Exothermic materials
A heat dissipating material with controlled graphene thickness and N/C ratio, combined with polyvinyl alcohol resin and surface treatment, addresses dispersibility issues, achieving high thermal conductivity and mechanical strength.
Patent Information
- Application Number
- JP2020180233
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-28
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-10-28
AI Technical Summary
Existing heat dissipating materials using graphene in resins suffer from insufficient dispersibility, limiting the improvement in thermal conductivity.
A heat dissipating material comprising resin and graphene with specific thickness and nitrogen-to-carbon ratio (N/C) is developed, enhancing dispersibility and thermal conductivity by using polyvinyl alcohol resin and surface treatment agents to improve graphene dispersion.
The material achieves lightweight and high thermal conductivity, with improved mechanical strength and flexibility, forming efficient heat conduction paths through surface contact.
Smart Images

Figure 0007559501000001 
Figure 0007559501000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a heat dissipation material containing a resin and graphene. [Background technology]
[0002] In recent years, there has been a demand for smaller, more dense, and lighter electronic devices, such as portable devices like smartphones and laptops, LED lighting equipment, and power semiconductors. These electronic devices are required to efficiently dissipate the heat generated by the electrical devices in order to reduce malfunctions caused by heat.
[0003] As a heat dissipation material, a thermally conductive composition in which a metal filler is dispersed in a resin is known. In order to further improve the thermal conductivity of such a heat conductive composition, it is effective to increase the amount of the metal filler, but there is a problem that the heat dissipation material becomes hard and the weight increases.
[0004] In recent years, as thermally conductive compositions using graphene, there have been proposed an electrically insulating thermally conductive composition containing 5 to 80 parts by weight of a resin, 20 to 95 parts by weight of an electrically insulating thermally conductive powder, and 0.0001 to 2 parts by weight of graphene (see, for example, Patent Document 1), and a polycarbonate resin composition containing 70 to 99.5 mass% of a polycarbonate-based resin (A) in which a mass ratio of a polycarbonate-polyorganosiloxane copolymer (A-1) to an aromatic polycarbonate (A-2) other than (A-1) is 5:95 to 100:0, and 30 to 0.5 mass% of a graphene sheet (B) (see, for example, Patent Document 2). In addition, a heat dissipation film has been proposed, which is composed of a heat transfer layer containing graphene fine particles and a binder resin, and a plastic film bonded to at least one surface of the heat transfer layer, and the thickness of the heat transfer layer is 30 to 250 g / m. 2A heat dissipation film (see, for example, Patent Document 3) has been proposed, which is characterized in that a mass ratio of the binder resin to the graphene fine particles in the heat transfer layer is 0.001 to 0.1, and the graphene fine particles in the heat transfer layer are oriented substantially parallel to the plastic film. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-188645 A [Patent Document 2] International Publication No. 2012 / 173111 [Patent Document 3] JP 2014-127518 A Summary of the Invention [Problem to be solved by the invention]
[0006] Graphene is a carbon material having a planar structure, and is known to have excellent thermal conductivity. For example, inorganic fine particles made of alumina or other aggregate particles conduct heat by point contact, whereas graphene having a planar structure can contact by surface, and therefore it is considered that it can conduct heat efficiently. However, graphene generally tends to have lower dispersibility in resin than inorganic fine particles, and if the dispersibility is insufficient, the effect of improving thermal conductivity by surface contact cannot be sufficiently obtained. The techniques described in Patent Documents 1 to 3 have insufficient dispersibility of graphene in resin, and further improvement of thermal conductivity has been required.
[0007] Therefore, an object of the present invention is to provide a heat dissipation material that is lightweight and has excellent thermal conductivity. [Means for solving the problem]
[0008] In order to solve the above problems, the present invention provides a heat dissipation material containing a resin and graphene, wherein the graphene has an average thickness of 0.3 nm or more and 20 nm or less, and an elemental ratio of nitrogen to carbon (N / C ratio) measured by X-ray photoelectron spectroscopy of 0.005 or more and 0.020 or less. Effect of the Invention
[0009] The heat dissipation material of the present invention is lightweight and has excellent thermal conductivity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The heat dissipation material of the present invention contains a resin and graphene. It may further contain inorganic fine particles. The resin is a structural material of the heat dissipation material, and imparts physical properties such as mechanical strength, flexibility, adhesiveness, and heat resistance as necessary, and also plays a role in fixing the heat conduction path formed by the graphene and inorganic fine particles. Graphene is a lightweight material with excellent thermal conductivity, and has a thin sheet-like structure, so it plays a role in efficiently forming a heat conduction path. In addition, the inorganic fine particles are also a structural material with excellent thermal conductivity, and when used in combination with graphene, they play a role in further improving thermal conductivity.
[0011] <Resin> Examples of the resin include thermoplastic resins, thermosetting resins, rubber, silicone resins, etc., and can be selected according to the desired properties such as mechanical strength, flexibility, adhesiveness, heat resistance, etc. Two or more of these may be contained.
[0012] Examples of thermoplastic resins include vinyl resins, ABS resins, polycarbonate resins, polyamide resins, polyimide resins, polyacrylate resins, polyacetal resins, polyester resins, polyphenylene sulfide resins, and polyether ether ketone resins. Examples of vinyl resins include polyolefin resins such as polyethylene and polypropylene, polystyrene resins, polyvinyl acetate resins, and polyvinyl alcohol resins. Examples of polyester resins include polyethylene terephthalate resins, polybutylene terephthalate resins, and polyethylene naphthalate resins.
[0013] Examples of the thermosetting resin include epoxy resin, urethane resin, and phenol resin.
[0014] It is preferable to select a resin from among these according to the desired characteristics. For example, polyacrylate resins and silicone resins are preferable for imparting adhesiveness and tackiness to the heat dissipation material, polyimide resins and polycarbonate resins are preferable for improving the strength of the heat dissipation material, and thermosetting resins are preferable for improving the heat resistance of the heat dissipation material.
[0015] Among these, from the viewpoints of having better affinity with the surface-treated graphene described below and further improving the dispersibility of graphene to further improve thermal conductivity, vinyl resin, ABS resin, polycarbonate resin, polyamide resin, polyimide resin, polyacrylate resin, polyester resin, polyphenylene sulfide resin, epoxy resin, urethane resin, silicone resin, and phenol resin are preferred, vinyl resin, polyamide resin, polyimide resin, polyacrylate resin, polyester resin, epoxy resin, urethane resin, and phenol resin are more preferred, and vinyl resin, polyimide resin, polyacrylate resin, and epoxy resin are even more preferred.
