Dispersion liquid, composition, sealing member, light-emitting device, lighting fixture, display device
Surface-modified metal oxide particles with a specific molar ratio of methyl to hydrocarbon groups address dispersibility issues in various silicone resins, enhancing LED package brightness and transparency by ensuring uniform dispersion and light scattering.
Patent Information
- Application Number
- JP2020165846
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-30
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Existing silicone resins used for LED encapsulation face challenges in dispersing metal oxide particles due to differences in hydrophobicity and heat resistance, leading to aggregation and reduced transparency, especially when used with methyl-based silicone resins, which are required for high heat resistance and extended LED lifespan.
Surface-modified metal oxide particles are developed using a silane compound with a methyl group and a silicone compound containing a hydrocarbon group, with a specific molar ratio of methyl to hydrocarbon groups, ensuring dispersibility in both methyl-based and phenyl-based silicone resins, as measured by Fourier transform infrared spectrophotometry.
The solution allows for uniform dispersion of metal oxide particles in both types of silicone resins, enhancing light scattering and brightness while maintaining transparency, thus improving the light extraction efficiency of LED packages.
Smart Images

Figure 0007559478000002 
Figure 0007559478000003 
Figure 0007559478000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a dispersion liquid, a composition, a sealing member, a light-emitting device, a lighting fixture, and a display device, each of which contains metal oxide particles whose surfaces have been modified with a silane compound and a silicone compound. [Background technology]
[0002] Light-emitting diodes (LEDs) are widely used as light sources with advantages such as small size, long life, and low-voltage operation. The LED chip in an LED package is generally sealed with a sealing material containing resin to prevent contact with deterioration factors present in the external environment such as oxygen and moisture. Therefore, the light emitted from the LED chip passes through the sealing material and is emitted toward the outside. Therefore, in order to increase the luminous flux emitted from the LED package, it is important to efficiently extract the light emitted from the LED chip to the outside of the LED package.
[0003] As an encapsulating material for improving the extraction efficiency of light emitted from an LED chip, a composition for forming a light-scattering complex containing metal oxide particles surface-modified with a surface-modifying material containing at least one functional group selected from an alkenyl group, an H-Si group, and an alkoxy group, and a matrix resin composition is known (see, for example, Patent Document 1).
[0004] In this light-scattering complex-forming composition, a dispersion liquid containing metal oxide particles is mixed into a silicone resin while maintaining a relatively high transparency. The metal oxide particles used have a small dispersed particle size and a high refractive index. As a result, the light-scattering complex obtained by curing the light-scattering complex-forming composition has reduced deterioration in light transmittance and improved light scattering properties. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2016 / 142992 Summary of the Invention [Problem to be solved by the invention]
[0006] Silicone resins used as LED encapsulation materials generally contain methyl and phenyl groups, which are hydrocarbon groups, and the ratio of functional groups is adjusted depending on the application. For example, for lighting applications, the structure contains many phenyl groups, which have a high refractive index, to increase the amount of light extracted from the LED chip. On the other hand, for automotive applications, the structure contains many methyl groups, which have high heat resistance, to suppress the deterioration of the silicone encapsulation resin caused by high-power LEDs. For this reason, it has been necessary to design the modification of the metal oxide particle surface for each type and application of silicone sealing resin.
[0007] In addition, in recent years, there has been an increasing demand for methyl-based silicone resins that contain many methyl groups with high heat resistance in order to extend the lifespan of LEDs. Compared with phenyl-based silicone resins and the like that have been commonly used in the past, methyl-based silicone resins have a large content of methyl groups and a high degree of hydrophobicity. Therefore, as in the invention described in Patent Document 1, even if the surface of metal oxide particles is hydrophobized, when mixed with methyl-based silicone resin, there is a problem that the metal oxide particles aggregate with each other, making it impossible to obtain a transparent composition.
[0008] In order to solve the above problems, a method has been studied in which metal oxide particles are directly dispersed in a silane compound for primary modification, and then a silicone compound is used for secondary modification to obtain surface-modified metal oxide particles that can be dispersed in a methyl-based silicone resin. Hereinafter, the "surface-modified metal oxide particles" may be abbreviated to "surface-modified metal oxide particles".
[0009] However, the surface-modified metal oxide particles obtained by the above method could not be dispersed in a phenyl-based silicone resin containing many phenyl groups. Therefore, there has been a demand for surface-modified metal oxide particles that can be dispersed in both methyl-based silicone resins and phenyl-based silicone resins.
[0010] The present invention has been made in order to solve the above-mentioned problems, and has an object to provide a dispersion liquid containing surface-modified metal oxide particles that can be dispersed in either methyl-based silicone resin or phenyl-based silicone resin, a composition containing the dispersion liquid, a sealing member formed using the composition, a light-emitting device having the sealing member, and a lighting fixture and a display device including the light-emitting device. [Means for solving the problem]
[0011] In order to solve the above problems, one aspect of the present invention is a dispersion liquid containing metal oxide particles surface-modified with a silane compound and a silicone compound, and a solvent, wherein the silane compound contains a methyl group, and the silicone compound is aromatic The above-mentioned aromatic The molar ratio of the methyl groups to the hydrocarbon groups (methyl groups / aromatic Hydrocarbon group) is 0.01 or more and 10 or less, The dispersion liquid was dried in a vacuum to obtain the metal oxide particles, and the obtained particles were measured at 800 cm by a Fourier transform infrared spectrophotometer. -1 More than 3800cm -1 The present invention provides a dispersion liquid that satisfies the following formula (1) when a transmission spectrum is measured in the following wave number range and the spectral values are normalized so that the maximum value of the spectrum in the range is 100 and the minimum value is 0: IA / IB≦3.5 (1) (In the formula, "IA" is 3500 cm -1 The spectral value at 1100 cm -1 The spectral values at are shown.)
[0012] In one aspect of the present invention, The total content of the silane compound and the silicone compound relative to the metal oxide particles is 190% by mass or more and 1000% by mass or less. may be also possible.
[0013] In order to solve the above problems, one aspect of the present invention provides a composition comprising the above dispersion and a silicone resin component.
[0014] In order to solve the above problems, one aspect of the present invention provides a sealing member which is a cured product of the above composition.
[0015] In order to solve the above problem, one aspect of the present invention provides a light-emitting device including the above-mentioned sealing member and a light-emitting element sealed by the sealing member.
[0016] In order to solve the above problem, one aspect of the present invention provides a lighting fixture including the above light-emitting device.
[0017] In order to solve the above problem, one aspect of the present invention provides a display device including the above light-emitting device. Effect of the Invention
[0018] According to the present invention, it is possible to provide a dispersion liquid containing surface-modified metal oxide particles that can be dispersed in either a methyl-based silicone resin or a phenyl-based silicone resin, a composition containing the dispersion liquid, a sealing member formed using the composition, a light-emitting device having the sealing member, and a lighting fixture and a display device including the light-emitting device. [Brief description of the drawings]
[0019] [Figure 1] 1 is a schematic diagram illustrating an example of a light emitting device according to an embodiment of the present invention. [Diagram 2] FIG. 4 is a schematic diagram showing another example of a light emitting device according to an embodiment of the present invention. [Diagram 3] FIG. 4 is a schematic diagram showing another example of a light emitting device according to an embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram showing another example of a light emitting device according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The following describes embodiments of the dispersion of the present invention, a composition containing the dispersion, a sealing member formed using the composition, a light-emitting device having the sealing member, and a lighting fixture and a display device including the light-emitting device. It should be noted that the present embodiment is specifically described to allow a better understanding of the gist of the invention, and does not limit the present invention unless otherwise specified.
[0021] <1. Idea of the inventors> First, prior to a detailed description of the present invention, the idea behind the present inventors will be described.
[0022] In general, in the manufacture of a sealing material (composition) that is a raw material for a sealing member, metal oxide particles are modified with a surface modification material and dispersed in a resin such as a silicone resin. However, compared with the phenyl-based silicone resin that has been commonly used in the past, the methyl-based silicone resin has a large methyl group content and a high degree of hydrophobicity. Therefore, even when modified with a surface modification material as described above, it has been difficult to uniformly disperse the metal oxide particles in the methyl-based silicone resin.
[0023] Therefore, the present inventors conducted extensive research to solve this problem and discovered that simply increasing the amount of surface modification material used does not significantly improve the dispersibility of metal oxide particles in methyl-based silicone resin.
[0024] Based on this result, the present inventors conducted further studies and focused on the modification state of the surface modification material on the surface of the metal oxide particles. That is, even if the metal oxide particles are modified using a large amount of the surface modification material, if only a small amount of the surface modification material is attached to the surface of the metal oxide particles, the surface of the metal oxide particles is not sufficiently hydrophobic. On the other hand, even if the metal oxide particles are modified using a small amount of the surface modification material, if the adhesion ratio of the surface modification material to the surface of the metal oxide particles is high and a large amount of the surface modification material is attached to the surface of the metal oxide particles, the surface of the metal oxide particles is sufficiently hydrophobic.
[0025] The present inventors have found that when a silane compound or a silicone compound is used as the surface modification material, the degree of adhesion of the surface modification material to the metal oxide particles can be measured and observed by a Fourier transform infrared spectrophotometer (FT-IR). The inventors have found that if the metal oxide particles are surface-modified with a silane compound and a silicone compound by the method described below, the metal oxide particles can be dispersed in a methyl-based silicone resin, which has been difficult to disperse in the past. Furthermore, the inventors have found that by surface-modifying the metal oxide particles with a silane compound containing a methyl group and a silicone compound containing a hydrocarbon group having a carbon number of 2 or more, at a molar ratio of the methyl group to the hydrocarbon group of 0.01 to 10, it is possible to obtain surface-modified metal oxide particles that can be dispersed in both methyl-based silicone resins and phenyl-based silicone resins.
[0026] <2.Dispersion> The dispersion liquid according to this embodiment will be described. The dispersion liquid according to this embodiment contains metal oxide particles surface-modified with a silane compound and a silicone compound, and a solvent, wherein the silane compound contains a methyl group, the silicone compound contains a hydrocarbon group having two or more carbon atoms, and the ratio of the methyl group to the hydrocarbon group (methyl group / hydrocarbon group) is 0.01 or more and 10 or less. In this embodiment, the metal oxide particles obtained by drying the dispersion liquid by vacuum drying are measured for a wavelength of 800 cm using a Fourier transform infrared spectrophotometer. -1 More than 3800cm -1 When the transmission spectrum is measured in the following wave number range and the spectrum values are normalized so that the maximum value of the spectrum in that range is 100 and the minimum value is 0, the following formula (1) is satisfied. IA / IB≦3.5 (1) (In the formula, "IA" is 3500 cm -1 The spectrum value, "IB", is 1100c m -1 The spectral values at are shown.) By satisfying the above conditions, the dispersion liquid according to this embodiment can disperse in both methyl-based silicone resins and phenyl-based silicone resins.
[0027] To explain in detail, in the transmission spectrum measured by a Fourier transform infrared spectrophotometer, -1 The position is attributed to a siloxane bond (Si-O-Si bond) and has a wave number of 3500 cm -1 The position of is attributed to a silanol group (Si-OH group). Silane compounds and silicone compounds contain Si-OH groups capable of forming Si-O-Si bonds and groups capable of forming Si-OH groups, respectively. Therefore, -1 Spectral values at (IA) and 1100cm -1 By comparing the spectral value (IB) at 0.05 with that at 0.15, it is possible to observe the reaction degree of Si-OH of the silane compound and silicone compound, and groups capable of forming Si-OH groups.
[0028] The present inventors have found that when the IA / IB ratio is 3.5 or less, the silane compound is sufficiently attached to the surface of the metal oxide particles, which allows the metal oxide particles to be dispersed in the methyl-based silicone resin without agglomeration when mixed with the methyl-based silicone resin.
[0029] On the other hand, when IA / IB exceeds 3.5, silane compound and silicone compound are not sufficiently attached to the surface of metal oxide particles, and the dispersibility of metal oxide particles in methyl-based silicone resin cannot be excellent.As a result, when the dispersion liquid is mixed with methyl-based silicone resin, the aggregation of metal oxide particles occurs, and the obtained composition becomes turbid.As mentioned above, IA / IB is 3.5 or less, but it is preferably 3.0 or less, more preferably 2.5 or less, and even more preferably 2.0 or less.
[0030] Moreover, since IA=0 is preferable, the lower limit of IA / IB is 0. However, since even if a small amount of silanol groups (Si-OH groups) remain, it can be mixed into a methyl-based silicone resin, the lower limit of IA / IB may be 0, 0.1, 0.5, 1.0, or 1.5.
[0031] Specifically, the measurement of the transmission spectrum of metal oxide particles using a Fourier transform infrared spectrophotometer (FT-IR) can be carried out as follows. The dispersion of this embodiment is dried by vacuum drying. The drying conditions may be adjusted appropriately depending on the amount and concentration of the dispersion. For example, 10 g of a dispersion with a solid content of 30 mass % may be dried at 100°C and 20 hPa or less for 2 hours or more. As a vacuum dryer, VACUUM OVEN VOS-201SD manufactured by EYELA Tokyo Rikakikai Co., Ltd. may be used. Next, 0.01 g to 0.05 g of the metal oxide particles obtained by drying can be used for measurement with a Fourier transform infrared spectrophotometer (for example, manufactured by JASCO Corporation, model number: FT / IR-670 Plus).
