Coating material composition, silicone rubber molded article, and fuel cell separator

A coating material composition using ethylene/α-olefin/non-conjugated polyene random copolymer and organosilicon compounds addresses the hydrofluoric acid resistance issue in silicone rubber, offering durable and flexible coatings for fuel cell separators.

JP7558909B2Active Publication Date: 2024-10-01SHIN ETSU CHEMICAL CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021135639
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-08-23
Publication Date
2024-10-01
Estimated Expiration
2041-08-23

AI Technical Summary

Technical Problem

Silicone rubber materials lack sufficient hydrofluoric acid resistance, and combinations with other resins result in complex structures that are difficult to implement practically.

Method used

A coating material composition comprising an ethylene/α-olefin/non-conjugated polyene random copolymer with hydrosilyl groups connected via sylalkylene or sylarylene bonds, an organosilicon compound without siloxane bonds, and an addition reaction catalyst, which forms a durable and acid-resistant coating on silicone rubber.

Benefits of technology

The composition provides excellent hydrofluoric acid resistance and flexibility, suitable for use as a sealing material in fuel cell separators, maintaining strength and flexibility even after exposure to corrosive environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558909000001
    Figure 0007558909000001
  • Figure 0007558909000002
    Figure 0007558909000002
  • Figure 0007558909000003
    Figure 0007558909000003
Patent Text Reader

Abstract

To provide an acidity resistant material excellent particularly in hydrogen fluoride acidity resistance, and a silicone rubber member coated with the same.SOLUTION: A coating material composition includes: (A) 100 pts.mass of an ethylene-α-olefin-nonconjugated polyene random copolymer composed of a random copolymer of nonconjugated polyene, ethylene, and α-olefin; (B) an organosilicon compound having two or more hydrosilyl groups which are bonded to other silicon atoms through 1-30C silalkylene bonds or 6-30C silarylene bonds and have no siloxane bond, in one molecule, in an amount of the mole ratio of hydrosilyl groups in the constituent (B) to addition reactive unsaturated groups in the constituent (A) of 0.5-5.0 (hydrosilyl groups / unsaturated groups=0.5-5.0); and (C) an addition reaction catalyst in an amount to the constituent (A) of 0.5-1,000 ppm in terms of a metal atom.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating material composition, a silicone rubber molded article, and a fuel cell separator. [Background technology]

[0002] Polymer electrolyte fuel cells have come to be used as an alternative technology to on-board internal combustion engines, and commercial vehicles have been developed that use fuel cells to drive motors. One of the components that make up polymer electrolyte fuel cells is the separator. A separator is generally made of a flat plate with multiple parallel grooves formed on both sides or one side, and plays a role in transmitting electricity generated by the gas diffusion electrode in the fuel cell to the outside. At the same time, it also plays a role in draining water generated in the grooves during the power generation process and ensuring that they serve as a flow path for the reactant gas flowing into the fuel cell. There is a demand for separators for fuel cells to be more compact. In addition, since many separators are used in layers, there is a demand for separator sealing materials that are highly durable and can be used for a long period of time.

[0003] In addition, the membrane electrode assembly (MEA), which is the power generating part of a polymer electrolyte fuel cell, is composed of a fuel electrode (anode), an electrolyte membrane, and an air electrode (cathode), and the electrolyte membrane is mainly made of a fluoropolymer with sulfonic acid groups. The sealing material used in the separator of a polymer electrolyte fuel cell must be resistant to the sulfuric acid and hydrofluoric acid that are generated by this electrolyte membrane.

[0004] As sealing materials for solid polymer fuel cell separators, silicone rubber, ethylene-propylene-diene rubber, fluororubber, etc. have been proposed. Among them, silicone rubber is excellent in various properties such as moldability, heat resistance, cold resistance, elasticity, compression set, and water vapor resistance, and silicone rubber obtained by curing an addition-type liquid silicone rubber composition has been widely studied. The addition of silicone resin or hydrotalcite has also been considered for improving acid resistance (Patent Document 1, Patent Document 2), but the drawback that the siloxane bond, which is the main skeleton of polydimethylsiloxane, is extremely susceptible to cleavage by high concentration hydrofluoric acid has not been overcome. In addition, there is an example of crosslinking ethylene-propylene-diene rubber with a hydrosilicone compound (Patent Document 3), but it is difficult to obtain sufficient acid resistance because the siloxane bond in the hydrosilicone is broken by hydrofluoric acid.

[0005] Furthermore, it has been proposed to seal the outer periphery of silicone rubber with ethylene propylene rubber or fluororubber, which have excellent resistance to hydrofluoric acid (Patent Document 4 and Patent Document 5). However, this method has problems such as the complex shape, the difficulty in matching the hardness and compression behavior of both materials, and different behavior depending on the temperature range. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2002-309092 A [Patent Document 2] JP 2017-016813 A [Patent Document 3] JP 2019-175842 A [Patent Document 4] JP 2008-204819 A [Patent Document 5] JP 2009-026654 A Summary of the Invention [Problem to be solved by the invention]

[0007] So far, silicone rubber alone has not been able to provide sufficient resistance to hydrofluoric acid, and the structure of combining silicone rubber with other resins is complicated, making it quite difficult to use in practice.