[0016] As the vinyl resin, polyvinyl alcohol resin is preferable because it has a better affinity with graphene. Although only polyvinyl alcohol resin may be contained as the resin, it is preferable to contain polyvinyl alcohol resin together with the above-mentioned resin, which can further improve the dispersibility of graphene and further improve the affinity with the resin contained together with the polyvinyl alcohol resin. In particular, the graphene used in the present invention having an element ratio of nitrogen to carbon (N / C ratio) of 0.005 to 0.020 has polyvinyl alcohol resin present in its vicinity due to interactions such as hydrogen bonds between oxygen-containing functional groups of graphene and / or functional groups of the surface treatment agent and hydroxyl groups of the polyvinyl alcohol resin, so that the dispersibility of graphene can be further improved and the thermal conductivity of the heat dissipation material can be further improved.
[0017] The saponification rate of the polyvinyl alcohol resin is preferably 70% or more and 100% or less. By setting the saponification rate in this range, the dispersibility of graphene can be further improved, and the thermal conductivity of the heat dissipation material can be improved. By setting the saponification rate of the polyvinyl alcohol resin to 70% or more, the dispersibility of graphene can be further improved, and the heat conduction path in the heat dissipation material can be more easily formed, and therefore the thermal conductivity can be further improved. The saponification rate of the polyvinyl alcohol resin is more preferably 75% or more, more preferably 80% or more, and even more preferably 85% or more. On the other hand, when the heat dissipation material contains a resin other than the polyvinyl alcohol resin, from the viewpoint of further improving the affinity with the resin other than the polyvinyl alcohol resin and further improving the thermal conductivity of the heat dissipation material, the saponification rate of the polyvinyl alcohol is preferably 99.9% or less, more preferably 98% or less, and even more preferably 95% or less. Here, the saponification rate of the polyvinyl alcohol resin can be determined according to JIS K6726-1994.
[0018] The polyvinyl alcohol resin may be an unmodified polyvinyl alcohol resin or a modified polyvinyl alcohol resin.
[0019] Examples of unmodified polyvinyl alcohol resins include those under the trade name "Kuraray Poval" (registered trademark) (Kuraray Co., Ltd.), those under the trade name "GOHSENOL" (registered trademark) (Mitsubishi Chemical Corporation), those under the trade name "Denka Poval" (registered trademark) (Denka Co., Ltd.), and those under the trade name "J-Poval" (Nippon Vinyl Acetate & Poval Co., Ltd.).
[0020] Examples of modified polyvinyl alcohol resins include those having a carboxyl group, a sulfonic acid group, a cationic group (quaternary ammonium salt), or an ethylene oxide group in the side chain, such as the L, T, and WO series under the trade name "Gohsenx" (Mitsubishi Chemical Corporation). From the viewpoint of further improving the dispersibility of graphene, among these, those having a carboxyl group or a sulfonic acid group in the side chain are more preferred, such as the T series or L series under the trade name "Gohsenx" (Mitsubishi Chemical Corporation). Those having a sulfonic acid group are even more preferred, such as the L series under the trade name "Gohsenx" (Mitsubishi Chemical Corporation).
[0021] The degree of polymerization of the polyvinyl alcohol resin is preferably 100 or more, more preferably 200 or more, and even more preferably 300 or more, from the viewpoint of further improving the dispersibility of graphene and further improving the thermal conductivity of the heat dissipation material. On the other hand, when the heat dissipation material contains a resin other than the polyvinyl alcohol resin, the degree of polymerization of the polyvinyl alcohol resin is preferably 10,000 or less, more preferably 5,000 or less, and even more preferably 1,000 or less, from the viewpoint of further improving the affinity with the resin other than the polyvinyl alcohol and further improving the thermal conductivity of the heat dissipation material. Here, the degree of polymerization of the polyvinyl alcohol resin can be determined according to JIS6726-1994.
[0022] Two or more kinds of polyvinyl alcohol resins may be contained. In such a case, it is preferable that the saponification rate and polymerization degree of the two or more kinds of polyvinyl alcohol resins as a whole are within the above-mentioned ranges.
[0023] When the heat dissipation material of the present invention contains a polyvinyl alcohol resin as a resin, it is preferable that the polyvinyl alcohol resin is contained in an amount of 5 parts by weight or more and 300 parts by weight or less relative to 100 parts by weight of graphene. If the content of the polyvinyl alcohol resin is 5 parts by weight or more, the dispersibility of graphene can be further improved, and the thermal conductivity of the heat dissipation material can be further improved. The content of the polyvinyl alcohol resin is preferably 10 parts by weight or more, more preferably 20 parts by weight or more. On the other hand, if the content of the polyvinyl alcohol resin is 300 parts by weight or less, the thermal conductivity of graphene is not easily inhibited. From the viewpoint of further increasing the thermal conductivity, the content of the polyvinyl alcohol resin is preferably 300 parts by weight or less, more preferably 200 parts by weight or less, and even more preferably 150 parts by weight or less.
[0024] The contents of graphene and polyvinyl alcohol resin in the heat dissipation material of the present invention can be determined from the raw material composition when the raw material composition used in the heat dissipation material is known.
[0025] <Graphene> Next, the graphene used in the present invention will be described.
[0026] Graphene is, in the strictest sense, a one-atom-thick sp 2 It refers to a sheet of bonded carbon atoms (single-layer graphene), but in this specification, the term graphene also refers to a flaky form of stacked single-layer graphene. Similarly, graphene oxide is also referred to as a flaky form of stacked graphene. Graphene, as a thermally conductive filler, has a thin layer shape and many thermal conduction paths per unit weight, and it is easy to form a good thermally conductive network in a heat dissipation material.
[0027] In this specification, graphene oxide is defined as a material having an O / C ratio, which is the atomic ratio of oxygen atoms to carbon atoms, measured by X-ray photoelectron spectroscopy (XPS), of more than 0.4, and graphene is defined as a material having an O / C ratio of 0.4 or less. Reduced graphene oxide obtained by reducing graphene oxide and having an O / C ratio of 0.4 or less is also defined as graphene.
[0028] Furthermore, graphene and graphene oxide may be subjected to a surface treatment for the purpose of improving dispersibility, etc., and in this specification, graphene or graphene oxide having such a surface treatment agent attached thereto will also be referred to as "graphene" or "graphene oxide".
[0029] The graphene in the present invention has an average thickness of 0.3 nm or more and 20 nm or less, and an element ratio of nitrogen to carbon (N / C ratio) measured by X-ray photoelectron spectroscopy of 0.005 or more and 0.020 or less.
[0030] In heat dissipation materials, when thin graphene is well dispersed in a resin, it has the property of easily forming a heat conduction path due to surface contact between graphene particles. On the other hand, thin graphene has a tendency to easily aggregate in a resin due to its large specific surface area, and even when thin graphene is applied to a conventionally known heat dissipation material, the dispersibility and thermal conductivity are insufficient. Therefore, in the present invention, by using graphene having an element ratio of nitrogen to carbon (N / C ratio) measured by XPS within a specific range as the thin graphene, the dispersibility of graphene in a resin can be improved, a heat conduction path can be efficiently formed, and the thermal conductivity of the heat dissipation material can be greatly improved.