[0032] However, it was difficult to disperse surface-modified metal oxide particles with an IA / IB ratio of 3.5 or less in phenyl-based silicone resins. Therefore, the present inventors conducted further studies and found that by performing surface modification so that the molar ratio of the methyl groups to the hydrocarbon groups is 0.01 or more and 10 or less, it is possible to obtain surface-modified metal oxide particles that are dispersible in both methyl-based silicone resins and phenyl-based silicone resins. In order to disperse in methyl-based silicone resin, surface modification in a silane compound containing a methyl group is essential. Metal oxide particles surface-modified in this way have poor affinity with the phenyl group contained in silicone resin for LEDs. Silicone compounds have a higher affinity for silicone resin than silane compounds. Therefore, it is speculated that by treating the surface with a silicone compound containing a hydrocarbon group with two or more carbon atoms, which has a higher affinity for phenyl groups than methyl groups, it is possible to obtain highly versatile surface-modified metal oxide particles that can be dispersed in both methyl-based silicone resin and phenyl-based silicone resin.
[0033] The present inventors had thought that surface-modified metal oxide particles that can be dispersed in methyl-based silicone resins have high affinity with methyl groups, and therefore would be difficult to disperse in phenyl-based silicone resins. Therefore, the result that highly versatile surface-modified metal oxide particles that can be dispersed in both methyl-based silicone resins and phenyl-based silicone resins can be obtained by adjusting the molar ratio of methyl groups and hydrocarbon groups having two or more carbon atoms was unexpected.
[0034] In this embodiment, the molar ratio of the methyl groups to the hydrocarbon groups (methyl groups / hydrocarbon groups) is 0.01 or more and 10 or less, preferably 0.03 or more and 8 or less, more preferably 0.05 or more and 5 or less, and even more preferably 0.1 or more and 3 or less. By setting the molar ratio to 0.01 or more and 10 or less, it becomes possible to disperse metal oxide particles transparently in either methyl-based silicone resin or phenyl-based silicone resin. If the molar ratio of methyl groups / hydrocarbon groups is less than 0.01, the number of methyl groups is too small to disperse the metal oxide particles in the methyl-based silicone resin. On the other hand, if the molar ratio of methyl groups / hydrocarbon groups is more than 10, the metal oxide particles cannot be dispersed in the phenyl-based silicone resin.
[0035] The molar ratio of methyl groups to hydrocarbon groups having 2 or more carbon atoms means a value measured by the following method using NMR (nuclear magnetic resonance spectroscopy). That is, it means the molar ratio of methyl groups contained in the surface-modified metal oxide particles to hydrocarbon groups having 2 or more carbon atoms. Therefore, it essentially means the molar ratio of methyl groups contained in the silane compound and silicone compound to hydrocarbon groups having 2 or more carbon atoms. 15 g of the dispersion liquid adjusted to a solid content of 30% by mass is mixed with 15 g of methanol to precipitate the surface-modified metal oxide particles. This mixture is subjected to solid-liquid separation using a centrifuge, and the solid portion (surface-modified metal oxide particles) is collected. Several milligrams of the collected surface-modified metal oxide particles are taken and dissolved in deuterated chloroform to a concentration of 1% by mass. Using this dissolving solution, a benchtop NMR device (manufactured by Nanalysis, model number NMReady60Pro ( 1 H / 19 F)) to separate hydrocarbon groups with two or more carbon atoms and methyl groups. 1 Measure the H-liquid NMR spectrum. From the spectrum obtained, calculate the spectral area (integral value) of the hydrocarbon groups with two or more carbon atoms and the methyl groups, and calculate the integral value of the methyl groups / integral value of the hydrocarbon groups with two or more carbon atoms. This makes it possible to calculate the molar ratio of methyl groups to hydrocarbon groups with two or more carbon atoms. The solid content of the dispersion does not need to be 30% by mass, and it is sufficient that the amount required for NMR measurement is collected.
[0036] (2.1 Metal oxide particles) The metal oxide particles scatter the light emitted from the light emitting element in the sealing member described below. In addition, depending on the type of metal oxide particles, the metal oxide particles improve the refractive index of the sealing member. As a result, the metal oxide particles contribute to improving the brightness of the light in the light emitting device.
[0037] The metal oxide particles are not particularly limited. In the present embodiment, examples of the metal oxide particles include zirconium oxide particles, titanium oxide particles, zinc oxide particles, iron oxide particles, copper oxide particles, tin oxide particles, cerium oxide particles, tantalum oxide particles, niobium oxide particles, tungsten oxide particles, europium oxide particles, yttrium oxide particles, molybdenum oxide particles, indium oxide particles, antimony oxide particles, germanium oxide particles, zinc oxide particles, bismuth oxide particles, and hafnium oxide particles, as well as potassium titanate particles, barium titanate particles, strontium titanate particles, potassium niobate particles, lithium niobate particles, calcium tungstate particles, and the like. Preferably used are metal oxide particles including at least one selected from the group consisting of sodium particles, yttria-stabilized zirconia particles, alumina-stabilized zirconia particles, calcia-stabilized zirconia particles, magnesia-stabilized zirconia particles, scandia-stabilized zirconia particles, hafnia-stabilized zirconia particles, ytterbia-stabilized zirconia particles, ceria-stabilized zirconia particles, indium-stabilized zirconia particles, strontium-stabilized zirconia particles, samarium oxide-stabilized zirconia particles, gadolinium oxide-stabilized zirconia particles, antimony-doped tin oxide particles, and indium-doped tin oxide particles.
[0038] Among the above, from the viewpoint of improving transparency and compatibility (affinity) with the encapsulating resin (resin component), it is preferable that the metal oxide particles be at least one type selected from the group consisting of zirconium oxide particles and titanium oxide particles. Moreover, from the viewpoint of improving the refractive index of the sealing member, the metal oxide particles preferably have a refractive index of 1.7 or more.
[0039] The metal oxide particles are more preferably at least one of zirconium oxide particles and titanium oxide particles, and particularly preferably zirconium oxide particles.
[0040] The average primary particle size of the metal oxide particles is preferably 1 nm or more and 200 nm or less, more preferably 3 nm or more and 150 nm or less, and even more preferably 10 nm or more and 100 nm or less. By having the average primary particle size of the metal oxide particles in the above range, it is possible to suppress a decrease in the transparency of the sealing member. As a result, the brightness of the light from the light emitting device can be further improved.
[0041] The average primary particle size of metal oxide particles can be measured, for example, by observation with a transmission electron microscope. First, inorganic oxide particles are observed with a transmission electron microscope to obtain a transmission electron microscope image. Next, a predetermined number of inorganic oxide particles, for example, 100 particles, are selected from the transmission electron microscope image. The longest straight line segment (maximum major axis) of each of these inorganic oxide particles is then measured, and the arithmetic average of these measured values is calculated.
[0042] Here, when the metal oxide particles are aggregated, the aggregate particle size of the aggregate is not measured.The maximum major axis of a predetermined number of metal oxide particles (primary particles) constituting the aggregate is measured and used as the average primary particle size.
[0043] The average dispersed particle diameter of the metal oxide particles in the dispersion of the present embodiment is not particularly limited, but is, for example, 10 nm or more and 300 nm or less, preferably 20 nm or more and 250 nm or less, and more preferably 30 nm or more and 200 nm or less. When the average dispersed particle diameter of the metal oxide particles is 10 nm or more, the brightness of the light of the light-emitting device to be described later, which is manufactured using this dispersion, is improved. In addition, when the average dispersed particle diameter of the metal oxide particles is 300 nm or less, the decrease in the light transmittance of the dispersion, the composition to be described later, and the sealing member to be manufactured using this can be suppressed. As a result, the brightness of the light of the light-emitting device is improved.
[0044] The average dispersed particle size of the metal oxide particles can be the particle size D50 of the metal oxide particles when the cumulative percentage of the scattering intensity distribution obtained by the dynamic light scattering method is 50%, and can be measured by a dynamic light scattering particle size distribution meter (for example, HORIBA, model number: SZ-100SP). The measurement can be performed using a quartz cell with an optical path length of 10 mm x 10 mm for a dispersion liquid adjusted to a solid content of 5 mass%. In this specification, the "solid content" refers to the residue when the volatile components in the dispersion liquid are removed. For example, when 1.2 g of the dispersion liquid is placed in a magnetic crucible and heated on a hot plate at 150°C for 1 hour, the components that remain without volatilization (metal oxide particles, surface modification materials, etc.) can be regarded as the solid content.
[0045] The average dispersed particle diameter of the metal oxide particles is measured and calculated based on the diameter of the dispersed metal oxide particles, regardless of whether the metal oxide particles are dispersed as primary particles or secondary particles. In the present embodiment, the average dispersed particle diameter of the metal oxide particles may be measured as the average dispersed particle diameter of the metal oxide particles to which a surface modification material is attached. In the dispersion liquid, there may be metal oxide particles to which a surface modification material is attached and metal oxide particles to which no surface modification material is attached. Therefore, the average dispersed particle diameter of the metal oxide particles is usually measured as a value in a mixed state of these.
[0046] The metal oxide particles described above have a surface modification material, which will be described below, attached to their surfaces, which allows the metal oxide particles to be stably dispersed in a dispersion liquid and a composition produced using the metal oxide particles.
[0047] (2.2 Silane Compounds) In the surface-modified metal oxide particles according to this embodiment, the metal oxide particles are surface-modified with a silane compound containing a methyl group. In the present embodiment, the silane compound may be used in combination with a silane compound containing a methyl group and a silane compound containing a hydrocarbon group having 2 or more carbon atoms, as long as the ratio of methyl group / hydrocarbon group is within a predetermined range. Also, a silane compound containing a functional group other than a methyl group or a hydrocarbon group having 2 or more carbon atoms may be used in combination.
[0048] From the viewpoint of attaching more silane compounds to the metal oxide particles, in this embodiment, it is essential to modify the surfaces of the metal oxide particles with a silane compound containing a methyl group. However, if the silane compound containing a methyl group is sufficiently attached to the surfaces of the metal oxide particles, the subsequent surface modification is not particularly limited as long as it does not inhibit the compatibility with the silicone resin or enhances the compatibility. Silicone resins for LEDs generally contain methyl and phenyl groups, which are hydrocarbon groups, as functional groups. Therefore, the silane compound of this embodiment may be subjected to primary modification and secondary modification with a silane compound containing a methyl group, or may be subjected to primary modification with a silane compound containing a methyl group and then secondary modification with a hydrocarbon group having 2 or more carbon atoms. From the viewpoint of improving the compatibility with the phenyl group in the silicone resin for LEDs and improving the stability of the dispersion, it is preferable that the surfaces of the metal oxide particles are modified with a silane compound containing a methyl group and a silane compound containing a hydrocarbon group having 2 or more carbon atoms. Therefore, in this embodiment, it is preferable that the silane compound contains a methyl group and a hydrocarbon group having 2 or more carbon atoms.
[0049] These silane compounds, at least a part of which adheres to the surface of metal oxide particles, modify the surface, thereby preventing the aggregation of the metal oxide particles, and further improve the compatibility with silicone resin components for LEDs, in other words, silicone resin components containing methyl groups and phenyl groups.
[0050] Here, the term "attachment" of a silane compound to a metal oxide particle means that the silane compound comes into contact with or bonds to the metal oxide particle through an interaction or reaction between them. Examples of the contact include physical adsorption. Examples of the bond include ionic bonds, hydrogen bonds, covalent bonds, etc.
[0051] The silane compound containing a methyl group is not particularly limited as long as it can be attached to the surface of metal oxide particles. As the silane compound containing a methyl group, a silane compound containing a methyl group and an alkoxy group, a silane compound containing a methyl group and an H-Si group, or a silane compound containing a methyl group, an alkoxy group, and an H-Si group can be used. The silane compound containing a methyl group may be used alone or in combination of two or more. Of the silane compounds containing a methyl group, those containing an alkoxy group, particularly a methoxy group, are preferred because they are easily attached to metal oxide particles.
[0052] As the silane compound containing a methyl group and an alkoxy group, for example, at least one selected from the group consisting of methyltrimethoxysilane, methyltriethoxysilane, methyltripoxysilane, methylphenyldimethoxysilane, methylphenyldiethoxysilane, trimethylmethoxysilane, trimethylethoxysilane, methoxydimethyl(phenyl)silane, ethoxydimethyl(phenyl)silane, dimethyl(methoxy)phenylsilane, and dimethyl(ethoxy)phenylsilane can be used. As the silane compound containing a methyl group and an H-Si group, at least one selected from the group consisting of dimethylchlorosilane, methyldichlorosilane, and methylphenylchlorosilane can be used. As the silane compound containing a methyl group, an alkoxy group, and an H-Si group, for example, diethoxymethylsilane or ethoxydimethylsilane can be used.
[0053] Among the above, silane compounds containing a methyl group are preferable because they have a low viscosity and facilitate the dispersion of metal oxide particles in the dispersion step described below. The number of alkoxy groups in such a silane compound containing a methyl group and an alkoxy group is preferably 1 or more and 3 or less, and more preferably 3. The number of carbon atoms in the alkoxy group is preferably 1 or more and 5 or less. The number of methyl groups in the silane compound containing a methyl group and an alkoxy group is preferably 1 or more and 3 or less, and more preferably 1. The total number of alkoxy groups and methyl groups in the silane compound containing an alkyl group and an alkoxy group is 2 or more and 4 or less, and is preferably 4. The silane compound containing such a methyl group includes, for example, at least one selected from the group consisting of methyltrimethoxysilane, methyltriethoxysilane, and methyltrippropoxysilane. From the viewpoint of easy adhesion to the surface of metal oxide particles, methyltrimethoxysilane is preferred, methyltriethoxysilane is preferred, and methyltrimethoxysilane is more preferred.
