Modified hollow particles and method for producing same
Modified hollow particles with a dense outer shell address the strength and dispersibility issues of conventional hollow particles, resulting in coatings with enhanced hardness, strength, and transparency for antireflection films.
Patent Information
- Application Number
- JP2020202046
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-04
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2040-12-04
AI Technical Summary
Hollow particles used in antireflection films suffer from reduced strength and hardness due to their lower refractive index, leading to issues like particle aggregation, difficulty in redispersing, and decreased scratch resistance, especially when nano-sized.
Development of modified hollow particles with a dense outer shell containing inorganic oxide, achieved by coating and firing hollow particles with an inorganic compound, followed by removal of the coated compound to enhance dispersibility and maintain particle integrity.
The modified hollow particles provide a coating with high hardness, strength, and excellent adhesion to substrates, while maintaining low reflectance and transparency, addressing the limitations of conventional hollow particles.
Smart Images

Figure 0007557354000004 
Figure 0007557354000003 
Figure 0007557354000001
Abstract
Description
[Technical field]
[0001] The present invention relates to hollow particles having a dense outer shell and a method for producing the same. [Background technology]
[0002] Conventionally, in order to prevent reflection on the surface of a substrate such as a sheet or lens made of glass or plastic, an anti-reflection film is formed on the surface. For example, a coating film made of a low refractive index material such as fluororesin or magnesium fluoride is formed on the surface of a substrate such as glass or plastic by a coating method, a vapor deposition method, a CVD method, or the like. However, these methods are expensive in terms of cost. Therefore, it is known to form an anti-reflection film by applying a coating liquid containing composite oxide colloidal particles made of silica and an inorganic oxide other than silica and having a refractive index of 1.36 to 1.44 to the surface of the substrate (see, for example, Patent Document 1).
[0003] In addition, methods for producing porous hollow particles are known (see, for example, Patent Documents 2 and 3). Hollow particles have a lower refractive index than solid particles, and a transparent coating formed using hollow particles has a low refractive index and excellent antireflection performance.
[0004] However, once a particle dispersion is dried, it undergoes secondary aggregation. It is difficult to redisperse the aggregated particles in a solvent, resin, or the like in the form of primary particles. This problem becomes more pronounced in particles with smaller particle diameters, such as nano-sized particles. In order to improve redispersibility, it is known to treat the surface of the particles with a polymer such as polyacrylic acid or polyvinylpyrrolidone, and a surfactant (see, for example, Patent Document 4), or to incorporate polysilsesquioxane into the particles (see, for example, Patent Document 5). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-133105 [Patent Document 2] JP 2001-233611 A [Patent Document 3] JP 2013-226539 A [Patent Document 4] JP 2004-043892 A [Patent Document 5] JP 2014-185051 A Summary of the Invention [Problem to be solved by the invention]
[0006] Hollow particles have a cavity inside the shell, so they have a lower refractive index than solid particles, but their strength is low. Therefore, when they are used in an anti-reflective film, the anti-reflective performance is improved, but the hardness and strength (scratch resistance) of the film may decrease. Therefore, it is necessary to densify the particles (shell) to achieve sufficient hardness and strength. For example, the particles may be sintered to achieve this densification.
[0007] However, as described above, the hollow particle dispersion may cause the particles to aggregate simply by drying. In addition, even if the hollow particles are treated as in Patent Document 4 or Patent Document 5, the particles will aggregate when baked (for example, at 300° C. or higher), making it difficult to redisperse them in a solvent or the like. If there are many aggregated particles, they cannot be monodispersed in the coating solution and the coating, and the coating cannot be flattened. This causes a decrease in the scratch resistance of the coating and an increase in haze. In order to redisperse the aggregated particles, it is possible to mechanically disperse them using a bead mill or the like, but there is a risk that the particles will be destroyed and the original shape of the hollow particles will not be maintained. In addition, if there are many "cracks" in the particles, the uniformity of the particles cannot be obtained unless centrifugation or the like is performed, and there is a risk that the yield will be significantly reduced or the refractive index will increase. Such issues are prominent in nano-sized hollow particles.
[0008] For this reason, there is a demand for hollow particles having a denser particle (outer shell) than conventional hollow particles, and having sufficient hardness and strength.
[0009] Furthermore, the particles are required to have high dispersibility in a solvent or resin.
[0010] Furthermore, a substrate with a transparent coating (anti-reflective coating) using these particles is required to suppress particle aggregation, and to have sufficient hardness and strength, as well as a low refractive index. [Means for solving the problem]
[0011] To solve these problems, we discovered the following "modified hollow particles." These particles have a cavity inside the shell containing inorganic oxide, and the density of the shell is 1.85 × 10 3 kg / m 3 The average primary particle size (D1) is 20 to 1000 nm, and the ratio (D2 / D1) of the average particle size (D2) measured by dynamic light scattering to the average primary particle size (D1) is 1.0 to 1.8.
[0012] The particles have a cavity inside a dense shell containing an inorganic oxide, and have sufficient hardness, strength, and high dispersibility. A coating solution containing such particles can provide a transparent coating film with high hardness (pencil hardness) and high strength (scratch resistance).
[0013] In order to obtain the modified hollow particles, the following production method was found.
[0014] First, a dispersion of hollow particles containing an inorganic oxide in the outer shell is prepared (first step). Next, the hollow particles are coated with an inorganic compound (second step). Next, the hollow particles coated with the inorganic compound are fired at 300 to 1200°C (third step). Next, the fired product of the hollow particles coated with the inorganic compound is suspended in a solvent, and the inorganic compound coating the particles is removed to obtain modified hollow particles (fourth step).
[0015] The density of the shell of the modified hollow particles is 0.10×10 lower than that of the shell of the hollow particles in the first step. 3 kg / m 3 It is higher than that and has a dense outer shell. Effect of the Invention
[0016] The particles of the present invention provide a coating solution capable of producing a coating film having low reflectance, excellent adhesion to a substrate, and high hardness and strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The modified hollow particles according to the present invention have an outer shell containing an inorganic oxide and a cavity inside the outer shell (hereinafter, the modified hollow particles according to the present invention may be simply referred to as "particles"). The average primary particle diameter (D1) of the particles is 20 to 1000 nm. Here, the diameter of a circle (equivalent circle diameter) equivalent to the particle area obtained by image processing of an SEM image is defined as the primary particle diameter. Furthermore, the ratio (D2 / D1) of the average particle diameter (D2) measured by dynamic light scattering to the average primary particle diameter (D1) is in the range of 1.0 to 1.8.
[0018] When the average primary particle diameter (D1) is in the range of 20 to 1000 nm, the particles can exist stably. In addition, the particles have good dispersibility in a coating solution or a coating film, and a coating film having high transparency, hardness, and strength can be obtained. This average diameter (D1) is preferably 20 to 800 nm. In particular, when the particles are used in an anti-reflective film, 20 to 110 nm is preferable.
[0019] The ratio (D2 / D1) of the average particle size (D2) measured by dynamic light scattering to the average primary particle size (D1) in the range of 1.0 to 1.8 indicates that the proportion of aggregated particles is small. Therefore, the particles have high dispersibility in a solvent or matrix forming components. In addition, when used as a coated substrate, high transparency is obtained. If the ratio (D2 / D1) is less than 1.0, it is difficult to obtain the particles. Conversely, if it exceeds 1.8, when this particle is used as a coated substrate, the proportion of aggregated particles increases, and there is a risk of an increase in haze. The ratio (D2 / D1) is preferably 1.0 to 1.6, more preferably 1.0 to 1.4.
[0020] The density of the outer shell is 1.85×103 kg / m 3 That's it. The density is 1.85×10 3 kg / m 3 If the particle is used on a coated substrate, the antireflection performance, strength and pencil hardness of the coating may be insufficient. 3 kg / m 3 More preferably, 2.10×10 3 kg / m 3 That's all.
[0021] The density of the outer shell (ρs) is determined by the refractive index of the outer shell (n S ) is obtained by formula (2). Formula (2) is derived from the Grandstone-Dale formula.
[0022]
number
[0023]
number
[0024] Here, the density of the inorganic oxide in formula (2) (ρ Q ) and refractive index (n Q ) should be a value according to the material that makes up the shell. For example, if the material that makes up the shell is silica (SiO2), then each should be 2.2×10 3 kg / m 3 and 1.46, the density of the outer shell of the particle (ρs) can be calculated. Similarly, for alumina (γ-Al2O3), it is 3.6×10 3 kg / m 3 and 1.70, and 5.7 × 10 for zirconia (ZrO2). 3 kg / m 3 and 2.13, and for titania (anatase type TiO2) it is 5.3 × 10 3 kg / m 3 and 2.52, and for titania (rutile type TiO2) it is 4.2 × 10 3 kg / m 3and 2.72, and 5.6 × 10 for zinc oxide (ZnO). 3 kg / m 3 and 2.1, and 7.0 x 10 for tin oxide (SnO2). 3 kg / m 3 and 2.0, and 3.8×10 for antimony oxide (Sb2O5). 3 kg / m 3 and 1.67, the density (ρs) of the particle's outer shell can be calculated. When the constituent material of the outer shell is a mixture of inorganic oxides or an inorganic composite oxide, the density and refractive index can be calculated according to the constituent components and their ratios. The refractive index in this application means the refractive index at a wavelength of 550 nm.
[0025] Furthermore, the carbon content of the particles is preferably 0.50% by mass or less. The carbon contained in the particles is derived from organic compounds such as organic silicon compounds, metal salts, reducing agents, pH adjusters, cleaning solutions, and solvents. This includes those that are intentionally added for the production of particles, as well as those that are inevitably present in raw materials. If organic compounds are contained, the hardness and strength of the outer shell are weak, so there is a risk that a transparent coating with sufficient hardness and strength cannot be obtained. The carbon content derived from such organic substances can be determined by analyzing the amount of C (carbon) as described later. The carbon content is more preferably 0.30% by mass or less, even more preferably 0.10% by mass or less, and particularly preferably 0.05% by mass or less.
[0026] Furthermore, the particle 29 In the area Q1 of the peak appearing at a chemical shift of -78 to -88 ppm, the area Q2 of the peak appearing at a chemical shift of -88 to -98 ppm, the area Q3 of the peak appearing at a chemical shift of -98 to -108 ppm, and the area Q4 of the peak appearing at a chemical shift of -108 to -117 ppm in the Si-NMR spectroscopy, it is preferable that the ratio ((Q1+Q2) / ΣQ) is 0.05 to 0.50 and the ratio ((Q1+Q2+Q3) / Q4) is 0.05 to 1.00, where ΣQ=Q1+Q2+Q3+Q4.
[0027] The peak assigned to Q1 is due to one (-OSi) group and three (-OH) groups bonded to a Si atom, the peak assigned to Q2 is due to two (-OSi) groups and two (-OH) groups bonded to a Si atom, the peak assigned to Q3 is due to three (-OSi) groups and one (-OH) group bonded to a Si atom, and the peak assigned to Q4 is due to four (-OSi) groups bonded to a Si atom.
[0028] Here, if the ratio ((Q1+Q2) / ΣQ) and the ratio ((Q1+Q2+Q3) / Q4) are within this range, the particles are dense and a transparent coating having sufficient hardness and strength can be obtained, although the detailed reason is unclear. The ratio ((Q1+Q2) / ΣQ) is more preferably 0.08 to 0.50, and even more preferably 0.10 to 0.40. Moreover, the ratio ((Q1+Q2+Q3) / Q4) is more preferably 0.10 to 1.00, and even more preferably 0.20 to 0.90.
[0029] Refractive index of the particle, n a The refractive index is preferably 1.07 to 1.35. When the refractive index is within this range, a transparent coating film can be obtained. The refractive index is more preferably 1.07 to 1.30, and further preferably 1.07 to 1.28.
[0030] Refractive index of the outer shell, n S The refractive index n is preferably 1.36 or more. S If the refractive index n is 1.36 or more, the shell is dense. S The upper limit of the refractive index n is not particularly set, but is, for example, 1.46. S As shown in formula (1), the average diameter of the primary particles D1, the average diameter of the inner cavity of the outer shell D O , the refractive index of the particle, n a , and the refractive index of the cavity n P The refractive index of the cavity, n P varies depending on the state inside the cavity. For example, if the inside of the cavity is gas, the refractive index is 1.00. If the inside of the cavity is liquid, the refractive index is the refractive index of the liquid. This results in a coating that is transparent and has sufficient hardness and strength. Here, the refractive index n SIf the refractive index n is less than 1.36, the hardness of the coating may be insufficient. S is more preferably 1.37 or more, and further preferably 1.40 or more.
[0031] The average thickness of the shell is preferably 3 to 50 nm. This allows the shell structure to be stably maintained, allowing the particles to exist stably. Also, a coating having high transparency, hardness and strength is obtained. Here, if the shell is thin with an average thickness of less than 3 nm, the particle structure may not be maintained. Conversely, if it exceeds 50 nm, the refractive index of the shell may become too high. The average thickness is more preferably 5 to 30 nm, and further preferably 7 to 25 nm.
