Ceramic Core
A ceramic core with a layered structure and controlled porosity addresses strength and solubility issues, enabling efficient production of high-quality single-crystal or directionally solidified alloys by suppressing recrystallization and facilitating easy disintegration.
Patent Information
- Application Number
- JP2021058880
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-30
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2041-03-30
AI Technical Summary
Ceramic cores used in precision casting for high-temperature applications, such as turbine blades, face challenges with strength, surface roughness, and solubility, leading to potential recrystallization defects and inefficiencies in manufacturing single-crystal or directionally solidified alloys.
A ceramic core with a layered structure and specific composition, made from a mixture of inorganic particles, is designed to have a porosity of 20-40% and a smooth outer surface, allowing it to withstand high temperatures and easily disintegrate during casting, while being soluble in alkaline solutions.
The ceramic core effectively suppresses recrystallization defects, ensures high yield production of single-crystal or directionally solidified alloys, and simplifies post-processing due to its smooth surface and excellent collapsibility.
Smart Images

Figure 0007557409000006 
Figure 0007557409000007 
Figure 0007557409000012
Abstract
Description
[Technical field]
[0001] The present invention relates to a ceramic core having excellent disintegratability. [Background technology]
[0002] Superalloys such as Ti-based alloys, Ni-based alloys, and Co-based alloys are used in heat-resistant structural components such as turbine blades, jet engines, and turbochargers that are used in high-temperature environments (e.g., 1100°C or higher). Among these heat-resistant structural components, for example, turbine blades are provided with hollow cooling holes, which are air passages that are designed in a complex and highly precise manner, in order to ensure both strength and cooling function.
[0003] Heat-resistant structural components having hollow cooling holes are generally metal castings produced by a precision casting method such as the lost wax method (Patent Document 1). Specifically, heat-resistant structural components are produced by using a mold with an internal space corresponding to the external structure of the component and a core with a shape corresponding to the desired hollow cooling hole, pouring the molten superalloy (molten metal) into the cavity formed by the mold and core and allowing it to solidify, and then dissolving the core with an alkaline solution or the like to form the hollow cooling hole.
[0004] Since heat-resistant structural components require high strength in high-temperature environments, when producing metal castings by precision casting, it is necessary to control the crystallinity of the alloy, especially when the molten metal is cooled. Specifically, after pouring molten metal into the space formed by the mold and the core, the molten metal is cooled and pulled out in one direction to solidify. This produces a metal casting made of a single crystal alloy or a directionally solidified alloy, which is called the directional solidification method. Metal castings made of a single crystal alloy or a directionally solidified alloy have high strength that can withstand use in high-temperature environments.
[0005] Figure 1 shows a schematic diagram of a method for producing metal castings using the unidirectional solidification method. Figure 2 shows a schematic diagram of the internal structure of a mold with a core inside. Mold 1, into which molten metal such as a Ni-based alloy has been poured, is pulled downward from a heating furnace 2, which is kept at a temperature at which the metal will melt, while being cooled by a cooling plate 3, to produce a metal casting 4 (see Figure 1). In particular, when producing a metal casting made of a single crystal alloy, a part for selecting crystals, called a selector 5, or a seed crystal 6 is placed inside the mold (see Figure 2). As mentioned above, cores are used when producing the cooling structure inside the casting, and the structure of cores is becoming more complex every year in order to create more complex and efficient cooling structures.
[0006] During casting, the core is exposed to molten metal at around 1500°C for a long period of time, and may be damaged or deformed due to thermal expansion or the pouring of molten metal. For this reason, the core is required to have mechanical strength at high temperatures and stability that does not cause dimensional deformation. Generally, molds and cores are required to be heat resistant to molten metal, so refractory materials made of ceramic are used. For this reason, the core for this purpose is also called a ceramic core (hereinafter, the ceramic core will also be simply called the core).
