Steel plates, components and their manufacturing methods
A steel composition and manufacturing process for high-strength steel sheets with controlled microstructure and cooling rates address the challenges of achieving excellent formability and stability, enabling complex automobile parts production with reduced scrap.
Patent Information
- Application Number
- JP2023567952
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-09-15
- Filing Date
- 2023-06-29
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2043-06-29
AI Technical Summary
Existing high-strength steel sheets face challenges in achieving tensile strength of 780 MPa or more with excellent press formability, ductility, stretch flange formability, and material stability in the width direction, as well as sufficient ductility for forming complex automobile parts, while minimizing environmental impact through reduced scrap generation.
A steel composition with specific chemical elements (C: 0.05-0.20%, Si: 0.40-1.50%, Mn: 1.9-3.5%, controlled microstructure of polygonal ferrite, bainite, martensite, and retained austenite, and a manufacturing process involving annealing and controlled cooling rates to achieve the desired properties.
The solution results in a steel plate with high tensile strength, improved press formability, ductility, and stable material properties across the width, enabling the production of complex automobile components with reduced scrap and enhanced yield.
Smart Images

Figure 0007559978000001 
Figure 0007559978000002 
Figure 0007559978000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel plate, a member, and a manufacturing method thereof. More specifically, the present invention relates to a steel plate, a member, and a manufacturing method thereof, which has a tensile strength (TS) of 780 MPa or more and has excellent formability and material stability. The present invention relates to a steel plate, a member, and a manufacturing method thereof, which are used in various applications such as automobiles. [Background technology]
[0002] In recent years, the strengthening of CO2 emission regulations for automobiles has been promoted within an international framework from the viewpoint of global environmental conservation. The most effective way to improve the fuel efficiency of automobiles is to reduce the weight of automobile bodies by using thinner steel sheets for automobile frame members, and the use of high-strength steel sheets has been increasing with the aim of contributing to low fuel consumption of automobiles. In general, as the strength of steel sheets increases, they become more susceptible to cracking during press forming due to reduced ductility and stretch flange formability. For this reason, steel sheets with improved ductility and stretch flange formability compared to conventional steel sheets are desired. In addition, as the strength increases, the yield ratio (YR) (YR = yield strength YS / tensile strength TS) increases, which increases the springback after forming, resulting in a problem of reduced dimensional accuracy after press forming. From the viewpoint of press formability, therefore, steel sheets with low YR are desired.
[0003] On the other hand, from the viewpoint of carbon neutrality, the amount of CO2 emissions generated in all processes from material production to product manufacturing is also an important indicator. Therefore, if the amount of scrap generated during product manufacturing increases, the total amount of CO2 emitted will increase, and there is concern that the environmental burden will increase. For this reason, there is a demand for using up all the materials in the manufacturing process (improving yield), and excellent material stability in the plate width direction is also required for steel plates. However, as the strength of steel plates increases, variations in formability such as ductility in the plate width direction and hole expandability become apparent. This makes it easier for cracks to occur during press forming, and therefore there is a need to set restrictions on the blanking position in order to ensure quality, which poses the issue of reduced yield.
[0004] As a technology for improving the formability of high-strength steel sheets, TRIP steel sheets with residual austenite dispersed in the structure have been developed. For example, Patent Document 1 discloses that austempering (carbon distribution associated with bainite transformation) is performed by annealing steel containing 0.04-0.12% C, 0.8-2.5% Si, and 0.5-2.0% Mn at 300-500°C for 10-900 seconds to generate 2-10% residual γ, thereby obtaining a steel sheet with high ductility (TS×El≧21000MPa·%) and high stretch flange formability of 70% or more.
[0005] DP steel (Dual Phase steel) has been developed as a steel sheet with low YR and excellent ductility that is effective in reducing springback. A typical DP steel is a multi-phase steel with martensite dispersed in the ferrite structure, which is the main phase. However, DP steel has a drawback in that it has poor stretch flange formability because cracks are easily generated due to stress concentration at the interface between ferrite and martensite. For example, Patent Document 2 and Patent Document 3 disclose technologies for improving the stretch flange formability of DP steel.
[0006] Patent Document 2 discloses that the volume fraction of ferrite in the entire structure is controlled to 5 to 30%, the volume fraction of martensite is controlled to 50 to 95%, and the ferrite grains are controlled to have an average grain size of 3 μm or less in equivalent circle diameter, and the martensite grains are controlled to have an average grain size of 6 μm or less in equivalent circle diameter, thereby improving ductility and stretch flange formability.
[0007] Patent Document 3 discloses a technology for suppressing deterioration of stretch flange formability by controlling the volume fraction of ferrite to 50% or more and the volume fraction of martensite to 3 to 30% relative to the total structure, and by setting the average grain size of ferrite to 10 μm or less and the average grain size of martensite to 5 μm or less. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent No. 5515623 [Patent Document 2] JP 2008-297609 A [Patent Document 3] Patent No. 3936440 Summary of the Invention [Problem to be solved by the invention]
[0009] However, although Patent Document 1 and Patent Document 2 disclose a method for manufacturing a steel sheet having excellent ductility and stretch flange formability, it is difficult to further increase the strength to, for example, 780 MPa or more, because it is necessary to form a large amount of soft phase ferrite. In addition, Patent Document 3 discloses a method for manufacturing a DP steel sheet having low YR and excellent ductility and stretch flange formability, but since it is a DP structure, the area ratio of the martensite structure increases as the strength of the steel sheet increases, decreasing the ductility, and it has become clear that the ductility is not necessarily sufficient in forming difficult-to-form parts such as center pillars, as breakage is observed at the bending ridge where ductility is required. In addition, none of the patent documents discloses a technology for suppressing the variation in ductility and stretch flange formability in the sheet width direction. Therefore, from the viewpoint of press formability, there is a demand for the development of a high-strength steel sheet having low YR, excellent ductility and stretch flange formability, and excellent material stability in the sheet width direction from the viewpoint of improving material yield. In view of the above circumstances, the present invention aims to provide a steel plate, a member, and a manufacturing method thereof, which have a tensile strength (TS) of 780 MPa or more, excellent press formability, ductility, and stretch flange formability, and excellent material stability in the plate width direction.
[0010] Here, the tensile strength refers to the tensile strength (TS) obtained in accordance with JIS Z2241 (2011). Excellent press formability means that the yield ratio YR obtained in accordance with JIS Z2241 (2011) is 0.8 or less. The term "excellent ductility" means that the total elongation EL obtained in accordance with JIS Z2241 (2011) satisfies any one of the following (A) to (C). (A) TS: 780MPa or more but less than 980MPa, EL: 16.0% or more, (B) TS: 980 MPa or more but less than 1180 MPa, EL: 14.0% or more, (C) TS: 1180MPa or more, EL: 12.0% or more The term "excellent stretch flange formability" means that the hole expansion ratio λ(%) (={(d-d0) / d0}×100) obtained by a hole expansion test conforming to the JFST1001 regulations is 30% or more. "Excellent material stability in the sheet width direction" means that the sheet width of region A, which continuously satisfies the following formulas (1) and (2) with respect to EL and λ at measurement position X in the sheet width direction, is 80% or more of the total sheet width. -10≦100×[(EL(%) at measurement position X in area A - EL(%) at center of strip width) / EL(%) at center of strip width]≦10 (1) -10≦100×[(λ(%) at measurement position X in area A - λ(%) at center of strip width) / λ(%) at center of strip width]≦10 (2) (In formulas (1) and (2), the measurement positions X are 23 positions in total among the 24 divided positions of the width W of the steel plate (the 23 contact positions of adjacent widths when the width W is divided into 24 equal widths). In other words, the measurement positions X are W / 24, 2W / 24, 3W / 24, 4W / 24, 5W / 24, 6W / 24, 7W / 24, 8W / 24, 9W / 24, 10W / 24, 11W / 24, 12W / 24, 13W / 24, 14W / 24, 15W / 24, 16W / 24, 17W / 24, 18W / 24, 19W / 24, 20W / 24, 21W / 24, 22W / 24, and 23W / 24, totaling 23 positions.) Here, for example, when the measurement position X where the formula (1) and the formula (2) are continuously satisfied is 2W / 24 to 20W / 24, the sheet width of the region A where the formula (1) and the formula (2) are continuously satisfied is 100×(20-2+1) / 23=83% of the total sheet width. [Means for solving the problem]
[0011] In order to solve the above problems, the present inventors have thoroughly investigated various factors affecting press formability, ductility, stretch flange formability and material stability of various thin steel sheets having a tensile strength of 780 MPa or more from the viewpoints of the chemical composition and microstructure of the steel sheets and manufacturing conditions. As a result, the steel contains, by mass%, C: 0.05 to 0.20%, Si: 0.40 to 1.50%, Mn: 1.9 to 3.5%, P: 0.02% or less, S: 0.01% or less, sol.Al: 1.00% or less, and N: less than 0.015%, the area ratio of polygonal ferrite is 10% to 80%, the total area ratio of upper bainite, tempered martensite, and lower bainite is 10% to 70%, the area ratio of retained austenite (residual γ) is 3% to 15%, and the area ratio of quenched martensite is 15% or less (including 0%). In addition, the total area ratio (volume factor) of quenched martensite and retained γ with an aspect ratio of 3 or less and a circle equivalent diameter of 2.0 μm or more with respect to the total area of quenched martensite and retained γ is 20% or less, and the C concentration is 0.5 mass% or more. C≧0.5 It has been discovered that by making the steel structure such that the area ratio of the above-mentioned thin film CrNbO2 to the entire structure is 20% or less, it is possible to obtain a high-strength cold-rolled steel sheet that has excellent press formability, ductility, and stretch flange formability, as well as excellent material stability in the sheet width direction (small material variation).