[0032] The pore volume of the particle measured by N2 adsorption is 1.0 cm 3 When the pore volume is in this range, the outer shell of the particle is dense. 3 If the pore volume is greater than 0.8 cm3 / g, the shell is sparse (porous), and the hardness and strength of the shell may be weak. In addition, the structure of the shell may not be maintained. Furthermore, when the particles are used in a coated substrate, sufficient hardness and strength may not be obtained. The pore volume is more preferably 0.8 cm3 / g. 3 / g, more preferably less than 0.5 cm 3 / g, most preferably less than 0.0 cm 3 / g.
[0033] The shape of the particles is not particularly limited. For example, it may be spherical, ellipsoidal (rugby ball), cocoon-like, confetti-like, chain-like, dice-like, etc. Among them, spherical particles are preferred because they have high dispersibility and can be uniformly dispersed in the coating.
[0034] The cavity inside the shell preferably has a shape that follows the outer shape of the particle. In other words, the more uniform the thickness of the shell, the better. Although it depends on the thickness of the shell, sufficient hardness and strength can be obtained even when stress is applied to the particle.
[0035] Also, it is preferable that the cavity is substantially composed of one space. Among hollow particles, there may be "particles having multiple spaces inside the shell" that are formed by coalescence of multiple hollow particles. To obtain a transparent coating with a low refractive index, it is better to have fewer such particles. In other words, it is preferable that "particles having multiple spaces inside the shell" account for less than 50% of the total particles. More preferably, it is less than 20%, even more preferably less than 10%, particularly preferably less than 5%, and most preferably 0%.
[0036] The ratio of voids in the particle is preferably 10 to 85%. If the ratio of voids is less than 10%, the refractive index may be too high. Conversely, if the ratio exceeds 85%, there is a risk that sufficient hardness and strength may not be obtained, or that it may be difficult to maintain the hollow structure. The ratio of voids is more preferably 18 to 80%, and even more preferably 30 to 70%.
[0037] The material constituting the outer shell is preferably an oxide containing silicon. Examples of the oxide containing silicon include oxides containing at least one element selected from aluminum, zirconium, titanium, zinc, tin, and antimony and silica. These inorganic oxides may be used alone, in the form of a mixture, or in the form of a composite oxide.
[0038] The content of silicon in the particles is preferably 90% by mass or more when the silicon content is expressed as silica. This improves the compatibility between the particles and the matrix forming components. Therefore, the particles can be highly dispersed in the transparent coating, and the strength and hardness of the coating are improved. The content of silicon is more preferably 95% by mass or more, even more preferably 98% by mass or more, and particularly preferably 100% by mass.
[0039] The content of each of the elements belonging to the alkali metals and alkaline earth metals, which are impurities of the particles, is preferably 1 ppm or less relative to the particles when the element is expressed as an oxide. This reduces the adhesion of the particles, so that the particles are uniformly dispersed in the coating solution or the coating, and a transparent coating is obtained. In addition, the stability of the coating solution is improved, and the coating performance is improved in terms of film hardness and transparency. Here, if the content of each is more than 1 ppm, the rate at which the particles stick to each other increases, and there is a risk that sufficient film hardness cannot be obtained or transparency becomes insufficient. The content is more preferably 0.1 ppm or less. The alkali metals represent Li, Na, K, Rb, Cs, and Fr, and the alkaline earth metals represent Be, Mg, Ca, Sr, Ba, and Ra.
[0040] In addition, the content of each of Fe, Ti, Zn, Pd, Ag, Mn, Co, Mo, Sn, Al, and Zr, which are impurities of the particles and do not contribute to the composition of the particles, is preferably less than 0.1 ppm, the content of each of Cu, Ni, and Cr is preferably less than 1 ppb, and the content of each of U and Th is preferably less than 0.3 ppb. If the content of these impurities is within this range, a transparent coating can be obtained. If the content of these impurities is high, the dispersion liquid may be colored and a transparent coating may not be obtained. In addition, when used in semiconductor circuits such as highly integrated logic and memory, which require high purity, or in optical sensors, the metal elements may cause insulation failure of the circuit, short the circuit, or reduce the light transmittance. This may cause a decrease in the dielectric constant of the insulating film, an increase in the impedance of the metal wiring, a delay in the response speed, an increase in power consumption, etc. In particular, U and Th are not preferable because they generate radioactivity and, even if present in trace amounts, may cause semiconductor malfunction due to radioactivity.
[0041] To obtain particles with a low content of such impurities, it is preferable to use a material that does not contain these elements and has high chemical resistance when preparing the particles. Specifically, plastics such as Teflon (registered trademark), FRP, and carbon fiber, and alkali-free glass are preferable. In addition, it is preferable to purify the raw materials used by distillation, ion exchange, and filter removal.
[0042] As described above, methods for obtaining high-purity particles include preparing raw materials with few impurities in advance and suppressing contamination from the device for preparing the particles. It is also possible to reduce impurities from particles prepared without taking such measures. As a method for reducing impurities, known methods such as ion exchange and ultrafiltration can be used.
[0043] The particles of the present invention can also be dispersed in an organic material such as an organic solvent or an organic resin. In this case, it is preferable to use an organosilicon compound to surface treat the particles. As the organosilicon compound, it is preferable to use an organosilicon compound (n is 1 to 3) represented by the following formula (3). Here, when an organosilicon compound with n being 0 is used, it is preferable to use a partial hydrolyzate of the organosilicon compound.
[0044] R n -SiX 4-n ...Equation (3) (In the formula, R represents an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms and may be the same or different. Examples of the substituent include an epoxy group, an alkoxy group, a vinyl group, a (meth)acryloyloxy group, a mercapto group, a halogen atom, an amino group, and a phenylamino group. X represents an alkoxy group having 1 to 4 carbon atoms, a hydroxyl group, a halogen atom, or a hydrogen atom, and n represents an integer of 0 to 3.)
[0045] Specific examples of the organic silicon compound include tetramethoxysilane, tetraethoxysilane, tetraisopropoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, diphenyldiethoxysilane, isobutyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(βmethoxyethoxy)silane, 3,3,3-trifluoropropyltrimethoxysilane, methyl-3,3,3-trifluoropropyldimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxytripropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-methacryloyl ... Examples of suitable silanes include γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-methacryloxypropyltriethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, trimethylsilanol, methyltrichlorosilane, methyldichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, phenyltrichlorosilane, diphenyldichlorosilane, vinyltrichlorosilane, trimethylbromosilane, and diethylsilane.
[0046] The surface treatment of the particles is carried out by preparing an alcohol dispersion of the particles, adding a predetermined amount of the organosilicon compound represented by formula (3) and water to the dispersion, and hydrolyzing the organosilicon compound. In this hydrolysis, an acid or an alkali is used as a hydrolysis catalyst, if necessary. Furthermore, if necessary, impurities may be reduced by ion exchange, ultrafiltration, etc., at least either before or after the surface treatment.
[0047] The organic silicon compound is R n -SiO (4-n) / 2 It is preferable that the amount is 0.1 to 100 parts by mass (solid content). If the particles are surface-treated with an organosilicon compound, the compatibility with the matrix-forming components is improved.
[0048] Here, if the amount of the organosilicon compound is less than 0.1 parts by mass, the effect of adding the compound is not sufficiently obtained. Rather, the dispersibility of the particles becomes insufficient, and there is a possibility that haze occurs in the obtained transparent coating film. Even if the amount of the organosilicon compound is more than 100 parts by mass, the dispersibility of the particles is not further improved. Furthermore, since the number of sites bonded to the matrix increases, there is a possibility that the adhesion to the substrate becomes insufficient. The amount of the organosilicon compound is more preferably about 2 to 80 parts by mass, and further preferably 3 to 50 parts by mass.
[0049] [Method of manufacturing modified hollow particles] The method for producing modified hollow particles according to the present invention is described below. First, a dispersion of hollow particles containing an inorganic oxide in the shell is prepared (first step). The hollow particles are coated with an inorganic compound (second step). Next, the coated hollow particles are fired (third step). The firing reduces the pore volume of the particles (shell), making the shell dense. Next, the fired particles are suspended in a solvent, and the coating inorganic compound is removed (fourth step). By removing the inorganic compound, particles with high dispersibility in the solvent are obtained.
[0050] The modified hollow particles thus produced are inhibited from agglomerating and have sufficient hardness and strength. The density of the shell of the modified hollow particles is 0.1×10 lower than the density of the shell of the hollow particles produced in the first step. 3 kg / m 3 Each step is described below.
[0051] [First step] The "hollow particles containing an inorganic oxide in the shell" prepared as a starting material in this step are particles having a cavity inside an outer shell made of an inorganic oxide. Hereinafter, this starting material may be simply referred to as "hollow particles."
[0052] The hollow particles are not particularly limited as long as the modified hollow particles can be produced by the above-mentioned method and the obtained modified hollow particles can be used in a coating solution capable of producing a coated substrate. For example, the modified hollow particles may be produced by a conventionally known method. The hollow particles have the same properties as the modified hollow particles described above, except for the properties described below.
[0053] The silicon content in the hollow particles is preferably 80% by mass or more when the silicon content is expressed as silica. This makes it difficult for the composition of the particles themselves to be damaged in the firing process described below and the process of removing the coated inorganic compound. The silicon content is more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 100% by mass.
[0054] If necessary, the hollow particles may be coated with an organosilicon compound represented by the above formula (3) in which n is 0 to 3.
[0055] The coating amount of the organic silicon compound is R n -SiO (4-n) / 2 The solid content is preferably 500 parts by mass or less. If the hollow particles are coated with an organosilicon compound, the shell structure of the hollow particles is easily maintained. In other words, if the shell structure of the hollow particles can be maintained, coating with an organosilicon compound is not necessary. Here, if the amount of coating with the organosilicon compound exceeds 500 parts by mass, the shell of the particles becomes thick, and the refractive index may become too high.
[0056] The content of alkali metal in hollow particles is preferably less than 5% by mass relative to the hollow particles when the alkali metal is expressed as an oxide. The alkali metals are Li, Na, K, Rb, Cs, and Fr. Here, when the content of alkali metal is 5% by mass or more, depending on the type and amount of inorganic compound to be coated, the content of alkali metal, and the temperature during firing, the melting point of hollow particles may be lowered and the particles may adhere to inorganic compounds, or the hollow particles themselves may adhere. The content of alkali metal is more preferably less than 1% by mass, and even more preferably less than 0.1% by mass.
[0057] The content of alkaline earth metal in the hollow particles is preferably less than 1% by mass relative to the hollow particles when the alkaline earth metal is expressed as an oxide. The alkaline earth metals are Be, Mg, Ca, Sr, Ba, and Ra. When the content of alkaline earth metal is 1% by mass or more, depending on the type and amount of inorganic compound to be coated, the content of alkaline earth metal, and the temperature during firing, the melting point of the hollow particles may be lowered and the inorganic compound may be stuck to the hollow particles, or the inorganic oxide hollow particles themselves may be stuck to the hollow particles. The content of alkaline earth metal is more preferably less than 0.1% by mass, and even more preferably less than 0.05% by mass.
[0058] The dispersion medium and concentration of the hollow particle dispersion are not particularly limited as long as the hollow particles are stably dispersed in the liquid without causing aggregation or precipitation.
[0059] Examples of the dispersion medium include water, methanol, ethanol, isopropyl alcohol, acetone, propylene glycol monomethyl ether, and diacetylacetone, with water being preferred from the standpoint of dispersion stability.
[0060] The concentration of the dispersion is preferably 0.01 to 40% by mass as solid content. If the concentration of the dispersion is less than 0.01% by mass, the efficiency of coating with the inorganic compound described below may decrease. In addition, it may take a long time to remove the dispersion medium for the firing process. On the other hand, if the concentration exceeds 40% by mass, uneven coating may occur during coating with the inorganic compound, or the stability of the dispersion may decrease. The concentration of the dispersion is more preferably 0.1 to 30% by mass, and even more preferably 1 to 20% by mass.
[0061] [Second process] A solution of a compound containing silicon and an aqueous solution of an alkali-soluble compound of an inorganic element other than silicon are added to a dispersion liquid of hollow particles to coat the hollow particles with the inorganic compound. At this time, it is preferable to add them so that the MOx fraction (=MOx / (SiO2+MOx)) is 0.05 to 0.67. Here, MOx indicates the mass percentage when the compound of an inorganic element other than silicon is expressed as an oxide, and SiO2 indicates the mass percentage when silicon is expressed as an oxide (SiO2). The sum of both is 100 mass%.
[0062] If the MOx fraction is less than 0.05, it is difficult to obtain modified hollow particles in a monodispersed state. Conversely, if it exceeds 0.67, it is difficult to form a coating layer. The MOx fraction is more preferably 0.15 to 0.45, and further preferably 0.20 to 0.40.
[0063] In this step, the solution of the silicon-containing compound and the aqueous solution of the compound of an inorganic element other than silicon may be added continuously or intermittently, but it is preferable to add both simultaneously. Here, the solution of the silicon-containing compound is at least one selected from a solution of a silicate, an acidic silicic acid solution, and a solution of an organic silicon compound.
[0064] The silicate is preferably at least one of an alkali metal silicate, an organic base silicate, and an ammonium silicate. Examples of the alkali metal silicate include sodium silicate (water glass) and potassium silicate. Examples of the organic base include quaternary ammonium salts such as tetraethylammonium salts, and amines such as monoethanolamine, diethanolamine, and triethanolamine. Examples of the ammonium silicate and the organic base silicate include silicates such as ammonium silicate, quaternary ammonium silicate, and amine silicate. In addition, an alkaline solution in which ammonia, quaternary ammonium hydroxide, and an amine compound are added to a silicic acid solution may be used.
