How lithium hydroxide is produced
The method addresses the high costs of producing lithium hydroxide by using a lithium selective adsorbent and impurity removal processes to concentrate and purify lithium hydroxide, achieving cost-effective and high-purity production.
Patent Information
- Application Number
- JP2019100890
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-05-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2039-05-30
AI Technical Summary
Existing methods for producing lithium hydroxide from lithium-containing solutions with metal impurities are costly due to low selectivity of extractants and high chemical consumption, and conventional processes for converting lithium carbonate to lithium hydroxide are also expensive.
A method involving lithium adsorption, elution, impurity removal, conversion, and crystallization steps using a lithium selective adsorbent, such as manganese oxide, to concentrate and purify lithium hydroxide, including oxidation and ion exchange processes to remove impurities effectively.
This method allows for the production of high-purity lithium hydroxide at lower costs by concentrating lithium and selectively converting it to hydroxide without using additional lithium compounds, while reducing the load on subsequent steps through impurity removal and crystallization.
Smart Images

Figure 0007558647000007 
Figure 0007558647000008 
Figure 0007558647000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing lithium hydroxide. More specifically, the present invention relates to a method for producing lithium hydroxide at low cost from a lithium-containing solution containing metal impurities other than lithium, such as salt lake brine. [Background technology]
[0002] Lithium is widely used in the industrial world, such as as an additive for ceramics or glass, glass flux for continuous steel casting, grease, medicines, and batteries. In particular, lithium-ion batteries, which are secondary batteries, have the advantages of high energy density and high voltage, and their use has expanded recently not only in electronic devices such as laptops but also in on-board batteries for electric and hybrid vehicles, leading to a rapid increase in demand. As a result, the demand for lithium, the raw material, has also increased rapidly along with this rapid increase in demand.
[0003] Lithium has been produced in the form of lithium hydroxide or lithium carbonate by refining salt lake brine or lithium-containing ores such as lithia (Li2O·Al2O3·2SiO4). Since the lithium content is low compared to other components, a concentration process is first carried out to increase the lithium concentration, and then a conversion process is carried out to convert it into lithium carbonate.
[0004] For example, when using salt lake brine as the raw material, solar concentration is mainly used in major lithium producing countries such as Chile and Argentina. In this method, first, in the concentration process, salt lake brine is concentrated in a concentration pond called a solar pond, and the main components such as sodium and potassium are precipitated and removed as salts such as sodium chloride and potassium chloride, and lithium chloride, which has high solubility, is concentrated in the aqueous solution. After concentration, impurities are removed in a purification process as necessary, and in the next conversion process, sodium carbonate is added to convert lithium chloride into lithium carbonate, which has low solubility. In this conversion process, lithium carbonate precipitates as a solid due to its low solubility. It is possible to recover lithium carbonate by this method.
[0005] The solar concentration method requires chemicals and equipment for the purification and conversion processes, but has the advantage that relatively few chemicals and equipment are required. In addition, the concentration process uses ponds and the energy source is sunlight, so the equipment and energy costs are very low. However, concentration using solar ponds has the disadvantage that it takes several years, which makes it difficult to respond to sudden increases in production. In addition, this method has the disadvantage that it is dependent on the weather, and is only used in places with very little rainfall, such as the highlands of South America. Furthermore, if the salt lake brine contains a lot of sulfate ions, lithium sulfate, which is less soluble than lithium chloride, will precipitate together with sodium chloride and potassium chloride during the concentration process, making it difficult to use in principle. Since most salt lake brines contain sulfate ions, the solar concentration method cannot be widely applied.
[0006] Unlike the above-mentioned solar concentration method, the solvent extraction method, ion exchange method, chromatographic separation method, etc. have been widely used as a method for producing lithium hydroxide and the like that is not affected by climatic conditions or the liquid properties of salt lake brine. However, salt lake brine containing a lot of lithium contains impurities such as sodium, potassium, magnesium, calcium, etc. in overwhelmingly larger amounts than lithium. For this reason, when the solvent extraction method is used in the concentration process, there is a problem that the selectivity of the extractant for lithium is low. In other words, it is necessary to first remove the impurities from the liquid containing a lot of impurities using a large amount of chemicals, which increases the overall cost. The ion exchange method also has a problem that the selectivity of the ion exchange resin for lithium is low, and like the solvent extraction method, there is a problem that the cost of the concentration process is high.
