Interlayer film for laminated glass, roll body, and method for producing laminated glass

The interlayer film for laminated glass, featuring printed marks for alignment and identification, addresses the challenge of incorrect combinations in manufacturing, enhancing efficiency and reducing waste and performance issues.

JP7557366B2Active Publication Date: 2024-09-27SEKISUI CHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020526158
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-28
Filing Date
2019-12-20
Publication Date
2024-09-27
Estimated Expiration
2039-12-20

AI Technical Summary

Technical Problem

The manufacturing process of laminated glass is hindered by the difficulty in distinguishing between interlayer films, leading to incorrect combinations with laminated glass members, increased waste due to trim cutting, and potential performance or appearance issues such as double images and variations in shade areas.

Method used

An interlayer film for laminated glass is introduced with a printed mark or product information on its surface to guide accurate positioning and identification, enhancing manufacturing efficiency and reducing waste.

Benefits of technology

The printed interlayer film improves the manufacturing efficiency of laminated glass by ensuring correct alignment and reducing discarded material, while minimizing performance issues like double images and shade area variations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557366000014
    Figure 0007557366000014
  • Figure 0007557366000008
    Figure 0007557366000008
  • Figure 0007557366000012
    Figure 0007557366000012
Patent Text Reader

Abstract

Provided is an interlayer film for laminated glass that can improve the manufacturing efficiency of laminated glass. The interlayer film for laminated glass according to the present invention comprises an interlayer film for laminated glass main body and a printed portion printed on a first surface of the interlayer film for laminated glass main body, the printed portion being a mark for indicating the bonding position to a laminated glass component or product information about the interlayer film for laminated glass.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an interlayer film for laminated glass used to obtain laminated glass. The present invention also relates to a roll using the interlayer film for laminated glass and a method for producing laminated glass using the interlayer film for laminated glass. [Background technology]

[0002] Laminated glass generally has excellent safety because even if it is broken by an external impact, the amount of glass fragments scattered is small. For this reason, the laminated glass is widely used in automobiles, railway vehicles, aircraft, ships, buildings, etc. The laminated glass is produced by sandwiching an interlayer film for laminated glass between a pair of glass plates.

[0003] For example, the laminated glass is used as a windshield and side glass of an automobile. A head-up display (HUD) is known as the laminated glass used in an automobile. The HUD can display measurement information such as speed, which is the driving data of the automobile, on the windshield of the automobile, and the driver can recognize the display as if it is being projected in front of the windshield.

[0004] The following Patent Document 1 discloses an interlayer film for laminated glass used in laminated glass that is a head-up display. This interlayer film contains a thermoplastic resin, has one end and another end opposite to the one end and having a thickness greater than the one end, and has a display-corresponding area corresponding to the display area of ​​the head-up display. In this interlayer film, the display-corresponding area and a surrounding area adjacent to the display-corresponding area are visually distinguishable, or the color or gloss of the display-corresponding area is different from the color or gloss of the surrounding area adjacent to the display-corresponding area. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] WO2017 / 039004A1 Summary of the Invention [Problem to be solved by the invention]

[0006] Laminated glass is produced by bonding a laminated glass member and an interlayer film together, and then trimming off any part of the interlayer film that protrudes from the edge of the laminated glass member (trim cut).

[0007] In the manufacturing process of laminated glass, the laminated glass member and the interlayer film must be used in an appropriate combination. However, the appearance of multiple interlayer films is often similar, and it can be difficult to distinguish the interlayer film during manufacturing. Taking advantage of the difficulty in distinguishing between interlayer films, some companies have taken advantage of the fact that it is difficult to distinguish between interlayer films by replacing the labels of other companies' products and selling counterfeit products.

[0008] In the manufacturing process of the laminated glass, it is desirable to bond the laminated glass member and the interlayer film at an appropriate position. If the laminated glass member and the interlayer film are not bonded at an appropriate position, the amount of the interlayer film discarded by trimming may increase, or the manufactured laminated glass may have defects in performance or appearance.

[0009] For example, when the interlayer film has a shade region, the position, width, etc. of the shade region may vary among the laminated glasses produced. In particular, when producing laminated glasses having asymmetrical shapes such as side glass, the position, width, etc. of the shade region are likely to vary.

[0010] In addition, a wedge-shaped interlayer film may be used as an interlayer film for HUDs. Double images can be effectively suppressed by aligning the display corresponding area of ​​the interlayer film, whose wedge angle has been adjusted, with the display corresponding area of ​​the laminated glass member. However, even if the wedge angle of the interlayer film is adjusted, if the laminated glass member and the interlayer film are not bonded together in an appropriate position, a misalignment between these display corresponding areas may occur, resulting in double images. In particular, a wedge-shaped interlayer film having a portion where the amount of increase in thickness changes from one end to the other end is prone to double images due to the misalignment between the display corresponding areas.

[0011] As described above, if the laminated glass components and the interlayer film are not used in an appropriate combination or are not attached to each other in an appropriate position, the manufacturing efficiency of the laminated glass will decrease.

[0012] An object of the present invention is to provide an interlayer film for laminated glass that can improve the production efficiency of laminated glass. Another object of the present invention is to provide a roll using the interlayer film for laminated glass, and a method for producing laminated glass using the interlayer film for laminated glass. [Means for solving the problem]

[0013] According to a broad aspect of the present invention, there is provided an interlayer film for laminated glass (in this specification, "interlayer film for laminated glass" may be abbreviated to "interlayer film") comprising an interlayer film for laminated glass main body and a printed portion displayed by printing on a first surface of the interlayer film for laminated glass main body, the printed portion being a marker for a bonding position to a laminated glass component or product information about the interlayer film for laminated glass.

[0014] In a specific aspect of the interlayer film according to the present invention, the printed portion serves as a marker for indicating a position for bonding to a laminated glass member.

[0015] In a specific aspect of the interlayer film according to the present invention, the printed portion is displayed as a line, a letter, a symbol, or a graphic.

[0016] In a specific aspect of the interlayer film according to the present invention, the printed portion has a portion displayed as a line having a line width of 10 mm or less.

[0017] In a specific aspect of the interlayer film according to the present invention, the printed portion is displayed by UV laser printing.

[0018] In a specific aspect of the interlayer film according to the present invention, the interlayer film has one end and another end opposite the one end, the thickness of the other end is greater than the thickness of the one end, and the wedge angle of the entire interlayer film is 0.1 mrad or more.

[0019] In a specific aspect of the interlayer film according to the present invention, the interlayer film is an interlayer film for laminated glass used in laminated glass that is a head-up display, and has a display corresponding area that corresponds to the display area of ​​the head-up display.

[0020] In a specific aspect of the interlayer film according to the present invention, the interlayer film has a shaded area.

[0021] In a specific aspect of the interlayer film according to the present invention, the interlayer film is used in a front glass, a side glass, a rear glass, or a roof glass of a vehicle.

[0022] According to a broad aspect of the present invention, there is provided a roll body including a winding core and the above-mentioned interlayer film for laminated glass, the interlayer film for laminated glass being wound around an outer periphery of the winding core.

[0023] According to a broad aspect of the present invention, there is provided a method for producing laminated glass comprising a first laminated glass member, a second laminated glass member, and an interlayer film for laminated glass disposed between the first laminated glass member and the second laminated glass member, the method comprising a first arranging step of arranging the first laminated glass member on a first surface of the interlayer film for laminated glass described above, and a second arranging step of arranging the second laminated glass member on a second surface of the interlayer film for laminated glass opposite to the first surface, in which in the first arranging step, the first laminated glass member and the interlayer film for laminated glass are bonded together using the printed portion of the interlayer film for laminated glass as a mark, or in the second arranging step, the second laminated glass member and the interlayer film for laminated glass are bonded together using the printed portion of the interlayer film for laminated glass as a mark. Effect of the Invention

[0024] The interlayer film for laminated glass according to the present invention comprises an interlayer film for laminated glass main body, and a printed portion displayed by printing on a first surface of the interlayer film for laminated glass main body. In the interlayer film according to the present invention, the printed portion is a mark for the bonding position to the laminated glass component, or is product information about the interlayer film for laminated glass. Since the interlayer film for laminated glass according to the present invention has the above configuration, it is possible to increase the manufacturing efficiency of laminated glass. [Brief description of the drawings]

[0025] [Figure 1] 1(a) and 1(b) are a cross-sectional view and a front view that typically show an interlayer film for laminated glass according to a first embodiment of the present invention. [Diagram 2] 2(a) and (b) are a cross-sectional view and a front view that typically show an interlayer film for laminated glass according to a second embodiment of the present invention. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates an interlayer film for laminated glass according to a third embodiment of the present invention. [Figure 4]FIG. 4 is a cross-sectional view that illustrates a schematic diagram of an interlayer film for laminated glass according to a fourth embodiment of the present invention. [Diagram 5] FIG. 5 is a cross-sectional view that illustrates an interlayer film for laminated glass according to a fifth embodiment of the present invention. [Figure 6] FIG. 6 is a cross-sectional view that illustrates a schematic diagram of an interlayer film for laminated glass according to a sixth embodiment of the present invention. [Figure 7] 7(a) and (b) are a cross-sectional view and a front view that typically show an interlayer film for laminated glass according to a seventh embodiment of the present invention. [Figure 8] 8(a) and 8(b) are a cross-sectional view and a front view that typically show an interlayer film for laminated glass according to an eighth embodiment of the present invention. [Figure 9] FIG. 9 is a cross-sectional view that illustrates a modified example of the interlayer film for laminated glass according to the first embodiment of the present invention. [Figure 10] FIG. 10 is a cross-sectional view showing an example of laminated glass using the interlayer film for laminated glass shown in FIG. [Figure 11] FIG. 11 is a perspective view that typically illustrates a roll around which the interlayer film for laminated glass shown in FIG. 1 is wound. [Figure 12] FIG. 12 is a diagram for explaining a preliminary pressing method in the evaluation of double images in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The present invention will be described in detail below.

[0027] The interlayer film for laminated glass according to the present invention (sometimes abbreviated as "interlayer film" in this specification) is used for laminated glass.

[0028] The interlayer film according to the present invention comprises an interlayer film for laminated glass (sometimes abbreviated as "interlayer film body" in this specification) and a printed portion displayed by printing on a first surface of the interlayer film for laminated glass body. The interlayer film body includes the portion of the interlayer film excluding the printed portion. In the interlayer film according to the present invention, the printed portion is a marker for the bonding position to a laminated glass component, or is product information about the interlayer film for laminated glass.

[0029] The printed portion may be a marker for the bonding position to the laminated glass component, or may be product information about the interlayer film for laminated glass, or may be both a marker for the bonding position to the laminated glass component and product information about the interlayer film for laminated glass.

[0030] The interlayer film according to the present invention has the above-mentioned features, and therefore can improve the efficiency of laminated glass production. The interlayer film according to the present invention has the above-mentioned features, and therefore can easily distinguish the interlayer film, reduce the amount of interlayer film discarded by trim cutting, and improve the performance or appearance of the manufactured laminated glass.

[0031] The printed portion is preferably displayed as a line, a letter, a symbol or a graphic.

[0032] The intermediate film body has a one-layer structure or a two or more layer structure. The intermediate film body may have a one-layer structure, a two-layer structure, or a two or more layer structure. The intermediate film body may have a three-layer structure, or a three or more layer structure. The intermediate film body may be a single-layer intermediate film body, or a multi-layer intermediate film body. The number of layers of the intermediate film body is the same as the number of layers of the intermediate film.

[0033] The printed portion may be provided only on the first surface of the intermediate film body, or may be provided on the first surface and on a second surface opposite to the first surface of the intermediate film body. The intermediate film may have the printed portion on the first surface of the intermediate film, or may have the printed portion on the first surface of the intermediate film and on a second surface opposite to the first surface of the intermediate film.

[0034] The printed portion and the interlayer film body are preferably distinguishable by visual inspection. In this case, the printed portion and the interlayer film body may be distinguishable by visual inspection under normal conditions (e.g., under fluorescent lamp irradiation), or may be distinguishable by visual inspection when irradiated with light of a specific wavelength. The printed portion and the interlayer film body may not be distinguishable by visual inspection under normal conditions, but may be distinguishable by visual inspection when irradiated with light of a specific wavelength. In particular, when the printed portion and the interlayer film body are distinguishable by visual inspection when irradiated with light of a specific wavelength, even after the laminated glass is manufactured, product information of the interlayer film and the laminated glass can be tracked by irradiating the laminated glass with light of a specific wavelength.

[0035] Whether or not the printed portion and the intermediate film body are visually distinguishable is determined by whether or not a person with normal eyesight (e.g., 1.0 eyesight) can distinguish between the printed portion and the intermediate film body when visually observing the first surface of the intermediate film (the surface having the printed portion) from a position 70 cm away from the first surface.

[0036] The printed portion is an area in which lines, letters, symbols, figures, etc. are printed. Therefore, the printed portion is different from an area in which the glossiness is changed by embossing the surface of the interlayer film, and the printed portion is different from a colored portion in an interlayer film formed from a resin composition containing a colorant, etc.

[0037] The printed portion is a mark for indicating the position for bonding to the laminated glass member or product information for the interlayer film for laminated glass, and is therefore different from a printed portion formed for design purposes.

[0038] The printed part may have lines, characters, symbols, or figures. The printed part may be a combination of lines, characters, symbols, and figures. Examples of figures include circular, triangular, rectangular, and dotted figures. The printed part may have a barcode, a two-dimensional code, or the like. Examples of the two-dimensional code include QR Code (registered trademark).

[0039] The printed portion preferably has a line as a marker for the bonding position to the laminated glass member.The printed portion preferably has a portion displayed as a line as a marker for the bonding position to the laminated glass member.

[0040] Examples of the lines include lines (markers) for alignment with the edges of the laminated glass member, and lines (markers) for alignment of the HUD area.

[0041] The position where the lines for alignment with the edge of the laminated glass member are printed and the position where the lines for alignment with the HUD area are printed may be changed as appropriate depending on the size of the laminated glass member used.

[0042] The above-mentioned line may be a straight line, a broken line, or a curved line. Furthermore, the above-mentioned line may be a solid line, a dotted line, or a wavy line.

[0043] The line width of the line is preferably 0.01 mm or more, more preferably 0.1 mm or more. The line width of the line is preferably 330 mm or less, more preferably 300 mm or less, even more preferably 250 mm or less, even more preferably 200 mm or less, even more preferably 150 mm or less, even more preferably 100 mm or less, particularly preferably 10 mm or less, and most preferably 5 mm or less. When the line width is equal to or greater than the lower limit and equal to or less than the upper limit, the discrimination of the printed portion can be improved, and the lamination to the laminated glass member can be facilitated.

[0044] The above-mentioned printed portion as product information of the interlayer film for laminated glass is preferably displayed as lines, letters, symbols, or figures.

[0045] The product information may include a manufacturer's name, a product name, a trademark, a lot number, a bar code, a two-dimensional code, etc. The product information may be displayed in the form of a printed portion by using lines, letters, symbols, figures, or a combination of these.

[0046] The color of the printed portion is not particularly limited, and examples thereof include white, black, red, blue, yellow, and green. The printed portion may be translucent. Translucent means that the printed portion is not completely transparent and can be seen through. The printed portion may be colorless under a normal light source (e.g., under fluorescent light) and may emit light when irradiated with light of a specific wavelength.

[0047] The printed portion may or may not be removed by trim cutting during the production of the laminated glass. If the printed portion is completely removed by trim cutting, the printed portion will not be present in the interlayer film of the produced laminated glass. The printed portion is preferably removed by trim cutting during the production of the laminated glass. If the printed portion is not removed by trim cutting, the printed portion will be present in the interlayer film of the produced laminated glass.

