Activated carbon fiber material and its manufacturing method

By producing activated carbon fibers with a specific surface area of 2580 m²/g or more through controlled carbonization and activation processes, the fibers demonstrate superior adsorption and desorption capabilities for high-concentration fuel gases, addressing the limitations of existing carbon fibers in automobile canisters.

JP7557410B2Active Publication Date: 2024-09-27NIPPON PAPER IND CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021059517
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-31
Publication Date
2024-09-27
Estimated Expiration
2041-03-31

AI Technical Summary

Technical Problem

Activated carbon fibers have not been effectively utilized in automobile canisters due to challenges in achieving a specific surface area of 2500 m²/g or more, limiting their adsorption and desorption performance for high-concentration evaporated fuel gases.

Method used

The production of activated carbon fibers with a specific surface area of 2580 m²/g or more is achieved through a method involving a precursor fiber sheet treated with a phosphoric acid or organic sulfonic acid catalyst, followed by carbonization and activation treatments at specific temperatures, including a second carbonization step at 910°C or higher.

Benefits of technology

The resulting activated carbon fibers exhibit excellent adsorption and desorption performance for high-concentration evaporated fuel gases, meeting the demands of stringent emission regulations and idling stop systems in automobiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557410000003
    Figure 0007557410000003
  • Figure 0007557410000002
    Figure 0007557410000002
  • Figure 0007557410000001
    Figure 0007557410000001
Patent Text Reader

Abstract

To provide an activated carbon fiber material with a specific surface area of 2580 m2 / g and a manufacturing method thereof, and to provide an activated carbon fiber material with excellent adsorption-desorption performance against high-concentration evaporated fuel gas that can be generated from gasoline.SOLUTION: A manufacturing method according to the present invention including (A) and (B) below is used to obtain an activated carbon fiber material with a specific surface area of 2580 m2 / g. (A) A precursor fiber sheet holding one or both of a phosphate-based catalyst and an organosulfonate-based catalyst is subjected to a first carbonization treatment and a first activation treatment under conditions of a maximum temperature of less than 910°C to obtain a first activated carbon fiber material. (B) The first activated carbon fiber material is subjected to a second carbonization treatment under the condition of a maximum temperature of 910°C or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to activated carbon fiber materials and methods for making the same. [Background technology]

[0002] In gasoline-powered vehicles, the pressure inside the fuel tank fluctuates with changes in outside temperature, etc., causing the evaporated fuel gas that fills the fuel tank to be released from the fuel tank. The evaporated fuel gas that is released is considered to be one of the substances that cause PM2.5 and photochemical smog, and in order to prevent it from being released into the atmosphere, a canister equipped with an adsorbent such as activated carbon is provided. (Hereinafter, in this specification, a canister installed in an automobile may be abbreviated to "automobile canister" or simply "canister.")

[0003] With the growing awareness of environmental conservation in recent years, gas emission regulations have tended to be strengthened year by year, and therefore higher adsorption performance is required for canisters as well. In addition, with the spread of idling stops and the like, the intake capacity of automobiles tends to be restricted, so gasoline adsorbed in the adsorbent in the canister tends to be difficult to desorb. Therefore, there is a demand for even higher performance adsorbents used in canisters. Activated carbon is used as the adsorbent used in canisters, and as for its shape, those molded into granular, pellet, or honeycomb shapes have been proposed (for example, Patent Document 1, etc.). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-173137 A Summary of the Invention [Problem to be solved by the invention]

[0005] In contrast to the traditional powdered and granular activated carbon, activated carbon fiber (or fibrous activated carbon) is sometimes called the third type of activated carbon. Activated carbon fiber, among the activated carbons in the broad sense, is said to have fine pores directly open on the outer surface and to have a tendency to have a fast adsorption and desorption rate. However, activated carbon fiber has not yet been put to practical use in canisters, and research and development has not yet progressed sufficiently to determine what characteristics activated carbon fiber has that are suitable for practical use in canisters.

[0006] In the development of adsorbents, various physical properties and performance are considered. The specific surface area is one of the most basic indicators of adsorbents, and this is also the case with activated carbon fiber. Nevertheless, the specific surface area of ​​activated carbon fiber is at most 2500 m 2 / g, and 2580m 2 / g or more. 2 The physical properties and performance of activated carbon fibers with a specific surface area of ​​2580 m / g or more have not yet been confirmed in detail. 2 It was also unclear whether activated carbon fibers having a molecular weight of 1000 or more per unit area of ​​100 / g or more were suitable for canisters in which the properties against evaporated fuel gases generated by the evaporation of gasoline are important.

[0007] In light of the above, one of the issues we are trying to solve is the problem of the specific surface area of ​​2580 m 2 / g or more and a method for producing the same. Another problem to be solved is to provide an activated carbon fiber material that has excellent adsorption and desorption performance for high-concentration evaporated fuel gas that can be generated from gasoline. [Means for solving the problem]

[0008] The inventors have found that the specific surface area is 2580 m 2 As a result of intensive research into the manufacture of activated carbon fiber material with a carbonization rate of 2580m / g or higher, it was found that by performing an additional carbonization process at a specified temperature after the carbonization and activation processes, it is possible to manufacture activated carbon fiber material with a carbonization rate of 2580m / g or higher. 2We succeeded in obtaining activated carbon fiber material with a molecular weight of 2580m / g or more. 2 It has been found that activated carbon fiber materials with a carbon content of 0.1 to 1.0 carbon dioxide per 1000 carbon dioxide / g or more have excellent adsorption and desorption performance for high-concentration evaporated fuel gases that can be generated from gasoline.

[0009] The invention presented in this disclosure has been made based on such findings and can be understood from multiple perspectives as several aspects, and includes, for example, the following as means for solving the problems.