[0007] The chromatographic separation method is a method for separating and recovering lithium by utilizing the difference in elution rate between lithium and impurities other than lithium in a liquid (Patent Document 1). This method also has problems in that the amount of chemicals used in the concentration process is large and the number of steps required is large, resulting in high equipment costs.
[0008] In contrast to the above-mentioned method, Non-Patent Document 1 discloses a method using a lithium-selective adsorbent as a "lithium recovery system from brine." In Non-Patent Document 1, lithium carbonate is the final target, and after lithium is adsorbed using a lithium-selective adsorbent in a concentration process, an alkali carbonate is added in a conversion process to remove impurities, followed by heating and concentration, and finally, carbonate is added to precipitate lithium carbonate, thereby obtaining lithium carbonate powder.
[0009] In recent years, the demand for NCA, a nickel-based positive electrode material, has been increasing as a positive electrode material for automotive batteries, and when used for this purpose, it is economically preferable for lithium to be supplied as lithium hydroxide. This lithium hydroxide has been produced by adding hydrated lime to the above-mentioned lithium carbonate, but there is a problem in that the process of producing lithium hydroxide from lithium carbonate is costly. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] International Publication No. 2012 / 163791 [Non-patent literature]
[0011] [Non-Patent Document 1] Yu, Eihei, "Lithium recovery system from brine", [online], June 11, 2010, Kagawa Industrial Support Foundation, [November 22, 2018], Internet (www.kagawa-isf.jp / rist / seika-happyou / 21tang.pdf) Summary of the Invention [Problem to be solved by the invention]
[0012] In the concentration step, when lithium hydroxide is produced by a conventional solvent extraction method or the like, there is a problem that the cost is high in order to obtain lithium from a liquid containing a large amount of impurities. In addition, Non-Patent Document 1 discloses a method for obtaining lithium carbonate using a lithium selective adsorbent in the conversion step, but does not disclose a method for producing lithium hydroxide in the conversion step without passing through other lithium compounds such as lithium carbonate.
[0013] In view of the above circumstances, an object of the present invention is to provide a method for producing lithium hydroxide, which can produce lithium hydroxide at low cost. [Means for solving the problem]
[0014] The method for producing lithium hydroxide of the first invention includes the following steps (1) to (4): (1) lithium adsorption step: a step of contacting a first lithium-containing solution with a lithium-selective adsorbent to allow lithium to be adsorbed onto the lithium-selective adsorbent, (2) lithium elution step: a step of eluting lithium from the lithium-selective adsorbent to which lithium has been adsorbed, to obtain a second lithium-containing solution, (3) impurity removal step: a step of removing a portion of metal ions from the second lithium-containing solution to obtain a third lithium-containing solution, and (4) conversion step: a step of converting a lithium salt contained in the third lithium-containing solution into lithium hydroxide, to obtain a lithium hydroxide-containing solution in which lithium hydroxide is dissolved, and the impurity removal step is Able to oxidize manganese An oxidation step of adding an oxidizing agent to obtain an oxidized liquid; To increase pH The method includes a neutralization step of adding an alkali to obtain a neutralized solution, and an ion exchange step of contacting the neutralized solution with an ion exchange resin to obtain the third lithium-containing solution. death, The lithium selective adsorbent is a manganese oxide obtained by contacting lithium manganese oxide with an acid and removing lithium from the lithium manganese oxide. It is characterized by the above. The method for producing lithium hydroxide of a second invention is characterized in that, in the first invention, a crystallization step of solidifying the lithium hydroxide dissolved in the lithium hydroxide-containing solution is provided after the conversion step. The method for producing lithium hydroxide according to a third aspect of the present invention is characterized in that, in the first or second aspect of the present invention, the pH of the neutralized solution after the neutralization step is 8.5 or more and 12 or less. No. 4 The lithium hydroxide production method of the present invention is as follows: 3 In any one of the inventions, the pH of the solution in the lithium adsorption step is 3 or more and 10 or less. No. 5 The lithium hydroxide production method of the present invention is as follows: 4 In any one of the inventions, the hydrogen ion concentration of the acid used in the lithium elution step is 0.3 mol / L or more and 2.0 mol / L or less. Effect of the Invention