[0048] Methods for forming the printed portion include laser printing, inkjet printing, magic marker printing, labeler printing, and the like.

[0049] The printed portion is preferably a printed portion displayed by laser printing, inkjet printing or labeler printing, more preferably a printed portion displayed by laser printing or inkjet printing, and even more preferably a printed portion displayed by laser printing. The laser printing is preferably UV laser printing. If the printed portion is a printed portion displayed by laser printing such as UV laser printing, the printed portion is easily erased due to the influence of heat and pressure applied during the production of the laminated glass, and as a result, the printed portion can be made difficult to see in the laminated glass. If the printed portion is a printed portion that is colorless under a normal light source and emits light when irradiated with light of a specific wavelength, the printed portion is preferably a printed portion displayed by inkjet printing. A printed portion having such properties can be displayed by inkjet printing a fluorescent toner such as "Lynx UV Fluorescent Ink 1121" manufactured by Almark Co., Ltd.

[0050] It is preferable that the printed portion can be made invisible by heating. When the laminated glass is formed by thermocompression bonding, it is preferable that the printed portion can be made invisible by heating during thermocompression bonding. It is preferable that the printed portion can be made invisible by heating at 70°C or higher. It is more preferable that the printed portion can be made invisible by heating at 120°C or higher.

[0051] An example of a commercially available device that can be used for the UV laser printing is the "MD-U1000C" manufactured by Keyence Corporation.

[0052] Commercially available devices that can be used for the inkjet printing include the MK-U6000 manufactured by Keyence Corp. Commercially available devices that can inkjet print fluorescent toner include the LINX 7900 manufactured by Almark Corp.

[0053] An example of a commercially available device that can be used for the above magic marker printing is "AMK-Magic LL" manufactured by Ayaha Engineering Co., Ltd.

[0054] An example of a commercially available device that can be used for the label printing is "AMK-Clean" manufactured by Ayaha Engineering Co., Ltd.

[0055] When the laminated glass is subjected to the light irradiation test described below, it is preferable that there is no difference in the luminance of the shadow cast by the area of ​​the interlayer film in the laminated glass that corresponds to the above-mentioned printed portion.

[0056] Light irradiation test: Prepare an interlayer film that is 30 cm long and 15 cm wide. The vertical direction is preferably the TD direction of the interlayer film, and the horizontal direction is preferably the MD direction of the interlayer film. Prepare a first clear glass having a thickness of 2 mm conforming to JIS R3202:2011 and a second clear glass having a thickness of 2 mm conforming to JIS R3202:2011. The interlayer film is sandwiched between the first clear glass and the second clear glass so that the printed portion of the interlayer film is located on the first clear glass side, and is pre-pressed under conditions of 240°C and a linear pressure of 98 N / cm. Then, the laminated glass is obtained by pressing under conditions of 140°C and a pressure of 1.3 MPa. A strong light source device is installed at a height of 80 cm from the floor, facing perpendicular to the floor, at an angle of 15 degrees from the floor. The laminated glass is placed at a position 175 cm away from the strong light source device and with the center of the laminated glass 1 m above the floor, so that the surface direction of the laminated glass is perpendicular to the irradiation direction of the strong light source and the first clear glass side of the laminated glass faces the strong light source. Light is irradiated onto the laminated glass from the strong light source, and an inspector with 1.0 eyesight visually checks the shadow projected by the area of ​​the interlayer film of the laminated glass corresponding to the above-mentioned printed part 25 cm behind the laminated glass, and judges whether there is a difference in the brightness of the shadow.

[0057] In the light irradiation test, when the printed portion is provided on both the first and second surfaces of the interlayer film body and different luminance values ​​are obtained on both sides of the laminated glass, the laminated glass is obtained in a specific positional relationship, i.e., the printed portion that provides a higher luminance value is positioned on the first clear glass side, and the printed portion that provides a lower luminance value is positioned on the second clear glass side.

[0058] In the laminated glass used in the light irradiation test, the parallel light transmittance of the region of the interlayer film corresponding to the printed portion is preferably 60% or more, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 85% or more.

[0059] In the laminated glass used in the light irradiation test, the absolute value of the difference between the parallel light transmittance of the region of the interlayer corresponding to the printed portion and the parallel light transmittance of the region corresponding to the non-printed portion around the printed portion is preferably 15% or less, more preferably 10% or less, and even more preferably 5% or less. The non-printed portion around the printed portion means the region within 5 mm from the printed portion.

[0060] The parallel light transmittance is measured in accordance with JIS R3106:1998. Specifically, it is measured using a spectrophotometer in a state where the laminated glass is placed parallel to the normal to the optical axis on the optical path between the light source and the integrating sphere and at a point 13 cm away from the integrating sphere so that only the transmitted parallel light is received by the integrating sphere. The parallel light transmittance means the visible light transmittance calculated from the spectral transmittance measured in this state. An example of the spectrophotometer is the "U-4100" manufactured by Hitachi High-Tech Corporation.

[0061] The intermediate film preferably has one end and another end opposite to the one end, the one end and the other end being end portions on both sides facing each other in the intermediate film.

[0062] The interlayer film preferably has an MD direction and a TD direction. The interlayer film is obtained, for example, by melt extrusion molding. The MD direction is the flow direction of the interlayer film during production. The TD direction is a direction perpendicular to the flow direction of the interlayer film during production and perpendicular to the thickness direction of the interlayer film. The one end and the other end are preferably located on both sides of the TD direction.

[0063] In the interlayer film according to the present invention, the thickness of the other end may be the same as the thickness of the one end.In the interlayer film according to the present invention, the thickness of the other end may be greater than the thickness of the one end.An interlayer film having a greater thickness at the other end than the thickness at the one end is a wedge-shaped interlayer film.

[0064] The interlayer film according to the present invention may have a display corresponding area corresponding to the display area of ​​a head-up display. The display corresponding area is an area in which information can be displayed satisfactorily.

[0065] The display corresponding region preferably has a length direction and a width direction. Since the interlayer film has excellent versatility, the width direction of the display corresponding region is preferably a direction connecting the one end and the other end. The display corresponding region is preferably strip-shaped.

[0066] From the viewpoint of suppressing double images, the interlayer film is preferably a wedge-shaped interlayer film.

[0067] From the viewpoint of further suppressing double images, the interlayer preferably has a portion whose cross-sectional shape in the thickness direction is wedge-shaped. The interlayer preferably has a portion whose thickness gradually increases from one end to the other end. The interlayer preferably has a wedge-shaped cross-sectional shape in the thickness direction of the display-corresponding region. Examples of the cross-sectional shape in the thickness direction of the interlayer include a trapezoid, a triangle, and a pentagon.

[0068] From the viewpoint of further suppressing ghost images, it is preferable that the interlayer has a portion in which the amount of increase in thickness increases from one end side to the other end side in the region where the thickness increases. From the viewpoint of further suppressing ghost images, it is preferable that the interlayer has a portion in which the wedge angle increases from one end side to the other end side in the region where the cross-sectional shape in the thickness direction is wedge-shaped.

[0069] When the interlayer film according to the present invention is a wedge-shaped interlayer film, from the viewpoint of effectively suppressing ghost images, the wedge angle of the entire interlayer film is preferably 0.1 mrad (0.00575 degrees) or more, more preferably 0.2 mrad (0.0115 degrees) or more, and is preferably 2 mrad (0.1146 degrees) or less, more preferably 0.7 mrad (0.0401 degrees) or less.

[0070] The wedge angle of the interlayer film is the interior angle at the intersection of a straight line connecting the first surface (one surface) of the interlayer film between the maximum and minimum thickness parts of the interlayer film, and a straight line connecting the second surface (the other surface) of the interlayer film between the maximum and minimum thickness parts of the interlayer film. Note that when there are multiple maximum thickness parts, multiple minimum thickness parts, the maximum thickness part is in a fixed region, or the minimum thickness part is in a fixed region, the maximum thickness part and the minimum thickness part for determining the wedge angle are selected so that the determined wedge angle is largest.

[0071] The measuring device used to measure the wedge angle of the interlayer and the thickness of the interlayer described below is, for example, a contact type thickness measuring device "TOF-4R" (manufactured by Yamabun Denki Co., Ltd.).

[0072] The thickness is measured using the above-mentioned measuring device at a membrane transport speed of 2.15 mm / min to 2.25 mm / min over the shortest distance from one end to the other end.

[0073] An example of a measuring device used to measure the wedge angle (θ) of the interlayer film after it has been formed into laminated glass and the thickness of the interlayer film described below is a non-contact multilayer film thickness measuring device (for example, "OPTIGAUGE" manufactured by Lumetrics, Inc.). When a non-contact multilayer film thickness measuring device is used, the thickness of the interlayer film can be measured in the form of laminated glass.

[0074] Even if the wedge angle of the interlayer film is adjusted to suppress double images, double images may still occur if there is a misalignment between the display-corresponding area of ​​the interlayer film and the display-corresponding area of ​​the laminated glass member. In the present invention, because the interlayer film is provided with the above-mentioned printed portion, the attachment position to the laminated glass member can be properly recognized and misalignment between the display-corresponding area of ​​the interlayer film and the display-corresponding area of ​​the laminated glass member can be effectively suppressed, resulting in effective suppression of double images.

[0075] When the interlayer film according to the present invention has the display corresponding area, it is preferable that the display corresponding area is located within a region extending from a position 18 cm from the one end toward the other end to a position 61.8 cm from the one end toward the other end. In this case, double images can be effectively suppressed.

[0076] When the interlayer film according to the present invention is a wedge-shaped interlayer film, it is preferable that the interlayer film has a portion whose cross section in the thickness direction is wedge-shaped in the region from a position 18 cm from the one end toward the other end to a position 61.8 cm from the one end toward the other end. In this case, ghosting can be effectively suppressed. Note that it is sufficient that the portion whose cross section in the thickness direction is wedge-shaped exists in at least a part of the region.

[0077] The interlayer film according to the present invention and the interlayer film body may have a shade region. The interlayer film according to the present invention may have the display corresponding region and the shade region. In this case, the shade region may be separated from the display corresponding region. The interlayer film according to the present invention may have the shade region without having the display corresponding region. The shade region is provided for the purpose of preventing the driver from feeling glare while driving due to, for example, sunlight or outdoor lighting. The shade region may be provided to provide heat insulation. The shade region is preferably located at the edge of the interlayer film. The shade region is preferably strip-shaped.

[0078] In the shade region, a colorant or a filler may be used to change the color and the visible light transmittance. The colorant or the filler may be contained in only a part of the region in the thickness direction of the interlayer film, or may be contained in the entire region in the thickness direction of the interlayer film. The shade region is different from the printed portion. The printed portion may be formed on the surface of the shade region.

[0079] In addition, when the interlayer film has a shade region, there may be variation in the position, width, etc. of the shade region among the multiple laminated glasses produced. In the present invention, since the interlayer film has the above-mentioned printed portion, the attachment position to the laminated glass member can be properly recognized and the positional deviation between the display-corresponding region of the interlayer film and the display-corresponding region of the laminated glass member can be effectively suppressed, and as a result, the variation in the position, width, etc. of the shade region can be effectively suppressed.

[0080] From the viewpoint of improving the display and widening the field of view, the visible light transmittance of the display corresponding area is preferably 80% or more, more preferably 88% or more, and even more preferably 90% or more. The visible light transmittance of the display corresponding area is preferably higher than that of the shade area. The visible light transmittance of the display corresponding area may be lower than that of the shade area. The visible light transmittance of the display corresponding area is preferably 50% or more higher, more preferably 60% or more higher than that of the shade area.

[0081] For example, when the visible light transmittance varies in the interlayer film in the display corresponding area and the shade area, the visible light transmittance is measured at the center position of the display corresponding area and the center position of the shade area.

[0082] The visible light transmittance of the obtained laminated glass at wavelengths of 380 nm to 780 nm can be measured using a spectrophotometer (Hitachi High-Technologies Corporation's "U-4100") in accordance with JIS R3211: 1998. It is preferable to use, as the glass plate, clear glass having a thickness of 2 mm in accordance with JIS R3202: 2011.

[0083] Hereinafter, specific embodiments of the present invention will be described with reference to the drawings.

[0084] 1(a) and (b) are a cross-sectional view and a front view showing a schematic diagram of an interlayer film for laminated glass according to a first embodiment of the present invention. Fig. 1(a) is a cross-sectional view taken along line II in Fig. 1(b). Note that the sizes and dimensions of the interlayer film and printed parts in Fig. 1 and the figures described below have been appropriately altered from their actual sizes and shapes for the sake of convenience.

[0085] Fig. 1(a) shows a cross section in the thickness direction of the interlayer film 11. Note that, for convenience of illustration, in Fig. 1(a) and in the figures described below, the thickness and wedge angle (θ) of the interlayer film and each layer constituting the interlayer film are shown to be different from the actual thickness and wedge angle. Also, for convenience of illustration, printed parts are not shown in Fig. 1(a).

[0086] The interlayer film 11 shown in Fig. 1 comprises a first layer 1 (interlayer), a second layer 2 (surface layer), a third layer 3 (surface layer), and a printed portion 4. The first layer 1, the second layer 2, and the third layer 3 form an interlayer film body. The interlayer film body comprises the first layer 1, the second layer 2, and the third layer 3. The third layer 3 has a colored portion 3X that contains a colorant, and a non-colored portion 3Y that does not contain a colorant.

[0087] A second layer 2 is disposed on a first surface side of the first layer 1 and laminated thereon. A third layer 3 is disposed on a second surface side opposite to the first surface of the first layer 1 and laminated thereon. The first layer 1 is disposed and sandwiched between the second layer 2 and the third layer 3. The interlayer film 11 is used to obtain laminated glass. The interlayer film 11 is an interlayer film for laminated glass. The interlayer film 11 has a three-layer structure and is a multilayer interlayer film.

[0088] The intermediate film 11 has one end 11a and the other end 11b opposite to the one end 11a. The one end 11a and the other end 11b are end portions on both sides facing each other. The cross-sectional shape in the thickness direction of the second layer 2 and the third layer 3 is wedge-shaped. The cross-sectional shape in the thickness direction of the first layer 1 is rectangular. The second layer 2 and the third layer 3 are thicker on the other end 11b side than on the one end 11a side. Therefore, the thickness of the other end 11b of the intermediate film 11 is thicker than the thickness of the one end 11a. Therefore, the intermediate film 11 has a thin region and a thick region. Also, the thickness of the colored portion 3X is thicker on the other end 11b side than on the one end 11a side.

[0089] The intermediate film 11 has a region where the thickness increases from one end 11a to the other end 11b. In the region where the thickness increases, the amount of increase in thickness of the intermediate film 11 is uniform from one end 11a to the other end 11b.

[0090] The intermediate film 11 has a display corresponding region R1 corresponding to the display region of the head-up display. The intermediate film 11 has a surrounding region R2 adjacent to the display corresponding region R1. In this embodiment, the display corresponding region R1 is a region from a position 18 cm from one end 11a toward the other end 11b to a position 63.8 cm from one end 11a toward the other end 11b.

[0091] The intermediate film 11 has a shaded region R3 separate from the display corresponding region R1. The shaded region R3 is located at the edge of the intermediate film 11. The shaded region R3 corresponds to the region where the colored portion 3X exists.