[0007] A typical ceramic core used in the above-mentioned precision casting method is manufactured by pouring ceramic clay or ceramic slurry (hereinafter referred to as clay and slurry, respectively) into a mold, forming it, and then firing it to obtain a so-called near-net shape (a state close to the finished product that does not require post-processing). Conventional ceramic cores are manufactured, for example, by an injection molding method (also called a CIM method) that uses a mold. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 7-214234 [Non-patent literature]
[0009] [Non-Patent Document 1] Hidetaka Oguma and 5 others, "Mitsubishi Heavy Industries Technical Review", Mitsubishi Heavy Industries, Ltd., Vol. 52, No. 4, (2015), Special Feature on New Products and New Technologies, pp. 5-14 Summary of the Invention [Problem to be solved by the invention]
[0010] The ceramic core can be manufactured by additive manufacturing, etc., in addition to the injection molding method. The additive manufacturing method makes it possible to easily obtain members having complex shapes with fewer steps than conventional processing methods.
[0011] When ceramic cores are manufactured by additive manufacturing, it is possible to manufacture cores with complex shapes and more efficiently than with conventional manufacturing methods. However, additive manufacturing may have a lower strength than cores manufactured by conventional injection molding methods due to the layered structure. In addition, the outer periphery of the additively manufactured core is likely to become uneven (surface roughness is likely to become rough), and additional work may be required in a post-process. Therefore, ceramic cores manufactured by additive manufacturing are required to have low surface roughness (smoothness) so that the opposing casting surface is smooth, and strength that can withstand high-temperature casting.
[0012] In addition, when casting metal castings made of single crystal alloys or directionally solidified alloys, the molten metal undergoes thermal contraction during cooling and solidification. If the ceramic core is too strong and does not collapse sufficiently, the solidifying metal may be subjected to stress, resulting in poor recrystallization (polycrystallization). After cooling is complete, the ceramic core is dissolved and removed using an alkaline solution such as an aqueous sodium hydroxide solution, or physically collapsed and removed, so it is also required to be soluble in the alkaline solution.
[0013] The present invention has been made in consideration of the above circumstances, and has an object to provide a ceramic core for use in a unidirectional solidification method, which has excellent disintegrability and solubility and can suppress the occurrence of poor recrystallization. [Means for solving the problem]
[0014] The ceramic core of the present invention is a ceramic core used in a directional solidification method in which molten metal is poured into the space formed by a mold and a core, and the molten metal is cooled and pulled out in one direction while solidifying to obtain a metal casting made of a single crystal alloy or a directionally solidified alloy, and is characterized in that it is a porous ceramic body having a layered structure with a stacking direction that does not coincide with the solidification direction of the alloy.
[0015] The ceramic core is characterized in that it has the layered structure at a portion of a cross section of the ceramic core and the alloy perpendicular to the solidification direction, the portion corresponding to a cross section in which the area ratio of the ceramic core to the alloy changes when viewed from before to after the solidification direction.
[0016] The ceramic core is characterized in that the base material is a molded body having the layered structure described above, which is made of a mixture of two or more types of inorganic particles selected from silica, alumina, zircon, magnesia, calcia, yttria, and zirconia, and the pores of the base material are partially sealed and the base material has a coating layer on its outermost surface.
[0017] The coating layer is characterized by containing silica.
[0018] The outermost surface has an arithmetic mean roughness of 10 μm or less.
[0019] The ceramic core has a porosity of 20% to 40% as measured by Archimedes' method.
[0020] The ceramic core is characterized in having the layered structure in a region corresponding to a cross section in which the area ratio of the ceramic core to the alloy in a cross section across the solidification direction changes by 2% or more per mm across the solidification direction. Effect of the Invention
[0021] The ceramic core of the present invention is a ceramic core used in a unidirectional solidification method in which molten metal is poured into a space formed by a mold and a core, and the molten metal is cooled and drawn out in one direction while solidifying to obtain a metal casting made of a single crystal alloy or a directionally solidified alloy. Since the ceramic core is a ceramic porous body having a layered structure with a lamination direction that does not match the solidification direction of the alloy, the ceramic core is easily broken down and collapsed in small pieces starting from between the layers of the layered structure in accordance with the thermal contraction during casting. Since the core has excellent collapseability, recrystallization (polycrystallization) is unlikely to occur when the molten metal solidifies and thermally contracts, and single crystal alloys or directionally solidified alloys can be produced with a high yield by casting using the unidirectional solidification method. In addition, the ceramic core of the present invention has excellent solubility, and when it is dissolved and removed with an alkaline solution after casting, the alkaline solution easily penetrates between the layers of the layered structure.