[0012] The present invention has been made based on the above findings, and the gist of the present invention is as follows. [1] In mass percent, C: 0.05-0.20%, Si: 0.40-1.50%, Mn: 1.9-3.5%, P: 0.02% or less, S: 0.01% or less, Sol.Al: 1.00% or less, N: Contains less than 0.015% The balance being iron and unavoidable impurities; Area ratio of polygonal ferrite: 10% or more and 80% or less, The total area ratio of upper bainite, tempered martensite and lower bainite is 10% or more and 70% or less, Volume fraction of retained austenite: 3% or more and 15% or less; Area ratio of hardened martensite: 15% or less (including 0%), Further, the steel structure is composed of a remaining structure, The total area ratio of the quenched martensite and the retained austenite having an aspect ratio of 3 or less and an equivalent circle diameter of 2.0 μm or more is 20% or less, The carbon-enriched region (S C≧0.5 ) is 20% or less in area. [2] The component composition further includes, in mass%, Ti: 0.1% or less, B: 0.01% or less, The steel plate according to [1], containing one or two selected from the following: [3] The component composition further includes, in mass%, Cu: 1% or less, Ni: 1% or less, Cr: 1% or less, Mo: 0.5% or less V: 0.5% or less, Nb: 0.1% or less, The steel sheet according to [1] or [2], containing one or more selected from the following: [4] The component composition further includes, in mass%, Mg: 0.0050% or less, Ca: 0.0050% or less, Sn: 0.1% or less, Sb: 0.1% or less, REM: 0.0050% or less, The steel sheet according to any one of [1] to [3], which contains one or more selected from the following: [5] The steel sheet according to any one of [1] to [4], which has a zinc plating layer on a surface thereof. [6] A member made using the steel plate according to any one of [1] to [5]. [7] A method for producing a steel sheet, comprising: subjecting a steel slab having a chemical composition according to any one of [1] to [4] to hot rolling, pickling and cold rolling; and then annealing the resulting cold-rolled steel sheet, The annealing is A holding step of heating the cold-rolled steel sheet to an annealing temperature of 750 to 880 ° C. and holding the annealing temperature for 10 to 500 seconds; A first cooling step of cooling the annealed material to a first cooling stop temperature of 350 to 550° C. at a first average cooling rate of 2 to 50° C. / s; A second cooling step in which the steel is held at a residence temperature of 350 to 550°C for 10 to 60 seconds and then cooled to a second cooling stop temperature of 150 to 360°C at a second average cooling rate of 3 to 50°C / s; and a third cooling step of cooling the steel sheet at a third average cooling rate of 0.05 to 1.0°C / s in a temperature range from the second cooling stop temperature to 50°C. [8] The method for producing a steel sheet according to [7], wherein in the second cooling step, the steel sheet is retained at a retention temperature of 350 to 550°C for 10 s to 60 s, and a hot-dip galvanizing treatment or an alloyed hot-dip galvanizing treatment is performed on a surface of the steel sheet. [9] The method for producing a steel sheet according to [7], further comprising the step of: after the annealing, subjecting the surface of the steel sheet to an electrolytic galvanizing treatment.
[10] A method for producing a component, comprising the step of subjecting the steel plate according to any one of [1] to [5] to at least one of forming and joining to form a component. Effect of the Invention
[0013] According to the present invention, it is possible to obtain a steel sheet which has a high strength, tensile strength TS of 780 MPa or more, excellent press formability, ductility and stretch flange formability, and excellent material stability in the sheet width direction. When the steel sheet of the present invention is applied to the frame members of an automobile body, it can be used to manufacture difficult-to-form parts of complex shapes by cold pressing, which can contribute greatly to reducing the weight of the automobile body. Furthermore, since the material variation in the plate width direction is small, the blanking position of the steel sheet is not limited, and the material yield can be significantly improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be specifically described below. Note that the present invention is not limited to the following embodiments. The steel sheet of the present invention contains, by mass%, C: 0.05-0.20%, Si: 0.40-1.50%, Mn: 1.9-3.5%, P: 0.02% or less, S: 0.01% or less, sol.Al: 1.00% or less, N: less than 0.015%, with the balance being iron and unavoidable impurities. The steel sheet of the present invention has a composition in which the area ratio of polygonal ferrite is 10% or more and 80% or less, the total area ratio of upper bainite, tempered martensite, and lower bainite is 10% or more and 70% or less, and the residual austenite is 0.02% or less. The steel structure has a volume fraction of quenched martensite of 3% or more and 15% or less, an area fraction of quenched martensite of 15% or less (including 0%), and further comprises a residual structure, and the total area fraction of quenched martensite and retained austenite has an aspect ratio of 3 or less and a circle equivalent diameter of 2.0 μm or more relative to the total area fraction of quenched martensite and retained austenite of 20% or less, and a C concentration of 0.5 mass% or more relative to the total structure. C≧0.5 ) is 20% or less. Hereinafter, the steel sheet of the present invention will be described in the order of chemical composition and steel structure. First, the reasons for limiting the chemical composition of the present invention will be described. In the following description, all % indicating the steel composition is mass % unless otherwise specified.
[0015] <C:0.05~0.20%> C is added from the viewpoints of securing a predetermined strength through transformation strengthening and of securing a predetermined amount of retained austenite (residual γ) to improve ductility. If the C content is less than 0.05%, these effects cannot be sufficiently secured. On the other hand, if the C content exceeds 0.20%, the martensitic transformation start temperature (Ms point) decreases. As a result, in the third cooling step in which cooling is performed at a third average cooling rate of 0.05 to 1.0°C / s in the temperature range from the second cooling stop temperature to 50°C, martensitic transformation and the subsequent tempering of martensite do not occur sufficiently. Therefore, the hardened martensite and the 0.5 mass% or more C enriched region (S C≧0.5 ) is promoted, resulting in a decrease in stretch flangeability and material stability in the plate width direction. For this reason, the C content is set to 0.05% or more and 0.20% or less. The C content is preferably 0.08% or more. Also, the C content is preferably 0.18% or less.
[0016] <Si:0.40~1.50%> Silicon is added from the viewpoints of strengthening ferrite to increase strength, and suppressing the formation of carbides in martensite and bainite to secure a predetermined amount of retained γ and improve ductility. If the Si content is less than 0.40%, these effects cannot be sufficiently secured. On the other hand, when the Si content exceeds 1.50%, carbon partitioning to untransformed austenite is excessively promoted, and the C enriched region (S C≧0.5 ) is promoted, which reduces the stretch flangeability and the material stability in the sheet width direction. Therefore, the Si content is set to 0.40% or more and 1.50% or less. The Si content is preferably 0.60% or more. Also, the Si content is preferably 1.20% or less.
[0017] <Mn:1.9~3.5%> Mn is added from the viewpoints of improving the hardenability of steel sheets, promoting high strength through transformation strengthening, and improving ductility by promoting the formation of retained austenite, which, like Si, suppresses the formation of carbides in bainite and contributes to ductility. To obtain these effects, a Mn content of 1.9% or more is required. On the other hand, if the Mn content exceeds 3.5%, the bainite transformation is significantly delayed, the required amount of retained austenite cannot be secured, and the ductility is reduced. On the other hand, when the Mn content exceeds 3.5%, it becomes difficult to suppress the formation of coarse martensite after quenching, and the stretch flange formability deteriorates. Therefore, the Mn content is set to 1.9% or more and 3.5% or less. The Mn content is preferably 2.1% or more. Also, the Mn content is preferably 3.3% or less.