[0015] According to the first invention, the lithium contained in the liquid can be concentrated to a high concentration by the lithium adsorption step and the lithium elution step. The subsequent conversion step decomposes the lithium salt and allows the lithium ions to bind with hydroxide ions, making it possible to directly produce lithium hydroxide without using other lithium compounds such as lithium carbonate. In addition, the impurity removal step is provided between the lithium elution step and the conversion step, making it possible to selectively convert alkali metals such as lithium into hydroxides without causing problems in the membrane used in the conversion step. In addition, the impurity removal process includes an oxidation process, a neutralization process, and an ion exchange process, so that metal ions other than alkali metals and boron can be removed at a high level. The presence of the oxidation process makes it possible to remove manganese before the neutralization process, thereby reducing the load in the neutralization process. Furthermore, since the lithium selective adsorbent is a specific manganese oxide, it becomes easy to concentrate lithium to a high concentration. According to the second invention, by providing a crystallization step after the conversion step, lithium hydroxide can be solidified to a high purity by utilizing the difference in solubility. According to the third aspect of the present invention, the pH of the neutralized liquid after the neutralization step is 8.5 or more and 12 or less, so that impurities can be removed more reliably in the neutralization step. No. 4 According to the invention, the pH of the solution in the lithium adsorption step is 3 or more and 10 or less, so that lithium is more reliably adsorbed. No. 5 According to the invention, the hydrogen ion concentration of the acid used in the lithium elution step is 0.3 mol / L or more and 2.0 mol / L or less, so that the elution of manganese constituting the lithium selective adsorbent can be suppressed. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a flow diagram showing a method for producing lithium hydroxide according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a flow diagram showing a configuration of an impurity removing step in the manufacturing method of FIG. [Diagram 3]FIG. 1 is a flow diagram showing a configuration of an impurity removing step in a method for producing lithium hydroxide according to a second embodiment of the present invention. [Figure 4] 4 is a graph showing the relationship between the lithium concentration of the first lithium-containing solution after it has flowed out of the column and the amount of the solution passed in Example 1. [Diagram 5] 4 is a graph showing the relationship between the lithium concentration of the second lithium-containing solution after it has flowed out of the column and the amount of the solution passed in Example 1. [Figure 6] 4 is a graph showing the relationship between the lithium concentration in a lithium hydroxide-containing solution and the current-flow time in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Next, an embodiment of the present invention will be described with reference to the drawings. However, the embodiment described below is an example of a method for producing lithium hydroxide to embody the technical concept of the present invention, and the method for producing lithium hydroxide of the present invention is not limited to the following embodiment.
[0018] The method for producing lithium hydroxide according to the present invention includes the following steps (1) to (4). (1) Lithium adsorption step: a step of contacting a first lithium-containing solution with a lithium-selective adsorbent to allow lithium to be adsorbed onto the lithium-selective adsorbent. (2) Lithium elution step: a step of eluting lithium from the lithium selective adsorbent to which lithium has been adsorbed, to obtain a second lithium-containing solution. (3) Impurity removing step: a step of removing a portion of metal ions from the second lithium-containing solution to obtain a third lithium-containing solution. (4) Conversion step: a step of converting the lithium salt contained in the third lithium-containing solution into lithium hydroxide to obtain a lithium hydroxide solution in which lithium hydroxide is dissolved.
[0019] In the method for producing lithium hydroxide, the lithium contained in the liquid can be concentrated to a high concentration by including the lithium adsorption step and the lithium elution step. The subsequent conversion step allows lithium hydroxide to be produced directly without using other lithium compounds such as lithium carbonate. In addition, the impurity removal step between the lithium elution step and the conversion step allows alkali metals such as lithium to be selectively converted into hydroxides without causing problems in the membrane used in the conversion step.
[0020] In addition, in the method for producing lithium hydroxide, it is preferable to provide a crystallization step of solidifying the lithium hydroxide dissolved in the lithium hydroxide-containing solution after the conversion step, whereby the lithium hydroxide can be solidified to a high purity by utilizing the difference in solubility.
[0021] In the method for producing lithium hydroxide, the impurity removing step preferably includes a neutralizing step of adding an alkali to the second lithium-containing solution to obtain a neutralized solution, and an ion exchange step of contacting the neutralized solution with an ion exchange resin to obtain the third lithium-containing solution, thereby making it possible to remove metal ions other than alkali metals and boron at a high level.