[0054] The hydrocarbon group having 2 or more carbon atoms is not particularly limited as long as it is compatible with the silicone resin for LEDs. For example, it may be an aliphatic hydrocarbon group having 2 or more carbon atoms, or an aromatic hydrocarbon group. The number of carbon atoms in the hydrocarbon group may be appropriately selected depending on the type of functional group contained in the silicone resin for LEDs. Considering that silicone resin for LEDs usually contains methyl groups and phenyl groups, the number of carbon atoms is preferably 2 to 20, more preferably 3 to 16, even more preferably 4 to 12, and even more preferably 5 to 9.
[0055] The aliphatic hydrocarbon group may be an alkyl group, an alkenyl group, or an alkynyl group. It may be a chain aliphatic hydrocarbon group or a cyclic aliphatic hydrocarbon group. The alkyl group may be, for example, an ethyl group, a propyl group, a butyl group, a pentyl group, or a hexyl group. The alkenyl group may be, for example, a vinyl group, an allyl group, a propenyl group, or a butenyl group. The alkynyl group may be, for example, an ethynyl group, a propynyl group, or a butynyl group.
[0056] The aromatic hydrocarbon group may be an aryl group or an aralkyl group. As the aryl group, for example, a phenyl group, a tolyl group, a xylyl group, a biphenyl group, a 1-naphthyl group, a 2-naphthyl group, a phenanthryl group, etc. can be used. As the aralkyl group, for example, a trityl group, a benzyl group, a phenylethyl group, a phenylpropyl group, a styryl group, a benzylidene group, etc. can be used.
[0057] Among the above, from the viewpoint of excellent compatibility with silicone resins for LEDs, the hydrocarbon group having 2 or more carbon atoms is preferably a phenyl group or a xylyl group, and more preferably a phenyl group.
[0058] As the silane compound containing a hydrocarbon group having two or more carbon atoms, for example, at least one selected from the group consisting of phenyltrimethoxysilane, phenyltriethoxysilane, methylphenylchlorosilane, diphenylchlorosilane, phenyldichlorosilane, methylphenyldimethoxysilane, diphenylmonomethoxysilane, methylphenyldiethoxysilane, and diphenylmonoethoxysilane can be used. Among these, it is preferable to use phenyltrimethoxysilane, since it is easy to adjust the compatibility with the silicone resin for LED.
[0059] The content of the silane compound in the dispersion is not particularly limited, but is preferably 50% by mass or more and 700% by mass or less, more preferably 70% by mass or more and 600% by mass or less, and even more preferably 90% by mass or more and 500% by mass or less, relative to the metal oxide particles. This allows the silane compound to be densely attached to the surfaces of the metal oxide particles, improving the dispersion stability of the metal oxide particles and improving the dispersibility in methyl-based silicone resins and phenyl-based silicone resins.
[0060] (2.3 Silicone Compounds) Silicone compounds containing a hydrocarbon group having 2 or more carbon atoms have a relatively large molecular weight, and contribute to improving the affinity with the silicone resin component described later. The silicone compound is present in the vicinity of the surface of the metal oxide particles surface-modified with the silane compound. The silicone compound also plays a role of mediating between the metal oxide particles surface-modified with the silane compound and the silicone resin component described later. Therefore, the silicone compound is not particularly limited as long as it contains a hydrocarbon group having 2 or more carbon atoms and is compatible with the metal oxide particles surface-modified with the silane compound and the silicone resin component.
[0061] The silicone compound only needs to be present between the metal oxide particles surface-modified with the silane compound and the silicone resin component, and therefore only needs to be present in the vicinity of the surface of the metal oxide particles surface-modified with the silane compound, and may or may not be attached to the metal oxide particles surface-modified with the silane compound. In other words, in this embodiment, "surface modified with a silane compound and a silicone compound" means that the silane compound is attached to a metal oxide particle, and the silicone compound is present in the vicinity of the surface of the metal oxide particle to which the silane compound is attached.
[0062] Since the silicone resin for LED contains a methyl group and a phenyl group, the silicone compound of this embodiment may contain a methyl group in addition to the hydrocarbon group having 2 or more carbon atoms. The hydrocarbon group having 2 or more carbon atoms may be the same as that described for the silane compound. The silicone compound of the present embodiment may be used in combination with a silicone compound that does not contain a hydrocarbon group having two or more carbon atoms and that contains a methyl group.
[0063] Examples of silicone compounds containing a hydrocarbon group having two or more carbon atoms include alkoxy group-containing phenyl silicone, methylphenyl silicone, methylphenyl hydrogen silicone, diphenyl hydrogen silicone, alkoxy-terminated phenyl silicone, alkoxy-terminated methylphenyl silicone, alkoxy-terminated methylphenyl silicone, alkoxy group-containing phenyl silicone, etc. These silicone compounds may be used alone or in combination of two or more.
[0064] Examples of silicone compounds containing a methyl group and not containing a hydrocarbon group having two or more carbon atoms include dimethyl silicone, methyl hydrogen silicone, alkoxy group-containing dimethyl silicone, alkoxy one-terminated trimethyl one-terminated (methyl group one-terminated) dimethyl silicone, etc. These silicone compounds may be used alone or in combination of two or more.
[0065] The silicone compound may be a monomer, an oligomer, or a resin (polymer). It is preferable to use a monomer or an oligomer because it is easy to modify the surface.
[0066] Among the above, from the viewpoints of ease of reaction and high hydrophobicity, the silicone compound containing a hydrocarbon group having two or more carbon atoms preferably includes at least one selected from the group consisting of alkoxy group-containing phenylsilicone, methylphenylsilicone, phenylsilicone having alkoxy at both ends, methylphenylsilicone having alkoxy at both ends, alkoxy group-containing methylphenylsilicone, and alkoxy group-containing phenylsilicone, and more preferably includes methoxy group-containing phenylsilicone. From the viewpoint of ease of reaction, the silicone compound containing a methyl group and not containing a hydrocarbon group having two or more carbon atoms preferably contains dimethyl silicone, alkoxy group-containing dimethyl silicone, alkoxy one-terminated trimethyl one-terminated (methyl group one-terminated) dimethyl silicone, and more preferably contains at least one selected from the group consisting of dimethyl silicone and methoxy group-containing dimethyl silicone.
[0067] The content of the silicone compound in the dispersion is not particularly limited, but is preferably 10% by mass or more and 500% by mass or less, more preferably 15% by mass or more and 400% by mass or less, and even more preferably 100% by mass or more and 300% by mass or less, based on the metal oxide particles. This allows a sufficient amount of silicone compound to be attached to the surface of the metal oxide particles, improving the dispersion stability of the metal oxide particles and improving the dispersibility in the methyl-based silicone resin. Furthermore, the amount of free silicone compound can be reduced, and the unintended aggregation of the metal oxide particles in the methyl-based silicone resin and the phenyl-based silicone resin can be suppressed.
[0068] The dispersion may also contain, as a surface modification material, a general surface modification material other than the above-mentioned silane compound and silicone compound, a dispersant, and the like.
[0069] The total content of the silane compound and the silicone compound relative to the metal oxide particles is not particularly limited, and is preferably 100% by mass or more and 1000% by mass or less, more preferably 150% by mass or more and 800% by mass or less, and even more preferably 190% by mass or more and 600% by mass or less. When the total amount of the silane compound and the silicone compound is within the above-mentioned range, the dispersibility of the metal oxide particles can be sufficiently improved while reducing the amount of the free silane compound and the silicone compound.
[0070] (2.4 Solvent) The dispersion liquid according to the present embodiment contains a solvent as a dispersion medium for dispersing the metal oxide particles. The solvent is not particularly limited as long as it can disperse the metal oxide particles to which the silane compound is attached and can be mixed with the silicone resin component described later, but a hydrophobic solvent is preferred. Examples of such hydrophobic solvents include aromatics, saturated hydrocarbons, unsaturated hydrocarbons, etc. These hydrophobic solvents may be used alone or in combination of two or more.
[0071] Among the above, the hydrophobic solvent is preferably an aromatic, particularly an aromatic hydrocarbon, which has excellent compatibility with the silicone resin for LEDs, and contributes to improving the viscosity characteristics of the resulting composition and the quality (transparency, shape, etc.) of the formed sealing member.
[0072] Examples of such aromatic hydrocarbons include benzene, toluene, ethylbenzene, 1-phenylpropane, isopropylbenzene, n-butylbenzene, tert-butylbenzene, sec-butylbenzene, o-xylene, m-xylene, p-xylene, 2-ethyltoluene, 3-ethyltoluene, 4-ethyltoluene, etc. These aromatic hydrocarbons may be used alone or in combination of two or more.
[0073] Among the above, from the viewpoints of the stability of the dispersion liquid and ease of handling in removing the hydrophobic solvent medium during the production of the composition described below, the hydrophobic solvent is preferably at least one selected from the group consisting of toluene, o-xylene, m-xylene, p-xylene, and benzene, and more preferably toluene.
[0074] The content of the solvent contained in the dispersion liquid may be appropriately adjusted to obtain a desired solid content. The content of the solvent is, for example, preferably 40% by mass or more and 95% by mass or less, more preferably 50% by mass or more and 90% by mass or less, and even more preferably 60% by mass or more and 80% by mass or less. This makes it easier to mix the dispersion liquid with the resin component described later, particularly the silicone resin for LEDs.
[0075] The dispersion of the present embodiment may contain a hydrophilic solvent. The hydrophilic solvent may be contained in the dispersion due to, for example, a method described later. Examples of such hydrophilic solvents include alcohol-based solvents, ketone-based solvents, and nitrile-based solvents. These hydrophilic solvents may be used alone or in combination of two or more.
[0076] Examples of the alcohol-based solvent include branched or linear alcohol compounds having 1 to 4 carbon atoms and ether condensates thereof. These alcohol-based solvents may be used alone or in combination of two or more. The alcohol compound contained in the alcohol-based solvent may be any of primary alcohol, secondary alcohol, and tertiary alcohol. The alcohol compound contained in the alcohol-based solvent may be any of monohydric alcohol, dihydric alcohol, and trihydric alcohol. More specifically, examples of alcohol-based solvents include methanol, ethanol, 1-propanol, isopropyl alcohol, 1-butyl alcohol, 2-butanol, isobutyl alcohol, tert-butyl alcohol, methanediol, 1,2-ethanediol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 2-butene-1,4-diol, 1,4-butynediol, glycerin, diethylene glycol, and 3-methoxy-1,2-propanediol.
[0077] Examples of the ketone solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone. An example of the nitrile solvent is acetonitrile.
[0078] From the viewpoint of having excellent affinity with both water and hydrophobic solvents and promoting miscibility between them, the hydrophilic solvent preferably includes an alcohol-based solvent. In this case, the number of carbon atoms in the alcohol compound constituting the alcohol-based solvent is preferably 1 or more and 3 or less, more preferably 1 or more and 2 or less. Among the above, methanol and ethanol, particularly methanol, can be preferably used since it can fully exert the effect of the alcohol solvent.
[0079] The content of the hydrophilic solvent in the dispersion is, for example, preferably 10% by mass or less, more preferably 7% by mass or less, further preferably 5% by mass or less, and particularly preferably 3% by mass or less. The content of the hydrophilic solvent may be 0% by mass.
[0080] (2.5 Other Ingredients) The dispersion according to the present embodiment may contain components other than those described above. For example, the dispersion according to the present embodiment may contain components other than those described above as necessary, such as general additives such as dispersants, dispersion aids, antioxidants, flow regulators, thickeners, pH adjusters, and preservatives. The dispersion liquid according to the present embodiment may also contain components that may be contained due to the method described below, such as an acid, water, and alcohol.
[0081] In this specification, the dispersion according to the present embodiment is distinguished from the composition according to the present embodiment that contains a resin component and can form a sealing member by curing. That is, the dispersion according to the present embodiment does not contain the resin component described later to such an extent that a sealing member can be formed even by simply curing. More specifically, the mass ratio of the resin component to the metal oxide particles in the dispersion according to the present embodiment is preferably in the range of 0:100 to 40:60, more preferably in the range of 0:100 to 20:80, in terms of resin component:inorganic oxide particles. More preferably, the dispersion according to the present embodiment does not essentially contain the resin component described later, and particularly preferably does not completely contain the resin component described later.
[0082] The dispersion according to the present embodiment is a dispersion containing metal oxide particles surface-modified by a specific silane compound and a solvent, and satisfies the above formula (1), so it can be dispersed in both methyl-based silicone resin and phenyl-based silicone resin. Therefore, even when the dispersion according to the present embodiment is dispersed in both methyl-based silicone resin and phenyl-based silicone resin, the occurrence of turbidity such as white turbidity is suppressed. Furthermore, the viscosity change of the silicone resin for LED containing the surface-modified metal oxide particles is also suppressed.
[0083] <3. Method for producing dispersion liquid> Next, a method for producing the dispersion liquid according to this embodiment will be described.