[0065] The acidic silicic acid solution may be a silicic acid solution obtained by removing the alkali by treating an aqueous solution of alkaline silicate with a cation exchange resin, etc. In particular, an acidic silicic acid solution having a pH of 2 to 4 and a concentration of silicon in the solution converted into SiO2 (hereinafter, this "SiO2 converted concentration" may be simply referred to as "SiO2 concentration") of about 7 mass% or less is preferred.
[0066] As the organosilicon compound, the organosilicon compound of the above formula (3) is preferred. Incidentally, in the organosilicon compound of formula (3), compounds in which n is 0 to 3 are poorly hydrophilic. For this reason, it is preferable to hydrolyze the compound in advance so that it can be mixed uniformly in the reaction system. For the hydrolysis, a well-known method can be adopted. When a basic catalyst such as an alkali metal hydroxide, aqueous ammonia, or amine is used as a catalyst for hydrolysis, the basic catalyst can be removed after hydrolysis and the resulting solution can be used as an acidic solution. In addition, when an acidic catalyst such as an organic acid or an inorganic acid is used to prepare a hydrolyzate, it is preferable to remove the acidic catalyst by ion exchange or the like after hydrolysis. The obtained hydrolyzate of the organosilicon compound is preferably used in the form of an aqueous solution. Here, the aqueous solution means that the hydrolyzate is not in a cloudy gel state but is transparent.
[0067] When compounds of inorganic elements other than silicon are expressed as oxides (MOx), the oxides include at least one of Al2O3, B2O3, TiO2, ZrO2, SnO2, CeO2, P2O5, Sb2O3, MoO3, ZnO2, and WO3. Examples of composite oxides of inorganic elements other than silicon include TiO2-Al2O3 and TiO2-ZrO2. Among them, Al2O3 is preferably used because it is easy to control the amount of coating and remove it as silica alumina (SiO2-Al2O3). Note that oxides of alkali metals and oxides of alkaline earth metals are not treated as MOx.
[0068] As the raw material for such oxides of inorganic elements other than silicon (MOx), alkali-soluble inorganic compounds and organometallic compounds are preferable.
[0069] Examples of alkali-soluble inorganic compounds include alkali metal salts or alkaline earth metal salts, ammonium salts, and quaternary ammonium salts of metal or nonmetal oxoacids that form oxides of inorganic elements other than silicon.Specific examples of suitable compounds include sodium aluminate, sodium tetraborate, ammonium zirconyl carbonate, potassium antimonate, potassium stannate, sodium aluminosilicate, sodium molybdate, ammonium cerium nitrate, and sodium phosphate.
[0070] The organometallic compound is preferably an organometallic compound represented by the following formula (4).
[0071] R n -MX a-n ...Equation (4) In the formula, M is a metal element selected from Al, Fe, Ti, Zr, Sn, Ce, P, Sb, Mo, Zn, B, and W, and R is an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms, which may be the same or different. Examples of the substituent include an epoxy group, an alkoxy group, a (meth)acryloyloxy group, a mercapto group, a halogen atom, an amino group, and a phenylamino group. X is an alkoxy group having 1 to 4 carbon atoms, a hydroxyl group, a halogen atom, or a hydrogen atom, a is an integer of 2 to 5, and n is an integer of 0 to 4.
[0072] Specific examples of the organometallic compound include aluminum trimethoxide, aluminum triethoxide, aluminum tri-n-propoxide, aluminum triisopropoxide, aluminum tri-n-butoxide, monomethoxyaluminum diethoxide, monoethoxyaluminum diisopropoxide, monoisopropoxyaluminum di-sec-butoxide, dimethoxyaluminum monoethoxide, diethoxyaluminum monoisopropoxide, aluminum ethyl acetoacetate dimethoxide, aluminum ethyl acetoacetate diethoxide, aluminum ethyl acetoacetate diisopropoxide, acetoalkoxyaluminum diisopropoxide, methylaluminum dimethoxide, methylaluminum diethoxide, methylaluminum diisopropoxide, ethylaluminum diisopropoxide, dimethoxyaluminum chloride, diethoxyaluminum chloride, diisopropoxyaluminum chloride, diisopropoxyaluminum bromide, dimethoxyaluminum hydroxide, diisopropoxyaluminum hydroxide, trimethoxy iron, Triethoxy iron, triisopropoxy iron, dimethoxymethyl iron, diethoxyisopropyl iron, tetramethoxy titanium, tetraethoxy titanium, tetra n-propoxy titanium, tetraisopropoxy titanium, tetrabutoxy titanium, trimethoxymethyl titanium, trimethoxyethyl titanium, trimethoxypropyl titaniums, trimethoxyallyl titaniums, trimethoxyphenyl titaniums, trimethoxy(acetylacetate) titanium, triethoxymethyl titanium, triethoxyethyl titanium, triethoxypropyl titaniums, trimethoxyvinyl titanium , triethoxyphenyl titaniums, tripropoxymethyl titaniums, tripropoxyethyl titaniums, tripropoxybutyl titaniums, tripropoxyphenyl titaniums, tributoxymethyl titaniums, tributoxy(acetylacetonate)titaniums, dimethoxydimethyl titanium, dimethoxydidiethyl titanium, dimethoxydipropyl titaniums, dimethoxydibutyl titanium, dimethoxydi(acetylacetonate)titanium, diethoxydimethyl titanium, diethoxydiethyl titanium, diethoxydipropyl titaniums, dipropoxydimethyl titaniums,Dipropoxydiethyltitanium, dibutoxydimethyltitanium, dibutoxydiethyltitanium, dibutoxydi(acetylacetonato)titanium, diisopropoxybis(acetylacetonato)titanium, isopropoxy(2-ethylexandiolate)titanium, di-n-butoxybis(triethanolaminato)titanium, tetramethoxyzirconium, tetraethoxyzirconium, tetraisopropoxyzirconium, tetrabutoxyzirconium, trimethoxymethylzirconium, trimethoxyethoxy chiral zirconium, trimethoxypropyl zirconium, trimethoxybutyl zirconium, trimethoxyallyl zirconium, trimethoxyphenyl zirconium, trimethoxy(acetylacetonate)zirconium, triethoxymethyl zirconium, triethoxyethyl zirconium, triethoxypropyl zirconium, triethoxyvinyl zirconium, triethoxyphenyl zirconium, tripropoxymethyl zirconium, tripropoxypropyl zirconium, tributoxymethyl zirconium, dimethoxydimethyl zirconium, dimethoxydiethyl zirconium, dimethoxydipropyl zirconium, dimethoxydiphenyl zirconium, dimethoxydi(acetylacetonate)zirconium, diethoxydimethyl zirconium, diethoxydiethyl zirconium, diethoxydipropyl zirconium, dipropoxydimethyl zirconium, dipropoxydipropyl zirconium, dibutoxydimethyl zirconium, dibutoxydibutyl zirconium, tetramethoxyphenyl zirconium, tri ... Examples of the tin oxide include tetramethoxytin, tetraethoxytin, tetraisopropoxytin, tetrabutoxytins, trimethoxymethyltin, trimethoxyethyltin, trimethoxyisopropyltin, trimethoxybutyltins, triethoxymethyltin, triethoxyisopropyltin, triisopropoxymethyltin, triisopropoxybutyltins, triisopropoxyphenyltin, dimethoxydimethyltin, dimethoxydiisopropyltin, diethoxydiethyltin, and diethoxydibutyltins. As with the above compound group, the tin oxide may be a tin oxide containing any one of cerium, phosphorus, antimony, molybdenum, zinc, boron, and tungsten, any one of a methoxy group, an ethoxy group, and an isopropoxyl group,Examples of the metal alkoxide include metal alkoxides having the formula:
[0073] In this step, the reaction system during the addition of the solution is preferably in an alkaline atmosphere. That is, the dispersion of hollow particles in the first step may be made alkaline in advance with an alkaline catalyst or the like, or the alkaline catalyst may be added together with another solution, or both may be used in combination. The pH of this reaction system is preferably 8 or more. If the pH is less than 8, there is a risk that the coating will be insufficient. The pH is more preferably 8.5 or more, and even more preferably 9 or more. The upper limit of the pH is not limited as long as the inorganic oxide hollow particles themselves are not dissolved, but is, for example, about 13.5. The upper limit of the pH is more preferably 13 or less, and even more preferably 12.5 or less.
[0074] Examples of the alkaline catalyst include compounds exhibiting basicity, such as ammonia, amines, alkali metal hydrides, alkaline earth metal hydrides, alkali metal hydroxides, alkaline earth metal hydroxides, quaternary ammonium compounds, and amine coupling agents.
[0075] In addition, the conditions such as the reaction temperature in this coating step are not particularly limited as long as the inorganic compound can be coated on the hollow particles and the inorganic compound can be removed in a subsequent step. However, in consideration of the equipment capacity and production costs, it is preferable to produce the particles under normal pressure at a temperature between normal temperature and below the boiling point of the solvent. For example, when the solvent is water, the reaction temperature is preferably less than 100°C, more preferably 30 to 98°C. In addition, the addition time of the solution is preferably 10 to 2900 minutes, more preferably 30 to 100 minutes.
[0076] Hereinafter, the hollow particles coated with the inorganic compound may be simply referred to as “coated hollow particles.” If necessary, the coated hollow particles may be washed with an ultrafiltration membrane, an ion exchange resin, or the like to remove the alkali catalyst and the like.
[0077] The coating amount of the inorganic compound is preferably 10 parts by mass or more in terms of solid content per 100 parts by mass of the solid content of the hollow particles. This coating amount is determined by taking a predetermined amount of the dispersion of the particles before and after coating, drying it at 120°C, and determining the difference in solid content.
[0078] Here, if the coating amount is less than 10 parts by mass, it is difficult to obtain modified hollow particles in a monodispersed state. Conversely, the greater the coating amount, the easier it is to obtain modified hollow particles in a monodispersed state. However, an excessive coating amount can cause a decrease in efficiency during coating and in the efficiency of removing the coating in the fourth step described below, which in turn can cause a decrease in the production efficiency of modified hollow particles. For this reason, there is no particular upper limit to the coating amount, but it is, for example, about 500 parts by mass. The coating amount is more preferably 30 parts by mass or more, and even more preferably 50 parts by mass or more.
[0079] The average thickness of the coating of the inorganic compound is preferably 3 nm or more. Here, if the average coating thickness is less than 3 nm, it is difficult to obtain modified hollow particles in a monodispersed state. Conversely, the thicker the coating, the easier it is to obtain modified hollow particles in a monodispersed state. However, an excessive coating thickness causes a decrease in the efficiency of coating and the efficiency of removing the coating in the fourth step described below, and ultimately causes a decrease in the production efficiency of modified hollow particles. For this reason, there is no particular upper limit for the coating thickness, but it is, for example, about 50 nm. The average coating thickness is more preferably 5 nm or more, and even more preferably 8 nm or more.
[0080] The hollow particles are coated with at least one inorganic compound selected from the inorganic compounds listed below. Examples include silica alumina, silica boron oxide, silica titania, silica zirconia, silica tin oxide, silica cerium oxide, silica phosphorus oxide, silica antimony oxide, silica molybdenum oxide, silica zinc oxide, silica tungsten oxide, silica titania alumina, and silica titania zirconia. Among these, silica alumina is preferred because it is easy to maintain the particle shape after firing in the third step described below.
[0081] It is desired that the composition of these inorganic compounds is suitable for coating the hollow particles, for densifying the hollow particles by the firing in the third step described below, and for suspending and removing the hollow particles in a solvent in the subsequent fourth step to obtain the desired modified hollow particles. Specifically, as described above, the MOx fraction (=MOx / (SiO2+MOx)) is preferably 0.05 to 0.67. The detailed reason for this is unclear, but it is believed that if the MOx fraction is in this range, the hollow particles are densified by firing and are easily removed from the hollow particles, possibly because the coated inorganic compound is relatively porous. In addition, if the MOx fraction is in this range, it is well matched with the MOx fraction of the inorganic compound added for coating, and the MOx fraction of the coated inorganic compound is roughly equivalent to the MOx fraction of the added inorganic compound. The composition of the coated inorganic compound is determined by the difference in chemical analysis values of the particles before and after coating.
[0082] As described above, after the inorganic compound is coated on the hollow particles, it is calcined and suspended in a solvent and then removed. For this reason, it is preferable that the calcined inorganic compound has high dispersibility or solubility in the solvent.
[0083] The content of the alkali metal in the inorganic compound is preferably less than 10 mass % relative to the inorganic compound expressed as an oxide, where the alkali metal is Li, Na, K, Rb, Cs, or Fr.
[0084] Here, when the content of the alkali metal is 10% by mass or more, depending on the type and coating amount of the inorganic compound, the content of the alkali metal, and the firing temperature in the third step described later, the melting point of the inorganic compound may be lowered, causing the inorganic compound to adhere to the hollow particles or the inorganic compound itself to adhere, making it difficult to remove the inorganic compound. The content of the alkali metal is more preferably less than 8% by mass, and even more preferably less than 3% by mass.