[0031] The average thickness of graphene is 0.3 nm or more and 20 nm or less. The average thickness of graphene in the present invention refers to the arithmetic average value of the thicknesses of 10 graphenes randomly selected in the heat dissipation material. The average thickness of graphene is substantially the minimum value of 0.3 nm, which indicates that it is a single layer with a thickness of one carbon atom. From the viewpoint of further improving the thermal conductivity of the heat dissipation material, the average thickness of graphene is more preferably 0.6 nm or more, and even more preferably 1.8 nm or more. On the other hand, if the average thickness of graphene exceeds 20 nm, the dispersibility decreases and the thermal conductivity of the heat dissipation material decreases. In addition, graphene tends to be rigid, and when the heat dissipation material further contains inorganic fine particles, it is difficult to contact with the inorganic fine particles, so that the formation of a heat conduction path becomes insufficient and the thermal conductivity decreases. From the viewpoint of further improving the dispersibility of graphene and further improving the thermal conductivity of the heat dissipation material, the average thickness of graphene is preferably 10 nm or less, more preferably 8 nm or less, and even more preferably 6 nm or less. Here, the average thickness of graphene in the heat dissipation material can be calculated by enlarging and observing the cross section of the heat dissipation material using a transmission electron microscope (TEM), measuring the thickness of each of ten randomly selected graphene points, and calculating the arithmetic average value. Note that the thickness of each graphene is the arithmetic average value of the thickness measurements at five randomly selected points on each graphene.
[0032] As a method for adjusting the average thickness of graphene to fall within the above range, for example, a method for manufacturing a heat dissipation member described later, particularly a method for mixing a graphene dispersion with a resin using a preferred mixing device described later in the step (step 2) of mixing the graphene dispersion with a resin, may be mentioned. Alternatively, commercially available graphene oxide or graphene having a desired average thickness may be used.
[0033] As described above, graphene and graphene oxide may be surface-treated, and in particular, a surface treatment agent containing nitrogen atoms tends to increase the dispersibility of graphene. Furthermore, the surface treatment agent enhances the interaction between the resin and graphene, and can further improve the dispersibility of graphene and the binding strength between graphene and other components.
[0034] When graphene is treated with a surface treatment agent containing nitrogen atoms, the amount of the surface treatment agent attached to the graphene can be determined from the atomic ratio of nitrogen to carbon (N / C ratio) measured by XPS. The N / C ratio of graphene in the present invention is 0.005 or more and less than 0.020. When the N / C ratio of graphene is less than 0.005, the dispersibility decreases, the formation of the heat conduction path in the heat dissipation material becomes insufficient, and the thermal conductivity decreases. From the viewpoint of further improving the dispersibility of graphene and further improving the thermal conductivity of the heat dissipation material, the N / C ratio is preferably 0.006 or more, more preferably 0.008 or more. On the other hand, when the N / C ratio of graphene exceeds 0.020, aggregation of graphene particles easily occurs, and therefore the thermal conductivity of the heat conduction path formed by graphene, that is, the thermal conductivity at the contact point between graphenes or between graphene and inorganic fine particles, decreases. From the viewpoint of further improving the thermal conductivity of the heat dissipation material, the N / C ratio of graphene is preferably 0.018 or less, more preferably 0.016 or less. Here, the N / C ratio of graphene can be measured by collecting graphene from the heat dissipation material and using XPS. The C1s main peak based on carbon atoms is set to 284.3 eV, and the N1s peak based on nitrogen atoms is assigned to a peak near 402 eV. The N / C ratio is calculated from the area ratio of each peak, and the value obtained is rounded off to the fourth decimal place to the third decimal place. The N / C ratio of graphene can be easily adjusted to the above-mentioned range, for example, by the amount of the surface treatment agent to be described later.
[0035] The surface treatment agent is attached to the surface of graphene and has the effect of further increasing the dispersibility of graphene. In this specification, graphene with such a surface treatment agent attached thereto may be referred to as "surface-treated graphene". Here, in the present invention, "the surface treatment agent is attached to graphene" means that the surface treatment agent remains in the surface-treated graphene after a washing step of dispersing the surface-treated graphene in 100 times the mass ratio of water and filtering the same is repeated five or more times, and then the surface-treated graphene is dried by a method such as freeze-drying or spray-drying. The surface treatment agent remains means that the surface treatment agent molecules can be detected in the form of proton-added molecules in the positive secondary ion spectrum when the surface-treated graphene after drying is analyzed by time-of-flight secondary ion mass spectrometry (TOF-SIMS). However, when the surface treatment agent is a neutralized salt, it can be detected in the form of protons added to the surface treatment agent molecules from which anion molecules have been removed. The chemical structure of the surface treatment agent contained in the surface-treated graphene can be identified by TOF-SIMS. The amount of the surface treatment agent is quantified using a sample obtained by repeating a washing process of dispersing the surface-treated graphene in 100 times its mass of water and filtering it five or more times, and then freeze-drying the resultant.
[0036] From the viewpoint of ease of adsorption to the graphene surface, the surface treatment agent is preferably a compound having an aromatic ring, and more preferably further having a basic group, preferably an amino group.
[0037] Examples of the compound having an amino group and an aromatic ring include benzylamine, phenylethylamine, dopamine, and salts thereof. Some of the hydrogen atoms in these compounds may be substituted.
[0038] The size of the graphene in the direction parallel to the graphene layer is preferably 0.10 μm or more, and the thermal conductivity of the heat dissipation material can be further improved. In addition, when the heat dissipation material contains inorganic fine particles described later, a heat conduction path bridging between the inorganic fine particles can be more effectively formed, and the thermal conductivity can be further improved. The size of the graphene is more preferably 0.50 μm or more, and more preferably 1 μm or more. On the other hand, the size of the graphene in the direction parallel to the graphene layer is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 20 μm or less, from the viewpoint of further improving the dispersibility of the graphene and further improving the thermal conductivity of the heat dissipation material. Here, the size of the graphene in the direction parallel to the graphene layer can be calculated by observing the cross section of the heat dissipation material with a transmission electron microscope (TEM), observing the cross section of each of the graphenes at 10 randomly selected graphenes, measuring the length in the direction parallel to the graphene layer, and calculating the arithmetic average value, in the same manner as in the measurement method of the average thickness of graphene.
[0039] The size of the graphene in the direction parallel to the graphene layer can be easily adjusted to the above-mentioned range by micronizing the graphene oxide or reduced graphene by a method described later. Alternatively, commercially available graphene oxide or graphene of a desired size may be used.