[0022] In addition, in the method for producing lithium hydroxide, it is preferable that the impurity removing step includes a step of adding an oxidizing agent to the second lithium-containing solution to obtain an oxidation solution, a neutralization step of adding an alkali to the oxidation solution to obtain a neutralization solution, and an ion exchange step of contacting the neutralization solution with an ion exchange resin to obtain the third lithium-containing solution. This makes it possible to remove metal ions other than alkali metals and boron at a high level. The presence of the oxidation step makes it possible to remove manganese before the neutralization step, thereby reducing the load in the neutralization step.
[0023] In the method for producing lithium hydroxide, the pH of the neutralized solution after the neutralization step is preferably 8.5 or more and 12 or less, so that impurities can be more reliably removed in the neutralization step.
[0024] In the method for producing lithium hydroxide, the lithium selective adsorbent is preferably a manganese oxide obtained by contacting lithium manganate with an acid and removing lithium from the lithium manganate, which makes it easy to concentrate lithium to a high concentration.
[0025] In the method for producing lithium hydroxide, the pH of the solution in the lithium adsorption step is preferably 3 or more and 10 or less, which ensures the adsorption of lithium.
[0026] In the method for producing lithium hydroxide, the hydrogen ion concentration of the acid used in the lithium elution step is preferably 0.3 mol / L or more and 2.0 mol / L or less, which makes it possible to suppress the elution of manganese constituting the lithium selective adsorbent.
[0027] (First embodiment) <Lithium adsorption process> Fig. 1 shows a method for producing lithium hydroxide according to a first embodiment of the present invention. As shown in Fig. 1, the lithium adsorption step is a step in which a lithium selective adsorbent is brought into contact with a first lithium-containing solution having a relatively low lithium concentration, such as salt lake brine, and lithium is selectively adsorbed from the first lithium-containing solution onto the lithium selective adsorbent. The reaction formula in the lithium adsorption step is shown in Equation 1. Here, H 1.6 Mn 1.6 The reaction formula using O4 is shown, but it is not particularly limited to this. For example, it is also possible to use a lithium selective adsorbent obtained from lithium manganese oxide having a spinel structure. In addition, these lithium selective adsorbents are preferably manganese oxides obtained by contacting lithium manganese oxide with an acid and removing lithium from the lithium manganese oxide.
[0028] [Number 1] H 1.6 Mn 1.6 O4+1.6LiCl → Li 1.6 Mn 1.6 O4+1.6HCl
[0029] The method of contacting them is not particularly limited. For example, the contacting method includes a column method and a batch mixing method. In the column method, when the lithium selective adsorbent is used as a fine powder, the liquid passing resistance is high, and continuous liquid passing is often difficult. For this reason, it is preferable to use pellets prepared by kneading the lithium selective adsorbent (including the case where it is a precursor before becoming the lithium selective adsorbent) with a binder such as an alumina binder and sintering the mixture.
[0030] In the lithium adsorption step, the pH of the first lithium-containing solution is preferably 3 or more and 10 or less. Since the reaction in the lithium adsorption step is a reaction of adsorbing lithium and generating an acid, if the pH of the aqueous solution is low, the reaction rate may be slow or the reaction itself may not occur. For this reason, it is desirable to increase the pH of the first lithium-containing solution before contacting the first lithium-containing solution with the lithium selective adsorbent. However, if the first lithium-containing solution contains magnesium, if the pH becomes too high, magnesium hydroxide will precipitate, and this magnesium hydroxide will cover the surface of the lithium selective adsorbent, physically inhibiting the adsorption reaction of lithium. In particular, when a column method is adopted as a contact method, blockages will often occur in the column due to magnesium hydroxide. For these reasons, the pH of the first lithium-containing solution is preferably 10 or less.
[0031] In addition, if the pH is 3 or less after passing through the column, the lower part of the column may not be able to efficiently adsorb lithium. In the circulation method, it is preferable to add a neutralizing agent to the effluent after passing through the column to adjust the pH to the above range, and then return it to the column. When using the column method, the passing speed may be changed according to the required processing amount. If a precipitate occurs after neutralization, a filtration device such as a filter press or a check filter can be used appropriately to smoothly pass through the column. After the adsorption operation, in order to perform the next lithium elution step, the lithium selective adsorbent after lithium adsorption is washed with water as necessary. In the case of passing through the column, after passing the first lithium-containing solution, relatively high purity distilled water or the like is passed through the column to extrude and wash the first lithium-containing solution remaining inside. In the case of batch mixing, after solid-liquid separation, water is poured onto the lithium selective adsorbent after lithium adsorption to remove the first lithium-containing solution that adheres thereto.