[0084] The method for producing a dispersion liquid according to this embodiment includes a step B of mixing a silane compound containing a methyl group with metal oxide particles to obtain a mixed liquid, a step C of dispersing the metal oxide particles in the mixed liquid to obtain a dispersion liquid (first dispersion liquid), and a step F of adding a silicone compound containing a hydrocarbon group having two or more carbon atoms to the dispersion liquid containing the metal oxide particles to obtain a dispersion liquid (third dispersion liquid).
[0085] The total content of the silane compound containing a methyl group, the silicone compound containing a hydrocarbon group having two or more carbon atoms, and the metal oxide particles can also be evaluated based on the solid content. In addition, the total content of the silane compound containing a methyl group, the silicone compound containing a hydrocarbon group having a carbon number of 2 or more, and the metal oxide particles does not include the alcohol generated by hydrolysis of the silane compound described below. That is, the total content of the silane compound containing a methyl group, the silicone compound containing a hydrocarbon group having a carbon number of 2 or more, and the metal oxide particles means the total content of the silane compound, the hydrolyzed silane compound, the silicone compound, and the metal oxide particles. It goes without saying that the total content is a value including the content of the metal oxide particles surface-modified with the silane compound containing a methyl group and the silicone compound containing a hydrocarbon group having a carbon number of 2 or more.
[0086] Furthermore, in this embodiment, prior to the above-mentioned step B, a step A (hydrolysis step) may be included in which a silane compound containing a methyl group is mixed with water to obtain a hydrolyzed liquid containing a hydrolyzed silane compound containing a methyl group. In addition, when the metal oxide particles are surface-modified with a silane compound containing a hydrocarbon group having two or more carbon atoms, the silane compound containing a hydrocarbon group having two or more carbon atoms may also have a step A (hydrolysis step) for obtaining a hydrolyzed liquid, like the silane compound containing a methyl group. Each step will be described in detail below.
[0087] (Step A (First Hydrolysis Step)) In the first hydrolysis step, the silane compound containing a methyl group is mixed with water to obtain a hydrolysis liquid containing the hydrolyzed silane compound containing a methyl group. By using the mixture in which at least a part of the silane compound containing a methyl group is hydrolyzed in advance, the silane compound containing a methyl group is easily attached to the metal oxide particles in the dispersion step C described below.
[0088] The content of the methyl group-containing silane compound in the hydrolyzed liquid is not particularly limited and can be the remainder of other components in the hydrolyzed liquid. For example, the content is preferably from 60% by mass to 99% by mass, more preferably from 70% by mass to 97% by mass, and even more preferably from 80% by mass to 95% by mass.
[0089] In the first hydrolysis step, a surface modification material other than the silane compound containing a methyl group may be contained in the hydrolysis liquid.
[0090] In the first hydrolysis step, the hydrolysis liquid contains water, which serves as a substrate for the hydrolysis reaction of the surface modification material, such as a silane compound containing a methyl group. The content of water in the hydrolysis liquid is not particularly limited, and can be appropriately set according to the amount of the silane compound containing a methyl group. For example, the amount of water added to the hydrolysis liquid is preferably 0.5 mol to 5 mol, more preferably 0.6 mol to 3 mol, and even more preferably 0.7 mol to 2 mol, per mol of the silane compound containing a methyl group. This allows the hydrolysis reaction of the silane compound containing a methyl group to proceed sufficiently, while more reliably preventing the aggregation of inorganic oxide particles in the dispersion liquid produced with an excess amount of water.
[0091] Alternatively, the water content in the hydrolyzed liquid is, for example, preferably from 1% by mass to 20% by mass, more preferably from 1% by mass to 15% by mass, and even more preferably from 1% by mass to 10% by mass.
[0092] In addition to the methyl-containing silane compound and water, a catalyst may be added to the hydrolysis liquid. For example, an acid or a base can be used as the catalyst. The acid catalyzes the hydrolysis reaction of the silane compound containing a methyl group in the hydrolysis solution. On the other hand, the base catalyzes the condensation reaction between the hydrolyzed silane compound containing a methyl group and a functional group, such as a hydroxyl group or a silanol group, on the surface of the metal oxide particles. This makes it easier for the silane compound containing a methyl group to adhere to the metal oxide particles in the dispersion step (step C) described below, and improves the dispersion stability of the metal oxide particles.
[0093] Here, the above-mentioned "acid" refers to an acid based on the so-called Bronsted-Lowry definition, and refers to a substance that donates a proton in the hydrolysis reaction of a surface modification material such as a silane compound containing a methyl group. The above-mentioned "base" refers to a base based on the so-called Bronsted-Lowry definition, and refers to a substance that accepts a proton in the hydrolysis reaction of a silane compound containing a methyl group and the subsequent condensation reaction.
[0094] The acid is not particularly limited as long as it can supply protons in the hydrolysis reaction of the silane compound containing a methyl group, and examples thereof include inorganic acids such as hydrochloric acid, hydrobromic acid, hydroiodic acid, sulfuric acid, nitric acid, boric acid, phosphoric acid, etc., and organic acids such as acetic acid, citric acid, formic acid, etc. These organic acids may be used alone or in combination of two or more.
[0095] The base is not particularly limited as long as it can accept a proton in the hydrolysis reaction of a silane compound containing a methyl group, and examples thereof include sodium hydroxide, potassium hydroxide, barium hydroxide, calcium hydroxide, ammonia, amines, etc. These bases may be used alone or in combination of two or more.
[0096] Among the above, it is preferable to use an acid as the catalyst. As the acid, from the viewpoint of acidity, an inorganic acid is preferable, and hydrochloric acid is more preferable.
[0097] The content of the catalyst in the hydrolysis liquid is not particularly limited, but is preferably from 10 ppm to 1000 ppm, more preferably from 20 ppm to 800 ppm, and even more preferably from 30 ppm to 600 ppm, for example, which can sufficiently promote the hydrolysis of the silane compound containing a methyl group while suppressing side reactions of the silane compound containing a methyl group.
[0098] The hydrolysis liquid may also contain a hydrophilic solvent, which promotes the miscibility of water and the silane compounds in the hydrolysis liquid and further promotes the hydrolysis reaction of these silane compounds.
[0099] Examples of such hydrophilic solvents include various hydrophilic solvents that can be contained in the dispersion liquid described below.
[0100] Among the above, from the viewpoint of having excellent affinity with both water and the hydrophobic solvent and promoting miscibility thereof, the hydrophilic solvent preferably includes at least one selected from the group consisting of alcohol-based solvents, and more preferably includes at least one of methanol and ethanol.
[0101] The content of the hydrophilic solvent in the hydrolysis liquid is not particularly limited, but is preferably 60% by mass or less, more preferably 50% by mass or less. This allows the content of the silane compound and water in the hydrolysis liquid to be sufficiently large. The content of the hydrophilic solvent in the hydrolysis liquid is preferably 10% by mass or more, more preferably 15% by mass or more. This allows the miscibility of the silane compound containing a methyl group and water to be further promoted, and as a result, the hydrolysis reaction of the silane compound containing a methyl group can be efficiently promoted. The hydrolysis liquid does not need to contain a hydrophilic solvent other than the compound derived from the hydrolysis reaction.
[0102] In the hydrolysis step, after the hydrolysis liquid is prepared, it may be kept at a certain temperature for a certain period of time, which can further promote the hydrolysis of the silane compound. In this treatment, the temperature of the hydrolysis liquid is not particularly limited and can be appropriately changed depending on the type of silane compound, but is preferably, for example, from 5°C to 65°C, and more preferably from 30°C to 60°C.
[0103] The retention time is not particularly limited, but is preferably, for example, from 10 minutes to 180 minutes, and more preferably from 30 minutes to 120 minutes. During the above-mentioned holding of the hydrolyzed liquid, the hydrolyzed liquid may be appropriately stirred.
[0104] (Step A (Second Hydrolysis Step)) When the metal oxide particles are surface-modified with a silane compound containing a hydrocarbon group having two or more carbon atoms, a second hydrolysis step may be carried out to obtain a hydrolyzed liquid of the silane compound containing a hydrocarbon group having two or more carbon atoms. In the second hydrolysis step, a silane compound containing a hydrocarbon group having two or more carbon atoms is mixed with water to obtain a hydrolyzed liquid containing a hydrolyzed silane compound containing a hydrocarbon group having two or more carbon atoms. By using a mixed liquid in which at least a part of the silane compound containing a hydrocarbon group having two or more carbon atoms is hydrolyzed in advance in this manner, the silane compound containing a hydrocarbon group having two or more carbon atoms is easily attached to the metal oxide particles in the addition step F described below. The second hydrolysis step can be carried out in the same manner as in the first hydrolysis step, except that the silane compound containing a methyl group in the first hydrolysis step is replaced with a silane compound containing a hydrocarbon group having two or more carbon atoms.
[0105] (Process B (mixing process)) In the mixing step, the silane compound containing a methyl group and the metal oxide particles are mixed to obtain a mixed liquid. In the mixing step, in addition to the silane compound containing a methyl group and the metal oxide particles, water and a catalyst may be mixed. Note that, when a hydrolyzed liquid is obtained by the above-mentioned first hydrolysis step, the mixed liquid is obtained by mixing the hydrolyzed liquid and the metal oxide particles.
[0106] Mixing is then performed so that the content of the metal oxide particles in the mixed liquid is 10% by mass or more and 49% by mass or less, and the total content of the silane compound containing a methyl group and the inorganic oxide particles is 65% by mass or more and 98% by mass or less.
[0107] Thus, in this embodiment, the total content of the silane compound containing a methyl group and the metal oxide particles in the mixed liquid is very large. Furthermore, the dispersion medium, such as an organic solvent or water, which has been conventionally considered essential, is not contained in the mixed liquid or is mixed in only a very small amount. Alternatively, a small amount of an unavoidable alcohol compound is contained due to hydrolysis. Even in such a case, by going through the dispersion process, the metal oxide particles can be uniformly dispersed in the mixed liquid, and uniform adhesion (surface modification) of the silane compound containing a methyl group to the metal oxide particles can be achieved.
[0108] To explain in detail, when metal oxide particles are surface-modified in a liquid phase with a surface-modifying material such as a silane compound, generally, the metal oxide particles are mixed with not only the surface-modifying material but also a dispersion medium to obtain a mixed liquid, and the mixed liquid is dispersed using a dispersing machine.Here, when such surface-modified metal oxide particles are mixed with a methyl-based silicone resin, they cannot be sufficiently dispersed in the methyl-based silicone resin and aggregate, resulting in a problem of turbidity such as white turbidity in the methyl-based silicone resin.In such a case, the inorganic oxide particles added do not fully exhibit the desired performance.
[0109] Silane compounds containing methyl groups have low molecular weights and relatively low viscosity. Furthermore, since they are hydrolyzed in the above-mentioned hydrolysis step, they have good adhesion to metal oxide particles. Therefore, silane compounds containing methyl groups are extremely suitable for dispersing metal oxide particles in high-concentration silane compounds.
[0110] If the total content of the silane compound containing a methyl group and the metal oxide particles is less than 65% by mass, the amount of components other than the above two components, such as the dispersion medium, becomes too much, and the silane compound containing a methyl group cannot be sufficiently attached to the surface of the metal oxide particles in the dispersion step (step C) described below. As a result, many hydroxyl groups remain on the surface of the metal oxide particles, and when the resulting dispersion is mixed with a hydrophobic material, the metal oxide particles aggregate, causing the hydrophobic material to become turbid. The total content of the silane compound containing a methyl group and the metal oxide particles may be 65% by mass or more, but is preferably 70% by mass or more, and more preferably 75% by mass or more.
[0111] On the other hand, if the total content of the silane compound containing a methyl group and the metal oxide particles exceeds 98% by mass, the viscosity of the mixture becomes too high, and the silane compound containing a methyl group cannot be sufficiently attached to the surfaces of the metal oxide particles in the dispersion step (step C) described below. The total content of the silane compound containing a methyl group and the metal oxide particles may be 98% by mass or less, but is preferably 97% by mass or less, and more preferably 95% by mass or less.
[0112] As described above, the content of the metal oxide particles in the mixed liquid is 10% by mass or more and 49% by mass or less, which allows the amount of the silane compound containing a methyl group relative to the metal oxide particles to be within an appropriate range, allows the silane compound containing a methyl group to be uniformly attached to the surfaces of the metal oxide particles, and also prevents the viscosity of the mixed liquid from increasing.
[0113] On the other hand, when the content of metal oxide particles in the mixed liquid is less than 10% by mass, the amount of the silane compound containing a methyl group becomes excessive relative to the metal oxide particles, and the excess silane compound containing a methyl group in the resulting dispersion induces aggregation of the metal oxide particles. The content of metal oxide particles in the mixed liquid is preferably 20% by mass or more, and more preferably 30% by mass or more.
[0114] Furthermore, if the content of metal oxide particles exceeds 49% by mass, the amount of the silane compound containing a methyl group relative to the metal oxide particles is insufficient, and a sufficient amount of the silane compound containing a methyl group does not adhere to the metal oxide particles. Furthermore, as a result of the content of metal oxide particles being too high, the viscosity of the mixed liquid becomes too high, and the metal oxide particles cannot be sufficiently dispersed in the dispersion step (step C) described below. The content of metal oxide particles in the mixed liquid is preferably 45% by mass or less, and more preferably 40% by mass or less.
