Spherical crystalline silica powder and its manufacturing method

By crystallizing and acid-treating spherical amorphous silica powder, the powder achieves high thermal expansion and low dielectric loss, addressing the limitations of existing silica powders for high-frequency electronic devices.

JP7557633B2Active Publication Date: 2024-09-27DENKA CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023542450
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-08-20
Filing Date
2022-08-19
Publication Date
2024-09-27
Estimated Expiration
2042-08-19

AI Technical Summary

Technical Problem

Existing spherical silica powders, particularly those manufactured by flame melting, have low thermal expansion coefficients and high dielectric loss tangents, making them unsuitable for high-frequency electronic devices where low transmission loss and thermal stability are required.

Method used

Crystallizing spherical amorphous silica powder by heating, treating it with acid, and further heat-treating it to achieve a high coefficient of linear thermal expansion and a low dielectric loss tangent, with specific control over water molecule desorption and crystal composition.

Benefits of technology

The resulting spherical crystalline silica powder provides resin molded articles with high thermal expansion and low dielectric loss, enhancing stability and signal transmission in electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557633000004
    Figure 0007557633000004
  • Figure 0007557633000003
    Figure 0007557633000003
  • Figure 0007557633000002
    Figure 0007557633000002
Patent Text Reader

Abstract

Provided are: spherical crystalline silica powder that is capable of providing a resin molded product which has a high linear thermal expansion coefficient and a low dielectric loss tangent; and a method for producing the same. In the spherical crystalline silica powder, the number of water molecules that are eliminated at 50-1,000°C when the temperature is raised up to 1,000°C under the condition of 25-30°C / min is 10 μmol / g or less, and 10 mass% or more of the entirety of the powder is α-quartz crystal. The method for producing spherical crystalline silica powder comprises: (i) heating spherical amorphous silica powder to obtain spherical crystalline silica powder, (ii) bringing the spherical crystalline silica powder into contact with acid, and (iii) heating, at 800-1,400°C, the spherical crystalline silica powder that has been processed in (ii).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a spherical crystalline silica powder and a method for producing the same. [Background technology]

[0002] Silica powder is widely used as a filler for resins. In particular, spherical silica powder can be highly dispersed in resins and is therefore preferably used as a filler for semiconductor element encapsulants. The filler for semiconductor element encapsulants preferably has a high thermal expansion coefficient so that the encapsulant does not warp or crack due to temperature changes during reflow or temperature changes during temperature cycle testing. However, spherical silica powder produced by the flame fusion method, which is one of the methods for producing spherical silica powder, tends to have a low thermal expansion coefficient because it is amorphous. Therefore, attempts have been made to improve the thermal expansion coefficient and thermal conductivity by heating spherical amorphous silica powder at high temperatures to crystallize it (for example, Patent Document 1). It is known that crystalline silica powder has different crystal structures depending on pressure and temperature. Examples of the crystal structure of crystalline silica powder include α-quartz, cristobalite, tridymite, etc. Patent Document 2 describes a silica powder having two or more crystal forms selected from α-quartz, tridymite, and cristobalite.

[0003] Incidentally, with the increase in the amount of information communication in the field of communication, the use of high frequency bands in electronic devices and communication devices is spreading. With the application of high frequency bands, materials with low dielectric tangent are required to prevent transmission loss of circuit signals. Patent Document 3 proposes that spherical amorphous silica powder obtained by the powder fusion method is heat-treated at a specified temperature for a specified time to produce spherical amorphous silica with a reduced dielectric tangent.

[0004] [Patent Document 1] International Publication No. 2016 / 031823 [Patent Document 2] JP 2005-231973 A [Patent Document 3] Patent Publication No. 2021-38138 Summary of the Invention

[0005] An object of the present invention is to provide a spherical crystalline silica powder capable of giving a resin molded article having a high linear thermal expansion coefficient and a low dielectric loss tangent, and a method for producing the same.

[0006] The present inventors discovered that by crystallizing spherical amorphous silica powder and then contacting it with an acid and further heat-treating it, a spherical crystalline silica powder having a high linear thermal expansion coefficient and a reduced dielectric tangent can be obtained, and that the number of water molecules released from the obtained spherical crystalline silica powder at 50°C to 1000°C is 10 μmol / g or less, which led to the completion of the present invention.

[0007] The present invention has the following aspects. [1] When the temperature is increased from 25°C to 1000°C at a rate of 30°C / min, the number of water molecules desorbed between 50°C and 1000°C is 10μmol / g or less; A spherical crystalline silica powder in which 10% by mass or more of the entire powder is α-quartz crystals. [2] The spherical crystalline silica powder according to [1], wherein the crystallinity of the entire powder as measured by X-ray diffraction is 30 to 98%. [3] The spherical crystalline silica powder according to [1] or [2], wherein 20 to 90 mass % of the entire powder is α-quartz crystals. [4] The spherical crystalline silica powder according to any one of [1] to [3], wherein 0 to 70 mass % of the entire powder is cristobalite crystals. [5] A spherical crystalline silica powder according to any one of [1] to [4], having an alkaline earth metal element content of less than 10,000 μg / g calculated as oxide. [6] A resin composition comprising the spherical crystalline silica powder according to any one of [1] to [5] and a resin. [7] (i) heating a spherical amorphous silica powder to obtain a spherical crystalline silica powder; (ii) contacting the spherical crystalline silica powder with an acid; and (iii) A method for producing a spherical crystalline silica powder, comprising heating the spherical crystalline silica powder treated by (ii) at 800 to 1400°C. [8] The method according to [7], wherein in (i) a mixture of spherical amorphous silica powder and a solvent is heated to obtain spherical crystalline silica powder.

[0008] According to the present invention, there are provided a spherical crystalline silica powder capable of giving a resin molded article having a high linear thermal expansion coefficient and a low dielectric tangent, and a method for producing the same. [Brief description of the drawings]

[0009] [Figure 1] 1 is a graph showing the thermal expansion behavior measured by thermomechanical analysis (TMA) of test pieces containing the silica powder of Examples 1-5, Comparative Example 1-1 (amorphous silica powder), Comparative Example 1-3 (spherical cristobalite crystals), or Reference Example (crushed quartz). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] An embodiment of the present invention will be described in detail below. The present invention is not limited to the following embodiment, and can be practiced by making appropriate modifications within the scope that does not impair the effects of the present invention. In this specification, the description of "to" means "not less than or equal to". For example, "X to Y" means not less than X and not more than Y. In this specification, "powder" means "aggregation of particles".