[0032] <Lithium elution process> As shown in Fig. 2, in the lithium elution step, the lithium selective adsorbent having lithium adsorbed thereon is brought into contact with a mineral acid such as hydrochloric acid to obtain a second lithium-containing solution. The lithium selective adsorbent after lithium adsorption is in the form of, for example, lithium manganate, and the lithium is eluted by contacting the lithium selective adsorbent after lithium adsorption with a mineral acid such as hydrochloric acid. The contact method is generally a column method, but a batch mixing method may also be used, and any contact method is acceptable. The reaction formula during lithium elution is shown in Equation 2.
[0033] [Number 2] Li 1.6 Mn 1.6 O4+1.6HCl → H 1.6 Mn 1.6 O4+1.6LiCl
[0034] Here, Li is used as lithium manganese oxide. 1.6 Mn 1.6O4 is shown, but is not limited thereto. For example, it is possible to use a lithium selective adsorbent obtained from lithium manganese oxide having a spinel structure. The concentration of the mineral acid needs to be sufficient to elute lithium, but if the concentration is too high, the lithium manganese oxide will dissolve and be worn out. If the concentration is too low, lithium will not elute. The mineral acid can be hydrochloric acid, sulfuric acid, or nitric acid. In any case where any of these acids is used, the acid concentration is preferably 0.3 mol / L or more and 2.0 mol / L or less. When using a column method, the liquid passing speed can be changed according to the required processing volume.
[0035] The eluate obtained in this step, i.e., the second lithium-containing solution, contains sodium, potassium, magnesium, and calcium that are slightly accompanied in the lithium adsorption step. It also contains manganese that is eluted from the lithium selective adsorbent. In addition, when a granule using an alumina binder is used as the lithium selective adsorbent, the second lithium-containing solution contains aluminum. Among these impurities, polyvalent metals other than sodium and potassium cause problems such as shortening the life of the membrane in the subsequent conversion step, so they are removed in the impurity removal step. In addition, the lithium selective adsorbent after lithium adsorption returns to the lithium selective adsorbent by the elution operation and is in a state where it can adsorb lithium again. For this reason, it can be reused in the lithium adsorption step. When reused, it is preferable to wash the lithium selective adsorbent with water.
[0036] <Impurity removal process> As shown in FIG. 1, in the impurity removal step, a part of the metal ions is removed from the second lithium-containing solution to obtain a third lithium-containing solution. FIG. 2 shows a flow diagram showing the configuration of the impurity removal step according to this embodiment. In this embodiment, the impurity removal step includes a neutralization step and an ion exchange step. Note that the impurity removal step is not limited to the configuration shown here. The impurity removal step may be any step that removes a part or all of the metal that affects the membrane in the conversion step.
[0037] <Neutralization process during impurity removal process> As shown in FIG. 2, in the neutralization step, an alkali is added to the second lithium-containing solution to obtain a neutralized solution and a neutralized precipitate containing impurities. In the neutralization step, the pH increases due to the added alkali, and magnesium mainly becomes a hydroxide and precipitates as a neutralized precipitate. At the same time, manganese is also removed as a hydroxide. To precipitate and remove magnesium and manganese, an alkaline solution is sufficient, but if the pH is too high, the cost of the neutralizing agent increases, which is not preferable. For this reason, the pH of the neutralized solution after the neutralization step is preferably 8.5 or more and 12 or less.
[0038] <Ion exchange process during impurity removal process> As shown in Figure 2, in the ion exchange process, the neutralized solution is brought into contact with an ion exchange resin to obtain a third lithium-containing solution from which some of the impurities have been removed. In the ion exchange process, calcium that cannot be removed in the neutralization process, aluminum that remains depending on the pH of the neutralization process, and trace amounts of manganese and magnesium that could not be completely removed in the neutralization process are removed.
[0039] The ion exchange resin used is preferably a chelating resin. For example, an iminodiacetic acid type resin can be used. The pH of the neutralized liquid in the ion exchange step is determined by the ion exchange resin. However, it is preferable to carry out the ion exchange step directly on the neutralized liquid obtained in the neutralization step. The method of contacting the ion exchange resin with the neutralized liquid is preferably a column method. However, a batch mixing method may also be adopted.