[0115] The content of the silane compound containing a methyl group relative to the content of the metal oxide particles in the mixed liquid is not particularly limited, but is preferably 100% by mass or more and 800% by mass or less, more preferably 140% by mass or more and 600% by mass or less, and even more preferably 180% by mass or more and 400% by mass or less. This allows the amount of the silane compound containing a methyl group relative to the metal oxide particles to be within an appropriate range, and allows the silane compound containing a methyl group to be uniformly attached to the surfaces of the metal oxide particles.
[0116] In the mixing step, an organic solvent may be further mixed into the mixed solution. By mixing the organic solvent into the mixed solution, it becomes possible to control the reactivity of the silane compound, and it becomes possible to control the degree of adhesion of the silane compound to the surface of the metal oxide particles. Furthermore, the organic solvent makes it possible to adjust the viscosity of the mixed solution.
[0117] Examples of such organic solvents include the hydrophobic solvents and hydrophilic solvents exemplified as the dispersion medium of the dispersion liquid according to the present embodiment described above. These organic solvents may be used alone or in combination of two or more.
[0118] The content of the organic solvent in the mixed solution is not particularly limited as long as it satisfies the above-mentioned content of the metal oxide particles and the silane compound containing a methyl group. It goes without saying that the mixed solution does not necessarily need to contain an organic solvent.
[0119] (Process C (dispersion process)) In the dispersing step, the metal oxide particles are dispersed in the mixed liquid obtained in the mixing step to obtain a first dispersion in which the metal oxide particles are dispersed. In this embodiment, the metal oxide particles are dispersed in a hydrolyzed silane compound containing a high concentration of methyl groups. Therefore, in the first dispersion obtained, the silane compound containing methyl groups is attached relatively uniformly to the surfaces of the metal oxide particles, and the first dispersion in which the metal oxide particles are relatively uniformly dispersed is obtained.
[0120] Dispersion of the metal oxide particles can be carried out by using a known dispersing machine, such as a bead mill, a ball mill, a homogenizer, a disperser, or a stirrer.
[0121] Here, in the dispersion step, it is preferable to disperse the metal oxide particles in the mixed liquid by applying the minimum necessary energy without applying excessive energy so that the particle diameter (dispersed particle diameter) of the metal oxide particles in the dispersion liquid becomes approximately uniform.
[0122] Furthermore, after the dispersion step, a solvent addition step D (first addition step) may be included in which a hydrophobic solvent is added to the first dispersion to obtain a second dispersion. The hydrophobic solvent may be any of the hydrophobic solvents listed above as the dispersion medium of the dispersion liquid according to the present embodiment. These hydrophobic solvents may be used alone or in combination of two or more.
[0123] (Step D (first addition step)) In the first addition step, a hydrophobic solvent is added to the first dispersion liquid to obtain a second dispersion liquid adjusted to a desired solid content (concentration). The first dispersion obtained in the dispersion step C has a high solid content (concentration), and therefore has a high viscosity and poor handleability. However, when a hydrophobic solvent is added to the obtained first dispersion in order to reduce the solid content, the particles aggregate due to the low hydrophobicity of the particle surfaces, and a uniform dispersion cannot be obtained.
[0124] Therefore, the present inventors have also found that a dispersion having a low solid content can be prepared by heating the obtained first dispersion and gradually adding a hydrophobic solvent thereto.
[0125] The mechanism is presumed to be as follows. By heating the first dispersion, the polymerization of the silane compound containing a methyl group attached to the metal oxide particles proceeds, improving the hydrophobicity of the particle surface. If the polymerization reaction proceeds too far, the metal oxide particles will aggregate. Therefore, by gradually adding a hydrophobic solvent to the first dispersion in which the polymerization reaction is proceeding, the surface is gradually made hydrophobic while suppressing excessive polymerization reaction. This allows the hydrophobic solvent to be gradually mixed into the first dispersion. That is, a dispersion adjusted to the desired solid content can be obtained by adding an amount of hydrophobic solvent that does not cause the metal oxide particles to aggregate, and allowing the polymerization reaction of the methyl group-containing silane compound to proceed to an extent that the silane compound is compatible with the added amount of hydrophobic solvent.
[0126] As described above, the hydrophobic solvent may be added gradually so as not to cause the metal oxide particles to aggregate. Therefore, the first dispersion may be heated before the solvent is added, the hydrophobic solvent may be added before the first dispersion is heated, or the first dispersion may be heated and the hydrophobic solvent may be added at the same time. That is, the first addition step may be step d1 of heating the first dispersion and then adding a hydrophobic solvent at a rate at which the metal oxide particles do not aggregate, or step d2 of adding a hydrophobic solvent while heating the first dispersion at a rate at which the metal oxide particles do not aggregate, or step d3 of adding a hydrophobic solvent at a rate at which the metal oxide particles do not aggregate and then heating the first dispersion.
[0127] The rate at which the metal oxide particles do not aggregate is not particularly limited. For example, the hydrophobic solvent may be added continuously at a rate at which the solid content is reduced to a range of 3% by mass or more and 20% by mass or less in 1 hour. The amount of hydrophobic solvent added may be appropriately adjusted so that the amount of hydrophobic solvent added is increased when the heating temperature is high, and decreased when the heating temperature is low.
[0128] For example, the hydrophobic solvent may be added stepwise every 30 minutes, every hour, or every two hours so that the solid content is reduced to within a range of 3% by mass or more and 20% by mass or less. The amount of hydrophobic solvent added may be appropriately adjusted so that a larger amount of hydrophobic solvent is added at one time when the heating temperature is high, and a smaller amount of hydrophobic solvent is added at one time when the heating temperature is low.
[0129] The heating temperature is not particularly limited as long as it is a temperature at which the polymerization reaction of the silane compound containing a methyl group proceeds. The heating temperature is preferably, for example, 35°C or more and 80°C or less. By setting the heating temperature at 35°C or more, the polymerization reaction of the silane compound containing a methyl group can proceed. On the other hand, by setting the heating temperature at 80°C or less, the aggregation of metal oxide particles due to the rapid reaction of the silane compound containing a methyl group can be suppressed.
[0130] The heating time may be appropriately carried out until the adjustment of the solid content is completed, and is preferably, for example, 4 hours or more and 12 hours or less. By heating for 4 hours or more, the polymerization reaction of the silane compound containing a methyl group progresses, and it becomes possible to mix it with the solvent. On the other hand, by heating for 12 hours or less, it is possible to suppress the aggregation of metal oxide particles due to the excessive progress of the polymerization reaction of the silane compound containing a methyl group.
[0131] From the viewpoint of ease of handling in removing the dispersion medium during the production of the composition described below, the hydrophobic solvent is preferably at least one selected from the group consisting of toluene, o-xylene, m-xylene, p-xylene and benzene, and more preferably toluene.
[0132] The content of the hydrophobic solvent in the final second dispersion may be appropriately adjusted to a desired solid content. The content of the hydrophobic solvent is, for example, preferably 40% by mass or more and 95% by mass or less, more preferably 50% by mass or more and 90% by mass or less, and even more preferably 60% by mass or more and 80% by mass or less. The first addition step provides a second dispersion adjusted to a desired solid content. The use of the second dispersion improves the handling properties of the dispersion in the following steps.
[0133] (Process E (removal process)) In this embodiment, step D may be followed by step E of removing the alcohol produced by hydrolysis. It is presumed that the provision of the removal step improves the production efficiency of the composition described below. The method for removing the solvent is not particularly limited, but for example, an evaporator can be used. The removal step may be carried out until the alcohol is completely removed, or about 5% by mass of the alcohol may remain.
[0134] (Step F (second addition step)) In the second addition step, a silicone compound containing a hydrocarbon group having two or more carbon atoms is added to the second dispersion to obtain a third dispersion. As described above, in the second dispersion, the silane compound containing a methyl group is relatively uniformly attached to the surface of the metal oxide particles. Therefore, the silicone compound is relatively uniformly present near the surface of the metal oxide particles via the silane compound containing a methyl group.
[0135] In the second addition step, the mixture of the second dispersion liquid and the silicone compound may be held at a predetermined temperature for a predetermined time, which can further promote the surface modification of the metal oxide particles with the silicone compound.
[0136] Examples of the silicone compound include the silicone compounds described above. These silicone compounds may be used alone or in combination of two or more.
[0137] The silicone compound can be added to the second dispersion so that the content of the silicone compound in the second dispersion is, for example, preferably 10% by mass or more and 500% by mass or less with respect to the metal oxide particles. In addition, taking into consideration the amount of the methyl group contained in the silane compound and the amount of the hydrocarbon group having 2 or more carbon atoms contained in the silicone compound, the silicone compound is added so that the ratio of the methyl group / hydrocarbon group having 2 or more carbon atoms is 0.01 to 10. This allows a sufficient amount of silicone compound to be attached to the surface of the metal oxide particles, improving the dispersion stability of the metal oxide particles and improving the dispersibility in the silicone resin for LEDs. Furthermore, the amount of the free silicone compound can be reduced, and unintended aggregation of the metal oxide particles in the silicone resin for LEDs can be suppressed.
[0138] In the second addition step, the holding temperature is not particularly limited and can be changed appropriately depending on the type of silicone compound, but is preferably, for example, 40°C or higher and 150°C or lower, and more preferably 50°C or higher and 140°C or lower.
[0139] The retention time is not particularly limited, but is preferably, for example, from 1 hour to 24 hours, and more preferably from 2 hours to 20 hours. During the above-mentioned holding, the third dispersion liquid may be appropriately stirred.
[0140] In the second addition step, the treatment with the silicone compound may be carried out multiple times. For example, by using different types of silicone compounds and carrying out the treatment with the silicone compound multiple times, it becomes easier to control the surface state of the metal oxide particles according to the type of methyl-based silicone resin. In the second addition step, the solid content may be measured after the treatment with the silicone compound, and the hydrophobic solvent may be added so as to obtain a desired solid content. By reducing the solid content, it becomes easier to mix with the silicone resin component described later.
[0141] In the second addition step, a silane compound containing a methyl group or a silane compound containing a hydrocarbon group having a carbon number of 2 or more may be added. By adding these silane compounds, it becomes easy to adjust the ratio of methyl groups / hydrocarbon groups. For the silane compound containing a methyl group or the silane compound containing a hydrocarbon group having two or more carbon atoms, the hydrolyzed liquid obtained by the above-mentioned first or second hydrolysis step may be used.
[0142] When a silane compound is added in the second addition step, the amount added, including the amount of the silane compound containing a methyl group mixed in the mixing step B, may be, for example, 100 mass % or more and 700 mass % or less relative to the metal oxide particles. Furthermore, when a silane compound containing a hydrocarbon group having two or more carbon atoms is added in the second addition step, the amount of the hydrocarbon group contained in the silicone compound is also taken into consideration, and the compound is added so that the molar ratio of methyl groups to the hydrocarbon group having two or more carbon atoms is 0.01 or more and 10 or less. In the second addition step, the silane compound and the silicone compound may be added simultaneously, the silane compound may be added first and then the silicone compound, or the silicone compound may be added first and then the silane compound.
[0143] In this manner, a third dispersion liquid can be obtained in which the metal oxide particles to which the silane compound containing a methyl group is attached are surface-modified with a silicone compound.
[0144] In the dispersion liquid containing the surface-modified metal oxide particles produced by the method for producing the surface-modified metal oxide particles according to the present embodiment, the surface of the metal oxide particles is densely and sufficiently modified with a silane compound containing a methyl group or a methyl group and a hydrocarbon group having two or more carbon atoms, and further, a silicone compound containing a hydrocarbon group having two or more carbon atoms is present in the vicinity of the surface of the metal oxide particles. The surface-modified metal oxide particles thus surface-modified have excellent compatibility with both methyl-based silicone resins and phenyl-based silicone resins for LEDs, and can be dispersed relatively uniformly in both resins. Therefore, when the surface-modified metal oxide particles are dispersed in either methyl-based silicone resins or phenyl-based silicone resins, the occurrence of turbidity such as white turbidity is suppressed. Furthermore, the viscosity change of the silicone resin for LEDs containing the surface-modified metal oxide particles is also suppressed.
[0145] <4. Composition> Next, the composition according to this embodiment will be described. The composition according to the present embodiment includes a dispersion liquid containing the above-mentioned surface-modified metal oxide particles and a silicone resin component. That is, the composition according to the present embodiment is a mixture of the above-mentioned dispersion liquid and the silicone resin component. Therefore, the composition according to the present embodiment includes the above-mentioned metal oxide particles surface-modified with a silane compound containing a methyl group or a methyl group and a hydrocarbon group having two or more carbon atoms, a solvent, and a silicone resin component. Here, the silicone resin component means that the silicone resin is in a fluid state before it is cured.
[0146] The composition according to the present embodiment is cured as described below and used as a sealing member for a light emitting device. The composition according to the present embodiment contains metal oxide particles that contribute to improving the refractive index and transparency described above, and therefore can improve the brightness of light emitted from a light emitting device when used as a sealing member.
[0147] Furthermore, the composition according to the present embodiment contains surface-modified metal oxide particles in which the above-mentioned methyl-containing silane compound and the silicone compound containing a hydrocarbon group having two or more carbon atoms are sufficiently attached to the metal oxide particles to satisfy the above formula (1), so that even when a silicone resin component is contained, and even after the silicone resin component is cured, aggregation of the metal oxide particles is suppressed and a decrease in transparency is suppressed. Therefore, when the composition according to the present embodiment is used as a sealing member, the brightness of the light from the light-emitting device can be improved.