[0085] The content of the alkaline earth metal in the inorganic compound is preferably less than 3 mass % relative to the inorganic compound expressed as an oxide of the alkaline earth metal, where the alkaline earth metal is Be, Mg, Ca, Sr, Ba, or Ra.
[0086] Here, when the content of alkaline earth metal is 3% by mass or more, depending on the type and coating amount of inorganic compound, the content of alkaline earth metal, and the firing temperature in the third step described later, the melting point of the inorganic compound may be lowered, causing the inorganic compound itself to adhere to the hollow particles or the inorganic compound itself to adhere, making it difficult to remove the inorganic compound. The content of alkaline earth metal is more preferably less than 1% by mass, and even more preferably less than 0.1% by mass.
[0087] [Third step] Next, the coated hollow particles are fired at 300 to 1200°C. By firing within this range, the particles (shells) are densified. This reduces the pore volume of the particles, and increases the density of the particle shells. If the firing temperature is less than 300°C, the hollow particles may not be densified sufficiently. On the other hand, if the firing temperature exceeds 1200°C, the hollow particles themselves or the coated inorganic compound and the hollow particles may strongly aggregate, making it difficult to redisperse them as hollow particles. For this reason, there is a risk that the desired dispersion stability of the modified hollow particles may not be obtained, or that the shape of the hollow particles may not be maintained.
[0088] Whether the particles (shells) are densified can be determined simply as follows.
[0089] First, the coated hollow particles and the inorganic compound corresponding to the coated inorganic compound are each fired under the same conditions as in the third step. The density of the fired hollow particles is calculated based on the density difference between the two. The degree of densification can be determined by calculating the difference between the density of the fired hollow particles and the density of the hollow particles in the first step, which are the starting material.
[0090] This density can be determined by the gas displacement method using a fully automatic pycnometer (e.g., Ultrapyc1200e manufactured by Quantachrome Instruments) after crushing each of the above-mentioned fired products in a mortar. For the hollow particles in the first step, the solvent is removed from the dispersion under reduced pressure at room temperature, the particles are dried at 120°C, and then crushed in a mortar and measured in the same manner. However, to determine the density difference more accurately, it is preferable to compare the hollow particles in the first step themselves with the modified hollow particles themselves from which the inorganic compound coating has been removed in the fourth step described below.
[0091] The reduction in the pore volume of the particles can be easily determined by determining the difference in pore volume by the N2 adsorption method in the same manner as above. However, in order to determine the difference in pore volume more accurately, it is preferable to compare the hollow particles themselves in the first step with the modified hollow particles themselves from which the inorganic compound coating has been removed in the fourth step described below.
[0092] Hereinafter, the fired coated hollow particles may be simply referred to as "fired hollow particles".
[0093] In this firing step, the hollow particles are fired in a state of being coated with an inorganic compound. Therefore, although it depends on the firing temperature, the material of the hollow particles, and the material of the inorganic compound coating the hollow particles, in order to prevent the above-mentioned adhesion and to maintain the shape of the hollow particles, the firing temperature is preferably lower than the melting point of the hollow particles, and further lower than the melting point of the inorganic compound coating the hollow particles. The firing temperature is preferably 400 to 1000°C, more preferably 500 to 800°C.
[0094] The firing conditions in this firing step are not particularly limited as long as the hollow particles can be densified and the coated inorganic compound can be removed in a subsequent step. However, when subjecting the coated hollow particles to firing, it is desirable to remove the dispersion medium and further dry them in advance in order to ensure the efficiency and safety of the firing. In addition, the firing equipment is not particularly limited, but it is preferable to use a fluidized bed firing furnace or a rotary kiln in order to apply heat uniformly.
[0095] [Fourth step] Next, the calcined hollow particles obtained in the third step are suspended in a solvent to remove the coating inorganic compound and redisperse the particles, thereby obtaining modified hollow particles.
[0096] The type of solvent used for the suspension is not particularly limited as long as it can remove the coated inorganic compound and disperse the modified hollow particles, but water or an acidic aqueous solution is preferred. When an acidic aqueous solution is used, the inorganic compound is dissolved by the acid and can be removed efficiently. As the acid, conventionally known inorganic acids and organic acids can be used. Among them, hydrochloric acid is preferred because it is easy to work with in removing the inorganic compound.
[0097] The pH of the acidic aqueous solution is preferably 4 or less. If the pH is higher than 4, the dissolution of the inorganic compound by the acid may not be efficiently achieved. There is no particular lower limit for the pH, but it may be 0.0, for example. If the pH is extremely low, the surface potential of the silica decreases, so that the dispersion stability of the modified hollow particles cannot be maintained after redispersion, and they may aggregate. In addition, the efficiency of washing to remove the acid may be reduced. The pH is more preferably less than 3, and even more preferably less than 2.
[0098] The amount of the solvent used for suspension is not particularly limited as long as it can remove the coated inorganic compound and disperse the modified hollow particles, but it is preferably at least 10 times the mass of the calcined hollow particles, and more preferably at least 100 times the mass.
[0099] The coated inorganic compound can be effectively removed by heating the suspension, preferably at a temperature below the boiling point of the solvent.
[0100] To increase the removal efficiency, the suspension may be stirred or circulated, or both may be used in combination. Furthermore, ultrasonic waves or the like may be used.
[0101] The modified hollow particles and the inorganic compound can be separated by a known method such as centrifugation, ultrafiltration, etc. For example, as described above, the dispersion of modified hollow particles containing the coated inorganic compound dissolved by acid can be washed by a known washing method such as ultrafiltration. By washing, the elements of the dissolved inorganic compound are removed, and a dispersion of modified inorganic oxide hollow particles with high dispersion stability is obtained.
[0102] In addition, the elements of the inorganic compounds dissolved therein or alkali metal ions, etc. can be removed by contacting the dispersion with at least one of a cation exchange resin and an anion exchange resin. When washing, the washing can be performed effectively by heating the solution.
[0103] The modified hollow particles obtained by the above-mentioned production method have a shell density of 0.10×10 3 kg / m 3 The difference in density of the shell is preferably 0.20×10 3 kg / m 3 More preferably, 0.30×10 3 kg / m 3 The density (ρs) of the outer shell of the hollow particles is determined by the refractive index (n S ) is obtained from equation (2) which is derived from the Grandstone-Dale equation.
[0104] [Coating liquid for film formation] The particles of the present invention can be applied to a coating solution for forming a coating film. This coating solution contains the particles, a matrix forming component, and an organic solvent. In addition to these, the coating solution may contain additives such as a polymerization initiator, a leveling agent, and a surfactant.
[0105] Next, the main components contained in this coating liquid will be described.
[0106] The concentration of particles in the coating liquid is preferably 5 to 95% by mass in terms of solid content with respect to the total amount of solid content such as the particles and matrix-forming components contained therein.
[0107] If the particle concentration is less than 5% by mass, the refractive index of the coating may not be sufficiently reduced. Conversely, if it is more than 95% by mass, cracks may occur in the coating, adhesion to the substrate may be insufficient, and hardness, strength, transparency, haze, etc. may be deteriorated. The particle concentration is more preferably 10 to 85% by mass, and further preferably 20 to 70% by mass.
[0108] The matrix-forming component is preferably an organic resin-based matrix-forming component, such as a matrix-forming component of an ultraviolet-curable resin, a thermosetting resin, or a thermoplastic resin.
[0109] Examples of ultraviolet-curable resins include (meth)acrylic acid resins, γ-glycyloxy resins, urethane resins, and vinyl resins.
[0110] Examples of the thermosetting resin include urethane resin, melamine resin, silicon resin, butyral resin, reactive silicone resin, phenol resin, epoxy resin, unsaturated polyester resin, and thermosetting acrylic resin.
[0111] Examples of the thermoplastic resin include polyester resin, polycarbonate resin, polyamide resin, polyphenylene oxide resin, thermoplastic acrylic resin, vinyl chloride resin, fluororesin, vinyl acetate resin, and silicone rubber.
[0112] These resins may be copolymers or modified products of two or more kinds, or may be used in combination. Furthermore, these resins may be emulsion resins, water-soluble resins, or hydrophilic resins.
[0113] The components forming these resins are preferably monomers or oligomers in view of particle dispersibility and ease of coating.
[0114] The concentration of the matrix-forming component in the coating liquid is preferably 5 to 95% by mass in terms of solid content with respect to the total amount of solid contents such as the particles and the matrix-forming component contained therein.
[0115] Here, if the concentration of the matrix-forming component is less than 5% by mass, it is difficult to form a coating. Even if a coating is obtained, cracks may occur in the coating, adhesion to the substrate may be insufficient, and hardness, strength, transparency, haze, etc. may be deteriorated. Conversely, if it is more than 95% by mass, the amount of particles is small, so that the refractive index may not be sufficiently reduced. The concentration of this matrix-forming component is more preferably 15 to 90% by mass, and further preferably 30 to 80% by mass.
[0116] The organic solvent to be used is one that can disperse particles uniformly and dissolve or disperse additives such as matrix forming components and polymerization initiators. Among them, hydrophilic solvents and polar solvents are preferred. Examples of hydrophilic solvents include alcohols, esters, glycols, and ethers. Examples of polar solvents include esters and ketones.
[0117] Examples of alcohols include methanol, ethanol, propanol, 2-propanol, butanol, diacetone alcohol, furfuryl alcohol, and tetrahydrofurfuryl alcohol.
[0118] Examples of esters include methyl acetate, ethyl acetate, isopropyl acetate, propyl acetate, isobutyl acetate, butyl acetate, isopentyl acetate, pentyl acetate, 3-methoxybutyl acetate, 2-ethylbutyl acetate, cyclohexyl acetate, and ethylene glycol monoacetate.
[0119] The glycols include ethylene glycol and hexylene glycol.
[0120] Examples of ethers include diethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol isopropyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monomethyl ether acetate.
[0121] Examples of ketones include acetone, methyl ethyl ketone, methyl isobutyl ketone, butyl methyl ketone, cyclohexanone, methylcyclohexanone, dipropyl ketone, methyl pentyl ketone, and diisobutyl ketone.
[0122] Other polar solvents include dimethyl carbonate and toluene.
[0123] These may be used alone or in combination of two or more.
[0124] Any additive that can be used in the past for forming an anti-reflective film can be used as the additive. For example, a polymerization initiator, a leveling agent, etc. can be used to promote polymerization of the matrix-forming components and improve film-forming properties.
[0125] Examples of the polymerization initiator include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,6-dimethoxybenzoyl)2,4,4-trimethyl-pentylphosphine oxide, 2-hydroxymethyl-2-methylphenyl-propane-1-ketone, 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, and the like.
[0126] Examples of the leveling agent include acrylic leveling agents, silicone leveling agents, acrylic silicone leveling agents, etc. Among these leveling agents, those having a fluorine group are preferably used.
[0127] Regarding the concentration of these additives in the coating liquid, those contained as solids when the coating is formed are counted as matrix forming components for convenience, and after coating, they are counted as the matrix.
[0128] The solid content concentration of the coating liquid (the ratio of the total solid content of the particles and the solid content of the matrix-forming components to the coating liquid) is preferably 0.1 to 60% by mass.
[0129] Here, if the solid content concentration of the coating solution is less than 0.1% by mass, the coating may be difficult to apply due to low concentration stability of the coating material, and it may be difficult to obtain a uniform coating film. In addition, the haze or appearance may be deteriorated, and the productivity, manufacturing reliability, etc. may be reduced. Conversely, if the solid content concentration is higher than 60% by mass, the stability of the coating solution may be deteriorated. In addition, the viscosity of the coating solution may be increased, and the coatability may be reduced. Furthermore, the haze of the coating may be increased, the surface roughness may be increased, and the strength may be insufficient. The solid content concentration of the coating solution is more preferably 1 to 50% by mass.
[0130] [Method of manufacturing coated substrate] The coating liquid is used to form a coating on a substrate. From the viewpoint of visibility, the resulting coating is preferably transparent.
[0131] Specifically, the coating liquid is applied onto the substrate, and then dried and irradiated with ultraviolet light to form a coating on the substrate. The method of applying the coating liquid is not particularly limited as long as it can form a coating on the substrate. For example, well-known methods such as spraying, spinner, roll coating, bar coating, slit coater printing, gravure printing, and microgravure printing can be used. Drying is performed by heating to about 50 to 150°C, for example, to evaporate and remove the solvent. Thereafter, ultraviolet light is irradiated to promote polymerization of the resin component and harden the coating. The coating is mainly formed of a matrix (resin) component and particles.
[0132] In the coating, the ratio of the solid content of the particles and matrix-forming components in the coating liquid is the same as the ratio of the particle components and matrix in the coating. As mentioned above, the additives remaining as solids in the coating liquid are counted as the matrix.
[0133] The thickness of the coating can be appropriately selected depending on the application. For example, for an anti-reflection coating, the thickness is preferably 80 to 350 nm.
[0134] Here, if the film thickness is less than 80 nm, the strength and scratch resistance of the film may be insufficient. Also, if the film is too thin, sufficient antireflection performance may not be obtained. Conversely, if the film thickness is more than 350 nm, the antireflection performance may be reduced. Also, if the shrinkage is very large, cracks may occur. This film thickness is more preferably 85 to 220 nm, and further preferably 90 to 110 nm.