[0011] [Spherical crystalline silica powder] In the spherical crystalline silica powder according to this embodiment, when the temperature is raised from 25°C to 1000°C at a rate of 30°C / min, the number of water molecules desorbed at 50°C to 1000°C (hereinafter also referred to simply as "the number of water molecules desorbed" or "the number of H2O molecules desorbed") is 10 μmol / g or less, and 10 mass% or more of the entire powder is α-quartz crystals. "Spherical" means that when observed under a microscope, the projection has a shape close to a circle. Since it is a spherical powder, it can be filled into a resin at a high content without reducing the flowability. The average circularity and its measurement method will be described later. Here, "crystalline" means that the degree of crystallization is 20% or more. The method for measuring the degree of crystallization will be described later. Conventionally, attempts to crystallize spherical amorphous silica powder have been made to increase the thermal conductivity, etc. by increasing the degree of crystallization to 80% or more (e.g., Patent Documents 1 and 2). However, it has been surprisingly found that spherical crystalline silica in which the number of water molecules to be desorbed is 10 μmol / g or less and 10 mass% or more of the powder is α-quartz crystals can provide a resin molded product with a low dielectric tangent and a high linear thermal expansion coefficient, regardless of the degree of crystallization (both in cases where the degree of crystallization is less than 80% and in cases where the degree of crystallization is more than 80%).

[0012] The "number of desorbed water molecules" was measured using a Pyrolyzer GC / MS system (a combination of a JEOL gas chromatograph mass spectrometer (JMS-Q1500GC) and a Frontier Labs multi-shot pyrolyzer (EGA / PY-3030D)) by heating from 25°C to 1000°C at 30°C / min, and measuring the area value of the resulting mass chromatogram (m / z=18) in the range of 50°C to 1000°C. The number of desorbed water molecules was calculated from the measured area value by drawing a calibration curve using a standard substance with a known amount of dehydration. In one embodiment, the number of H2O molecules released is preferably less than 10 µmol / g, more preferably 9 µmol / g or less, even more preferably 8.8 µmol / g or less, and particularly preferably 8.5 µmol / g or less. In one embodiment, the number of H2O molecules released is preferably less than 10 µmol / g, more preferably 8 µmol / g or less, further preferably 6 µmol / g or less, and particularly preferably 4 µmol / g or less.

[0013] As a method for reducing the number of desorbed water molecules to 10 μmol / g or less, a method in which the spherical amorphous silica powder is crystallized, then contacted with an acid and further subjected to a heat treatment can be mentioned. The details of the production method will be described later. By adjusting the temperature and time of the crystallization process, the amount of hydroxyl groups on the powder surface can be reduced, thereby reducing the number of water molecules that are desorbed, but as described above, the crystal form of the spherical crystalline silica powder changes depending on the heating temperature during crystallization, and so increasing the temperature or prolonging the time in order to reduce the amount of hydroxyl groups on the powder surface may make it impossible to control the appropriate crystal phase. Also, the dielectric loss tangent of the resin molded product may become high.

[0014] The degree of crystallinity of the spherical crystalline silica powder as a whole powder measured by X-ray diffraction (hereinafter, simply referred to as "crystallinity") is preferably 30 to 98%, more preferably 35 to 90%, even more preferably 38 to 85%, and even more preferably 38 to 80%. By setting the degree of crystallinity to 30 to 98%, it is possible to easily obtain a spherical crystalline silica powder having a high linear thermal expansion coefficient. The degree of crystallinity is calculated from the ratio of the integrated peak area of ​​standard crystalline silica measured by X-ray diffraction (XRD) to the integrated peak area of ​​spherical crystalline silica (integral peak area of ​​spherical crystalline silica / integral peak area of ​​standard crystalline silica).

[0015] The degree of crystallization can be adjusted by adjusting the temperature and / or time in the step of crystallizing the spherical amorphous silica powder. It can also be adjusted by adjusting the temperature and / or time in the step of further heating after crystallization. The higher the temperature and the longer the time, the higher the degree of crystallization. The preferred temperature and / or time in the crystallization step and heating step will be described later. Furthermore, the degree of crystallization can also be adjusted using a crystallizing agent, which will be described later. When adjusting the degree of crystallization by temperature or time, it may be difficult to control the appropriate crystal phase, so it is preferable to adjust the degree of crystallization using a crystallizing agent, which will be described later, in terms of ease of controlling the crystal phase.

[0016] From the viewpoint of reducing the viscosity when mixed with a resin, the spherical crystalline silica powder preferably has an average circularity of 0.80 or more, more preferably 0.85 or more, and even more preferably 0.90 or more.

[0017] The method for measuring the "average circularity" is as follows. The spherical crystalline silica powder is fixed with carbon tape and then osmium coated. The powder is then photographed at a magnification of 500 to 50,000 times using a scanning electron microscope, and the projected area (S) and projected perimeter (L) of the powder are calculated using an image analyzer, and the circularity is then calculated from the following formula (1). The circularity is calculated for any 200 powder particles, and the average value is taken as the average circularity. Circularity = 4πS / L 2 (1)

[0018] The spherical crystalline silica powder is composed of α-quartz crystals at 10% by mass or more of the entire powder, preferably 20% by mass or more of the entire powder, and more preferably 30% by mass or more of the entire powder. By including 10% by mass or more of α-quartz crystals, it is possible to obtain a resin molded product with a high linear thermal expansion coefficient and low dielectric tangent. In addition, when molded into a resin product, it can exhibit thermal expansion behavior similar to that of crushed quartz powder. When crushed quartz powder is used as a resin molded product, dimensional changes due to thermal expansion near the reflow temperature are small. Therefore, cracks and warping of molded products caused by temperature changes before and after the reflow process can be easily suppressed. In one embodiment, the spherical crystalline silica powder may be composed of α-quartz crystals at 40% by mass or more, or 45% by mass or more, of the entire powder. In one embodiment, the spherical crystalline silica powder is preferably 20 to 90 mass% α-quartz crystals, more preferably 25 to 85 mass% of the entire powder is α-quartz crystals, and even more preferably 30 to 70 mass% of the entire powder is α-quartz crystals.

[0019] The spherical crystalline silica powder is preferably 0 to 70% by mass of cristobalite crystals, more preferably 0 to 50% by mass of cristobalite crystals, even more preferably 0 to 40% by mass of cristobalite crystals, and particularly preferably 0 to 36% by mass of cristobalite crystals. The spherical crystalline silica powder does not need to contain cristobalite crystals. When it contains cristobalite, by making the content of cristobalite 70% by mass or less, it is possible to more easily manufacture a resin molded product having a high linear thermal expansion coefficient and a low dielectric tangent.