[0008] In view of the above, an object of the present invention is to provide an acid-resistant material that is particularly resistant to hydrofluoric acid, and a silicone rubber member coated with the acid-resistant material. [Means for solving the problem]

[0009] In order to solve the above problems, the present invention provides (A) an ethylene-α-olefin-non-conjugated polyene random copolymer consisting of a random copolymer of a non-conjugated polyene, ethylene, and an α-olefin: 100 parts by mass, (B) an organosilicon compound having two or more hydrosilyl groups per molecule, the hydrosilyl groups being bonded to other silicon atoms via a silalkylene bond having 1 to 30 carbon atoms or a silarylene bond having 6 to 30 carbon atoms, and having no siloxane bonds: an amount such that the molar ratio of addition-reactive unsaturated groups in component (A) to hydrosilyl groups in component (B) is hydrosilyl groups / unsaturated groups=0.5 to 5.0, and (C) Addition reaction catalyst: an amount of 0.5 to 1,000 ppm in terms of metal atoms relative to the component (A) The present invention provides a coating material composition comprising:

[0010] Such a coating material composition can provide an acid-resistant material that is particularly excellent in resistance to hydrofluoric acid, and a silicone rubber member coated with the material.

[0011] The content of the addition reactive unsaturated group in the component (A) is preferably 0.001 to 0.2 mol / 100 g.

[0012] If the content of unsaturated groups is within this range, sufficient strength can be obtained and necessary flexibility can easily be obtained.

[0013] The component (A) is preferably an ethylene-propylene-5-vinyl-2-norbornene copolymer.

[0014] In the present invention, it is preferable to use such a component (A).

[0015] The present invention also provides a silicone rubber molded article having a cured film of the above coating material composition.

[0016] The coating material composition of the present invention can be suitably used for coating silicone rubber molded articles.

[0017] The present invention also provides a separator for a fuel cell, comprising: The present invention provides a fuel cell separator comprising a separator substrate, a silicone rubber layer formed on one or both sides of the separator substrate, and a cured film of the coating material composition formed on the surface of the silicone rubber layer opposite to the surface in contact with the separator substrate.

[0018] The coating material composition of the present invention can be particularly suitably used as a sealing material for fuel cell separators. Effect of the Invention

[0019] According to the present invention, it is possible to provide a coating material composition having excellent resistance to hydrofluoric acid, in particular an EPDM rubber coating material composition, and a silicone rubber molded article coated with the same, which can be particularly suitably used as a sealing material for separators for fuel cells. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] As described above, there has been a demand for the development of an acid-resistant material that is particularly resistant to hydrofluoric acid, and a silicone rubber member coated with the acid-resistant material.

[0021] As a result of intensive research conducted by the present inventors in order to achieve the above-mentioned object, it was discovered that an EPDM (ethylene propylene diene monomer) rubber coating material composition containing an ethylene-α-olefin-non-conjugated polyene random copolymer, an organosilicon compound having a hydrosilyl group having a silalkylene bond or a silarylene bond, and an addition reaction catalyst has particularly excellent durability against hydrofluoric acid, which led to the completion of the present invention.

[0022] That is, the present invention provides a coating material composition comprising: (A) 100 parts by mass of an ethylene-α-olefin-non-conjugated polyene random copolymer consisting of a random copolymer of a non-conjugated polyene, ethylene, and an α-olefin; (B) an organosilicon compound having two or more hydrosilyl groups in one molecule, the hydrosilyl groups being bonded to other silicon atoms via a silalkylene bond having 1 to 30 carbon atoms or a silarylene bond having 6 to 30 carbon atoms, and having no siloxane bond, in an amount such that the molar ratio of addition-reactive unsaturated groups in component (A) to hydrosilyl groups in component (B) is hydrosilyl group / unsaturated group = 0.5 to 5.0; and (C) an addition reaction catalyst in an amount such that the molar ratio, calculated as metal atoms, is 0.5 to 1,000 ppm relative to component (A).

[0023] The present invention will be described in detail below, but the present invention is not limited thereto.

[0024] [(A) Ethylene-α-olefin-non-conjugated polyene random copolymer] The component (A) in the present invention is an ethylene-α-olefin-non-conjugated polyene random copolymer, which is the base polymer.

[0025] Examples of α-olefins include propylene, 1-butene, 1-pentene, 1-butene, and 1-hexene, and preferably have 3 to 10 carbon atoms, more preferably propylene and 1-butene, and further preferably propylene. These α-olefins may be used alone or in combination of two or more.

[0026] Examples of non-conjugated polyenes include 5-vinyl-2-vinylnorbornene, 1,4-hexadiene, dicyclopentadiene, etc., and 5-vinyl-2-vinylnorbornene is preferred because it has good reactivity with hydrosilyl groups and improves the heat resistance of the copolymer itself. These non-conjugated polyenes may be used alone or in combination of two or more.

[0027] The component (A) is preferably an ethylene-propylene-5-vinyl-2-norbornene copolymer.

[0028] It is preferable that the composition ratio of the ethylene-α-olefin-non-conjugated polyene in the ethylene-α-olefin-non-conjugated polyene random copolymer satisfies the following condition. (I) The ratio of ethylene to the total number of moles of ethylene and α-olefin is preferably from 30 to 90 mol %, particularly preferably from 40 to 80 mol %. (II) The amount of non-conjugated polyene in the ethylene-α-olefin-non-conjugated polyene random copolymer is preferably an amount such that the content of unsaturated groups reactive to addition to hydrosilyl groups is 0.001 to 0.2 mol / 100 g, and particularly preferably 0.002 to 0.1 mol / 100 g.

