Composition for forming thin film for energy storage device electrodes

A polymer-based thin film composition with an oxazoline group addresses the challenges of weight, conductivity, and stability issues in energy storage devices by providing adhesion and functionality as an undercoat layer without conductive carbon, enhancing performance and reducing costs.

JP7559746B2Active Publication Date: 2024-10-02NISSAN CHEM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021501935
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-02-21
Filing Date
2020-02-14
Publication Date
2024-10-02
Estimated Expiration
2040-02-14

AI Technical Summary

Technical Problem

Existing energy storage devices face challenges with undercoat layers containing conductive carbon materials, which increase weight and size, reduce conductivity due to increased insulating components, and have poor storage stability leading to agglomeration and high manufacturing costs.

Method used

A composition for forming a thin film using a polymer with an oxazoline group in the side chain, devoid of conductive carbon material, which provides adhesion to the electrode mixture layer and current collector, and functions as an undercoat layer.

Benefits of technology

The thin film composition achieves excellent adhesion and conductivity without conductive carbon, reducing internal resistance and manufacturing costs, while maintaining stability and preventing agglomeration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559746000007
    Figure 0007559746000007
  • Figure 0007559746000001
    Figure 0007559746000001
  • Figure 0007559746000002
    Figure 0007559746000002
Patent Text Reader

Abstract

For example, a composition for forming a thin film for an energy storage device electrode, which contains a polymer having an oxazoline group in a side chain obtained using an oxazoline group-containing monomer as represented by formula (1) and a solvent, but does not contain a conductive carbon material, can achieve good adhesion to an electrode mixture layer or a current collector in an energy storage device electrode, and provides a thin film that functions as an undercoat layer despite not containing a conductive carbon material. (wherein X represents a polymerizable carbon-carbon double bond-containing group, R 1 ~R 4 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 5 carbon atoms which may have a branched structure, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for forming a thin film for an electrode of an energy storage device. [Background technology]

[0002] In recent years, with the expansion of applications of energy storage devices such as lithium ion secondary batteries and electric double layer capacitors, there is a demand for lower internal resistance. One measure proposed to meet this demand is to place an undercoat layer containing a conductive carbon material between the electrode mixture layer and the current collector to reduce the resistance at the contact interface between them (see Patent Documents 1 and 2). However, if the weight per unit area (basis weight) of the undercoat layer is large, this causes the problem of the battery becoming heavy and large.

[0003] In addition, this undercoat layer is expected to increase adhesion with the electrode composite layer and the current collector and suppress deterioration due to interfacial peeling. However, since the conductive carbon material is a solid (powder) and has weak interactions with the current collector and electrode layer, a component with high adhesion other than the conductive carbon material is required to strongly adhere the undercoat layer to the current collector and electrode layer. However, if the content of components other than the conductive carbon material is increased, the insulating components increase, which reduces the conductivity of the undercoat layer and impairs the intended effect of reducing the resistance of the battery. Furthermore, the dispersion liquid containing the conductive carbon material used in forming these undercoat layers does not necessarily have good storage stability, and often causes problems such as aggregation of the conductive carbon material during storage. In addition, the dispersion process itself is costly, resulting in high manufacturing costs. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-170965 A [Patent Document 2] International Publication No. 2014 / 042080 Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in consideration of the above circumstances, and has an object to provide a thin film-forming composition for an energy storage device electrode, which can achieve good adhesion to an electrode mixture layer and a current collector in an energy storage device electrode, and which provides a thin film that functions as an undercoat layer despite not containing a conductive carbon material. [Means for solving the problem]

[0006] Means for Solving the Problems The present inventors have conducted extensive research in order to achieve the above object, and as a result have found that a composition containing a polymer having an oxazoline group in a side chain and not containing a conductive carbon material can exhibit good adhesion to an electrode mixture layer or a current collector, and can provide a thin film that functions as an undercoat layer despite not containing a conductive carbon material, thereby completing the present invention.

[0007] That is, the present invention provides 1. A composition for forming a thin film for an energy storage device electrode, comprising a polymer having an oxazoline group in a side chain and a solvent, and not containing a conductive carbon material; 2. A composition for forming a thin film for an energy storage device electrode according to 1, which is used for forming a thin film interposed between a current collector and an electrode mixture layer of an energy storage device; 3. The composition for forming a thin film for an energy storage device electrode according to 1, wherein the polymer is a radical polymer of at least two types of monomers, namely, an oxazoline monomer having a polymerizable carbon-carbon double bond-containing group at the 2-position and a (meth)acrylic monomer having a hydrophilic functional group. 4. The composition for forming a thin film for an energy storage device electrode according to 3, wherein the polymer is a radical polymer of an oxazoline monomer represented by formula (1) having a polymerizable carbon-carbon double bond-containing group at the 2-position, and one or more (meth)acrylic monomers having a hydrophilic functional group selected from (meth)acrylic acid, 2-hydroxyethyl acrylate, methoxypolyethylene glycol acrylate, a monoester of acrylic acid and polyethylene glycol, 2-aminoethyl acrylate and its salts, 2-hydroxyethyl methacrylate, methoxypolyethylene glycol methacrylate, a monoester of methacrylic acid and polyethylene glycol, 2-aminoethyl methacrylate and its salts, sodium (meth)acrylate, ammonium (meth)acrylate, (meth)acrylonitrile, (meth)acrylamide, N-methylol(meth)acrylamide, and N-(2-hydroxyethyl)(meth)acrylamide; [ka] (In the formula, X represents a chain hydrocarbon group containing a polymerizable carbon-carbon double bond, R 1 ~R 4 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 5 carbon atoms which may have a branched structure, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms. 5. An undercoat layer comprising a thin film obtained from the composition for forming a thin film for an energy storage device electrode according to any one of 1 to 4. 6. A composite current collector for an electrode of an energy storage device, comprising an undercoat layer of 5; 7. An electrode for an energy storage device comprising the composite current collector for an electrode of the energy storage device according to claim 6; 8. An energy storage device comprising the energy storage device electrode of 7. 9. Energy storage device 8, which is a lithium-ion secondary battery to provide. Effect of the Invention

[0008] The composition for forming a thin film for an energy storage device electrode of the present invention does not contain a conductive carbon material, and therefore exhibits excellent adhesion to an electrode mixture layer and a current collector. Furthermore, the composition of the present invention provides a thin film that functions as an undercoat layer, even though it does not contain a conductive carbon material. [Brief description of the drawings]

[0009] [Figure 1] FIG. 13 is a graph showing cycle test results of secondary batteries using electrodes D, E and F produced in Example 4-1, Comparative Example 4-1 and Comparative Example 4-2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in further detail below. The composition for forming a thin film for an energy storage device electrode according to the present invention (hereinafter simply referred to as the composition) is characterized in that it contains a polymer having an oxazoline group in its side chain and a solvent, but does not contain a conductive carbon material. Note that the conductive carbon material is a carbon material that is conductive by itself, such as carbon black, ketjen black, acetylene black, carbon whiskers, carbon nanotubes (CNTs), carbon fibers, natural graphite, and artificial graphite.