[0010] [1] Specific surface area is 2580-3200m 2 / g of activated carbon fiber material. [2] Total pore volume is 0.95 to 2.00 cm 3 / g. The activated carbon fiber material according to [1] above. [3] The activated carbon fiber material according to [1] or [2] above, which is an adsorbent for a canister. [4] A canister comprising the activated carbon fiber material according to [1] or [2] above. [5] Specific surface area is 2580 m 2 A method for producing an activated carbon fiber material having an activated carbon fiber content of 100% or more, comprising the steps of: (A) subjecting a precursor fiber sheet carrying either one or both of a phosphoric acid catalyst and an organic sulfonic acid catalyst to a first carbonization treatment and a first activation treatment under conditions of a maximum temperature of less than 910°C to obtain a first activated carbon fiber material; (B) subjecting the first activated carbon fiber material to a second carbonization treatment under a condition of a maximum temperature of 910° C. or more; A method comprising: [6] Specific surface area of ​​2580 m 2 A method for producing an activated carbon fiber material of at least 1 / g, Specific surface area is 2580m 2 Activated carbon fiber material with a specific surface area of ​​less than 2580 m2 is further carbonized at a maximum temperature of 910°C or higher. 2 / g or more of activated carbon fiber material. Effect of the Invention

[0011] According to one embodiment of the present invention, the specific surface area is 2580 m 2 / g or more and a method for producing the same. Moreover, according to one aspect of the present invention, it is possible to provide an activated carbon fiber material that has excellent adsorption and desorption performance for high-concentration evaporated fuel gas that can be generated from gasoline. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic diagram showing an example of a laminated adsorbent body formed by overlapping a plurality of sheet-shaped adsorbent bodies, and an example of the flow direction of a fluid passing through the laminated adsorbent body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention will be described. In this disclosure, unless otherwise specified, the expression "AA to BB" in relation to a numerical range means "AA or more and BB or less" (here, "AA" and "BB" indicate arbitrary numerical values). In addition, the units of the lower and upper limits are the same as the units immediately following the latter (i.e., "BB" here) unless otherwise specified. In addition, in this disclosure, the expression "X and / or Y" means both X and Y, or either one of them.

[0014] 1. Activated carbon fiber materials One embodiment of the activated carbon fiber material according to the present disclosure has a specific surface area of ​​2580 m 2 / g or more. Another embodiment of the activated carbon fiber material according to the present disclosure may be an activated carbon fiber material having a specific surface area of ​​2580 to 3200 m 2 / g of activated carbon fiber material.

[0015] <Specific surface area> The lower limit of the specific surface area of ​​the activated carbon fiber material is at least 2570 m 2 / g, preferably 2580m 2 / g or more, more preferably 2600m2 / g, more preferably 2650, 2680, or 2700 m 2 / g or more.

[0016] Activated carbon fibers having a high specific surface area can be suitable as an adsorbent for evaporated fuel gas from gasoline. The components of evaporated fuel gas from gasoline are also called volatile organic compounds (VOCs). In gasoline engines of automobiles, for example, the adsorption and desorption performance for n-butane may be used as an evaluation index. One embodiment of the activated carbon fiber material according to the present disclosure has a high specific surface area and is suitable as an adsorbent for high-concentration evaporated fuel gas, for example, high-concentration n-butane. Therefore, the activated carbon fiber material according to the present disclosure can be used as an adsorbent for a canister, as one embodiment.

[0017] The activated carbon fiber material having such a high specific surface area can be produced by the production method described below in detail. The upper limit of the specific surface area is not necessarily limited from the viewpoint of the adsorption and desorption performance for the evaporated fuel gas of high concentration, but is generally 3200, 3100, 3000, 2950, ​​2900, 2850, or 2800 m 2 / g or less.

[0018] The activated carbon fiber material of the present disclosure may be a more preferred embodiment by further satisfying any one or any two or more of the following specified items.

[0019] <Total pore volume> The lower limit of the total pore volume of the activated carbon fiber material according to the present disclosure is preferably 0.95 cm 3 / g or more, more preferably 1.00 cm / g or more, and even more preferably 1.05, 1.10, 1.20, or 1.30 cm 3 / g or more. The upper limit of the total pore volume of the activated carbon fiber material according to the present disclosure is preferably 2.00 cm 3 / g or less, 1.90, 1.80, 1.70, or 1.60 cm 3 / g or less. When the total pore volume is within the above range, the activated carbon fiber material can be suitable for use as an activated carbon fiber material having excellent adsorption / desorption performance for high-concentration evaporated fuel gas.

[0020] <Average pore size (average pore diameter)> In this disclosure, the term "pore size" refers to the diameter or width of the pore, and not the radius of the pore, unless otherwise specified. The lower limit of the average pore diameter of the activated carbon fiber material according to the present disclosure can be preferably 1.80 nm or more, more preferably 1.90 nm or more, and even more preferably 1.95 or 2.00 nm or more. The upper limit of the average pore size of the activated carbon fiber sheet according to the present disclosure can be preferably 4.00 nm or less, more preferably 3.50 nm or less, and even more preferably 3.00, 2.50, or 2.30 nm or less. When the average pore size is within the above range, the activated carbon fiber material can be suitable for use as an activated carbon fiber material having excellent adsorption / desorption performance for high-concentration evaporated fuel gas.

[0021] <Ultramicropore volume:V 0.7 > In the present invention, the term "ultramicropores" refers to pores having a pore diameter of 0.7 nm or less. The lower limit of the ultramicropore volume of the activated carbon fiber material according to the present disclosure is preferably 0.05 cm 3 / g or more, more preferably 0.07 cm 3 / g or more, more preferably 0.10 cm 3 / g or more. The upper limit of the ultramicropore volume of the activated carbon fiber material according to the present disclosure is preferably 0.20 cm 3 / g or less, more preferably 0.18 cm 3 / g or less, more preferably 0.15 cm 3 / g or less. When the ultramicropore volume is within the above range, the activated carbon fiber material is suitable for use as an activated carbon fiber material having excellent adsorption / desorption performance for high-concentration evaporated fuel gas.