[0040] The element ratio of oxygen to carbon (O / C ratio) of graphene measured by XPS is preferably 0.05 or more, more preferably 0.07 or more, and even more preferably 0.08 or more, from the viewpoint of further improving dispersibility by residual functional groups and further improving binding with resin. On the other hand, from the viewpoint of maintaining high thermal conductivity of graphene, the O / C ratio is preferably 0.35 or less, more preferably 0.20 or less, and even more preferably 0.15 or less. Here, the O / C ratio of graphene in the graphene dispersion can be measured by XPS after collecting graphene from a heat dissipation material. The C1s main peak based on carbon atoms is set to 284.3 eV, and the O1s peak based on oxygen atoms is assigned to a peak near 533 eV, and the O / C ratio is calculated from the area ratio of each peak, and the obtained value is rounded off to two decimal places to obtain the value. In addition, when a chemical peeling method is used, the O / C ratio of graphene can be easily adjusted to the above-mentioned range by adjusting the oxidation degree of the graphene oxide as a raw material or the reduction degree by the reduction reaction conditions. In addition, commercially available graphene oxide or graphene having a desired O / C ratio may be used.
[0041] The content of graphene in the heat dissipating material of the present invention is preferably 0.1 parts by weight or more, more preferably 0.5 parts by weight or more, and even more preferably 1 part by weight or more, relative to 100 parts by weight of the resin, from the viewpoint of further improving thermal conductivity. On the other hand, the content of graphene is preferably 20 parts by weight or less, more preferably 15 parts by weight or less, and even more preferably 10 parts by weight or less, relative to 100 parts by weight of the resin, from the viewpoint of improving the mechanical properties of the heat dissipating material.
[0042] The graphene used in the present invention may be one produced by a physical exfoliation method and then surface-treated, or may be one produced by a chemical exfoliation method including a surface treatment step. When produced by a chemical exfoliation method, the method for producing graphene oxide is not particularly limited, and a known method such as the Hummers method can be used. In addition, commercially available graphene oxide may be purchased.
[0043] <Inorganic fine particles> The heat dissipating material of the present invention may further contain inorganic fine particles in addition to the resin and graphene. Conventional heat dissipating materials using inorganic fine particles have insufficient thermal conductivity between inorganic fine particles, so in order to obtain the desired thermal conductivity, it is necessary to contain a large amount of inorganic fine particles that have a large specific gravity and are rigid, making it difficult to make the heat dissipating material lightweight and flexible. On the other hand, the heat dissipating material of the present invention has graphene as a bridge between the inorganic fine particles, so the content of the inorganic fine particles can be reduced and the distance between the inorganic fine particles can be increased, making it possible to make the heat dissipating material lightweight, thin, and flexible.
[0044] Examples of materials constituting the inorganic fine particles include aluminum oxide, aluminum nitride, magnesium nitride, zinc oxide, boron nitride, silicon carbide, silicon dioxide, beryllium oxide, diamond, tungsten carbide, and titanium oxide. Two or more of these may be used. Among these, aluminum oxide, aluminum nitride, zinc oxide, boron nitride, diamond, and titanium oxide are more preferable from the viewpoint of further improving thermal conductivity.
[0045] In the present invention, the inorganic fine particles refer to those having an average particle size of 100 μm or less. From the viewpoint of improving dispersibility in the heat dissipation material and further improving thermal conductivity, the average particle size of the inorganic fine particles is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more. On the other hand, from the viewpoint of maintaining the mechanical strength of the heat dissipation material, the average particle size of the inorganic fine particles is preferably 50 μm or less, more preferably 30 μm or less.
[0046] Here, the average particle size of inorganic fine particles refers to the particle size at an integrated value of 50% on a particle size distribution curve measured by a particle size distribution measuring device.
[0047] The content of inorganic fine particles in the heat dissipating material of the present invention is preferably 5% by volume or more, more preferably 10% by volume or more, and even more preferably 15% by volume or more, from the viewpoint of further improving thermal conductivity. Also, from the viewpoint of maintaining the mechanical strength of the heat dissipating material, the content of inorganic fine particles is preferably 70% by volume or less, more preferably 60% by volume or less, and even more preferably 50% by volume or less. Here, the volume % of the inorganic fine particles mixed in the heat dissipating material can be calculated by calculating the volume of the inorganic fine particles from the weight and density of the inorganic fine particles and dividing it by the volume of the entire heat dissipating material.
[0048] In addition to the above-mentioned components, the heat dissipating material of the present invention may contain additives such as a polymerization initiator, a curing agent, a flame retardant, and a plasticizer, if necessary.
[0049] The thermal conductivity of the heat dissipating material of the present invention is preferably 1.0 W / m·K or more, more preferably 1.2 W / m·K or more, and even more preferably 1.4 W / m·K or more. The higher the thermal conductivity, the better, and is not particularly limited. When the heat dissipating material of the present invention contains inorganic fine particles, the thermal conductivity is preferably 1.4 W / m·K or more, more preferably 2.0 W / m·K or more, and even more preferably 2.5 W / m·K or more. The higher the thermal conductivity, the better, and is not particularly limited. The thermal conductivity of the heat dissipating material of the present invention can be easily adjusted to the above-mentioned range, for example, by using the above-mentioned preferred graphene, or by adjusting the content of graphene and / or inorganic fine particles to the above-mentioned preferred range.
[0050] <Method of manufacturing heat dissipation material> The method for producing a heat dissipation material of the present invention preferably includes a step of producing a graphene dispersion (step 1) and a step of mixing the graphene dispersion with a resin (step 2). Since graphene is generally prone to irreversible aggregation when dried into a powder, it is preferable to mix it with a resin in the form of a dispersion.
[0051] <Step 1: Producing a graphene dispersion> The graphene dispersion preferably contains the above-mentioned graphene and a solvent. As the solvent, a polar solvent is preferable from the viewpoint of excellent dispersibility of graphene. From the viewpoint of affinity with the resin, N,N-dimethylformamide, N-methylpyrrolidone, N,N-dimethylacetamide, etc. are preferable. Two or more of these may be contained. Among these, N-methylpyrrolidone is preferable, and dispersibility can be further improved by solvating the surface treatment agent attached to the graphene.
[0052] A method for producing a graphene dispersion will be described below, taking as an example a case where graphene is produced by a chemical exfoliation method. It is preferable to have a step of obtaining graphene oxide by oxidatively exfoliating graphite (graphite exfoliation step) and a step of performing reduction (reduction step) in this order. If necessary, a step of attaching a surface treatment agent to graphene (surface treatment step) and / or a step of adjusting the size of graphene in a direction parallel to the graphene layer (fine-refining step) may be further included between the graphite exfoliation step and the reduction step. When surface-treated graphene is used, the surface treatment agent may be attached to graphene, or the surface-treated graphene may be obtained by performing a reduction treatment after attaching the surface treatment agent to graphene oxide. In addition, when graphene is fine-refined, the graphene oxide may be fine-refined, or the graphene after reduction may be fine-refined. From the viewpoint of uniformity of the reduction reaction, it is preferable to perform the reduction step in a fine-refined state of graphene oxide, and it is preferable to perform the fine-refining step before or during the reduction step. For this reason, it is preferable to include the graphite exfoliation step, the surface treatment step, the fine-refining step, and the reduction step in this order.