[0018] <P: 0.02% or less> P is an element that strengthens steel, but when its content is high, it deteriorates the spot weldability. Therefore, the P content is set to 0.02% or less, and preferably 0.01% or less. Although it may not contain P, since it takes a great cost to reduce it to less than 0.001%, the P content is preferably 0.001% or more.
[0019] <S: 0.01% or less> S has the effect of improving the scale peelability during hot rolling and suppressing nitriding during annealing, but it is an element that has an adverse effect on spot weldability, bendability, and hole expansion property. In order to reduce these adverse effects, at least the S content is set to 0.01% or less, and preferably 0.0020% or less. Although it may not contain S, since it takes a great cost to reduce it to less than 0.0001%, the S content is preferably 0.0001% or more from the viewpoint of manufacturing cost. The S content is more preferably 0.0005% or more, and still more preferably 0.0015% or more.
[0020] <sol.Al: 1.00% or less> Al is contained for the purpose of deoxidation or obtaining residual γ. The lower limit of sol.Al is not particularly defined, but in order to perform deoxidation stably, the sol.Al content is preferably 0.005% or more. The sol.Al content is more preferably 0.010% or more, and still more preferably 0.020% or more. On the other hand, when the sol.Al content exceeds 1.00%, a large amount of Al-based coarse inclusions increases, and the stretch flange formability decreases. Therefore, the sol.Al content is set to 1.00% or less.
[0021] <Less than 0.015% N> N is an element that forms nitrides such as BN, AlN, and TiN in steel and reduces the elongation flange formability. Therefore, it is necessary to limit its content. Thus, the N content is less than 0.015%. The N content is preferably 0.010% or less, and more preferably 0.005% or less. Note that it may not contain N, but it would cost a great deal to reduce it to less than 0.0001%. Therefore, from the perspective of manufacturing cost, the N content is preferably 0.0001% or more. The N content is more preferably 0.0010% or more, and even more preferably 0.0020% or more.
[0022] The component composition of the steel sheet in the present invention contains the above component elements as basic components, and the balance contains iron (Fe) and unavoidable impurities. Note that the component composition of the steel sheet in the present invention preferably has a component composition in which the balance consists of Fe and unavoidable impurities. In addition to the above components, the component composition of the steel sheet of the present invention can appropriately contain one or more selected from the following (A) to (C) as optional elements. (A) One or two selected from Ti: 0.1% or less and B: 0.01% or less (B) One or more selected from Cu: 1% or less, Ni: 1% or less, Cr: 1% or less, Mo: 0.5% or less, V: 0.5% or less, and Nb: 0.1% or less (C) One or more selected from Mg: 0.0050% or less, Ca: 0.0050% or less, Sn: 0.1% or less, Sb: 0.1% or less, and REM: 0.0050% or less
[0023] <Ti: 0.1% or less> Ti can fix N in steel as TiN, which has the effect of improving hot ductility and the effect of improving the hardenability of B. In addition, it has the effect of refining the structure due to the precipitation of TiC. To obtain these effects, it is desirable to set the Ti content to 0.002% or more. From the perspective of sufficiently fixing N, it is more preferable to set the Ti content to 0.008% or more. The Ti content is more preferably 0.010% or more. On the other hand, when the Ti content exceeds 0.1%, it will lead to an increase in rolling load and a decrease in ductility due to an increase in the amount of precipitation strengthening. Therefore, when containing Ti, the Ti content should be 0.1% or less. Preferably, the Ti content is 0.05% or less, and more preferably 0.03% or less.
[0024] <B: 0.01% or less> B is an element that improves the hardenability of steel and has the advantage of easily generating tempered martensite and / or bainite with a predetermined area ratio. Therefore, it is preferable to set the B content to 0.0005% or more. More preferably, the B content is 0.0010% or more. On the other hand, when the B content exceeds 0.01%, not only does its effect saturate, but it also causes a significant decrease in hot ductility and surface defects. Therefore, when containing B, the B content should be 0.01% or less. Preferably, the B content is 0.005% or less, and more preferably 0.003% or less.
[0025] <Cu: 1% or less> Cu improves the corrosion resistance in the usage environment of automobiles. In addition, the corrosion products of Cu can coat the surface of the steel plate and have the effect of suppressing hydrogen intrusion into the steel plate. Cu is an element that is mixed in when using scrap as a raw material. By allowing the mixing of Cu, recycled materials can be utilized as raw materials, and the manufacturing cost can be reduced. From such a perspective, it is preferable to contain 0.005% or more of Cu. From the perspective of further improving the stress corrosion cracking resistance characteristics, it is more preferable to contain 0.05% or more of Cu. The Cu content is more preferably 0.10% or more. More preferably, the Cu content is 0.25% or more, and even more preferably 0.50% or more. However, if the Cu content is too high, it will cause the generation of surface defects. Therefore, when containing Cu, the Cu content should be 1% or less.
[0026] <Ni: 1% or less> Ni, like Cu, is an element that has the effect of improving corrosion resistance. Also, Ni has the effect of suppressing the generation of surface defects that are likely to occur when containing Cu. Therefore, it is desirable to contain Ni at 0.01% or more. The Ni content is more preferably 0.04% or more, and even more preferably 0.06% or more. However, if the Ni content is too high, the scale formation in the heating furnace will become non-uniform, which will instead cause surface defects. Also, it will lead to an increase in cost. Therefore, when containing Ni, the Ni content should be 1% or less. Preferably, the Ni content is 0.5% or less, and more preferably 0.3% or less.
[0027] <Cr: 1% or less> Cr can be contained due to its effect of improving the hardenability of steel and its effect of suppressing carbide formation in martensite and upper / lower bainite. To obtain such effects, the Cr content is preferably 0.01% or more. The Cr content is more preferably 0.03% or more, and even more preferably 0.06% or more. However, if Cr is contained in excess, the pitting corrosion resistance will deteriorate. Therefore, when containing Cr, the Cr content should be 1% or less.
[0028] <Mo: 0.5% or less> Mo can be contained due to its effect of improving the hardenability of steel and its effect of suppressing carbide formation in martensite and upper / lower bainite. To obtain such effects, the Mo content is preferably 0.01% or more. The Mo content is more preferably 0.03% or more, and even more preferably 0.06% or more. More preferably, the Mo content is 0.1% or more, and even more preferably 0.2% or more. However, since Mo significantly deteriorates the chemical conversion treatment property of cold-rolled steel sheets, when Mo is contained, the Mo content should be 0.5% or less.
[0029] <V: 0.5% or less> V can be contained due to its effects of improving the hardenability of steel, suppressing carbide formation in martensite and upper / lower bainite, refining the structure, and precipitating carbides to improve the stress corrosion cracking resistance. To obtain these effects, the V content is preferably 0.003% or more. The V content is more preferably 0.005% or more, still more preferably 0.010% or more. Even more preferably, the V content is 0.020% or more, and even more preferably 0.050% or more. However, when a large amount of V is contained, the castability significantly deteriorates. Therefore, when V is contained, the V content should be 0.5% or less. Preferably, the V content is 0.3% or less, and more preferably 0.2% or less.
[0030] <Nb: 0.1% or less> Nb can be contained due to its effects of refining the steel structure and increasing the strength, promoting bainite transformation through grain refinement, improving bendability, and enhancing stress corrosion cracking resistance. To obtain these effects, the Nb content is preferably 0.002% or more. The Nb content is more preferably 0.004% or more, still more preferably 0.010% or more. However, when a large amount of Nb is contained, the precipitation strengthening becomes too strong and the ductility decreases. Also, it causes an increase in rolling load and deterioration of castability. Therefore, when Nb is contained, the Nb content should be 0.1% or less. Preferably, the Nb content is 0.05% or less, and more preferably 0.03% or less.
[0031] <Mg: 0.0050% or less> Mg fixes O as MgO and contributes to the improvement of formability such as bendability. Therefore, the Mg content is preferably 0.0002% or more. The Mg content is more preferably 0.0004% or more, and even more preferably 0.0006% or more. On the other hand, when a large amount of Mg is added, the surface quality and bendability deteriorate. Therefore, when Mg is contained, the Mg content is 0.0050% or less. Preferably, the Mg content is 0.0040% or less.