[0011] In the present invention, the polymer having an oxazoline group in a side chain (hereinafter referred to as oxazoline polymer) is not particularly limited as long as it is a polymer in which an oxazoline group is bonded to a repeating unit constituting a main chain directly or via a spacer group such as an alkylene group. Specifically, however, it is preferably a vinyl-based polymer having a repeating unit bonded to a polymer main chain or a spacer group at the 2-position of an oxazoline ring, which is obtained by radical polymerization of an oxazoline monomer having a polymerizable carbon-carbon double bond-containing group at the 2-position as shown in formula (1).

[0012] [ka]

[0013] The above X represents a polymerizable carbon-carbon double bond-containing group, R 1 ~R 4 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 5 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms. The polymerizable carbon-carbon double bond-containing group of the oxazoline monomer is not particularly limited as long as it contains a polymerizable carbon-carbon double bond, but is preferably a chain hydrocarbon group containing a polymerizable carbon-carbon double bond, and for example, an alkenyl group having 2 to 8 carbon atoms, such as a vinyl group, an allyl group, or an isopropenyl group, is preferred. Here, examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. The alkyl group having 1 to 5 carbon atoms may be linear, branched, or cyclic, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, and a cyclohexyl group. Specific examples of the aryl group having 6 to 20 carbon atoms include a phenyl group, a xylyl group, a tolyl group, a biphenyl group, and a naphthyl group. Specific examples of the aralkyl group having 7 to 20 carbon atoms include a benzyl group, a phenylethyl group, and a phenylcyclohexyl group.

[0014] Specific examples of the oxazoline monomer having a polymerizable carbon-carbon double bond-containing group at the 2-position represented by formula (1) include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-4-ethyl-2-oxazoline, 2-vinyl-4-propyl-2-oxazoline, 2-vinyl-4-butyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-vinyl-5-ethyl-2-oxazoline, 2-vinyl-5-propyl-2-oxazoline, 2-vinyl-5-butyl-2-oxazoline, and 2-isopropenyl-2-oxazoline. Examples of oxazoline include 2-isopropenyl-4-methyl-2-oxazoline, 2-isopropenyl-4-ethyl-2-oxazoline, 2-isopropenyl-4-propyl-2-oxazoline, 2-isopropenyl-4-butyl-2-oxazoline, 2-isopropenyl-5-methyl-2-oxazoline, 2-isopropenyl-5-ethyl-2-oxazoline, 2-isopropenyl-5-propyl-2-oxazoline, and 2-isopropenyl-5-butyl-2-oxazoline. From the viewpoint of availability, 2-isopropenyl-2-oxazoline is preferred.

[0015] In addition, in consideration of preparing the composition using an aqueous solvent, the oxazoline polymer is also preferably water-soluble. Such a water-soluble oxazoline polymer may be a homopolymer of the oxazoline monomer represented by the above formula (1). However, in order to further increase the solubility in water, it is preferable that the polymer is obtained by radical polymerization of at least two types of monomers, namely, the oxazoline monomer and a (meth)acrylic acid ester monomer having a hydrophilic functional group.

[0016] Specific examples of (meth)acrylic monomers having hydrophilic functional groups include (meth)acrylic acid, 2-hydroxyethyl acrylate, methoxypolyethylene glycol acrylate, monoesterified product of acrylic acid and polyethylene glycol, 2-aminoethyl acrylate and its salts, 2-hydroxyethyl methacrylate, methoxypolyethylene glycol methacrylate, monoesterified product of methacrylic acid and polyethylene glycol, 2-aminoethyl methacrylate and its salts, sodium (meth)acrylate, ammonium (meth)acrylate, (meth)acrylonitrile, (meth)acrylamide, N-methylol (meth)acrylamide, N-(2-hydroxyethyl) (meth)acrylamide, sodium styrenesulfonate, etc., which may be used alone or in combination of two or more. Among these, methoxypolyethylene glycol (meth)acrylate and monoesterified product of (meth)acrylic acid and polyethylene glycol are preferred.

[0017] In addition, other monomers than the above oxazoline monomers and (meth)acrylic monomers having a hydrophilic functional group can be used in combination, as long as they do not adversely affect the adhesion of the thin film obtained from the composition of the present invention to a current collector or the like. Specific examples of other monomers include (meth)acrylic acid ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, perfluoroethyl (meth)acrylate, and phenyl (meth)acrylate; α-olefin monomers such as ethylene, propylene, butene, and pentene; haloolefin monomers such as vinyl chloride, vinylidene chloride, and vinyl fluoride; styrene monomers such as styrene and α-methylstyrene; vinyl carboxylate ester monomers such as vinyl acetate and vinyl propionate; and vinyl ether monomers such as methyl vinyl ether and ethyl vinyl ether. These may be used alone or in combination of two or more.

[0018] In the monomer components used in the production of the oxazoline polymer used in the present invention, the content of the oxazoline monomer is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, from the viewpoint of further increasing the adhesion of the resulting thin film to a current collector, etc. The upper limit of the content of the oxazoline monomer in the monomer components is 100% by mass, and in this case, a homopolymer of the oxazoline monomer is obtained. On the other hand, in order to further increase the water solubility of the resulting oxazoline polymer, the content of the (meth)acrylic monomer having a hydrophilic functional group in the monomer component is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more. Furthermore, the content of other monomers in the monomer components is within a range that does not affect the adhesion of the resulting thin film to a current collector, etc., as described above, and cannot be determined in general because it varies depending on the type of monomer. However, the content may be appropriately set within a range of 5 to 95% by mass, preferably 10 to 90% by mass.

[0019] The average molecular weight of the oxazoline polymer is not particularly limited, but the weight average molecular weight is preferably 1,000 to 2,000,000, and more preferably 2,000 to 1,000,000. The weight average molecular weight is a polystyrene-equivalent value determined by gel permeation chromatography.