[0022] The ceramic core has a layered structure in a region corresponding to a cross section of the ceramic core and alloy perpendicular to the solidification direction where the area ratio of the ceramic core to the alloy changes when viewed from before to after the solidification direction. This makes the core more susceptible to collapse due to thermal contraction during casting (it has excellent collapsibility).
[0023] The ceramic core has a layered structure formed as a base material, which is a molded body made of a mixture of two or more types of inorganic particles selected from silica, alumina, zircon, magnesia, calcia, yttria, and zirconia. Some of the pores in the base material are sealed, and the core has a coating layer on the outermost surface of the base material, so that the core has a strength sufficient to withstand high-temperature casting.
[0024] Since the coating layer contains silica, it has excellent solubility in an alkaline solution.
[0025] Since the arithmetic mean roughness of the outermost surface is 10 μm or less, the surface of the core is smooth with small surface roughness, and the opposing casting surface (the inner surface of the metal casting) is smooth, eliminating the need for additional work in post-processing.
[0026] The ceramic core has a porosity of 20% to 40% as measured by Archimedes' method, and therefore has strength sufficient to withstand high-temperature casting while also exhibiting excellent collapsibility.
[0027] The ceramic core has a layered structure at a cross section where the area ratio of the ceramic core to the alloy in the cross section before and after the solidification direction changes by 2% or more per mm before and after the solidification direction, so that single crystal alloys or directionally solidified alloys can be produced with a higher yield by casting using the directional solidification method. [Brief description of the drawings]
[0028] [Figure 1] FIG. 1 is a schematic diagram of a method for producing a metal casting by directional solidification. [Diagram 2] FIG. 2 is a schematic diagram of the internal structure of a mold. [Diagram 3] FIG. 2 is a diagram showing the relationship between the stacking direction of the layered structure and the solidification direction. [Figure 4] FIG. 2 is a diagram showing the relationship between the stacking direction of the layered structure and the solidification direction. [Diagram 5] 1A-1C are schematic diagrams of examples of ceramic core arrangements within a mold. [Figure 6] 1 is a flowchart of a method for manufacturing a ceramic core of the present invention. [Figure 7] FIG. 2 is a perspective view showing the layered structure (stacking direction) of two types of molded bodies. [Figure 8] 1 is an electron microscope photograph of the surface of a test piece before coating. [Figure 9] 1 is an electron microscope photograph of the surface of a test piece after coating. [Figure 10] 1 is an electron microscope photograph of a cross section of a test piece after coating. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] When producing a metal casting made of a single crystal alloy or a directionally solidified alloy, recrystallization may occur due to the unique shape of each core. For example, in FIG. 2, the AA, BB, and CC cross sections of the ceramic core are cross sections of the ceramic core and the alloy perpendicular to the solidification direction Db of the alloy, in which the area ratio of the ceramic core to the alloy changes significantly when viewed from before to after the solidification direction, so that foreign crystals are likely to occur due to recrystallization during the production of the metal casting. Since the occurrence of foreign crystals leads to polycrystallization and is undesirable, in the past, the attitude (position) of the casting and the core was changed so that the area ratio of the cross sections of the core and the metal did not change significantly. However, as the structure of the core becomes more complex, it is becoming more difficult to deal with it just by changing the position. In response to this, the present inventors have found that by making the ceramic core used in the directional solidification method for obtaining a metal casting made of a single crystal alloy or a directionally solidified alloy into a ceramic porous body having a layered structure, the ceramic core has excellent disintegrability and solubility.
[0030] The ceramic core of the present invention will be described with reference to Figs. 3 to 5. Figs. 3 and 4 are schematic diagrams of casting by unidirectional solidification using a ceramic core produced by the additive manufacturing method described later, and are diagrams showing the relationship between the lamination direction and the solidification direction of the layered structure of the ceramic core. The ceramic core is a ceramic porous core produced by molding ceramic powder as a raw material by the additive manufacturing method and then firing it. The ceramic core is used as a core for the unidirectional solidification method in which molten metal is poured into the space formed by the mold and the core, and the molten metal is cooled and drawn out in one direction while solidifying to obtain a metal casting made of a single crystal alloy or a directionally solidified alloy.