[0148] In order to obtain a highly transparent composition, the content of metal oxide particles in the composition of this embodiment is preferably 5% by mass or more and 50% by mass or less, more preferably 5% by mass or more and 40% by mass or less, and even more preferably 10% by mass or more and 35% by mass or less.
[0149] The contents of the silane compound containing a methyl group and the silicone compound containing a hydrocarbon group having two or more carbon atoms can correspond to the contents in the surface-modified metal oxide particles according to this embodiment.
[0150] The silicone resin component is the main component in the composition according to this embodiment. When the composition according to this embodiment is used as an encapsulating material, the silicone resin component cures to encapsulate the light-emitting element, thereby preventing deterioration factors from the external environment, such as moisture and oxygen, from reaching the light-emitting element. In this embodiment, the cured product obtained from the silicone resin component is basically transparent and can transmit the light emitted from the light-emitting element.
[0151] The silicone resin component is not particularly limited as long as it is a silicone resin component for LEDs for sealing LEDs. The silicone resin component preferably contains a methyl group and a phenyl group. The silicone resin component may be a methyl-based silicone resin component or a phenyl-based silicone resin component. The methyl-based silicone resin component means a silicone resin component containing a large number of methyl groups. The methyl-based silicone resin component may be a methyl-group-containing silicone resin component, a methylphenyl silicone resin component, or a dimethyl silicone resin component. From the viewpoint of high versatility, the methylphenyl silicone resin component is preferred. The phenyl-based silicone resin component means a silicone resin component that contains a large amount of phenyl groups. The phenyl-based silicone resin component may be a silicone resin component containing a phenyl group, a methylphenyl silicone resin component, or a diphenyl silicone resin. From the viewpoint of high versatility, the methylphenyl silicone resin component is preferred.
[0152] The content of the silicone resin component in the composition according to this embodiment can be the balance of other components, but is preferably, for example, from 10% by mass to 70% by mass. The mass ratio of the silicone resin component to the surface-modified metal oxide particles in the composition according to this embodiment is preferably in the range of 50:50 to 90:10 (silicone resin:surface-modified metal oxide particles), and more preferably in the range of 60:40 to 80:20.
[0153] The composition according to the present embodiment may contain the solvent derived from the dispersion according to the present embodiment, or may have been removed. That is, the solvent derived from the dispersion may be completely removed, or may remain in the composition in an amount of about 1% by mass to about 10% by mass, or about 2% by mass to about 5% by mass.
[0154] The composition according to the present embodiment may contain phosphor particles as long as the purpose of the present invention is not impaired. The phosphor particles absorb light of a specific wavelength emitted from a light-emitting element and emit light of a specified wavelength. In other words, the phosphor particles enable conversion of the wavelength of light and adjustment of the color tone.
[0155] There are no particular limitations on the phosphor particles as long as they can be used in a light emitting device as described below, and they can be appropriately selected and used so that the light emitting device emits a desired color. The content of the phosphor particles in the composition of this embodiment can be appropriately adjusted so as to obtain a desired brightness.
[0156] The composition according to the present embodiment may contain commonly used additives such as preservatives, polymerization initiators, polymerization inhibitors, curing catalysts, light diffusing agents, etc., within the scope of not impairing the object of the present invention. As the light diffusing agent, it is preferable to use silica particles having an average particle size of 1 μm or more and 30 μm or less.
[0157] The composition according to the present embodiment contains surface-modified metal oxide particles in which the above-mentioned methyl-containing silane compound and the silicone compound containing a hydrocarbon group having two or more carbon atoms are sufficiently attached to the metal oxide particles to satisfy the above formula (1), so that aggregation of the metal oxide particles is suppressed and a decrease in transparency is suppressed, regardless of whether the silicone resin component is a methyl-based silicone resin or a phenyl-based silicone resin. Therefore, the composition according to the present embodiment can be used to form a sealing member that improves the brightness of light from a light-emitting device.
[0158] <5. Method for producing the composition> Next, a method for producing the composition according to this embodiment will be described.
[0159] The method for producing a composition according to this embodiment includes a step H of obtaining a composition by adding a silicone resin component to the third dispersion obtained by the above-mentioned method for producing surface-modified metal oxide particles.
[0160] (Step G (3rd addition step)) In the third addition step, a silicone resin component is added to the third dispersion liquid, and the composition is adjusted to a desired solid content (concentration).
[0161] The content of the silicone resin component in the final composition may be appropriately adjusted so as to obtain a desired solid content. The content of the silicone resin component is preferably, for example, 10% by mass or more and 70% by mass or less. The third addition step provides a composition adjusted to the desired solids content.
[0162] (Process H (removal process)) In this embodiment, after step G, step H of removing the solvent contained in the third dispersion may be provided. The method for removing the solvent is not particularly limited, but for example, an evaporator can be used. The removal step may be carried out until the solvent is completely removed, or about 5% by mass of the solvent may remain.
[0163] In this manner, the composition according to the present embodiment can be obtained.
[0164] <6. Sealing member> The sealing member according to this embodiment is a cured product of the composition according to this embodiment. The sealing member according to this embodiment is usually used as a sealing member disposed on a light-emitting element or as a part thereof. The thickness and shape of the sealing member according to this embodiment can be appropriately adjusted depending on the desired application and characteristics, and are not particularly limited.
[0165] The sealing member according to the present embodiment can be manufactured by curing the composition according to the present embodiment as described above. The curing method of the composition can be selected according to the properties of the silicone resin in the composition according to the present embodiment, and examples of the curing method include heat curing and electron beam curing. More specifically, the sealing member according to the present embodiment can be obtained by curing the silicone resin in the composition according to the present embodiment through an addition reaction or a polymerization reaction.
[0166] The average dispersed particle size of the metal oxide particles in the sealing member is preferably 10 nm or more and 300 nm or less, more preferably 20 nm or more and 250 nm or less, and further preferably 30 nm or more and 200 nm or less.
[0167] The average dispersed particle diameter of the metal oxide particles in the sealing member is the average particle diameter (median diameter) based on the number distribution measured by observing the sealing member with a transmission electron microscope (TEM). The average dispersed particle diameter of the metal oxide particles in the sealing member according to the present embodiment is a value measured and calculated based on the dispersed particle diameter of the metal oxide particles in the sealing member. The average dispersed particle diameter is measured and calculated based on the diameter of the metal oxide particles in a dispersed state, regardless of whether the metal oxide particles are dispersed in the state of primary particles or secondary particles. In the present embodiment, the average particle diameter of the metal oxide particles in the sealing member may be measured as the average particle diameter of the metal oxide particles surface-modified with the silane compound and the silicone compound. Since the sealing member may contain metal oxide particles surface-modified with the silane compound and the silicone compound, and metal oxide particles not surface-modified with the silane compound and the silicone compound, the average particle diameter of the metal oxide particles in the sealing member is usually measured as a value in a mixed state of these.
[0168] The sealing member according to the present embodiment is a cured product of the composition according to the present embodiment, and therefore has excellent refractive index and transparency, making it possible to obtain a sealing member with excellent light extraction efficiency that improves the brightness of the light emitting device.
[0169] <7. Light emitting device> Next, a light emitting device according to this embodiment will be described. The light emitting device according to this embodiment includes the above-mentioned sealing member and a light emitting element sealed in the sealing member.
[0170] Examples of the light-emitting element include a light-emitting diode (LED), an organic light-emitting diode (OLED), etc. The sealing member according to this embodiment is particularly suitable for sealing a light-emitting diode.
[0171] Hereinafter, the light emitting device according to this embodiment will be described by taking an example in which the light emitting element is a light emitting diode on a chip, that is, an LED chip, and the light emitting device is an LED package. 1 to 4 are schematic diagrams (cross-sectional views) illustrating an example of a light emitting device according to an embodiment of the present invention. In addition, the size of each component in the drawings is appropriately exaggerated for ease of explanation, and does not indicate the actual dimensions or ratios between components. In addition, in this specification and drawings, components having substantially the same functional configuration are assigned the same reference numerals to avoid redundant explanation.
[0172] The light emitting device (LED package) 1A shown in Figure 1 comprises a substrate 2 having a recess 21, a light emitting element (LED chip) 3 arranged on the bottom surface of the recess 21 of the substrate 2, and a sealing member 4A that covers and seals the light emitting element 3 in the recess 21. The sealing member 4A is composed of the sealing member according to the present embodiment described above. Therefore, metal oxide particles derived from the composition according to the present embodiment described above are dispersed in the sealing member 4A, and as a result, the light extraction efficiency of the light emitting device 1A is improved. Furthermore, phosphor particles 5 are dispersed in the sealing member 4A. The phosphor particles 5 convert the wavelength of at least a part of the light emitted from the light emitting element 3.
[0173] The light emitting device 1B shown in FIG. 2 differs from the light emitting device 1A in that the sealing member 4B has two layers. That is, the sealing member 4B has a first layer 41B that directly covers the light emitting element 3 and a second layer 43B that covers the first layer 41B. Both the first layer 41B and the second layer 43B are sealing members according to the present embodiment. Phosphor particles 5 are dispersed in the first layer 41B. On the other hand, the second layer 43B does not contain phosphor particles 5. In the light emitting device 1B, metal oxide particles derived from the composition according to the present embodiment described above are dispersed in the first layer 41B and the second layer 43B constituting the sealing member 4B, thereby improving the brightness of light.
[0174] The light emitting device 1C shown in FIG. 3 is also different from the light emitting device 1A in that the configuration of the sealing member 4C is different from that of the sealing member 4A. The sealing member 4C has a first layer 41C that directly covers the light emitting element 3 and a second layer 43C that covers the first layer 41C. The first layer 41C is not the sealing member according to this embodiment, but is a sealing member made of a resin that does not contain the above-mentioned metal oxide particles, and is made of a resin that can be used for a sealing member. In addition, phosphor particles 5 are dispersed in the first layer 41C. On the other hand, the second layer 43C is the sealing member according to this embodiment. In the light emitting device 1C, the metal oxide particles derived from the composition according to this embodiment are dispersed in the second layer 43C constituting the sealing member 4C, thereby improving the light extraction efficiency.
[0175] In the light emitting device 1D shown in FIG. 4, the sealing member 4D has a first layer 41D that directly covers the light emitting element 3, a second layer 43D that covers the first layer 41D, and a third layer 45D that further covers the second layer 43D. The first layer 41D and the second layer 43D are sealing members made of a resin that does not contain the above-mentioned metal oxide particles, and are made of a resin that can be used for a sealing member, etc., rather than the sealing member according to this embodiment. In addition, phosphor particles 5 are dispersed in the second layer 43D. On the other hand, the third layer 45D is the sealing member according to this embodiment. In the light emitting device 1D, the brightness of light is improved by dispersing metal oxide particles derived from the composition according to this embodiment described above in the third layer 45D constituting the sealing member 4D.
[0176] The light emitting device according to the present embodiment is not limited to the illustrated embodiment. For example, the light emitting device according to the present embodiment does not need to include phosphor particles in the sealing member. The sealing member according to the present embodiment can be present at any position in the sealing member.
[0177] As described above, in the light emitting device according to this embodiment, the light emitting element is sealed with the sealing member of this embodiment, and therefore the brightness of the light is improved.
[0178] In addition, in the light emitting device according to the present embodiment, the light emitting element is sealed with the composition according to the present embodiment as described above. Therefore, in one aspect, the present invention also relates to a method for manufacturing a light emitting device, which includes a step of sealing the light emitting element with the composition according to the present embodiment. In the same aspect, the manufacturing method may include a step of mixing the dispersion according to the present embodiment and a resin component to obtain the composition.
[0179] The light emitting element can be sealed by applying the composition according to this embodiment onto the light emitting element using a dispenser or the like, and then curing the composition.
[0180] <8.Lighting equipment, display devices> The light emitting device according to the present embodiment as described above can be used in, for example, a lighting fixture or a display device. Accordingly, one aspect of the present invention relates to a lighting fixture or a display device including the light emitting device according to the present embodiment. Examples of lighting fixtures include general lighting devices such as indoor lights and outdoor lights, and lighting for switches of electronic devices such as mobile phones and office automation equipment. Since the lighting fixture according to this embodiment is equipped with the light-emitting device according to this embodiment, even if the same light-emitting element is used, the emitted luminous flux is greater than in the conventional lighting fixture, and the surrounding environment can be brighter.
[0181] Examples of display devices include mobile phones, personal digital assistants, electronic dictionaries, digital cameras, computers, televisions, and peripheral devices thereof. Since the display device according to this embodiment is equipped with the light-emitting device according to this embodiment, even if the same light-emitting element is used, the emitted light flux is greater than in the conventional case, and, for example, a clearer and brighter display can be provided. EXAMPLES
[0182] The present invention will be described in more detail below with reference to examples and comparative examples. Note that the examples described below are merely examples of the present invention and do not limit the present invention.
[0183] [Example 1] (Preparation of Dispersion) (1) First hydrolysis step 90.78 parts by mass of methyltrimethoxysilane (product name: KBM-13, manufactured by Shin-Etsu Kogyo Chemical Co., Ltd.), 9.21 parts by mass of water, and 0.01 parts by mass of hydrochloric acid (1N) were added and mixed to obtain a hydrolyzed liquid. Next, this hydrolyzed liquid was stirred at 60° C. for 30 minutes to carry out hydrolysis treatment of methyltrimethoxysilane, thereby obtaining a hydrolyzed liquid.
