned chemical composition of the steel sheet and whose crystal orientation is controlled so that the magnetization easy axis of the crystal grains coincides with the rolling direction X.
[0051] Furthermore, when the above-mentioned final annealing treatment is performed, the oxide layer containing silica as a main component reacts with the annealing separator containing magnesia as a main component to form a glass film containing composite oxides such as forsterite (Mg2SiO4) on the surface of the steel sheet. In the final annealing process, the final annealing treatment is performed with the steel sheet wound in a coil shape. The formation of a glass film on the surface of the steel sheet during the final annealing treatment can prevent the occurrence of seizure on the coiled steel sheet.
[0052] [Pickling process] Subsequently, the finish annealed sheet is subjected to pickling.
[0053] The pickling solution contains one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni, the total concentration of each element is 0.0001 to 0.1000%, and the pH is -1 to 5. The temperature of the pickling solution is 15°C to 100°C, and the steel sheet is immersed in the pickling solution for 5 to 200 seconds.
[0054] If the total concentration of one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni in the pickling solution is less than 0.0001%, the inhibitor control effect in the thickness direction is insufficient, which is not preferable. If the total concentration of one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni in the pickling solution is more than 0.1000%, the effect of improving magnetic properties is saturated, and the cost of the pickling solution increases, which is not preferable. Therefore, the total concentration of one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni in the pickling solution is 0.0001 to 0.1000%.
[0055] If the pH of the pickling solution is less than -1, the acidity becomes too strong and the handling of the pickling solution becomes difficult, which is not preferable. If the pH of the pickling solution is more than 5, the inhibitor control effect in the thickness direction by the pickling process becomes insufficient, which is not preferable. Therefore, the pH of the pickling solution is -1 or more and 5 or less.
[0056] If the temperature of the pickling solution is less than 15°C, the inhibitor control effect in the thickness direction by the pickling treatment becomes insufficient, which is not preferable. If the temperature of the pickling solution is more than 100°C, the handling of the pickling solution becomes difficult, which is not preferable. Therefore, the temperature of the pickling solution is 15°C or more and 100°C or less.
[0057] When the time for which the steel sheet is immersed in the pickling solution in the pickling treatment is less than 5 seconds, the effect of inhibitor control in the sheet thickness direction by the pickling treatment becomes insufficient, which is not preferable. When the time for which the steel sheet is immersed in the pickling solution in the pickling treatment exceeds 200 seconds, the equipment becomes long and large, which is not preferable. Therefore, the time for which the steel sheet is immersed in the pickling solution in the pickling treatment is 5 seconds or more and 200 seconds or less.
[0058] When the finish annealed sheet is pickled under the above-mentioned conditions, the MnS precipitates in the steel are replaced by sulfides such as Cu in the steel sheet surface layer, or are coated with Cu, etc., so that the heat transfer coefficient of the steel sheet surface layer containing the precipitates becomes constant. Here, "replacement" refers to the Mn portion of the originally formed MnS being replaced by Cu, etc. derived from the pickling solution, and MnS is replaced with sulfides such as Cu, and "coated" refers to the newly precipitated Cu, etc. derived from the pickling solution, around the originally formed MnS. Since such a phenomenon in the present invention is not affected by the precipitation method of Cu, etc., either the substitution with sulfides such as Cu or the coating with Cu, etc. may occur during the pickling treatment. This allows the heat propagation effect of laser irradiation, etc. to be constant on the steel sheet surface layer. Under the above-mentioned conditions, only the heat transfer coefficient of the surface layer is uniformed by pickling, so that the Ra of the groove side surface close to the surface layer is reduced. In contrast, the Mn portion of MnS, which is a precipitate near the bottom of the groove away from the surface, is not replaced by metal during pickling, nor is it coated. Therefore, the heat transfer coefficient is not uniformed, and the Ra of the bottom of the groove is not reduced compared to the side of the groove. Therefore, MnS is not sufficiently replaced by sulfides such as Cu during pickling. Also If the steel sheet is not coated with Cu or the like, the heat transfer coefficient of the steel sheet surface varies greatly, and the Ra of both the groove bottom and side surfaces increases. On the other hand, even if the pickling time or the pickling solution concentration is set to a certain level, the effect of stabilizing the heat transfer coefficient saturates, and the effect of stabilizing the heat transfer coefficient in the depth direction is not obtained, there is no further reduction in the groove side Ra, and the Ra of the groove bottom does not change. In addition, the pickling conditions here change depending on the depth of the groove to be formed. The deeper the groove to be formed, the longer the pickling time, the higher the concentration of the pickling solution, or the lower the pH, to obtain better iron loss characteristics.
[0059] [Process for forming linear grooves on the steel plate surface] In the subsequent laser irradiation process, a laser is irradiated onto the surface (one side only) of the steel plate on which the glass coating has been formed, to form a plurality of grooves on the surface of the steel plate extending in a direction intersecting the rolling direction at intervals of 1 to 20 mm along the rolling direction.