[0031] Figures 3 and 4 show different combinations of the relationship between the stacking direction Da of the ceramic core and the solidification direction Db of the alloy when producing the metal casting. In Figure 3(a), the stacking direction Da is perpendicular to the solidification direction Db at an angle α=90°, and in Figure 3(b), the stacking direction Da is inclined at an angle α=45° to the solidification direction Db, and the directions do not match in each figure. In contrast, in Figure 4, the stacking direction Da and the solidification direction Db match.
[0032] As shown in Figs. 3(a) and (b), in the unidirectional solidification method, when the solidification direction Db does not coincide with the stacking direction Da of the ceramic core 7 having a layered structure, the ceramic core 7 is easily broken and collapsed in accordance with the thermal contraction of the cast metal 4 during casting, starting from the interlayer of the layered structure. The ceramic core of the present invention has excellent core collapse properties, so that recrystallization (polycrystallization) is unlikely to occur when the molten metal solidifies and thermally contracts, and a single crystal alloy or a directionally solidified alloy can be produced with a high yield by casting using the unidirectional solidification method. In addition, when the ceramic core of the present invention is eluted and removed with an alkaline solution after casting, the alkaline solution easily penetrates between the layers of the layered structure, and it is also excellent in solubility. On the other hand, when the stacking direction Da and the solidification direction Db coincide with each other as shown in Fig. 4, the ceramic core 7 is unlikely to break and collapse in accordance with the thermal contraction of the cast metal 4 during casting.
[0033] When producing metal castings such as turbine blades by the unidirectional solidification method, the ceramic core has a substantially wing-like shape, and therefore, when the ceramic core is placed inside the mold, it is placed so that the long axis direction of the core is substantially the same as the solidification direction. Therefore, when the lamination direction of the core is set along the short axis direction of the core, the lamination direction and the solidification direction are unlikely to coincide with each other, which is preferable because the core has excellent disintegration properties.
[0034] The ceramic core has a layered structure at a portion corresponding to a cross section where the area ratio of the ceramic core to the alloy changes when viewed before and after the solidification direction among the cross sections of the ceramic core and the alloy perpendicular to the solidification direction. The ceramic core only needs to have a layered structure at a portion corresponding to a cross section where the area ratio of the ceramic core to the alloy changes when viewed before and after the solidification direction among the cross sections of the ceramic core and the alloy perpendicular to the solidification direction, and may not have a layered structure at a portion corresponding to a cross section where the area ratio of the ceramic core to the alloy does not change when viewed before and after the solidification direction among the cross sections of the ceramic core and the alloy perpendicular to the solidification direction. When the layered structure is present at a portion corresponding to a cross section where the area ratio of the ceramic core to the alloy changes, the core is more likely to collapse due to thermal contraction during casting (it has better collapse properties).
[0035] The ceramic core is based on a molded body having a layered structure made of a mixture of two or more inorganic particles selected from silica, alumina, zircon, magnesia, calcia, yttria, and zirconia, some of whose pores are sealed, and has a coating layer on the outermost surface. The mixture of inorganic particles that is the raw material of the molded body, the material that seals the pores, and the material of the coating layer may each contain the same inorganic particles or different inorganic particles.
[0036] If the molded body contains different inorganic particles, for example silica (SiO 2 ) and zircon (ZrSiO 4 The molded body is made of ceramic powder consisting of silica (SiO 2 ) and zircon (ZrSiO 4 ) can be used as a sol.
[0037] The sealing of the pores and the formation of the coating layer are carried out, for example, by impregnating the molded body with a sol. When the molded body is impregnated with a sol, the outer peripheral surface of the molded body is coated with a coating layer. By sealing the pores and forming the coating layer, the strength inside the ceramic core is improved, and a smooth film without defects is formed on the outermost peripheral surface, so that the mechanical strength of the ceramic core as a whole is improved and the ceramic core has a strength that can withstand high-temperature casting. The coating layer may or may not contain silica. When the coating layer contains silica, it is preferable because the ceramic core after casting has excellent solubility in an alkaline solution.
[0038] The outermost peripheral surface of the ceramic core is preferably smooth from the viewpoint of improving the strength of the core and making the cast metal near-shape. Specifically, the arithmetic mean roughness of the outermost peripheral surface is preferably 10 μm or less. When the arithmetic mean roughness of the outermost peripheral surface is 10 μm or less, the surface of the core is smooth and has small surface roughness, and the opposing cast surface (the inner peripheral surface of the metal casting) is smooth, making additional work in a post-process unnecessary. More preferably, it is 8 μm or less. The lower limit of the arithmetic mean roughness of the outermost peripheral surface is not particularly limited, but is usually 0.5 μm or more.