[0029] If (I) is within this range, the glass transition temperature is kept low and it is suitable for in-vehicle use. In addition, if the content of unsaturated groups in (II) is 0.001 mol / 100 g or more, sufficient strength is obtained, and if it is 0.2 mol / 100 g or less, the required flexibility is easily obtained.

[0030] Regarding the molecular weight of the ethylene-α-olefin-non-conjugated polyene random copolymer, the number average molecular weight Mn (polystyrene equivalent by gel permeation chromatography (GPC)) is preferably 300 to 8,000, particularly 500 to 6,000. By making the number average molecular weight 300 or more, the necessary rubber strength can be obtained. On the other hand, from the viewpoint of manufacturability, it is preferably 8,000 or less.

[0031] [(B) Organosilicon compound having a hydrosilyl group] The component (B) in the present invention is an organosilicon compound having a hydrosilyl group, which is blended as a crosslinking agent that undergoes an addition reaction with the component (A) to form a cured coating.

[0032] The component (B) is characterized in that it has two or more hydrosilyl groups in one molecule, preferably 2 to 30, more preferably 2 to 20, even more preferably 2 to 10, and most preferably 2 to 5. In addition, the hydrosilyl groups are characterized in that they are bonded to other silicon atoms via a silalkylene bond having 1 to 30, preferably 2 to 20, and more preferably 2 to 10 carbon atoms, or a silarylene bond having 6 to 30, preferably 6 to 20, and more preferably 6 to 10 carbon atoms.

[0033] Here, the "other silicon atom" to which the hydrosilyl group is bonded via a silalkylene bond or a silarylene bond may be any other silicon atom contained in the organosilicon compound, and may be a silicon atom constituting another hydrosilyl group or a silicon atom other than the above.

[0034] In addition, a silalkylene bond refers to a structure in which a silicon atom and another silicon atom are linked and bonded via an alkylene group, and a silarylene bond refers to a structure in which a silicon atom and another silicon atom are linked and bonded via an arylene group.

[0035] Furthermore, component (B) does not have the siloxane bond found in general silicones, which dramatically improves the acid resistance, particularly the resistance to hydrofluoric acid, of the coating material composition of the present invention.

[0036] A specific example of the structure of component (B) is an organosilicon compound in which two hydrosilyl groups are linked via an alkylene group or an arylene group, as shown in formula (1-1) below.

[0037] [ka] (In the formula, R is a group selected from an alkylene group having 1 to 30 carbon atoms and an arylene group having 6 to 30 carbon atoms.)

[0038] In formula (1-1), R is particularly preferably an alkylene group having 2 to 6 carbon atoms or a phenylene group. Specific examples of the organosilicon compound represented by formula (1-1) include the following compounds.

[0039] [ka]

[0040] Another specific example of the structure of component (B) is an organosilicon compound represented by the following formula (1-2).

[0041] [ka] (In the formula, R is a group selected from an alkylene group having 1 to 30 carbon atoms or an arylene group having 6 to 30 carbon atoms. R 1 is a methyl group or a phenyl group. 2 is an alkylene group having 1 to 30 carbon atoms. x is an integer of 2 to 4.

[0042] In formula (1-2), R is particularly preferably an alkylene group having 2 to 6 carbon atoms or a phenylene group. 2 Particularly preferred is an ethylene group or a propylene group. Specific examples of the organosilicon compound represented by formula (1-2) include the following compounds.

[0043] [ka] (In the above formula, R is the same as above.)

[0044] Another specific example of the structure of the component (B) is an organosilicon compound represented by the following formula (1-3).

[0045] [ka] (In the formula, R is a group selected from an alkylene group having 1 to 30 carbon atoms or an arylene group having 6 to 30 carbon atoms. Z is a divalent hydrocarbon group having 10 to 30 carbon atoms, which may contain an aromatic ring or an oxygen atom.)

[0046] In the formula (1-3), R is particularly preferably an alkylene group having 2 to 6 carbon atoms or a phenylene group. Specific examples of the organosilicon compound represented by the formula (1-3) include the following compounds.

[0047] [ka] (In the above formula, R is the same as above.)

[0048] The amount of the (B) component is preferably such that the molar ratio of the addition-reactive unsaturated groups in the (A) component to the hydrosilyl groups in the (B) component is hydrosilyl groups / unsaturated groups = 0.5 to 5.0, particularly 0.8 to 3.0. If this ratio is less than 0.5, the strength of the resulting cured product may be significantly reduced, and if it is more than 5.0, the flexibility of the resulting rubber cured product may be lost, resulting in insufficient sealing properties. The (B) component may be used alone or in combination of two or more types.

[0049] The blend amount of component (B) is preferably 0.5 to 50 parts by mass per 100 parts by mass of component (A). If the blend amount of component (B) is within this range, more sufficient resistance to hydrofluoric acid can be obtained.

[0050] [(C) Addition reaction catalyst] The addition reaction catalyst is a hydrosilylation catalyst for causing an addition reaction between the unsaturated groups contained in the ethylene-α-olefin-non-conjugated polyene random copolymer (A) and the hydrosilyl groups contained in the organosilicon compound (B). Examples of the addition reaction catalyst include platinum-based catalysts such as platinum black, platinic chloride, chloroplatinic acid, reaction products of chloroplatinic acid with monohydric alcohols, complexes of chloroplatinic acid with olefins, platinum bisacetoacetate, and other platinum group metal catalysts, such as palladium-based catalysts and rhodium-based catalysts, with platinum-based catalysts being particularly preferred.