[0020] The spherical crystalline silica powder is preferably tridymite crystals in an amount of 0 to 70% by mass, more preferably 0 to 40% by mass. The spherical crystalline silica powder does not have to contain tridymite crystals. When it contains tridymite crystals, the content of the tridymite crystals is set to 70% by mass or less, so that a resin molded product having a high linear thermal expansion coefficient and a low dielectric tangent can be more easily manufactured.

[0021] The content of each crystal type in the spherical crystalline silica powder can be measured by X-ray diffraction measurement and Rietveld analysis.

[0022] The average powder diameter of spherical crystalline silica powder (cumulative 50% diameter by volume D 50 The volume-based cumulative 50% diameter D is preferably 0.1 to 100 μm, more preferably 0.2 to 50 μm, and even more preferably 0.3 to 10 μm. By setting the average powder diameter of the spherical crystalline silica powder to 0.1 to 100 μm, the fillability into the resin tends to be improved. 50 " means the powder diameter at which the cumulative value corresponds to 50% in the volume-based cumulative particle size distribution measured using a laser diffraction particle size distribution analyzer (refractive index: 1.50).

[0023] The specific surface area of ​​spherical crystalline silica powder is 6m 2 / g or less is preferable, and 5.5m 2 / g or less is more preferable, and 5m 2 / g or less is more preferable. 2 / g or less, it is easy to achieve a lower dielectric tangent. The lower limit of the specific surface area of ​​spherical crystalline silica powder is 1 m 2 / g or more is preferred. In one embodiment, the specific surface area of ​​the spherical crystalline silica powder is 1 to 6 m 2 The specific surface area of ​​the spherical crystalline silica powder is a value measured by a fully automatic specific surface area diameter measuring device according to the BET single point method.

[0024] When producing spherical crystalline silica powder, an alkali metal compound or an alkaline earth metal compound may be used as a crystallizing agent to promote crystallization. In order to further reduce the dielectric tangent, the content of alkaline earth metal elements (Be, Mg, Ca, Sr, Ba, etc.) remaining in the powder is preferably less than 10000 μg / g, more preferably less than 9000 μg / g, calculated as oxide. The content of alkali metal elements (Li, Na, etc.) remaining in the powder is preferably less than 30000 μg / g, calculated as oxide. The content (in terms of oxide) of alkali metal compounds and alkaline earth metal elements in the spherical crystalline silica powder is measured using an ICP emission spectrometer.

[0025] From the viewpoint of reducing impurities, the spherical crystalline silica powder preferably has a U content of 10 ppb or less, a Th content of 20 ppb or less, an Fe content of 200 ppm or less, and / or an Al content of 1 mass% or less (10000 ppm or less). The content of the above impurities in the spherical crystalline silica powder is measured using an ICP emission spectrometer.

[0026] The spherical crystalline silica powder has a linear thermal expansion coefficient (CTE1) of 3.5×10 or less at a glass transition temperature Tg of a test piece (resin molded product) prepared by the method described below. -5 / K~4.5×10 -5 / K, more preferably 3.7×10 -5 / K~4.3×10 -5 / K, and more preferably 3.8×10 -5 / K~4.0×10-5 / K. Because it has a high coefficient of linear thermal expansion (CTE1) below the glass transition temperature Tg, it can prevent warping and cracks during temperature cycling when the product is in use. The spherical crystalline silica powder has a linear thermal expansion coefficient (CTE2) in a temperature range exceeding the glass transition temperature Tg of a test piece (resin molded product) produced by the method described below, which is preferably 10.0×10 -5 / K~11.5×10 -5 / K, more preferably 10.5×10 -5 / K~11.3×10 -5 / K, and more preferably 10.6×10 -5 / K~11.1×10 -5 / K. Since the coefficient of linear thermal expansion (CTE2) is high in the temperature range exceeding the glass transition temperature Tg, warping and cracks during reflow can be prevented.

[0027] The test specimens are prepared by mixing a liquid epoxy resin (e.g., "JER828" manufactured by Mitsubishi Chemical Corporation) and a curing agent (4,4-Diaminodiphenylmethane) in a weight ratio of 4:1, filling the mixture with spherical crystalline silica powder to a volumetric ratio of 40%, and curing the mixture at 200°C to produce a cured product. The cured product is processed to produce test specimens measuring 4 mm x 4 mm x 15 mm.

[0028] The linear thermal expansion coefficients CTE1 and CTE2 are measured using a thermomechanical analyzer at a temperature range of -10°C to 270°C and a heating rate of 5°C / min. The linear thermal expansion coefficient (CTE1) at or below the glass transition temperature Tg and the linear thermal expansion coefficient (CTE2) in the temperature range above the glass transition temperature Tg are calculated.

[0029] The spherical crystalline silica powder has a dielectric loss tangent (tan δ) of preferably 7.0×10 -4 More preferably, it is 6.9×10 or less. -4 More preferably, it is 6.8×10 or less. -4 The dielectric tangent (tan δ) is 7.0×10 -4By setting it as follows, it is possible to further prevent transmission loss of circuit signals in electronic devices, communication devices, and the like that use high frequency bands.

[0030] The spherical crystalline silica powder has a dielectric constant (εr) of preferably 2.5 or more, more preferably 2.6 or more, and even more preferably 2.65 or more, in the resin sheet produced by the method described below. By making the dielectric constant (εr) 2.5 or more, the dielectric constant becomes high, and electronic devices, communication devices, etc. can be made smaller.

[0031] It has been found that by crystallizing spherical amorphous silica powder, contacting it with an acid and further heat-treating it, a spherical crystalline silica powder having a high linear thermal expansion coefficient and a reduced dielectric tangent can be obtained.

[0032] The resin sheet was produced by mixing spherical crystalline silica powder and polyethylene resin powder so that the loading amount of the spherical crystalline silica powder was 40 volume %, pouring the resulting resin composition into a metal frame with a diameter of 3 cm in an amount to give a thickness of approximately 0.3 mm, forming the sheet into a sheet using a nanoimprinting device, and cutting the resulting sheet into a size of 1.5 cm x 1.5 cm to prepare a resin sheet for testing.