[0040] <Conversion process> As shown in FIG. 1, in the conversion step, the lithium salt contained in the third lithium-containing solution is converted to lithium hydroxide to obtain a lithium hydroxide-containing solution in which lithium hydroxide is dissolved. In the third lithium-containing solution, lithium salts such as lithium chloride, lithium sulfate, and lithium nitrate are dissolved by the mineral acid used for elution. In this step, for example, by electrodialysis using a bipolar membrane, these aqueous solutions are converted into a lithium hydroxide-containing solution containing lithium hydroxide and a mineral acid such as hydrochloric acid, sulfuric acid, or nitric acid. That is, by performing electrodialysis, the lithium salt in the third lithium-containing solution is decomposed, and the lithium ions of the lithium salt pass through the cationic membrane and combine with the hydroxide ions to become lithium hydroxide, and for example, the chloride ions pass through the anionic membrane to become hydrochloric acid. The recovered mineral acid can be recycled to the elution step. This can reduce the amount of mineral acid used.
[0041] In addition to electrodialysis using a bipolar membrane, the conversion process may also include electrodialysis using an ion exchange membrane. When a cation exchange membrane is used as the ion exchange membrane, lithium hydroxide is produced in the cathode chamber.
[0042] <Crystallization process> Lithium hydroxide is obtained by evaporating the lithium hydroxide-containing solution obtained in the conversion step to dryness. However, this lithium hydroxide-containing solution contains alkali metals such as sodium or potassium, and if it is evaporated to dryness as it is, the solid obtained from it will contain a large amount of hydroxides other than lithium hydroxide. For this reason, it is preferable to provide a crystallization step for solidifying the lithium hydroxide dissolved in the lithium hydroxide-containing solution after the conversion step.
[0043] In the crystallization process, the lithium hydroxide dissolved in the lithium hydroxide-containing solution is solidified to obtain solid lithium hydroxide. The crystallization mother liquor is obtained together with this solid lithium hydroxide. In the conversion process, lithium becomes lithium hydroxide, and alkali metals such as sodium and potassium also become hydroxides. Therefore, these are also contained in the lithium hydroxide-containing solution obtained in the conversion process. Furthermore, chloride ions, which are anions, also pass through the membrane and are contained in the lithium hydroxide-containing solution. In the crystallization process, the difference in solubility of each hydroxide is utilized to solidify lithium hydroxide and separate the impurities contained therein.
[0044] In the crystallization process, the lithium hydroxide-containing solution is heated and concentrated. During this process, the concentration of metal ions contained in the solution increases, and lithium hydroxide, which has a relatively low solubility, precipitates and solidifies first. This precipitated lithium hydroxide is recovered as solid lithium hydroxide. During this process, sodium hydroxide and potassium hydroxide, which have a relatively high solubility, are left in the aqueous solution without being precipitated. This increases the purity of the recovered lithium hydroxide.
[0045] For example, the solubility of lithium hydroxide at 60℃ is 13.2g / 100g-water, which is extremely low when compared to sodium hydroxide's 174g / 100g-water and potassium hydroxide's 154g / 100g-water. Since chloride ions are 2g / L even during the heating and concentration process, they do not precipitate in lithium hydroxide as alkali metal chlorides.
[0046] This process can be carried out industrially by continuous crystallization using a crystallizer. It can also be carried out by batch crystallization. The crystallization mother liquor generated in the crystallization process is a concentrated alkaline aqueous solution. This crystallization mother liquor contains lithium hydroxide to the extent of its solubility, so by repeating this in the lithium adsorption process, the lithium recovery rate increases. In addition, the cost of the neutralizing agent is reduced.
[0047] Second embodiment 3 is a flow diagram showing the configuration of the impurity removal step in the method for producing lithium hydroxide according to the second embodiment of the present invention. The difference between this embodiment and the first embodiment is that the impurity removal step includes an oxidation step. The other points are the same as those of the first embodiment. The oxidation step, which is the difference, will be described below.
[0048] <Oxidation process during impurity removal process> The oxidation step is a step in which an oxidizing agent such as air, oxygen, or sodium hypochlorite is added to the second lithium-containing solution obtained in the lithium elution step to oxidize the manganese in the second lithium-containing solution and turn it into insoluble manganese dioxide, thereby precipitating and removing the manganese dissolved in the solution. Manganese can also be removed in the neutralization step, but by providing the oxidation step, manganese is removed before the neutralization step, so the load of removing manganese in the neutralization step can be reduced. In addition, the manganese precipitated and removed in the oxidation step can be reused. The types of oxidizing agents used in the oxidation step include air, oxygen, and sodium hypochlorite. The redox potential of the second lithium-containing solution is set to a pH and potential that is in the manganese dioxide region on the potential-pH diagram. EXAMPLES
[0049] Specific examples of the method for producing lithium hydroxide according to the present invention will be described below, but the present invention is not limited to these examples.