[0053] [Graphite peeling process] First, graphene oxide is obtained by oxidatively exfoliating graphite. As the conditions for oxidative exfoliation, the Hummers method, the modified Hummers method, or the like can be used. The oxidation degree of graphene oxide can be adjusted by changing the amount of oxidizing agent used in the oxidation reaction of graphite. Specifically, the greater the amount of sodium nitrate and potassium permanganate used in the oxidation reaction relative to graphite, the higher the oxidation degree, and the smaller the amount, the lower the oxidation degree. The weight ratio of sodium nitrate to graphite is preferably 0.200 or more and 0.800 or less. The ratio of potassium permanganate to graphite is preferably 1.00 or more and 4.0 or less.
[0054] [Surface treatment process] Next, the graphene oxide and the surface treatment agent are mixed to adhere the surface treatment agent to the graphene. Examples of the mixing method include a method of mixing using a mixer or kneader such as an automatic mortar, a triple roll, a bead mill, a planetary ball mill, a homogenizer, a homodisper, a homomixer, a planetary mixer, or a twin-screw kneader.
[0055] [Refining process] Next, the graphene oxide is refined. Examples of the refinement method include a method of colliding a dispersion liquid to which pressure has been applied with a single ceramic ball, a method of using a liquid-liquid shear type wet jet mill in which dispersion liquids to which pressure has been applied are collided with each other to perform dispersion, and a method of applying ultrasonic waves to the dispersion liquid. In the refinement step, the graphene oxide or graphene tends to be refined as the processing pressure and output are higher, and the graphene tends to be refined as the processing time is longer. The size of the graphene after reduction can be adjusted by the type, processing conditions, and processing time of the refinement process in the refinement step. In order to adjust the size parallel to the graphene layer to the above-mentioned range, the solid content concentration of the graphene oxide or graphene in the refinement step is preferably 0.01% by weight or more and 2% by weight or less. In addition, when performing ultrasonic treatment, the ultrasonic output is preferably 100 W or more and 3000 W or less.
[0056] [Reduction process] Next, the fine graphene oxide is reduced. A preferable reduction method is chemical reduction. In the case of chemical reduction, examples of the reducing agent include organic reducing agents and inorganic reducing agents. Among these, inorganic reducing agents are more preferable from the viewpoint of ease of cleaning after reduction, and sodium dithionite, potassium dithionite, etc. are more preferable.
[0057] After the reduction step, the purity of the graphene can be improved by a washing step, preferably by dilution with water and filtration.
[0058] The graphene obtained after the reduction step is preferably redispersed in the above-mentioned solvent without drying. After redispersion in the solvent, it is preferable to remove water by distillation or to perform solvent replacement by repeating dispersion in the solvent and filtration.
[0059] <Step 2: Mixing graphene dispersion and resin> Examples of the method for mixing the graphene dispersion and the resin include a method of adding the resin to the graphene dispersion and mixing it, and a method of adding a dispersion or solution in which the resin is dispersed or dissolved in an appropriate solvent to the graphene dispersion and mixing it, etc. As a mixing device, a device capable of applying a shear force is preferable, and examples thereof include a planetary mixer, "Filmix" (registered trademark) (Primix Corporation), a self-revolving mixer, a planetary ball mill, and a three-roll mill.
[0060] From the viewpoint of suppressing aggregation of graphene, it is preferable to use a wet process, and for example, it is preferable that graphene is mixed in the state of a dispersion with the resin solution.
[0061] In the case where the resin contains a polyvinyl alcohol resin and another resin, the graphene dispersion may be mixed with the polyvinyl alcohol resin and then the other resin may be mixed, or the polyvinyl alcohol resin may be mixed into a solution in which the graphene dispersion and the other resin are mixed. The polyvinyl alcohol resin is preferably added as a polyvinyl alcohol resin solution. From the viewpoint of more uniformly mixing the graphene and the other resin, a method in which the graphene dispersion and the polyvinyl alcohol resin solution are mixed and then the other resin is mixed is preferred. The above-mentioned mixing device is preferably used for mixing the graphene dispersion and the polyvinyl alcohol resin solution.
[0062] In the process of mixing the graphene dispersion and the resin, a high shear mixer may be used to perform a strong stirring process at a shear rate of 5,000 to 50,000 per second. By peeling off the graphene with a high shear mixer, stacks of graphene can be eliminated, and the average thickness of graphene can be easily adjusted to the above-mentioned preferred range. As the high shear mixer, a thin film rotation type, a rotor / stator type, or a media mill type is preferably used, and examples of such high shear mixers include "Filmix" (registered trademark) 30-30 type (Primix Corporation), "Clearmix" (registered trademark) CLM-0.8S (M Technique Co., Ltd.), "Labostar" (registered trademark) Mini LMZ015 (Ashizawa Finetech Co., Ltd.), and Super Shear Mixer SDRT0.35-0.75 (Satake Chemical Machinery Co., Ltd.).
[0063] As described above, the shear rate in the strong stirring treatment is preferably 5,000 to 50,000 per second. By setting the shear rate at 5,000 or more per second, the peeling of graphene is promoted, and the average thickness of graphene can be easily adjusted to the above-mentioned range. In addition, the strong stirring treatment time is preferably 15 seconds or more and 300 seconds or less.
[0064] In addition, when the graphene dispersion becomes highly viscous and mixing with a stirring blade is difficult, for example, a propellerless type rotation-revolution mixer can be used. Examples of the propellerless rotation-revolution mixer include "Awatori Rentaro" (registered trademark) manufactured by Thinky Corporation and "Kakuhunter" (registered trademark) manufactured by Shashin Kagaku Co., Ltd. The rotation speed is preferably 1000 rpm or more, more preferably 2000 rpm or more, and the treatment time is preferably 5 minutes or more, more preferably 10 minutes or more, and even more preferably 15 minutes or more.
[0065] The heat dissipating material of the present invention may be molded into a desired shape for use. The shape of the heat dissipating material of the present invention is not particularly limited, and may be, for example, a sheet or pellet. It may be molded into a complex shape according to the shape of the object of application. From the viewpoint of excellent handling such as application by utilizing the light weight and flexibility of the heat dissipating material of the present invention, it is preferable that the heat dissipating material be in a sheet shape.
[0066] When the heat-dissipating material of the present invention contains a polymerization initiator and a curing agent, the heat-dissipating material may be cured by any curing method before use. EXAMPLES
[0067] The present invention will be described below with reference to examples. First, the evaluation methods used in the examples and comparative examples will be described.