[0092] A printed portion 4 is formed on the surface of the interlayer film body. The printed portion 4 is displayed by printing on the surface of the interlayer film body. The printed portion 4 is a mark for indicating the bonding position to the laminated glass member G1. The printed portion 4 has two solid lines 4a and two dotted lines 4b. The area between the two dotted lines 4b corresponds to the display corresponding area R1 of the interlayer film 11. The two solid lines 4a are a mark for alignment with the edge of the laminated glass member G1. The two dotted lines 4b are a mark for alignment of the HUD area.

[0093] The laminated glass can be produced satisfactorily by bonding the interlayer film 11 to the laminated glass member G1 while aligning the two solid lines 4a with the ends of the laminated glass member G1 and the two dotted lines 4b with the display-compatible area of ​​the laminated glass member G1.

[0094] The interlayer film may have a shape as shown in Fig. 1(a) and may be a single layer, two layers, or four or more layers. Fig. 9 is a cross-sectional view that typically shows a modified example of the interlayer film for laminated glass according to the first embodiment of the present invention, that is, a modified example of the interlayer film 11. As in the interlayer film 11-2 shown in Fig. 9, the shade region R3 may be formed without partially forming the colored portion 3X containing a colorant. In addition, the interlayer film may have a shape as shown in Figs. 1(a) and 12 and the shade region R3 may be a region that is not a shade region or may be a transparent region.

[0095] FIG. 11 is a perspective view that typically illustrates a roll around which the interlayer film for laminated glass shown in FIG. 1 is wound.

[0096] The interlayer film 11 may be wound into a roll 51 of the interlayer film 11 .

[0097] 11 includes a winding core 61 and an intermediate film 11. The intermediate film 11 is wound around the outer periphery of the winding core 61.

[0098] 2(a) and (b) are a cross-sectional view and a front view, respectively, that show a schematic diagram of an interlayer film for laminated glass according to a second embodiment of the present invention. FIG. 2(a) is a cross-sectional view taken along line II in FIG. 2(b). FIG. 2(a) shows a cross section in the thickness direction of the interlayer film 11A. For convenience of illustration, FIG. 2(a) does not show the printed portion.

[0099] The interlayer film 11A shown in FIG. 2 includes a first layer 1A and a printed portion 4A. The first layer 1A constitutes an interlayer film body. The interlayer film body is the first layer 1A. The interlayer film 11A has a one-layer structure consisting of only the first layer 1A. The interlayer film 11A is a single-layer interlayer film. The interlayer film 11A is used to obtain laminated glass. The interlayer film 11A is an interlayer film for laminated glass. The first layer 1A also has a colored portion 1AX that contains a colorant and a non-colored portion 1AY that does not contain a colorant.

[0100] The intermediate film 11A has one end 11a and the other end 11b opposite the one end 11a. The one end 11a and the other end 11b are opposite ends. The thickness of the other end 11b of the intermediate film 11A is greater than the thickness of the one end 11a. Therefore, the intermediate film 11A and the first layer 1A have a thin region and a thick region. Also, the thickness of the colored portion 1AX is greater on the other end 11b side than on the one end 11a side.

[0101] The intermediate film 11A has a region where the thickness increases from one end 11a to the other end 11b. In the region where the thickness increases, the amount of increase in thickness of the intermediate film 11A is uniform from one end 11a to the other end 11b.

[0102] The intermediate film 11A and the first layer 1A have portions 11Aa, 1Aa whose cross-sectional shape in the thickness direction is rectangular, and portions 11Ab, 1Ab whose cross-sectional shape in the thickness direction is wedge-shaped.

[0103] The intermediate film 11A has a display corresponding region R1 corresponding to the display region of the head-up display. The intermediate film 11A has a surrounding region R2 adjacent to the display corresponding region R1.

[0104] The intermediate film 11A has a shade region R3 apart from the display corresponding region R1. The shade region R3 is located at the edge of the intermediate film 11A. The shade region R3 corresponds to the region where the colored portion 1AX is present.

[0105] A printed portion 4A is formed on the surface of the first layer 1A. The printed portion 4A is displayed by printing on the surface of the interlayer film body. The printed portion 4A is a mark for the bonding position to the laminated glass member G1A. The printed portion 4A has two dotted lines 4Ab. The two dotted lines 4b are marks for alignment with the edge of the laminated glass member G1A.

[0106] By aligning the two dotted lines 4Ab with the ends of the glass laminate member G1A and bonding the interlayer film 11A to the glass laminate member G1A, a good laminated glass can be produced.

[0107] The intermediate film may have two or more layers in the shape shown in Fig. 2(a). The colored portion 1AX containing the coloring agent may be partially left unformed in the shape shown in Fig. 2(a) to form the shaded region R3. The intermediate film may have the shape shown in Fig. 2(a) and the shaded region R3 may be a region that is not a shaded region or may be a transparent region.

[0108] Fig. 3 is a cross-sectional view showing a schematic diagram of an interlayer film for laminated glass according to a third embodiment of the present invention. Fig. 3 shows a cross section in the thickness direction of the interlayer film 11B. For convenience of illustration, printed portions are not shown in Fig. 3.

[0109] The intermediate film 11B shown in Fig. 3 includes a first layer 1B (intermediate layer), a second layer 2B (surface layer), a third layer 3B (surface layer), and a printed portion. The third layer 3B includes a colored portion 3BX that contains a colorant, and a non-colored portion 3BY that does not contain a colorant. The intermediate film 11 and the intermediate film 11B have different amounts of thickness increase in the areas where the thickness increases.

[0110] The intermediate film 11B has a region where the thickness increases from the one end 11a side to the other end 11b side. The intermediate film 11B has a portion where the increase in thickness increases from the one end 11a side to the other end 11b side in the region where the thickness increases. The intermediate film 11B also has a region where the cross-sectional shape in the thickness direction is wedge-shaped. The intermediate film 11B has a portion where the wedge angle increases from the one end side to the other end side in the region where the cross-sectional shape in the thickness direction is wedge-shaped. The shade region R3 may be formed in the shape shown in FIG. 3 without partially forming the colored portion 3BX containing the coloring agent. The intermediate film may have the shape shown in FIG. 3, and the shade region R3 portion may be a region that is not a shade region, or may be a transparent region.

[0111] Fig. 4 is a cross-sectional view showing a schematic diagram of an interlayer film for laminated glass according to a fourth embodiment of the present invention. Fig. 4 shows a cross section in the thickness direction of an interlayer film 11C. For convenience of illustration, printed portions are not shown in Fig. 4.

[0112] The intermediate film 11C shown in FIG. 4 comprises a first layer 1C which is an intermediate film main body, and a printed portion. The first layer 1C has a colored portion 1CX which contains a colorant, and a non-colored portion 1CY which does not contain a colorant. The intermediate film main body is constituted by the first layer 1C. The intermediate film 11C has a single-layer structure consisting of only the first layer 1C. The intermediate film 11C is a single-layer intermediate film. The amount of increase in thickness in the area where the thickness is increased is different between the intermediate film 11A and the intermediate film 11C.

[0113] The intermediate film 11C has a region where the thickness increases from one end 11a to the other end 11b. In the region where the thickness increases, the intermediate film 11C has a portion where the amount of increase in thickness increases from one end 11a to the other end 11b. The intermediate film 11C also has a region where the cross-sectional shape in the thickness direction is wedge-shaped. In the region where the cross-sectional shape in the thickness direction is wedge-shaped, the intermediate film 11C has a portion where the wedge angle increases from one end to the other end.

[0114] The intermediate film 11C and the first layer 1C have portions 11Ca, 1Ca whose cross-sectional shape in the thickness direction is rectangular and portions 11Cb, 1Cb whose cross-sectional shape in the thickness direction is wedge-shaped. In the shape shown in Fig. 4, the shaded region R3 may be formed without partially forming the colored portion 1CX containing a coloring agent. In addition, in the shape shown in Fig. 4, the shaded region R3 of the intermediate film may be a region that is not a shaded region or may be a transparent region.

[0115] Fig. 5 is a cross-sectional view showing a schematic diagram of an interlayer film for laminated glass according to a fifth embodiment of the present invention. Fig. 5 shows a cross section in the thickness direction of an interlayer film 11D. For convenience of illustration, printed portions are not shown in Fig. 5.

[0116] The intermediate film 11D shown in Fig. 5 includes a first layer 1D (intermediate layer), a second layer 2D (surface layer), a third layer 3D (surface layer), and a printed portion. The third layer 3D includes a colored portion 3DX that includes a colorant, and a non-colored portion 3DY that does not include a colorant. The intermediate film 11 and the intermediate film 11D have different amounts of thickness increase in the areas where the thickness increases.

[0117] The intermediate film 11D has a region where the thickness increases from the one end 11a side to the other end 11b side. The intermediate film 11D has a portion where the increase in thickness decreases from the one end 11a side to the other end 11b side in the region where the thickness increases. The intermediate film 11D also has a region where the cross-sectional shape in the thickness direction is wedge-shaped. The intermediate film 11D has a portion where the wedge angle decreases from the one end side to the other end side in the region where the cross-sectional shape in the thickness direction is wedge-shaped. The shade region R3 may be formed in the shape shown in FIG. 5 without partially forming the colored portion 3DX containing a coloring agent. The intermediate film may have a shape shown in FIG. 5, and the shade region R3 may be a region that is not a shade region or may be a transparent region.

[0118] Fig. 6 is a cross-sectional view showing a schematic diagram of an interlayer film for laminated glass according to a sixth embodiment of the present invention. Fig. 6 shows a cross section in the thickness direction of the interlayer film 11E. For convenience of illustration, printed portions are not shown in Fig. 6.

[0119] The intermediate film 11E shown in FIG. 6 includes a first layer 1E and a printed portion. The first layer 1E includes a colored portion 1EX that includes a colorant and a non-colored portion 1EY that does not include a colorant. The first layer 1E constitutes the intermediate film body. The intermediate film body is the first layer 1E. The intermediate film 11E has a single-layer structure including only the first layer 1E. The intermediate film 11E is a single-layer intermediate film. The intermediate film 11A and the intermediate film 11E differ in the amount of thickness increase in the region where the thickness is increased.

[0120] The intermediate film 11E has a region where the thickness increases from one end 11a to the other end 11b. In the region where the thickness increases, the intermediate film 11E has a portion where the increase in thickness decreases from one end 11a to the other end 11b. The intermediate film 11E also has a region where the cross-sectional shape in the thickness direction is wedge-shaped. In the region where the cross-sectional shape in the thickness direction is wedge-shaped, the intermediate film 11E has a portion where the wedge angle decreases from one end to the other end.

[0121] The intermediate film 11E and the first layer 1E have portions 11Ea, 1Ea whose cross-sectional shape in the thickness direction is rectangular and portions 11Eb, 1Eb whose cross-sectional shape in the thickness direction is wedge-shaped. In the shape shown in Fig. 6, the shaded region R3 may be formed without partially forming the colored portion 1EX containing a coloring agent. In addition, in the shape shown in Fig. 6, the shaded region R3 of the intermediate film may be a region that is not a shaded region or may be a transparent region.

[0122] 7(a) and (b) are a cross-sectional view and a front view showing an interlayer film for laminated glass according to a seventh embodiment of the present invention. Fig. 7(a) is a cross-sectional view taken along line II in Fig. 7(b). Fig. 7(a) shows a cross section in the thickness direction of the interlayer film 11F. For convenience of illustration, the printed portion is not shown in Fig. 7(a).

[0123] The interlayer film 11F shown in FIG. 7 includes a first layer 1F and a printed portion 4F. The first layer 1F constitutes an interlayer film main body. The interlayer film main body is the first layer 1F. The interlayer film 11F has a single-layer structure consisting of only the first layer 1F. The interlayer film 11F is a single-layer interlayer film. The interlayer film 11F is used to obtain laminated glass. The interlayer film 11F is an interlayer film for laminated glass.

[0124] The intermediate film 11F has one end 11a and the other end 11b opposite to the one end 11a. The one end 11a and the other end 11b are end portions on both sides facing each other. In the intermediate film 11F, the thickness of the other end 11b is the same as the thickness of the one end 11a.

[0125] A printed portion 4F is formed on the surface of the first layer 1F. The printed portion 4F is displayed by printing on the surface of the interlayer film body. In the printed portion 4A, the two dotted lines 4Fb mark the bonding position to the laminated glass member G1F, and the letters "ABCDE" 4Fc are product information of the interlayer film for laminated glass. Instead of letters, the printed portion may be product information such as symbols and figures. The printed portion may also be product information such as a two-dimensional code and a barcode.

[0126] By aligning the two dotted lines 4Fb with the display-corresponding area of ​​the glass laminate member G1F and bonding the interlayer film 11F to the glass laminate member G1F, a good laminated glass can be produced.

[0127] Figures 8(a) and (b) are a cross-sectional view and a front view, respectively, that show an interlayer film for laminated glass according to an eighth embodiment of the present invention. Figure 8(a) is a cross-sectional view taken along line II in Figure 8(b). Figure 8(a) shows a cross section in the thickness direction of the interlayer film 11G. For convenience of illustration, the printed portion is not shown in Figure 8(a).

[0128] The intermediate film 11G shown in Fig. 8 includes a first layer 1G (intermediate layer), a second layer 2G (surface layer), a third layer 3G (surface layer), and a printed portion 4G. The first layer 1G, the second layer 2G, and the third layer 3G form an intermediate film body. The intermediate film body includes the first layer 1G, the second layer 2G, and the third layer 3G. The third layer 3G has a colored portion 3GX that includes a colorant, and a non-colored portion 3GY that does not include a colorant.

[0129] A second layer 2G is disposed on a first surface side of the first layer 1G and laminated thereon. A third layer 3G is disposed on a second surface side opposite to the first surface of the first layer 1G and laminated thereon. The first layer 1G is disposed and sandwiched between the second layer 2G and the third layer 3G. The interlayer film 11G is used to obtain laminated glass. The interlayer film 11G is an interlayer film for laminated glass. The interlayer film 11G has a three-layer structure and is a multilayer interlayer film.

[0130] The intermediate film 11G has one end 11a and the other end 11b on the opposite side to the one end 11a. The one end 11a and the other end 11b are opposite ends. In the intermediate film 11G, the thickness of the other end 11b is the same as the thickness of the one end 11a. Moreover, the thickness of the colored portion 3GX is smaller on the other end 11b side than on the one end 11a side.

[0131] The intermediate film 11G has a shaded region R3. The shaded region R3 is located at the edge of the intermediate film 11G. The shaded region R3 corresponds to the region where the colored portion 3GX is present.

[0132] A printed portion 4G is formed on the surface of the interlayer film body. The printed portion 4G is displayed by printing on the surface of the interlayer film body. The printed portion 4G is a mark for the bonding position to the laminated glass member G1G. The printed portion 4G has two solid lines 4Ga. The two solid lines 4Ga are a mark for alignment with the edge of the laminated glass member G1G.

[0133] By aligning the two solid lines 4Ga with the ends of the glass laminate member G1G and attaching the interlayer film 11G to the glass laminate member G1G, a good laminated glass can be produced.

[0134] The intermediate film may be a single layer, two layers, or four or more layers in the shape shown in Fig. 8(a). The shade region R3 may be formed without forming a part of the colored portion 3GX containing a coloring agent in the shape shown in Fig. 8(a). Also, the intermediate film may be a non-shade region or a transparent region in the shape shown in Fig. 8(a).

[0135] The thickness of the interlayer film is not particularly limited. The thickness of the interlayer film indicates the total thickness of each layer constituting the interlayer film. Therefore, in the case of a multi-layer interlayer film 11, the thickness of the interlayer film indicates the total thickness of the first layer 1, the second layer 2, and the third layer 3.