[0060] In the laser irradiation step, a laser irradiation device rotates a polygon mirror to irradiate a laser beam onto the surface of the steel sheet, and scans the laser beam in a direction forming an angle of 0 to 30° with the rolling direction.
[0061] Simultaneously with the irradiation of the laser light, an assist gas such as air or an inert gas is sprayed onto the portion of the steel sheet to be irradiated with the laser light. The inert gas is, for example, nitrogen or argon. The assist gas plays a role in removing the components melted or evaporated from the steel sheet by the laser irradiation. By spraying the assist gas, the laser light reaches the steel sheet without being hindered by the melted or evaporated components, so that the grooves are stably formed.
[0062] As the laser light source, for example, a high-power laser generally used for industrial purposes, such as a fiber laser, a YAG laser, a semiconductor laser, or a CO2 laser, can be used. In addition, a pulsed laser or a continuous wave laser may be used as the laser light source as long as it can stably form a groove. As the laser light, it is preferable to use a single mode laser that has high light-collecting ability and is suitable for forming a groove.
[0063] As the conditions for the laser light irradiation, for example, it is preferable to set the laser output to 200 W to 3000 W, the laser light focusing spot diameter in the rolling direction (i.e., the diameter including 86% of the laser output, hereinafter abbreviated as 86% diameter) to 10 μm to 200 μm, the laser light focusing spot diameter in the sheet width direction (86% diameter) to 10 μm to 1000 μm, and the laser scanning speed to 5 m / s to 50 m / s. These laser irradiation conditions are appropriately adjusted so that a groove depth D of 10 to 50 μm is obtained.
[0064] In the final insulating film forming step, an insulating coating liquid containing, for example, colloidal silica and phosphate is applied from above the glass film to the steel sheet surface on which the grooves have been formed by the above-mentioned laser irradiation. Then, a heat treatment is carried out under a predetermined temperature condition (for example, 840 to 920°C), thereby finally obtaining a grain-oriented electrical steel sheet having the grooves, glass film, and insulating film according to the present invention.
[0065] For the groove shape formed in the obtained grain-oriented electrical steel sheet, the groove depth D, groove width W and surface roughness Ra of the groove bottom surface and groove side surface were measured using the measurement method described above. EXAMPLES
[0066] The grain-oriented electrical steel sheet of the present invention will be described in more detail below with reference to examples. Note that the examples shown below are merely examples of the grain-oriented electrical steel sheet according to the present embodiment, and the grain-oriented electrical steel sheet according to the present embodiment is not limited to the examples shown below.
[0067] A slab having a chemical composition containing, in mass fractions, 3.0% Si, 0.08% C, 0.05% acid-soluble Al, 0.01% N, 0.12% Mn, 0.05% Cr, 0.04% Cu, 0.01% P, 0.02% Sn, 0.01% Sb, 0.005% Ni, 0.007% S, 0.001% Se, with the remainder being Fe and impurities, was hot rolled to obtain a hot-rolled steel sheet having a thickness of 2.3 mm.
[0068] Next, the above hot-rolled steel sheets were subjected to an annealing treatment under temperature conditions of heating at 1000° C. for 1 minute. After the annealing treatment, cold rolling was performed to obtain a cold-rolled steel sheet having a thickness of 0.23 mm. Subsequently, the cold-rolled steel sheet was subjected to a decarburization annealing treatment under the temperature condition of heating at 800°C for 2 minutes, and then an annealing separator containing magnesia (MgO) as a main component was applied to the surface of the cold-rolled steel sheet.
[0069] Next, the cold-rolled steel sheet coated with the annealing separator was subjected to a final annealing treatment under the temperature condition of heating at 1200°C for 20 hours. As a result, a steel sheet was obtained that had the above-mentioned chemical composition, had a crystal orientation controlled so that the magnetization easy axis of the crystal grains coincided with the rolling direction, and had a glass film formed on the surface.
[0070] The surface of the finish annealed sheet was pickled using the pickling solution and conditions shown in Table 1. 。
[0071] Table 1 shows the components, concentration, pH value, and immersion time of the pickling solution used. [Table 1]
[0072] Next, the surface of the steel sheet was irradiated with a laser to form a plurality of grooves extending in a direction intersecting the rolling direction on the surface of the steel sheet at predetermined intervals along the rolling direction.
[0073] The laser light irradiation conditions were adjusted so that the desired groove depth D was obtained: laser output in the range of 200 W to 3000 W, the focused spot diameter (86% diameter) of the laser light in the rolling direction in the range of 10 μm to 500 μm, the focused spot diameter (86% diameter) of the laser light in the plate width direction in the range of 10 μm to 1000 μm, the laser scanning speed in the range of 5 m / s to 50 m / s, and the laser scanning pitch (spacing PL) in the range of 1 mm to 20 mm.