[0068] [Measurement Example 1: Graphene thickness and size of graphene in the plane direction parallel to the graphene layer] The heat dissipation materials prepared in each Example and Comparative Example were milled with an ion milling device (IM4000, manufactured by Hitachi, Ltd.), and a cross section of the heat dissipation material was exposed to prepare a measurement sample. This sample was observed using a transmission electron microscope (JEM-ARM200F, manufactured by JEOL Ltd.), and the thickness of each of 10 randomly selected graphenes in the heat dissipation material was measured, and the average thickness of the graphene was calculated by obtaining the arithmetic average value. The thickness of each graphene was taken as the arithmetic average value of the thickness measurements of 5 randomly selected points in each graphene. In addition, for 10 randomly selected graphenes in the same manner, the cross section of each graphene was observed, the length in the direction parallel to the graphene layer was measured, and the arithmetic average value was obtained to calculate the size of the graphene in the plane direction parallel to the graphene layer.
[0069] [Measurement example 2: Measurement of O / C ratio and N / C ratio by X-ray photoelectron spectroscopy] The reduced graphene dispersion liquid produced in each Example and Comparative Example was filtered using a suction filter, and then washed five times by diluting with water to 0.5% by mass and suction filtering, and then freeze-dried to obtain graphene powder. The obtained graphene powder was subjected to photoelectron spectroscopy using an X-ray photoelectron spectrometer Quantera SXM (manufactured by PHI). The excitation X-ray was monochromatic Al K α1,2 The X-ray diameter was 200 μm, and the photoelectron escape angle was 45°. The C1s main peak due to carbon atoms was assigned to 284.3 eV, the O1s peak due to oxygen atoms was assigned to a peak near 533 eV, and the N1s peak due to nitrogen atoms was assigned to a peak near 402 eV. The O / C ratio was calculated from the area ratio of the O1s peak and the C1s peak, and the obtained value was rounded to the second decimal place. In addition, the N / C was calculated from the area ratio of the N1s peak and the C1s peak, and the obtained value was rounded to the third decimal place to the third decimal place. Note that the O / C ratio and N / C ratio of graphene did not change between the graphene dispersion and the heat dissipation material, so they were measured using the graphene dispersion.
[0070] [Measurement example 3: Thermal conductivity measurement] The heat dissipating materials prepared in each of the examples and comparative examples were weighed using an electronic balance. Then, the weighed heat dissipating material was completely immersed in distilled water filled in a measuring cylinder to a predetermined volume, and the volume of the heat dissipating material was calculated from the difference in the indicated volume of the measuring cylinder before and after immersion. The density d of the heat dissipating material was calculated from the weight and volume. Furthermore, the thermal diffusion rate κ in the surface direction of the heat dissipating material was measured using a Thermowave Analyzer TA (manufactured by Bethel Co., Ltd.). In addition, the specific heat C of the heat dissipating material was measured using a differential scanning calorimeter DSC 7020 (manufactured by Seiko Instruments Inc.). Using the above values, the thermal conductivity α was calculated from the product of the density d, the specific heat C, and the thermal diffusion rate κ.
[0071] [Synthesis Example 1: Preparation of graphene oxide] Using 1500 mesh natural graphite powder (Shanghai Yifan Graphite Co., Ltd.) as the raw material, 220 ml of 98% concentrated sulfuric acid, 5 g of sodium nitrate, and 30 g of potassium permanganate were added to 10 g of natural graphite powder in an ice bath, and the mixture was mechanically stirred for 1 hour while maintaining the temperature of the mixture below 20 °C. The mixture was removed from the ice bath and stirred in a 35 °C water bath for 4 hours, after which 500 ml of ion-exchanged water was added and the resulting suspension was stirred at 90 °C for another 15 minutes. Finally, 600 ml of ion-exchanged water and 50 ml of hydrogen peroxide were added and stirred for 5 minutes to obtain a graphene oxide dispersion. The mixture was filtered while still hot, and the metal ions were washed with a dilute hydrochloric acid solution, the acid was washed with ion-exchanged water, and washing was repeated until the pH reached 7 to prepare graphene oxide. The elemental ratio of oxygen atoms to carbon atoms (O / C ratio) of the prepared graphene oxide measured by X-ray photoelectron spectroscopy was 0.53.
[0072] [Synthesis Example 2: Preparation of graphene oxide] Graphene oxide was prepared in the same manner as in Synthesis Example 1, except that 1500 mesh natural graphite powder (Shanghai Yifan Graphite Co., Ltd.) was changed to AGB-32 (manufactured by Ito Graphite Industries Co., Ltd.) The elemental ratio of oxygen atoms to carbon atoms (O / C ratio) of the prepared graphene oxide measured by X-ray photoelectron spectroscopy was 0.51.
[0073] [Example 1] (Preparation of graphene N-methylpyrrolidone dispersion paste) The graphene oxide prepared in Synthesis Example 1 was diluted with ion-exchanged water to a concentration of 30 mg / ml, and treated for 30 minutes at 3,000 rpm using a Homo Disper 2.5 (Primix Corporation) to obtain a uniform graphene oxide dispersion. 20 ml of the obtained graphene oxide dispersion was mixed with 0.3 g of dopamine hydrochloride as a surface treatment agent, and treated for 60 minutes at 3,000 rpm using a Homo Disper 2.5 (Primix Corporation). The treated graphene oxide dispersion was subjected to ultrasonic irradiation at an output of 300 W for 30 minutes (microparticulation process) using an ultrasonic device UP400S (Hielscher). The graphene oxide dispersion that had been subjected to the micronization process was diluted to 5 mg / ml using ion-exchanged water, and 0.3 g of sodium dithionite was added to 20 ml of the diluted dispersion, and the mixture was stirred at 3,000 rpm for 1 hour on a water bath at 40°C using a Homo Disper 2.5 type (Primix Corporation). The mixture was then filtered using a vacuum suction filter, and the washing process of diluting the mixture to 0.5% by weight using water and suction filtering was repeated five times to obtain a graphene aqueous dispersion. N-methylpyrrolidone was added to the obtained graphene aqueous dispersion to a concentration of 0.5% by weight, and the mixture was treated for 60 seconds at a rotation speed of 40 m / s (shear rate: 20,000 per second) using a "Filmix" (registered trademark) 30-30 type (Primix Corporation). After the treatment, the solvent was removed by vacuum suction filtration. In order to further remove moisture, N-methylpyrrolidone was added until the graphene concentration reached 0.5% by weight, and the mixture was diluted by treatment at a rotation speed of 3,000 rpm for 30 minutes using a Homo Disper 2.5 type (Primix Corporation). The process of filtering by reduced pressure and suction until the filtrate no longer dripped was repeated twice, yielding an N-methylpyrrolidone dispersion paste containing 5.0% by weight of surface-treated graphene as the filtrate.