[0039] The arithmetic mean roughness Ra in the present invention is calculated in accordance with JIS B 0601. A contact or non-contact surface roughness measuring instrument is used for the measurement. Since the core is obtained by the additive manufacturing method and has a surface roughness of about 10 μm or less as described above, the measurement condition is preferably a cutoff value of 2.5 mm (the measurement length is at least three times this).
[0040] As described above, the ceramic core is a ceramic porous body. The porosity of this porous body measured based on the Archimedes method is preferably 20% to 40%. From the viewpoint of collapsibility, the porosity is more preferably 30% to 40%, and from the viewpoint of strength required for use, the porosity is more preferably 20% to 30%. When the porosity is within this range, a sufficient amount of ceramic parts required for the strength of the core is secured, and the core contains sufficient void parts to serve as a path for the penetration of an alkaline solution, so that the core has strength that can withstand high-temperature casting and excellent collapsibility.
[0041] The porosity in the present invention is measured by the following Archimedes method. First, the dry weight W1 of the core is measured. Next, the core is immersed in water to saturate it, and the underwater weight W2 is measured by suspending the core in the water. Finally, the core is taken out of the water, the surface moisture is quickly wiped off, and the saturated weight W3 is measured. Using these, the apparent porosity (%) is measured according to the following formula. Note that the amount of pores measured by this method is only the pores (surface-connected pores) that are open to the core surface, and does not include closed pores (surface non-connected pores). Porosity (%) = 100 x (saturated weight W3 - dry weight W1) / (saturated weight W3 - submerged weight W2) = 100 x [open pore volume] / [external volume]
[0042] The ceramic core preferably has a layered structure in a section corresponding to a cross section where the area ratio of the ceramic core to the alloy changes by 2% or more per mm in the solidification direction in the cross section in the solidification direction. This ensures that the layered structure is always located in a section where recrystallization is relatively likely to occur, allowing single crystal alloys or directionally solidified alloys to be produced with a higher yield by casting using the directional solidification method.
[0043] FIG. 5 is a schematic diagram of an example of the arrangement of ceramic cores in a mold. In FIG. 5(a), the long axis direction of the mold 1 coincides with the solidification direction Db, but the stacking direction Da is inclined with respect to the solidification direction Db. In FIG. 5(b), the long axis direction of the mold 1 does not coincide with the solidification direction Db, and the stacking direction Da is also inclined with respect to the solidification direction Db. As for the ceramic core 7, the direction and shape of the mold can be freely selected as long as the solidification direction Db and the stacking direction Da do not coincide with each other.
[0044] The angle α between the solidification direction Db and the stacking direction Da can be freely selected as long as it is other than 0°. From the viewpoint of collapsibility, the angle α is preferably 45° to 90°. When the angle α is within this range, the strength of the core in the direction of the stress when the molten metal solidifies and shrinks is lower, resulting in better collapsibility.
[0045] An embodiment of the method for producing a ceramic core of the present invention will be described below with reference to Fig. 6. However, the method for producing a ceramic core of the present invention is not limited to the following.
[0046] FIG. 6 is a flow chart of the manufacturing method. As shown in FIG. 6, the manufacturing method S1 of the ceramic core includes a mixing step S10 of mixing two or more kinds of inorganic particles, an additive manufacturing step S20 of forming a molded body by additive manufacturing using the mixture obtained in the mixing step S10, an impregnation step S30 of impregnating the molded body with a reinforcing agent, and a sintering step S40 of sintering the molded body impregnated with the reinforcing agent. The manufacturing method S1 of the ceramic core further includes an impregnation step S50 of impregnating the molded body obtained in the sintering step S40 with a reinforcing agent. The manufacturing method of the ceramic core of the present invention does not have to include the impregnation step S50.
[0047] In the mixing step S10, for example, silica powder having an average particle size of about 40 μm and zircon powder having an average particle size of about 20 μm are mixed using a ball mill to obtain a mixture of these two types of inorganic particles. Note that the inorganic particles are not limited to these, and other materials may be used. For example, alumina or zirconia may be selected, and amorphous silica or cristobalite may be selected as silica. The average particle size can be measured, for example, using a particle size distribution measuring device using a laser light scattering method.
