Preparation method of octadecanol / silicon dioxide aerogel composite material
Octadecanol/silica aerogel composite material prepared by one-step synthesis method solves the problems of complicated preparation of composite phase change materials and insufficient compressive strength in the prior art, and realizes efficient and low-cost production of thermal insulation materials , has the advantages of high latent heat, low thermal conductivity, stable shape and high compression strength.
Patent Information
- Application Number
- CN202411069874.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
The existing porous matrix composite phase change materials are cumbersome, with poor compressive strength, making it difficult to achieve rapid and large-scale production of efficient overall shape and stable thermal insulation materials.
Using a one-step synthesis method, terephthaldehyde, octadecanol and anhydrous ethanol were mixed, 3-aminopropyltriethoxysilane and deionized water were added, and autoclave reaction and drying were carried out to prepare octadecanol/dihydrate. Silicon oxide aerogel composite material.
The high latent heat, low thermal conductivity of the material is achieved, stable shape, high compression strength and good hydrophobicity, simplified the preparation process, reduced costs, and improved production efficiency and application effect.
Smart Images

Figure CN118978896A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of battery thermal protection, and in particular relates to a method for preparing an octadecyl alcohol / silicon dioxide aerogel composite material. Background Art
[0002] In many countries, electric vehicles (EVs) are being developed to replace traditional fuel vehicles, which have an impact on the environment and resources. For EVs, lithium-ion batteries (LIBs) have proven to be a promising alternative due to their high specific energy density, long cycle life, and low self-discharge. However, batteries with high energy density may cause more serious thermal hazards if the energy is not released properly or the generated heat cannot be effectively dissipated. In order to ensure the excellent electrochemical performance and energy safety of lithium-ion batteries, many battery thermal management systems (BTMS) have been developed to ensure that the batteries operate within the appropriate temperature range.
[0003] Phase change materials are an important component of battery thermal management systems because they can absorb and release large amounts of heat during phase change, making them ideal for a variety of industrial and residential applications. Depending on the specific conditions, these so-called "smart energy management materials" can store energy by melting / solidifying and release energy with minimal losses. Phase change materials can be divided into solid-gas, liquid-gas, solid-solid and solid-solid. Among them, solid-liquid PCMs show application prospects due to their higher phase change enthalpy and smaller volume change than solid-solid and liquid / solid-gas systems.
[0004] So far, most of the reported porous-based composite phase change materials are powdery and have poor compressive strength. Composite phase change materials are usually prepared by physical combination methods such as solution impregnation or melt infiltration. For example, Chinese invention patent CN202010446299.9 discloses a method for preparing an improved silica aerogel and a silica aerogel, including the following steps:
[0005] S1, ethyl orthosilicate, anhydrous ethanol and deionized water were mixed evenly in a molar ratio of 1:15:5, an acid was added to adjust the pH to 2-4 and hydrolyzed for 1-3 hours, 3-aminopropyl trihydroxysilane was added and stirred evenly, and a base was added to adjust the pH to 8.5-10 for condensation to form a wet gel;
[0006] S2. The wet gel in step S1 is aged and replaced with anhydrous ethanol twice, placed in trimethylchlorosilane or hexamethyldisilazane n-hexane solution for modification, taken out, placed in a polyacyl chloride compound solution for 10 min to 30 min, taken out, placed in anhydrous ethanol, taken out, and dried to obtain the improved silica aerogel.
[0007] The above preparation method is relatively cumbersome and requires repeated immersion in different solutions. Therefore, it is crucial to adopt a simple one-step strategy to directly develop a composite phase change material with high compressive strength and overall shape stability for practical applications. In order to achieve rapid and large-scale production of monolithic silica aerogel-based organic composite phase change materials with good thermal insulation performance and high compressive strength. Summary of the invention
[0008] In view of this, the purpose of the present invention is to provide a method for preparing an octadecyl alcohol / silicon dioxide aerogel composite material. The preparation method of the present invention is a one-step synthesis method, which can realize the rapid and large-scale production of a silica aerogel-based organic composite phase change material.
[0009] The specific technical solution adopted by the present invention is:
[0010] A preparation method of an octadecyl alcohol / silicon dioxide aerogel composite material comprises the following steps: mixing terephthalaldehyde, octadecyl alcohol and anhydrous ethanol, and stirring evenly to obtain a mixed solution; then adding 3-aminopropyltriethoxysilane and deionized water to the mixed solution, stirring evenly, and transferring to an autoclave for reaction; after the reaction is completed, placing the obtained product in an oven for drying treatment, and obtaining an octadecyl alcohol / silicon dioxide aerogel phase change material.