[0136] The maximum thickness of the intermediate film is preferably 0.1 mm or more, more preferably 0.25 mm or more, even more preferably 0.5 mm or more, particularly preferably 0.8 mm or more, and is preferably 3 mm or less, more preferably 2 mm or less, and even more preferably 1.5 mm or less.

[0137] The distance between one end and the other end of the interlayer film is designated as X. The interlayer film preferably has a minimum thickness in a region of 0X to 0.2X from one end toward the inside, and a maximum thickness in a region of 0X to 0.2X from the other end toward the inside. It is more preferable that the interlayer film has a minimum thickness in a region of 0X to 0.1X from one end toward the inside, and a maximum thickness in a region of 0X to 0.1X from the other end toward the inside. It is preferable that the interlayer film has a minimum thickness at one end, and a maximum thickness at the other end.

[0138] The intermediate films 11, 11A, 11B, 11C, 11D, and 11E have a maximum thickness at the other end 11b and a minimum thickness at the one end 11a.

[0139] From the viewpoint of practical use and from the viewpoint of sufficiently increasing adhesive strength and penetration resistance, the maximum thickness of the surface layer is preferably 0.001 mm or more, more preferably 0.2 mm or more, even more preferably 0.3 mm or more, and is preferably 1 mm or less, more preferably 0.8 mm or less.

[0140] From the viewpoint of practical use and from the viewpoint of sufficiently increasing the penetration resistance, the maximum thickness of the layer (intermediate layer) disposed between the two surface layers is preferably 0.001 mm or more, more preferably 0.1 mm or more, even more preferably 0.2 mm or more, and is preferably 0.8 mm or less, more preferably 0.6 mm or less, even more preferably 0.3 mm or less.

[0141] The distance X between one end and the other end of the intermediate film is preferably 0.5 m or more, more preferably 0.8 m or more, and even more preferably 1 m or more, and is preferably 3 m or less, more preferably 2 m or less, and even more preferably 1.5 m or less.

[0142] After preparing a pre-printed intermediate film (an intermediate film without a printed portion), the intermediate film having the intermediate film body and the printed portion can be manufactured by printing lines, letters, symbols, figures, etc. on the surface of the pre-printed intermediate film to form a printed portion.

[0143] The printed portion may be formed of a composition different from the composition for forming the interlayer film body. The composition for forming the printed portion may contain a colorant. Examples of the colorant include dyes and pigments.

[0144] The materials constituting each layer of the multi-layer interlayer film, and the interlayer film body in the case of a single-layer interlayer film, will be described in detail below.

[0145] (thermoplastic resin) The intermediate film preferably contains a thermoplastic resin. The intermediate film preferably contains a polyvinyl acetal resin as a thermoplastic resin. The intermediate film body preferably contains a thermoplastic resin (hereinafter may be referred to as a thermoplastic resin (0)). The intermediate film body preferably contains a polyvinyl acetal resin (hereinafter may be referred to as a polyvinyl acetal resin (0)) as a thermoplastic resin (0). The printed portion may contain a thermoplastic resin. The printed portion may contain a polyvinyl acetal resin. The thermoplastic resin contained in the intermediate film body and the thermoplastic resin contained in the printed portion may be the same or different. The first layer preferably contains a thermoplastic resin (hereinafter may be referred to as a thermoplastic resin (1)). The first layer preferably contains a polyvinyl acetal resin (hereinafter may be referred to as a polyvinyl acetal resin (1)) as a thermoplastic resin (1). The second layer preferably contains a thermoplastic resin (hereinafter may be referred to as a thermoplastic resin (2)). The second layer preferably contains a polyvinyl acetal resin (hereinafter, may be referred to as polyvinyl acetal resin (2)) as the thermoplastic resin (2). The third layer preferably contains a thermoplastic resin (hereinafter, may be referred to as thermoplastic resin (3)). The third layer preferably contains a polyvinyl acetal resin (hereinafter, may be referred to as polyvinyl acetal resin (3)) as the thermoplastic resin (3). The thermoplastic resin (1), the thermoplastic resin (2), and the thermoplastic resin (3) may be the same or different. Since sound insulation is further improved, the thermoplastic resin (1) is preferably different from the thermoplastic resin (2) and the thermoplastic resin (3). The polyvinyl acetal resin (1), the polyvinyl acetal resin (2), and the polyvinyl acetal resin (3) may be the same or different. Since the sound insulation property is further improved, it is preferable that the polyvinyl acetal resin (1) is different from the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3).The thermoplastic resin (0), the thermoplastic resin (1), the thermoplastic resin (2), and the thermoplastic resin (3) may each be used alone or in combination of two or more thereof. The polyvinyl acetal resin (0), the polyvinyl acetal resin (1), the polyvinyl acetal resin (2), and the polyvinyl acetal resin (3) may each be used alone or in combination of two or more thereof.

[0146] Examples of the thermoplastic resin include polyvinyl acetal resin, ethylene-vinyl acetate copolymer resin, ethylene-acrylic acid copolymer resin, polyurethane resin, (meth)acrylic resin, polyolefin resin, polyvinyl alcohol resin, etc. Thermoplastic resins other than these may also be used.

[0147] The thermoplastic resin is preferably a polyvinyl acetal resin. By using the polyvinyl acetal resin in combination with a plasticizer, the adhesive strength of the layer containing the polyvinyl acetal resin and the plasticizer to the laminated glass member or other layer is further increased.

[0148] The polyvinyl acetal resin can be produced, for example, by acetalizing polyvinyl alcohol (PVA) with an aldehyde. The polyvinyl acetal resin is preferably an acetalized product of polyvinyl alcohol. The polyvinyl alcohol can be obtained, for example, by saponifying polyvinyl acetate. The degree of saponification of the polyvinyl alcohol is generally within the range of 70 mol% to 99.9 mol%.

[0149] The average degree of polymerization of the polyvinyl alcohol (PVA) is preferably 200 or more, more preferably 500 or more, even more preferably 1500 or more, even more preferably 1600 or more, particularly preferably 2600 or more, most preferably 2700 or more, and preferably 5000 or less, more preferably 4000 or less, and even more preferably 3500 or less. When the average degree of polymerization is equal to or more than the lower limit, the penetration resistance of the laminated glass is further improved. When the average degree of polymerization is equal to or less than the upper limit, the interlayer film is easily formed.

[0150] The average degree of polymerization of the polyvinyl alcohol is determined by a method in accordance with JIS K6726 "Testing method for polyvinyl alcohol."

[0151] The number of carbon atoms in the acetal group contained in the polyvinyl acetal resin is not particularly limited. The aldehyde used in producing the polyvinyl acetal resin is not particularly limited. The number of carbon atoms in the acetal group in the polyvinyl acetal resin is preferably 3 to 5, and more preferably 3 or 4. When the number of carbon atoms in the acetal group in the polyvinyl acetal resin is 3 or more, the glass transition temperature of the interlayer film becomes sufficiently low.

[0152] The aldehyde is not particularly limited. In general, an aldehyde having 1 to 10 carbon atoms is preferably used. Examples of the aldehyde having 1 to 10 carbon atoms include propionaldehyde, n-butylaldehyde, isobutyraldehyde, n-valeraldehyde, 2-ethylbutyraldehyde, n-hexylaldehyde, n-octylaldehyde, n-nonylaldehyde, n-decylaldehyde, formaldehyde, acetaldehyde, and benzaldehyde. The aldehyde is preferably propionaldehyde, n-butylaldehyde, isobutyraldehyde, n-hexylaldehyde, or n-valeraldehyde, more preferably propionaldehyde, n-butylaldehyde, or isobutyraldehyde, and even more preferably n-butylaldehyde. The aldehydes may be used alone or in combination of two or more.

[0153] The hydroxyl group content (hydroxyl group amount) of the polyvinyl acetal resin (0) is preferably 15 mol% or more, more preferably 18 mol% or more, and preferably 40 mol% or less, more preferably 35 mol% or less. When the hydroxyl group content is equal to or more than the lower limit, the adhesive strength of the interlayer film is further increased. When the hydroxyl group content is equal to or less than the upper limit, the flexibility of the interlayer film is increased, making it easier to handle.

[0154] The hydroxyl group content (hydroxyl group amount) of the polyvinyl acetal resin (1) is preferably 17 mol% or more, more preferably 20 mol% or more, even more preferably 22 mol% or more, and preferably 28 mol% or less, more preferably 27 mol% or less, even more preferably 25 mol% or less, and particularly preferably 24 mol% or less. When the hydroxyl group content is equal to or more than the lower limit, the mechanical strength of the interlayer film is further increased. In particular, when the hydroxyl group content of the polyvinyl acetal resin (1) is 20 mol% or more, the reaction efficiency is high and the productivity is excellent, and when it is 28 mol% or less, the sound insulation of the laminated glass is further increased. In addition, when the hydroxyl group content is equal to or less than the upper limit, the flexibility of the interlayer film is high, and the handling of the interlayer film is easy.

[0155] The hydroxyl group content of each of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) is preferably 25 mol% or more, more preferably 28 mol% or more, even more preferably 30 mol% or more, even more preferably 31.5 mol% or more, particularly preferably 32 mol% or more, and most preferably 33 mol% or more. The hydroxyl group content of each of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) is preferably 38 mol% or less, more preferably 37 mol% or less, even more preferably 36.5 mol% or less, and particularly preferably 36 mol% or less. When the hydroxyl group content is the lower limit or more, the adhesive strength of the interlayer film is further increased. When the hydroxyl group content is the upper limit or less, the flexibility of the interlayer film is increased, and the handling of the interlayer film is facilitated.

[0156] From the viewpoint of further improving the sound insulation, the hydroxyl group content of the polyvinyl acetal resin (1) is preferably lower than the hydroxyl group content of the polyvinyl acetal resin (2). From the viewpoint of further improving the sound insulation, the hydroxyl group content of the polyvinyl acetal resin (1) is preferably lower than the hydroxyl group content of the polyvinyl acetal resin (3). From the viewpoint of further improving the sound insulation, the absolute value of the difference between the hydroxyl group content of the polyvinyl acetal resin (1) and the hydroxyl group content of the polyvinyl acetal resin (2) is preferably 1 mol % or more, more preferably 5 mol % or more, even more preferably 9 mol % or more, particularly preferably 10 mol % or more, and most preferably 12 mol % or more. From the viewpoint of further improving sound insulation, the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin (1) and the hydroxyl content of the polyvinyl acetal resin (3) is preferably 1 mol% or more, more preferably 5 mol% or more, even more preferably 9 mol% or more, particularly preferably 10 mol% or more, and most preferably 12 mol% or more. The absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin (1) and the hydroxyl content of the polyvinyl acetal resin (2), and the absolute value of the difference between the hydroxyl content of the polyvinyl acetal resin (1) and the hydroxyl content of the polyvinyl acetal resin (3) are preferably 20 mol% or less.

[0157] The hydroxyl content of the polyvinyl acetal resin is a molar fraction calculated by dividing the amount of ethylene groups to which hydroxyl groups are bonded by the total amount of ethylene groups in the main chain, and expressed as a percentage. The amount of ethylene groups to which hydroxyl groups are bonded can be measured, for example, in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral."

[0158] The degree of acetylation (amount of acetyl groups) of the polyvinyl acetal resin (0) is preferably 0.1 mol% or more, more preferably 0.3 mol% or more, even more preferably 0.5 mol% or more, and is preferably 30 mol% or less, more preferably 25 mol% or less, even more preferably 20 mol% or less. When the degree of acetylation is equal to or more than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetylation is equal to or less than the upper limit, the moisture resistance of the interlayer film and the laminated glass is increased.

[0159] The degree of acetylation (amount of acetyl groups) of the polyvinyl acetal resin (1) is preferably 0.01 mol% or more, more preferably 0.1 mol% or more, even more preferably 7 mol% or more, even more preferably 9 mol% or more, and preferably 30 mol% or less, more preferably 25 mol% or less, even more preferably 24 mol% or less, and particularly preferably 20 mol% or less. When the degree of acetylation is equal to or more than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetylation is equal to or less than the upper limit, the moisture resistance of the interlayer film and the laminated glass is increased. In particular, when the degree of acetylation of the polyvinyl acetal resin (1) is 0.1 mol% or more and 25 mol% or less, the penetration resistance is excellent.

[0160] The degree of acetylation of each of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) is preferably 0.01 mol% or more, more preferably 0.5 mol% or more, and preferably 10 mol% or less, more preferably 2 mol% or less. When the degree of acetylation is equal to or more than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetylation is equal to or less than the upper limit, the moisture resistance of the interlayer film and the laminated glass is increased.

[0161] The degree of acetylation is a molar fraction calculated by dividing the amount of ethylene groups to which acetyl groups are bonded by the total amount of ethylene groups in the main chain, expressed as a percentage. The amount of ethylene groups to which acetyl groups are bonded can be measured, for example, in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral."

[0162] The degree of acetalization of the polyvinyl acetal resin (0) (the degree of butyralization in the case of a polyvinyl butyral resin) is preferably 60 mol% or more, more preferably 63 mol% or more, and preferably 85 mol% or less, more preferably 75 mol% or less, and even more preferably 70 mol% or less. When the degree of acetalization is equal to or more than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetalization is equal to or less than the upper limit, the reaction time required to produce the polyvinyl acetal resin is shortened.

[0163] The degree of acetalization of the polyvinyl acetal resin (1) (the degree of butyralization in the case of a polyvinyl butyral resin) is preferably 47 mol% or more, more preferably 60 mol% or more, and preferably 85 mol% or less, more preferably 80 mol% or less, and even more preferably 75 mol% or less. When the degree of acetalization is equal to or more than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetalization is equal to or less than the upper limit, the reaction time required to produce the polyvinyl acetal resin is shortened.

[0164] The degree of acetalization of each of the polyvinyl acetal resin (2) and the polyvinyl acetal resin (3) (the degree of butyralization in the case of a polyvinyl butyral resin) is preferably 55 mol% or more, more preferably 60 mol% or more, and preferably 75 mol% or less, more preferably 71 mol% or less. When the degree of acetalization is equal to or more than the lower limit, the compatibility of the polyvinyl acetal resin with the plasticizer is increased. When the degree of acetalization is equal to or less than the upper limit, the reaction time required to produce the polyvinyl acetal resin is shortened.

[0165] The degree of acetalization is determined as follows. The amount of ethylene groups to which hydroxyl groups are bonded and the amount of ethylene groups to which acetyl groups are bonded are subtracted from the total amount of ethylene groups in the main chain. The obtained value is divided by the total amount of ethylene groups in the main chain to determine the molar fraction. The resulting percentage is the degree of acetalization.

[0166] The hydroxyl group content (hydroxyl group amount), acetalization degree (butyralization degree), and acetylation degree are preferably calculated from the results measured by a method conforming to JIS K6728 "Testing Method for Polyvinyl Butyral". However, measurements according to ASTM D1396-92 may also be used. When the polyvinyl acetal resin is a polyvinyl butyral resin, the hydroxyl group content (hydroxyl group amount), acetalization degree (butyralization degree), and acetylation degree can be calculated from the results measured by a method conforming to JIS K6728 "Testing Method for Polyvinyl Butyral".

[0167] In the 100% by weight of the thermoplastic resin contained in the interlayer film body, the content of the polyvinyl acetal resin is preferably 10% by weight or more, more preferably 30% by weight or more, even more preferably 50% by weight or more, still more preferably 70% by weight or more, particularly preferably 80% by weight or more, and most preferably 90% by weight or more. The main component (50% by weight or more) of the thermoplastic resin in the interlayer film body is preferably polyvinyl acetal resin.