[0022] <Micropore volume: V 2.0 > In this disclosure, the term "micropore" refers to pores with a pore diameter of 2.0 nm or less. The lower limit of the micropore volume of the activated carbon fiber material according to the present disclosure is preferably 0.50 cm 3 / g or more, more preferably 0.60, 0.65, or 0.70 cm 3 / g or more, more preferably 0.75 cm 3 / g or more. The upper limit of the micropore volume of the activated carbon fiber sheet of the present invention is preferably 1.40, 1.20, or 1.00 cm 3 / g or less, more preferably 0.90 cm 3 / g or less, more preferably 0.80 cm 3 / g or less. When the micropore volume is within the above range, the activated carbon fiber material is suitable for use as an activated carbon fiber material having excellent adsorption / desorption performance for high-concentration evaporated fuel gas.

[0023] <Pore volume of pores with diameters greater than 0.7 nm and less than 2.0 nm: V 0.7-2.0 > Pore ​​volume V of pores with diameters greater than 0.7 nm and less than 2.0 nm 0.7-2.0 can be calculated by the following formula 1 using the value a of the ultramicropore volume and the value b of the micropore volume.

[0024] <Expression 1> V 0.7-2.0 =ba

[0025] In the activated carbon fiber material according to the present disclosure, the pore volume V of pores having a pore diameter of more than 0.7 nm and not more than 2.0 nm is 0.7-2.0 The lower limit is preferably 0.20 cm 3 / g or more, more preferably 0.30, 0.40, 0.50, or 0.55 cm 3 / g or more, more preferably 0.58 or 0.60 cm 3 / g or more. In the activated carbon fiber sheet according to the present disclosure, the pore volume V of pores having a pore diameter of more than 0.7 nm and not more than 2.0 nm is 0.7-2.0 The upper limit is preferably 1.20 cm 3 / g or less, more preferably 1.00 cm 3 / g or less, more preferably 0.90, 0.80, 0.75, or 0.70 cm 3 / g or less. Pore ​​volume V 0.7-2.0 When the carbon fiber has a molecular weight of 100 or more and a molecular weight of 100 or more, the carbon fiber material has a molecular weight of 100 or more and a molecular weight of 100 or more.

[0026] <Ratio of ultramicropore volume to micropore volume: R 0.7 / 2.0 > The ratio R of the volume of ultramicropores with a pore diameter of 0.7 nm or less to the volume of micropores with a pore diameter of 2.0 nm or less 0.7 / 2.0 can be calculated by the following formula 2 using the ultramicropore volume value a and the micropore volume value b.

[0027] <Expression 2> R 0.7 / 2.0 = a / b × 100(%)

[0028] In the activated carbon fiber material according to the present disclosure, the abundance ratio R of the ultramicropore volume to the micropore volume 0.7 / 2.0 The lower limit value of may be preferably 5.0% or more, more preferably 10.0% or more, and further preferably 12.0 or 13.0% or more. In the activated carbon fiber material according to the present disclosure, the abundance ratio R of the ultramicropore volume to the micropore volume 0.7 / 2.0 The upper limit value of may be preferably 60.0, 50.0, or 40.0% or less, more preferably 30.0 or 25.0% or less, and even more preferably 20.0, 18.0, 17.0, 16.0, or 15.0% or less. Ultramicropore volume abundance ratio R 0.7 / 2.0When it is within the above range, it can be suitable as an activated carbon fiber material excellent in the adsorption and desorption performance for high-concentration evaporation fuel gas.

[0029] <Density> The lower limit value of the density of the activated carbon fiber material according to the present disclosure is preferably 0.010 g / cm 3 or more, more preferably 0.020 g / cm 3 or more, still more preferably 0.030, 0.040, 0.050, 0.060 g / cm 3 or more. The upper limit value of the density of the activated carbon fiber sheet according to the present disclosure is preferably 0.200 g / cm 3 or less, more preferably 0.150 g / cm 3 or less, still more preferably 0.120, 0.100, 0.090, 0.080, 0.070 g / cm 3 or less.

[0030] When the density is within the above range, within the range of the capacity of the adsorbent that can be stored in the canister, it can be used as an adsorbent excellent in the adsorption and desorption performance per volume required for the canister. Further, by setting it to be equal to or higher than the above lower limit value, it is possible to avoid a decrease in the mechanical properties (for example, strength, etc.) of the activated carbon fiber material. Also, the density of the activated carbon fiber material can suppress the pressure loss of the activated carbon fiber material by adjusting it in combination with other requirements such as the thickness of the activated carbon fiber material and the degree of compression when stored in the canister.

[0031] The thickness and density of the activated carbon fiber material can be adjusted by adjusting the type of the precursor fiber, the thickness and density of the raw material sheet, or by performing treatments such as pressing the activated carbon fiber sheet.

[0032] <n-butane adsorption and desorption performance> The activated carbon fiber material according to the present disclosure preferably has a predetermined n-butane adsorption / desorption performance as an adsorbent. The n-butane adsorption / desorption performance is an index of the adsorption / desorption performance of evaporated fuel gas, so that an adsorbent having excellent n-butane adsorption / desorption performance is suitable for automobile canister applications. The n-butane adsorption / desorption performance can be expressed as the effective adsorption amount of n-butane per weight of the activated carbon fiber material, which is determined by the amount of n-butane adsorbed from the adsorbent when placed under predetermined desorption conditions after sufficient absorption breakthrough.

[0033] In a preferred embodiment of the activated carbon fiber material according to the present disclosure, the "effective adsorption / desorption amount" of n-butane determined according to the measurement method shown in the following Examples can be preferably 1.50 g or more, more preferably 2.00 g or more, and even more preferably 2.30 g or more.

[0034] In a preferred embodiment of the activated carbon fiber material according to the present disclosure, the "effective adsorption / desorption rate" of n-butane determined according to the measurement method shown in the following Examples is preferably 30.0 wt% or more, more preferably 40.0 wt% or more, and even more preferably 45.0, 50.0, 55.0, or 60.0 wt% or more.