[0135] However, particles with a large average particle size may not be completely wrapped because they are larger than the thickness of the coating. In addition to the above-mentioned anti-reflection coating, the particles of the present invention are also applicable to semiconductor mounting applications and hard coat applications because they have transparency, high hardness and strength.
[0136] The refractive index of the coating is preferably 1.10 to 1.45.
[0137] Here, it is difficult to obtain a coating with a refractive index of less than 1.10. Conversely, if the refractive index exceeds 1.45, the antireflection performance may be insufficient, depending on the refractive index of the substrate or the refractive index of another film formed under the coating if necessary. The refractive index of this coating is more preferably 1.15 to 1.35.
[0138] The light transmittance of the coated substrate is preferably 85.0% or more.
[0139] Here, if the light transmittance is less than 85.0%, there is a risk that the clarity of the image will be insufficient in a display device, etc. This light transmittance is more preferably 90.0% or more.
[0140] The haze of the coated substrate is preferably 3% or less, and more preferably 0.3% or less.
[0141] The reflectance of the coated substrate is preferably 2.5% or less, and more preferably 1.5% or less.
[0142] The strength of the coating (scratch resistance) was measured using #0000 steel wool with a load of 1500g / cm 2 It is preferable that no streaky scratches are observed on the film surface after at least 100 strokes, more preferably no scratches are observed after 500 strokes, and even more preferably no scratches are observed after 1000 strokes.
[0143] The pencil hardness of the coating is preferably 2H or more.
[0144] Here, if the hardness is less than 2H, the hardness is insufficient as an anti-reflection film.The pencil hardness is more preferably 3H or more, and further preferably 4H or more.
[0145] The substrate may be a known one. For example, transparent resin substrates such as polycarbonate, acrylic resin, polyethylene terephthalate (PET), triacetyl cellulose (TAC), polymethyl methacrylate resin (PMMA), and cycloolefin polymer (COP) are preferred. These substrates have excellent adhesion to the transparent coating formed by the above-mentioned coating liquid, and a substrate with a coating excellent in hardness, strength, etc. can be obtained. For this reason, it is suitable for use with thin substrates. There is no particular restriction on the thickness of the substrate, but it is preferably 10 to 100 μm, more preferably 20 to 80 μm.
[0146] In addition, a substrate having a coating film formed on the substrate may be used. Examples of the coating film include a conventionally known primer film, hard coat film, high refractive index film, conductive film, etc.
[0147] Examples of the present invention will be described below. Note that, with regard to the coating solution for forming a coating film, the use of particles surface-treated with an organosilicon compound will be exemplified.
[0148] [Example 1] Preparation of Dispersion of Hollow Particles (1) (First Step) The starting material of this Example 1, "hollow particles containing an inorganic oxide in the outer shell" (1), was produced with reference to Example 3 of the above-mentioned Patent Document 2.
[0149] First, 15 g of silica sol (Cataloid SI-550 manufactured by JGC Catalysts and Chemicals, average particle size 5 nm, SiO2 concentration 20% by mass) and 985 g of pure water were mixed and heated to 80° C. The pH of this mixture was 10.5.
[0150] To this mixture, 12.9 kg of a sodium silicate aqueous solution (SiO2 concentration 1.17% by mass) and 12.9 kg of a sodium aluminate aqueous solution with a concentration of 0.83% by mass calculated as the aluminum content in the liquid as Al2O3 (hereinafter, this "Al2O3 equivalent concentration" may be simply referred to as "Al2O3 concentration") were added simultaneously. During this time, the temperature of the reaction solution was maintained at 80°C. The pH of the reaction solution rose to 12.5 immediately after the addition, and thereafter showed almost no change. After the addition was completed, the reaction solution was cooled to room temperature and washed with an ultrafiltration membrane to obtain a dispersion of silica alumina core particles with a solid content concentration of 20% by mass.
[0151] 1720g of pure water was added to 500g of this dispersion of core particles and heated to 98°C. While maintaining this temperature, 2.1kg of silicic acid solution (SiO2 concentration 3.5% by mass) obtained by dealkalizing a sodium silicate aqueous solution with a cation exchange resin was added to obtain a dispersion of silica alumina particles. This was washed with an ultrafiltration membrane and the solid content concentration was adjusted to 13% by mass.
[0152] 1,125 g of pure water was added to 500 g of this dispersion of silica alumina particles, and concentrated hydrochloric acid having a concentration of 35.5% by mass was added dropwise to adjust the pH to 1.0, thereby carrying out dealumination treatment.
[0153] Next, 10 kg of a pH 3.0 hydrochloric acid solution and 5 kg of pure water were added to the mixture, and the dissolved aluminum salt was separated and washed using an ultrafiltration membrane.The solvent was then replaced with ethanol using an ultrafiltration membrane to obtain a dispersion of silica-based hollow particles having a first silica layer with a solid content of 20% by mass.
[0154] 1500g of this dispersion of silica-based hollow particles was mixed with 500g of pure water, 1750g of ethanol, and 626g of ammonia water with a concentration of 28% by mass. After heating this mixture to 35°C, 73g of tetraethoxysilane (SiO2 concentration: 28% by mass) was added, and the surface of the silica-based hollow particles on which the first silica coating layer was formed was coated with a hydrolysis polycondensation product of tetraethoxysilane to form a second silica layer.
[0155] Next, 1000 g of pure water was added to this, and the solid content concentration was concentrated to 5% by mass using an evaporator. Next, ammonia water with a concentration of 15% by mass was added to adjust the pH to 10.0. This was heated in an autoclave at 180°C for 2 hours to obtain a dispersion of hollow particles (1), i.e., hollow particles (1) containing inorganic oxide (silica) in the outer shell. The solid content concentration of this dispersion was 5% by mass. The particles were spherical, with an average primary particle diameter of 75 nm and an outer shell thickness of 10 nm. The refractive index of the particles was 1.23, and the density of the outer shell was 1.82 x 10 3 kg / m 3 It was.
[0156] <Coating hollow particles with inorganic compound (second step)> A 1% by mass aqueous sodium hydroxide solution was added to 5.0 kg of the dispersion of hollow particles (1) to adjust the pH to 12.3. Next, this was heated to 98°C, and 5.6 kg of silicic acid solution (SiO2 concentration 3.5% by mass) and 9.6 kg of sodium aluminate aqueous solution (Al2O3 concentration 1.0% by mass) were added simultaneously over 60 minutes. During this time, the temperature of the reaction solution was maintained at 98°C. After the addition was completed, the reaction solution was cooled to room temperature and washed with an ultrafiltration membrane to obtain a dispersion of hollow particles (1) coated with silica alumina. The solid content concentration of this dispersion was 20% by mass.
[0157] <Firing of coated hollow particles (third process)> 1.0 kg of the dispersion of the coated hollow particles (1) was dried at 110° C. for 24 hours and then calcined at 800° C. for 6 hours to obtain calcined powder of the coated hollow particles (1) (calcined hollow particles (1)).
[0158] <Removal of coated inorganic compound (fourth step)> 100 g of the calcined hollow particles (1) was added to 10 kg of a pH 3.0 aqueous hydrochloric acid solution heated to 50°C, and the mixture was stirred for 3 hours while maintaining the temperature to remove the coated inorganic compounds. Next, using an ultrafiltration membrane, 40 kg of a pH 3.0 aqueous hydrochloric acid solution and 40 kg of pure water were added to separate and remove the dissolved inorganic compounds. 1000 g of the obtained aqueous dispersion was ion-exchanged for 3 hours using 400 g of a cation exchange resin (Diaion SK1B, manufactured by Mitsubishi Chemical Corporation), and then ion-exchanged for 3 hours using 200 g of an anion exchange resin (Diaion SA20A, manufactured by Mitsubishi Chemical Corporation). Thereafter, the mixture was ion-exchanged for 3 hours at 80°C using 200 g of a cation exchange resin (Diaion SK1B, manufactured by Mitsubishi Chemical Corporation), and further washed to obtain an aqueous dispersion of the modified hollow particles (1) of the present invention. The solid content of this dispersion was 10 mass%.
[0159] The hollow particles (1), the coated hollow particles (1), and the modified hollow particles (1) were measured by the following methods.
[0160] The characteristics of each manufacturing process of the modified hollow particles (1) are shown in Table 1 (the same applies to the following Examples. Comparative Examples are shown in Table 2). The properties of the modified hollow particles (1) are shown in Table 3 (the same applies to the following Examples. Comparative Examples are shown in Table 4).
[0161] The physical properties of the particles were measured by image analysis.
[0162] Specifically, the particle dispersion was first diluted to 0.01% by mass, and then dried on a collodion film of a copper cell for an electron microscope. Then, this was photographed at a magnification of 1,000,000 times using a field emission transmission electron microscope (HF5000 manufactured by Hitachi High-Technologies Corporation). Random 1,000 particles in the obtained photographic projections (SEM images, TEM photographs) were measured using the following methods (1) to (5).
[0163] (1) Average primary particle size (D1) The particle area was calculated from the SEM image processing, and the equivalent circle diameter was calculated from the area. The average of the equivalent circle diameters was taken as the average primary particle diameter.
[0164] (2) Cavity diameter and cavity ratio The area of the cavity inside the outer shell of the particle was calculated from the TEM photograph, and the circle equivalent diameter was calculated from the area, which was taken as the cavity diameter. The average value of these cavity diameters was D O It was decided.
[0165] Similarly, the ratio of the cavity volume to the particle volume was calculated from the equivalent circle diameter and cavity diameter of the above particles, and the average was taken as the ratio of the cavities in the particle.
[0166] (3) Covering thickness The thickness of the coating portion on the outer shell of the coated hollow particles (1) was obtained from the TEM photograph, and the average value was taken as the coating thickness.
[0167] (4) Particle shape The ratio of the minor axis to the major axis of the particles was calculated from the SEM image, and particles with an average major axis / minor axis ratio of less than 1.2 were considered to be spherical.
[0168] (5) Cavity shape and percentage of particles with one cavity The ratio of the minor axis to the major axis of the cavities inside the outer shell of the particles was calculated from the TEM photographs. If the average major axis / minor axis ratio was less than 1.2, the particles were deemed spherical. The number of cavities in the particles was also counted, and the ratio was calculated.
[0169] (6) Refractive index of the particles (n a ) The dispersion of hollow particles (1) or modified hollow particles (1) was placed in an evaporator to evaporate the dispersion medium. The dispersion was then dried at 120°C to obtain a powder. A few drops of a standard refractive index liquid with a known refractive index were placed on a glass plate, and the powder was mixed with the drop. This operation was performed with various standard refractive index liquids, and the refractive index of the standard refractive index liquid when the mixed liquid became transparent was taken as the refractive index of the particles.
[0170] (7) Density of the particle’s outer shell (ρs) The average primary particle diameter of the particles (D1) and the average cavity diameter inside the outer shell (D O ), the refractive index of the particles (n a) to obtain the particle's outer shell refractive index (n s ) was calculated, and the density of the particle's outer shell (ρs) was calculated using the above-mentioned equation (2).
[0171] (8) Average particle size by dynamic light scattering method (D2) The dynamic light scattering particle size was measured using a dynamic light scattering particle size distribution measuring device (NICOMP N3000 manufactured by Particle Sizing Systems).
[0172] Specifically, 0.3 g of the aqueous dispersion of the modified hollow particles (1) was diluted to 10 g with an aqueous sodium hydroxide solution having a pH of 11.0, and the average particle size was measured using the particle size measuring device.
[0173] Using this value and the above-mentioned average primary particle diameter (D1), the ratio (D2 / D1) was calculated.
[0174] (9) Carbon content The carbon content in the particles (1) was measured by drying a dispersion of the particles (1) at 120° C. and calcining it at 400° C. using a carbon-sulfur analyzer (HORIBA EMIA-320V).
[0175] (10) 29 Q1, Q2, Q3, Q4 and their ratios by Si-NMR A MIBK dispersion of particle (1) was placed in a dedicated glass cell, and 5% by mass of tetramethylsilane was added as a reference substance. The NMR was measured using an NMR device (JNM-EX270 manufactured by JEOL Ltd., analysis software Excalibur manufactured by JEOL Ltd.). More specifically, the single pulse non-decoupling method was used. 29 The ratios ((Q1+Q2) / ΣQ) and ((Q1+Q2+Q3) / Q4) of the areas of the peaks appearing at chemical shifts of -78 to -88 ppm (Q1), -88 to -98 ppm (Q2), -98 to -108 ppm (Q3), and -108 to -117 ppm (Q4) in the Si-NMR spectroscopy were calculated.
[0176] (11) Pore volume by N2 adsorption method The dispersion of hollow particles (1) or modified hollow particles (1) was dried in an evaporator at 105° C. 1 g of the powder was placed in a cell, and nitrogen was adsorbed using a nitrogen adsorption device (Microtrack-Bel, BELSORP-miniII) to measure the pore volume.
[0177] (12) Silica content The particle dispersion was dried for 12 hours at 120° C. The silica (SiO2) content was determined using an X-ray fluorescence analyzer (EA600VX, manufactured by Hitachi High-Tech Science Corporation).