[0168] (Plasticizer) From the viewpoint of further increasing the adhesive strength of the interlayer film, it is preferable that the interlayer film contains a plasticizer. From the viewpoint of further increasing the adhesive strength of the interlayer film, it is preferable that the interlayer film main body contains a plasticizer (hereinafter, may be referred to as plasticizer (0)). The printed part may contain a plasticizer. The plasticizer contained in the interlayer film main body and the plasticizer contained in the printed part may be the same or different. It is preferable that the first layer contains a plasticizer (hereinafter, may be referred to as plasticizer (1)). It is preferable that the second layer contains a plasticizer (hereinafter, may be referred to as plasticizer (2)). It is preferable that the third layer contains a plasticizer (hereinafter, may be referred to as plasticizer (3)). When the thermoplastic resin contained in the interlayer film is a polyvinyl acetal resin, it is particularly preferable that the interlayer film (each layer) contains a plasticizer. It is preferable that the layer containing the polyvinyl acetal resin contains a plasticizer.

[0169] The plasticizer is not particularly limited. Conventionally known plasticizers can be used as the plasticizer. The plasticizer may be used alone or in combination of two or more.

[0170] The plasticizer may be an organic ester plasticizer such as a monobasic organic acid ester or a polybasic organic acid ester, or an organic phosphoric acid plasticizer such as an organic phosphoric acid plasticizer or an organic phosphorous acid plasticizer. The plasticizer is preferably an organic ester plasticizer. The plasticizer is preferably a liquid plasticizer.

[0171] The monobasic organic acid ester may be a glycol ester obtained by reacting a glycol with a monobasic organic acid. The glycol may be triethylene glycol, tetraethylene glycol, or tripropylene glycol. The monobasic organic acid may be butyric acid, isobutyric acid, caproic acid, 2-ethylbutyric acid, heptyl acid, n-octylic acid, 2-ethylhexyl acid, n-nonyl acid, or decyl acid.

[0172] Examples of the polybasic organic acid ester include ester compounds of a polybasic organic acid and an alcohol having a linear or branched structure with 4 to 8 carbon atoms. Examples of the polybasic organic acid include adipic acid, sebacic acid, and azelaic acid.

[0173] Examples of the organic ester plasticizer include triethylene glycol di-2-ethylpropanoate, triethylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylhexanoate, triethylene glycol dicaprylate, triethylene glycol di-n-octanoate, triethylene glycol di-n-heptanoate, tetraethylene glycol di-n-heptanoate, dibutyl sebacate, dioctyl azelate, dibutyl carbitol adipate, ethylene glycol di-2-ethylbutyrate, 1,3-propylene glycol di-2-ethylbutyrate, 1,4-butylene glycol di-2-ethylbutyrate, di Examples of suitable plasticizers include ethylene glycol di-2-ethylbutyrate, diethylene glycol di-2-ethylhexanoate, dipropylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylpentanoate, tetraethylene glycol di-2-ethylbutyrate, diethylene glycol dicaprylate, dihexyl adipate, dioctyl adipate, hexylcyclohexyl adipate, a mixture of heptyl adipate and nonyl adipate, diisononyl adipate, diisodecyl adipate, heptylnonyl adipate, dibutyl sebacate, oil-modified alkyd sebacate, and a mixture of phosphoric acid ester and adipate. Other organic ester plasticizers may also be used. Other adipic acid esters than the above-mentioned adipic acid esters may also be used.

[0174] The organic phosphoric acid plasticizers include tributoxyethyl phosphate, isodecylphenyl phosphate, and triisopropyl phosphate.

[0175] The plasticizer is preferably a diester plasticizer represented by the following formula (1).

[0176] [ka]

[0177] In the above formula (1), R1 and R2 each represent an organic group having 5 to 10 carbon atoms, R3 represents an ethylene group, an isopropylene group or an n-propylene group, and p represents an integer of 3 to 10. In the above formula (1), R1 and R2 each are preferably an organic group having 6 to 10 carbon atoms.

[0178] The plasticizer preferably comprises triethylene glycol di-2-ethylhexanoate (3GO) or triethylene glycol di-2-ethylbutyrate (3GH), more preferably triethylene glycol di-2-ethylhexanoate.

[0179] In the interlayer film body, the content of the plasticizer (0) relative to 100 parts by weight of the thermoplastic resin (0) is defined as the content (0). The content (0) is preferably 25 parts by weight or more, more preferably 30 parts by weight or more, and preferably 100 parts by weight or less, more preferably 60 parts by weight or less, and even more preferably 50 parts by weight or less. When the content (0) is equal to or more than the lower limit, the penetration resistance of the laminated glass is further increased. When the content (0) is equal to or less than the upper limit, the transparency of the interlayer film is further increased.

[0180] In the first layer, the content of the plasticizer (1) relative to 100 parts by weight of the thermoplastic resin (1) is defined as the content (1). The content (1) is preferably 50 parts by weight or more, more preferably 55 parts by weight or more, even more preferably 60 parts by weight or more, and is preferably 100 parts by weight or less, more preferably 90 parts by weight or less, even more preferably 85 parts by weight or less, and particularly preferably 80 parts by weight or less. When the content (1) is equal to or more than the lower limit, the flexibility of the interlayer film is increased, and the interlayer film is easy to handle. When the content (1) is equal to or less than the upper limit, the penetration resistance of the laminated glass is further increased.

[0181] In the second layer, the content of the plasticizer (2) relative to 100 parts by weight of the thermoplastic resin (2) is defined as the content (2). In the third layer, the content of the plasticizer (3) relative to 100 parts by weight of the thermoplastic resin (3) is defined as the content (3). The content (2) and the content (3) are each preferably 10 parts by weight or more, more preferably 15 parts by weight or more, even more preferably 20 parts by weight or more, and particularly preferably 24 parts by weight or more. The content (2) and the content (3) are each preferably 40 parts by weight or less, more preferably 35 parts by weight or less, even more preferably 32 parts by weight or less, and particularly preferably 30 parts by weight or less. When the content (2) and the content (3) are not less than the lower limit, the flexibility of the interlayer film is increased, and the handling of the interlayer film is facilitated. When the content (2) and the content (3) are not more than the upper limit, the penetration resistance of the laminated glass is further increased.

[0182] In order to improve the sound insulation of the laminated glass, the content (1) is preferably greater than the content (2), and the content (1) is preferably greater than the content (3).

[0183] From the viewpoint of further improving the sound insulation of the laminated glass, the absolute value of the difference between the content (2) and the content (1) and the absolute value of the difference between the content (3) and the content (1) are each preferably 10 parts by weight or more, more preferably 15 parts by weight or more, and even more preferably 20 parts by weight or more. The absolute value of the difference between the content (2) and the content (1) and the absolute value of the difference between the content (3) and the content (1) are each preferably 80 parts by weight or less, more preferably 75 parts by weight or less, and even more preferably 70 parts by weight or less.

[0184] (Heat-shielding material) The intermediate film and the intermediate film main body preferably contain a heat-shielding material. The printed portion may contain a heat-shielding material. The heat-shielding material contained in the intermediate film main body and the heat-shielding material contained in the printed portion may be the same or different. The first layer preferably contains a heat-shielding material. The second layer preferably contains a heat-shielding material. The third layer preferably contains a heat-shielding material. Only one type of heat-shielding material may be used, or two or more types may be used in combination.

[0185] The heat-shielding material preferably contains at least one component X selected from a phthalocyanine compound, a naphthalocyanine compound, and an anthracyanine compound, or contains heat-shielding particles. In this case, the heat-shielding material may contain both the component X and the heat-shielding particles.

[0186] Ingredient X: The interlayer film and the interlayer film main body preferably contain at least one component X selected from a phthalocyanine compound, a naphthalocyanine compound, and an anthracyanine compound. The printed portion may contain the component X. The component X contained in the interlayer film main body and the component X contained in the printed portion may be the same or different. The first layer preferably contains the component X. The second layer preferably contains the component X. The third layer preferably contains the component X. The component X is a heat-shielding material. Only one type of the component X may be used, or two or more types may be used in combination.

[0187] There is no particular limitation on the above-mentioned component X. As the component X, a conventionally known phthalocyanine compound, naphthalocyanine compound, or anthracyanine compound can be used.

[0188] The component X may be phthalocyanine, a derivative of phthalocyanine, naphthalocyanine, a derivative of naphthalocyanine, an anthracyanine, or a derivative of anthracyanine. The phthalocyanine compound and the derivative of phthalocyanine each preferably have a phthalocyanine skeleton. The naphthalocyanine compound and the derivative of naphthalocyanine each preferably have a naphthalocyanine skeleton. The anthracyanine compound and the derivative of anthracyanine each preferably have an anthracyanine skeleton.

[0189] From the viewpoint of further improving the heat insulation properties of the interlayer film and laminated glass, the above-mentioned component X is preferably at least one selected from the group consisting of phthalocyanine, phthalocyanine derivatives, naphthalocyanine and naphthalocyanine derivatives, and more preferably at least one of phthalocyanine and phthalocyanine derivatives.

[0190] From the viewpoint of effectively increasing the heat shielding property and maintaining the visible light transmittance at a higher level for a long period of time, the above component X preferably contains a vanadium atom or a copper atom. The above component X preferably contains a vanadium atom, and also preferably contains a copper atom. The above component X is more preferably at least one of phthalocyanine containing a vanadium atom or a copper atom and a derivative of phthalocyanine containing a vanadium atom or a copper atom. From the viewpoint of further increasing the heat shielding property of the interlayer film and the laminated glass, the above component X preferably has a structural unit in which an oxygen atom is bonded to a vanadium atom.

[0191] In 100% by weight of the intermediate film body or in 100% by weight of the layer containing the component X (first layer, second layer or third layer), the content of the component X is preferably 0.001% by weight or more, more preferably 0.005% by weight or more, even more preferably 0.01% by weight or more, and particularly preferably 0.02% by weight or more. In 100% by weight of the intermediate film body or in 100% by weight of the layer containing the component X (first layer, second layer or third layer), the content of the component X is preferably 0.2% by weight or less, more preferably 0.1% by weight or less, even more preferably 0.05% by weight or less, and particularly preferably 0.04% by weight or less. When the content of the component X is equal to or more than the lower limit and equal to or less than the upper limit, the heat shielding property is sufficiently high and the visible light transmittance is sufficiently high. For example, it is possible to make the visible light transmittance 70% or more.

[0192] Heat shielding particles: The intermediate film and the intermediate film main body preferably contain heat-shielding particles. The printed portion may contain heat-shielding particles. The heat-shielding particles contained in the intermediate film main body and the heat-shielding particles contained in the printed portion may be the same or different. The first layer preferably contains the heat-shielding particles. The second layer preferably contains the heat-shielding particles. The third layer preferably contains the heat-shielding particles. The heat-shielding particles are a heat-shielding material. The use of the heat-shielding particles can effectively block infrared rays (heat rays). Only one type of the heat-shielding particles may be used, or two or more types may be used in combination.

[0193] From the viewpoint of further enhancing the heat shielding property of the laminated glass, the heat shielding particles are more preferably metal oxide particles.The heat shielding particles are preferably particles formed of a metal oxide (metal oxide particles).

[0194] Infrared rays, which have wavelengths of 780 nm or more, longer than visible light, have a smaller amount of energy than ultraviolet rays. However, infrared rays have a large thermal effect, and when infrared rays are absorbed by a substance, they are released as heat. For this reason, infrared rays are generally called heat rays. By using the above heat-shielding particles, infrared rays (heat rays) can be effectively blocked. Note that heat-shielding particles refer to particles that can absorb infrared rays.

[0195] Specific examples of the heat shielding particles include metal oxide particles such as aluminum-doped tin oxide particles, indium-doped tin oxide particles, antimony-doped tin oxide particles (ATO particles), gallium-doped zinc oxide particles (GZO particles), indium-doped zinc oxide particles (IZO particles), aluminum-doped zinc oxide particles (AZO particles), niobium-doped titanium oxide particles, sodium-doped tungsten oxide particles, cesium-doped tungsten oxide particles, thallium-doped tungsten oxide particles, rubidium-doped tungsten oxide particles, tin-doped indium oxide particles (ITO particles), tin-doped zinc oxide particles, and silicon-doped zinc oxide particles, as well as lanthanum hexaboride (LaB6) particles. Heat shielding particles other than these may also be used. Metal oxide particles are preferred because of their high heat ray shielding function, ATO particles, GZO particles, IZO particles, ITO particles or tungsten oxide particles are more preferred, ATO particles, ITO particles or tungsten oxide particles are even more preferred, and ITO particles or tungsten oxide particles are particularly preferred. When the heat shielding particles include ITO particles or tungsten oxide particles, the heat shielding particles may include ITO particles and tungsten oxide particles. In particular, tin-doped indium oxide particles (ITO particles) are preferred because of their high heat ray shielding function and easy availability, and tungsten oxide particles are also preferred.

[0196] From the viewpoint of further improving the heat insulating properties of the interlayer film and the laminated glass, the tungsten oxide particles are preferably metal-doped tungsten oxide particles. The "tungsten oxide particles" include metal-doped tungsten oxide particles. Specific examples of the metal-doped tungsten oxide particles include sodium-doped tungsten oxide particles, cesium-doped tungsten oxide particles, thallium-doped tungsten oxide particles, and rubidium-doped tungsten oxide particles.

[0197] From the viewpoint of further increasing the heat insulating property of the interlayer film and the laminated glass, cesium-doped tungsten oxide particles are particularly preferred. From the viewpoint of further increasing the heat insulating property of the interlayer film and the laminated glass, the cesium-doped tungsten oxide particles are represented by the formula: Cs 0.33 Tungsten oxide particles represented by WO3 are preferred.

[0198] The average particle size of the heat shielding particles is preferably 0.01 μm or more, more preferably 0.02 μm or more, and is preferably 0.1 μm or less, more preferably 0.05 μm or less. When the average particle size is equal to or more than the lower limit, the heat shielding properties are sufficiently high. When the average particle size is equal to or less than the upper limit, the dispersibility of the heat shielding particles is high.

[0199] The "average particle size" refers to the volume average particle size. The average particle size can be measured using a particle size distribution measuring device (manufactured by Nikkiso Co., Ltd., "UPA-EX150") or the like.

[0200] The content of the heat shielding particles in 100% by weight of the intermediate film body or in 100% by weight of the layer containing the heat shielding particles (first layer, second layer or third layer) is preferably 0.01% by weight or more, more preferably 0.1% by weight or more, even more preferably 1% by weight or more, and particularly preferably 1.5% by weight or more. The content of the heat shielding particles in 100% by weight of the intermediate film body or in 100% by weight of the layer containing the heat shielding particles (first layer, second layer or third layer) is preferably 6% by weight or less, more preferably 5.5% by weight or less, even more preferably 4% by weight or less, particularly preferably 3.5% by weight or less, and most preferably 3% by weight or less. When the content of the heat shielding particles is equal to or more than the lower limit and equal to or less than the upper limit, the heat shielding property is sufficiently high and the visible light transmittance is sufficiently high.

[0201] (Metal Salts) The intermediate film and the intermediate film body preferably contain at least one metal salt (hereinafter, sometimes referred to as metal salt M) of an alkali metal salt and an alkaline earth metal salt. The printed part may contain the metal salt M. The metal salt M contained in the intermediate film body and the metal salt M contained in the printed part may be the same or different. The first layer preferably contains the metal salt M. The second layer preferably contains the metal salt M. The third layer preferably contains the metal salt M. The alkaline earth metal means six metals, Be, Mg, Ca, Sr, Ba, and Ra. The use of the metal salt M makes it easy to control the adhesion between the intermediate film and a laminated glass member such as a glass plate or the adhesion between each layer in the intermediate film. The metal salt M may be used alone or in combination of two or more.

