Zn-Al-Mg-plated checkered steel sheet
The Zn-Al-Mg-based plated striped steel sheet addresses deformation and thickness variations by controlling thermal expansion and using a specific chemical composition and slow heating/cooling, achieving improved flatness, corrosion resistance, and workability.
Patent Information
- Application Number
- JP2023513023
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-06
- Filing Date
- 2022-04-05
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2042-04-05
AI Technical Summary
Striped steel sheets used outdoors require corrosion resistance and anti-slip properties but face issues with deformation and variations in plating layer thickness due to differences in thermal expansion and contraction between convex and flat portions, leading to poor flatness and workability.
A Zn-Al-Mg-based plated striped steel sheet with a specific chemical composition and controlled layer thickness ratios, along with a slow heating and cooling process to minimize thermal expansion differences, ensuring uniform plating and improved flatness, corrosion resistance, and workability.
The solution provides a Zn-Al-Mg-based plated striped steel sheet with enhanced flatness, corrosion resistance, and workability by minimizing deformation and variations in plating thickness, even with Zn-Al-Mg plating baths of lower viscosity.
Smart Images

Figure 0007560786000009 
Figure 0007560786000010 
Figure 0007560786000011
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a Zn-Al-Mg-based plated checkered steel sheet. [Background technology]
[0002] Checkered steel plate is a steel plate with a continuous anti-slip convex portion (i.e., protrusion portion) formed on the surface by rolling. In general, the convex portions have a certain width, length, and height, and are provided at a certain angle and pitch relative to the rolling direction. Checkered steel plate is usually manufactured by hot rolling. Checkered steel plate is used for floor plates or steps of large vehicles (buses, trucks, etc.), floor plates of multi-storey car parks, floor plates of factories, decks of ships, temporary scaffolding or stairs at construction sites, etc.
[0003] For example, Patent Document 1 describes a hot-dip plated checkered steel sheet having a base steel sheet, a Ni plating layer disposed on a surface of the base steel sheet, and a hot-dip plated layer disposed on a surface of the Ni plating layer, the hot-dip plated checkered steel sheet having a convex portion and a flat portion on a sheet surface, the Ni plating layer of the convex portion having a thickness of 0.07 to 0.4 μm per side, the Ni plating layer of the flat portion having a thickness of 0.05 to 0.35 μm per side, the Ni plating layer of the convex portion having a thickness of more than 100% and not more than 400% of the thickness of the Ni plating layer of the flat portion, and the coating weight of the hot-dip plated layer being 60 to 400 g / m per side. 2 The hot-dip plated checkered steel sheet has a chemical composition, in mass%, of Al: more than 1.0% and not more than 26%, Mg: 0.05 to 10%, Si: 0 to 1.0%, Sn: 0 to 3.0%, Ca: 0 to 1.0%, and the balance being Zn and impurities."
[0004] In addition, Patent Document 2 states that "After pickling the strip-shaped checkered steel plate, the annealing temperature is 450 to 850°C, and the tension of the steel strip in the annealing furnace is 0.3 to 2.0 kg / mm 2 , Steel strip tension in plating line: 0.3~3.0kg / mm 2 Gas pressure for molten metal wiping: 0.02-1.5kg / cm 2The present invention discloses a continuous hot-dip metal plating method for strip-shaped checkered steel sheet, which performs hot-dip metal plating continuously under conditions that satisfy the requirements of (a) above. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2019 / 054483 [Patent Document 2] Patent No. 2743774 Summary of the Invention [Problem to be solved by the invention]
[0006] Since checkered steel sheets are often used outdoors, they are required to have corrosion resistance. Therefore, as disclosed in Patent Documents 1 and 2, the checkered steel sheets are subjected to hot-dip galvanization to improve the corrosion resistance.