[0032] <Ca: 0.0050% or less> Ca fixes S as CaS and contributes to the improvement of bendability and the improvement of stress relaxation fracture resistance characteristics. Therefore, the Ca content is preferably 0.0002% or more. The Ca content is more preferably 0.0005% or more, and even more preferably 0.0010% or more. On the other hand, when a large amount of Ca is added, the surface quality and bendability deteriorate. Therefore, when Ca is contained, the Ca content is 0.0050% or less. Preferably, the Ca content is 0.0040% or less.
[0033] <Sn: 0.1% or less> Sn suppresses oxidation and nitridation of the steel sheet surface layer portion, and suppresses the reduction of the content of C and B in the surface layer due to this. Due to this effect, the formation of ferrite in the steel sheet surface layer portion is suppressed, the strength is increased, and the fatigue resistance characteristics are improved. From such a viewpoint, the Sn content is preferably 0.002% or more. The Sn content is more preferably 0.004% or more, and even more preferably 0.006% or more. More preferably, the Sn content is 0.008% or more, and even more preferably 0.010% or more. The Sn content is preferably 0.030% or more, and more preferably 0.060% or more. On the other hand, when the Sn content exceeds 0.1%, the castability deteriorates. Also, Sn segregates at the old γ grain boundaries, and the stress relaxation fracture resistance characteristics deteriorate. Therefore, when Sn is contained, the Sn content is 0.1% or less.
[0034] <Sb: 0.1% or less> Sb suppresses oxidation and nitridation of the surface layer of the steel sheet, thereby suppressing the reduction in the content of C and B in the surface layer. Due to this effect, ferrite formation in the surface layer of the steel sheet is suppressed, the strength is increased, and the fatigue resistance characteristics are improved. From such a viewpoint, the Sb content is preferably 0.002% or more. The Sb content is more preferably 0.004% or more, and still more preferably 0.006% or more. More preferably, the Sb content is 0.008% or more, and even more preferably 0.010% or more. The Sb content is preferably 0.025% or more, and more preferably 0.050% or more. On the other hand, when the Sb content exceeds 0.1%, the castability deteriorates, and it segregates at the prior γ grain boundaries, resulting in deterioration of the stress corrosion cracking resistance characteristics. Therefore, when containing Sb, the Sb content should be 0.1% or less.
[0035] <REM:0.0050% or less> REM is an element that suppresses the adverse effect of sulfide on the stretch flange formability by spheroidizing the shape of sulfide and improves the stretch flange formability. In order to obtain these effects, it is preferable to set the REM content to 0.0005% or more. The REM content is more preferably 0.0010% or more, and still more preferably 0.0020% or more. On the other hand, when the REM content exceeds 0.0050%, the improvement effect of the stretch flange formability saturates. Therefore, when containing REM, the REM content should be 0.0050% or less.
[0036] In addition, REM as used in the present invention refers to scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and lanthanoid elements from lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. The REM concentration in the present invention is the total content of one or more elements selected from the above-mentioned REM. REM is not particularly limited, but it is preferably included Sc, Y, Ce, and La.
[0037] When the optional components are contained in amounts less than the lower limit, the optional elements contained in amounts less than the lower limit do not impair the effects of the present invention. Therefore, when the optional elements are contained in amounts less than the lower limit, the optional elements are considered to be contained as inevitable impurities.
[0038] Next, the mechanical properties of the steel sheet (cold-rolled steel sheet excellent in material stability) to which the present invention is directed will be described.
[0039] The steel sheet of the present invention has a tensile strength (TS) of 780 MPa or more. There is no particular upper limit to the tensile strength, but from the viewpoint of compatibility with other properties, the tensile strength is preferably 1300 MPa or less.
[0040] In the steel sheet of the present invention, the total elongation EL is ensured to be 16.0% or more at TS: 780 MPa or more, 14.0% or more at TS: 980 MPa or more, and 12.0% or more at TS: 1180 MPa or more, thereby significantly improving the stability of press forming. By ensuring that the hole expansion ratio λ is 30% or more, cracks during press forming can be suppressed, so λ is set to 30% or more.
[0041] In the steel sheet of the present invention, the sheet width of region A where EL and λ at measurement position X in the sheet width direction continuously satisfy the following formulas (1) and (2) is 80% or more of the total sheet width. -10≦100×[(EL(%) at measurement position X in area A - EL(%) at center of strip width) / EL(%) at center of strip width]≦10 (1) -10≦100×[(λ(%) at measurement position X in area A - λ(%) at center of strip width) / λ(%) at center of strip width]≦10 (2) In formulas (1) and (2), the measurement positions X are 23 positions in total among the 24 division positions of the width W of the steel plate (23 contact positions of adjacent widths when the width W is divided into 24 equal widths). That is, the measurement positions X are 23 positions in total, namely, W / 24, 2W / 24, 3W / 24, 4W / 24, 5W / 24, 6W / 24, 7W / 24, 8W / 24, 9W / 24, 10W / 24, 11W / 24, 12W / 24, 13W / 24, 14W / 24, 15W / 24, 16W / 24, 17W / 24, 18W / 24, 19W / 24, 20W / 24, 21W / 24, 22W / 24, and 23W / 24 in the width direction. Here, for example, when the measurement position X where the formula (1) and the formula (2) are continuously satisfied is 2W / 24 to 20W / 24, the sheet width of the region A where the formula (1) and the formula (2) are continuously satisfied is 100×(20-2+1) / 23=83% of the total sheet width. In the steel sheet of the present invention, the above-mentioned region A has a length in the sheet width direction that is 80% or more of the entire sheet width. In other words, the area where the deviation of EL in the strip width direction is 10% or less from the measured value at the strip width center position and the deviation of λ in the strip width direction is 10% or less from the measured value at the strip width center position is set to be 80% or more of the entire strip width area. The range of the unsteady part is permitted to be up to 20% in total at both ends in the strip width direction. The very ends of the steel plates are not used to ensure quality because they come into contact with other structures during transportation and work processes. For this reason, the usable effective plate width does not reach 100%. Therefore, it is preferable to make the effective plate width less than 100%. By making the region where the deviation of EL in the sheet width direction is 10% or less of the measured value at the sheet width center position and the deviation of λ is 10% or less 80% or more of the entire sheet width, the yield can be significantly improved, so in the present invention, the region where the deviation of EL in the sheet width direction is 10% or less of the measured value at the sheet width center position and the deviation of λ is 10% or less is 80% or more of the entire sheet width, preferably 85% or more.
[0042] <YR≦0.8、TS≧780MPa、EL≧16.0%> <YR≦0.8、TS≧980MPa、EL≧14.0%> <YR≦0.8、TS≧1180MPa、EL≧12.0%> To evaluate tensile properties, a JIS No. 5 tensile test piece is taken from the center of the plate width, and a tensile test (in accordance with JIS Z2241 (2011)) is performed with N=3. Each evaluation is based on the average value of the three points. A steel plate with a tensile strength of 780 MPa or more is considered to be a high-strength steel plate. A steel plate with a yield ratio YR of 0.8 or less is considered to have excellent press formability. A steel plate with a total elongation EL of 16.0% or more for TS: 780 MPa or more, 14.0% or more for TS: 980 MPa or more, and 12.0% or more for TS: 1180 MPa or more is considered to have excellent ductility.
[0043] <λ≧30%> The evaluation of stretch flange formability is performed by taking a test piece from the center position of the sheet width, and performing a hole expansion test in accordance with the provisions of the Japan Iron and Steel Federation standard JFST1001 with N=3. That is, after punching a sample of 100 mm x 100 mm square size using a punching tool with a punch diameter of 10 mm and a clearance of 13%, a conical punch with an apex angle of 60 degrees is used to expand the hole until a crack penetrating the sheet thickness occurs, with the burrs generated during the formation of the punched hole being on the outside. In this case, d0: initial hole diameter (mm), d: hole diameter at the time of crack occurrence (mm), the hole expansion ratio λ (%) = {(d-d0) / d0} × 100 is calculated, and the average value of the three points obtained by carrying out the test is evaluated as λ. A steel having λ of 30% or more is judged to have excellent hole expansion properties and excellent stretch flangeability. It is preferably 40% or more.
[0044] <Evaluation of material stability in the plate width direction> To evaluate the material stability in the width direction, 23 points (including the width center) of the evaluation material are taken from both width directions at intervals of 100 mm or less from the width center position (the 12W / 24 position mentioned above), and EL and λ are calculated at each position (measurement position X).The material stability in the width direction is evaluated by calculating the ratio of the difference between the measurement value at the width center position and each position to the measurement value at the width center position. Using EL and λ at the center of the plate width as the standard, the group of consecutive measurements in which the difference in EL and λ is 10% or less is defined as the region in which the difference in EL and λ is 10% or less, and steel in which this region accounts for 80% or more of the total plate width is determined to have excellent material stability. The width of the steel plate in the present invention is preferably 600 mm or more, and 1700 mm or less.