[0020] The oxazoline polymer used in the present invention can be produced by polymerizing the various monomers described above by a known radical polymerization method described in, for example, JP-A-6-32844 and JP-A-2013-72002. In addition, the oxazoline polymer usable in the present invention can be obtained as a commercially available product. Examples of such commercially available products include Epocross WS-300 (manufactured by Nippon Shokubai Co., Ltd., solid content concentration 10% by mass, aqueous solution), Epocross WS-700 (manufactured by Nippon Shokubai Co., Ltd., solid content concentration 25% by mass, aqueous solution), Epocross WS-500 (manufactured by Nippon Shokubai Co., Ltd., solid content concentration 39% by mass, water / 1-methoxy-2-propanol solution), Poly(2-ethyl-2-oxazoline) (Aldrich), Poly(2-ethyl-2-oxazoline) (Alfa Aesar), and Poly(2-ethyl-2-oxazoline) (VWR International, LLC). When the solvent is commercially available as a solution, it may be used as is or may be replaced with the desired solvent before use.

[0021] The solvent is not particularly limited as long as it is one that has been conventionally used in the preparation of this type of composition, and examples thereof include organic solvents such as water; ethers such as tetrahydrofuran (THF), diethyl ether, 1,2-dimethoxyethane (DME); halogenated hydrocarbons such as methylene chloride, chloroform, 1,2-dichloroethane; amides such as N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP); ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone; alcohols such as methanol, ethanol, isopropanol, n-butanol, t-butanol, n-propanol; aliphatic hydrocarbons such as n-heptane, n-hexane, cyclohexane; aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene; glycol ethers such as ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether; and glycols such as ethylene glycol and propylene glycol. These solvents can be used alone or in combination of two or more.

[0022] Among these, water, NMP, DMF, THF, methanol, ethanol, n-propanol, isopropanol, n-butanol, and t-butanol are preferred. From the viewpoint of improving the coatability, it is preferred to include ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, acetone, methyl ethyl ketone, cyclohexanone, methanol, ethanol, n-propanol, isopropanol, n-butanol, t-butanol, and propylene glycol. From the viewpoint of reducing costs, it is preferred to include water. These solvents can be used alone or in combination of two or more for the purpose of improving the coatability and reducing costs. When using a mixed solvent of water and alcohols, the mixing ratio is not particularly limited, but the mass ratio of water:alcohols is preferably about 1:1 to 10:1.

[0023] In addition, when the above-mentioned oxazoline polymer is used, the film-forming properties are good even when a hydrophilic solvent such as alcohols, glycol ethers, or glycols is used. Furthermore, even when a mixed solvent of the above-mentioned hydrophilic solvent and water or water alone is used, the film-forming properties are not reduced. In recent years, due to the trend toward eliminating organic solvents, there is a demand for materials that use water as a solvent. Therefore, in the composition of the present invention, it is preferable to use a mixed solvent of a hydrophilic solvent and water, or water alone.

[0024] The composition of the present invention may contain a crosslinking agent that is soluble in the above-mentioned solvents. The crosslinking agent may be either a compound that undergoes a crosslinking reaction with the oxazoline group of the oxazoline polymer or a compound that undergoes self-crosslinking. From the viewpoint of further enhancing the solvent resistance of the resulting thin film, however, a compound that undergoes a crosslinking reaction with the oxazoline group is preferred.

[0025] The compound that undergoes a crosslinking reaction with an oxazoline group is not particularly limited as long as it has two or more functional groups reactive with an oxazoline group, such as a carboxyl group, a hydroxyl group, a thiol group, an amino group, a sulfinic acid group, or an epoxy group, but a compound having two or more carboxyl groups is preferred. Note that compounds having functional groups that undergo a crosslinking reaction by heating during thin film formation or in the presence of an acid catalyst, such as sodium salts, potassium salts, lithium salts, and ammonium salts of carboxylic acids, can also be used as crosslinking agents. Specific examples of the compound that undergoes a crosslinking reaction with an oxazoline group include metal salts of synthetic polymers such as polyacrylic acid and copolymers thereof, and natural polymers such as carboxymethylcellulose and alginic acid, which exhibit crosslinking reactivity in the presence of an acid catalyst, and ammonium salts of the above-mentioned synthetic polymers and natural polymers, which exhibit crosslinking reactivity upon heating. In particular, sodium polyacrylate, lithium polyacrylate, ammonium polyacrylate, sodium carboxymethylcellulose, lithium carboxymethylcellulose, ammonium carboxymethylcellulose, and the like, which exhibit crosslinking reactivity in the presence of an acid catalyst or under heating conditions, are preferred.

[0026] Compounds that undergo a crosslinking reaction with such oxazoline groups can be obtained as commercially available products, and examples of such commercially available products include sodium polyacrylate (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd., polymerization degree 2,700 to 7,500), sodium carboxymethylcellulose (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), sodium alginate (manufactured by Kanto Chemical Co., Ltd., Deer Grade 1), Aron A-30 (ammonium polyacrylate, manufactured by Toagosei Co., Ltd., solid content concentration 32 mass%, aqueous solution), DN-800H (ammonium carboxymethylcellulose, manufactured by Daicel FineChem Co., Ltd.), and ammonium alginate (manufactured by Kimika Co., Ltd.).

[0027] Examples of self-crosslinking compounds include compounds that have crosslinkable functional groups in the same molecule that react with each other, such as an aldehyde group, epoxy group, vinyl group, isocyanate group, or alkoxy group with a hydroxyl group, an aldehyde group, amino group, isocyanate group, or epoxy group with a carboxyl group, or an isocyanate group or aldehyde group with an amino group, as well as compounds that have hydroxyl groups (dehydration condensation), mercapto groups (disulfide bonds), ester groups (Claisen condensation), silanol groups (dehydration condensation), vinyl groups, acrylic groups, or the like that react with the same crosslinkable functional groups. Specific examples of self-crosslinking compounds include multifunctional acrylates that exhibit crosslinking reactivity in the presence of an acid catalyst, tetraalkoxysilanes, block copolymers of monomers having a blocked isocyanate group, and monomers having at least one of a hydroxyl group, a carboxylic acid, and an amino group.