[0035] In a preferred embodiment of the activated carbon fiber material according to the present disclosure, the "effective adsorption / desorption rate" of n-butane determined according to the measurement method shown in the following Examples is preferably 70.0% or more, more preferably 77.0% or more, and even more preferably 80.0, 83.0, or 85.0%.

[0036] The activated carbon fiber material according to the present disclosure is not particularly limited in its external shape, but is generally produced by carbonizing and activating a sheet raw material such as a nonwoven fabric sheet, and may have a sheet shape. In the present disclosure, the sheet-shaped activated carbon fiber material is also referred to as an activated carbon fiber sheet.

[0037] In another embodiment of the present disclosure, an adsorptive laminate for storage in an adsorbent chamber of an automobile canister may be provided, the adsorptive laminate being a laminate in which a plurality of the above-described activated carbon fiber sheets are superimposed.

[0038] FIG. 1 shows one embodiment of the adsorption laminate of the present invention. The dimensions of the sheet, such as length and thickness, are shown diagrammatically and are not limited thereto. The number of sheets is shown as four as an example, but is not limited thereto.

[0039] The adsorption laminate 1 shown in Fig. 1 is a laminate formed by stacking four activated carbon fiber sheets 10. The activated carbon fiber sheets 10 are formed by stacking the main surfaces 10a of the sheets one on top of the other.

[0040] The adsorption laminate may be generally rectangular or cubic in shape. The adsorption laminate may be formed to match the shape of the adsorbent chamber in which the activated carbon fiber sheet is housed, or may be rolled into a cylindrical shape. In this way, the activated carbon fiber sheet of the present invention can be easily processed or molded into various shapes, and is a material with excellent handling properties.

[0041] 2. Canister The activated carbon fiber material according to the present disclosure is suitable as an adsorbent to be stored in an automobile canister. That is, the present disclosure also provides an automobile canister as another embodiment of the present invention.

[0042] The vehicle canister of the present disclosure is equipped with an activated carbon fiber material as an adsorbent. The structure of the vehicle canister is not particularly limited, and a general structure can be adopted. For example, the vehicle canister may have the following structure.

[0043] <First embodiment of the canister> A housing and an adsorbent chamber that accommodates an adsorbent within the housing; a first opening for providing gas flow communication between the adsorbent chamber and the engine; a second opening for providing gas movable communication between the adsorbent chamber and the fuel tank; a third opening that opens when a predetermined pressure is applied from the adsorbent chamber or from the outside air, and communicates between the adsorbent chamber and the outside air so that gas can move between the adsorbent chamber and the outside air; A canister comprising:

[0044] The first, second, and third openings are each an inlet / outlet through which gas enters and exits. The arrangement of the openings, which are gas inlet / outlet, is not particularly limited, but the third opening, which is an outside air inlet / outlet, is preferably arranged at a position where the gas passes through the adsorbent sufficiently when the gas moves between the first and / or second openings. For example, an embodiment may be adopted in which the first and second openings are provided in a first side portion of the housing, and the third opening is provided in a second side portion opposite the first side portion.

[0045] The adsorbent chamber may be divided into a plurality of chambers. For example, the adsorbent chamber may be divided into two or more compartments by a partition wall. A perforated plate having gas permeability may be used as the partition wall. Also, an external second housing may be provided separately from the first housing, and the first housing and the second housing may be communicated with each other via a gas passage to provide an additional adsorbent chamber. When a plurality of compartments or housings are provided in this way, as a preferred embodiment, the adsorbent or adsorbent chamber may be arranged in each compartment or housing so that the adsorption capacity decreases from the first or second opening through which gas flows in from the engine or fuel tank toward the third opening.

[0046] Another embodiment of the canister according to the present disclosure may include, for example, a configuration having a plurality of adsorbent chambers as follows. <Second embodiment of the canister> A canister for an automobile having a main chamber and a sub-chamber for storing an adsorbent, the main chamber has a larger capacity for accommodating the adsorbent than the sub-chamber, and is disposed at a position closer to an opening communicating with a fuel tank or an opening communicating with an internal combustion engine, the sub-chamber has a smaller capacity for accommodating the adsorbent than the main chamber, and is disposed at a position closer to an opening communicating with outside air, The main chamber has a specific surface area of ​​2580 to 3200 m 2 A canister containing activated carbon fiber having a molecular weight of 1 / g.

[0047] <Modification of the second embodiment of the canister> In the second embodiment, the sub-chamber has a specific surface area of ​​2580 m 2 A canister containing less than 1 / g of activated carbon fiber material.

[0048] The activated carbon fiber material according to the present disclosure has high adsorption and desorption performance for high-concentration n-butane. Therefore, it may be an advantageous embodiment to store the activated carbon fiber material according to the present disclosure in a portion of the canister that is likely to come into contact with high-concentration evaporated fuel gas. In the above-mentioned second embodiment, the activated carbon fiber material according to the present disclosure is stored in the main chamber. In contrast, it may be preferable to store an adsorbent having excellent adsorption and desorption performance for low-concentration n-butane in the sub-chamber.

[0049] 3. Manufacturing method of activated carbon fiber material The activated carbon fiber material according to the present disclosure can be produced by carbonizing and activating a fiber material. In the present disclosure, the fiber before carbonization and activation is referred to as a "precursor fiber", and a sheet formed of the precursor fiber is referred to as a "precursor fiber sheet". In the present disclosure, the term "fiber diameter" does not mean the radius of the fiber, but the diameter or width of the fiber, unless otherwise specified. In addition, the "fiber diameter" of activated carbon fiber is used for the fiber of the activated carbon material after carbonization and activation.

[0050] A preferred embodiment of the method for producing an activated carbon fiber material according to the present disclosure includes, for example, a method including the following (A) and (B). (A) A precursor fiber sheet carrying either one or both of a phosphoric acid-based catalyst and an organic sulfonic acid-based catalyst is subjected to a first carbonization treatment and a first activation treatment under conditions of a maximum temperature of less than 910°C to obtain a first activated carbon fiber material. (B) subjecting the first activated carbon fiber material to a second carbonization treatment under conditions of a maximum temperature of 910°C or higher.