[0007] On the other hand, checkered steel plate is also required to be flat since it is used for scaffolding, anti-slip purposes, etc. However, checkered steel sheet is a steel sheet with local differences in sheet thickness due to the convex and flat portions. Therefore, when the checkered steel sheet is hot-dip plated to improve corrosion resistance, the checkered steel sheet is deformed due to differences in the amount of expansion and contraction caused by temperature changes between the convex and flat portions of the checkered steel sheet. When the deformed plated checkered steel sheet is made into a product, the flatness is deteriorated. Furthermore, when the flatness is deteriorated, the thickness of the plating layer varies, and the corrosion resistance and workability are deteriorated. In particular, since a Zn-Al-Mg alloy-based plating bath has a lower viscosity than a Zn-based plating bath, if the flatness of the checkered steel sheet is poor, the thickness of the plating layer is likely to vary, and the corrosion resistance and workability are reduced. Therefore, further improvement in the flatness of the Zn-Al-Mg-based plated checkered steel sheet is required.
[0008] Therefore, an object of the present disclosure is to provide a Zn-Al-Mg-plated checkered steel sheet having excellent flatness, corrosion resistance and workability. [Means for solving the problem]
[0009] The above problems are solved by the following means. <1> A Zn-Al-Mg-based plated checkered steel sheet having a base checkered steel sheet on one sheet surface of which a convex portion and a flat portion are provided, and a plating layer including a Zn-Al-Mg alloy layer arranged on the sheet surface of the base checkered steel sheet on which the convex portion and the flat portion are provided, The plating layer comprises, in mass %, Zn: over 65.0%, Al: over 1.0% to less than 25.0% Mg: over 1.0% to less than 12.5% Sn: 0% to 5.0%, Bi: 0% to less than 5.0% In: 0% to less than 2.0% Ca: 0%~3.00%, Y: 0%~0.5%, La: 0% to less than 0.5%, Ce: 0% to less than 0.5%, Si: 0% to less than 2.5% Cr: 0% to less than 0.25%, Ti: 0% to less than 0.25% Zr: 0% to less than 0.25% Mo: 0% to less than 0.25% W: 0% to less than 0.25%, Ag: 0% to less than 0.25% P: 0% to less than 0.25%, Ni: 0% to less than 0.25% Co: 0% to less than 0.25% V: 0% to less than 0.25%, Nb: 0% to less than 0.25%, Cu: 0% to less than 0.25% Mn: 0% to less than 0.25% Li: 0% to less than 0.25%, Na: 0% to less than 0.25% K: 0% to less than 0.25%, Fe: 0%~5.0%, Sr: 0% to less than 0.5%, Sb: 0% to less than 0.5% Pb: 0% to less than 0.5%, B: 0% to less than 0.5%, and It has a chemical composition made up of impurities, when observing a cross section cut at a longitudinal center of the protrusion perpendicular to the longitudinal direction of the protrusion and along the sheet thickness direction, a layer thickness ratio of the plating layer of the flat portion on the left and right of the protrusion (layer thickness of the left plating layer / layer thickness of the right plating layer) is 0.2 or more and 5.0 or less, A Zn-Al-Mg based plated checkered steel sheet in which a stripe height Tt, where T is the thickness of the plain checkered steel sheet at the convex portion and t is the thickness of the plain checkered steel sheet at the flat portion, and a gap height x, when the plated checkered steel sheet is placed stationary, between a resting surface and a sheet surface of the plated checkered steel sheet facing the resting surface, satisfy the following formulas 1 and 2. Formula 1: x / (Tt)≦1.5 Formula 2:0.5 <T-t≦t In formulas 1 and 2, the units of the plate thickness T, t, and gap height x of the plain checkered steel plate are "mm." <2> The Al concentration is more than 5.0% and less than 25.0%, and the Mg concentration is more than 3.0% and less than 12.5%. <1> Zn-Al-Mg-plated checkered steel sheet according to claim 1. <3> The plating layer includes an Al-Fe alloy layer between the base checkered steel sheet and the Zn-Al-Mg alloy layer. <1> or <2> Zn-Al-Mg-plated checkered steel sheet according to claim 1. Effect of the Invention
[0010] According to the present disclosure, it is possible to provide a Zn-Al-Mg-plated checkered steel sheet having excellent flatness, corrosion resistance and workability. [Brief description of the drawings]