[0028] Such a self-crosslinking compound can be obtained as a commercially available product. Examples of such commercially available products include, for example, polyfunctional acrylates such as A-9300 (ethoxylated isocyanuric acid triacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.), A-GLY-9E (ethoxylated glycerine triacrylate (EO9mol), manufactured by Shin-Nakamura Chemical Co., Ltd.), and A-TMMT (pentaerythritol tetraacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.), tetraalkoxysilanes such as tetramethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) and tetraethoxysilane (manufactured by Toyoko Kagaku Co., Ltd.), and polymers having a blocked isocyanate group such as Elastron series E-37, H-3, H38, BAP, NEW BAP-15, C-52, F-29, W-11P, MF-9, and MF-25K (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.).

[0029] These crosslinking agents may be used alone or in combination of two or more kinds. The content of the crosslinking agent varies depending on the solvent used, the base material used, the required viscosity and film shape, etc., but is usually 0.001 to 80 mass % relative to the oxazoline polymer, preferably 0.01 to 50 mass %, and more preferably 0.05 to 40 mass %. The composition of the present invention may contain, as a catalyst for promoting the crosslinking reaction, an acidic compound such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium p-toluenesulfonate, salicylic acid, sulfosalicylic acid, citric acid, benzoic acid, hydroxybenzoic acid, or naphthalenecarboxylic acid, and / or a thermal acid generator such as 2,4,4,6-tetrabromocyclohexadienone, benzoin tosylate, 2-nitrobenzyl tosylate, or an organic sulfonic acid alkyl ester. The content of the catalyst is usually 0.0001 to 20 mass %, preferably 0.0005 to 10 mass %, and more preferably 0.001 to 3 mass %, based on the conductive carbon material dispersant (oxazoline polymer).

[0030] Furthermore, the composition of the present invention may contain other polymers. The content of the polymers is not particularly limited, but is preferably about 0.0001 to 99% by mass, and more preferably about 0.001 to 90% by mass in the composition. Other polymers include fluorine-based resins such as polyvinylidene fluoride (PVdF), polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer [P(VDF-HFP)], and vinylidene fluoride-chlorotrifluoroethylene copolymer [P(VDF-CTFE)]; polyolefin-based resins such as polyvinylpyrrolidone, ethylene-propylene-diene terpolymer, PE (polyethylene), PP (polypropylene), EVA (ethylene-vinyl acetate copolymer), and EEA (ethylene-ethyl acrylate copolymer); polystyrene-based resins such as PS (polystyrene), HIPS (high impact polystyrene), AS (acrylonitrile-styrene copolymer), ABS (acrylonitrile-butadiene-styrene copolymer), MS (methyl methacrylate-styrene copolymer), and styrene-butadiene rubber; polycarbonate resins; vinyl chloride resins; polyamide resins; polyimide resins; and polyacrylic. (Meth)acrylic resins such as sodium acrylate and PMMA (polymethyl methacrylate); polyester resins such as PET (polyethylene terephthalate), polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, PLA (polylactic acid), poly-3-hydroxybutyric acid, polycaprolactone, polybutylene succinate, and polyethylene succinate / adipate; polyphenylene ether resins; modified polyphenylene ether resins; polyacetal resins; polysulfone resins; polyphenylene sulfide resins; polyvinyl alcohol resins; polyglycolic acid; modified starch; cellulose acetate, carboxymethyl cellulose, cellulose triacetate; chitin, chitosan; lignin and other thermoplastic resins, polyaniline and its semi-oxidized form, emeraldine base; polythiophene; polypyrrole; polyphenylene vinylene; polyphenylene; conductive polymers such as polyacetylene, as well as epoxy resins; urethane acrylates; phenolic resins; melamine resins; urea resins;Examples of the solvent include thermosetting resins such as alkyd resins and photocurable resins, but since it is preferable to use water as the solvent in the composition of the present invention, other polymers include water-soluble ones such as sodium polyacrylate, sodium carboxymethylcellulose, water-soluble cellulose ether, sodium alginate, polyvinyl alcohol, polystyrene sulfonic acid, polyethylene glycol, etc., with sodium polyacrylate, sodium carboxymethylcellulose, etc. being particularly preferable;

[0031] Other polymers can also be obtained as commercially available products. Examples of such commercially available products include sodium polyacrylate (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd., polymerization degree 2,700 to 7,500), sodium carboxymethylcellulose (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), sodium alginate (manufactured by Kanto Chemical Co., Ltd., decagrade 1), Metolose SH series (hydroxypropyl methylcellulose, manufactured by Shin-Etsu Chemical Co., Ltd.), Metolose SE series (hydroxyethyl methylcellulose, manufactured by Shin-Etsu Chemical Co., Ltd.), JC-25 (fully saponified polyvinyl alcohol, manufactured by Nippon Vaccination & Poval Co., Ltd.), JM-17 (intermediately saponified polyvinyl alcohol, manufactured by Nippon Vaccination & Poval Co., Ltd.), JP-03 (partially saponified polyvinyl alcohol, manufactured by Nippon Vaccination & Poval Co., Ltd.), and polystyrene sulfonic acid (manufactured by Aldrich, solids concentration 18% by mass, aqueous solution).

[0032] The method for preparing the composition of the present invention is not particularly limited, and a dispersion may be prepared by mixing an oxazoline polymer and a solvent, as well as a crosslinking agent and other polymers that are used as necessary, in any order. In this case, it is preferable to subject the mixture to a dispersion treatment. Examples of the dispersion treatment include mechanical treatments such as wet treatments using a ball mill, a bead mill, a jet mill, or the like, and ultrasonic treatments using a bath or probe type sonicator, with wet treatments using a jet mill and ultrasonic treatments being particularly preferable. The time for the dispersion treatment is not limited, but is preferably about 1 minute to 10 hours, and more preferably about 5 minutes to 5 hours. During this time, a heat treatment may be carried out, if necessary. When optional components such as a crosslinking agent are used, they may be added after the mixture of the oxazoline polymer and the solvent is prepared.

[0033] In the present invention, the solids concentration of the composition is not particularly limited, but in consideration of forming a thin film with a desired thickness, the solids concentration is preferably 20 mass % or less, more preferably 15 mass % or less, and even more preferably 10 mass % or less. The lower limit is arbitrary, but from a practical viewpoint, it is preferably 0.1 mass % or more, more preferably 0.5 mass % or more, and even more preferably 1 mass % or more. The solid content refers to the total amount of components other than the solvent that constitute the composition.