[0178] (13) Content of alkali metals and other elements The alkali metal contents in the particles, the Fe, Ti, Zn, Pd, Ag, Mn, Co, Mo, Sn, Al, Zr contents, the Cu, Ni, Cr contents, and the U, Th contents were measured by dissolving the particles in hydrofluoric acid, heating to remove the hydrofluoric acid, and then adding pure water as necessary. The resulting solution was then measured using an ICP inductively coupled plasma optical emission spectrometer / mass spectrometer (ICPM-8500, manufactured by Shimadzu Corporation).
[0179] <Production of Coating Solution for Coating Formation> The solvent in the aqueous dispersion of the modified hollow particles (1) was replaced with ethanol using an ultrafiltration membrane to obtain an ethanol dispersion of the particles (1) with a solid content concentration of 10 mass %.
[0180] Next, 3 g of 3-methacryloxypropyltrimethoxysilane (KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd.) was added to 100 g of the ethanol dispersion of the particles (1), and the mixture was heated at 30° C. for 24 hours. Thereafter, the solvent was replaced with methyl isobutyl ketone (MIBK) using an evaporator, and an MIBK dispersion of the particles (1) with a solid content concentration of 5% by mass was obtained.
[0181] To 42 g of the MIBK dispersion of the particles (1), 1.26 g of dipentaerythritol hexaacrylate (DPE-6A manufactured by Kyoeisha Chemical Co., Ltd., solid content concentration 100% by mass), 0.14 g of 1,6-hexanediol diacrylate (A-HD-N manufactured by Shin-Nakamura Chemical Co., Ltd., solid content concentration 100% by mass), 0.06 g of reactive silicone oil for water repellent materials (X-22-174DX manufactured by Shin-Etsu Chemical Co., Ltd., solid content concentration 100% by mass), 0.44 g of silicone-modified polyurethane acrylate (Shikoh UT-4314 manufactured by Nippon Synthetic Chemical Industry Co., Ltd., solid content concentration 30% by mass), and 0.44 g of a photopolymerization initiator (Omnirad manufactured by IGM Resins BV) were added as matrix forming components. 0.1 g of TPO (solid content concentration 100% by mass) was mixed with 50 g of isopropyl alcohol, 9 g of methyl isobutyl ketone, and 11 g of isopropyl glycol as organic solvents to obtain a coating solution (1) for forming a coating film with a solid content concentration of 3% by mass.
[0182] <Manufacture of base material with anti-reflection transparent coating> A hard coat paint (ELCOM HP-1004, manufactured by JGC Catalysts and Chemicals Co., Ltd.) was applied to a TAC film (FT-PB80UL-M, manufactured by PANAC Co., Ltd., thickness 80 μm, refractive index 1.51) using a bar coater method (#18) and dried at 80 °C for 120 seconds. Then, 300 mJ / cm 2 The hard coat film was then cured by irradiation with ultraviolet light of 1000 ohms to prepare a hard coat film. The hard coat film had a thickness of 8 μm.
[0183] Next, the coating solution for forming the coating film was applied by the bar coater method (#4) and dried at 80°C for 120 seconds. Then, it was dried at 400 mJ / cm2 under a N2 atmosphere. 2 The coating was cured by exposure to ultraviolet light of 1000 nm to obtain a substrate (1) with a transparent anti-reflection coating.
[0184] The anti-reflection transparent coated substrate was measured for the following items, and the results are shown in Table 5 (the same applies to the following Examples. Comparative Examples are shown in Table 6).
[0185] (14) Film thickness, refractive index, reflectance The film thickness, film refractive index, and reflectance of light with a wavelength of 550 nm of the anti-reflection transparent coated substrate were measured using an ellipsometer (EMS-1, manufactured by ULVAC Corporation).
[0186] (15) Total light transmittance, haze The total light transmittance and haze of the anti-reflection transparent coated substrate were measured using a haze meter (manufactured by Suga Test Instruments Co., Ltd.).
[0187] (16) Adhesion The surface of a substrate with a transparent anti-reflective coating was scratched with a knife to create 11 parallel lines spaced 1 mm apart to create 100 squares. Cellophane tape was then adhered to the surface, and the adhesion was evaluated by classifying the number of squares that remained without the coating when the cellophane tape was peeled off into the following three levels. Number of remaining squares: 90 or more: ◎ Number of remaining squares: 85-89: Number of remaining squares: 84 or less: △
[0188] (17) Measurement of scratch resistance #0000 steel wool, load 1500g / cm 2 After sliding, the film surface was visually observed and evaluated according to the following criteria. Evaluation criteria; No streaky scratches: ◎ Slight streak marks: ○ Numerous streak-like scratches are observed: △ The entire surface is scraped off: ×
[0189] (18) Pencil hardness The pencil hardness was measured using a pencil hardness tester in accordance with JIS K 5400. That is, a pencil was set at an angle of 45 degrees to the transparent coating surface, and a predetermined load was applied and pulled at a constant speed to observe whether scratches were present.
[0190] [Example 2] <First step> 30 g of silica alumina sol (Cataloid USBB-120 manufactured by JGC Catalysts and Chemicals, average particle size 25 nm, solid content concentration 20% by mass) and 1.97 g of pure water were mixed and heated to 98° C. A 1% by mass aqueous sodium hydroxide solution was added thereto to adjust the pH of the mixture to 11.0.
[0191] To this mixture, 1.45 kg of a sodium silicate aqueous solution (SiO2 concentration 3.0% by mass) and 1.45 kg of a sodium aluminate aqueous solution (Al2O3 concentration 1.0% by mass) were added simultaneously. Next, 3.98 kg of a sodium silicate aqueous solution (SiO2 concentration 3.0% by mass) and 1.33 kg of a sodium aluminate aqueous solution (Al2O3 concentration 1.0% by mass) were added simultaneously. During this time, the temperature of the reaction solution was maintained at 98°C. The pH of the reaction solution rose to 12.0 immediately after the addition, and thereafter showed little change.
[0192] Next, this was washed with an ultrafiltration membrane to adjust the solid concentration to 13 mass %, and then filtered with a capsule filter having an opening of 1 μm to obtain a dispersion liquid of silica alumina particles.
[0193] 1,125 g of pure water was added to 500 g of this dispersion of silica alumina particles, and concentrated hydrochloric acid having a concentration of 35.5% by mass was added dropwise to adjust the pH to 1.0, thereby carrying out dealumination treatment.
[0194] Next, 10 kg of a hydrochloric acid aqueous solution with a pH of 3.0 and 5 kg of pure water were added to the mixture, and the dissolved aluminum salt was separated and washed using an ultrafiltration membrane to obtain a dispersion of silica-based hollow particles with a solid content concentration of 5% by mass. Then, ammonia water with a concentration of 15% by mass was added to adjust the pH to 10.0. This was heated in an autoclave at 150°C for 3 hours to obtain a dispersion of hollow particles (2). The solid content concentration of this dispersion was 5% by mass. The particles were spherical, with an average primary particle diameter of 75 nm and an outer shell thickness of 10 nm. The refractive index of the particles was 1.21 and the density of the outer shell was 1.75×10 3 kg / m 3 It was.
[0195] <Second process> The dispersion of hollow particles (2) obtained in the first step was used, and the silicic acid liquid and the aqueous sodium aluminate solution were added over 90 minutes. Except for this, the procedure was the same as in Example 1 to obtain a dispersion of hollow particles (2) coated with silica alumina. The solid content of this dispersion was 20% by mass.
[0196] <Third step> Calcined hollow particles (2) were obtained in the same manner as in Example 1 using the dispersion of the coated hollow particles (2).
[0197] 〈Fourth step〉 The calcined hollow particles (2) were used to obtain an aqueous dispersion of modified hollow particles (2) in the same manner as in Example 1. The solid content of this dispersion was 10% by mass.
[0198] <Manufacture of coating liquid for forming transparent film and base material with transparent film for antireflection> Next, using this aqueous dispersion of modified hollow particles (2), a coating solution for film formation and a substrate with an anti-reflection transparent film were produced in the same manner as in Example 1, and the respective properties were evaluated.
[0199] [Example 3] Calcined hollow particles (3) were obtained in the same manner as in Example 1, except that in the third step, the dispersion of the coated hollow particles (2) was used and calcined at 330° C. for 6 hours.
[0200] In the subsequent steps, an aqueous dispersion of modified hollow particles having a solid content concentration of 10 mass%, a coating liquid for forming a coating film, and a substrate with an anti-reflection transparent coating were produced using the fired hollow particles (3) in the same manner as in Example 1, and the properties of each were evaluated.
[0201] [Example 4] Calcined hollow particles (4) were obtained in the same manner as in Example 1, except that in the third step, the dispersion of the coated hollow particles (2) was used and calcined at 1180° C. for 6 hours.
[0202] In the subsequent steps, an aqueous dispersion of modified hollow particles having a solid content of 10 mass%, a coating solution for forming a coating film, and a substrate with an anti-reflection transparent coating were produced using the fired hollow particles (4) in the same manner as in Example 1, and the properties of each were evaluated.
[0203] [Example 5] In the second step, 4.0 kg of the dispersion of hollow particles (2) was used, the amount of the silicic acid liquid was 3.0 kg, and the amount of the sodium aluminate aqueous solution was 0.6 kg, and these were added over 30 minutes in the same manner as in Example 1, to obtain a dispersion of hollow particles (5) coated with silica alumina. The solid content concentration of this dispersion was 20 mass%.
[0204] In the third step, the dispersion of the coated hollow particles (5) was used, and calcination was carried out at 500° C. for 3 hours in the same manner as in Example 1 to obtain calcined hollow particles (5).
[0205] In the subsequent steps, an aqueous dispersion of modified hollow particles having a solid content concentration of 10 mass%, a coating liquid for forming a coating film, and a substrate with an anti-reflection transparent coating were produced using the fired hollow particles (5) in the same manner as in Example 1, and the properties of each were evaluated.
[0206] [Example 6] In the second step, 1.0 kg of the dispersion of hollow particles (2) was used, the amount of the silicic acid liquid was 2.3 kg, and the amount of the sodium aluminate aqueous solution was 16.2 kg, and these were added over 90 minutes in the same manner as in Example 1, to obtain a dispersion of hollow particles (6) coated with silica alumina. The solid content concentration of this dispersion was 20 mass%.
[0207] In the third step, the dispersion of the coated hollow particles (6) was used, and calcination was carried out at 900° C. for 10 hours in the same manner as in Example 1 to obtain calcined hollow particles (6).
[0208] In the fourth step, 100 g of the calcined hollow particles (6) was added to 40 kg of a pH 1.0 aqueous hydrochloric acid solution heated to 50°C, and the mixture was stirred for 3 hours while maintaining the temperature, to remove the coated inorganic compounds. Next, using an ultrafiltration membrane, 160 kg of a pH 1.0 aqueous hydrochloric acid solution and 160 kg of pure water were added to separate and remove the dissolved inorganic compounds. Thereafter, ion exchange and washing were performed in the same manner as in Example 1, to obtain an aqueous dispersion of modified hollow particles (6) with a solid content concentration of 10% by mass. The solid content concentration of this dispersion was 10% by mass.
[0209] In the subsequent steps, a coating solution for forming a film and a substrate with an antireflection transparent film were produced in the same manner as in Example 1 using the aqueous dispersion of the particles (6), and the respective properties were evaluated.
[0210] [Example 7] In the second step, 1.0 kg of the dispersion of hollow particles (2) was used, the amount of the silicic acid liquid was 0.54 kg, and the amount of the sodium aluminate aqueous solution was 0.93 kg, and these were added over 90 minutes in the same manner as in Example 1, to obtain a dispersion of hollow particles (7) coated with silica alumina. The solid content concentration of this dispersion was 20 mass%.
[0211] In the third step, calcined hollow particles (7) were obtained in the same manner as in Example 1, except that the dispersion of the coated hollow particles (7) was used and calcined at 500° C. for 3 hours.
[0212] In the subsequent steps, an aqueous dispersion of modified hollow particles having a solid content of 10 mass%, a coating solution for forming a coating film, and a substrate with an anti-reflection transparent coating were produced using the fired hollow particles (7) in the same manner as in Example 1, and the properties of each were evaluated.
[0213] [Example 8] In the second step, 1.0 kg of the dispersion of hollow particles (2) was used, the amount of the silicic acid liquid was 4.62 kg, and the amount of the sodium aluminate aqueous solution was 7.97 kg, and these were added over 2900 minutes in the same manner as in Example 1, to obtain a dispersion of hollow particles (8) coated with silica alumina. The solid content concentration of this dispersion was 20 mass%.
[0214] In the third step, the dispersion of the coated hollow particles (8) was used, and calcination was carried out at 900° C. for 10 hours in the same manner as in Example 1 to obtain calcined hollow particles (8).
[0215] In the subsequent steps, an aqueous dispersion of modified hollow particles having a solid content of 10 mass%, a coating liquid for forming a coating film, and a substrate with an anti-reflection transparent coating were produced using the fired hollow particles (8) in the same manner as in Example 6, and the properties of each were evaluated.