[0051] With only the above (A) processing, the 2 It has been difficult to obtain activated carbon fibers with a high specific surface area of ​​1000m3 / g or more. However, by adding the above treatment (B), activated carbon fibers with a high specific surface area can be easily obtained. Although the addition of the above treatment (B) increases the number of manufacturing processes, the operation is a type of carbonization treatment, so it can be carried out using existing equipment without preparing new manufacturing equipment.

[0052] As an example of an embodiment of a method for producing an activated carbon fiber material according to the present disclosure, a method for producing an activated carbon fiber sheet is described below.

[0053] 3-1. Preparation of raw material sheet (precursor fiber sheet) <Type of fiber> Examples of fibers constituting the raw material sheet include cellulose-based fibers, pitch-based fibers, PAN-based fibers, and phenolic resin-based fibers, and preferably cellulose-based fibers.

[0054] <Cellulosic fibers> Cellulosic fibers are fibers composed mainly of cellulose and / or its derivatives. The cellulose and cellulose derivatives may be of any origin, such as chemically synthesized products, plant-derived cellulose, regenerated cellulose, and cellulose produced by bacteria. As the cellulose fibers, preferred examples include fibers made of plant-derived cellulose materials obtained from trees and fibers made of long fibrous regenerated cellulose materials obtained by dissolving plant-derived cellulose materials (cotton, pulp, etc.) through chemical treatment. These fibers may also contain components such as lignin and hemicellulose.

[0055] Examples of raw materials for cellulosic fibers (plant-based cellulose materials, regenerated cellulose materials) include plant cellulose fibers such as cotton (short-staple cotton, medium-staple cotton, long-staple cotton, extra-long staple cotton, etc.), hemp, bamboo, paper mulberry, trefoil, banana, and tunicates; regenerated cellulose fibers such as cuprammonium rayon, viscose rayon, polynosic rayon, and cellulose made from bamboo; refined cellulose fibers spun with an organic solvent (N-methylmorpholine N-oxide); and acetate fibers such as diacetate and triacetate. Among these, at least one selected from cuprammonium rayon, viscose rayon, and refined cellulose fibers is preferred because of their availability.

[0056] The form of the cellulose-based fiber is not particularly limited, and can be prepared according to the purpose, such as raw yarn (unprocessed yarn), false twisted yarn, dyed yarn, single yarn, doubled and twisted yarn, and covered yarn. When the cellulose-based fiber contains two or more kinds of raw materials, it may be a blended yarn, a blended twisted yarn, and the like. Furthermore, the raw materials in the above-mentioned various forms may be used alone or in combination of two or more kinds as the cellulose-based fiber. Among these, non-twisted yarn is preferable in terms of achieving both moldability and mechanical strength of the composite material.

[0057] <Fiber sheet> A fiber sheet is a material made by processing a large number of fibers into a thin, wide sheet, and includes woven fabrics, knitted fabrics, nonwoven fabrics, and the like.

[0058] There is no particular restriction on the method for weaving the cellulosic fibers, and any common method can be used. There is also no particular restriction on the weaving structure of the fabric, and any of the three basic weaves, plain weave, twill weave, and satin weave, can be used.

[0059] In the woven fabric formed of cellulosic fibers, the gap between the warp and weft yarns of the cellulosic fibers is preferably 0.1 to 0.8 mm, more preferably 0.2 to 0.6 mm, and even more preferably 0.25 to 0.5 mm. Furthermore, the basis weight of the woven fabric made of cellulosic fibers is preferably 50 to 500 g / m 2 , more preferably 100 to 400 g / m 2 It is possible.

[0060] By setting the cellulosic fibers and the woven fabric made of cellulosic fibers within the above range, the carbon fiber fabric obtained by heat treating the woven fabric can have excellent strength.

[0061] The method for producing the nonwoven fabric is not particularly limited, and examples thereof include a method of obtaining a fiber sheet using the above-mentioned fibers cut to an appropriate length as a raw material by a dry method or a wet method, a method of obtaining a fiber sheet directly from a solution by an electrospinning method, etc. Furthermore, after obtaining the nonwoven fabric, a treatment such as resin bonding, thermal bonding, spunlace, needle punching, etc. may be added in order to bond the fibers together.

[0062] 3-2.Catalyst The catalyst is supported on the raw material sheet prepared as described above. The catalyst is supported on the raw material sheet and carbonized, and then activated with water vapor, carbon dioxide, air gas, or the like to obtain a porous activated carbon fiber sheet. Examples of the catalyst that can be used include phosphoric acid catalysts and organic sulfonic acid catalysts.

[0063] <Phosphoric acid catalyst> Examples of phosphoric acid catalysts include phosphoric acid, metaphosphoric acid, pyrophosphoric acid, phosphorous acid, phosphonic acid, phosphonous acid, phosphinic acid, and other phosphorus oxyacids, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, dimethylphosphonopropanamide, ammonium polyphosphate, polyphosphonitrile chloride, and condensates of phosphoric acid, tetrakis(hydroxymethyl)phosphonium salt, or tris(1-aziridinyl)phosphine oxide with urea, thiourea, melamine, guanine, cyanamide, hydrazine, dicyandiamide, or methylol derivatives thereof, and preferably diammonium hydrogen phosphate. One phosphoric acid catalyst may be used alone, or two or more may be used in combination. When the phosphoric acid catalyst is used as an aqueous solution, its concentration may be preferably 0.05 to 2.0 mol / L, more preferably 0.1 to 1.0 mol / L.

[0064] <Organic sulfonic acid catalyst> As the organic sulfonic acid, an organic compound having one or more sulfo groups can be used, and for example, compounds having sulfo groups bonded to various carbon skeletons such as aliphatic and aromatic compounds can be used. From the viewpoint of handling, organic sulfonic acid catalysts having low molecular weights are preferred.