[0202] The metal salt M preferably contains at least one metal selected from the group consisting of Li, Na, K, Rb, Cs, Mg, Ca, Sr and Ba. The metal salt contained in the interlayer film preferably contains at least one metal selected from the group consisting of K and Mg.

[0203] The metal salt M is more preferably an alkali metal salt of an organic acid having 2 to 16 carbon atoms, or an alkaline earth metal salt of an organic acid having 2 to 16 carbon atoms. The metal salt M is also more preferably a magnesium salt of an organic acid having 2 to 16 carbon atoms. The metal salt M is further preferably a magnesium salt of a carboxylate having 2 to 16 carbon atoms, or a potassium salt of a carboxylate having 2 to 16 carbon atoms.

[0204] Examples of the magnesium salt of a carboxylate having 2 to 16 carbon atoms and the potassium salt of a carboxylate having 2 to 16 carbon atoms include magnesium acetate, potassium acetate, magnesium propionate, potassium propionate, magnesium 2-ethylbutyrate, potassium 2-ethylbutanoate, magnesium 2-ethylhexanoate, and potassium 2-ethylhexanoate.

[0205] The total content of Mg and K in the interlayer containing the metal salt M or in the layer (first layer, second layer or third layer) containing the metal salt M is preferably 5 ppm or more, more preferably 10 ppm or more, even more preferably 20 ppm or more, and is preferably 300 ppm or less, more preferably 250 ppm or less, even more preferably 200 ppm or less. When the total content of Mg and K is equal to or more than the above lower limit and equal to or less than the above upper limit, the adhesion between the interlayer and the glass plate or the adhesion between the layers in the interlayer can be controlled more effectively.

[0206] (UV protection agent) The interlayer film and the interlayer film main body preferably contain an ultraviolet shielding agent. The printed portion may contain an ultraviolet shielding agent. The ultraviolet shielding agent contained in the interlayer film main body and the ultraviolet shielding agent contained in the printed portion may be the same or different. The first layer preferably contains an ultraviolet shielding agent. The second layer preferably contains an ultraviolet shielding agent. The third layer preferably contains an ultraviolet shielding agent. By using an ultraviolet shielding agent, the visible light transmittance is more unlikely to decrease even when the interlayer film and the laminated glass are used for a long period of time. Only one type of ultraviolet shielding agent may be used, or two or more types may be used in combination.

[0207] The ultraviolet shielding agent includes an ultraviolet absorbing agent. The ultraviolet shielding agent is preferably an ultraviolet absorbing agent.

[0208] Examples of the ultraviolet ray shielding agent include ultraviolet ray shielding agents containing metal atoms, ultraviolet ray shielding agents containing metal oxides, ultraviolet ray shielding agents having a benzotriazole structure (benzotriazole compounds), ultraviolet ray shielding agents having a benzophenone structure (benzophenone compounds), ultraviolet ray shielding agents having a triazine structure (triazine compounds), ultraviolet ray shielding agents having a malonic acid ester structure (malonic acid ester compounds), ultraviolet ray shielding agents having an oxalic acid anilide structure (oxalic acid anilide compounds), and ultraviolet ray shielding agents having a benzoate structure (benzoate compounds).

[0209] Examples of the ultraviolet shielding agent containing the metal atom include platinum particles, platinum particles whose surfaces are coated with silica, palladium particles, and palladium particles whose surfaces are coated with silica, etc. It is preferable that the ultraviolet shielding agent is not a heat shielding particle.

[0210] The ultraviolet shielding agent is preferably an ultraviolet shielding agent having a benzotriazole structure, an ultraviolet shielding agent having a benzophenone structure, an ultraviolet shielding agent having a triazine structure, or an ultraviolet shielding agent having a benzoate structure. The ultraviolet shielding agent is more preferably an ultraviolet shielding agent having a benzotriazole structure or an ultraviolet shielding agent having a benzophenone structure, and further preferably an ultraviolet shielding agent having a benzotriazole structure.

[0211] Examples of the ultraviolet shielding agent containing the metal oxide include zinc oxide, titanium oxide, and cerium oxide. Furthermore, the ultraviolet shielding agent containing the metal oxide may be surface-coated. Examples of the surface-coating material of the ultraviolet shielding agent containing the metal oxide include insulating metal oxides, hydrolyzable organic silicon compounds, and silicone compounds.

[0212] The insulating metal oxide includes silica, alumina, zirconia, etc. The insulating metal oxide has a band gap energy of, for example, 5.0 eV or more.

[0213] Examples of the ultraviolet shielding agent having the benzotriazole structure include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (BASF's "Tinuvin P"), 2-(2'-hydroxy-3',5'-di-t-butylphenyl)benzotriazole (BASF's "Tinuvin 320"), 2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole (BASF's "Tinuvin 326"), and 2-(2'-hydroxy-3',5'-di-amylphenyl)benzotriazole (BASF's "Tinuvin 328"), etc. Since the ultraviolet shielding agent has excellent ultraviolet shielding performance, it is preferable that the ultraviolet shielding agent has a benzotriazole structure containing a halogen atom, and more preferably has a benzotriazole structure containing a chlorine atom.

[0214] Examples of the ultraviolet screening agent having a benzophenone structure include octabenzone ("Chimassorb 81" manufactured by BASF).

[0215] Examples of the ultraviolet screening agent having a triazine structure include "LA-F70" manufactured by ADEKA Corporation and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol ("Tinuvin 1577FF" manufactured by BASF).

[0216] Examples of the ultraviolet screening agent having a malonic acid ester structure include dimethyl 2-(p-methoxybenzylidene)malonate, tetraethyl-2,2-(1,4-phenylenedimethylidene)bismalonate, and 2-(p-methoxybenzylidene)-bis(1,2,2,6,6-pentamethyl-4-piperidinyl)malonate.

[0217] Commercially available ultraviolet screening agents having the above malonic acid ester structure include Hostavin B-CAP, Hostavin PR-25, and Hostavin PR-31 (all manufactured by Clariant).

[0218] Examples of ultraviolet screening agents having the above-mentioned oxalic acid anilide structure include oxalic acid diamides having an aryl group substituted on the nitrogen atom, such as N-(2-ethylphenyl)-N'-(2-ethoxy-5-t-butylphenyl)oxalic acid diamide, N-(2-ethylphenyl)-N'-(2-ethoxy-phenyl)oxalic acid diamide, and 2-ethyl-2'-ethoxy-oxyanilide ("Sanduvor VSU" manufactured by Clariant).

[0219] Examples of the ultraviolet screening agent having a benzoate structure include 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate ("Tinuvin 120" manufactured by BASF).

[0220] In 100% by weight of the intermediate film body or in 100% by weight of the layer (first layer, second layer or third layer) containing the ultraviolet ray shielding agent, the content of the ultraviolet ray shielding agent is preferably 0.1% by weight or more, more preferably 0.2% by weight or more, even more preferably 0.3% by weight or more, and particularly preferably 0.5% by weight or more. In 100% by weight of the intermediate film body or in 100% by weight of the layer (first layer, second layer or third layer) containing the ultraviolet ray shielding agent, the content of the ultraviolet ray shielding agent is preferably 2.5% by weight or less, more preferably 2% by weight or less, even more preferably 1% by weight or less, and particularly preferably 0.8% by weight or less. When the content of the ultraviolet ray shielding agent is the above lower limit or more and the above upper limit or less, the decrease in visible light transmittance after a period of time can be further suppressed. In particular, by having the content of the ultraviolet ray shielding agent be 0.2% by weight or more in 100% by weight of the layer containing the ultraviolet ray shielding agent, it is possible to significantly suppress the decrease in visible light transmittance of the interlayer film and laminated glass over a period of time.

[0221] (Antioxidants) The intermediate film and the intermediate film main body preferably contain an antioxidant. The printed portion may contain an antioxidant. The antioxidant contained in the intermediate film main body and the antioxidant contained in the printed portion may be the same or different. The first layer preferably contains an antioxidant. The second layer preferably contains an antioxidant. The third layer preferably contains an antioxidant. Only one type of antioxidant may be used, or two or more types may be used in combination.

[0222] The antioxidants include phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants. The phenol-based antioxidants are antioxidants having a phenol skeleton. The sulfur-based antioxidants are antioxidants containing sulfur atoms. The phosphorus-based antioxidants are antioxidants containing phosphorus atoms.

[0223] The antioxidant is preferably a phenol-based antioxidant or a phosphorus-based antioxidant.

[0224] The phenol-based antioxidants include 2,6-di-t-butyl-p-cresol (BHT), butyl hydroxyanisole (BHA), 2,6-di-t-butyl-4-ethylphenol, stearyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis-(4-methyl-6-butylphenol), 2,2'-methylenebis-(4-ethyl-6-t-butylphenol), 4,4'-butylidene-bis-(3-methyl-6-t-butylphenol), 1,1,3-tris-(2-methyl-hydroxy-5- t-butylphenyl)butane, tetrakis[methylene-3-(3',5'-butyl-4-hydroxyphenyl)propionate]methane, 1,3,3-tris-(2-methyl-4-hydroxy-5-t-butylphenol)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, bis(3,3'-t-butylphenol)butyric acid glycol ester, and bis(3-t-butyl-4-hydroxy-5-methylbenzenepropanoic acid)ethylenebis(oxyethylene). One or more of these antioxidants are preferably used.

[0225] Examples of the phosphorus-based antioxidant include tridecyl phosphite, tris(tridecyl)phosphite, triphenyl phosphite, trinonylphenyl phosphite, bis(tridecyl)pentaerythritol diphosphite, bis(decyl)pentaerythritol diphosphite, tris(2,4-di-t-butylphenyl)phosphite, bis(2,4-di-t-butyl-6-methylphenyl)ethyl ester phosphorous acid, and 2,2'-methylenebis(4,6-di-t-butyl-1-phenyloxy)(2-ethylhexyloxy)phosphorus, etc. One or more of these antioxidants are preferably used.

[0226] Commercially available examples of the antioxidant include "IRGANOX 245" manufactured by BASF, "IRGAFOS 168" manufactured by BASF, "IRGAFOS 38" manufactured by BASF, "Sumilizer BHT" manufactured by Sumitomo Chemical Co., Ltd., "H-BHT" manufactured by Sakai Chemical Industry Co., Ltd., and "IRGANOX 1010" manufactured by BASF.

[0227] In order to maintain the high visible light transmittance of the interlayer film and laminated glass for a long period of time, the content of the antioxidant is preferably 0.1% by weight or more in 100% by weight of the interlayer film body or 100% by weight of the layer containing the antioxidant (first layer, second layer or third layer). In addition, since the effect of adding the antioxidant becomes saturated, the content of the antioxidant is preferably 2% by weight or less in 100% by weight of the interlayer film body or 100% by weight of the layer containing the antioxidant.

[0228] (Other ingredients) The intermediate film, the intermediate film body, the printed portion, the first layer, the second layer and the third layer may each contain additives such as coupling agents, dispersants, surfactants, flame retardants, antistatic agents, pigments, dyes, adhesion regulators other than metal salts, moisture resistant agents, fluorescent brighteners, infrared absorbing agents, etc. These additives may be used alone or in combination of two or more.

[0229] (Laminated glass) FIG. 10 is a cross-sectional view showing an example of laminated glass using the interlayer film for laminated glass shown in FIG.

[0230] The laminated glass 21 shown in Fig. 10 includes an interlayer film portion 11X, a first laminated glass member 22, and a second laminated glass member 23. The interlayer film portion 11X is disposed and sandwiched between the first laminated glass member 22 and the second laminated glass member 23. The first laminated glass member 22 is disposed on a first surface of the interlayer film portion 11X. The second laminated glass member 23 is disposed on a second surface opposite to the first surface of the interlayer film portion 11X.

[0231] The intermediate film portion 11X is formed by the intermediate film 11. For example, when manufacturing the laminated glass 21, the intermediate film portion 11X can be formed by trimming and cutting the intermediate film 11. The intermediate film portion 11X may have a printed portion 4. The intermediate film portion 11X does not have to have a printed portion 4.

[0232] Examples of the laminated glass member include glass plates and PET (polyethylene terephthalate) films. The laminated glass includes not only a laminated glass having an intermediate film sandwiched between two glass plates, but also a laminated glass having an intermediate film sandwiched between a glass plate and a PET film or the like. The laminated glass is a laminate including glass plates, and preferably contains at least one glass plate. It is preferable that the first laminated glass member and the second laminated glass member are glass plates or PET (polyethylene terephthalate) films, respectively, and that the first laminated glass member and the second laminated glass member each contain at least one glass plate. It is particularly preferable that both the first laminated glass member and the second laminated glass member are glass plates.

[0233] The glass plate includes inorganic glass and organic glass. The inorganic glass includes float plate glass, heat absorbing plate glass, heat reflecting plate glass, polished plate glass, patterned plate glass, lined plate glass, green glass, etc. The organic glass is a synthetic resin glass that replaces inorganic glass. The organic glass includes polycarbonate plate and poly(meth)acrylic resin plate, etc. The poly(meth)acrylic resin plate includes polymethyl(meth)acrylate plate, etc.

[0234] The thickness of each of the first laminated glass member and the second laminated glass member is not particularly limited, but is preferably 1 mm or more and preferably 5 mm or less. When the laminated glass member is a glass plate, the thickness of the glass plate is preferably 1 mm or more and preferably 5 mm or less. When the laminated glass member is a PET film, the thickness of the PET film is preferably 0.03 mm or more and preferably 0.5 mm or less.

[0235] (Method of manufacturing laminated glass) A method for producing laminated glass according to the present invention is a method for producing laminated glass comprising a first laminated glass member, a second laminated glass member, and an interlayer film for laminated glass disposed between the first laminated glass member and the second laminated glass member.

[0236] The method for producing laminated glass according to the present invention includes a first disposing step of disposing the first laminated glass component on a first surface of the interlayer film for laminated glass described above, and a second disposing step of disposing the second laminated glass component on a second surface of the interlayer film for laminated glass opposite to the first surface.

[0237] The method for producing laminated glass according to the present invention includes the following (1) or (2): (1) in the first arranging step, the first laminated glass component and the interlayer film for laminated glass are bonded together using the printed portion of the interlayer film for laminated glass as a mark; (2) in the second arranging step, the second laminated glass component and the interlayer film for laminated glass are bonded together using the printed portion of the interlayer film for laminated glass as a mark.

[0238] The method for producing laminated glass according to the present invention preferably includes, after the second arranging step, a pressure bonding step of pressure bonding the first laminated glass component, the interlayer film, and the second laminated glass component together.

[0239] The pressure-bonding step may include a preliminary bonding step and a main pressure-bonding step. An example of the pressure-bonding step is shown below.

[0240] The laminate of the first laminated glass member, the interlayer film, and the second laminated glass member obtained in the second arrangement step is passed through a pressing roll or placed in a rubber bag and suctioned under reduced pressure. This allows air remaining between the first laminated glass member and the interlayer film and between the second laminated glass member and the interlayer film to be degassed. Then, preliminary bonding is performed under conditions of about 70°C to 110°C (preliminary bonding step). Then, the preliminarily bonded laminate is placed in an autoclave or pressed, and pressure-bonded at about 120°C to 150°C and a pressure of 1 MPa to 1.5 MPa (main pressure-bonding step).

[0241] In the method for producing laminated glass according to the present invention, it is preferable that the interlayer film is trimmed along edges of the first and second laminated glass components after the second arrangement step, the preliminary bonding step, or the main pressure bonding step.