[0045] Next, the steel structure of the steel plate of the present invention will be described.
[0046] <Area ratio of polygonal ferrite: 10% to 80%> From the viewpoint of ensuring a low YR and high ductility, the area ratio of polygonal ferrite is set to 10% or more, and in order to obtain even higher ductility, it is preferably set to 20% or more. On the other hand, if the polygonal ferrite exceeds 80%, the desired strength cannot be obtained, so the area ratio of polygonal ferrite is set to 80% or less, preferably 75% or less, and more preferably 70%.
[0047] <Total area ratio of upper bainite, tempered martensite and lower bainite: 10% to 70%> In order to obtain a desired strength, the total area ratio of upper bainite, tempered martensite and lower bainite is set to 10% or more, and in order to obtain even higher strength, it is preferably set to 15% or more. However, if the total area ratio of upper bainite, tempered martensite and lower bainite exceeds 70%, ductility decreases due to excessively high strength, so the area ratio is set to 70% or less, more preferably 65% or less, and further preferably 60% or less.
[0048] <Volume fraction of retained austenite (retained γ): 3% to 15%> If the volume fraction of retained austenite falls below 3%, the desired ductility cannot be ensured. From the viewpoint of ductility, the volume fraction of the retained austenite is set to 3% or more, and preferably 5% or more. On the other hand, if the retained austenite exceeds 15%, the stretch flangeability is deteriorated, so the retained austenite is set to 15% or less, and more preferably 13% or less.
[0049] <Area ratio of hardened martensite: 15% or less (including 0%)> Since the hard quenched martensite structure reduces λ, its area ratio must be suppressed. To obtain the desired λ, the area ratio of quenched martensite is set to 15% or less. To obtain λ more stably, the area ratio of quenched martensite is preferably 12% or less, more preferably 10% or less.
[0050] <Remaining organization> The steel structure is made up of the remaining structure except for the above. The area ratio of the remaining structure is preferably 5% or less. The remaining structure may be carbide or pearlite. These structures may be determined by SEM observation as described later.
[0051] <Total area ratio of quenched martensite and retained austenite with an aspect ratio of 3 or less and a circle equivalent diameter of 2.0 μm or more relative to the total area ratio of quenched martensite and retained austenite: 20% or less> The retained austenite becomes a hard martensite structure due to the TRIP effect during press forming, tensile processing, etc. Therefore, in the present invention, from the viewpoint of stretch flangeability, the quenched martensite and the retained austenite are controlled together. When quenched martensite or retained austenite with a circle equivalent diameter of 2.0 μm or more is formed, voids are formed at the stress concentration area at the interface with other structures, which may deteriorate the stretch flangeability. Furthermore, when the aspect ratio of quenched martensite or retained austenite is 3 or less, stress concentration is likely to occur at the interface with other structures, which may promote void formation and deteriorate stretch flange formability. Therefore, the total area ratio of quenched martensite and retained austenite with an aspect ratio of 3 or less and a circle equivalent diameter of 2.0 μm or more is set to 20% or less relative to the total area ratio of quenched martensite and retained austenite. This total area ratio is preferably 18% or less, and more preferably 16% or less. The total area ratio of quenched martensite and retained austenite having an aspect ratio of 3 or less and an equivalent circle diameter of 2.0 μm or more relative to the total area ratio of quenched martensite and retained austenite is not particularly limited, but since it is difficult to control it to 0% from the viewpoint of operability, it is preferably 2% or more, and more preferably 4% or more. The above-mentioned equivalent circle diameter is preferably 20.0 μm or less.
[0052] <C-enriched region (S C≧0.5 ) Area ratio: 20% or less The hardness of quenched martensite is determined by the amount of C dissolved in the quenched martensite. When the difference in hardness between quenched martensite and other structures increases, the formation of voids is promoted at the interface of the stress concentration area. Structures with a large amount of dissolved C are quenched martensite and retained austenite. Retained austenite is a structure that contributes to high ductility, and has a C concentration of 0.5 mass% or more. If the area ratio of structures with a C concentration of 0.5 mass% or more is 20% or less for all constituent structures, it is possible to ensure stretch flange formability while improving ductility, and it is also possible to reduce the variation in material properties in the plate width direction, making it possible to manufacture steel plate with excellent material stability. For this reason, the C-enriched region (S C≧0.5 The area ratio (space factor) of the insulating layer 20 is 20% or less. This area ratio is preferably 15% or less, and more preferably 12% or less. Moreover, this area ratio is preferably 3% or more, and more preferably 5% or more.
[0053] Next, a method for measuring the steel structure will be described.
[0054] The area ratios of polygonal ferrite, upper bainite, tempered martensite, lower bainite, and hardened martensite (fresh martensite) were measured by cutting out a cross section of the plate thickness parallel to the rolling direction, mirror-polishing it, and then etching it with 1 vol% nital. Ten fields of view were observed at 5,000x magnification using an SEM at the 1 / 4 thickness position, and the photographed structure was quantified using image analysis. Polygonal ferrite is a relatively equiaxed ferrite with almost no carbides inside. It is the area that appears the blackest under SEM. Upper bainite is a ferrite structure with the formation of carbides or retained austenite inside that appear white under SEM. If it is difficult to distinguish between upper bainite and polygonal ferrite, the region of ferrite with an aspect ratio of ≦2.0 is classified as polygonal ferrite, and the region with an aspect ratio >2.0 is classified as upper bainite, and the area ratio is calculated. Here, the aspect ratio is calculated by determining the major axis length a at which the particle length is the longest, and the minor axis length b at the particle length when it crosses the particle the longest in the direction perpendicular to that, and a / b is the aspect ratio. Tempered martensite and lower bainite are regions with lath-shaped substructure and carbide precipitation inside when viewed under SEM. Hardened martensite (fresh martensite) is a blocky region that appears white under an SEM, with no internal substructure visible. The remaining structure is a carbide and / or pearlite structure, which can be confirmed by white contrast under SEM. Carbide has a particle size of 1 μm or less, and pearlite can be distinguished from carbide because it has a lamellar (layer) structure.
[0055] The above-mentioned quantitative evaluation of the structure and the measurement of the aspect ratio and equivalent circle diameter of the quenched martensite and the retained austenite can be performed using image analysis software, for example, Image J (Fiji). A cross section of the plate parallel to the rolling direction is cut out, mirror-polished, and then etched with 1 vol% nital. Ten fields of view are observed at 5000x magnification with an SEM at the 1 / 4 thickness position, and each structure is identified and quantitatively evaluated using the Trainable Weka segmentation method, which can identify regions using machine learning in Image J (Fiji). In addition, the aspect ratio and circle equivalent diameter of the quenched martensite and retained austenite can be measured using a particle analysis program, which is also a function of Image J, and only the quenched martensite and retained austenite identified as described above are extracted and measured.
[0056] The volume fraction of retained austenite is determined by chemically polishing the surface layer at 1 / 4 thickness position and then performing X-ray diffraction. A Co-Kα source is used for the incident X-rays, and the volume fraction of retained austenite is calculated from the intensity ratio of the (200), (211), and (220) planes of ferrite to the (200), (220), and (311) planes of austenite. Here, since the retained austenite is randomly distributed, the volume fraction of retained austenite determined by X-ray diffraction can be taken as the area fraction of retained austenite.
[0057] The area ratio S of the C-enriched region where the C concentration is 0.5 mass% or more C≧0.5 The measurement was performed at 1 / 4 of the thickness of the plate cross section parallel to the rolling direction using a JEOL field emission electron probe microanalyzer (FE-EPMA) JXA-8500F. The acceleration voltage was 6 kV and the probe current was 7 × 10 -8 A: The C concentration distribution is measured by mapping analysis with the beam diameter at its minimum, and the area ratio where the C concentration is 0.5 mass% or more is calculated. However, to eliminate the effects of contamination, the background amount is subtracted so that the average value of C obtained in the analysis is equal to the carbon amount in the base material. In other words, if the average value of the measured carbon amount is greater than the carbon amount in the base material, the increase is considered to be contamination, and the true carbon amount at each position is determined by subtracting the increase uniformly from the analysis value at each position.