[0048] In the additive manufacturing process S20, the molded body can be formed by a method freely selected from the additive manufacturing methods shown below or other additive manufacturing methods. As additive manufacturing methods, for example, there are a powder deposition method in which raw material powder is deposited only in a predetermined place and sintered or melted by irradiating it with laser light, and a powder bed method in which raw material powder is deposited on one side of a base plate of an additive manufacturing device and sintered or melted by irradiating it with laser light only in a predetermined place. In addition, there is a binder injection method in which the raw material powder is solidified by injecting a binder (binder) for solidifying the powder raw material from an inkjet nozzle, and then molded. In either method, the deposition of raw material powder and the solidification or solidification of the raw material powder are repeated, and an additive manufacturing product (molded body) is formed by stacking layers.
[0049] The impregnation step S30 is performed following the additive manufacturing step S20. In the impregnation step S30 of this embodiment, the molded body obtained in the additive manufacturing step S20 is impregnated with a reinforcing agent. In this step, for example, the molded body is impregnated with a solution in which a silane coupling agent is dissolved in an organic solvent as a reinforcing agent.
[0050] In the sintering step S40, the molded body impregnated with the reinforcing agent in the impregnation step S30 is dried, and then sintered, for example, by firing for two hours at about 1250° C. By subjecting the additively manufactured molded body to the impregnation step S30 and the sintering step S40, the layers of the layered structure are connected and sintered, promoting integration of the molded body and improving the strength of the core.
[0051] The impregnation step S50 is carried out following the sintering step S40. In the impregnation step S50 of this embodiment, the molded body obtained in the sintering step S40 is vacuum-impregnated with a reinforcing agent. In the vacuum impregnation, for example, a water dispersion of nano-silica (silica sol) is used as a reinforcing agent to impregnate the molded body in a reduced pressure vessel, and the air contained in the molded body is removed and the reinforcing agent is pressed in. After the vacuum impregnation, for example, firing is performed at 400°C to 600°C. This step seals some of the pores inside the molded body, and a coating layer is formed on the outermost peripheral surface. Examples of the reinforcing agent used in this step include the above-mentioned silica sol, a mixture of silica and alumina, or a sol of a mixture of silica and zircon. The impregnation step S50 may be repeated multiple times. When the impregnation step S50 is repeated multiple times, the reinforcing agent used in each impregnation step may be the same or different. A specific example of a suitable coating layer is a multilayer structure having a silica layer and a reinforcing silica layer containing 95 mass% or more of silica and zircon.
[0052] In the impregnation process S50, the core is impregnated multiple times with silica slurry (silica sol), and then impregnated (coated) with a mixture of silica and zircon. This results in a layered structure inside the core and a smooth outer periphery that also contains silica, making it an ideal ceramic core with excellent solubility.
[0053] At the end of the impregnation step S50, the molded body is fired, for example, at about 1300° C. for 2 hours to obtain a ceramic core. By impregnating the silica sol in the impregnation step S50 after the sintering step S40, the porosity of the core can be reduced, the strength can be improved, and the surface step (surface roughness) can be reduced.
[0054] The manufacturing method of the present invention can manufacture a core having an uneven surface, which is impossible to manufacture by injection molding due to the problem of demolition, by forming the base material of the core by an additive manufacturing process. This makes it suitable for manufacturing metal castings of complex shapes. In addition, the manufacturing method of the present invention includes an additive manufacturing process, so that a ceramic core designed to have a desired layered structure can be freely manufactured at a portion corresponding to a cross section where the area ratio of the ceramic core and the alloy changes when viewed from before to after the solidification direction among the cross sections of the ceramic core and the alloy perpendicular to the solidification direction, and recrystallization can be suppressed by micro-fracturing the core during thermal contraction during casting.
[0055] The manufacturing method of the present invention includes an impregnation step of impregnating a compact with a reinforcing agent between the additive manufacturing step and the sintering step, so that a ceramic core having a smooth surface and a layered structure inside can be manufactured. This makes it possible to manufacture a ceramic core with small surface roughness, strength sufficient to withstand high-temperature casting, and excellent disintegrability and solubility.