[0051] The amount of component (C) is 0.5 to 1,000 ppm in terms of metal atoms relative to component (A). The amount of catalyst added may be any amount that can promote the addition reaction, and is usually preferably 0.5 to 1,000 ppm, more preferably about 1 to 500 ppm, of platinum group metal (mass equivalent) relative to component (A). If the amount is less than 0.5 ppm, the addition reaction may not be promoted sufficiently, resulting in insufficient curing, and even if the amount exceeds 1,000 ppm, the effect on reactivity may not change, which may be uneconomical.

[0052] [Other ingredients] Furthermore, the coating material composition of the present invention can also contain, as other components as necessary, fillers such as silica, quartz powder, diatomaceous earth, carbon, calcium carbonate, calcium oxide, etc., plasticizers such as paraffin-based process oil, nitrogen-containing compounds, acetylene compounds, phosphorus compounds, nitrile compounds, carboxylates, tin compounds, mercury compounds, sulfur compounds, hydrosilylation reaction inhibitors such as ethynylcyclohexanol, etc.

[0053] [Coating material composition] The method for producing the coating material composition of the present invention is not particularly limited, but it can be produced by mixing the above-mentioned components (A) to (C) and other components according to a conventional method.

[0054] The coating material composition of the present invention may be coated as it is, or may be diluted with a solvent before coating. When diluting, any solvent that dissolves each component may be selected, but a hydrocarbon solvent with excellent solubility is preferable. Among them, an aliphatic hydrocarbon solvent that can suppress the swelling of the silicone rubber when coated on the silicone rubber layer is particularly preferable, and n-hexane or n-heptane is more preferable. When the solution is prepared, the coating method may be brush coating or spray coating.

[0055] The coating amount can be adjusted by the coating method, the number of coatings, the concentration of the coating material composition, etc., and the coating amount of the cured product after drying and curing is 0.05 to 5 g / m 2 is preferable, and 0.1 to 2 g / m 2 is particularly preferred. 2 If the thickness is set to 5 g / m or more, deterioration of the silicone rubber layer can be sufficiently suppressed. 2 If the content is within the range described below, it is possible to impart excellent elasticity and compression set properties to the silicone rubber layer.

[0056] The curing conditions for the coating material composition of the present invention are usually 100 to 200°C for 10 seconds to 2 hours, and preferably 20 seconds to 30 minutes at 120 to 180°C for curing and molding. After curing and molding (i.e., after the first curing), a post-cure (secondary curing) may be performed for the purpose of improving the adhesiveness and curing properties of the cured product. Considering the heat resistance temperature of the (A) component, the post-cure conditions are 80 to 180°C for 30 minutes to 10 hours, and preferably 100 to 150°C for about 1 to 8 hours.

[0057] Furthermore, the composition containing the components (A), (B) and (C) may be used as a single EPDM molding rather than as a coating material.

[0058] [Silicone rubber molded products] The present invention also provides a silicone rubber molded article having a cured film of the coating material composition of the present invention.

[0059] The coating material composition of the present invention is preferably used because forming a cured film of the coating material composition on the surface of a silicone rubber molded article can impart acid resistance, particularly resistance to hydrofluoric acid, to the silicone rubber.

[0060] The silicone rubber is not particularly limited, but examples thereof include addition curing silicone rubber, peroxide curing silicone rubber, condensation curing silicone rubber, ultraviolet curing silicone rubber, etc., which are usually commercially available. Among them, addition curing silicone rubber is preferable because it has good moldability and excellent compression set. Examples of the addition curing silicone rubber include a silicone rubber composition containing the following components (a) to (d).

[0061] [(a) Alkenyl-containing organopolysiloxane] Component (a) is an organopolysiloxane containing two or more alkenyl groups bonded to silicon atoms in one molecule, and is the main component (base polymer) that forms the elastic sealing layer (cured silicone rubber). As this organopolysiloxane, one represented by the following average composition formula (I) can be used. R 1 a SiO (4-a) / 2 …(I) (In the formula, R 1 are the same or different monovalent hydrocarbon groups having 1 to 10 carbon atoms, preferably 1 to 8 carbon atoms, and a is a positive number ranging from 1.5 to 2.8, preferably 1.8 to 2.5, and more preferably 1.95 to 2.05.

[0062] Here, the above R 1Examples of the monovalent hydrocarbon group represented by the formula include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, cyclohexyl, octyl, nonyl, and decyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; aralkyl groups such as benzyl, phenylethyl, and phenylpropyl; and alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, hexenyl, cyclohexenyl, and octenyl. Note that some or all of the hydrogen atoms in these groups may be substituted with halogen atoms such as fluorine, bromine, and chlorine. In particular, all R 1 More than 90% of the R groups, especially all R groups except for alkenyl groups 1 The group is preferably a methyl group.

[0063] Also, R 1 Among these, at least two must be alkenyl groups (preferably having 2 to 8 carbon atoms, more preferably having 2 to 6 carbon atoms, and particularly preferably vinyl groups). The content of alkenyl groups in the organopolysiloxane must be 5.0×10 -6 mol / g~5.0×10 -3 mol / g, specifically 1.0×10 -5 mol / g~1.0×10 -3 mol / g. The amount of alkenyl groups is preferably 5.0×10 -6 If the ratio is 5.0×10 mol / g or more, the rubber hardness is high and sufficient sealing performance is obtained. -3 If it is less than mol / g, the crosslink density will not become too high and the rubber will not become brittle.