[0074] (Preparation of polyvinyl alcohol resin solution) 5% by weight of polyvinyl alcohol resin (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., saponification rate 88%, polymerization degree 500) was added to 95% by weight of N-methylpyrrolidone, and the mixture was heated to 90°C in a sealed container while stirring with a magnetic stirrer to completely dissolve the polyvinyl alcohol resin, thereby obtaining an N-methylpyrrolidone solution containing 5.0% by weight of polyvinyl alcohol resin.
[0075] (Preparation of graphene dispersion) 5 g of the polyvinyl alcohol resin solution was added to 20 g of the graphene N-methylpyrrolidone dispersion paste, and then the mixture was stirred for 15 minutes (strong stirring) at a rotation speed of 40 m / s (shear rate: 20,000 per second) using a "Filmix" (registered trademark) 30-30 type (Primix Corporation) to obtain a graphene dispersion. The graphene solids concentration of the obtained graphene dispersion was 4 wt %, and the polyvinyl alcohol resin content was 25 wt parts relative to 100 wt parts of graphene.
[0076] (Preparation of heat dissipating material) 32 g of bisphenol A epoxy resin (manufactured by Mitsubishi Chemical Corporation, product number "jER" (registered trademark) 828), 17.5 g of phenol novolac curing agent (manufactured by DIC Corporation, product number TD2090), and 0.5 g of 2-ethyl-4-methylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.) as a curing accelerator were thoroughly mixed, and 25 g of the above-mentioned graphene dispersion was further added and mixed for 15 minutes at a rotation speed of 2,000 rpm using "Awatori Rentaro" (registered trademark) manufactured by Thinky Corporation. The resulting mixture was applied to a polyimide film "Kapton" (registered trademark) (manufactured by Toray DuPont Co., Ltd.) using an applicator to a film thickness of 1 mm to form a coating film. The coating film was dried at 120 ° C for 60 minutes, and then vacuum-dried for 8 hours while heating at 50 ° C in a vacuum dryer to obtain a heat dissipation material.
[0077] The obtained graphene dispersion and heat dissipation material were evaluated by the above-mentioned methods, and the results are shown in Table 1.
[0078] [Example 2] A heat dissipation material was produced and evaluated in the same manner as in Example 1, except that in the preparation of the graphene dispersion, N-methylpyrrolidone not containing a polyvinyl alcohol resin was used instead of the polyvinyl alcohol resin solution.
[0079] [Example 3] A graphene dispersion was obtained in the same manner as in Example 1, except that the strong stirring treatment time was extended to 30 minutes. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0080] [Example 4] A graphene dispersion was obtained in the same manner as in Example 1, except that the strong stirring treatment time was shortened to 5 minutes. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0081] [Example 5] A graphene dispersion was obtained in the same manner as in Example 1, except that the amount of sodium dithionite added was reduced to 0.1 g. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0082] [Example 6] A graphene dispersion was obtained in the same manner as in Example 1, except that the amount of sodium dithionite added was reduced to 0.01 g. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0083] [Example 7] A graphene dispersion was obtained in the same manner as in Example 1, except that the microparticulation step was extended to 120 minutes. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0084] [Example 8] A graphene dispersion was obtained in the same manner as in Example 1, except that the microparticulation step was shortened to 5 minutes. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0085] [Example 9] Except for not carrying out the microparticulation step, a graphene dispersion was obtained in the same manner as in Example 1. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0086] [Example 10] A graphene dispersion was obtained in the same manner as in Example 1, except that dopamine hydrochloride was changed to benzylamine hydrochloride. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0087] [Example 11] A graphene dispersion was obtained in the same manner as in Example 1, except that dopamine hydrochloride was changed to phenylethylamine hydrochloride. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0088] [Example 12] In preparing the graphene dispersion, 2 g of the polyvinyl alcohol resin solution was added to 20 g of the NMP dispersion paste containing 5.0 wt % of surface-treated graphene, and 3 g of NMP was added, and the graphene dispersion was obtained in the same manner as in Example 1. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0089] [Example 13] A graphene dispersion was prepared in the same manner as in Example 1.
[0090] In preparing the polyvinyl alcohol resin solution, 4 g of polyvinyl alcohol resin and 16 g of N-methylpyrrolidone were heated to 120°C in a sealed container under stirring with a magnetic stirrer to dissolve the polyvinyl alcohol resin and obtain a polyvinyl alcohol resin solution with a concentration of 20 wt%.
[0091] In preparing the graphene dispersion, 20 g of the graphene N-methylpyrrolidone dispersion paste was added to 5 g of the obtained 20 wt% polyvinyl alcohol / N-methylpyrrolidone solution, and the mixture was heated again in a sealed container at 120°C for 8 hours, after which the mixture was mixed with a spatula and treated for 15 minutes at a rotation speed of 40 m / s (shear rate: 20,000 per second) using a "Filmix" (registered trademark) 30-30 type (Primix Corporation) to obtain a graphene dispersion. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0092] [Example 14] A graphene dispersion was prepared in the same manner as in Example 1.
[0093] In preparing the polyvinyl alcohol solution, 10 g of polyvinyl alcohol resin and 10 g of N-methylpyrrolidone were heated to 120°C in a sealed container under stirring with a magnetic stirrer to partially dissolve the polyvinyl alcohol resin, thereby obtaining a polyvinyl alcohol resin dispersion with a concentration of 50% by weight.
[0094] In preparing the graphene dispersion, 20 g of the graphene N-methylpyrrolidone dispersion paste was added to 5 g of the obtained 50 wt % polyvinyl alcohol resin dispersion, and the mixture was heated again in a sealed container at 120° C. for 8 hours, after which the mixture was mixed with a spatula and treated for 15 minutes at a rotation speed of 40 m / s (shear rate: 20,000 per second) using a “Filmix” (registered trademark) 30-30 type (Primix Corporation) to obtain a graphene dispersion. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0095] [Example 15] A graphene dispersion was prepared in the same manner as in Example 1.