[0056] The method for producing a heat-resistant structural component using the ceramic core of the present invention will be described below. The method for producing a heat-resistant structural component of the present invention includes a directional solidification method in which molten metal is poured into a space formed by a mold and a core, and the molten metal is cooled and drawn out in one direction to solidify, thereby obtaining a metal casting made of a single crystal alloy or a directionally solidified alloy, and is characterized in that the core has a layered structure and is arranged inside the mold so that the layered direction of the layered structure does not coincide with the solidification direction of the alloy. EXAMPLES
[0057] In order to evaluate the effect of the lamination direction of the additively manufactured ceramic core on various physical properties of the core, evaluation samples were prepared by the following procedure and various tests were performed.
[0058] Silica (SiO 2 ) and zircon (ZrSiO 4 The ceramic powder used was N700, manufactured by Noritake Company Limited, which consists of .
[0059] Two types of molded bodies with different lamination directions of the layered structure were obtained by layer-forming the ceramic powder N700 using projet460plus (manufactured by 3D Systems). Specifically, the molded body was molded by spraying a binder from above on the raw material powder spread over the entire molding area to harden the cross section, and when one layer was hardened, the raw material powder of the next layer was supplied on top of it and the same process was repeated. Thereafter, the molded body was fired at 1250 ° C for 2 hours to obtain a test piece (Example 1). The test piece is before the coating (impregnation) described later is performed, and becomes the substrate that is the object of impregnation. The layered structure (lamination direction) of the test piece of Example 1 is shown in Figure 7. The test piece 8 in which the long axis direction Dc and the lamination direction Da are perpendicular to each other is called Type A (Figure 7 (a)), and the test piece 8 in which the long axis direction Dc and the lamination direction Da are the same is called Type B (Figure 7 (b)).
[0060] The two types of test pieces (types A and B) after the above-mentioned firing were used as substrates and impregnated with silica sol, which is a reinforcing agent, to seal the pores inside the substrate and coat the outermost periphery of the test pieces. In the process of impregnating the substrate with silica sol (silica slurry), the silica sol was hardened by vacuum impregnation, drying, and heat treatment at 450°C. This impregnation process was repeated to obtain test pieces after one impregnation (Example 2), two impregnations (Example 3), three impregnations (Example 4), four impregnations (Example 5), and five impregnations (Example 6). In the various evaluations described below, a test piece molded by injection molding (Comparative Example 1) was also evaluated in addition to the above-mentioned Examples 1 to 6.
[0061] The test pieces prepared by the above procedure were subjected to the following various evaluations.
[0062] The porosity was calculated from the amount of pores measured by the above-mentioned method based on Archimedes' method.
[0063] The three-point bending strength was measured with an EZ-test CE (Shimadzu Corporation) using samples (long side length approximately 40 mm) obtained by dividing a 3 × 4 × 120 mm test piece into three along the longitudinal axis, with a span of 30 mm.
[0064] For the high-temperature deformation, a load of 15 g was placed at the center of a 3 x 20 x 120 mm test piece, and the amount of deformation was measured at 1530°C for two hours.
[0065] The dissolution rate was calculated from the change in weight before and after immersion of the test piece in a 25% by mass NaOH aqueous solution at 250° C. for 30 minutes.
[0066] The Barcol strength was measured using a Barcol hardness tester GYZJ934-1.
[0067] The arithmetic mean surface roughness was measured in accordance with JIS B 0601 using a Surfcom manufactured by Tokyo Seimitsu Co., Ltd., using the method described above with a cutoff of 2.5 mm and a measurement length of 10 mm.
[0068] The evaluation results of the porosity and three-point bending strength of Examples 1 to 6 and Comparative Example 1 are shown in Table 1 below.
[0069] [Table 1]
[0070] The ceramic cores (Examples 1 to 6) manufactured by the additive manufacturing method showed different three-point bending strengths for Type A and Type B, and it was found that the strength differed depending on the lamination direction. In addition, the porosity was high at about 60% in Example 1 where no impregnation was performed, but by repeating the impregnation, the porosity was reduced to the same level as that of test pieces molded by existing injection molding, and the strength was also improved (Example 6).