[0050] Example 1 <Lithium adsorption process> As a lithium selective adsorbent, H 1.6 Mn 1.6 O4 was used. This lithium selective adsorbent, 600 mL in volume (bulk density: 1.0), was packed into a 1 L column (inner diameter 50 mm). A first lithium-containing solution with a pH of 8 was then passed through the column. The first lithium-containing solution contained chlorides or sulfates of lithium, sodium, magnesium, potassium, and calcium, and boric acid, as shown in Table 1. The metal concentrations were analyzed by ICP-AES.
[0051] [Table 1]
[0052] 90 L of this first lithium-containing solution was passed through the column at a flow rate of 100 mL / min. FIG. 4 shows the relationship between the lithium concentration of the first lithium-containing solution after it has flowed out of the column and the amount of the solution passed. Note that BV on the X-axis of the graph stands for Bed Volume, and is a unit that indicates how many times the volume of the lithium selective adsorbent in the column. In this embodiment, the capacity of the lithium selective adsorbent is 600 mL, so 90 L is 150 BV. In addition, the flow rate may also be indicated as SV. SV stands for Space Velocity, and indicates the amount of solution passed per unit time (1 hour). In this embodiment, it is 100 mL / min, so it is 6 L / h, and therefore SV10.
[0053] As shown in Figure 4, the amount of lithium in the first lithium-containing solution after it had flowed out of the column became approximately the same as the amount of lithium originally contained in the first lithium-containing solution when about 100 BV, i.e., 60 L, had been passed through the column, and it can be seen that lithium had been sufficiently adsorbed onto the lithium-selective adsorbent at this point.
[0054] After 90 L of the first lithium-containing solution had been passed through the column, 15 L (BV25) of distilled water was passed through the column at 100 L / min (SV10) to push out the first lithium-containing solution remaining inside the column, thereby washing the inside of the column.
[0055] <Lithium elution process> As the mineral acid, a hydrochloric acid solution with a concentration of 0.5 mol / L was passed through the column at a flow rate of 100 mL / min (SV10) at only 9 L (BV15). Figure 5 shows the relationship between the lithium concentration of the second lithium-containing solution after it has flowed out of the column and the amount of the solution passed. From Figure 5, it can be seen that the second lithium-containing solution before 0.6 L (BV1) and after 4.8 L (BV8) contains almost no lithium. From this result, the second lithium-containing solution of BV2 to 7 was used in the subsequent steps. The metal concentrations of the second lithium-containing solution used in the subsequent steps are shown in Table 2. The metal concentrations were analyzed by ICP-AES.
[0056] [Table 2]
[0057] By carrying out the lithium adsorption process and the lithium elution process, the lithium in the solution is concentrated, and the concentrations of sodium, magnesium, potassium, and calcium, which were extremely high compared to lithium in the first lithium-containing solution, are reduced, indicating that lithium is selectively recovered.
[0058] <Neutralization process (impurity removal process)> 6.5 L of the second lithium-containing solution (pH 0.6) obtained in the lithium elution step was placed in a 20 L plastic tank, and 66 mL of an 8 mol / L NaOH aqueous solution was added while stirring and mixing at room temperature. The pH of the solution was then adjusted to 10 while stirring and mixing for 30 minutes. The precipitate and aqueous solution that were produced were subjected to solid-liquid separation using 5C filter paper. The aqueous solution after solid-liquid separation is the neutralized solution. The metal concentrations are shown in Table 3. The metal concentrations were analyzed by ICP-AES.
[0059] [Table 3]
[0060] As shown in Table 3, the magnesium and aluminum concentrations in the neutralized solution were reduced to 0.002 g / L, and the manganese concentration was <0.001 g / L, below the detection limit. It was found that magnesium and manganese were removed from the neutralized solution by this process.
[0061] <Ion exchange process (impurity removal process)> 5L of the neutralized solution and 500mL of chelating resin (Diaion CR11, manufactured by Mitsubishi Chemical Corporation) were placed in a 20L plastic container. The mixture was stirred and mixed at room temperature for 30 minutes. After stirring and mixing, the contents were separated into solid and liquid using 5C filter paper. The metal concentration of the third lithium-containing solution, which was the liquid after solid-liquid separation, is shown in Table 4.