[0184] (2)Mixing process A mixture was obtained by mixing 30 parts by mass of zirconium oxide (ZrO2) particles (manufactured by Sumitomo Osaka Cement Co., Ltd.) having an average primary particle size of 12 nm with 70 parts by mass of the hydrolysis liquid described above. The content of the zirconium oxide particles in the mixture was 30% by mass, the content of methyltrimethoxysilane was 63.5% by mass, and the total content of the zirconium oxide particles and methyltrimethoxysilane was 93.5% by mass.
[0185] (3) Dispersion process This mixture was subjected to a dispersion treatment in a beads mill for 6 hours, and then the beads were removed to obtain a first dispersion. The solids content of the first dispersion (at 100° C. for 1 hour) was measured and found to be 70% by mass.
[0186] (4) First Addition Step The obtained first dispersion was heated for 2 hours at 60° C. Next, toluene was added to the dispersion so that the solid content was 40 mass %, and the mixture was heated at 60° C. for 2 hours. Next, toluene was added to the dispersion so that the solid content was 30% by mass, and the mixture was heated at 60° C. for 1 hour. Next, toluene was added to the dispersion so that the solid content was 20% by mass, and the mixture was heated at 60° C. for 1 hour to obtain a second dispersion.
[0187] (FT-IR analysis) A portion of the second dispersion was taken and dried in a vacuum dryer. Using 0.01 g to 0.05 g of the obtained surface-modified zirconium oxide particles, a Fourier transform infrared spectrophotometer (model number: FT / IR-670 Plus, manufactured by JASCO Corporation) was used to measure the surface-modified zirconium oxide particles at 800 cm -1 More than 3800cm -1 The transmission spectrum was measured in the following wave number range. The spectrum values were normalized so that the maximum value of the spectrum in this measurement range was 100 and the minimum value was 0. -1 Value of (IA) and 1100cm -1 The value of IA / IB was calculated, and the result was 7.
[0188] (5) Second Addition Step 66.7 parts by mass of the second dispersion, the solid content of which had been adjusted to 15% by mass with toluene, was mixed with 33.3 parts by mass of a silicone compound containing a methyl group and a phenyl group (product name: KR213 (high phenyl content), manufactured by Shin-Etsu Chemical Co., Ltd.) and stirred at 100°C for 3 hours to obtain the dispersion of Example 1 (third dispersion).
[0189] (Evaluation of Dispersion) (1) FT-IR analysis 10 g of the dispersion liquid according to Example 1, in which the solid content was adjusted to 30% by mass with toluene, was dried for 2 hours under conditions of 100°C and 20 hPa using a vacuum dryer (EYELA Tokyo Rikakiki Co., Ltd., device name: VACUUM OVEN VOS-201SD). Next, 0.01 g to 0.05 g of the obtained metal oxide particles were used to measure the chromatographic diffraction pattern at 800 cm using a Fourier transform infrared spectrophotometer (model number: FT / IR-670 Plus, manufactured by JASCO Corporation). -1 More than 3800cm -1 The transmission spectrum was measured in the following wave number range. The spectrum values were normalized so that the maximum value of the spectrum in this measurement range was 100 and the minimum value was 0. -1 Value of (IA) and 1100cm -1 The value of IA / IB was calculated. As a result, the IA / IB ratio was 1.9. The results are shown in Table 1.
[0190] (2)NMR measurement 15 g of the dispersion liquid according to Example 1, in which the solid content had been adjusted to 30% by mass with toluene, was mixed with 15 g of methanol to precipitate the surface-modified zirconium oxide particles. This mixture was subjected to solid-liquid separation using a centrifuge, and the solid portion (surface-modified zirconium oxide particles) was collected. Several mg of the collected surface-modified zirconium oxide particles were taken and dissolved in deuterated chloroform to a concentration of 1% by mass. Using this dissolving solution, a benchtop NMR device (manufactured by Nanalysis, model number NMReady60Pro ( 1 H / 19 F)) to separate the phenyl and methyl groups. 1The H-liquid NMR spectrum was measured. From the spectrum obtained, the peak areas (integral values) of the phenyl group and the methyl group were calculated, and the molar ratio of the methyl group to the phenyl group was calculated by calculating the integral value of the methyl group / the integral value of the phenyl group. The results are shown in Table 1. The molar ratio of methyl groups to phenyl groups (methyl groups / phenyl groups) was 0.45. The results are shown in Table 1.
[0191] (Preparation of Composition A) 16.7 g of the dispersion liquid according to Example 1, in which the solid content was adjusted to 30 mass % with toluene, was mixed with 95 g of a methyl-based silicone resin component (product name: KER-2500-A / B, manufactured by Shin-Etsu Chemical Co., Ltd.). Next, the toluene was removed from this mixed liquid using an evaporator, thereby obtaining a composition A according to Example 1 containing a methyl-based silicone resin component.
[0192] The viscosity of the obtained composition A was measured using a rheometer (product name: Rheostress RS-6000, manufactured by HAAKE) at 25° C. and a shear rate of 1 (1 / s). As a result, the viscosity A of Composition A was 8 Pa·s. The results are shown in Table 1.
[0193] (Preparation of cured product A) This composition was filled into a Teflon (registered trademark)-coated SUS container with a thickness of 1 mm to a thickness of 1 mm. It was then heated at 100°C for 2 hours and then at 150°C for 4 hours to obtain a cured product A according to Example 1. The thickness of the cured product A taken out of the container was about 1 mm.
[0194] The transmittance of the cured product A taken out of the container was measured using an integrating sphere with a spectrophotometer (manufactured by JASCO Corporation, model number: V-770). The transmittance A of the cured product A containing a methyl-based silicone resin was 70%. The results are shown in Table 1.
[0195] (Preparation of Composition B and Cured Product B) 16.7 g of the dispersion liquid according to Example 1, in which the solid content was adjusted to 30 mass % with toluene, was mixed with 95 g of a phenyl-based silicone resin component (product name: OE-6520, manufactured by Dow Corning Toray Co., Ltd.). Next, the toluene was removed from this mixture using an evaporator to obtain composition B according to Example 1, which contains a phenyl-based silicone resin component. The viscosity B of composition B, which was measured in the same manner as composition A, is shown in Table 1. Next, the composition was cured in the same manner as composition A to obtain a cured product B according to Example 1. The thickness of the cured product B taken out of the container was about 1 mm. The transmittance B was measured in the same manner as for the cured product A and is shown in Table 1.
[0196] (LED package fabrication and brightness evaluation) (1) Preparation of the composition 5.0 g of the dispersion according to Example 1, in which the solid content was adjusted to 30 mass % with toluene, was mixed with 3.5 g of a methyl-based silicone resin component (product name: KER-2500-B, manufactured by Shin-Etsu Chemical Co., Ltd.) In other words, the total mass of the zirconia and the surface modification material and the methyl-based silicone resin component were mixed at a mass ratio of 30:70. Next, the toluene was removed from this mixed liquid using an evaporator, thereby obtaining a composition C according to Example 1 for producing a sealing member.
[0197] (2) Fabrication of LED package 14 parts by mass of a methyl silicone resin component (product name: KER-2500-A / B, manufactured by Shin-Etsu Chemical Co., Ltd.) was added to 1 part by mass of the obtained composition C, and the surface-modified zirconium oxide particles in the composition were adjusted to 2% by mass, and mixed. A composition (total amount of surface-modified zirconium oxide particles and resin: phosphor particles = 100:38) in which 0.38 parts by mass of phosphor particles (yttrium aluminum garnet: YAG) was mixed with 1 part by mass of this composition was filled in an LED lead frame to a thickness of 300 μm. Then, it was kept at room temperature for 3 hours. Next, the composition was slowly heated and cured to form a sealing member, and a white LED package according to Example 1 was produced.
[0198] (3) Evaluation The brightness of the obtained white LED package was measured by applying a voltage of 3 V and a current of 150 mA to the LED package using a total luminous flux measurement system (manufactured by Otsuka Electronics Co., Ltd.). As a result, the brightness of this white LED package was 74.4 lm. The results are shown in Table 1.
[0199] [Example 2] A dispersion (third dispersion) of Example 2 was obtained in exactly the same manner as in Example 1, except that instead of mixing 66.7 parts by mass of the second dispersion, the solid content of which was adjusted to 15% by mass with toluene, and 33.3 parts by mass of a silicone compound containing a methyl group and a phenyl group, 90.9 parts by mass of the second dispersion and 9.1 parts by mass of the above silicone compound were mixed.
[0200] The IA / IB and the methyl group / phenyl group ratio of the dispersion liquid of Example 2 were measured in the same manner as in Example 1. The results are shown in Table 1.
[0201] Compositions A and B and cured products A and B of Example 2 were obtained in the same manner as in Example 1, except that the dispersion of Example 2 was used instead of the dispersion of Example 1. The viscosities of the compositions and the transmittances of the cured products were measured in the same manner as in Example 1, and the results are shown in Table 1.
[0202] Composition C according to Example 2 and an LED package according to Example 2 were obtained in the same manner as in Example 1, except that the dispersion according to Example 2 was used instead of the dispersion according to Example 1. The results of evaluation in the same manner as in Example 1 are shown in Table 1.
[0203] [Example 3] A dispersion of Example 3 (third dispersion) was obtained in exactly the same manner as in Example 1, except that instead of mixing 66.7 parts by mass of the second dispersion, the solid content of which was adjusted to 15% by mass with toluene, and 33.3 parts by mass of the silicone compound containing a methyl group and a phenyl group, 95.2 parts by mass of the second dispersion and 4.8 parts by mass of the above silicone compound were mixed.
[0204] The IA / IB and the methyl group / phenyl group ratio of the dispersion liquid of Example 3 were measured in the same manner as in Example 1. The results are shown in Table 1.
[0205] Compositions A and B and cured products A and B of Example 3 were obtained in the same manner as in Example 1, except that the dispersion of Example 3 was used instead of the dispersion of Example 1. The viscosities of the compositions and the transmittances of the cured products were measured in the same manner as in Example 1, and the results are shown in Table 1.
[0206] Composition C according to Example 3 and an LED package according to Example 3 were obtained in the same manner as in Example 1, except that the dispersion according to Example 3 was used instead of the dispersion according to Example 1. The results of evaluation in the same manner as in Example 1 are shown in Table 1.
[0207] [Example 4] (Second hydrolysis step) 91.66 parts by mass of phenyltrimethoxysilane (product name: KBM-103, manufactured by Shin-Etsu Kogyo Chemical Co., Ltd.), 8.33 parts by mass of water, and 0.01 parts by mass of hydrochloric acid (1N) were added and mixed to obtain a hydrolyzed liquid. Next, this hydrolyzed liquid was stirred at 60° C. for 30 minutes to carry out hydrolysis treatment of phenyltrimethoxysilane, thereby obtaining a hydrolyzed liquid.
[0208] (Preparation of Dispersion) 62.5 parts by mass of the second dispersion obtained in the production process of Example 1 and adjusted to a solid content of 15% by mass, 6.3 parts by mass of the above-mentioned phenyltrimethoxysilane hydrolyzate, and 31.2 parts by mass of a silicone compound containing a methyl group and a phenyl group (product name: KR213 (high phenyl content), manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and stirred at 100°C for 3 hours to obtain a dispersion related to Example 4 (third dispersion).
[0209] The IA / IB and the methyl group / phenyl group ratio of the dispersion liquid of Example 4 were measured in the same manner as in Example 1. The results are shown in Table 1.
[0210] Compositions A and B and cured products A and B of Example 4 were obtained in the same manner as in Example 1, except that the dispersion of Example 4 was used instead of the dispersion of Example 1. The viscosities of the compositions and the transmittances of the cured products were measured in the same manner as in Example 1, and the results are shown in Table 1.
[0211] Composition C according to Example 4 and an LED package according to Example 4 were obtained in the same manner as in Example 1, except that the dispersion according to Example 4 was used instead of the dispersion according to Example 1. The results of evaluation in the same manner as in Example 1 are shown in Table 1.
[0212] [Example 5] A dispersion liquid of Example 5 was obtained in the same manner as in Example 4, except that instead of mixing 62.5 parts by mass of the second dispersion liquid, 6.3 parts by mass of the hydrolyzed liquid of phenyltrimethoxysilane, and 31.2 parts by mass of a silicone compound containing a methyl group and a phenyl group in Example 4, 60.6 parts by mass of the second dispersion liquid, 9.1 parts by mass of the hydrolyzed liquid of phenyltrimethoxysilane, and 30.3 parts by mass of a silicone compound containing a methyl group and a phenyl group were mixed.
[0213] The IA / IB and the methyl group / phenyl group ratio of the dispersion liquid of Example 5 were measured in the same manner as in Example 1. The results are shown in Table 1.
[0214] Compositions A and B and cured products A and B of Example 5 were obtained in the same manner as in Example 1, except that the dispersion of Example 5 was used instead of the dispersion of Example 1. The viscosities of the compositions and the transmittances of the cured products were measured in the same manner as in Example 1, and the results are shown in Table 1.
[0215] Composition C according to Example 5 and an LED package according to Example 5 were obtained in the same manner as in Example 1, except that the dispersion according to Example 5 was used instead of the dispersion according to Example 1. The results of evaluation in the same manner as in Example 1 are shown in Table 1.