[0065] Examples of the organic sulfonic acid catalyst include a compound represented by R-SO3H (wherein R represents a linear / branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms, and the alkyl group, cycloalkyl group, and aryl group may each be substituted with an alkyl group, a hydroxyl group, or a halogen group). Examples of the organic sulfonic acid catalyst include methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, 1-hexanesulfonic acid, vinylsulfonic acid, cyclohexanesulfonic acid, p-toluenesulfonic acid, p-phenolsulfonic acid, naphthalenesulfonic acid, benzenesulfonic acid, and camphorsulfonic acid. Of these, methanesulfonic acid can be preferably used. In addition, the organic sulfonic acid catalyst may be used alone or in combination of two or more kinds.

[0066] When the organic sulfonic acid is used as an aqueous solution, the concentration thereof may be preferably 0.05 to 2.0 mol / L, more preferably 0.1 to 1.0 mol / L.

[0067] <Mixed catalyst> The phosphoric acid catalyst and the organic sulfonic acid catalyst may be mixed and used as a mixed catalyst. The mixing ratio may be appropriately adjusted.

[0068] <Catalyst retention> The catalyst is retained on the raw material sheet. Here, "retained" means that the catalyst is kept in contact with the raw material sheet, and can be in various forms such as adhesion, adsorption, impregnation, etc. There are no particular limitations on the method for retaining the catalyst, and examples of the method include a method of immersing the raw material sheet in an aqueous solution containing the catalyst, a method of sprinkling the aqueous solution containing the catalyst on the raw material sheet, a method of contacting the raw material sheet with vaporized catalyst vapor, and a method of mixing the fibers of the raw material sheet with an aqueous solution containing the catalyst and making paper.

[0069] From the viewpoint of sufficient carbonization, it is preferable to use a method in which the raw material sheet is immersed in an aqueous solution containing a catalyst, and the catalyst is impregnated into the inside of the fibers. The temperature when immersing in the aqueous solution containing a catalyst is not particularly limited, but room temperature is preferable. The immersion time is preferably 10 seconds to 120 minutes, more preferably 20 seconds to 30 minutes. By immersion, for example, 1 to 150 mass %, preferably 5 to 60 mass % of the catalyst is adsorbed on the fibers constituting the raw material sheet. After immersion, it is preferable to take out the raw material sheet and dry it. As a drying method, for example, any method such as leaving it at room temperature or introducing it into a dryer may be used. After taking it out from the aqueous solution containing the catalyst, the drying may be performed until the excess moisture evaporates and there is no change in the sample weight. For example, in the case of drying at room temperature, the drying time may be 0.5 days or more. After there is almost no change in mass due to drying, the raw material sheet retaining the catalyst is carbonized.

[0070] 3-3. First carbonization process After preparing the raw material sheet carrying the catalyst, the sheet is carbonized. The carbonization treatment to obtain the activated carbon fiber sheet can be carried out according to a general method for carbonizing activated carbon, but in a preferred embodiment, the carbonization treatment can be carried out as follows.

[0071] The carbonization treatment is usually carried out in an inert gas atmosphere. In the present invention, the inert gas atmosphere means an oxygen-free or low-oxygen atmosphere in which carbon is unlikely to undergo a combustion reaction and is carbonized, and is preferably, for example, an argon, nitrogen, or other gas atmosphere.

[0072] The raw material sheet carrying the catalyst is heated in the above-mentioned predetermined gas atmosphere to be carbonized. In one embodiment, the heat treatment is performed by increasing the temperature from room temperature and maintaining the maximum temperature for a predetermined period of time.

[0073] The lower limit of the maximum temperature may be preferably 300° C. or higher, more preferably 350, 400, or 500° C. or higher, and even more preferably 600, 700, 750, or 800° C. or higher. The maximum temperature limit is below 910°C, or may be as high as 900°C. By setting the maximum temperature in the heat treatment as described above, a carbon fiber sheet in which the fiber morphology is maintained can be obtained. If the heating temperature is below the lower limit, the carbon content of the carbon fiber is 80% or less, and carbonization tends to be insufficient.

[0074] The lower limit of the heat treatment time, including the time for increasing the temperature, can be preferably 10 minutes or more, more preferably 11 minutes or more, even more preferably 12 minutes or more, and more preferably 30 minutes or more. The upper limit of the heat treatment time can be any value, but is preferably 180 minutes or less, more preferably 160 minutes or less, and even more preferably 140 minutes or less. By thoroughly impregnating the raw material sheet with the catalyst, setting the heating temperature at the above-mentioned preferred temperature, and adjusting the heat treatment time, it is possible to adjust the degree of progress of pore formation and adjust the physical properties of the porous body, such as the specific surface area, the volume of various pores, the average pore diameter, etc. If the heat treatment time is shorter than the above-mentioned lower limit, carbonization is likely to be insufficient.

[0075] 3-4. First activation treatment The activation treatment in the present disclosure can be carried out, for example, by continuously supplying water vapor after the above-mentioned heat treatment and maintaining the material at an appropriate activation temperature for a predetermined period of time, thereby obtaining an activated carbon fiber sheet.

[0076] The lower limit of the activation temperature is preferably 300° C. or higher, more preferably 350, 400, or 500° C. or higher, and even more preferably 600, 700, 750, or 800° C. or higher. On the other hand, the upper limit of the activation temperature is less than 910°C, or may be 900°C. When the activation treatment is carried out consecutively after the heat treatment, it is desirable to adjust the maximum temperature during the activation treatment to be approximately the same as the maximum temperature during the heat treatment.

[0077] The lower limit of the activation time is preferably 1 minute or more, more preferably 5 minutes or more. The upper limit of the activation time can be any value, but is preferably 180 minutes or less, more preferably 160 minutes or less, and even more preferably 140 minutes or less, 100 minutes or less, 50 minutes or less, or 30 minutes or less.