[0242] The interlayer film and the laminated glass can be used in automobiles, railroad vehicles, aircraft, ships, buildings, and the like. The interlayer film is preferably an interlayer film for buildings or vehicles, and more preferably an interlayer film for vehicles. The interlayer film can be used for applications other than these. The interlayer film is suitably used for the front glass, side glass, rear glass, or roof glass of a vehicle. Furthermore, the laminated glass is preferably a laminated glass for buildings or vehicles, and more preferably a laminated glass for vehicles. The laminated glass can be used for applications other than these. The laminated glass is suitably used for the front glass, side glass, rear glass, or roof glass of a vehicle.

[0243] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. It should be noted that the following Examples 2 and 20 are for reference purposes only.

[0244] In the polyvinyl acetal resin used, n-butyl aldehyde with 4 carbon atoms was used for acetalization. For the polyvinyl acetal resin, the degree of acetalization (degree of butyralization), the degree of acetylation, and the content of hydroxyl groups were measured by a method conforming to JIS K6728 "Testing Method for Polyvinyl Butyral." When measured by ASTM D1396-92, the values ​​were similar to those obtained by a method conforming to JIS K6728 "Testing Method for Polyvinyl Butyral."

[0245] Example 1 Preparation of the composition for forming the first layer: The following components were blended and thoroughly kneaded in a mixing roll to obtain a composition for forming a first layer.

[0246] Polyvinyl acetal resin (average polymerization degree 1700, hydroxyl group content 30.5 mol%, acetylation degree 1.0 mol%, acetalization degree 68.5 mol%) 100 parts by weight Triethylene glycol di-2-ethylhexanoate (3GO) 40 parts by weight Tinuvin 326 (2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole, "Tinuvin 326" manufactured by BASF) in an amount of 0.2% by weight in the resulting first layer (interlayer film body). BHT (2,6-di-t-butyl-p-cresol) in an amount of 0.2% by weight in the resulting first layer (interlayer film body)

[0247] Preparation of interlayer and roll body: The composition for forming the first layer was extruded using an extruder to obtain a pre-printed intermediate film having a uniform thickness. The obtained pre-printed intermediate film had a width of 1000 mm, a length of 125 mm, and a thickness of 780 μm.

[0248] Using Keyence's "MD-U1000C," we used a UV laser to print characters containing the product information of the interlayer film at a position 15 mm from one end of the unprinted interlayer film, forming a white printed area, and fabricating an interlayer film that includes the interlayer film body and the printed area (see Figures 7 and 8 for the outer shape). The intensity of UV irradiation was set to 60%. Note that 100% intensity of UV irradiation means a laser diode output of 2.5 W.

[0249] The obtained interlayer film was wound in a length of 125 m around the outer circumference of a core (manufactured by Koga Polymer Co., Ltd., material: talc-containing polypropylene, outer diameter 15 cm x height 120 cm) at a winding tension of 1.3 N / cm to produce a roll body.

[0250] Example 2 An interlayer film and a roll body were produced in the same manner as in Example 1, except that a red printed portion was formed by inkjet printing using a Keyence Corporation "MK-U6000."

[0251] Example 3 Preparation of the composition for forming the first layer excluding the shaded area: The following components were blended and thoroughly kneaded with a mixing roll to obtain a composition for forming the first layer excluding the shaded region.

[0252] Polyvinyl acetal resin (average polymerization degree 1700, hydroxyl group content 30.5 mol%, acetylation degree 1.0 mol%, acetalization degree 68.5 mol%) 100 parts by weight Triethylene glycol di-2-ethylhexanoate (3GO) 40 parts by weight Tinuvin 326 (2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole, BASF "Tinuvin 326") in an amount of 0.2% by weight in the resulting first layer (excluding the shaded area). BHT (2,6-di-t-butyl-p-cresol) in an amount to provide 0.2% by weight in the resulting first layer (excluding the shaded area)

[0253] Preparation of the composition for forming the shaded area in the first layer: The following components were blended and thoroughly kneaded with a mixing roll to obtain a composition for forming the shade region in the first layer.

[0254] Polyvinyl acetal resin (average polymerization degree 1700, hydroxyl group content 30.5 mol%, acetylation degree 1.0 mol%, acetalization degree 68.5 mol%) 100 parts by weight Triethylene glycol di-2-ethylhexanoate (3GO) 40 parts by weight Tinuvin 326 (2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole, BASF "Tinuvin 326") in an amount of 0.2% by weight in the resulting first layer (shaded area) BHT (2,6-di-t-butyl-p-cresol) in an amount to give 0.2% by weight in the resulting first layer (shaded area) SG-1505 (anthraquinone compound, "BLUE SG-1505" manufactured by Sumika Color Co., Ltd.) (colorant) in an amount of 0.025% by weight in the resulting first layer (shade region)

[0255] Preparation of interlayer and roll body: The composition for forming the first layer excluding the shaded region and the composition for forming the shaded region in the first layer were extruded using an extruder to obtain a pre-printed intermediate film with a uniform thickness. The obtained pre-printed intermediate film had a width of 990 mm, a length of 125 mm, and a thickness of 780 μm, and had a shaded region in a region between one end and a position 150 mm from the one end toward the other end. Using a Keyence Corporation "MD-U1000C," solid lines with a line width of 0.5 mm were UV laser printed at a position 20 mm from one end of the pre-printed intermediate film and a position 20 mm from the other end to form a white printed portion, and an intermediate film having an intermediate film body and a printed portion was produced (see Figures 7 and 8 for the shape of the outer shell). The intensity of UV irradiation was 60%.

[0256] The printed portions are lines for alignment with the edges of the laminated glass member.

[0257] The obtained interlayer film was wound around the outer periphery of a core in a roll shape in the same manner as in Example 1 to prepare a roll body.

[0258] Example 4 An interlayer film and a roll body were produced in the same manner as in Example 3, except that a white printed portion was formed by UV laser printing a dotted line having a line width of 1 mm.

[0259] Example 5 An interlayer film and a roll body were produced in the same manner as in Example 3, except that a blue printed portion was formed by inkjet printing a dotted line having a line width of 1 mm using a Keyence Corporation "MK-U6000".

[0260] Example 6 An interlayer film and a roll body were produced in the same manner as in Example 3, except that a solid line having a line width of 5 mm was printed by UV laser to form a white printed portion.

[0261] Example 7 An interlayer film and a roll body were produced in the same manner as in Example 3, except that a dotted line having a line width of 10 m was printed by UV laser to form a white printed portion.

[0262] Example 8 An intermediate film and a roll body were produced in the same manner as in Example 3, except that a black printed area was formed by labeling 5 mm-wide dotted lines at a position 30 mm from one end of the unprinted intermediate film and a position 20 mm from the other end using "AMK-Clean" manufactured by Ayaha Engineering Co., Ltd.

[0263] Comparative Example 1 An interlayer film and a roll body were produced in the same manner as in Example 3, except that a printed portion was not formed.

[0264] Example 9 The composition for forming the first layer obtained in Example 1 was extruded using an extruder to obtain a pre-printed intermediate film having a portion with a wedge-shaped cross section in the thickness direction. The obtained pre-printed intermediate film had a width (distance between one end and the other end) of 990 mm, a length of 125 mm, and an average thickness of 1028 μm.

[0265] Using Keyence's "MD-U1000C," a solid line with a line width of 0.5 mm was printed with a UV laser at a position 180 mm from one end of the unprinted interlayer film and a position 412 mm from the other end to form a white printed area, producing an interlayer film comprising an interlayer film body and a printed area. The intensity of UV irradiation was 50%.

[0266] The printed parts are lines for aligning the HUD area.

[0267] The obtained interlayer film had a minimum thickness at one end and a maximum thickness at the other end. The thickness at one end was 780 μm, and the thickness at the other end was 1275 μm. The obtained interlayer film had a portion where the increase in thickness was smaller from one end to the other end in the region where the thickness increased, and an interlayer film having a portion where the wedge angle was smaller from one end to the other end in the region where the cross-sectional shape in the thickness direction was wedge-shaped (see FIG. 6 for the outer shape). When the distance between one end and the other end was X, the most protruding part of the convex part of the interlayer film was located at a position 0.3X from one end. The wedge angle of the entire interlayer film was 0.5 mrad.

[0268] The obtained interlayer film was wound around the outer periphery of a core in a roll shape in the same manner as in Example 1 to prepare a roll body.

[0269] Example 10 Preparation of the composition for forming the first layer: The following components were blended and thoroughly kneaded in a mixing roll to obtain a composition for forming a first layer.

[0270] Polyvinyl acetal resin (average degree of polymerization 3000, hydroxyl group content 22 mol%, acetylation degree 13 mol%, acetalization degree 65 mol%) 100 parts by weight Triethylene glycol di-2-ethylhexanoate (3GO) 60 parts by weight Tinuvin 326 (2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole, "Tinuvin 326" manufactured by BASF) in an amount of 0.2% by weight in the resulting first layer. BHT (2,6-di-t-butyl-p-cresol) in an amount of 0.2% by weight in the resulting first layer

[0271] Preparation of compositions for forming the second and third layers: The following components were blended and thoroughly kneaded with a mixing roll to obtain compositions for forming the second layer and the third layer.

[0272] Polyvinyl acetal resin (average polymerization degree 1700, hydroxyl group content 30.5 mol%, acetylation degree 1 mol%, acetalization degree 68.5 mol%) 100 parts by weight Triethylene glycol di-2-ethylhexanoate (3GO) 38 parts by weight Tinuvin 326 (2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole, "Tinuvin 326" manufactured by BASF) in an amount of 0.2% by weight in the resulting second and third layers. BHT (2,6-di-t-butyl-p-cresol) in an amount of 0.2% by weight in the resulting second and third layers

[0273] Preparation of interlayer and roll body: The composition for forming the first layer and the compositions for forming the second and third layers were co-extruded using a co-extruder to obtain a pre-printed intermediate film having a portion with a wedge-shaped cross-sectional shape in the thickness direction. The obtained pre-printed intermediate film had a width (distance between one end and the other end) of 990 mm, a length of 125 m, and an average thickness of 1028 μm.

[0274] Using a Keyence MD-U1000C, a solid line with a line width of 0.5 mm was printed with a UV laser at a position 180 mm from one end of the interlayer before printing and at a position 352 mm from the other end to form a white printed area, and the interlayer was produced. The intensity of the UV irradiation was 60%.

[0275] The printed parts are lines for aligning the HUD area.

[0276] The interlayer film obtained had a minimum thickness at one end and a maximum thickness at the other end. The thickness at one end was 780 μm, and the thickness at the other end was 1275 μm. The interlayer film obtained had a portion where the increase in thickness was smaller from one end to the other end in the region where the thickness was increasing, and had a portion where the wedge angle was smaller from one end to the other end in the region where the cross-sectional shape in the thickness direction was wedge-shaped (see FIG. 5 for the outer shape). When the distance between one end and the other end was X, the most protruding part of the convex part of the interlayer film was located at a position 0.3X from the one end. The wedge angle of the entire interlayer film was 0.5 mrad.

[0277] The obtained interlayer film was wound around the outer periphery of a core in a roll shape in the same manner as in Example 1 to prepare a roll body.

[0278] Example 11 An interlayer film and a roll body were produced in the same manner as in Example 10, except that a white printed portion was formed by UV laser printing a solid line with a line width of 2 mm at a position 15 mm from one end of the unprinted interlayer film and at a position 15 mm from the other end. The printed portions were lines for alignment with the ends of the laminated glass component.

[0279] Example 12 An interlayer film and a roll body were produced in the same manner as in Example 11, except that a green printed portion was formed by inkjet printing a solid line having a line width of 1 mm using a Keyence Corporation "MK-U6000".

[0280] (Example 13) An interlayer film and a roll body were produced in the same manner as in Example 11, except that a white printed portion was formed by UV laser printing a solid line having a line width of 1 mm at a position 35 mm from one end side and a position 35 mm from the other end side of the unprinted interlayer film. The intensity of UV irradiation was 80%.

[0281] Example 14 An intermediate film and a roll body were produced in the same manner as in Example 11, except that a red printed area was formed by labeling 1 mm-wide dotted lines at a position 10 mm from one end of the unprinted intermediate film and a position 10 mm from the other end using "AMK-Clean" manufactured by Ayaha Engineering Co., Ltd.

[0282] Comparative Example 2 An interlayer film and a roll body were produced in the same manner as in Example 10, except that a printed portion was not formed.

[0283] Example 15 An interlayer film and a roll body were produced in the same manner as in Example 10, except that the dimensions of the interlayer film, such as its width, were changed as shown in Table 4, and a white printed portion was formed by UV laser printing a dotted line 100 mm wide at a position 10 mm from one end of the unprinted interlayer film and at a position 10 mm from the other end.

[0284] Example 16 An interlayer film and a roll body were produced in the same manner as in Example 10, except that the dimensions of the interlayer film, such as its width, were changed as shown in Table 4, and a white printed portion was formed by UV laser printing a dotted line with a line width of 220 mm at a position 5 mm from one end of the unprinted interlayer film and at a position 5 mm from the other end.

[0285] (Example 17) An interlayer film and a roll body were produced in the same manner as in Example 3, except that the dimensions of the interlayer film, such as its width, were changed as shown in Table 4, and a white printed portion was formed 5 mm from one end of the unprinted interlayer film by UV laser printing a solid line 300 mm wide.

[0286] (Example 18) An interlayer film and a roll body were produced in the same manner as in Example 1, except that a white printed area was formed by UV laser printing a two-dimensional code (QR code (registered trademark)) containing product information of the interlayer film at a position 100 mm from one end of the unprinted interlayer film.

[0287] (Example 19) An interlayer film and a roll body were produced in the same manner as in Example 1, except that a barcode containing product information about the interlayer film was printed by UV laser to form a white printed area 120 mm from one end of the unprinted interlayer film.

[0288] (Example 20) An interlayer film and a roll body were produced in the same manner as in Example 10, except that the dimensions such as the shape and width of the interlayer film were changed as shown in Table 4, and a colorless (transparent) printed portion was formed at a position 150 mm from one end of the interlayer film before printing by inkjet printing characters that are the product information of the interlayer film using "LINX 7900" manufactured by Almark. Incidentally, "Lynx UV Fluorescent Ink 1121" manufactured by Almark was used as the fluorescent toner.

[0289] Example 21 Preparation of the composition for forming the first layer: The following components were blended and thoroughly kneaded in a mixing roll to obtain a composition for forming a first layer.

[0290] Polyvinyl acetal resin (average degree of polymerization 3000, hydroxyl group content 22 mol%, acetylation degree 13 mol%, acetalization degree 65 mol%) 100 parts by weight Triethylene glycol di-2-ethylhexanoate (3GO) 60 parts by weight Tinuvin 326 (2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole, "Tinuvin 326" manufactured by BASF) in an amount of 0.2% by weight in the resulting first layer. BHT (2,6-di-t-butyl-p-cresol) in an amount of 0.2% by weight in the resulting first layer

[0291] Preparation of the composition for forming the second layer and the third layer except for the shaded area: The following components were blended and thoroughly kneaded with a mixing roll to obtain compositions for forming the second layer and the third layer.

[0292] Polyvinyl acetal resin (average polymerization degree 1700, hydroxyl group content 30.5 mol%, acetylation degree 1 mol%, acetalization degree 68.5 mol%) 100 parts by weight Triethylene glycol di-2-ethylhexanoate (3GO) 38 parts by weight Tinuvin 326 (2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole, "Tinuvin 326" manufactured by BASF) in an amount of 0.2% by weight in the resulting second and third layers. BHT (2,6-di-t-butyl-p-cresol) in an amount to provide 0.2% by weight in the resulting second and third layers, excluding the shaded areas.