[0033] The dielectric constant and dielectric loss tangent were measured by connecting a 36GHz cavity resonator to a vector network analyzer, placing a test resin sheet to cover a 10mm diameter hole in the cavity resonator, and measuring the resonance frequency (f0) and unloaded Q value (Qu). After each measurement, the evaluation sample was rotated 90 degrees and the same measurement was repeated five times, and the average values ​​of f0 and Qu were taken as the measured value. Analysis software was used to calculate the dielectric constant from f0 and the dielectric loss tangent (tan δc) from Qu. The measurement conditions were a temperature of 20°C and a humidity of 60% RH.

[0034] The spherical crystalline silica powder has a thermal conductivity of preferably 0.48 W / mK or more, more preferably 0.50 W / mK or more, and even more preferably 0.55 W / mK or more, measured on a resin sheet produced by the method described below. By making the thermal conductivity 0.48 W / mK or more, the specific conductivity of the produced resin sheet can be improved. Crystallization of spherical amorphous silica improves its thermal conductivity, and it was found that the thermal conductivity can be further improved by contacting the crystallized silica with acid and then heating it. The thermal conductivity is a value calculated by multiplying the thermal diffusivity, specific gravity, and specific heat measured by the following methods. The thermal diffusivity was determined by the laser flash method using the processed resin sheet. A xenon flash analyzer (NETZSCH, product name: LFA447 NanoFlash) was used as the measuring device. The resin sheet was prepared by mixing a liquid epoxy resin (for example, "JER828" manufactured by Mitsubishi Chemical Corporation) and a curing agent (4,4-Diaminodiphenylmethane) in a weight ratio of 4:1, filling the mixture with spherical crystalline silica powder to a volume ratio of 40%, and curing at 200°C to prepare a cured product. The cured product was processed to obtain a disk-shaped test piece with a diameter of 10 mm and a thickness of 1 mm. The specific gravity of the powder was determined using Archimedes' method. The specific heat was measured using a differential scanning calorimeter (manufactured by TA Instruments, product name: Q2000) by heating from room temperature to 200° C. at a heating rate of 10° C. / min in a nitrogen atmosphere.

[0035] (Application) The spherical crystalline silica powder according to the present embodiment can be filled in resin with good dispersibility and high content, and can be used as a filler for resin molded products for various applications such as electronic devices and communication devices. In particular, it can provide resin molded products with high thermal expansion coefficients and low dielectric tangents, and can be preferably used in the manufacture of semiconductor encapsulants for electronic devices and communication devices that use high frequencies. Resin molded products containing the spherical crystalline silica powder can suppress cracks and warping during temperature changes before and after reflow processing and temperature cycles during use.

[0036] [Manufacturing method] The method for producing the spherical crystalline silica powder according to this embodiment is as follows: (i) heating a spherical amorphous silica powder to obtain a spherical crystalline silica powder; (ii) contacting the spherical crystalline silica powder with an acid; and (iii) Heating the spherical crystalline silica powder treated by (ii) at 800 to 1400° C. Before the step (i), a step (i′) of preparing a spherical amorphous silica powder may be included.

[0037] <Step (i'): Preparation of spherical amorphous silica powder> In the optional step (i'), spherical amorphous silica powder is prepared. The spherical amorphous silica powder may be one produced by a conventional method, but from the viewpoint of productivity and production costs, it is preferable to use spherical amorphous silica powder produced by a flame fusion method. In the flame fusion method, the ore powder is melted and spheroidized at a temperature above the melting point of the ore powder (for example, a temperature of 1800°C or higher) by injecting the powder into a high-temperature flame formed by a combustible gas and a combustion supporting gas using a burner. From the viewpoint of cost reduction, the raw material is preferably a pulverized product of a mineral and / or ore. Examples of the mineral or ore include silica sand and silica stone. The average powder size of the raw material is not limited and can be appropriately selected from the viewpoint of workability. Average powder diameter of raw material (50% cumulative diameter by volume D 50) is preferably 0.1 to 100 μm, more preferably 0.2 to 50 μm, and even more preferably 0.3 to 10 μm. The resulting spherical amorphous silica powder is classified as necessary.

[0038] The spherical amorphous silica powder has an average circularity of preferably 0.80 or more, more preferably 0.85 or more, and even more preferably 0.90 or more. The method for measuring the average circularity is as described above.

[0039] Average powder diameter of spherical amorphous silica powder (cumulative 50% diameter by volume D 50 ) is preferably 0.1 to 100 μm, more preferably 0.2 to 50 μm, and even more preferably 0.3 to 10 μm.

[0040] <Step (i): Crystallization step> In step (i), the spherical amorphous silica powder is heated to obtain a spherical crystalline silica powder. The spherical amorphous silica powder is crystallized by heating at a predetermined temperature to become a crystalline silica powder. The heating temperature is preferably 900 to 1250°C, more preferably 950 to 1200°C, and even more preferably 1000 to 1200°C so that 10% by mass or more of the entire powder becomes α-quartz crystals. The heating time is preferably 2 to 40 hours, more preferably 3 to 30 hours, and even more preferably 4 to 24 hours. The heating method is not particularly limited, and can be performed using a known electric furnace or the like. Thereafter, it is cooled to room temperature (26°C).

[0041] Since spherical crystalline silica powder can give resin molded products with a high linear thermal expansion coefficient and low dielectric tangent even though the degree of crystallinity is lower than that of conventional products, the crystallization process can be carried out under milder conditions (lower temperature and / or shorter time) than conventional products.

[0042] A crystallizing agent can be used to promote crystallization. Examples of the crystallizing agent include oxides and carbonates of alkali metals or alkaline earth metals. Specific examples of the crystallizing agent include MgCO3, CaCO3, SrCO3, Li2O, Na2O, etc., and it is preferable to use one or more selected from these. When using a crystallizing agent, the raw material spherical amorphous silica powder and the crystallizing agent are mixed (for example, mixed for 2 to 10 minutes using a grinder such as a vibration mill or various mixers), and then heated in an electric furnace or the like.

[0043] The proportion of the crystallizing agent used is preferably 1 to 10 mol, more preferably 2 to 8 mol, and further preferably 3 to 5 mol, based on 100 mol of the spherical amorphous silica powder.

[0044] In step (i), the spherical amorphous silica powder (preferably a mixture of the spherical amorphous silica powder and a crystallizing agent) may be mixed with a solvent and then heated to obtain a spherical crystalline silica powder. By heating the mixture of the spherical amorphous silica powder and the solvent, the crystallinity and crystal type can be easily adjusted. Examples of the solvent include water and alcohol. The amount of the solvent used may be, for example, 1 to 30 ml per 10 g of the spherical amorphous silica powder. The crystallized silica powder can be crushed and classified using a vibrating sieve or the like, if necessary.