[0034] The oxazoline polymer contained in the composition of the present invention has high adhesion to a current collecting substrate used in an electrode of an energy storage device. Therefore, a thin film obtained from the composition of the present invention is particularly suitable as an adhesive layer that is interposed between a current collecting substrate and an electrode mixture layer that constitute an electrode of an energy storage device and that bonds the two together. Furthermore, although the thin film obtained from the composition of the present invention does not contain a conductive carbon material, it does not affect the conductivity between the current collecting substrate and the electrode mixture layer, and therefore the thin film of the present invention can be used as a functional layer similar to a conventional undercoat layer containing a conductive carbon material. Examples of the energy storage device include various energy storage devices such as an electric double layer capacitor, a lithium secondary battery, a lithium ion secondary battery, a proton polymer battery, a nickel-metal hydride battery, an aluminum solid capacitor, an electrolytic capacitor, and a lead-acid battery. The conductive thin film obtained from the composition for a conductive thin film of the present invention can be particularly suitably applied to electrodes of an electric double layer capacitor and a lithium ion secondary battery.

[0035] In producing an electrode using the composition of the present invention, it is preferable to first form a thin film (undercoat layer) on a current collector using the composition of the present invention to produce a composite current collector. This composite current collector can be prepared by applying the above-mentioned composition onto a current collector and drying it naturally or by heating to form a thin film. The current collector may be one that has been used as a current collector for electrodes for energy storage devices. For example, copper, aluminum, titanium, stainless steel, nickel, gold, silver, and alloys thereof, carbon materials, metal oxides, conductive polymers, etc. may be used, but when the electrode structure is produced by applying welding such as ultrasonic welding, it is preferable to use a metal foil made of copper, aluminum, titanium, stainless steel, or an alloy thereof. The thickness of the current collector is not particularly limited, but in the present invention, it is preferably 1 to 100 μm. The thickness of the thin film is not particularly limited, but in consideration of reducing the internal resistance, it is preferably from 1 nm to 10 μm, more preferably from 1 nm to 1 μm, and even more preferably from 1 to 500 nm.

[0036] The thickness of the thin film can be determined, for example, by cutting a test piece of an appropriate size from the composite current collector, exposing the cross section by a method such as tearing it by hand, and observing the exposed part of the thin film on the cross section with a microscope such as a scanning electron microscope (SEM). The thickness of the thin film can be adjusted by a known method. For example, when the thin film is formed by coating, the thickness can be adjusted by changing the solid content concentration of the composition, the number of coatings, the clearance of the coating liquid inlet of the coater, etc. To make the film thicker, increase the solids concentration, increase the number of coats, or increase the clearance.To make the film thinner, decrease the solids concentration, decrease the number of coats, or decrease the clearance.

[0037] Examples of methods for applying the composition include spin coating, dip coating, flow coating, inkjet coating, casting, spray coating, bar coating, gravure coating, slit coating, roll coating, flexographic printing, transfer printing, brush coating, blade coating, air knife coating, and die coating. From the standpoint of work efficiency and the like, the inkjet method, casting, dip coating, bar coating, blade coating, roll coating, gravure coating, flexographic printing, spray coating, and die coating are preferred. The temperature for drying by heating is not limited, but is preferably about 50 to 200°C, and more preferably about 80 to 150°C.

[0038] The electrode for an energy storage device of the present invention can be produced by forming an electrode mixture layer on the thin film. In this case, the electrode mixture layer may be formed directly on the thin film of the present invention, or may be formed in a manner in which a conventionally known conductive layer containing a conductive carbon material or the like is interposed between the electrode mixture layer and the thin film of the present invention. However, in consideration of reducing the internal resistance of the device, it is preferable to form the electrode mixture layer directly on the thin film of the present invention. Here, as the active material, various active materials that have conventionally been used in electrodes for energy storage devices can be used. For example, in the case of lithium secondary batteries or lithium ion secondary batteries, chalcogen compounds capable of absorbing and releasing lithium ions or lithium ion-containing chalcogen compounds, polyanion compounds, elemental sulfur and compounds thereof, etc. can be used as the positive electrode active material. Examples of chalcogen compounds capable of absorbing and releasing lithium ions include FeS2, TiS2, MoS2, V2O6, and V6O 13 , MnO2, etc. Examples of lithium ion-containing chalcogen compounds include LiCoO2, LiMnO2, LiMn2O4, LiMo2O4, LiV3O8, LiNiO2, and Li x Ni y M 1-yO2 (wherein M represents at least one metal element selected from Co, Mn, Ti, Cr, V, Al, Sn, Pb, and Zn, and 0.05≦x≦1.10, 0.5≦y≦1.0). An example of the polyanion compound is LiFePO4. Examples of sulfur compounds include Li2S and rubeanic acid.

[0039] On the other hand, as the negative electrode active material constituting the negative electrode, at least one element selected from alkali metals, alkali alloys, and elements in Groups 4 to 15 of the periodic table that absorb and release lithium ions, as well as an oxide, sulfide, or nitride, or a carbon material that can reversibly absorb and release lithium ions, can be used. Examples of the alkali metal include Li, Na, and K, and examples of the alkali metal alloy include Li-Al, Li-Mg, Li-Al-Ni, Na-Hg, and Na-Zn. Examples of the simple substance of at least one element selected from the elements of Groups 4 to 15 of the periodic table that absorbs and releases lithium ions include silicon, tin, aluminum, zinc, and arsenic. Similarly, examples of oxides include tin silicon oxide (SnSiO3), lithium bismuth oxide (Li3BiO4), lithium zinc oxide (Li2ZnO2), and lithium titanium oxide (Li4Ti5O 12 ), titanium oxide, etc. Similarly, lithium iron sulfide (Li x FeS2(0≦x≦3)), lithium copper sulfide (Li x CuS (0≦x≦3) etc. Similarly, examples of the nitride include lithium-containing transition metal nitrides, specifically Li x M y Examples include N (M=Co, Ni, Cu, 0≦x≦3, 0≦y≦0.5), lithium iron nitride (Li3FeN4), etc. Examples of carbon materials capable of reversibly absorbing and releasing lithium ions include graphite, carbon black, coke, glassy carbon, carbon fiber, carbon nanotubes, and sintered bodies of these.

[0040] In the case of an electric double layer capacitor, a carbonaceous material can be used as the active material. The carbonaceous material may be activated carbon, for example, activated carbon obtained by carbonizing a phenolic resin and then activating the carbon.

[0041] The electrode mixture layer can be formed by applying an electrode slurry prepared by mixing the active material described above, the binder polymer described below, and a solvent as necessary, onto the thin film of the present invention, and drying it naturally or by heating.