[0293] Preparation of the composition for forming the shaded area in the second layer: The following components were blended and thoroughly kneaded with a mixing roll to obtain a composition for forming the shade region in the second layer.

[0294] Polyvinyl acetal resin (average polymerization degree 1700, hydroxyl group content 30.5 mol%, acetylation degree 1.0 mol%, acetalization degree 68.5 mol%) 100 parts by weight Triethylene glycol di-2-ethylhexanoate (3GO) 40 parts by weight Tinuvin 326 (2-(2'-hydroxy-3'-t-butyl-5-methylphenyl)-5-chlorobenzotriazole, BASF "Tinuvin 326") in an amount of 0.2% by weight in the resulting second layer (shaded area) BHT (2,6-di-t-butyl-p-cresol) in an amount that results in 0.2% by weight in the resulting interlayer (shade area) SG-1505 (anthraquinone compound, "BLUE SG-1505" manufactured by Sumika Color Co., Ltd.) (colorant) in an amount of 0.025% by weight in the resulting interlayer film (shade region)

[0295] Preparation of interlayer and roll body: A composition for forming the first layer, a composition for forming the second layer excluding the shaded region, a composition for forming the shaded region in the second layer, and a composition for forming the third layer were co-extruded using a co-extruder to obtain a pre-printed intermediate film. The obtained pre-printed intermediate film had a width (distance between one end and the other end) of 1016 mm, a length of 125 m, and a thickness of 780 μm, and had a shaded region in the region between one end and a position 150 mm from the one end toward the other end. Using Almark's "LINX 7900," a solid line with a line width of 5 mm was inkjet printed at a position 10 mm from one end of the pre-printed intermediate film and a position 10 mm from the other end to form a colorless (transparent) printed part, and an intermediate film having an intermediate film body and a printed part was produced (see Figures 7 and 8 for the shape of the outer shell). In addition, Almark's "Lynx UV Fluorescent Ink 1121" was used as the fluorescent toner.

[0296] The obtained interlayer film was wound around the outer periphery of a core in a roll shape in the same manner as in Example 1 to prepare a roll body.

[0297] (evaluation) (1) Distinguishability between the interlayer film itself and the printed part (1-1) Distinguishing ability under fluorescent lighting The interlayer films obtained in Examples 1 to 21 were evaluated as follows. When a person with a visual acuity of 1.0 visually examined the surface of the interlayer film having a printed portion from a position 70 cm away from the surface in a room illuminated with a fluorescent lamp, it was determined whether or not the printed portion could be distinguished from the interlayer film body. Note that the interlayer films obtained in Comparative Examples 1 and 2 were not evaluated because they did not have a printed portion.

[0298] (1-2) Discrimination under irradiation with light of 365 nm wavelength The interlayer films obtained in Examples 20 and 21 using fluorescent toner were evaluated as follows: When light with a wavelength of 365 nm was irradiated and a person with a visual acuity of 1.0 visually examined the surface of the interlayer film having a printed portion from a position 70 cm away, it was judged whether the printed portion could be distinguished from the main body of the interlayer film.

[0299] [Criteria for distinguishing between the interlayer film body and the printed part] ○: The interlayer film body and the printed part can be clearly distinguished. △: The interlayer film body and the printed part are slightly distinguishable ×: The interlayer film body and the printed part cannot be distinguished.

[0300] (2) Light irradiation test (2-1) Brightness Two clear float glasses (first and second clear float glasses) with a size of 300 mm x 150 mm and a thickness of 2 mm in accordance with JIS R3202:2011 were prepared. A roll-shaped interlayer film was developed and cut into a length of 30 cm in the TD direction (vertical) and 15 cm in the MD direction (horizontal), to prepare an interlayer film for light irradiation test. The interlayer film for light irradiation test was prepared so that the surface of the interlayer film for light irradiation test had the above-mentioned printed part and a part where the above-mentioned printed part was not formed. The interlayer film for light irradiation test was sandwiched between the first clear float glass and the second clear float glass so that the printed part of the interlayer film for light irradiation test was located on the first clear float glass side, and pre-pressed under conditions of 240 ° C and a linear pressure of 98 N / cm. Then, it was pressed under conditions of 140 ° C and a pressure of 1.3 MPa to obtain a laminated glass for light irradiation test.

[0301] A strong light source device ("S-Light SA160" manufactured by Nippon Gijutsu Center Co., Ltd.) was installed at a height of 80 cm from the floor, facing perpendicularly to the floor at an angle of 15 degrees from the floor. The laminated glass for light irradiation test was placed at a position 175 cm away from the strong light source device and at a position where the center of the laminated glass was 1 m above the floor, so that the surface direction of the laminated glass for light irradiation test was perpendicular to the irradiation direction of the strong light source and the first clear glass side of the laminated glass was the strong light source side. Light was irradiated from the strong light source to the laminated glass, and an inspector with a visual acuity of 1.0 visually confirmed the shadow projected by the area of ​​the interlayer of the laminated glass for light irradiation test corresponding to the above-mentioned printed part on the back side 25 cm from the laminated glass for light irradiation test, and judged the presence or absence of a difference in the brightness of the shadow.

[0302] The interlayer films obtained in Comparative Examples 1 and 2 were not evaluated because no printed portion was formed thereon.

[0303] [Criteria for light irradiation test (brightness)] A: No difference in brightness B: There is a difference in brightness

[0304] When the evaluation result was "A," a person with a visual acuity of 1.0 was unable to distinguish between the printed portion and the interlayer film body when visually observing the surface of the laminated glass for light irradiation test on the first clear float glass side from a distance of 70 cm.

[0305] (2-2) Difference in parallel light transmittance between the area corresponding to the printed portion and the area corresponding to the non-printed portion Using a laminated glass for light irradiation test, the parallel light transmittance of the area corresponding to the printed part and the area corresponding to the non-printed part around the printed part was measured in accordance with JIS R3106:1998 as follows. Using a spectrophotometer (Hitachi High-Tech Corporation "U-4100"), the laminated glass for light irradiation test was installed so that the area corresponding to the printed part or the area corresponding to the non-printed part around the printed part was located parallel to the normal line of the optical axis on the optical path between the light source and the integrating sphere and 13 cm away from the integrating sphere so that only the transmitted parallel light was received by the integrating sphere. In this state, the spectral transmittance was measured. The visible light transmittance was calculated from the obtained spectral transmittance, and the parallel light transmittance of the area corresponding to the printed part and the parallel light transmittance of the area corresponding to the non-printed part around the printed part were obtained. The absolute value of the difference between the parallel light transmittance of the area corresponding to the printed part and the parallel light transmittance of the area corresponding to the non-printed part around the printed part was obtained.

[0306] [Criteria for light irradiation test (difference in parallel light transmittance)] A: The absolute value of the difference in parallel light transmittance is 5% or less B: The absolute value of the difference in parallel light transmittance exceeds 5%

[0307] (3) Shade area misalignment For the interlayer films obtained in Examples 3 to 8, 17, and 21 and Comparative Example 1, the following evaluation of positional deviation of the shade region was performed.

[0308] Laminated glass preparation: A pair of glass plates (clear glass, size 510 mm×910 mm, thickness 2.0 mm) having the outer shape of the laminated glass member G1G shown in FIG. 8 was prepared. For the interlayer film obtained in Examples 3 to 8, 17, and 21, a roll-shaped interlayer film was developed, and the first laminated glass member and the second laminated glass member were bonded together using the printed portion as a guide, and the protruding portion was trimmed off to obtain a laminate. For the interlayer film obtained in Comparative Example 1, a roll-shaped interlayer film was developed, and the first laminated glass member and the second laminated glass member were bonded together, and the protruding portion was trimmed off to obtain a laminate. The obtained laminate was preheated in an oven until the surface temperature of the glass plate reached 50° C., and then transferred into a rubber bag. The rubber bag was then connected to a suction vacuum machine, and heated while simultaneously maintaining a reduced pressure of -600 mmHg, so that the temperature of the laminate (pre-bonding temperature) reached 90°C in 18 minutes, and then the pressure was returned to atmospheric pressure to terminate the pre-bonding, thereby obtaining a pre-bonded laminate. The pre-bonded laminate was bonded in an autoclave at 150°C and a pressure of 1.2 MPa to obtain a laminated glass.

[0309] In the same manner, a total of 10 pieces of laminated glass were produced.

[0310] Ten sheets of laminated glass were lined up, and the positions of the tips of the shaded areas were visually confirmed.

[0311] [Criteria for determining the positional deviation of the shaded area] ○: No misalignment of the shaded area is observed ×: Positional deviation of the shaded area is observed

[0312] (4) Double image The interlayer films obtained in Examples 9 to 16 and Comparative Example 2 were evaluated for double images as follows.

[0313] Laminated glass preparation: A pair of glass plates (clear glass, size 510 mm×920 mm, thickness 2.0 mm) was prepared. For the interlayer film obtained in Examples 9 to 16, a roll-shaped interlayer film was developed, and the first laminated glass member and the second laminated glass member were bonded together using the printed portion as a guide, and the protruding portion was trimmed off to obtain a laminate. For the interlayer film obtained in Comparative Example 2, a roll-shaped interlayer film was developed, and the first laminated glass member and the second laminated glass member were bonded together, and the protruding portion was trimmed off to obtain a laminate. The obtained laminate was fitted into an EPDM rubber tube (frame member) as shown in FIG. 12. The width of the rubber tube was 15 mm. Next, the laminate fitted into the EPDM rubber tube was pre-pressed. The pre-pressed laminate was pressed at 150° C. and a pressure of 1.2 MPa using an autoclave to obtain a laminated glass.

[0314] In the same manner, a total of 10 pieces of laminated glass were produced.

[0315] The obtained laminated glass was placed at the position of the windshield. Display information from a display unit placed below the laminated glass was reflected onto the laminated glass, and the presence or absence of double images was visually confirmed at a specified position (the center of the display-compatible area). The presence or absence of double images was judged according to the following criteria.

[0316] [Criteria for determining double images] ○: No double images were observed for any of the laminated glass. ×: Double images are observed in 1 or more of the 10 images.

[0317] Details and results are shown in the following Tables 1 to 4. In Tables 1 to 4, "markers for alignment with the edge of the laminated glass member" or "markers for alignment of the HUD area" are described as "markers for alignment."

[0318] [Table 1]

[0319] [Table 2]

[0320] [Table 3]

[0321] [Table 4] [Explanation of symbols]

[0322] 1,1A,1B,1C,1D,1E,1F,1G...First layer 1Aa, 1Ca, 1Ea... Sections with a rectangular cross-sectional shape in the thickness direction 1Ab, 1Cb, 1Eb... Sections whose cross-sectional shape in the thickness direction is wedge-shaped 1AX,1CX,1EX…Colored section 1AY,1CY,1EY…Uncolored area 2, 2B, 2D, 2G...Second layer 3,3B,3D,3G…Third layer 3X,3BX,3DX,3GX…Colored section 3Y,3BY,3DY,3GY…Uncolored part 4, 4A, 4F, 4G…Printing section 4a, 4Aa, 4Ga...solid line 4b, 4Ab, 4Fb…dotted line 4Fc...letters 11,11A,11B,11C,11D,11E,11F,11G,11-2...Intermediate film 11a…one end 11b...other end 11Aa, 11Ca, 11Ea... Sections with a rectangular cross-sectional shape in the thickness direction 11Ab, 11Cb, 11Eb... Sections whose cross-sectional shape in the thickness direction is wedge-shaped 11X...Intermediate film part 21...Laminated glass 22...First laminated glass member 23...Second laminated glass member R1: Display area R2: Surrounding area R3: Shade area G1, G1A, G1F, G1G...Laminated glass components 51...Roll body 61...Core

Claims

1. An interlayer film for laminated glass includes: an interlayer film for laminated glass; and a printed portion that is displayed by printing on a first surface of the interlayer film for laminated glass; The printed portion is a printed portion displayed by UV laser printing, The interlayer film for laminated glass, wherein the printed portion is a mark for a bonding position to a laminated glass member or is product information of the interlayer film for laminated glass.

2. The interlayer film for laminated glass according to claim 1 , wherein the printed portion is a mark for a bonding position to a laminated glass member.

3. The interlayer film for laminated glass according to claim 1 or 2, wherein the printed portion is displayed as a line, a character, a symbol or a graphic.

4. The interlayer film for laminated glass according to claim 3 , wherein the printed portion has a portion displayed as a line having a line width of 10 mm or less.

5. A wire has one end and another end opposite the one end, The thickness of the other end is greater than the thickness of the one end, The interlayer film for laminated glass according to any one of claims 1 to 4, wherein the interlayer film has a wedge angle of 0.1 mrad or more throughout the entire film.

6. An intermediate film for laminated glass as described in any one of claims 1 to 5, wherein, when laminated glass is obtained by the production method described below, in the obtained laminated glass, the absolute value of the difference between the parallel light transmittance of a region of the intermediate film corresponding to the printed portion and the parallel light transmittance of a region corresponding to the non-printed portion around the printed portion is 5% or less. Method for producing laminated glass: Prepare a first clear glass having a thickness of 2 mm conforming to JIS R3202:2011 and a second clear glass having a thickness of 2 mm conforming to JIS R3202:2011. The interlayer film is sandwiched between the first clear glass and the second clear glass so that the printed portion of the interlayer film is located on the first clear glass side, and pre-press-bonded under conditions of 240°C and a linear pressure of 98 N / cm. Then, press-bonding is performed under conditions of 140°C and a pressure of 1.3 MPa to obtain laminated glass.

7. An interlayer film for laminated glass used in laminated glass for a head-up display, The interlayer film for laminated glass according to any one of claims 1 to 6, having a display corresponding area corresponding to a display area of ​​a head-up display.

8. The interlayer film for laminated glass according to any one of claims 1 to 7, which has a shade region.

9. The interlayer film for laminated glass according to any one of claims 1 to 8, which is used for a front glass, a side glass, a rear glass, or a roof glass of a vehicle.

10. A winding core and The interlayer film for laminated glass according to any one of claims 1 to 9, The interlayer film for laminated glass is wound around the outer periphery of the winding core.

11. A method for producing laminated glass comprising: a first laminated glass member; a second laminated glass member; and an interlayer film for laminated glass disposed between the first laminated glass member and the second laminated glass member, the method comprising the steps of: the interlayer film for laminated glass comprises an interlayer film for laminated glass main body and a printed portion displayed by printing on a first surface of the interlayer film main body, the printed portion being a mark for indicating a position for attachment to a laminated glass component, a first disposing step of disposing the first laminated glass component on a first surface of the interlayer film for laminated glass; a second disposing step of disposing the second laminated glass component on a second surface of the interlayer film for laminated glass opposite to the first surface, the first arranging step is to bond the first laminated glass member and the interlayer film for laminated glass together using the printed portion of the interlayer film for laminated glass as a mark, or the second arranging step is to bond the second laminated glass member and the interlayer film for laminated glass together using the printed portion of the interlayer film for laminated glass as a mark.

Citation Information

Patent Citations

  • Laminated glass having plastic film inserted therein

    JP2009161407A

  • Resin and method for producing resin

    JP2017110036A

  • Method for producing laminated glass laminate from laminate having plasticizer-containing polyvinyl acetal sheet and polyvinyl acetal sheet having less plasticizer

    JP2018052810A

  • Processing method of substrate

    JP2018083228A

  • Interlayer film for laminated glass, and laminated glass

    WO2017039004A1