[0216] [Example 6] A dispersion liquid of Example 6 was obtained in the same manner as in Example 4, except that instead of mixing 62.5 parts by mass of the second dispersion liquid, 6.3 parts by mass of the hydrolyzed liquid of phenyltrimethoxysilane, and 31.2 parts by mass of a silicone compound containing a methyl group and a phenyl group in Example 4, 64.5 parts by mass of the second dispersion liquid, 3.2 parts by mass of the hydrolyzed liquid of phenyltrimethoxysilane, and 32.3 parts by mass of a silicone compound containing a methyl group and a phenyl group were mixed.
[0217] The IA / IB and the methyl group / phenyl group ratio of the dispersion liquid of Example 6 were measured in the same manner as in Example 1. The results are shown in Table 1.
[0218] Compositions A and B and cured products A and B of Example 6 were obtained in the same manner as in Example 1, except that the dispersion of Example 6 was used instead of the dispersion of Example 1. The viscosities of the compositions and the transmittances of the cured products were measured in the same manner as in Example 1, and the results are shown in Table 1.
[0219] Composition C according to Example 6 and an LED package according to Example 6 were obtained in the same manner as in Example 1, except that the dispersion according to Example 6 was used instead of the dispersion according to Example 1. The results of evaluation performed in the same manner as in Example 1 are shown in Table 1.
[0220] [Example 7] A dispersion liquid of Example 7 was obtained in the same manner as in Example 4, except that instead of mixing 62.5 parts by mass of the second dispersion liquid, 6.3 parts by mass of the hydrolyzed liquid of phenyltrimethoxysilane, and 31.2 parts by mass of the silicone compound containing a methyl group and a phenyl group in Example 4, 65.4 parts by mass of the second dispersion liquid, 2.0 parts by mass of the hydrolyzed liquid of phenyltrimethoxysilane, and 32.6 parts by mass of the silicone compound containing a methyl group and a phenyl group were mixed.
[0221] The IA / IB and the methyl group / phenyl group ratio of the dispersion liquid of Example 7 were measured in the same manner as in Example 1. The results are shown in Table 1.
[0222] Compositions A and B and cured products A and B of Example 7 were obtained in the same manner as in Example 1, except that the dispersion of Example 7 was used instead of the dispersion of Example 1. The viscosities of the compositions and the transmittances of the cured products were measured in the same manner as in Example 1, and the results are shown in Table 1.
[0223] Composition C according to Example 7 and an LED package according to Example 7 were obtained in the same manner as in Example 1, except that the dispersion according to Example 7 was used instead of the dispersion according to Example 1. The results of evaluation in the same manner as in Example 1 are shown in Table 1.
[0224] [Example 8] A dispersion liquid of Example 8 was obtained in the same manner as in Example 4, except that instead of mixing 62.5 parts by mass of the second dispersion liquid, 6.3 parts by mass of the hydrolyzed liquid of phenyltrimethoxysilane, and 31.2 parts by mass of a silicone compound containing a methyl group and a phenyl group in Example 4, 62.9 parts by mass of the second dispersion liquid, 5.7 parts by mass of phenyltrimethoxysilane, and 31.4 parts by mass of a silicone compound containing a methyl group and a phenyl group were mixed.
[0225] The IA / IB and the methyl group / phenyl group ratio of the dispersion liquid of Example 8 were measured in the same manner as in Example 1. The results are shown in Table 1.
[0226] Compositions A and B and cured products A and B of Example 8 were obtained in the same manner as in Example 1, except that the dispersion of Example 8 was used instead of the dispersion of Example 1. The viscosities of the compositions and the transmittances of the cured products were measured in the same manner as in Example 1, and the results are shown in Table 1.
[0227] Composition C according to Example 8 and an LED package according to Example 8 were obtained in the same manner as in Example 1, except that the dispersion according to Example 8 was used instead of the dispersion according to Example 1. The results of evaluation performed in the same manner as in Example 1 are shown in Table 1.
[0228] [Comparative Example 1] A dispersion of Comparative Example 1 (third dispersion) was obtained in exactly the same manner as in Example 1, except that instead of mixing 66.7 parts by mass of the second dispersion, the solid content of which had been adjusted to 15% by mass with toluene, and 33.3 parts by mass of the silicone compound containing a methyl group and a phenyl group, 95.5 parts by mass of the second dispersion and 4.5 parts by mass of the above silicone compound were mixed.
[0229] The IA / IB and the methyl group / phenyl group ratio of the dispersion liquid of Comparative Example 1 were measured in the same manner as in Example 1. The results are shown in Table 1.
[0230] A composition A according to Comparative Example 1 and a cured product A according to Comparative Example 1 were obtained in the same manner as in Example 1, except that the dispersion according to Comparative Example 1 was used instead of the dispersion according to Example 1. The viscosity of the composition and the transmittance of the cured product were measured in the same manner as in Example 1, and the results are shown in Table 1. In the same manner as in Example 1, an attempt was made to obtain composition B and cured product B using the dispersion liquid of Comparative Example 1. However, the dispersion liquid of Comparative Example 1 could not be dispersed in the phenyl-based silicone resin component, and composition B became cloudy and aggregated, so that cured product B could not be produced.
[0231] Composition C according to Comparative Example 1 and an LED package according to Comparative Example 1 were obtained in the same manner as in Example 1, except that the dispersion according to Comparative Example 1 was used instead of the dispersion according to Example 1. The results of evaluation performed in the same manner as in Example 1 are shown in Table 1.
[0232] [Comparative Example 2] A mixing step and a dispersion step were performed in the same manner as in Example 1, except that in the mixing step of Example 1, instead of mixing 70 parts by mass of the hydrolyzed liquid of methyltrimethoxysilane, 20 parts by mass of the hydrolyzed liquid and 50 parts by mass of isopropyl alcohol (IPA) were used, to obtain a dispersion liquid (first dispersion liquid). The solid content of the dispersion (at 100° C. for 1 hour) was measured and found to be 38% by mass.
[0233] (4) First Addition Step Toluene was added to the obtained dispersion (first dispersion) so that the solid content was 20% by mass, and the mixture was heated at 60°C for 2 hours. Next, toluene equivalent to the amount of volatilized was added to the dispersion, and the mixture was heated at 60°C for 2 hours. Next, toluene equivalent to the amount of volatilized was added to the dispersion, and the mixture was heated at 60°C for 1 hour. Next, toluene equivalent to the amount of volatilized was added to the dispersion, and the mixture was heated at 60°C for 1 hour, whereby surface modification was promoted and a dispersion (second dispersion) in which isopropyl alcohol was replaced with toluene was obtained.
[0234] (5) Second Addition Step 89 parts by mass of the second dispersion, the solid content of which had been adjusted to 15% by mass, and 11 parts by mass of a silicone compound containing a methyl group and a phenyl group (product name: KR213 (high phenyl content), manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and heated at 110°C for 1 hour to obtain the dispersion of Comparative Example 2 (third dispersion).
[0235] The IA / IB and the methyl group / phenyl group ratio of the dispersion liquid of Comparative Example 2 were measured in the same manner as in Example 1. The results are shown in Table 1.
[0236] Composition B and cured product B of Comparative Example 1 were obtained in the same manner as in Example 1, except that the dispersion of Comparative Example 2 was used instead of the dispersion of Example 1. The results of viscosity and transmittance measured in the same manner as in Example 1 are shown in Table 1. In the same manner as in Example 1, an attempt was made to obtain composition A and cured product A using the dispersion liquid of Comparative Example 2. However, the dispersion liquid of Comparative Example 2 could not be dispersed in the methyl-based silicone resin component, and composition A became cloudy and aggregated, so that cured product A could not be produced.
[0237] [Comparative Example 3] A dispersion (second dispersion) was obtained by performing the mixing step, the dispersing step, and the first adding step in the same manner as in Example 1, except that in the mixing step of Example 1, 70 parts by mass of the hydrolyzed liquid of phenyltrimethoxysilane obtained in the hydrolysis step of Example 4 was used instead of using 70 parts by mass of the hydrolyzed liquid of methyltrimethoxysilane. 89 parts by mass of the second dispersion liquid, the solid content of which had been adjusted to 15% by mass, and 11 parts by mass of a silicone compound containing a methyl group and a phenyl group (product name: KR213 (high phenyl content), manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed and heated at 110°C for 1 hour to obtain a dispersion liquid of Comparative Example 3 (third dispersion liquid).
[0238] The IA / IB and the methyl group / phenyl group ratio of the dispersion liquid of Comparative Example 3 were measured in the same manner as in Example 1. The results are shown in Table 1.
[0239] Composition B and cured product B of Comparative Example 1 were obtained in the same manner as in Example 1, except that the dispersion of Comparative Example 3 was used instead of the dispersion of Example 1. The results of viscosity and transmittance measured in the same manner as in Example 1 are shown in Table 1. In the same manner as in Example 1, an attempt was made to obtain composition A and cured product A using the dispersion liquid of Comparative Example 3. However, the dispersion liquid of Comparative Example 3 could not be dispersed in the methyl-based silicone resin component, and composition A became cloudy and aggregated, so that cured product A could not be produced.
[0240] [Comparative Example 4] A dispersion (second dispersion) was obtained by performing the mixing step, the dispersing step, and the first adding step in the same manner as in Example 1, except that in the mixing step of Example 1, 70 parts by mass of the above-mentioned phenyltrimethoxysilane hydrolyzed liquid was used instead of using 70 parts by mass of the methyltrimethoxysilane hydrolyzed liquid. 91 parts by mass of the second dispersion liquid, the solid content of which was adjusted to 15% by mass, and 9 parts by mass of the above-mentioned methyltrimethoxysilane hydrolyzate liquid were mixed and stirred at 130°C for 3 hours, thereby obtaining a dispersion liquid of Comparative Example 4 (third dispersion liquid).
[0241] The IA / IB and the methyl group / phenyl group ratio in Comparative Example 4 were measured in the same manner as in Example 1. The results are shown in Table 1.
[0242] An attempt was made to obtain a composition and a cured product according to Comparative Example 4 in the same manner as in Example 1, except that the dispersion according to Comparative Example 4 was used instead of the dispersion according to Example 1. However, the dispersion according to Comparative Example 4 could not disperse either the methyl-based silicone resin or the phenyl-based silicone resin, and both compositions A and B became cloudy and flocculated. Therefore, neither the cured product A nor the cured product B could be produced.
[0243] [Table 1]
[0244] By comparing Examples 1 to 8 and Comparative Examples 1 to 4, it was confirmed that zirconium oxide particles that have been sufficiently surface-modified with a silane compound containing a methyl group and a silicone compound containing a phenyl group, such that the methyl group / phenyl group ratio is 0.01 or more and 10 or less, and that satisfies IA / IB≦3.5, are well dispersed in both methyl-based phenyl silicone resins containing many methyl groups and phenyl-based silicone resins containing many phenyl groups. Furthermore, by comparing Examples 1 to 3 with Examples 4 to 8, it was confirmed that zirconia particles surface-modified with a silane compound containing a methyl group and a phenyl group and a silicone compound containing a methyl group and a phenyl group further improve the brightness of the LED package.
[0245] Although the preferred embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention. [Explanation of symbols]
[0246] 1A, 1B, 1C, 1D Light-emitting device 2. Board 21 Recess 3 Light emitting element 4A, 4B, 4C, 4D Sealing material 41B, 41C, 41D 1st layer 43B, 43C, 43D Second layer 45D 3rd Layer 5. Phosphor particles
Claims
1. A dispersion liquid comprising metal oxide particles surface-modified with a silane compound and a silicone compound, and a solvent, The silane compound contains a methyl group, The silicone compound contains an aromatic hydrocarbon group, a molar ratio of the methyl groups to the aromatic hydrocarbon groups (methyl groups / aromatic hydrocarbon groups) is 0.01 or more and 10 or less, The metal oxide particles obtained by drying the dispersion liquid by vacuum drying were measured using a Fourier transform infrared spectrophotometer at 800 cm -1 More than 3800cm -1 A dispersion that satisfies the following formula (1) when a transmission spectrum is measured in the following wave number range and the spectrum value is normalized so that the maximum value of the spectrum in the range is 100 and the minimum value of the spectrum in the range is 0: IA / IB≦3.5 (1) (Wherein, "IA" is 3500 cm -1 The spectral value at 1100 cm -1 The spectral values at are shown.)
2. The dispersion liquid described in claim 1, wherein the total content of the silane compound and the silicone compound relative to the metal oxide particles is 190 mass% or more and 1000 mass% or less.
3. A composition which is a mixture of the dispersion of claim 1 or 2 and a silicone resin component.
4. A sealing member which is a cured product of the composition according to claim 3.
5. A light emitting device comprising: the sealing member according to claim 4; and a light emitting element sealed with the sealing member.
6. A lighting fixture comprising the light emitting device according to claim 5.
7. A display device comprising the light emitting device according to claim 5 .
Citation Information
Patent Citations
High refractive index thermoplastic organic-inorganic hybrid material and production method thereof
JP2013133430A
Inorganic oxide particle dispersion liquid, resin composition, master batch, resin composite, and optical semiconductor light-emitting device
JP2016175804A
Dispersion liquid, composition, sealing member, light-emitting device, lighting apparatus and display device
JP2020002306A
Dispersion, composition, sealing member, light emitting device, lighting fixture and display device and method for producing dispersion
JP2020125427A
Composition for forming light scattering composite body, light scattering composite body and method for producing same
WO2016142992A1