[0096] In preparing the graphene dispersion, 20 g of N-methylpyrrolidone dispersion paste containing 5.0 wt% of surface-treated graphene was added to 5 g of polyvinyl alcohol powder, mixed for 15 minutes at a rotation speed of 2000 rpm using a planetary mixer, heated in a closed container at 120°C for 16 hours, and then mixed with a spatula and treated for 15 minutes at a rotation speed of 40 m / s (shear rate: 20,000 per second) using a "Filmix" (registered trademark) 30-30 type (Primix Corporation) to obtain a graphene dispersion. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0097] [Example 16] A graphene dispersion was obtained in the same manner as in the preparation of the polyvinyl alcohol resin solution, except that the polyvinyl alcohol resin had a saponification rate of 38% and a polymerization degree of 400 (manufactured by Nippon Vinyl Acetate & Poval Co., Ltd., product name "JMR-20L"). Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0098] [Example 17] A graphene dispersion was obtained in the same manner as in Example 1, except that in the preparation of the polyvinyl alcohol resin solution, the polyvinyl alcohol resin had a saponification rate of 75% and a polymerization degree of 500 (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0099] [Example 18] A graphene dispersion was obtained in the same manner as in Example 1, except that in the preparation of the polyvinyl alcohol resin solution, the polyvinyl alcohol resin had a saponification rate of 98% and a polymerization degree of 500 (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0100] [Example 19] A graphene dispersion was obtained in the same manner as in the preparation of the polyvinyl alcohol resin solution, except that the polyvinyl alcohol had a saponification rate of 88% and a polymerization degree of 1,500 (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was used. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0101] [Example 20] A graphene dispersion was obtained in the same manner as in the preparation of the polyvinyl alcohol resin solution, except that the polyvinyl alcohol resin had a saponification rate of 88% and a polymerization degree of 3,500 (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.). Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0102] [Example 21] In preparing the heat dissipation material, the epoxy resin was changed to 50 g of an ethylene-acrylic copolymer elastomer (manufactured by DuPont, product name "Vamac" (registered trademark) DP) as the polyacrylate resin, and the heating temperature of the coating film was set to 180°C. Except for this, the heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0103] [Example 22] In preparing the heat dissipation material, the heat dissipation material was produced and evaluated in the same manner as in Example 1, except that the epoxy resin was changed to 50 g of polyurethane resin (manufactured by Tosoh Corporation, product name "Coronate (registered trademark)" model number 4076).
[0104] [Example 23] In preparing the heat dissipation material, the heat dissipation material was produced and evaluated in the same manner as in Example 1, except that the epoxy resin was changed to 48.75 g of silicone resin (manufactured by Shin-Etsu Chemical Co., Ltd., product number KNS-320A) and 1.25 g of curing agent (manufactured by Shin-Etsu Chemical Co., Ltd., product number CAT-PL-50T).
[0105] [Example 24] A heat dissipating material was produced and evaluated in the same manner as in Example 1, except that the amount of graphene dispersion used in preparing the heat dissipating material was 10 g.
[0106] [Example 25] A heat dissipating material was produced and evaluated in the same manner as in Example 1, except that in the preparation of the heat dissipating material, the amount of the graphene dispersion used was 62.5 g.
[0107] [Comparative Example 1] Except for not using dopamine hydrochloride, a graphene dispersion was obtained in the same manner as in Example 1. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0108] [Comparative Example 2] A graphene dispersion was obtained in the same manner as in Example 1, except that the amount of dopamine hydrochloride added was increased to 1 g. Using the obtained graphene dispersion, a heat dissipation material was produced and evaluated in the same manner as in Example 1.
[0109] [Comparative Example 3] A graphene dispersion was obtained in the same manner as in Example 1, except that the graphene oxide dispersion produced in Synthesis Example 2 was used in the preparation of the graphene dispersion. A heat dissipation material was produced and evaluated in the same manner as in Example 1 using the obtained graphene dispersion.
[0110] [Example 26] A heat dissipation material was produced and evaluated in the same manner as in Example 1, except that in the preparation of the heat dissipation material, after the graphene dispersion liquid was added, 197.5 g (50 volume%) of aluminum oxide fine particles (manufactured by Showa Denko K.K., product number AS-40, average particle size 12 μm) was further added.
[0111] [Example 27] A heat dissipation material was produced and evaluated in the same manner as in Example 26, except that 197.5 g of aluminum oxide fine particles were replaced with 163 g (50 volume%) of aluminum nitride fine particles (Sigma-Aldrich, average particle size 10 μm).
[0112] [Example 28] A heat dissipation material was produced and evaluated in the same manner as in Example 26, except that in the preparation of the heat dissipation material, 197.5 g of aluminum oxide fine particles was replaced with 132.5 g (50 volume%) of silicon dioxide fine particles (Sigma-Aldrich, average particle size 5 μm).
[0113] [Example 29] In preparing the heat dissipation material, the amount of aluminum oxide fine particles (manufactured by Showa Denko K.K., product number AS-40, average particle size 12 μm) added was changed to 158 g (40 volume%), and the heat dissipation material was produced and evaluated in the same manner as in Example 26.
[0114] [Example 30] In preparing the heat dissipation material, the amount of aluminum oxide (manufactured by Showa Denko K.K., product number AS-40, average particle size 12 μm) added was changed to 118.5 g (30 volume%), and the heat dissipation material was produced and evaluated in the same manner as in Example 26.
[0115] [Comparative Example 4] A heat dissipating material was produced and evaluated in the same manner as in Example 26, except that the graphene dispersion liquid was not added in the preparation of the heat dissipating material.
[0116] The main compositions and evaluation results of each of the examples and comparative examples are shown in Tables 1 and 2.
[0117] [Table 1]
[0118] [Table 2]
Claims
1. A heat dissipation material containing a resin and reduced graphene oxide, the graphene has an average thickness of 0.3 nm or more and 20 nm or less, an atomic ratio of nitrogen to carbon (N / C ratio) of 0.005 or more and 0.020 or less, and an atomic ratio of oxygen to carbon (O / C ratio) of 0.05 or more and 0.35 or less, as measured by X-ray photoelectron spectroscopy.
2. A heat dissipation material as described in claim 1, wherein a surface treatment agent is adhered to the surface of graphene.
3. The heat dissipation material according to claim 1 or 2, wherein the graphene has a size of 0.10 μm or more and 100 μm or less in a direction parallel to the graphene layer.
4. The heat dissipation material according to any one of claims 1 to 3, containing as the resin a vinyl resin, a polystyrene resin, an ABS resin, a polycarbonate resin, a polyamide resin, a polyimide resin, a polyacrylate resin, a polyester resin, a polyphenylene sulfide resin, an epoxy resin, a urethane resin, a silicone resin and / or a phenol resin.
5. The heat dissipation material according to claim 4 , wherein the vinyl resin contains a polyvinyl alcohol resin.
6. The heat dissipating material according to claim 5 , wherein the saponification rate of the polyvinyl alcohol resin is 70% or more and 100% or less.
7. The heat dissipation material according to claim 5 or 6, comprising 5 parts by weight or more and 300 parts by weight or less of polyvinyl alcohol relative to 100 parts by weight of graphene.
8. The heat dissipation material according to any one of claims 1 to 7, further comprising inorganic fine particles.
Citation Information
Patent Citations
Electrically insulating and thermally conductive composition and electronic device
JP2012188645A
Heat dissipation film, and production method and apparatus therefor
JP2014127518A
Easily deformable aggregate and method for producing the same, thermal conductive resin composition, thermal conductive member and method for producing the same, and thermal conductive adhesive sheet
JP2015034269A
Thermally conductive resin composition, thermally conductive sheet and electronic component
JP2020117573A
Modified graphene, method of producing modified graphene, modified graphene-resin composite, modified graphene sheet, and modified graphene dispersion
JP2020138898A