[0045] <Step (ii): Contact with acid> In step (ii), the spherical crystalline silica powder is contacted with an acid. The acid has an acid dissociation constant pKa of 7.0 or less, preferably 6.0 or less, more preferably 5.0 or less at 25° C. Specific examples of the acid include acetic acid, nitric acid, hydrochloric acid, phosphoric acid, sulfuric acid, etc., and it is preferable to include at least one selected from these.

[0046] The amount of the acid used may be, for example, 50 to 1000 ml, or may be 100 to 500 ml, per 10 g of the spherical crystalline silica powder.

[0047] The method for contacting the spherical crystalline silica powder with the acid is not particularly limited, and can be carried out, for example, by adding the acid to the spherical crystalline silica powder and mixing them. The mixing method is not particularly limited, and for example, the spherical crystalline silica powder and the acid aqueous solution can be placed in a beaker and stirred at 10 to 90°C (preferably 30 to 70°C) for 10 to 600 minutes (preferably 30 to 180 minutes). Thereafter, the mixture is washed multiple times with water or ethanol, and then filtered to remove the acid. The resulting powder is heated in step (iii).

[0048] <Step (iii): Heating step> In step (iii), the spherical crystalline silica powder after the treatment in step (ii) is heated at 800 to 1400°C. The heating temperature is preferably 900 to 1300°C, more preferably 1000 to 1200°C. By heating the spherical crystalline silica powder at 800 to 1400°C, the number of water molecules that are desorbed can be reduced without significantly affecting the content ratio of α-quartz crystals and cristobalite crystals. In addition, the crystallinity can be easily adjusted. The heating time is preferably 30 minutes to 24 hours, more preferably 1 to 12 hours, and further preferably 2 to 8 hours. The heating method is not particularly limited, and a known electric furnace or the like can be used. After being allowed to cool naturally in the electric furnace, the spherical crystalline silica powder is recovered at 110°C to 300°C, and then further cooled to 25°C in an environment with a humidity of 40% RH or less. The step (iii) may be followed by a step of classifying the powder to have a desired average powder size.

[0049] The number of water molecules released, the degree of crystallinity, the crystal type, and the average powder diameter (volume-based cumulative 50% diameter D 50 ), average circularity, impurity content, etc. are as described above and therefore will not be described here.

[0050] [Resin composition] The resin composition according to this embodiment contains the above-mentioned spherical crystalline silica powder and a resin.

[0051] (resin) Examples of the resin include thermoplastic resins and thermosetting resins. Examples of the resin include polyethylene resins, polypropylene resins, epoxy resins, silicone resins, phenolic resins, melamine resins, urea resins, unsaturated polyester resins, fluororesins, polyamide-based resins such as polyimide resins, polyamideimide resins, and polyetherimide resins, polyester-based resins such as polybutylene terephthalate resins and polyethylene terephthalate resins, polyphenylene sulfide resins, wholly aromatic polyester resins, polysulfone resins, liquid crystal polymer resins, polyethersulfone resins, polycarbonate resins, maleimide-modified resins, ABS resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins. These may be used alone or in combination of two or more.

[0052] When the resin composition is used as a substrate material for high frequency bands or an insulating material, a known low dielectric resin used for this purpose can be used. Specifically, at least one resin selected from a hydrocarbon-based elastomer resin, a polyphenylene ether resin, and an aromatic polyene-based resin can be used. Among these, a hydrocarbon-based elastomer resin or a polyphenylene ether resin is preferred. The proportion of these resins is preferably 20 to 95% by mass, more preferably 30 to 95% by mass, based on the total mass of the resin composition.

[0053] The content of the spherical crystalline silica powder in the resin composition is not particularly limited and can be appropriately adjusted according to the purpose. For example, when used as a high-frequency substrate material or an insulating material, the content of the spherical crystalline silica powder may be in the range of 5 to 80 mass % relative to the total mass of the resin composition, and more preferably in the range of 5 to 70 mass %. The blending ratio of the resin and the spherical crystalline silica powder in the resin composition can be appropriately adjusted according to the desired dielectric properties such as the linear thermal expansion coefficient and the dielectric loss tangent, etc. For example, the amount of the resin can be adjusted in the range of 10 to 10,000 parts by mass per 100 parts by mass of the spherical crystalline silica powder.

[0054] The resin composition may contain a curing agent, a curing accelerator, a release agent, a coupling agent, a colorant, etc., within the scope of not impairing the effects of the present invention.

[0055] [Method of producing resin composition] The method for producing the resin composition is not particularly limited, and the resin composition can be produced by stirring, dissolving, mixing, and dispersing a predetermined amount of each material. The apparatus for mixing, stirring, dispersing, etc. of the mixture is not particularly limited, but a mortar and pestle machine equipped with a stirring and heating device, a three-roll mill, a ball mill, a planetary mixer, etc. can be used. These apparatuses may also be used in appropriate combination.

[0056] As described above, the resin composition containing the spherical crystalline silica powder according to this embodiment can achieve a high linear thermal expansion coefficient and a low dielectric loss tangent. Therefore, it can be preferably used for manufacturing semiconductor encapsulation materials for electronic devices and communication devices that use high frequencies. The obtained resin molded product can suppress cracks and warping due to temperature changes before and after reflow processing and temperature cycles during use. EXAMPLES

[0057] The present invention will be described in more detail below with reference to examples, but the interpretation of the present invention is not limited to these examples.

[0058] [Reference example] Crushed quartz powder (Fujifilm Wako Pure Chemical Industries, Ltd. "Silicon dioxide, 99.9%", average powder diameter D 50 10 g of silica powder (fine particle size: 20.7 μm) was placed in an alumina crucible and heat-treated for 4 hours at 1000° C. in an electric furnace. After heat treatment, the powder was cooled to 200° C. in the furnace and then cooled to room temperature in a desiccator (23° C.-10% RH). The resulting powder was used as the silica powder of the reference example.