[0064] The alkenyl group may be bonded to a silicon atom at a molecular chain terminal, or to a silicon atom in the middle of the molecular chain, or to both, but it is preferable for the alkenyl group to have alkenyl groups bonded to silicon atoms at least at both molecular chain terminals.

[0065] The structure of the organopolysiloxane is preferably a linear structure, but may be a branched structure, a cyclic structure, or a three-dimensional network structure. There is no particular limitation on the molecular weight, and anything from a liquid with low viscosity at room temperature (25°C) to a raw rubber with high viscosity can be used, but it is preferable that the weight-average degree of polymerization of the organopolysiloxane is 100 to 2,000, particularly 150 to 1,500. If the weight-average degree of polymerization is 100 or more, the silicone rubber cured product has appropriate elasticity and sufficient sealing properties can be obtained, and if it is 2,000 or less, the silicone rubber composition does not become highly viscous and difficult to mold. When the organopolysiloxane has a three-dimensional network structure, the weight-average molecular weight of the organopolysiloxane is preferably 100,000 or less (usually 3,000 to 100,000), more preferably about 5,000 to 50,000, for the same reason. The weight-average degree of polymerization or weight-average molecular weight can usually be determined as a polystyrene-equivalent value in molecular weight distribution (polymerization distribution) measurement by gel permeation chromatography (GPC) analysis using toluene as a developing solvent.

[0066] [(b) Organohydrogenpolysiloxane] Component (b) is an organohydrogenpolysiloxane containing three or more hydrogen atoms bonded to silicon atoms (hydrosilyl groups) in one molecule. The hydrosilyl groups in the molecule crosslink with the alkenyl groups bonded to silicon atoms in component (a) through a hydrosilyl addition reaction, acting as a crosslinking agent for curing the composition.

[0067] The organohydrogenpolysiloxane of component (b) is represented by the following average composition formula (II): R 2 b H c SiO (4-b-c) / 2 …(II) (In the formula, R 2are the same or different monovalent hydrocarbon groups having 1 to 10 carbon atoms, preferably 1 to 8 carbon atoms. In addition, b is 0.7 to 2.1, c is 0.001 to 1.0, and is a positive number that satisfies b+c=0.8 to 3.0. and preferably has 3 or more (usually 3 to 300), preferably 3 to 100, and more preferably 3 to 50 hydrosilyl groups in one molecule.

[0068] Here, R 2 Examples of the monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, cyclohexyl, octyl, nonyl, and decyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; and aralkyl groups such as benzyl, phenylethyl, and phenylpropyl. Some or all of the hydrogen atoms in these groups may be substituted with halogen atoms such as fluorine, bromine, and chlorine. In particular, when all R 2 More than 90% of the total R 2 The group is preferably a methyl group. Furthermore, b is preferably 0.8 to 2.0, c is preferably 0.01 to 1.0, and b+c is preferably 1.0 to 2.5.

[0069] The organohydrogenpolysiloxane of component (b) generally does not contain any functional groups other than hydrosilyl groups (for example, alkenyl groups, epoxy groups, polyvalent aromatic rings such as phenylene skeletons, etc.) in the molecule.

[0070] The molecular structure of the organohydrogenpolysiloxane may be any of linear, cyclic, branched, and three-dimensional network structures, and the number or degree of polymerization of silicon atoms in one molecule is preferably 2 to 300, particularly about 4 to 150, and is liquid at room temperature (25°C) (usually 1,000 mPa·s or less at 25°C, preferably about 0.1 to 500 mPa·s). The viscosity referred to here is the value measured using a rotational viscometer (e.g., BL type, BH type, BS type, cone-plate type, etc.) described in JIS K 7117-1:1999. The hydrogen atoms bonded to the silicon atoms may be located at either the terminal or the middle of the molecular chain, or may be located at both.

[0071] Examples of the organohydrogenpolysiloxane of component (b) above include 1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethylcyclotetrasiloxane, tris(hydrogendimethylsiloxy)methylsilane, tris(hydrogendimethylsiloxy)phenylsilane, methylhydrogencyclopolysiloxane, methylhydrogensiloxane-dimethylsiloxane cyclic copolymer, methylhydrogenpolysiloxane blocked at both ends with trimethylsiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymer blocked at both ends with trimethylsiloxy groups, dimethylpolysiloxane blocked at both ends with dimethylhydrogensiloxy groups, dimethylsiloxane blocked at both ends with dimethylhydrogensiloxy groups, and dimethylsiloxane blocked at both ends with dimethylhydrogensiloxy groups. Siloxane-methylhydrogensiloxane copolymer, methylhydrogensiloxane-diphenylsiloxane copolymer with trimethylsiloxy groups at both ends, methylhydrogensiloxane-diphenylsiloxane-dimethylsiloxane copolymer with trimethylsiloxy groups at both ends, methylhydrogensiloxane-methylphenylsiloxane-dimethylsiloxane copolymer with trimethylsiloxy groups at both ends, methylhydrogensiloxane-dimethylsiloxane-diphenylsiloxane copolymer with dimethylhydrogensiloxy groups at both ends, methylhydrogensiloxane-dimethylsiloxane-methylphenylsiloxane copolymer with dimethylhydrogensiloxy groups at both ends, (CH3)2HSiO 1 / 2 Units and SiO4 / 2 A copolymer consisting of (CH3)2HSiO units. 1 / 2 Units and SiO 4 / 2 Units and (C6H5)SiO 3 / 2 and copolymers consisting of the above-mentioned exemplary compounds in which part or all of the methyl groups have been substituted with other alkyl groups, phenyl groups, or the like.