[0062] [Table 4]
[0063] The ion exchange process reduced the amount of polyvalent metal ions other than alkali metals and boron to extremely low levels. Metal concentrations were analyzed by ICP-AES for Li, Na, K, and B, and by ICP-MS for Mg, Ca, Mn, and Al.
[0064] <Conversion process> Five liters of the third lithium-containing solution obtained in the impurity removal process was introduced into a bipolar membrane electrodialysis device (Astrom: Acilyzer EX3B), and lithium chloride was converted to lithium hydroxide. The volume of the lithium hydroxide-containing solution after conversion was 0.8 L. The relationship between the current application time and the lithium concentration in the lithium hydroxide aqueous solution is shown in Figure 6. The tester set the initial lithium concentration in the lithium hydroxide-containing solution to be 1.0 g / L. The lithium concentration in the lithium hydroxide-containing solution increased with the application of current, and was finally concentrated to 11 to 12 g / L. The metal concentrations after conversion are shown in Table 5. Analysis of the metal concentrations was performed using ICP-AES.
[0065] [Table 5]
[0066] By going through the above-mentioned steps, lithium was selectively recovered from an aqueous solution system, such as salt lake brine, which contains overwhelmingly more impurities such as sodium, potassium, magnesium, and calcium compared to lithium, and a lithium hydroxide-containing solution in which lithium hydroxide is dissolved could be obtained.
[0067] <Crystallization process> 0.8L of the lithium hydroxide-containing solution obtained in the conversion process was placed in a SUS beaker, heated with gentle stirring, and concentrated to 0.2L while maintaining a temperature of 90-100°C, and the precipitated lithium hydroxide was recovered. The analytical values of lithium hydroxide are shown in Table 6. It was confirmed that lithium hydroxide with a low impurity concentration could be recovered.
[0068] [Table 6]
Claims
1. The following steps (1) to (4): (1) a lithium adsorption step: a step of contacting a first lithium-containing solution with a lithium selective adsorbent to allow lithium to be adsorbed onto the lithium selective adsorbent; (2) Lithium elution step: a step of eluting lithium from the lithium selective adsorbent to which lithium has been adsorbed, to obtain a second lithium-containing solution; (3) an impurity removing step: removing a part of metal ions from the second lithium-containing solution to obtain a third lithium-containing solution; (4) a conversion step: a step of converting the lithium salt contained in the third lithium-containing solution into lithium hydroxide to obtain a lithium hydroxide-containing solution in which lithium hydroxide is dissolved; Inclusive of The impurity removing step includes: an oxidation step of adding an oxidizing agent capable of oxidizing manganese to the second lithium-containing solution to obtain an oxidized solution; a neutralization step of adding an alkali to the oxidized liquid so as to increase the pH of the liquid to obtain a neutralized liquid; an ion exchange step of contacting the neutralized solution with an ion exchange resin to obtain the third lithium-containing solution; Inclusive of The lithium selective adsorbent is a manganese oxide obtained by contacting lithium manganese oxide with an acid and releasing lithium from the lithium manganese oxide. A method for producing lithium hydroxide comprising the steps of:
2. After the conversion step, a crystallization step is provided for solidifying the lithium hydroxide dissolved in the lithium hydroxide-containing solution. The method for producing lithium hydroxide according to claim 1 .
3. The pH of the neutralized solution after the neutralization step is 8.5 or more and 12 or less. The method for producing lithium hydroxide according to claim 1 or 2.
4. The pH of the solution in the lithium adsorption step is 3 or more and 10 or less. The method for producing lithium hydroxide according to any one of claims 1 to 3.
5. The hydrogen ion concentration of the acid used in the lithium elution step is 0.3 mol / L or more and 2.0 mol / L or less; The method for producing lithium hydroxide according to any one of claims 1 to 4.
Citation Information
Patent Citations
Production of li adsorbent
JP1986278347A
Method for producing high-purity lithium hydroxide
JP2009269810A
Method for producing high-purity lithium hydroxide and hydrochloric acid
JP2011518257A
Method for removing iron and aluminum from lithium ion battery scarp and method for recovering valuable metals
JP2017036478A
Method for manufacturing a lithium chloride solution from brine
WO2012163791A1