[0059] Experiment 1 [Example 1-1] Spherical amorphous silica powder (manufactured by Denka Co., Ltd., "FB-5D", average powder diameter D50 SiO2:CaCO3) was weighed out so that the molar ratio (SiO2:CaCO3) was 100:3, and dry-mixed for 3 minutes using a vibration mixer (Resodyn). 50 g of the mixture was placed in an alumina crucible, and 5 ml of pure water was added and mixed. The crucible was then placed in an electric furnace and heat-treated at an electric furnace temperature of 1000°C for 12 hours (step (i)). After the heat treatment, the mixture was cooled to 200°C in the furnace and cooled to room temperature in a desiccator (23°C-10% RH), and the obtained powder was crushed using a mortar and classified using a sieve with 200 μm openings. The obtained powder was placed in a 500 ml beaker, 500 ml of 1M acetic acid was dropped therein, and the mixture was stirred for 60 minutes (step (ii)). After that, the acetic acid was removed by filtration, and the obtained residue was placed in an alumina crucible and placed in an electric furnace, where it was heat-treated at an electric furnace temperature of 1000°C for 4 hours (step (iii)). After the heat treatment, it was cooled to 200°C in the furnace, and then cooled to room temperature in a desiccator (23°C-10% RH) to obtain a spherical crystalline silica powder of Example 1-1.

[0060] [Example 1-2] A spherical crystalline silica powder of Example 1-2 was obtained in the same manner as in Example 1-1, except that the heating temperature in the step (iii) was 1200°C.

[0061] [Examples 1-3] The spherical amorphous silica powder of Example 1-3 was obtained in the same manner as in Example 1-1, except that in step (i), the molar ratio of the spherical amorphous silica powder to CaCO3 was weighed out to be 100:5, and in step (iii), the heating temperature was set to 1100°C.

[0062] [Examples 1-4] The spherical amorphous silica powder of Example 1-4 was obtained in the same manner as in Example 1-1, except that in step (i), the molar ratio of the spherical amorphous silica powder to CaCO3 was measured to be 100:5, and in step (iii), the heating temperature was 1200°C.

[0063] [Examples 1-5] The spherical crystalline silica powder of Example 1-5 was obtained in the same manner as in Example 1-1, except that in step (i), the heat treatment conditions were 1200°C and 24 hours, and in step (ii), 500 ml of 1M nitric acid was used instead of acetic acid.

[0064] [Comparative Example 1-1] Spherical amorphous silica powder (Denka Co., Ltd. "FB-5D", average powder diameter D 50 : 4.5 μm) was used as the silica powder of Comparative Example 1-1 (that is, steps (i) to (iii) were not carried out).

[0065] [Comparative Example 1-2] 10 g of the spherical amorphous silica powder of Comparative Example 1-1 was filled into an alumina crucible and heat-treated at 1000°C in an electric furnace for 4 hours. After the heat treatment, it was cooled to 200°C in the furnace and cooled to room temperature in a desiccator (23°C-10%RH) to obtain a silica powder of Comparative Example 1-2. When the crystallinity was measured by the method described below, the silica powder of Comparative Example 1-2 had the same crystallinity as Comparative Example 1-1, and crystallization had not progressed and it remained amorphous.

[0066] [Comparative Example 1-3] Spherical amorphous silica powder (manufactured by Denka Co., Ltd., "FB-5D", average powder diameter D 50 SiO2:CaCO3) was weighed out so that the molar ratio (SiO2:CaCO3) was 100:1, and dry-mixed for 3 minutes using a vibration mixer (Resodyn). The mixture was placed in a crucible and placed in an electric furnace, and heated to 1300°C at a heating rate of 10°C / min in the atmosphere, and held at 1300°C for 4 hours (step (i)). The mixture was allowed to cool naturally in the furnace to room temperature, and a silica powder of Comparative Example 1-3 was obtained.

[0067] Experiment 2 [Example 2-1] Spherical amorphous silica powder (manufactured by Denka Co., Ltd., "SFP-30M", average particle size D 50SiO2:CaCO3) was weighed out so that the molar ratio (SiO2:CaCO3) was 100:3, and dry-mixed for 3 minutes using a vibration mixer (Resodyn). 50 g of the mixture was placed in an alumina crucible, and 5 ml of pure water was added and mixed. The crucible was then placed in an electric furnace and heat-treated at an electric furnace temperature of 1100°C for 12 hours (step (i)). After the heat treatment, the mixture was cooled to 200°C in the furnace and cooled to room temperature in a desiccator (23°C-10% RH), and the obtained powder was crushed using a mortar and classified using a sieve with 200 μm openings. The obtained powder was placed in a 500 ml beaker, 500 ml of 1M acetic acid was dropped therein, and the mixture was stirred for 60 minutes (step (ii)). After that, the acetic acid was removed by filtration, and the obtained residue was placed in an alumina crucible and placed in an electric furnace, where it was heat-treated at an electric furnace temperature of 1000°C for 4 hours (step (iii)). After the heat treatment, it was cooled to 200°C in the furnace, and then cooled to room temperature in a desiccator (23°C-10% RH) to obtain a spherical crystalline silica powder of Example 2-1.

[0068] [Example 2-2] A spherical crystalline silica powder of Example 2-2 was obtained in the same manner as in Example 2-1, except that in step (i), the heat treatment conditions were changed to 1000° C. for 6 hours.

[0069] [Comparative Example 2-1] A silica powder of Comparative Example 2-1 was obtained in the same manner as in Example 2-1, except that the step (iii) was not performed.

[0070] [Comparative Example 2-2] A silica powder of Comparative Example 2-2 was obtained in the same manner as in Example 2-2, except that the step (iii) was not performed.

[0071] [Comparative Example 2-3] Spherical amorphous silica powder (manufactured by Denka Co., Ltd., "SFP-30M", average particle size D 50 The silica powder obtained was 0.68 μm and used as the silica powder of Comparative Example 4 (that is, steps (i) to (iii) were not carried out).

[0072] [Comparative Example 2-4] 10 g of the spherical amorphous silica powder of Comparative Example 2-3 was filled into an alumina crucible and heat-treated at 1000°C in an electric furnace for 4 hours. After the heat treatment, it was cooled to 200°C in the furnace and then cooled to room temperature in a desiccator (23°C-10%RH) to obtain a silica powder of Comparative Example 2-4. When the crystallinity was measured by the method described below, the silica powder of Comparative Example 2-4 had the same crystallinity as Comparative Example 2-3, and crystallization had not progressed and it remained amorphous.

[0073] Experiment 3 [Example 3-1] The spherical crystalline silica powder of Example 3-1 was obtained in the same manner as in Example 1-1, except that in step (i), the heat treatment conditions were 1200°C and 4 hours, and in step (ii), 500 ml of 1M nitric acid was used instead of acetic acid.