[0042] The binder polymer can be appropriately selected from known materials and used, and examples thereof include conductive polymers such as polyvinylidene fluoride (PVdF), polyvinylpyrrolidone, polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer [P(VDF-HFP)], vinylidene fluoride-chlorotrifluoroethylene copolymer [P(VDF-CTFE)], polyvinyl alcohol, polyimide, ethylene-propylene-diene terpolymer, styrene-butadiene rubber, carboxymethylcellulose (CMC), polyacrylic acid (PAA), and polyaniline. The amount of the binder polymer added is preferably 0.1 to 20 parts by mass, and particularly preferably 1 to 10 parts by mass, per 100 parts by mass of the active material. Examples of the solvent include those exemplified as the solvent for the composition above. An appropriate solvent may be selected from these solvents depending on the type of binder. In the case of a water-insoluble binder such as PVdF, NMP is preferred, and in the case of a water-soluble binder such as PAA, water is preferred.

[0043] The electrode slurry may contain a conductive material, such as carbon black, ketjen black, acetylene black, carbon whiskers, carbon fiber, natural graphite, artificial graphite, titanium oxide, ruthenium oxide, aluminum, and nickel.

[0044] The electrode slurry can be applied by the same method as the above-mentioned composition application method. The temperature for drying by heating may also be any temperature, but is preferably about 50 to 400°C, and more preferably about 80 to 150°C.

[0045] The electrode may be pressed as necessary. In this case, the pressing pressure is preferably 1 kN / cm or more. A commonly used pressing method can be used, but a mold pressing method or a roll pressing method is particularly preferred. The pressing pressure is not particularly limited, but is preferably 2 kN / cm or more, and more preferably 3 kN / cm or more. The upper limit of the pressing pressure is preferably about 40 kN / cm, and more preferably about 30 kN / cm.

[0046] The energy storage device of the present invention is equipped with the above-mentioned energy storage device electrode, and more specifically, is configured with at least a pair of positive and negative electrodes, a separator interposed between the electrodes, and an electrolyte, and at least one of the positive and negative electrodes is configured from the above-mentioned energy storage device electrode. This energy storage device is characterized by using the above-mentioned energy storage device electrodes as the electrodes, and other device components such as a separator and an electrolyte can be appropriately selected from known materials and used. Examples of the separator include a cellulose-based separator and a polyolefin-based separator. The electrolyte may be either liquid or solid, and may be either aqueous or non-aqueous, but the electrode for an energy storage device of the present invention can exhibit sufficient practical performance even when applied to a device using a non-aqueous electrolyte.

[0047] The non-aqueous electrolyte may be a non-aqueous electrolytic solution obtained by dissolving an electrolyte salt in a non-aqueous organic solvent. Examples of the electrolyte salt include lithium salts such as lithium tetrafluoroborate, lithium hexafluorophosphate, lithium perchlorate, and lithium trifluoromethanesulfonate; quaternary ammonium salts such as tetramethylammonium hexafluorophosphate, tetraethylammonium hexafluorophosphate, tetrapropylammonium hexafluorophosphate, methyltriethylammonium hexafluorophosphate, tetraethylammonium tetrafluoroborate, and tetraethylammonium perchlorate; and lithium imides such as lithium bis(trifluoromethanesulfonyl)imide and lithium bis(fluorosulfonyl)imide. Examples of the non-aqueous organic solvent include alkylene carbonates such as propylene carbonate, ethylene carbonate, and butylene carbonate; dialkyl carbonates such as dimethyl carbonate, methyl ethyl carbonate, and diethyl carbonate; nitriles such as acetonitrile; and amides such as dimethylformamide.

[0048] The shape of the energy storage device is not particularly limited, and various types of cells known in the art, such as a cylindrical type, a flat wound rectangular type, a laminated rectangular type, a coin type, a flat wound laminate type, and a laminated type, can be used. When applied to a coin type, the above-mentioned electrode for an energy storage device of the present invention may be punched into a predetermined disk shape and used. For example, a lithium-ion secondary battery can be produced by placing one electrode on a lid of a coin cell to which a washer and spacer are welded, placing a separator of the same shape impregnated with an electrolyte on top of that, and then placing the electrode for an energy storage device of the present invention on top with the electrode mixture layer facing down, placing a case and gasket on top, and sealing with a coin cell crimping machine.

[0049] When applied to a laminate type, an electrode structure can be used in which an electrode mixture layer is formed on part or the entire surface of the thin film (undercoat layer) of the present invention, and a metal tab is welded to the part (weld) where the electrode mixture layer is not formed. In this case, the electrode structure may include one or more electrodes, but generally, multiple positive and negative electrodes are used. It is preferable that the multiple electrodes for forming the positive electrode are stacked alternately with the multiple electrodes for forming the negative electrode, and in this case, it is preferable to interpose the above-mentioned separator between the positive electrode and the negative electrode. The metal tab may be welded to the welded portion of the outermost electrode of the plurality of electrodes, or may be welded by sandwiching the metal tab between the welded portions of any two adjacent electrodes of the plurality of electrodes.

[0050] The material of the metal tab is not particularly limited as long as it is one that is generally used in energy storage devices, and examples thereof include metals such as nickel, aluminum, titanium, and copper; and alloys such as stainless steel, nickel alloys, aluminum alloys, titanium alloys, and copper alloys. However, taking into consideration welding efficiency, it is preferable that the material is composed of at least one metal selected from aluminum, copper, and nickel. The metal tab is preferably in the form of a foil, and its thickness is preferably about 0.05 to 1 mm.