[0072] The amount of organohydrogenpolysiloxane of component (b) is 0.5 to 20 parts by mass, preferably 0.6 to 15 parts by mass, per 100 parts by mass of component (a), but it is particularly preferred that the molar ratio of alkenyl groups in component (a) to hydrosilyl groups in component (b) be hydrosilyl groups / alkenyl groups = 0.8 to 3.0, particularly 1.0 to 1.5. If this ratio is 0.8 or more and 3.0 or less, the compression set of the resulting cured rubber can be suppressed, thereby providing sufficient sealing properties.

[0073] [(c) Addition reaction catalyst] The addition reaction catalyst is a hydrosilylation catalyst for the addition reaction of the alkenyl group contained in the alkenyl group-containing organopolysiloxane of component (a) with the hydrosilyl group contained in the organohydrogenpolysiloxane of component (b). Examples of the addition reaction catalyst include the same as the above-mentioned component (C). Specifically, platinum-based catalysts such as platinum black, platinic chloride, chloroplatinic acid, reaction products of chloroplatinic acid and monohydric alcohols, complexes of chloroplatinic acid and olefins, platinum bisacetoacetate, and other platinum group metal-based catalysts, such as palladium-based catalysts and rhodium-based catalysts, are listed, and platinum-based catalysts are particularly preferred.

[0074] The amount of catalyst added may be any amount that can promote the addition reaction, and is usually preferably 0.5 to 1,000 ppm, more preferably about 1 to 500 ppm, of platinum group metal (mass equivalent) relative to component (a). If the amount is 0.5 ppm or more, the addition reaction is sufficiently promoted and curing is sufficient, and if the amount is 1,000 ppm or less, the effect on reactivity is obtained in proportion to the amount added, which is economical.

[0075] [(d) Fumed silica] The fumed silica, component (d), is essential for imparting sufficient strength to silicone rubber. The specific surface area of ​​fumed silica, as measured by the BET method, is 50 to 400 m 2 / g, preferably 100 to 350 m 2 / g. 50m 2 / g or more, acid resistance is good, and 2 If it is less than 1 / g, the compression set will be small.

[0076] These fumed silicas may be used as they are, but it is preferable to use those that have been previously treated with a surface hydrophobic treatment agent, or to use them by adding a surface treatment agent during kneading with component (a).These surface treatment agents include any of the well-known ones such as alkylalkoxysilanes, alkylchlorosilanes, alkylsilazanes, silane coupling agents, titanate-based treatment agents, and fatty acid esters, and they may be used alone or in combination of two or more kinds at the same time or at different times.

[0077] The amount of the fumed silica is 5 to 30 parts by mass, preferably 10 to 30 parts by mass, and more preferably 12 to 28 parts by mass, per 100 parts by mass of component (a). By making the amount 5 parts by mass or more, more sufficient rubber strength can be obtained, and by making it 30 parts by mass or less, compression set is small and good sealing properties can be obtained.

[0078]

[0043] The silicone rubber composition may contain, as other components as necessary, reinforcing agents such as precipitated silica and silicone resin, fillers such as quartz powder, diatomaceous earth and calcium carbonate, hydrosilylation reaction inhibitors such as nitrogen-containing compounds, acetylene compounds, phosphorus compounds, nitrile compounds, carboxylates, tin compounds, mercury compounds, sulfur compounds, ethynylcyclohexanol, heat resistance agents such as iron oxide and cerium oxide, internal release agents such as dimethyl silicone oil, adhesion imparting agents, thixotropy imparting agents, and the like.

[0079] The addition curing type silicone rubber composition can be prepared by uniformly mixing the components (a) to (d) and, if necessary, any optional components. The obtained silicone rubber composition should have a viscosity of usually 20 to 5,000 Pa·s, preferably about 30 to 1,000 Pa·s, at room temperature (25°C). The viscosity can be measured by a rotational viscometer. The molding method includes compression molding, casting molding, injection molding, etc.

[0080] The curing temperature of the above materials is usually 100 to 220°C for 10 seconds to 2 hours, and it is preferable to cure and mold the material at 120 to 200°C for about 20 seconds to 30 minutes. After the silicone rubber composition is cured and molded (i.e., after the first cure), a post cure (second cure) may be performed to improve adhesion and compression set of the cured product. The post cure conditions are usually 100 to 220°C for 30 minutes to 100 hours, and it is preferable to cure the material at 120 to 200°C for about 1 to 8 hours.

[0081] [Fuel cell separators] The present invention also provides a fuel cell separator comprising a separator substrate, a silicone rubber layer formed on one or both sides of the separator substrate, and a cured film of the coating material composition of the present invention formed on the surface of the silicone rubber layer opposite to the surface in contact with the separator substrate.

[0082] The method for producing the fuel cell separator of the present invention will be described below. The fuel cell separator of the present invention has a silicone rubber layer on one or both sides of a separator substrate, and a cured film of the coating material composition of the present invention, particularly an EPDM rubber coating material composition, is formed on the silicone rubber layer.