[0216] [Example 9] In the second step, the same procedure as in Example 1 was followed except that a dispersion of hollow particles (2) was used, and a sodium silicate aqueous solution (SiO2 concentration 3.5% by mass) was used instead of the silicic acid solution, and this and the sodium aluminate aqueous solution were added over 90 minutes. After the addition was completed, the reaction solution was cooled to room temperature and washed with an ultrafiltration membrane. Then, 0.56 kg of a sodium hydroxide aqueous solution having a 10% by mass as Na2O was added to obtain a dispersion of hollow particles (9) coated with silica alumina. The solid content concentration of this dispersion was 20% by mass.
[0217] In the third step, the dispersion of the coated hollow particles (9) was used, and calcination was carried out at 1180° C. for 6 hours in the same manner as in Example 1 to obtain calcined hollow particles (9).
[0218] In the subsequent steps, an aqueous dispersion of modified hollow particles having a solid content concentration of 10 mass%, a coating solution for forming a coating film, and a substrate with an anti-reflection transparent coating were produced using the fired hollow particles (9) in the same manner as in Example 1, and the properties of each were evaluated.
[0219] [Example 10] A dispersion of hollow particles (10) was obtained in the same manner as in Example 2, except that in the first step, the heat treatment in an autoclave was performed at 250° C. for 19 hours. The solid content concentration of this dispersion was 5 mass %. The average primary particle diameter of these particles was 75 nm, and the thickness of the outer shell was 10 nm. The refractive index of these particles was 1.22, and the density of the outer shell was 1.82×10 3 kg / m 3 It was.
[0220] In the subsequent steps, an aqueous dispersion of modified hollow particles having a solid content concentration of 10 mass %, a coating liquid for forming a coating film, and a substrate with an antireflection transparent coating were produced using the dispersion of hollow particles (10) in the same manner as in Example 1, and the properties of each were evaluated.
[0221] [Example 11] <First step> 25 g of silica sol (Cataloid SI-550 manufactured by JGC Catalysts and Chemicals, average particle size 5 nm, SiO2 concentration 20% by mass) and 980 g of pure water were mixed and heated to 80° C. A 1% by mass aqueous sodium hydroxide solution was added to the mixture to adjust the pH to 9.0.
[0222] To this mixture, 3.25 kg of sodium silicate aqueous solution (SiO2 concentration 3.0 mass%) and 3.25 kg of sodium aluminate aqueous solution (Al2O3 concentration 1.0 mass%) were added simultaneously. Next, 14.7 kg of sodium silicate aqueous solution (SiO2 concentration 3.0 mass%) and 4.9 kg of sodium aluminate aqueous solution (Al2O3 concentration 1.0 mass%) were added simultaneously. During this time, the temperature of the reaction solution was maintained at 80°C. The pH of the reaction solution rose to 11.0 immediately after the addition, and thereafter showed little change.
[0223] Next, this was washed with an ultrafiltration membrane to adjust the solid content concentration to 13 mass %, and then filtered with a capsule filter having an opening of 1 μm to obtain a dispersion liquid of silica alumina particles.
[0224] 1,125 g of pure water was added to 500 g of this dispersion of silica alumina particles, and concentrated hydrochloric acid having a concentration of 35.5% by mass was added dropwise to adjust the pH to 1.0, thereby carrying out dealumination treatment.
[0225] Next, 10 kg of a hydrochloric acid aqueous solution with a pH of 3.0 and 5 kg of pure water were added to the mixture, while the dissolved aluminum salt was separated and washed using an ultrafiltration membrane, to obtain a dispersion of silica-based hollow particles with a solid content concentration of 5% by mass. Next, ammonia water with a concentration of 15% by mass was added to adjust the pH to 10.0. This was heated in an autoclave at 200°C for 3 hours to obtain a dispersion of hollow particles (11). The solid content concentration of this dispersion was 5% by mass. The particles were spherical, with an average primary particle diameter of 20 nm and an outer shell thickness of 5 nm. The refractive index of the particles was 1.21, and the density of the outer shell was 1.75×10 3 kg / m 3 It was.
[0226] <Second process> A 1% by mass aqueous sodium hydroxide solution was added to 5.0 kg of the dispersion of hollow particles (11) to adjust the pH to 11.5. Then, this was heated to 80°C, and 4.44 kg of silicic acid solution (SiO2 concentration 3.5% by mass) and 7.66 kg of sodium aluminate aqueous solution (Al2O3 concentration 1.0% by mass) were added simultaneously over 60 minutes. During this time, the temperature of the reaction solution was maintained at 80°C. After the addition was completed, the reaction solution was cooled to room temperature and washed with an ultrafiltration membrane to obtain a dispersion of hollow particles (11) coated with silica alumina. The solid content concentration of this dispersion was 20% by mass.
[0227] In the third step, calcined hollow particles (11) were obtained in the same manner as in Example 1, except that a dispersion of the coated hollow particles (11) was used and calcined at 500° C. for 6 hours.
[0228] In the subsequent steps, an aqueous dispersion of modified hollow particles having a solid content concentration of 10 mass%, a coating liquid for forming a coating film, and a substrate with an anti-reflection transparent coating were produced using the fired hollow particles (11) in the same manner as in Example 1, and the properties of each were evaluated.
[0229] [Example 12] <First step> 21 g of silica sol (Cataloid SI-50 manufactured by JGC Catalysts and Chemicals, average particle size 25 nm, SiO2 concentration 48% by mass) and 979 g of pure water were mixed and heated to 98° C. A 1% by mass aqueous sodium hydroxide solution was added to adjust the pH to 12.5.
[0230] To this mixture, 31.8 kg of sodium silicate aqueous solution (SiO2 concentration 0.75 mass%) and 31.8 kg of sodium aluminate aqueous solution (Al2O3 concentration 0.25 mass%) were added simultaneously. Next, 10.5 kg of sodium silicate aqueous solution (SiO2 concentration 3.0 mass%) and 3.5 kg of sodium aluminate aqueous solution (Al2O3 concentration 1.0 mass%) were added simultaneously. During this time, the temperature of the reaction solution was maintained at 98°C. The pH of the reaction solution dropped to 11.5 immediately after the addition, and thereafter showed little change.
[0231] Next, this was washed with an ultrafiltration membrane to adjust the solid concentration to 25% by mass, and then filtered with a capsule filter having an opening of 1 μm to obtain a dispersion liquid of silica alumina particles.
[0232] 1,125 g of pure water was added to 500 g of this dispersion of silica alumina particles, and concentrated hydrochloric acid having a concentration of 35.5% by mass was added dropwise to adjust the pH to 1.0, thereby carrying out dealumination treatment.
[0233] Next, 30 kg of a hydrochloric acid aqueous solution with a pH of 3.0 and 5 kg of pure water were added to the mixture, while the dissolved aluminum salt was separated and washed using an ultrafiltration membrane, to obtain a dispersion of silica-based hollow particles with a solid content concentration of 5% by mass. Next, ammonia water with a concentration of 15% by mass was added to adjust the pH to 10.0. This was heated in an autoclave at 195°C for 48 hours to obtain a dispersion of hollow particles (12). The solid content concentration of this dispersion was 5% by mass. The particles were spherical, with an average primary particle diameter of 100 nm and an outer shell thickness of 8 nm. The refractive index of the particles was 1.15, and the density of the outer shell was 1.77×10 3 kg / m 3 It was.
[0234] <Second process> A 1% by mass aqueous sodium hydroxide solution was added to 5.0 kg of the dispersion of hollow particles (12) to adjust the pH to 12.3. Then, this was heated to 98°C, and 4.8 kg of silicic acid solution (SiO2 concentration 3.5% by mass) and 8.3 kg of sodium aluminate aqueous solution (Al2O3 concentration 1.0% by mass) were added simultaneously over 180 minutes. During this time, the temperature of the reaction solution was maintained at 98°C. After the addition was completed, the reaction solution was cooled to room temperature and washed with an ultrafiltration membrane to obtain a dispersion of hollow particles (12) coated with silica alumina. The solid content concentration of this dispersion was 20% by mass.
[0235] In the subsequent steps, an aqueous dispersion of modified hollow particles (12) having a solid content of 10 mass % was obtained in the same manner as in Example 1 using the dispersion of the coated hollow particles (12). <Production of Coating Solution for Coating Formation and Substrate with Transparent Anti-Reflection Coating> Using the aqueous dispersion of the particles (12), an MIBK dispersion of the particles (12) having a solid content concentration of 5 mass % was obtained in the same manner as in Example 1.
[0236] A coating solution (12) for forming a film having a solid content concentration of 3 mass% was obtained in the same manner as in Example 1, except that 33 g of the MIBK dispersion of particles (12), 1.67 g of dipentaerythritol hexaacrylate, 0.19 g of 1,6-hexanediol diacrylate, and 17.6 g of methyl isobutyl ketone were used.
[0237] Thereafter, a substrate with an antireflection transparent coating was produced in the same manner as in Example 1 using the coating solution (12) for forming a coating film, and each of the characteristics was evaluated.
[0238] [Example 13] <First step> 25 g of silica sol (Cataloid SI-80P manufactured by JGC Catalysts and Chemicals, average particle size 80 nm, SiO2 concentration 40% by mass) and 80 g of pure water were mixed and heated to 98° C. A 1% by mass aqueous sodium hydroxide solution was added to adjust the pH to 12.5.
[0239] To this mixture, 76 kg of sodium silicate aqueous solution (SiO2 concentration 15 mass%) and 76 kg of sodium aluminate aqueous solution (Al2O3 concentration 5.0 mass%) were added simultaneously. Next, 95.2 kg of sodium silicate aqueous solution (SiO2 concentration 3.0 mass%) and 31.7 kg of sodium aluminate aqueous solution (Al2O3 concentration 1.0 mass%) were added simultaneously. During this time, the temperature of the reaction solution was maintained at 98 ° C. The pH of the reaction solution hardly changed from 12.5. After the addition was completed, the reaction solution was cooled to room temperature and washed with an ultrafiltration membrane to adjust the solid concentration to 13 mass%, and then filtered with a capsule filter with a mesh size of 10 μm to obtain a dispersion of silica alumina particles.
[0240] 1,125 g of pure water was added to 500 g of this dispersion of silica alumina particles, and concentrated hydrochloric acid having a concentration of 35.5% by mass was added dropwise to adjust the pH to 0.5, thereby carrying out dealumination treatment.
[0241] Next, 30 kg of a hydrochloric acid aqueous solution with a pH of 3.0 and 20 kg of pure water were added to the mixture, while the dissolved aluminum salt was separated and washed using an ultrafiltration membrane, to obtain a dispersion of silica-based hollow particles with a solid content concentration of 5% by mass. Next, ammonia water with a concentration of 15% by mass was added to adjust the pH to 10.0. This was heated in an autoclave at 200°C for 3 hours to obtain a dispersion of hollow particles (13). The solid content concentration of this dispersion was 5% by mass. The particles were spherical, with an average primary particle diameter of 1000 nm and an outer shell thickness of 30 nm. The refractive index of the particles was 1.07, and the density of the outer shell was 1.77×10 3 kg / m 3 It was.
[0242] <Second process> A 1% by mass aqueous sodium hydroxide solution was added to 1.0 kg of the dispersion of hollow particles (13) to adjust the pH to 12.3. This was then heated to 98°C, and 2.13 kg of silicic acid solution (SiO2 concentration 0.3% by mass) and 3.15 kg of sodium aluminate aqueous solution (Al2O3 concentration 0.1% by mass) were added simultaneously over 90 minutes. During this time, the temperature of the reaction solution was maintained at 98°C. After the addition was completed, the reaction solution was cooled to room temperature and washed with an ultrafiltration membrane to obtain a dispersion of coated hollow particles (13) with a solid content concentration of 20% by mass.
[0243] In the subsequent steps, an aqueous dispersion of modified hollow particles (13) having a solid content concentration of 10 mass % was produced in the same manner as in Example 1 using the dispersion of the coated hollow particles (13), and each characteristic was evaluated.
[0244] The average particle size of the modified hollow particles (13) obtained here was larger than the film thickness of the coated substrate under investigation. Therefore, it was considered that it was not appropriate to compare the particles of the modified hollow particles (13) side by side with the particles of other Examples in the performance evaluation when used as an anti-reflection film. For this reason, the production of a coating solution for forming a coating film and a coated substrate was not carried out here.
[0245] [Example 14] <First step> In the same manner as in Example 1, a dispersion liquid of silica alumina particles with a solid content adjusted to 13 mass % was obtained.
[0246] 1,125 g of pure water was added to 500 g of this dispersion of silica alumina particles, and concentrated hydrochloric acid having a concentration of 35.5% by mass was added dropwise to adjust the pH to 0.3, thereby carrying out dealumination treatment.
[0247] Next, 50 kg of a pH 3.0 hydrochloric acid solution and 50 kg of pure water were added to the mixture, and the dissolved aluminum salt was separated and washed using an ultrafiltration membrane. This dealumination treatment and washing using the ultrafiltration membrane were repeated three times in total to obtain a dispersion of silica-based hollow particles with a solid content of 5% by mass.
[0248] Next, ammonia water with a concentration of 15% by mass was added to adjust the pH to 10.0. This was heat-treated in an autoclave at 150°C for 3 hours to obtain a dispersion of hollow particles (14). The solid content of this dispersion was 5% by mass. The particles were spherical, with an average primary particle diameter of 75 nm and an outer shell thickness of 10 nm. The refractive index of the particles was 1.21 and the density of the outer shell was 1.74 x 10 3 kg / m 3 It was.