[0071] The evaluation results of Examples 1 and 4 and Comparative Example 1 with respect to the dissolution rate, high-temperature deformation amount, Barcol hardness, and surface roughness (arithmetic mean roughness Ra) are shown in Table 2 below.
[0072] [Table 2]
[0073] Examples 1 and 4 showed solubility equal to or greater than that of Comparative Example 1. In addition, Type A of Example 4, which was impregnated three times, showed solubility and high-temperature deformability equivalent to those of Comparative Example 1. From this, it is considered that by controlling the direction of molten metal flow and the direction of thermal contraction of the metal, it is possible to suppress recrystallization of the metal during cooling without high-temperature deformation during casting. In Examples 1 and 4, both Types A and B have a lower Barcol hardness than Comparative Example 1. It is considered that the test pieces of the examples have a layered structure inside near the surface, which creates a fracture origin and causes micro-fracture when stress is applied during metal contraction, thereby suppressing metal recrystallization. Examples 1 and 4 showed a larger arithmetic mean roughness value than Comparative Example 1, but the surface roughness value became smaller as the number of impregnations increased, showing a tendency to become smoother.
[0074] 8 to 10 show electron microscope photographs of each test piece. FIG. 8 is an electron microscope photograph of the surface of the test piece of Example 1 before coating. FIG. 9 is an electron microscope photograph of the surface of the test piece of Example 4 after coating (three times impregnation), and FIG. 10 is an electron microscope photograph of the cross section of Example 4. From FIG. 8, it can be seen that the test piece manufactured using the additive manufacturing method has a layered structure. In FIG. 9, the surface is smoother than that in FIG. 8, and it can be seen that the layered structure of the outermost periphery has been smoothed by three times impregnation. In FIG. 10, no large voids are seen inside the cross section, and it is presumed that some of the pores have been sealed. [Industrial Applicability]
[0075] The ceramic core of the present invention is a core used in a directional solidification method, and has excellent disintegratability and solubility and can suppress the occurrence of recrystallization defects. Therefore, single crystal alloys or directionally solidified alloys can be produced with a higher yield by casting using the directional solidification method, and the core can be suitably used in the manufacture of heat-resistant structural components with complex structures. [Explanation of symbols]
[0076] 1. Mold 2 heating kiln 3 Cooling plate 4 Cast metal 5. Selectors 6 seed crystals 7 Ceramic Core 8 Test Pieces Da Stacking direction Db solidification direction Dc major axis direction
Claims
1. A ceramic core to be used in a directional solidification method in which molten metal is poured into a space formed by a mold and a core, and the molten metal is cooled and pulled out in one direction while being solidified to obtain a metal casting made of a single crystal alloy or a directionally solidified alloy, The ceramic core is a porous ceramic body having a layered structure with a lamination direction that does not coincide with the solidification direction of the alloy.
2. The ceramic core according to claim 1, characterized in that the ceramic core has the layered structure in a region corresponding to a cross section of the ceramic core and the alloy perpendicular to the solidification direction, where the area ratio of the ceramic core to the alloy changes when viewed from before to after the solidification direction.
3. The ceramic core according to claim 1 or 2, characterized in that the ceramic core is a core having a layered structure based on a molded body consisting of a mixture of any two or more types of inorganic particles selected from silica, alumina, zircon, magnesia, calcia, yttria, and zirconia, with some of the pores of the base material sealed and a coating layer on the outermost surface of the base material.
4. 4. The ceramic core of claim 3, wherein the coating layer comprises silica.
5. 5. The ceramic core according to claim 3, wherein the arithmetic mean roughness of the outermost surface is 10 μm or less.
6. 6. The ceramic core according to claim 1, wherein the ceramic core has a porosity of 20% to 40% as measured by Archimedes' method.
7. The ceramic core according to any one of claims 1 to 6, characterized in that the ceramic core has the layered structure at a location corresponding to a cross section in which the area ratio of the ceramic core to the alloy in a cross section before and after the solidification direction changes by 2% or more per mm before and after the solidification direction.
Citation Information
Patent Citations
Production of casting mold and ceramic core
JP1995214234A
Core for casting in die casting
JP1998314891A
Production of single crystal alloy blade
JP1999207451A
Method of manufacturing ceramic shaped article using powder shaping machine
JP2001247374A
Multilayer core and its manufacturing method
JP2004504945A