[0083] Metals that can be used as the separator substrate include aluminum, iron, copper, zinc, nickel, stainless steel, brass, titanium, and the like. Since acid resistance is required, corrosion-resistant materials such as stainless steel or those with modified surfaces are preferably used.

[0084] The thickness of the silicone rubber layer is usually from 50 to 5,000 μm, and preferably from about 100 to 3,000 μm.

[0085] Methods for forming a silicone rubber layer on the separator substrate include molding the silicone rubber composition into a seal shape by compression molding, casting, injection molding, or the like, and combining it with a separator, and methods for obtaining an integrated separator and seal material by screen printing, insert molding, or the like.

[0086] Methods for forming a cured film of the coating material composition of the present invention on the silicone rubber layer thus obtained include dipping, coating (brush application or spray application), screen printing, and the like.

[0087] The fuel cell separator manufactured by the above-mentioned method is particularly suitable as a separator for a solid polymer electrolyte fuel cell. It is assumed that a fluoropolymer having a sulfonic acid group is used as the electrolyte membrane of the solid polymer electrolyte fuel cell. Examples of the fluoropolymer having a sulfonic acid group include a copolymer of tetrafluoroethylene and perfluoro[2-(fluorosulfonylethoxy)propylvinylether], and examples of this copolymer include Nafion (registered trademark) manufactured by Typon Corporation. The EPDM rubber coating material composition of the present invention and the silicone rubber member coated therewith have resistance to sulfuric acid and hydrofluoric acid derived from the electrolyte membrane. EXAMPLES

[0088] The present invention will be specifically described below using examples and comparative examples, but the present invention is not limited to these.

[0089] An EPDM rubber coating composition was prepared using the components shown below.

[0090] [(A) Ethylene-α-olefin-non-conjugated polyene random copolymer] Two types of ethylene-propylene-5-vinyl-2-norbornene copolymers with different structures were prepared (EPDM-1 and EPDM-2). The average structure of EPDM-1 was ethylene:propylene=65:35 (molar ratio), vinyl group content=0.088mol / 100g, number average molecular weight=900. The average structure of EPDM-2 was ethylene:propylene=65:35 (molar ratio), vinyl group content=0.044mol / 100g, number average molecular weight=3,200.

[0091] [(B) Organosilicon compound having a hydrosilyl group] An organosilicon compound represented by the following formula (2) was prepared. [ka] (Amount of hydrosilyl groups: 0.0035 mol / g)

[0092] As comparative examples, organosilicon compounds represented by the following formulas (3) and (4) were prepared. [ka] (Amount of hydrosilyl groups: 0.0081 mol / g) [ka] (Amount of hydrosilyl groups: 0.0070 mol / g)

[0093] [(C) Addition reaction catalyst] A solution of chloroplatinic acid in 2-ethylhexanol (concentration: 5% by mass) was prepared.

[0094] [Other ingredients] Hydrosilylation reaction inhibitor: 1-ethynyl-1-cyclohexanol - Organic solvent for dilution: n-hexane

[0095] [Preparation of EPDM rubber coating composition] [Preparation Example 1] Coating material 1 was prepared by dissolving 100 g of EPDM-1 as component (A), 27 g of the organosilicon compound represented by the above formula (2) as component (B), 0.2 g of a 2-ethylhexanol solution of chloroplatinic acid (concentration: 5% by mass) as component (C) [40 ppm relative to component (A) in terms of platinum metal], and 0.4 g of 1-ethynyl-1-cyclohexanol as a hydrosilylation reaction inhibitor in 150 g of n-hexane.

[0096] [Preparation Example 2] Coating material 2 was prepared by dissolving 100 g of EPDM-2 as component (A), 23 g of the organosilicon compound represented by the above formula (2) as component (B), 0.2 g of a 2-ethylhexanol solution of chloroplatinic acid (concentration: 5% by mass) as component (C) [40 ppm relative to component (A) in terms of platinum metal], and 0.4 g of 1-ethynyl-1-cyclohexanol as a hydrosilylation reaction inhibitor in 300 g of n-hexane.

[0097] [Comparative Preparation Example 1] Coating material 3 was prepared in the same manner as in Preparation Example 1, except that 12.6 g of the organosilicon compound represented by the above formula (3) was used instead of the organosilicon compound represented by the above formula (2) described in Preparation Example 1.

[0098] [Comparative Preparation Example 2] Coating material 4 was prepared in the same manner as in Preparation Example 1, except that 14.5 g of the organosilicon compound represented by the above formula (4) was used instead of the organosilicon compound represented by the above formula (2) described in Preparation Example 1.