[0078] 3-5. Second carbonization process (or additional carbonization process) As described above, the first carbonization treatment and the first activation treatment increased the specific surface area to 2580 m 3 / g of activated carbon fiber can be obtained. In one embodiment of the method for producing an activated carbon fiber material according to the present disclosure, a second carbonization treatment is further performed. The second carbonization treatment may be performed continuously after the completion of the first activation treatment, or may be performed discontinuously, for example, after the activated carbon fiber material obtained by the first carbonization treatment and the first activation treatment is cooled.

[0079] The second carbonization treatment is carried out under temperature conditions where the maximum temperature is at least higher than that of the first carbonization treatment, and is preferably carried out under conditions where the maximum temperature is approximately 1000° C. More specifically, the range of the maximum temperature in the second carbonization treatment may have a lower limit of preferably 910, 920, 930, 940, or 950° C. or higher, more preferably 980° C. or higher, and even more preferably 1000° C. or higher. The upper limit of the maximum temperature may preferably be about 1200 or 1100° C. or lower. By setting the maximum temperature in the second carbonization treatment as described above, the specific surface area of ​​the activated carbon fiber can be increased.

[0080] The lower limit of the heat treatment time, including the time for increasing the temperature, can be preferably 10 minutes or more, more preferably 11 minutes or more, even more preferably 12 minutes or more, and more preferably 30 minutes or more. The upper limit of the heat treatment time can be any value, but is preferably 180 minutes or less, more preferably 160 minutes or less, and even more preferably 140, 120, 100, 80, or 60 minutes or less. Setting the heat treatment time in the second carbonization treatment in this manner is suitable for increasing the specific surface area of ​​the activated carbon fiber.

[0081] 3-6. Modification of existing activated carbon fiber materials (manufacturing method of modified activated carbon fiber) The present disclosure further provides a method for modifying pre-made activated carbon fiber materials having a low specific surface area to a high specific surface area.

[0082] In the manufacturing method of the activated carbon fiber modified with a high specific surface area, first, an activated carbon fiber material having a specific surface area of ​​2580 m 3 Such an activated carbon fiber material is not limited to the case where it is used continuously for the activated carbon fiber material obtained by the first carbonization treatment and the first activation treatment as described above, but may be prepared by separately purchasing activated carbon fibers that exist as ready-made products.

[0083] The specific surface area is 2580m 2 The activated carbon fiber material having a specific surface area of ​​less than 2580 m2 is subjected to an additional carbonization treatment in the same manner as in the second carbonization treatment described above. 3 / g or more. The suitable conditions are the same as those described for the second carbonization treatment. Here, the term "additional carbonization treatment" includes the meaning of an additional carbonization treatment since the activated carbon fiber material to be modified is also an activated carbon fiber and has already been subjected to a carbonization treatment and an activation treatment. EXAMPLES

[0084] The present invention will be described in detail below with reference to examples. However, the technical scope of the present invention is not limited to the following examples.

[0085] Various items relating to the physical properties and performance of the activated carbon fiber were measured and evaluated by the methods shown below. Various values ​​defining the present invention can be determined by the following measurement and evaluation methods.

[0086] <Specific surface area> Approximately 30 mg of activated carbon fiber sample was collected, vacuum dried at 200°C for 20 hours, weighed, and measured using a high-precision gas / vapor adsorption measuring device BELSORP-maxII (Microtrack-Bell). The adsorption amount of nitrogen gas at the boiling point of liquid nitrogen (77K) was measured at a relative pressure of 10 -8The adsorption isotherm was calculated by the BET method, in which the analysis relative pressure range was automatically determined under the conditions of adsorption isotherm type I (ISO9277), and the BET specific surface area per unit weight (unit: m 2 / g, and this is then used to calculate the specific surface area (unit: m 2 / g).

[0087] <Total pore volume> The total pore volume (unit: cm) obtained by the one-point method was calculated from the result of the isothermal adsorption curve obtained in the above specific surface area section at a relative pressure of 0.960. 3 / g) was calculated.

[0088] <Average pore size (average pore diameter) unit: nm> The average pore diameter was calculated according to the following formula 3.

[0089] <Expression 3> Average pore diameter = 4 x total pore volume x 10 3 ÷specific surface area

[0090] <Ultra-micropore volume> The isothermal adsorption curve obtained in the above specific surface area section was analyzed by the GCMC method using the analysis software BELMaster attached to the high-precision gas / vapor adsorption amount measuring device BELSORP-maxII (Microtrack Bell) with the analysis settings of "Smoothing (moving average processing using one point before and after each point of the pore distribution analysis)", "Distribution function: No-assumption", "Pore size definition: Solid and Fluid Def. Pore Size", and "Kernel: Slit-C-Adsorption". From the pore distribution curve obtained during adsorption, the cumulative pore volume of 0.7 nm was read and the ultramicropore volume (unit: cm 3 / g).

[0091] <Micropore volume> The isothermal adsorption curve obtained in the above specific surface area section was analyzed using the analysis software BELMaster attached to the high-precision gas / vapor adsorption measurement device BELSORP-maxII (MicrotracBEL). The analysis settings were "smoothing (moving average processing using one point before and after all points of the pore size distribution analysis)", "distribution function: No-assumption", "definition of pore diameter: Solid and Fluid Def. Pore Size", and "Kernel: Slit-C-Adsorption". From the results of the obtained pore size distribution curve during adsorption, the cumulative pore volume at 2.0 nm was read and taken as the micropore volume (unit: cm 3 / g).

[0092] <n-butane adsorption and desorption performance> With reference to the American Society for Testing and Materials standard Standard Test Method for Determination of Butane Working Capacity of Activated Carbon (ASTM D5228-16), the test container, the flow rate of n-butane, and the flow rate of the air for desorption were set independently and tested.