[0074] As described above, an insulating coating liquid containing colloidal silica and phosphate was applied to the steel sheet having grooves formed therein on top of the glass film, and then the steel sheet was heat-treated under temperature conditions of heating at 850°C for 1 minute, ultimately obtaining a grain-oriented electrical steel sheet having grooves formed therein, a glass film, and an insulating film.
[0075] As a comparative example, the results of pickling using a pickling solution outside the scope of the present invention are shown.
[0076] The groove shape thus formed was measured for groove depth D, groove width W, and surface roughness Ra of the groove bottom and side surfaces using the measurement method described above. For noise measurements, samples of 100 mm width x 500 mm length are taken from each grain-oriented electrical steel sheet. The length direction of the sample corresponds to the rolling direction RD, and the width direction corresponds to the sheet width direction TD. The magnetostriction of the sample is measured by an AC magnetostriction measurement method using a magnetostriction measurement device that includes a laser Doppler vibrometer, an excitation coil, an excitation power supply, a magnetic flux detection coil, an amplifier, and an oscilloscope. Specifically, an AC magnetic field is applied to the sample so that the maximum magnetic flux density is 1.7 T in the rolling direction and the frequency is 50 Hz. The change in length of the sample due to expansion and contraction of the magnetic domains is measured with a laser Doppler vibrometer to obtain a magnetostriction signal. The obtained magnetostriction signal is subjected to Fourier analysis to determine the amplitude Cn of each frequency component fn (n is a natural number equal to or greater than 1) of the magnetostriction signal. The noise characteristic (dB) is calculated using the A correction coefficient αn of each frequency component fn, as shown in the following equation. Noise characteristic = 20 × Log (√ (Σ (ρc × 2π × fn × αn × Cn / √2) 2) / Pe0) Here, ρc is the specific acoustic resistance, and ρc = 400. Pe0 is the minimum audible sound pressure, and Pe0 = 2 × 10-5 (Pa) is used. The A correction coefficient αn uses the value listed in Table 2 of JIS C 1509-1 (2005). Σ is 10 points in 100 Hz increments from 100 to 1000 Hz. The pickling conditions, iron loss W17 / 50 and noise (dB) are shown in Table 2 along with the measurement results.
[0077] In addition, SEM-EDS measurements were performed on the cross section of the grooves to perform element mapping, and if the mappings of Mn and S did not overlap, it was assumed that MnS did not exist, but was replaced by sulfides such as CuS, or was coated with Cu, etc., and the presence or absence of an effect of stabilizing heat transfer on the side and bottom of the grooves was evaluated. In the table, a circle indicates that there was an effect of stabilizing heat transfer, and a cross indicates that there was no effect of stabilizing heat transfer.
[0078] [Table 2]
[0079] From these results, it can be seen that by carrying out the pickling treatment of the embodiment (invention example), the surface roughness Ra value of the groove bottom surface and groove side surface was controlled within a certain range, and iron loss and noise were further reduced compared to the comparative example.
Claims
[Claim 1] In mass percent, Si: 2.50-4.50%, Mn: 0.01 to 0.15%, C: 0.085% or less, Acid-soluble Al: 0.065% or less, N: 0.012% or less, Cr: 0.3% or less, Cu: 0.4% or less, P: 0.5% or less, Sn: 0.3% or less, Sb: 0.3% or less, Ni: 1% or less, S: 0.015% or less, Se: 0.015% or less, Bi: 0.02% or less and the balance being Fe and impurities, and linear grooves extending in a direction perpendicular to the rolling direction and forming an angle of 0 to 30° thereon are formed at intervals of 1 to 20 mm on a steel sheet surface, The depth D of the groove is 10 to 50 μm, The groove width W is 20 to 200 μm, The surface roughness Ra value of the bottom surface of the groove is more than 5.0 μm and 10.0 μm or less, MnS on the bottom surface of the groove is not replaced with one or more sulfides selected from the group consisting of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni, and the bottom surface of the groove is not coated with one or more sulfides selected from the group consisting of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni, and The grain-oriented electrical steel sheet has a surface roughness Ra value of the groove side surface of 0.1 to 5.0 μm.
Citation Information
Patent Citations
Production of grain oriented electrical steel sheet having extremely good iron loss characteristic and film adhesiveness
JP1989198429A
Method for producing low core loss grain oriented silicon steel sheet
JP2007169762A
Grain-oriented electromagnetic steel sheet and production method thereof
JP2012031512A
Wound iron core
JP2019024039A
Grain-oriented electromagnetic steel sheet, wound iron core, method for manufacturing grain-oriented electromagnetic steel sheet, and method for manufacturing wound iron core
JP2019135323A