[0099] [Silicone rubber composition] (a1) 70 parts by mass of a dimethylpolysiloxane having both molecular chain terminals blocked with dimethylvinylsiloxy groups and a weight average degree of polymerization of 500; (d) a BET specific surface area of ​​200 m 230 parts by mass of fumed silica (Aerosil 200, manufactured by Nippon Aerosil Co., Ltd.) having a molecular weight of 1.0 to 1.2 g / g, 5 parts by mass of hexamethyldisilazane, 0.2 parts by mass of divinyltetramethyldisilazane, and 2.0 parts by mass of water were mixed at 25° C. for 30 minutes, and then the mixture was heated to 150° C. and stirred for 3 hours, followed by cooling. Further, 15 parts by mass of the (a1) dimethylpolysiloxane and 5 parts by mass of (a2) dimethylpolysiloxane having both molecular chain terminals blocked with trimethylsiloxy groups, 10 mol % of the side chain methyl groups substituted with vinyl groups, and a weight average polymerization degree of 200 were mixed therein, and the mixture was subjected to a dispersion treatment with a three-roll mill to obtain a silicone rubber base. To 100 parts by mass of this silicone rubber base, 1.3 parts by mass [hydrosilyl group / alkenyl group=1.2] of (b) methylhydrogenpolysiloxane having 18 hydrosilyl groups on its side chains as a crosslinking agent (degree of polymerization 40, hydrosilyl group amount 0.0073 mol / g) was added, and 0.05 parts by mass of ethynylcyclohexanol as a reaction inhibitor was added. Stirring was continued for 15 minutes, and then 0.1 parts by mass of (c) platinum catalyst (platinum metal equivalent concentration: 1% by mass) was mixed in to obtain a liquid silicone rubber composition.

[0100] [Preparation of cured silicone rubber] The silicone rubber composition was press molded at 120°C for 10 minutes to form a silicone rubber sheet with a thickness of 2.0 mm, which was then post-cured in an oven at 200°C for 4 hours, and then cut into a silicone rubber test piece measuring 25 mm x 50 mm.

[0101] [Examples 1 and 2, and Comparative Examples 1 to 3] [Preparation of coating sample] A silicone rubber test piece was immersed in each coating material for 10 seconds at room temperature (25°C) and then air-dried for 30 minutes (Example 1: Coating material 1, Example 2: Coating material 2, Comparative Example 1: No coating, Comparative Example 2: Coating material 3, Comparative Example 3: Coating material 4). The coating sample was then heated in an oven at 120°C for 30 minutes. The amount of coating (unit: g / m2) was calculated by dividing the weight change before and after coating by the surface area of ​​the test piece. 2 ) was calculated.

[0102] [Acid resistance test] An immersion solution with a hydrogen fluoride concentration of 2,500 ppm (by mass) was prepared by diluting 60% by mass hydrofluoric acid with pure water. The silicone rubber test pieces and coating samples prepared above were immersed in the immersion solution at 95°C for 120 hours. After the immersion test, the test pieces were thoroughly washed with pure water and dried in an oven at 120°C for 2 hours. The mass (mass reduction %) and surface condition of the test pieces before and after the immersion test were compared. Three pieces were tested under each condition to determine the change in mass, and the median value was used. The test results are shown in Table 1.

[0103] [Table 1]

[0104] In Examples 1 and 2, which used an organosilicon compound (formula (2)) in which a hydrosilyl group is bonded to other silicon atoms via a silarylene bond and has no siloxane bond, both maintained their gloss after the acid resistance test and the weight loss rate was also suppressed. In contrast, Comparative Example 1, which did not have a coating layer, showed a white appearance and a significant weight loss after the acid resistance test. In Comparative Example 2, which used an organosilicon compound (formula (3)) in which a hydrosilyl group is bonded to other silicon atoms via a siloxane bond rather than a silalkylene bond or silarylene bond, EPDM remained on the test piece after the acid resistance test, so the weight loss was suppressed, but the surface lost its gloss and became matte. In Comparative Example 3, the coating solution became cloudy and curing failure occurred due to poor compatibility with EPDM of an organosilicon compound (formula (4)) in which a hydrosilyl group is bonded to other silicon atoms via a siloxane bond.

[0105] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.

Claims

1. (A) an ethylene / α-olefin / non-conjugated polyene random copolymer comprising a random copolymer of a non-conjugated polyene, ethylene, and an α-olefin: 100 parts by mass, (B) an organosilicon compound having two or more hydrosilyl groups per molecule, the hydrosilyl groups being bonded to other silicon atoms via a silalkylene bond having 1 to 30 carbon atoms or a silarylene bond having 6 to 30 carbon atoms, and having no siloxane bonds: an amount such that the molar ratio of the addition-reactive unsaturated groups in component (A) to the hydrosilyl groups in component (B) is hydrosilyl groups / unsaturated groups = 0.5 to 5.0, (C) Addition reaction catalyst: an amount of 0.5 to 1,000 ppm in terms of metal atoms relative to the component (A) A coating material composition comprising:

2. 2. The coating material composition according to claim 1, wherein the content of the addition-reactive unsaturated group in the component (A) is 0.001 to 0.2 mol / 100 g.

3. 3. The coating material composition according to claim 1, wherein the component (A) is an ethylene-propylene-5-vinyl-2-norbornene copolymer.

4. A silicone rubber molded article having a cured film of the coating material composition according to any one of claims 1 to 3.

5. A separator for a fuel cell, 4. A fuel cell separator comprising: a separator substrate; a silicone rubber layer formed on one or both sides of the separator substrate; and a cured film of the coating material composition according to claim 1 formed on a surface of the silicone rubber layer opposite to the surface in contact with the separator substrate.

Citation Information

Patent Citations

  • Silicone rubber gasket

    JP1994093249A

  • Curable fluoropolyether rubber composition

    JP2001354764A

  • Sealing material for separator of solid polymer type fuel cell

    JP2002309092A

  • Fuel cell gasket

    JP2004055428A

  • Seal structure of fuel cell

    JP2008204819A