[0093] The mass of an empty test container (stainless steel container with a cross-section of 5.6 cm × 5.6 cm, a cross-sectional area of 31.4 cm 2 , a length of 2 cm, and a sample filling volume of 62.7 cm 3 ) was measured, and then the adsorbent was filled into the test container to 62.7 cm 3 . For example, the activated carbon fiber sheet was cut to a sheet width of 5.6 cm × a length of 2 cm and filled by laminating. The test container filled with the adsorbent was dried in a dryer at 115 ± 5 °C for 8 hours or more, and the dry weight was measured after cooling in a desiccator filled with silica gel

[0094] Next, the test tube was installed in the flow device, and at a test temperature of 25 °C, 0.5 L / min of 100% concentration n-butane gas was flowed into the test container to adsorb n-butane. The test container was removed from the flow device and its mass was measured. The flow of this 100% concentration n-butane gas was repeated until a constant mass was achieved, that is, until the adsorption amount was saturated. The test container was reinstalled in the flow device, and air was flowed through the test container at 2.0 L / min for 22.5 minutes at a test temperature of 25° C. (total volume of the test container was 719 times the volume of the test container) to desorb n-butane. The test container was removed from the flow device, and its mass was measured.

[0095] This adsorption and desorption procedure was repeated twice in total, and the first adsorption amount, effective adsorption / desorption amount, effective adsorption / desorption amount rate, and effective adsorption / desorption rate were calculated using the following equations 4, 5, 6, and 7.

[0096] <Expression 4> 1st adsorption amount = 1st n-butane adsorption amount The units of each value are as follows: First n-butane adsorption amount (unit: g)

[0097] <Formula 5> Effective adsorption / desorption amount = (2nd n-butane adsorption amount + 2nd n-butane desorption amount) ÷ 2 The units of each value are as follows: Effective adsorption / desorption amount (unit: g) Second n-butane adsorption amount (unit: g) Amount of n-butane desorbed in the second run (unit: g)

[0098] <Formula 6> Effective adsorption / desorption rate = Effective adsorption / desorption amount ÷ Dry weight of molded adsorbent × 100 The units of each value are as follows: Effective adsorption / desorption rate (unit: wt%) Effective adsorption / desorption amount (unit: g) Dry weight of molded adsorbent (unit: g)

[0099] <Formula 7> Effective adsorption / desorption rate = Effective adsorption / desorption amount ÷ 1st adsorption amount × 100 The units of each value are as follows: Effective adsorption / desorption rate (unit: %) Effective adsorption / desorption amount (unit: g) First adsorption amount (unit: g)

[0100] <Volume of adsorbent> The volume of the adsorbent was the same as the volume of the test vessel.

[0101] <Density of adsorbent: Unit: g / cm 3 > The adsorption density was calculated by the following formula 8.

[0102] <Formula 8> Density = dry weight of adsorbent ÷ volume of adsorbent

[0103] <Example 1> (1) Rayon fiber (17.0 dtex, fiber length 76 mm) with a basis weight of 400 g / m 2 The needle-punched nonwoven fabric was impregnated with a 6-10% aqueous solution of diammonium hydrogen phosphate, squeezed out, and then dried to allow 8-10% by weight of the pretreated nonwoven fabric to adhere. The temperature of the pretreated nonwoven fabric was raised to 900°C in 38 minutes in a nitrogen atmosphere, and the fabric was subsequently activated at that temperature for 18 minutes in a nitrogen stream containing water vapor with a dew point of 60°C.

[0104] (2) The activated carbon fiber obtained in (1) above was heated to 1000°C over 100 minutes and held at this temperature for 50 minutes.

[0105] <Comparative Example 1> Rayon fiber (17.0 dtex, fiber length 76 mm) with a basis weight of 400 g / m 2 The needle-punched nonwoven fabric was impregnated with a 6-10% aqueous solution of diammonium hydrogen phosphate, squeezed out, and dried to adhere 8-10% by weight. The obtained pretreated nonwoven fabric was heated to 900°C in a nitrogen atmosphere over 45 minutes and held at this temperature for 4 minutes. Subsequently, activation treatment was performed at that temperature for 18 minutes in a nitrogen stream containing water vapor with a dew point of 71°C.

[0106] <Comparative Example 2> Rayon fiber (17.0 dtex, fiber length 76 mm) with a basis weight of 400 g / m 2The needle-punched nonwoven fabric was impregnated with a 6-10% aqueous solution of diammonium hydrogen phosphate, squeezed out, and dried to adhere 8-10% by weight. The pretreated nonwoven fabric was heated to 900°C in a nitrogen atmosphere over 31 minutes and held at this temperature for 3 minutes. The fabric was then activated at that temperature for 9 minutes in a nitrogen stream containing water vapor with a dew point of 71°C.

[0107] The analytical results of the above-mentioned Examples and Comparative Examples are shown in Table 1. Furthermore, an outline of the manufacturing methods of the above-mentioned Examples and Comparative Examples is shown in Table 2.

[0108] [Table 1]

[0109] [Table 2]

Claims

1. Specific surface area is 2580 to 3200 m 2 / g, The total pore volume is 0.95 to 2.00 cm 3 / g; The average pore diameter is 1.90 to 4.00 nm, the abundance ratio R 0.7 / 2.0 of the ultramicropore volume to the micropore volume is 5.0 to 20.0%, The effective adsorption / desorption rate for 100% n-butane is 40.0 wt% or more. Activated carbon fiber material.

2. The activated carbon fiber material according to claim 1, having an ultramicropore volume of 0.07 to 0.15 cm 3 / g.

3. The activated carbon fiber material according to claim 1 or 2, which is an adsorbent for a canister.

4. A canister comprising the activated carbon fiber material according to claim 1 or 2.

Citation Information

Patent Citations

  • Activation furnace and activating method

    JP1987158108A

  • Method for producing carbon fiber and activated carbon fiber of lignin

    JP2013147768A

  • Adsorbent, process for producing the same, canister and method for using the same

    JP2013173137A

  • Method of producing graphite material, and graphite material

    JP2015048256A

  • Active carbon fiber for removing free chlorine, and treatment method of free chlorine-containing water using the same

    JP2017164741A