[0011] More preferably, the usage ratio of terephthalaldehyde, octadecyl alcohol and anhydrous ethanol is: 1-3g: 5-15g: 25-80ml.
[0012] More preferably, the volume ratio of anhydrous ethanol, 3-aminopropyltriethoxysilane and deionized water is: 25-80:4-8:1-10.
[0013] More preferably, the stirring is ultrasonic stirring, the ultrasonic power is 45W, and the stirring time is 20min.
[0014] More preferably, the reaction temperature in the autoclave is 100-150° C., and the reaction time is 18 to 36 hours.
[0015] More preferably, the drying treatment is as follows: the drying temperature is 50-90° C. and the treatment time is 12-36 hours.
[0016] Correspondingly, the present invention also provides an octadecyl alcohol / silicon dioxide aerogel composite material, which is prepared by the above-mentioned preparation method.
[0017] The present invention also provides application of the octadecyl alcohol / silicon dioxide aerogel composite material in the field of battery thermal runaway of electric vehicles.
[0018] More preferably, in specific application, the composite material is placed on the surface of the battery to wrap the battery.
[0019] The beneficial effects of the present invention are:
[0020] In the sol-gel process of the present invention, the organic phase change materials terephthalaldehyde and octadecyl alcohol in situ occupy the porous channels of the silica aerogel, which effectively avoids the complicated and multiple preparation processes, overcomes the shortcomings of the two-step method of low yield and long time consumption, and has the advantages of simple operation, easy control of conditions, low cost and strong operability.
[0021] Due to the low thermal conductivity of silica aerogel and the large latent heat of phase change materials, the octadecanol / silica aerogel composite phase change material of the present invention can first use silica aerogel to effectively isolate heat, and then use the phase change material to absorb heat, and has good thermal insulation performance, which can effectively delay the increase of surface temperature under the action of environmental heat flow, and is a suitable candidate for thermal protection applications. The present invention uses 3-aminopropyltriethoxysilane as a silicon source, which can improve the adhesion, dispersibility and strength of the material, and is also a coupling agent, so that the prepared octadecanol / silica aerogel composite phase change material has stable shape and high compressive strength. In summary, the octadecanol / silica aerogel composite phase change material of the present invention has the advantages of high latent heat, low thermal conductivity, stable shape, high compressive strength and good hydrophobicity. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The octadecyl alcohol / SiO synthesized in Example 2 2 Flow chart of the preparation of aerogel composite phase change materials.
[0023] Figure 2 The octadecyl alcohol / SiO synthesized in Example 2 2 Sample image of aerogel composite phase change material leakage test.
[0024] Figure 3 The octadecyl alcohol / SiO synthesized in Example 2 2 SEM image of aerogel composite phase change material.
[0025] Figure 4 The octadecyl alcohol / SiO synthesized in Example 2 2 DSC thermal analysis diagram of aerogel composite phase change material.
[0026] Figure 5 The octadecyl alcohol / SiO synthesized in Example 2 2 Thermogravimetric diagram of aerogel composite phase change material. DETAILED DESCRIPTION
[0027] In order to explain the technical content, structural features, achieved objectives and effects of the technical solution in detail, the following is a detailed description in conjunction with specific embodiments and accompanying drawings.
[0028] Example 1
[0029] A composite phase change material comprises the following components: terephthalaldehyde, octadecyl alcohol, 3-(aminopropyl)trioxysilane and anhydrous ethanol.
[0030] The preparation method of the composite phase change material comprises: mixing 1g of terephthalaldehyde, 5g of octadecyl alcohol and 25ml of anhydrous ethanol, and then ultrasonically stirring for 20 minutes to obtain a mixed solution. 4ml of 3-(aminopropyl)triethoxysilane and 1mL of deionized water are introduced into the mixture, ultrasonically stirred for 5 minutes, and then the obtained reactants are placed in a 50mL stainless steel autoclave and kept at 120°C for 24 hours. Place in an oven at 70°C for 48 hours to obtain an aerogel-based composite phase change material.
[0031] Example 2
[0032] A composite phase change material comprises the following components: terephthalaldehyde, polyethylene glycol, 3-(aminopropyl)trioxysilane and anhydrous ethanol.
[0033] The preparation method of the composite phase change material comprises: mixing 2g of terephthalaldehyde, 10g of polyethylene glycol and 60ml of anhydrous ethanol, and then ultrasonically stirring for 20 minutes to obtain a mixed solution. 6ml of 3-(aminopropyl)triethoxysilane and 2.5ml of deionized water are introduced into the mixture, ultrasonically stirred for 5 minutes, and then the obtained reactants are placed in a 50mL stainless steel autoclave and kept at 120°C for 24 hours. Place in an oven at 70°C for 48 hours to obtain an aerogel-based composite phase change material.