[0058] Next, a method for producing a steel sheet according to the present invention will be described. The method for producing a steel sheet of the present invention is a method for producing a steel sheet, which comprises hot rolling, pickling and cold rolling a steel slab having the above-mentioned composition, and then annealing the obtained cold-rolled steel sheet. The annealing includes a holding step of heating the cold-rolled steel sheet to an annealing temperature of 750 to 880 ° C. and holding the annealing temperature for 10 to 500 seconds, a first cooling step of cooling the cold-rolled steel sheet to the first cooling stop temperature at a first average cooling rate of 2 to 50 ° C. / s in a temperature range from the annealing temperature to a first cooling stop temperature of 350 to 550 ° C., a second cooling step of holding the steel sheet at a holding temperature of 350 to 550 ° C. for 10 s or more and 60 s or less, and then cooling the steel sheet to a second cooling stop temperature of 150 to 360 ° C. at a second average cooling rate of 3 to 50 ° C. / s, and a third cooling step of cooling the steel sheet to a temperature range from the second cooling stop temperature to 50 ° C. at a third average cooling rate of 0.05 to 1.0 ° C. / s.
[0059] <Hot rolling> Methods for hot rolling a steel slab include a method of heating the slab and then rolling it, a method of directly rolling the slab after continuous casting without heating it, and a method of rolling the slab after continuous casting after subjecting it to a short-term heat treatment. Hot rolling may be performed according to a conventional method, and for example, the slab heating temperature may be 1100 to 1300°C, the soaking temperature may be 20 to 300 min, the finish rolling temperature may be Ar3 transformation point to Ar3 transformation point + 200°C, and the coiling temperature may be 400 to 720°C. From the viewpoint of suppressing thickness fluctuation and stably ensuring high strength, the coiling temperature is preferably 430 to 530°C. The Ar3 transformation point can be calculated from the composition of the steel sheet and the following empirical formula (A). Ar3=910-203×[C]+44.7×[Mn]-30×[Si]+700×[P]+400×[sol.Al]-20×[B]+31.5×[Mo]+104×[V]+400×[Ti]...(A) In formula (A), [element] means the content (mass%) of each element. (An element that is not contained is 0 (zero) mass%).)
[0060] <Pickling> The pickling may be carried out in a conventional manner.
[0061] <Cold rolling> Cold rolling may be performed according to a conventional method, and the cumulative rolling reduction may be 30 to 85%. From the viewpoint of stably securing high strength and reducing anisotropy, the rolling reduction is preferably 35 to 85%. When the rolling load is high, softening annealing treatment can be performed at 450 to 730°C in a CAL (continuous annealing line) or BAF (box annealing furnace).
[0062] <Annealing> A cold-rolled steel sheet manufactured according to a conventional method is annealed under the following conditions. The annealing equipment is not particularly limited, but from the viewpoints of productivity and ensuring the desired heating and cooling rates, it is preferable to carry out the annealing in a continuous annealing line (CAL) or a continuous hot-dip galvanizing line (CGL).
[0063] [Holding process: Heat to an annealing temperature in the annealing temperature range of 750 to 880°C and hold at the annealing temperature for 10 to 500 seconds] If the annealing temperature (soaking temperature) is below 750°C, recrystallization does not occur sufficiently, and the processed structure during cold rolling remains, reducing formability. Furthermore, if the annealing temperature (soaking temperature) is below 750°C, the amount of polygonal ferrite increases, increasing the amount of C and Mn that concentrate in the reverse transformed austenite, making it difficult to obtain sufficient upper bainite, tempered martensite, lower bainite, and retained austenite, and therefore making it impossible to ensure the desired strength and ductility. For this reason, the annealing temperature (soaking temperature) is set to 750°C or higher. On the other hand, if the annealing temperature (soaking temperature) exceeds 880°C, the austenite single phase temperature is obtained, the desired polygonal ferrite cannot be obtained, the YR increases, and the ductility decreases. Therefore, the annealing temperature (soaking temperature) is set to 880°C or less. The annealing temperature (soaking temperature) is preferably 850°C or less, and more preferably 830°C or less.
[0064] Furthermore, if the time (soaking time) for holding at the annealing temperature is less than 10 seconds, the formation of austenite at the annealing temperature (soaking temperature) is insufficient, polygonal ferrite increases, and the specified amounts of upper bainite, tempered martensite, and lower bainite are not obtained, making it impossible to obtain the desired strength, and also making it impossible to obtain sufficient retained austenite, thereby failing to ensure the desired ductility. On the other hand, if the time for holding at the annealing temperature (soaking time) exceeds 500 seconds, the structure will become significantly coarse, making it impossible to ensure the desired strength. Therefore, the time for holding at the annealing temperature (soaking time) is 10 to 500 seconds. The time for holding at the annealing temperature (soaking time) is preferably 80 seconds or more, and more preferably 100 seconds or more. The time for holding at the annealing temperature (soaking time) is preferably 400 seconds or less, and more preferably 300 seconds or less.
[0065] [First cooling step: Cooling from the annealing temperature to the first cooling stop temperature of 350-550°C at a first average cooling rate of 2-50°C / s] After holding at a soaking temperature of 750°C to 880°C (after the above holding step), the steel sheet is cooled at a first average cooling rate of 2 to 50°C / s in the temperature range from the annealing temperature to a first cooling stop temperature of 350 to 550°C. If the first average cooling rate is less than 2°C / s, the operability decreases, so the first average cooling rate is set to 2°C / s or more. The first average cooling rate is preferably 5°C / s or more. On the other hand, if the first average cooling rate is too high, the sheet shape deteriorates, so the first average cooling rate is set to 50° C. / s or less. The first average cooling rate is preferably 40° C. / s or less, and more preferably less than 30° C. / s. Here, the first average cooling rate is "(annealing temperature (°C)-first cooling stop temperature (°C)) / cooling time (seconds) from the annealing temperature to the first cooling stop temperature".
[0066] [Second cooling step (1): Retention at 350-550℃ for 10s to 60s] At temperatures below the first cooling stop temperature and in the temperature range of 350°C to 550°C (dwell temperature), upper bainite can be formed, a predetermined amount of retained austenite can be obtained, and the desired ductility can be obtained. Bainite transformation has an incubation period, and the material must be held at that temperature for a certain period of time. If the holding temperature range including the holding start temperature (=first cooling stop temperature) and holding end temperature is outside the range of 350 to 550°C, and / or the holding time (hereinafter also referred to as holding time) is less than 10 s, the desired amount of bainite cannot be obtained, the formation of retained austenite is suppressed, and the desired ductility cannot be obtained. On the other hand, if the holding time exceeds 60 s, the concentration of C from bainite to the blocky untransformed γ progresses, leading to an increase in the amount of remaining blocky structure, and the desired λ cannot be obtained. Therefore, the holding time is set to 10 s or more and 60 s or less.
[0067] [Second cooling step (2): Cool to a second cooling stop temperature of 150 to 360°C at a second average cooling rate of 3 to 50°C / s] After the above-mentioned retention, it is necessary to cool quickly so that carbon concentration in the untransformed austenite does not proceed too much. If the average cooling rate in the temperature range from the retention end temperature to the cooling stop temperature of 150°C to 360°C is less than 3°C / s, carbon will concentrate into a block of untransformed γ, the amount of quenched martensite at the time of final cooling will increase, and λ will decrease. Therefore, from the viewpoint of improving λ, the second average cooling rate in the temperature range from the retention end temperature to the second cooling stop temperature of 150°C to 360°C is set to 3°C / s or more. The second average cooling rate is preferably 5°C / s or more, more preferably 8°C / s or more. If the cooling rate in this temperature range is too high, the sheet shape will deteriorate, so the cooling rate in this temperature range (second average cooling rate) is set to 50°C / s or less. It is preferably 40°C / s or less. If the second cooling stop temperature exceeds 360°C, the tempered martensite or lower bainite will not reach a predetermined area ratio, the area ratio of quenched martensite after annealing will increase, and stretch flange formability will deteriorate. For this reason, the second cooling stop temperature is set to 360°C or lower. On the other hand, if the second cooling end temperature is less than 150°C, the tempering effect of martensite cannot be sufficiently obtained during the cooling to 50°C in the next process, and not only does the amount of quenched martensite increase, but the C-enriched region (S C≧0.5 ) becomes excessive, which deteriorates the stretch flangeability. In addition, the volume fraction of retained austenite does not fall within the desired range, and sufficient ductility cannot be obtained. For this reason, the second cooling stop temperature is set to 150°C or higher. Here, the second average cooling rate is "retention end temperature (°C)-second cooling stop temperature (°C) / cooling time (seconds) from the retention end temperature to the second cooling stop temperature".