[0011] [Figure 1A] 1 is an SEM photograph (magnification: 500) showing an example of a cross section of a Zn-Al-Mg-based plated checkered steel sheet according to the present disclosure. [Figure 1B] 1 is an SEM photograph (2000x) showing an example of a cross section of a Zn-Al-Mg-plated checkered steel sheet according to the present disclosure. [Diagram 2]FIG. 2 is a schematic diagram for explaining a method for measuring a gap height x in a Zn-Al-Mg-plated checkered steel sheet according to the present disclosure. [Figure 3A] FIG. 2 is a schematic plan view showing an example of a base checkered steel sheet of the Zn-Al-Mg-plated checkered steel sheet of the present disclosure. [Figure 3B] FIG. 3B is a cross-sectional schematic diagram showing an example of a base checkered steel sheet of the Zn-Al-Mg-plated checkered steel sheet of the present disclosure, and is a cross-sectional schematic diagram of the GG cross section of FIG. 3A. [Figure 3C] FIG. 3B is a cross-sectional schematic diagram showing an example of a base checkered steel sheet of the Zn-Al-Mg-plated checkered steel sheet of the present disclosure, and is a cross-sectional schematic diagram of F-F in FIG. 3A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] An example of the present disclosure will be described below. In the present disclosure, the "%" designation for the content of each element in a chemical composition means "mass %." A numerical range expressed using "~" means that the range includes the numerical values before and after "~" as the lower and upper limits. When a numerical range is preceded by "to" and followed by "greater than" or "less than," it means that the numerical range does not include the numerical value as the lower limit or upper limit. The content of an element in a chemical composition is sometimes expressed as element concentration (for example, Zn concentration, Mg concentration, etc.).
[0013] The Zn-Al-Mg-based plated checkered steel sheet of the present disclosure (hereinafter also simply referred to as "plated checkered steel sheet") is a plated checkered steel sheet having a base checkered steel sheet having one sheet surface with convex portions and flat portions, and a plating layer including a Zn-Al-Mg alloy layer disposed on the sheet surface of the base checkered steel sheet having the convex portions and flat portions. The plated checkered steel sheet of the present disclosure has a plating layer that has a predetermined chemical composition, and when a cut surface is observed at the longitudinal center of the convex portion, cut perpendicular to the longitudinal direction of the convex portion and along the sheet thickness direction, the layer thickness ratio of the plating layer in the flat portion on the left and right of the convex portion (layer thickness of the left side plating layer / layer thickness of the right side plating layer) is 0.2 to 5.0, and when the sheet thickness of the base checkered steel sheet at the convex portion is T and the sheet thickness of the base checkered steel sheet at the flat portion is t, the stripe height Tt and the gap height x between the resting surface and the sheet surface of the plated checkered steel sheet facing the resting surface when the plated checkered steel sheet is placed stationary satisfy the following formulas 1 and 2. Formula 1: x / (Tt)≦1.5 Formula 2:0.5 <T-t≦t In formulas 1 and 2, the units of the plate thickness T, t, and gap height x of the plain checkered steel plate are "mm."
[0014] The plated checkered steel sheet of the present disclosure has the above-mentioned configuration, and is a Zn-Al-Mg-based plated checkered steel sheet excellent in flatness, corrosion resistance, and workability. The plated checkered steel sheet of the present disclosure was discovered based on the following findings.
[0015] The inventors have investigated ways to further improve the flatness and suppress the variation in the thickness of the plating layer even in a Zn-Al-Mg plating bath, which has a lower viscosity than a Zn plating bath. As a result, they have obtained the following findings.
[0016] The deterioration of the flatness of plated checkered steel sheet is influenced not only by the heating temperature of the bare checkered steel sheet before immersion in the plating bath, but also by the heating and cooling rates. Specifically, when the bare checkered steel sheet is hot-dip plated, the sudden heating and cooling before immersion in the plating bath causes a difference in the amount of expansion and contraction due to the sudden temperature change between the convex and flat parts, which have different sheet thicknesses, and the sheet is deformed. This is because, unlike a normal flat steel sheet, when heating and cooling, a difference occurs in the heating and cooling rate between the convex and flat parts of the bare checkered steel sheet.
[0017] Therefore, if the heating and cooling of the bare checkered steel sheet before immersion in the coating bath is performed at a slow heating rate and cooling rate, differences in the heating and cooling rates are unlikely to occur between the convex and flat parts, which have different sheet thicknesses. This allows the convex and flat parts to be heated and cooled as uniformly as possible, suppressing deformation. As a result, the flatness of the bare checkered steel sheet is further improved, and even with Zn-Al-Mg coating, the variation in the coating layer thickness is reduced, improving corrosion resistance and workability.