[0034] Example 3
[0035] A composite phase change material comprises the following components: terephthalaldehyde, polyethylene glycol, 3-(aminopropyl)trioxysilane and anhydrous ethanol.
[0036] The preparation method of the composite phase change material comprises: mixing 3g of terephthalaldehyde, 15g of polyethylene glycol and 80ml of anhydrous ethanol and ultrasonically stirring for 20 minutes to obtain a mixed solution. 8mL of 3-(aminopropyl)triethoxysilane and 10mL of deionized water are introduced into the mixture, ultrasonically stirred for 5 minutes, and then the resulting reactants are placed in a 50mL stainless steel autoclave and kept at 120°C for 24 hours. Place in an oven at 70°C for 48 hours to obtain an aerogel-based composite phase change material.
[0037] The octadecyl alcohol / SiO prepared in Example 2 2The aerogel composite phase change material was tested for leakage. The specific test method was to place the sample in a 100°C oven for 30 minutes to ensure that the composite phase change material completely underwent a solid-liquid phase change process. Then carefully observe whether there were any signs of phase change material leakage on the filter paper. The results are as follows: Figure 2 As shown, there is no leakage of the phase change material and the sample is successfully prepared.
[0038] Figure 3 The octadecyl alcohol / SiO synthesized in Example 2 2 SEM image of aerogel composite phase change material, from Figure 3 It can be seen that the granular silica aerogel is embedded between the flakes of octadecanol, which proves that the octadecanol / SiO 2 Aerogel composite phase change materials were successfully prepared.
[0039] Figure 4 The octadecyl alcohol / SiO synthesized in Example 2 2 DSC thermal analysis diagram of aerogel composite phase change material, from Figure 4 It can be concluded that the endothermic and exothermic enthalpy changes of the octadecyl alcohol / silica aerogel composite phase change material are 192.2 J / g and 169.3 J / g, respectively, and its Tm and Tc are 59.7°C and 54.4°C, respectively.
[0040] Figure 5 The octadecyl alcohol / SiO synthesized in Example 2 2 Thermogravimetric diagram of aerogel composite phase change material, from Figure 5 It can be seen that octadecyl alcohol@silica aerogel has good thermal stability within the phase transition temperature range.
[0041] Although the above embodiments have been described, once those skilled in the art know the basic creative concepts, they can make additional changes and modifications to these embodiments. Therefore, the above description is only an embodiment of the present invention and does not limit the patent protection scope of the present invention. Any equivalent structure or equivalent process transformation made by using the contents of the specification and drawings of the present invention, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing an octadecyl alcohol / silicon dioxide aerogel composite material, characterized in that: The method comprises the following steps: mixing terephthalaldehyde, octadecyl alcohol and anhydrous ethanol, and stirring evenly to obtain a mixed solution; then adding 3-aminopropyltriethoxysilane and deionized water to the mixed solution, stirring evenly, and transferring to an autoclave for reaction; after the reaction is completed, placing the obtained product in an oven for drying treatment, and obtaining an octadecyl alcohol / silicon dioxide aerogel phase change material.
2. The preparation method according to claim 1, characterized in that: The dosage ratio of terephthalaldehyde, octadecyl alcohol and anhydrous ethanol is: 1-3g: 5-15g: 25-80ml.
3. The preparation method according to claim 1, characterized in that: The volume ratio of the anhydrous ethanol, 3-aminopropyltriethoxysilane and deionized water is: 25-80:4-8:1-10.
4. The preparation method according to claim 1, characterized in that: The stirring is ultrasonic stirring, the ultrasonic power is 45W, and the stirring time is 20min.
5. The preparation method according to claim 1, characterized in that: The reaction temperature in the autoclave is 100-150°C and the reaction time is 18-36h.
6. The preparation method according to claim 1, characterized in that: The drying process is as follows: the drying temperature is 50-90° C. and the processing time is 12-36 hours.
7. An octadecyl alcohol / silicon dioxide aerogel composite material, characterized in that: Prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the octadecyl alcohol / silicon dioxide aerogel composite material according to claim 7 in the field of battery thermal runaway of electric vehicles.
9. The use according to claim 8, characterized in that: The composite material is placed on the surface of the battery to wrap the battery.
Citation Information
Cited By
Preparation method of silicon dioxide aerogel-based phase-change temperature-control regenerated cellulose fiber
CN121538745A
Preparation method of regenerated cellulose fiber with phase change temperature control based on silica aerogel
CN121538745B
Preparation method of phase-change temperature-control Lyocell fiber
CN122039244A
A method for preparing phase change temperature-controlled lyocell fibers