[0068] [Third cooling step: Cool the temperature range from the second cooling stop temperature to 50°C at a third average cooling rate of 0.05-1.0°C / s] If the cooling rate in the temperature range from the second cooling stop temperature to 50° C. exceeds 1.0° C. / s, the tempering effect of martensite is not sufficiently obtained, and the desired amount of retained austenite cannot be obtained. In addition, the C enrichment region (S C≧0.5 ) increases, which deteriorates the stretch flangeability and the material stability in the sheet width direction. For this reason, the cooling rate in the temperature range from the second cooling stop temperature to 50°C (third average cooling rate) is set to 1.0°C / s or less. By setting the cooling rate in the temperature range from the second cooling stop temperature to 50°C (third average cooling rate) to 1.0°C / s or less, the temperature variation in the sheet width direction can also be reduced, and the material stability in the sheet width direction can be further improved. On the other hand, if the cooling rate in the temperature range from the cooling stop temperature to 50° C. is slow, the treatment time becomes long and the operability deteriorates. For this reason, the cooling rate in the temperature range from the cooling stop temperature to 50° C. (third average cooling rate) is set to 0.05° C. / s or more. The third average cooling rate is preferably 0.08° C. / s or more, more preferably 0.10° C. / s or more. The third average cooling rate is preferably 0.80° C. / s or less, more preferably 0.60° C. / s or less. Here, the third average cooling rate is "second cooling stop temperature (°C)-50°C / cooling time (seconds) from the second cooling stop temperature (°C) to 50°C."
[0069] The surface of the steel sheet may be subjected to a galvanizing treatment to obtain a steel sheet having a galvanized layer on the surface. The type of plating treatment is not particularly limited, and may be either hot-dip galvanizing or electrogalvanizing. Furthermore, as an alloying hot-dip galvanizing treatment, a plating treatment for alloying may be performed after hot-dip galvanizing. Hot-dip galvanizing is used for automotive steel sheets, etc. When hot-dip galvanizing is performed, the steel sheet may be immersed in a hot-dip galvanizing bath after the holding step and the first cooling step in the above-mentioned annealing in a continuous annealing furnace at the upstream stage of a continuous hot-dip galvanizing line to form a hot-dip galvanized layer on the surface of the steel sheet, and further, may be subjected to an alloying treatment thereafter to produce an alloyed hot-dip galvanized steel sheet. Specifically, in the above-mentioned second cooling step, the steel sheet surface can be subjected to hot-dip galvanizing treatment or galvannealing hot-dip galvanizing treatment when it is retained at a retention temperature of 350 to 550° C. for 10 s to 60 s. The above-mentioned soaking and cooling steps and the plating step may each be performed in a separate line. Alternatively, electrolytic galvanization can be carried out after annealing, i.e., after the third cooling step.
[0070] The thickness of the steel plate of the present invention thus obtained is preferably 0.5 mm or more, and more preferably 2.0 mm or less. The sheet width is preferably 600 mm or more. The sheet width of the steel sheet of the present invention is preferably 1700 mm or less.
[0071] Next, the member of the present invention and the method for producing the same will be described.
[0072] The member of the present invention is obtained by subjecting the steel plate of the present invention to at least one of forming and joining. Also, the method for producing the member of the present invention includes a step of subjecting the steel plate of the present invention to at least one of forming and joining to obtain the member.
[0073] The steel plate of the present invention has a tensile strength of 780 MPa or more, is excellent in press formability, ductility, and stretch flange formability, and is excellent in material stability in the plate width direction. Therefore, a member obtained by using the steel plate of the present invention also has high strength, is excellent in press formability, ductility, and stretch flange formability, and is excellent in material stability in the plate width direction. In addition, the member of the present invention can be used to reduce weight. Therefore, the member of the present invention can be suitably used, for example, for vehicle body frame parts. The member of the present invention also includes a welded joint.
[0074] The forming process may be performed by a general processing method such as pressing, without any restrictions. The joining process may be performed by a general welding method such as spot welding or arc welding, riveting, or crimping, without any restrictions. EXAMPLES
[0075] A slab having the chemical composition shown in Table 1 produced by continuous casting was heated to 1200°C, and subjected to a hot rolling process in which the soaking time was 200 min., the finish rolling temperature was 900°C, and the coiling temperature was 550°C. The resulting cold-rolled steel sheet having a thickness of 1.4 mm was then cold-rolled at a rolling reduction ratio of 50%. The cold-rolled steel sheet was treated under the annealing conditions shown in Table 2 to produce the steel sheet of the present invention and the steel sheet of the comparative example. The width of the obtained steel plates was all 1500 mm.
[0076] [Table 1]
[0077] In addition, some of the steel sheets (cold-rolled steel sheets: CR) were subjected to a hot-dip galvanizing process when they were held at a holding temperature of 350 to 550°C for 10 s to 60 s to obtain hot-dip galvanized steel sheets (GI). Here, the steel sheets were immersed in a galvanizing bath at 440°C to 500°C to obtain hot-dip galvanizing, and then the coating weight was adjusted by gas wiping or the like. For the hot-dip galvanizing, a galvanizing bath containing 0.10% to 0.22% Al was used. Furthermore, some of the hot-dip galvanized steel sheets were subjected to an alloying process after the above hot-dip galvanizing process to obtain alloyed hot-dip galvanized steel sheets (GA). Here, the alloying process was performed in a temperature range of 460°C to 550°C. In addition, some of the steel sheets (cold-rolled steel sheets: CR) were subjected to electroplating to obtain electrogalvanized steel sheets (EG).
[0078] The steel structure was measured by the following method. The measurement results are shown in Table 3. The area ratios of polygonal ferrite, upper bainite, tempered martensite, lower bainite, and hardened martensite (fresh martensite) were measured by cutting out a cross section of the plate thickness parallel to the rolling direction, mirror polishing it, and then etching it with 1 vol% nital. Ten fields of view were observed at 5,000x magnification using an SEM at the 1 / 4 thickness position, and the photographed microstructural images were quantified using image analysis. Polygonal ferrite is a relatively equiaxed ferrite with almost no carbides inside. It is the area that appears the blackest under SEM. Upper bainite is a ferrite structure with the formation of carbides or retained austenite inside that appear white under SEM. When it was difficult to distinguish between upper bainite and polygonal ferrite, the area of ferrite with an aspect ratio of ≦2.0 was classified as polygonal ferrite, and the area with an aspect ratio of >2.0 was classified as upper bainite, and the area ratio was calculated. Here, the aspect ratio was calculated by determining the major axis length a at which the particle length is the longest, and the minor axis length b at the particle length when it crosses the particle the longest in the direction perpendicular to that, and a / b was defined as the aspect ratio. Tempered martensite and lower bainite are regions with lath-shaped substructure and carbide precipitation inside when viewed under SEM. Hardened martensite (fresh martensite) is a blocky region that appears white under an SEM, with no internal substructure visible. The remaining structure is a carbide and / or pearlite structure, which can be confirmed by white contrast under SEM. Carbide has a particle size of 1 μm or less, and pearlite can be distinguished from carbide because it has a lamellar (layer) structure.
[0079] The quantitative evaluation of the above-mentioned structure, and the measurement of the aspect ratio and circle equivalent diameter of the quenched martensite and the retained austenite were performed using Image J (Fiji) as image analysis software. A cross section of the plate parallel to the rolling direction was cut out, mirror-polished, and then etched with 1 vol% nital, and observed at 1 / 4 thickness position in 10 fields of view at 5000x magnification with an SEM, and each structure was identified and quantitatively evaluated using the Trainable Weka segmentation method, which can identify regions using machine learning in Image J (Fiji). In addition, the aspect ratio and circle equivalent diameter of the quenched martensite and retained austenite can be measured using a particle analysis program, which is also a function of Image J, and only the quenched martensite and retained austenite identified as described above were extracted and measured.
[0080] The volume fraction of retained austenite was determined by X-ray diffraction after chemical polishing of the 1 / 4 thickness position from the surface. A Co-Kα source was used for the incident X-rays, and the volume fraction of retained austenite was calculated from the intensity ratio of the (200), (211), and (220) planes of ferrite to the (200), (220), and (311) planes of austenite.