[0051] The welding method may be a known method used for welding metals together, specific examples of which include TIG welding, spot welding, laser welding, ultrasonic welding, etc., but it is preferable to join the electrode and the metal tab by ultrasonic welding. Examples of ultrasonic welding techniques include a technique in which multiple electrodes are placed between an anvil and a horn, a metal tab is placed at the weld, and ultrasonic waves are applied to weld them all at once, and a technique in which the electrodes are first welded together and then the metal tab is welded. In the present invention, in either method, not only are the metal tabs and the electrodes welded to each other at the welded portions, but the electrodes are also ultrasonically welded to each other. The pressure, frequency, output, processing time, etc. during welding are not particularly limited, and may be appropriately set taking into consideration the materials used, the presence or absence of an undercoat layer, the coating weight, etc. The electrode structure produced as described above is housed in a laminate pack, the above-mentioned electrolyte solution is injected, and the pack is heat-sealed to obtain a laminate cell. EXAMPLES

[0052] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The following devices were used for measurements, etc. (1) Probe-type ultrasound irradiation device Hielscher Ultrasonics, UIP1000 (2) Wire bar coater (forming the undercoat layer) PM-9050MC, manufactured by SMT Corporation (3) Homodisper (mixing of electrode slurry) TK Robomix (with Homo Disper 2.5 type (φ32)) manufactured by Primix Corporation (4) Bead mill (mixing electrode slurry) Mitsubishi Electric Corporation, FREQROL-E500 (5) Rotation and revolution mixer (degassing of electrode slurry) Thinky Corporation's Awatori Rentaro (ARE-310) (6) Roll press machine (electrode compression) SA-602, manufactured by Takumi Giken Co., Ltd. (7) Charge / discharge measuring device (secondary battery evaluation) Toyo Systems Co., Ltd., TOSCAT-3100 (8) Coin cell crimping machine Manual coin crimping machine CR2032 manufactured by Hosen Co., Ltd.

[0053] [1] Preparation of thin film-forming composition [Example 1-1] 6.94 g of WS-700 (manufactured by Nippon Shokubai Co., Ltd., solids concentration: 25.0% by mass), an aqueous solution containing an oxazoline polymer, 2.42 g of Aron A-30 (manufactured by Toagosei Co., Ltd., solids concentration: 31.6% by mass), an aqueous solution containing ammonium polyacrylate, and 40.64 g of pure water were mixed to prepare a thin film forming composition A, which is a homogeneous solution.

[0054] [Comparative Example 1-1] 2.00g of WS-700 (manufactured by Nippon Shokubai Co., Ltd., solid content concentration: 25.0 mass%), which is an aqueous solution containing an oxazoline polymer, 40.15g of pure water, and 7.35g of 2-propanol (manufactured by Junsei Chemical Co., Ltd., special reagent grade) were mixed, and 0.50g of TC-2010 (manufactured by Toda Kogyo Co., Ltd., multi-layered CNT), which is an electrically conductive carbon material, was further mixed therein. The obtained mixture was subjected to ultrasonic treatment for 30 minutes using a probe-type ultrasonic irradiation device, and a dispersion liquid in which the electrically conductive carbon material was uniformly dispersed was prepared. 0.70g of Aron A-30 (manufactured by Toagosei Co., Ltd., solid content concentration: 31.6 mass%), which is an aqueous solution containing ammonium polyacrylate (PAA-NH4), 41.84g of pure water, and 7.47g of 2-propanol (manufactured by Junsei Chemical Co., Ltd., special reagent grade) was mixed therein to prepare a thin film forming composition B, which is a uniform CNT dispersion liquid.

[0055] [2] Manufacturing of composite current collectors [Example 2-1] The thin film forming composition A prepared in Example 1-1 was uniformly spread on a copper foil (thickness 15 μm) current collector using a wire bar coater, and then dried at 110° C. for 20 minutes to form an undercoat layer, thereby producing a composite current collector A. The basis weight was measured and found to be 50 mg / m 2 It was.

[0056] [Comparative Example 2-1] A composite current collector B was produced in the same manner as in Example 2-1, except that the thin film-forming composition A was changed to the thin film-forming composition B prepared in Comparative Example 1-1. The basis weight was measured and found to be 47 mg / m 2 It was.

[0057] [3] Electrode manufacturing and adhesion evaluation [Example 3-1] 13.5 g of silicon (manufactured by Japan NER Co., Ltd.) as an active material, 3.6 g of polyacrylic acid (PAA, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a binder, 0.9 g of acetylene black (AB, manufactured by Denka Co., Ltd.) as a conductive assistant, and 42.0 g of water were mixed for 5 minutes at 3,000 rpm using a homodisper. Next, the mixture was mixed for 30 minutes at 2,000 rpm using a bead mill, and further degassed for 2 minutes at 1,000 rpm using a rotation-revolution mixer to prepare an electrode slurry (solid concentration 30 mass%, silicon: PAA: AB = 75: 20: 5 (mass ratio)). The obtained electrode slurry was spread on the composite current collector A prepared in Example 2-1, and then dried at 80 ° C for 30 minutes and then at 120 ° C for 30 minutes to form an active material layer on the undercoat layer, and further pressed with a roll press machine at a pressing pressure of 1.2 kN / cm to prepare an electrode A.

[0058] [Comparative Example 3-1] An electrode B was produced in the same manner as in Example 3-1, except that the composite current collector A was changed to the composite current collector B produced in Comparative Example 2-1.

[0059] [Comparative Example 3-2] An electrode C was produced in the same manner as in Example 3-1, except that the composite current collector A was changed to a pure copper foil.

[0060] Electrodes A to C prepared in Example 3-1 and Comparative Examples 3-1 and 3-2 were each cut into a width of 25 mm, and a 20 mm wide double-sided tape was attached to the electrode composite layer coating surface to fix it on a glass substrate. This was fixed to an adhesion / film peeling analyzer and a peeling test was performed at a peel angle of 90° and a peeling speed of 100 mm / min to measure the adhesion. The results are shown in Table 1.

[0061] [Table 1]

[0062] As shown in Table 1, the electrode of Example 3-1 having a thin film made using thin film-forming composition A not containing a conductive carbon material has superior adhesion both before and after pressing, compared to the electrode of Comparative Example 3-1 having a thin film containing a conductive carbon material and the electrode of Comparative Example 3-2 using a pure copper foil. In other words, it is found that the undercoat layer obtained from thin film-forming composition A has superior adhesion to the active material.

[0063] [4] Electrode fabrication and cycle characteristics evaluation [Example 4-1] 2.16 g of silicon monoxide (SiO, manufactured by Osaka Titanium Technologies Co., Ltd.) as an active material, 5.04 g of graphite (SNO-10, manufactured by SEC Carbon Co., Ltd.), 0.23 g of lithium polyacrylate (PAALi) as a binder, 0.39 g of acetylene black (AB, manufactured by Denka Co., Ltd.) as a conductive additive, and 11.69 g of water were mixed in a centrifugal mixer to prepare an electrode slurry (solid concentration 40 mass%, SiO:SNO-10:PAALi:AB=27.6:64.4:3.0:5.0 (mass ratio)). The obtained electrode slurry was spread on a composite current collector A, dried at 80°C for 30 minutes to form an active material layer on the undercoat layer, and further pressed with a roll press at a pressure of 0.1 kN / cm to prepare an electrode D.