[0249] <Second process> A dispersion of hollow particles (14) coated with silica alumina was obtained in the same manner as in Example 1, except that the dispersion of hollow particles (14) was used and the silicic acid liquid and the aqueous sodium aluminate solution were added over 90 minutes. The solid content of this dispersion was 20 mass%.
[0250] <Third step> Calcined hollow particles (14) were obtained in the same manner as in Example 1, except that the dispersion of the coated hollow particles (14) was used.
[0251] 〈Fourth step〉 100 g of the calcined hollow particles (14) was added to 10 kg of a hydrochloric acid solution of pH 1.0 heated to 50°C, and the mixture was stirred for 3 hours while maintaining the temperature to remove the coated inorganic compounds. Next, using an ultrafiltration membrane, 100 kg of a hydrochloric acid solution of pH 3.0 and 100 kg of pure water were added to separate and remove the dissolved inorganic compounds. To this, concentrated hydrochloric acid with a concentration of 35.5 mass% was dropped to adjust the pH to 0.3 and stirred. Next, using an ultrafiltration membrane, 50 kg of a hydrochloric acid solution of pH 3.0 and 50 kg of pure water were added to further separate and remove the dissolved inorganic compounds such as aluminum salts. 1000 g of the obtained aqueous dispersion was ion-exchanged for 3 hours using 400 g of a cation exchange resin (Diaion SK1B manufactured by Mitsubishi Chemical Corporation), and then ion-exchanged for 3 hours using 200 g of an anion exchange resin (Diaion SA20A manufactured by Mitsubishi Chemical Corporation). Thereafter, the mixture was subjected to ion exchange at 80° C. for 10 hours using 400 g of a cation exchange resin (Diaion SK1B, manufactured by Mitsubishi Chemical Corporation) and then washed to obtain an aqueous dispersion of modified hollow particles (14). The solid content of the dispersion was 10% by mass.
[0252] <Manufacture of coating liquid for forming transparent film and base material with transparent film for antireflection> Using the aqueous dispersion of the particles (14), a coating solution for forming a film and a substrate with an antireflection transparent film were produced in the same manner as in Example 1, and the respective properties were evaluated.
[0253] [Example 15] 2.4 kg of a 2.1% by mass aqueous solution of cetyltrimethylammonium bromide was placed in a separable flask, nitrogen gas was sealed in, and the mixture was heated to 80°C. 18 g of styrene was added to the mixture and stirred for 10 minutes, after which 10 g of a 10% by mass aqueous solution of 2.2'-azobis(2-amidinopropane) hydrochloride was added and stirred for 4 hours. Next, the mixture was washed with an ultrafiltration membrane to obtain a dispersion of polystyrene particles with a solid content concentration of 10% by mass.
[0254] 100 g of this dispersion was mixed with 350 g of pure water, 450 g of ethanol, and 100 g of ammonia water with a concentration of 28% by mass. After heating this mixture to 35°C, 41 g of tetraethoxysilane (SiO2 concentration: 28% by mass) was added and stirred for 3 hours to coat the surfaces of the polystyrene particles with a hydrolysis polycondensate of tetraethoxysilane.
[0255] Next, 1000 g of pure water was added to this, and the solid content concentration was concentrated to 5 mass% using an evaporator, after which 281 g of n-octane and 7.9 g of n-octyldimethylsilyl chloride were added and stirred. Next, this solution was transferred to an autoclave, and heat-treated at 400°C and a pressure of 6.8 MPa for 1 hour to remove the core, and then washed using an ultrafiltration membrane. Next, ammonia water with a concentration of 15 mass% was added to adjust the pH to 10.0. This was heat-treated in an autoclave at 195°C for 48 hours to obtain a dispersion of hollow particles (15). The solid content concentration of this dispersion was 5 mass%. The particles were spherical, with an average particle diameter of 102 nm and an outer shell thickness of 13 nm. In addition, the refractive index of these particles was 1.22, and the density of the outer shell was 1.79 x 10 3 kg / m 3 It was.
[0256] In the subsequent steps, an aqueous dispersion of modified hollow particles (15) having a solid content concentration of 10 mass % was produced in the same manner as in Example 14, using the dispersion of hollow particles (15).
[0257] Thereafter, using the aqueous dispersion of the particles (15), a coating solution for forming a film and a substrate with an antireflection transparent film were produced in the same manner as in Example 12, and the respective properties were evaluated.
[0258] [Comparative Example 1] In the production of the coating solution for forming a transparent film, a dispersion of hollow particles (2) in which the solid content concentration was adjusted to 10 mass % was used, and a coating solution for forming a transparent film and a substrate with an anti-reflection transparent film were produced in the same manner as in Example 1, and each property was evaluated.
[0259] [Comparative Example 2] In the third step, calcined hollow particles (R2) were obtained in the same manner as in Example 1, except that the dispersion of hollow particles (2) was used instead of the dispersion of coated hollow particles (1).
[0260] In the fourth step, the calcined hollow particles (R2) were used to attempt removal of the coated inorganic compound in the same manner as in Example 1. However, the particles did not redisperse and remained precipitated. For this reason, the coating solution for forming a coating film and the substrate with a coating film were not produced.
[0261] [Comparative Example 3] In the same manner as in Comparative Example 2, sintered hollow particles (R2) were obtained.
[0262] Thereafter, the fourth step was not carried out, and 100 g of the sintered hollow particles were added to 10 kg of pure water, and an attempt was made to disperse the particles using a bead mill. When the bead mill-treated product was analyzed by image analysis using an electron microscope, it was found that the outer shells of the hollow particles were destroyed and the particles were cracked, and the number of particles that maintained their shape as hollow particles was less than 10%. For this reason, a coating solution for forming a coating film and a substrate with a coating film were not produced.
[0263] [Comparative Example 4] Calcined hollow particles (R4) were obtained in the same manner as in Example 1, except that in the third step, the dispersion of the coated hollow particles (2) was used and calcined at 250° C. for 6 hours.
[0264] In the subsequent steps, an aqueous dispersion of modified hollow particles having a solid content of 10 mass%, a coating solution for forming a coating film, and a substrate with an anti-reflection transparent coating were produced in the same manner as in Example 1 using the fired hollow particles (R4), and the properties of each were evaluated.
[0265] [Comparative Example 5] Calcined hollow particles (R5) were obtained in the same manner as in Example 1, except that in the third step, the dispersion liquid of the coated hollow particles (CP2) was used and calcined at 1280° C. for 6 hours.
[0266] In the fourth step, the calcined hollow particles (R5) were used to attempt removal of the coated inorganic compound in the same manner as in Example 1. However, the particles did not redisperse and remained precipitated. For this reason, the coating solution for forming a coating film and the substrate with a coating film were not produced.
[0267] [Comparative Example 6] In the same manner as in Example 2, fired hollow particles (2) were obtained.
[0268] Thereafter, the fourth step was not carried out, and 100 g of the sintered hollow particles were added to 10 kg of pure water, and an attempt was made to disperse the particles using a bead mill. When the bead mill-treated product was analyzed by image analysis using an electron microscope, it was found that the outer shells of the hollow particles were destroyed and the particles were cracked, and the number of particles that maintained their shape as hollow particles was less than 10%. For this reason, a coating solution for forming a coating film and a substrate with a coating film were not produced.
[0269] [Comparative Example 7] In the second step, 4.0 kg of the dispersion of hollow particles (2) was used, the amount of the silicic acid liquid was 6.5 kg, and the amount of the sodium aluminate aqueous solution was 0.7 kg, and these were added over 90 minutes in the same manner as in Example 1, to obtain a dispersion of hollow particles (R7) coated with silica alumina. The solid content concentration of this dispersion was 20 mass%.
[0270] In the subsequent steps, an aqueous dispersion of modified hollow particles having a solid content concentration of 10 mass%, a coating solution for forming a coating film, and a substrate with an anti-reflection transparent coating were produced in the same manner as in Example 1 using the dispersion of the coated hollow particles (R7), and the properties of each were evaluated.
[0271] [Comparative Example 8] In the second step, 4.0 kg of the dispersion of hollow particles (2) was used, the amount of the silicic acid liquid was 2.0 kg, and the amount of the sodium aluminate aqueous solution was 16.3 kg, and these were added over 90 minutes in the same manner as in Example 1, to obtain a dispersion of hollow particles (R8) coated with silica alumina. The solid content concentration of this dispersion was 20 mass%.
[0272] In the subsequent steps, an aqueous dispersion of modified hollow particles having a solid content concentration of 10 mass%, a coating solution for forming a coating film, and a substrate with an anti-reflection transparent coating were produced in the same manner as in Example 1 using the dispersion of the coated hollow particles (R8), and the properties of each were evaluated.
[0273] [Comparative Example 9] In the second step, 5.0 kg of the dispersion of hollow particles (2) was used, and the amount of the silicic acid liquid and the amount of the sodium aluminate aqueous solution were changed to 0.4 kg and 0.7 kg, respectively, and these were added over 30 minutes in the same manner as in Example 1, to obtain a dispersion of hollow particles (R9) coated with silica alumina. The solid content concentration of this dispersion was 20 mass%.
[0274] In the subsequent steps, an aqueous dispersion of modified hollow particles having a solid content concentration of 10 mass%, a coating solution for forming a coating film, and a substrate with an anti-reflection transparent coating were produced in the same manner as in Example 1 using the dispersion of the coated hollow particles (R9), and the properties of each were evaluated.
[0275] [Comparative Example 10] Calcined hollow particles (R10) were obtained in the same manner as in Example 1, except that in the third step, calcination was performed at 230° C. for 6 hours.
[0276] In the subsequent steps, the fired hollow particles (R10) were used to produce an aqueous dispersion of the modified hollow particles having a solid content of 10 mass%, a coating liquid for forming a coating film, and a substrate with an anti-reflection transparent coating in the same manner as in Example 1, and the properties of each were evaluated.
[0277] [Table 1]
[0278] [Table 2]
[0279] [Table 3]
[0280]
Table 4
[0281]
Table 5
[0282]
Table 6
Claims
1. A particle having a cavity inside an outer shell containing an inorganic oxide, The density of the shell is 1.85×10 3 kg / m 3 That's all, The average primary particle diameter of the particles (D 1 ) is 20 to 1000 nm, The average particle diameter (D 2 ) and the average value of the primary particle diameter (D 1 ) and the ratio (D 2 / D 1 ) is 1.0 to 1.8, the particle has a peak area (Q 1 ) appearing at a chemical shift of -78 to -88 ppm, a peak area (Q 2 ) appearing at a chemical shift of -88 to -98 ppm, a peak area (Q 3 ) appearing at a chemical shift of -98 to -108 ppm, and a peak area (Q 4 ) appearing at a chemical shift of -108 to -117 ppm, the ratio ((Q 1 +Q 2 ) / (Q 1 +Q 2 +Q 3 +Q 4 )) being 0.05 to 0.50 and the ratio ((Q 1 +Q 2 +Q 3 ) / Q 4 ) being 0.05 to 1.00; The modified hollow particles have a carbon content of 0.50 mass % or less.
2. The modified hollow particles according to claim 1, characterized in that the average primary particle diameter (D 1 ) of the particles is 20 to 110 nm.
3. The modified hollow particle according to claim 1, characterized in that the particle has a pore volume measured by a nitrogen adsorption method of less than 1.0 cm 3 / g.
4. A first step of preparing a dispersion of hollow particles having an inorganic oxide in an outer shell; a second step of coating the hollow particles with an inorganic compound; a third step of firing the coated hollow particles at 300 to 1200° C.; a fourth step of suspending the hollow particles after the firing in a solvent to remove the inorganic compound; The density of the shell of the particle obtained in the fourth step is 0.10×10 lower than the density of the shell of the hollow particle obtained in the first step. 3 kg / m 3 or more.
5. 5. The method for producing modified hollow particles according to claim 4, wherein the hollow particles in the first step contain silicon.
6. The composition ratio of the inorganic compound is the MOx fraction (=MOx / (SiO 2 +MOx)) is 0.05 to 0.67 (where MOx is the mass percentage when inorganic elements other than silicon are expressed as oxides, SiO 2 is silicon oxide (SiO 2 5. The method for producing modified hollow particles according to claim 4, wherein the total of the two is taken as 100 mass %.
7. 5. The method for producing modified hollow particles according to claim 4, wherein the coating amount of the inorganic compound is 10 parts by mass or more in terms of solid content per 100 parts by mass of the solid content of the inorganic oxide hollow particles.
8. 5. The method for producing modified hollow particles according to claim 4, wherein the content of the alkali metal in the inorganic compound is less than 10 mass % in terms of oxide, based on the inorganic compound expressed as an oxide.
9. 5. The method for producing modified hollow particles according to claim 4, wherein the solvent is an acidic aqueous solution.
Citation Information
Patent Citations
Multiple oxide sol, its production and base material
JP1995133105A
Silica-based microparticle, method for producing dispersion with the same, and base material with coating film
JP2001233611A
Fine particle of noble metal and manufacturing method therefor
JP2004043892A
Conductive, fibrous, hollow silica particulate dispersoid and method for producing the same
JP2009143754A
Hollow silica particle