[0081] The area ratio S of the C-enriched region where the C concentration is 0.5 mass% or more C≧0.5 The measurement was performed at 1 / 4 of the thickness of the plate cross section parallel to the rolling direction using a JEOL field emission electron probe microanalyzer (FE-EPMA) JXA-8500F. The accelerating voltage was 6 kV and the probe current was 7 × 10 -8A, The C concentration distribution was measured by mapping analysis with the beam diameter at its minimum, and the area ratio where the C concentration was 0.5 mass% or more was calculated. However, to eliminate the effects of contamination, the background was subtracted so that the average value of C obtained in the analysis was equal to the carbon amount in the base material. In other words, if the average value of the measured carbon amount was greater than the carbon amount in the base material, the increase was considered to be contamination, and the true carbon amount at each position was determined by subtracting the increase uniformly from the analytical value at each position.
[0082] JIS No. 5 tensile test pieces and hole expansion test pieces were taken from the obtained steel plates, and tensile tests (based on JIS Z2241 (2011)) were performed with N=3. Each evaluation was based on the average value of the three points. Steel plates with a tensile strength of 780 MPa or more were judged to have excellent strength. Steel plates with a yield ratio YR of 0.8 or less were judged to have excellent press formability. Total elongation EL of 16.0% or more for TS: 780 MPa or more, 14.0% or more for TS: 980 MPa or more, and 12.0% or more for TS: 1180 MPa or more were judged to have excellent ductility.
[0083] In addition, for the evaluation of stretch flange formability, a test piece was taken from the center position of the plate width, and a hole expansion test in accordance with the provisions of the Japan Iron and Steel Federation standard JFST1001 was performed with N=3. That is, after punching a sample of 100mm x 100mm square size using a punching tool with a punch diameter of 10mm and clearance: 13%, a conical punch with an apex angle of 60 degrees was used to expand the hole until a crack penetrating the plate thickness occurred, with the burrs generated during the formation of the punched hole being on the outside. In this case, d0: initial hole diameter (mm), d: hole diameter at the time of crack occurrence (mm), the hole expansion ratio λ (%) = {(d-d0) / d0} × 100 was calculated, and the average value of the three points was evaluated as λ. Steels with λ of 30% or more were judged to have excellent hole expandability and stretch flangeability.
[0084] For the evaluation of the material stability in the width direction, 23 points (including the width center) of the evaluation material were taken from both width directions at intervals of 100 mm or less from the width center position (12W / 24 position (W: width)), and EL and λ were obtained at each position (measurement position X).The material stability in the width direction was evaluated by calculating the ratio of the difference between the measurement value at the width center position and each position to the measurement value at the center position. Using EL and λ at the center of the plate width as the standard, the group of consecutive measurements in which the difference in EL and λ was 10% or less was defined as the region in which the difference in EL and λ was 10% or less, and steels in which this region accounted for 80% or more of the total plate width were determined to have excellent material stability. A plate width in region A that satisfies the following formulas (1) and (2) is determined to be 80% or more of the total plate width, and the plate is judged to have excellent material stability in the plate width direction. -10≦100×[(EL(%) at measurement position X in area A - EL(%) at center of strip width) / EL(%) at center of strip width]≦10 (1) -10≦100×[(λ(%) at measurement position X in area A - λ(%) at center of strip width) / λ(%) at center of strip width]≦10 (2) (In formulas (1) and (2), the measurement positions X are 23 positions in total that are 24 divided positions of the width W of the steel plate. That is, the measurement positions X are W / 24, 2W / 24, 3W / 24, 4W / 24, 5W / 24, 6W / 24, 7W / 24, 8W / 24, 9W / 24, 10W / 24, 11W / 24, 12W / 24, 13W / 24, 14W / 24, 15W / 24, 16W / 24, 17W / 24, 18W / 24, 19W / 24, 20W / 24, 21W / 24, 22W / 24, and 23W / 24, totaling 23 positions.)
[0085] The measurement results are shown in Table 3.
[0086] [Table 2]
[0087] [Table 3]
[0088] The examples of the present invention shown in Tables 2 and 3 were excellent in strength, press formability, ductility, stretch flange formability, and material stability in the sheet width direction, whereas the comparative examples were inferior in any of these properties.
[0089] In addition, using the steel plate of the present invention, it was found that the components obtained by molding, the components obtained by joining, and the components obtained by further molding and joining have high strength and excellent press formability, ductility, stretch flange formability, and material stability in the width direction of the plate, similar to the steel plate of the present invention, because the steel plate of the present invention has high strength and is excellent in press formability, ductility, stretch flange formability, and material stability in the width direction of the plate.
Claims
1. In mass percent, C: 0.05-0.20%, Si: 0.40 to 1.50%, Mn: 1.9 to 3.5%, P: 0.02% or less, S: 0.01% or less, sol. Al: 0.331% or less, N: less than 0.015%; The balance being iron and unavoidable impurities; Area ratio of polygonal ferrite: 10% or more and 80% or less, Total area ratio of upper bainite, tempered martensite and lower bainite: 15% or more and 70% or less, Volume fraction of retained austenite: 3% or more and 15% or less, Area ratio of quenched martensite: 15% or less (including 0%), a steel structure having a remaining structure with an area ratio of 5% or less; having The total area ratio of the quenched martensite and the retained austenite having an aspect ratio of 3 or less and an equivalent circle diameter of 2.0 μm or more is 20% or less, The carbon-enriched region (S C≧0.5 ) is 20% or less in area ratio.
2. The steel sheet according to claim 1, wherein the component composition contains one or more selected from the following (A) to (C): (A) in mass %, Ti: 0.1% or less, B: 0.01% or less, One or two selected from the following: (B) in mass %, Cu: 1% or less, Ni: 1% or less, Cr: 1% or less, Mo: 0.5% or less, V: 0.5% or less, Nb: 0.1% or less, One or more selected from the following: (C) in mass %, Mg: 0.0050% or less, Ca: 0.0050% or less, Sn: 0.1% or less, Sb: 0.1% or less, REM: 0.0050% or less, Select one or more of the following:
3. The steel sheet according to claim 1 , which has a zinc plating layer on its surface.
4. The steel sheet according to claim 2 , which has a zinc plating layer on its surface.
5. A member made using the steel plate according to any one of claims 1 to 4.
6. A method for producing a steel sheet, comprising the steps of: subjecting a steel slab having the composition according to claim 1 or 2 to hot rolling, pickling and cold rolling; and then annealing the resulting cold-rolled steel sheet, The annealing is A holding step of heating the cold-rolled steel sheet to an annealing temperature of 750 to 880 ° C. and holding the annealing temperature for 10 to 500 seconds; A first cooling step of cooling the temperature range from the annealing temperature to a first cooling stop temperature of 350 to 550 ° C. at a first average cooling rate of 2 to 50 ° C. / s to the first cooling stop temperature; A second cooling step in which the steel sheet is held at a residence temperature of 350 to 550° C. for 10 s to 60 s and then cooled to a second cooling stop temperature of 150 to 360° C. at a second average cooling rate of 3 to 50° C. / s; and a third cooling step of cooling the steel at a temperature range from the second cooling stop temperature to 50° C. at a third average cooling rate of 0.05 to 1.0° C. / s, wherein the steel has a steel structure consisting of a residual structure in which the area ratio of polygonal ferrite is 10% or more and 80% or less, the total area ratio of upper bainite, tempered martensite, and lower bainite is 15% or more and 70% or less, the volume ratio of retained austenite is 3% or more and 15% or less, the area ratio of quenched martensite is 15% or less (including 0%), and further the area ratio is 5% or less, and the aspect ratio of the steel structure is 3 or less with respect to the total area ratio of the quenched martensite and the retained austenite, and the total area ratio of the quenched martensite and the retained austenite having a circle equivalent diameter of 2.0 μm or more is 20% or less, and the C concentration is 0.5 mass% or more with respect to the entire structure. C≧0.5 ) is 20% or less.
7. The method for producing a steel sheet according to claim 6, wherein in the second cooling step, when the steel sheet is retained at a retention temperature of 350 to 550 ° C. for 10 s to 60 s, a hot-dip galvanizing treatment or an alloyed hot-dip galvanizing treatment is performed on a surface of the steel sheet.
8. The method for producing a steel sheet according to claim 6, further comprising the step of electrolytic galvanizing a surface of the steel sheet after the annealing.
9. A method for manufacturing a component, comprising a step of subjecting the steel plate according to any one of claims 1 to 4 to at least one of forming and joining to form a component.
Citation Information
Patent Citations
Coating method for coarse base material
JP1980015623A
High-strength steel sheet having excellent elongation and excellent stretch flangeability and process for production of the same
JP2008297609A
Thin steel sheet and method for manufacturing the same
JP2020100894A
High-strength steel sheet for automobiles with excellent crash resistance and formability and its manufacturing method
JP3936440B2
High-strength steel sheet and process for production thereof
WO2009096596A1