[0074] [Example 3-2] The spherical crystalline silica powder of Example 3-2 was obtained in the same manner as in Example 1-1, except that in step (i), the heat treatment conditions were 1100°C and 6 hours, in step (ii), 500 ml of 1 M nitric acid was used instead of acetic acid, and in step (iii), the heat treatment conditions were 1100°C and 4 hours.

[0075] [Comparative Example 3-1] A silica powder of Comparative Example 3-1 was obtained in the same manner as in Example 3-1, except that steps (ii) and (iii) were not performed.

[0076] [Comparative Example 3-2] A silica powder of Comparative Example 3-2 was obtained in the same manner as in Example 3-2, except that steps (ii) and (iii) were not performed.

[0077] [measurement] The physical properties of the silica powders obtained in the examples and comparative examples were measured by the following methods. The results are shown in Tables 1 to 3.

[0078] (XRD measurement: Identification of crystal type and content in powder, and measurement of crystallinity) For the silica powders obtained in the examples and comparative examples, the X-ray diffraction patterns were measured under the following measurement conditions using a horizontal sample multipurpose X-ray diffractometer (manufactured by Rigaku Corporation, product name: RINT-UltimaIV) as the measuring device. X-ray source:CuKα Tube voltage: 40kV Tube current: 40mA Scan speed: 10.0° / min 2θ scan range: 10°~80°

[0079] For quantitative analysis of the crystal types, Rietveld method software (MDI, product name: Integrated Powder X-ray Software Jade+9.6) was used. The proportions (mass%) of various crystal types were calculated by Rietveld analysis after X-ray diffraction measurement of a sample in which α-alumina (internal standard substance) (NIST), a standard sample for X-ray diffraction, was added to silica powder so that its content was 50 mass% (based on the total mass of the spherical crystalline silica powder sample after addition). In Tables 1 to 3, the proportion of α-quartz crystals is shown as "Qua (wt%)" and the proportion of cristobalite crystals is shown as "Cri (wt%)."

[0080] The crystallinity was calculated by calculating the integrated area of ​​the peak of the standard crystalline material and the peak of the crystalline material of the prepared sample for each crystal, and the ratio of the crystalline area to the integrated area of ​​the standard crystalline material was calculated as the crystallinity. Crystallinity = integrated area of ​​the peak of the obtained crystalline silica / peak area of ​​the crystalline silica standard In Tables 1 to 3, the proportion of α-quartz crystals is shown as "Qua (wt%)" and the proportion of cristobalite crystals is shown as "Cri (wt%)."

[0081] (ICP measurement) Impurities in the silica powders obtained in the Examples and Comparative Examples were measured as follows. 1.2 ml of 46% hydrofluoric acid and 5 ml of ultrapure water were added to 0.1 g of silica powder, and the mixture was dried on a hot plate at 120 ° C. 0.3 ml of 96% sulfuric acid was added to the resulting residue, and after heating, the solution was adjusted to 6 ml to prepare a measurement sample. The resulting solid component was collected by filtration, heated together with the filter paper in an electric furnace at 500 ° C. for 2 hours, and the resulting solid was dissolved in alkali and salt, and then adjusted to 6 ml. The measurement sample was then analyzed by ICP emission spectroscopy (ICP spectrometer: SPECTRO, product name: CIROS-120) to measure the impurity content in the spherical crystalline silica powder.

[0082] (Linear thermal expansion coefficient: CTE1, CTE2) A liquid epoxy resin ("JER828" manufactured by Mitsubishi Chemical Corporation) and a curing agent (4,4-diaminodiphenylmethane) were mixed in a weight ratio of 4:1, and silica powder was added to the mixture to make a volumetric ratio of 40%. The mixture was then cured at 200°C for 4 hours to produce a cured product. The cured product was then processed to produce a test piece measuring 4 mm x 4 mm x 15 mm. The linear thermal expansion coefficient was evaluated using a TMA device (TMA4000SA, manufactured by Bruker AXS). The measurement conditions were a heating rate of 3°C / min, a measurement temperature of -10°C to 270°C, and a nitrogen atmosphere, and from the results obtained, the linear thermal expansion coefficient (CTE1) below the glass transition temperature Tg (155 to 160°C) and the linear thermal expansion coefficient (CTE2) in the temperature range above the glass transition temperature Tg (over 160°C) were calculated. The results are shown in Tables 1 to 3. The thermal expansion coefficient of the resin composition without silica powder is 3.4×10 -5 (CTE1), 9.7×10 -5 (CTE2) / ℃.

[0083] FIG. 1 shows the thermal expansion behavior measured for the test pieces using the silica powders of Reference Example, Example 1-5, Comparative Example 1-1, and Comparative Example 1-3. As shown in FIG. 1, the resin molded product containing the silica powder of Example 1-5 shows similar thermal expansion behavior to the resin molded product containing crushed quartz (Reference Example). The resin molded product containing the silica powder of Reference Example (crushed quartz) and the resin molded product containing the silica powder of Example 1-5 have higher linear thermal expansion coefficients (CTE1 and CTE2) than the resin molded product containing the silica powder of Comparative Example 1-1 (spherical amorphous silica powder). When the silica powder of Comparative Example 1-3 (spherical cristobalite crystals, not containing α-quartz crystals) is used, the linear thermal expansion coefficient is high, but the change at the reflow temperature (around 240 to 260 ° C.) is large, and it may be difficult to adjust the thermal expansion behavior of the resin molded product near that temperature. In contrast, the resin molded product containing the silica powder of Example 1-5 does not change the linear thermal expansion coefficient near the reflow temperature, so the thermal expansion behavior of the resin molded product can be easily controlled.

[0084] (Evaluation of dielectric properties) Silica powder and polyethylene resin powder (manufactured by Sumitomo Seika Chemicals Co., Ltd., product name: FLOTHEN (registered trademark) UF-20S) or polypropylene (PP) powder (manufactured by Sumitomo Seika Chemicals Co., Ltd., Flowblen QB200) were weighed so that the filling amount of the silica powder was 40 volume %, and mixed using a vibration mixer (manufactured by Resodyn) at an acceleration of 60 G and a processing time of 2 minutes to obtain a resin composition. The obtained resin composition was poured into a metal frame with a diameter of 3 cm in an amount to give a thickness of about 0.3 mm, and sheeted using a nanoimprint device (manufactured by SCIVAX Co., Ltd., product name: X-300) under conditions of 140 ° C, 5 minutes, and 30,000 N. The obtained sheet was cut into a size of 1.5 cm x 1.5 cm to obtain an evaluation sample. Next, a 36 GHz cavity resonator (manufactured by Samtec Co., Ltd.) was connected to a vector network analyzer (manufactured by Keysight Technologies, product name: 85107), and the evaluation sample was placed so as to cover a 10 mm diameter hole provided in the cavity resonator, and the resonance frequency (f0) and unloaded Q value (Qu) were measured. The evaluation sample was rotated 90 degrees for each measurement, and the same measurement was repeated five times. The average values ​​of the obtained f0 and Qu were taken as the measured values, and the dielectric constant was calculated from f0 and the dielectric loss tangent (tan δc) was calculated from Qu using analysis software (software manufactured by Samtec Co., Ltd.). The measurement was performed under conditions of a measurement temperature of 20°C and a humidity of 60% RH.