[0064] [Comparative Example 4-1] Except for changing the composite current collector A to the composite current collector B, an electrode E was produced in the same manner as in Example 4-1.

[0065] [Comparative Example 4-2] An electrode F was produced in the same manner as in Example 4-1, except that the composite current collector A was changed to a pure copper foil.

[0066] From each of the electrodes D to F produced in the above Example 4-1 and Comparative Examples 4-1 and 4-2, three disk-shaped electrodes having a diameter of 10 mm were punched out, and the mass of the electrode layer (the mass of the punched-out electrode minus the mass of the uncoated electrode portion punched out to a diameter of 10 mm) and the thickness of the electrode layer (the thickness of the punched-out electrode minus the thickness of the substrate) were measured, and the electrodes were vacuum-dried at 120°C for 15 hours and transferred to a glove box filled with argon. A gasket and a lithium foil (Honjo Chemical Co., Ltd., thickness 0.17 mm) punched to a diameter of 14 mm were placed on the lid of a 2032-type coin cell (Hosen Co., Ltd.) to which a washer and spacer were welded, and 100 μL of electrolyte (Kishida Chemical Co., Ltd., ethylene carbonate: dimethyl carbonate = 3: 7 (volume ratio), containing 1.2 mol / L of lithium hexafluorophosphate as an electrolyte and 20 vol% of fluoroethylene carbonate as an additive) were dropped on top of the gasket and then a separator (Celgard Co., Ltd., Celgard #2400) punched to a diameter of 16 mm was placed on top of the gasket and then an electrode was placed on top of the electrode with the surface coated with the active material facing down. After dropping 200 μL of electrolyte, a lid with a washer and spacer welded on top of the gasket and then sealed with a coin cell crimping machine. After that, the cell was left to stand for 15 hours, and three secondary batteries for testing were made.

[0067] The electrochemical characteristics of the fabricated test secondary battery were evaluated. In order to evaluate the effect of the undercoat layer on the battery, a charge-discharge test was performed using a charge-discharge measuring device under the conditions shown in Table 2. The results of the first cycle of the cycle test are shown in Figure 1.

[0068] [Table 2] Cutoff voltage: 1.5-0.005V Number of test batteries: 3 ·Temperature: Room temperature Constant voltage charging is cut off at 1 / 10 of each rate

[0069] As shown in FIG. 1, the battery including the composite current collector A having an undercoat layer prepared using the thin film forming composition of the present invention that does not contain a conductive carbon material exhibits initial characteristics equivalent to those of the battery including the composite current collector B having an undercoat layer prepared from a composition that contains a conductive carbon material, despite the absence of a conductive carbon material.

[0070] [5] Evaluation of storage stability and coatability of thin film forming compositions [Example 5-1, Comparative Example 5-1] The coatability was evaluated visually for the case where composite current collector A and composite current collector B were prepared using thin film forming composition A and thin film forming composition B immediately after preparation in Example 1-1 and Comparative Example 1-1 above, and the case where composite current collector A and composite current collector B were prepared using thin film forming composition A and thin film forming composition B after being left to stand at 50°C in an air atmosphere for 14 days after preparation. The evaluation was made as follows: ◯: uniform coatable; ×: coatable due to some agglomerates observed. The results are shown in Table 3. In addition, the particle size of each of the thin film-forming compositions A and B was measured immediately after preparation and after leaving them at 50° C. in an air atmosphere for 14 days. The median diameter (d 50 The results are shown in Table 3.

[0071] [Table 3]

[0072] As shown in Table 3, the thin film forming composition A prepared in Example 1-1 does not contain a conductive carbon material, and therefore does not suffer from non-uniformity due to aggregation of the conductive carbon material, the composition itself is stable, and has excellent coatability even after long-term storage.

Claims

1. A thin film-forming composition for an energy storage device electrode, for forming a thin film interposed between a current collector and an electrode mixture layer of the energy storage device electrode, comprising: A composition for forming a thin film for an energy storage device electrode, comprising a polymer having an oxazoline group in a side chain and a solvent, and not containing a conductive carbon material.

2. The thin film-forming composition for energy storage device electrodes according to claim 1, wherein the polymer is a radical polymer of at least two types of monomers: an oxazoline monomer having a polymerizable carbon-carbon double bond-containing group at the 2-position; and a (meth)acrylic monomer having a hydrophilic functional group.

3. The thin film-forming composition for energy storage device electrodes according to claim 2, wherein the polymer is a radical polymer of an oxazoline monomer represented by formula (1) having a polymerizable carbon-carbon double bond-containing group at the 2-position, and one or more (meth)acrylic monomers having a hydrophilic functional group selected from (meth)acrylic acid, 2-hydroxyethyl acrylate, methoxypolyethylene glycol acrylate, a monoester of acrylic acid and polyethylene glycol, 2-aminoethyl acrylate and its salts, 2-hydroxyethyl methacrylate, methoxypolyethylene glycol methacrylate, a monoester of methacrylic acid and polyethylene glycol, 2-aminoethyl methacrylate and its salts, sodium (meth)acrylate, ammonium (meth)acrylate, (meth)acrylonitrile, (meth)acrylamide, N-methylol(meth)acrylamide, and N-(2-hydroxyethyl)(meth)acrylamide. 【Chemistry 1】 (In the formula, X represents a chain hydrocarbon group containing a polymerizable carbon-carbon double bond, R 1 ~R 4 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 5 carbon atoms which may have a branched structure, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms.

4. An undercoat layer comprising a thin film obtained from the composition for forming a thin film for an energy storage device electrode according to any one of claims 1 to 3.

5. A composite current collector for an electrode of an energy storage device, comprising the undercoat layer according to claim 4.

6. An electrode for an energy storage device, comprising the composite current collector for an energy storage device electrode according to claim 5.

7. An energy storage device comprising the electrode for an energy storage device according to claim 6.

8. 8. The energy storage device according to claim 7, which is a lithium ion secondary battery.

Citation Information

Patent Citations

  • Positive electrode for lithium secondary battery, and its manufacturing method

    JP2010170965A

  • Composition for electrode slurry for battery

    JP2016072147A

  • Aqueous composition for forming secondary battery electrode, secondary battery electrode, and secondary battery

    WO2012133030A1

  • Composite current collector for energy storage device electrode, and electrode

    WO2014042080A1

  • Agent for dispersing electrically conductive carbon material, and dispersion of electrically conductive carbon material

    WO2015029949A1