[0085] (Number of water molecules released) Using a Pyrolyzer GC / MS system (a combination of a JEOL gas chromatograph mass spectrometer (JMS-Q1500GC) and a Frontier Labs multi-shot pyrolyzer (EGA / PY-3030D)), the temperature was raised from 25°C to 1000°C at 30°C / min, and the area value of the resulting mass chromatogram (m / z=18) in the range of 50°C to 1000°C was measured. The number of water molecules desorbed was calculated from the measured area value by drawing a calibration curve using aluminum hydroxide (Kojundo Chemical Co., Ltd.) as a standard substance with a known amount of dehydration. The amount of dehydration of aluminum hydroxide used as the standard substance was calculated using a thermogravimetric differential thermal analyzer (NETZSCH high-sensitivity differential thermobalance STA2500 Regulus) by heating from 25°C at a rate of 10°C / min, and the weight loss from 200°C to 320°C was used as the amount of dehydration.

[0086] (Measurement of thermal conductivity) The thermal conductivity of the resin composition was calculated by multiplying the thermal diffusivity, specific gravity, and specific heat. The thermal diffusivity was measured by a laser flash method using a sample after curing, which was processed to a size of 10 mm x 10 mm x 1 mm. A xenon flash analyzer (manufactured by NETZSCH, product name: LFA447 NanoFlash) was used as the measuring device. The specific gravity was measured using the Archimedes method. The specific heat was measured by using a differential scanning calorimeter (manufactured by TA Instruments, product name: Q2000) in a nitrogen atmosphere, by heating from room temperature to 200°C at a heating rate of 10°C / min.

[0087] [Table 1] [Table 2] [Table 3]

[0088] As shown in Tables 1 to 3, the spherical crystalline silica powders of each Example, in which the number of desorbed water molecules is 10 μmol / g or less and 10 mass % or more of the total powder is α-quartz crystals, can give resin molded articles with high linear thermal expansion coefficients (CTE1 and CTE2) and low dielectric tangents. The obtained resin molded articles also have high dielectric constants and high thermal conductivities. Furthermore, since the linear thermal expansion coefficient (CTE2) is similar to that of the reference example (crushed quartz), the thermal expansion behavior of the resin molded article near the reflow temperature can be easily controlled. In contrast, the amorphous silica powders of Comparative Examples 1-1 and 2-3, in which the number of desorbed water molecules exceeded 10 μmol / g and the α-quartz crystals were less than 10 mass%, had a low linear thermal expansion coefficient and a high dielectric tangent. The amorphous silica powders of Comparative Examples 1-2 and 2-4, in which the α-quartz crystals were less than 10 mass %, had low dielectric tangents but low linear thermal expansion coefficients (CTE1 and CTE2). The silica powder of Comparative Example 1-3, which is crystalline and does not contain α-quartz crystals, has a high linear thermal expansion coefficient, but a high dielectric loss tangent. As shown in Figure 1, the silica powder of Comparative Example 1-3 has a large change in the thermal expansion behavior of the resin molded product near the reflow temperature, making it difficult to control the thermal expansion behavior of the resin molded product. The silica powders of Comparative Examples 2-1, 2-2, 3-1, and 3-2, in which the number of desorbed water molecules exceeded 10 μmol / g, had a high linear thermal expansion coefficient, but also had a high dielectric tangent. Focusing on thermal conductivity, the spherical crystalline silica powder of each Example was able to achieve a high thermal conductivity of 0.48 W / mK or more. As is clear from Tables 1 to 3, it was found that the thermal conductivity improves each time the raw material amorphous spherical silica is crystallized (step (i)), and then contacted with acid and heat-treated (steps (ii) and (iii)). [Industrial Applicability]

[0089] As described above, the spherical crystalline silica powder according to the present invention has the characteristic of being able to provide a resin molded article having a high linear thermal expansion coefficient and a low dielectric loss tangent. Such a resin molded article containing the spherical crystalline silica powder can be suitably used, for example, as a filler for a sealing material for a semiconductor element.

Claims

1. When the temperature is increased from 25° C. to 1000° C. at a rate of 30° C. / min, the number of water molecules desorbed at 50° C. to 1000° C. is 10 μmol / g or less; A spherical crystalline silica powder, in which 10% by mass or more of the entire powder is α-quartz crystals.

2. 2. The spherical crystalline silica powder according to claim 1, wherein the crystallinity of the entire powder as measured by X-ray diffraction is 30 to 98%.

3. 3. The spherical crystalline silica powder according to claim 1, wherein 20 to 90 mass% of the powder as a whole is α-quartz crystals.

4. The spherical crystalline silica powder according to claim 1 or 2, wherein 0 to 70 mass% of the entire powder is cristobalite crystals.

5. 3. The spherical crystalline silica powder according to claim 1, wherein the content of alkaline earth metal elements is less than 10,000 μg / g calculated as oxide.

6. A resin composition comprising the spherical crystalline silica powder according to claim 1 or 2 and a resin.

7. (i) heating a spherical amorphous silica powder to obtain a spherical crystalline silica powder; (ii) contacting the spherical crystalline silica powder with an acid; and (iii) heating the spherical crystalline silica powder treated by (ii) at 800 to 1400°C.

8. 8. The method for producing spherical crystalline silica powder according to claim 7, wherein in (i), the mixture of spherical amorphous silica powder and the solvent is heated to obtain spherical crystalline silica powder.

Citation Information

Patent Citations

  • JP1974008638A

  • Production of highly pure crystalline silica

    JP1992238808A

  • Silica particle and method of manufacturing the same

    JP2005231973A

  • Spherical silica powder

    JP2021178770A

  • Spherical crystalline silica particles and method for producing same

    WO2018186308A1