[0018] That is, the inventors have found that a Zn-Al-Mg-based plated checkered steel sheet can be obtained that satisfies the layer thickness ratio of the plated layer in the flat portion, the above formula 1, and the above formula 2.
[0019] From the above findings, it has been found that the plated checkered steel sheet of the present disclosure is a Zn-Al-Mg plated checkered steel sheet excellent in flatness, corrosion resistance and formability.
[0020] Hereinafter, the details of the plated checkered steel sheet of the present disclosure will be described.
[0021] (Plain checkered steel plate) The plain checkered steel sheet is the steel sheet to be plated. The plain checkered steel sheet has a convex portion and a flat portion on one sheet surface. The raw checkered steel plate is usually given the shape of the convex parts by hot rolling. The steel type of the raw checkered steel plate is not particularly limited. For example, the raw checkered steel plate may be a steel type corresponding to the general structural rolled steel material specified in JIS G3101:2015. The convex shape of the green checkered steel sheet is imparted, for example, by transferring a concave shape formed on a working roll onto the steel sheet surface during the finishing stage of hot rolling. The plate surface opposite the plate surface on which the protrusions and flat portions are provided in the plate thickness direction has the surface properties of a normal steel plate. Specifically, the plate surface opposite the plate surface on which the protrusions and flat portions are provided in the plate thickness direction is a plate surface imparted by a normal rolling roll (i.e., a roll having normal roughness) facing the working roll on which the protrusions and flat portions are provided, for example, in the finish hot rolling stage.
[0022] The base checkered steel sheet may be a pre-plated checkered steel sheet that has been pre-plated. The pre-plated checkered steel sheet can be obtained, for example, by an electrolytic treatment method or a displacement plating method. In the electrolytic treatment method, the base checkered steel sheet is immersed in a sulfate bath or a chloride bath containing metal ions of various pre-plating components for electrolytic treatment to obtain a pre-plated checkered steel sheet. In the displacement plating method, the base checkered steel sheet is immersed in an aqueous solution containing metal ions of various pre-plating components and the pH of which is adjusted with sulfuric acid to cause displacement precipitation of metals to obtain a pre-plated checkered steel sheet. A representative example of pre-plated checkered steel sheet is pre-Ni plated checkered steel sheet.
[0023] (Plating layer) The plating layer includes a Zn-Al-Mg alloy layer. The plating layer may include an Al-Fe alloy layer in addition to the Zn-Al-Mg alloy layer. The Al-Fe alloy layer is disposed between the base checkered steel sheet and the Zn-Al-Mg alloy layer.
[0024] That is, the plating layer may be a single-layer structure of a Zn-Al-Mg alloy layer, or a laminate structure including a Zn-Al-Mg alloy layer and an Al-Fe alloy layer. In the case of a laminate structure, the Zn-Al-Mg alloy layer is preferably a layer constituting the surface of the plating layer. However, although an oxide film of the plating layer constituent elements is formed on the surface of the plating layer with a thickness of about 50 nm, it is considered to be thin compared to the overall thickness of the plating layer and does not constitute the main part of the plating layer.
[0025] The coating weight of the plating layer is 60 to 500 g / m per side. 2 is preferred. The coating weight of the plating layer is 60g / m 2 If the coating weight is more than 500g / m, corrosion resistance can be more reliably secured. 2 If the thickness is set to the value below, defects in appearance such as sagging patterns of the plating layer can be suppressed.
[0026] Next, the chemical composition of the plating layer will be described. The chemical composition of the plating layer is, in mass%, Zn: over 65.0%, Al: over 1.0% to less than 25.0% Mg: over 1.0% to less than 12.5% Sn: 0% to 5.0%, Bi: 0% to less than 5.0% In: 0% to less than 2.0% Ca: 0%~3.00%, Y: 0%~0.5%, La: 0% to less than 0.5%, Ce: 0% to less than 0.5%, Si: 0% to less than 2.5% Cr: 0% to less than 0.25%, Ti: 0% to less than 0.25% Zr: 0% to less than 0.25% Mo: 0% to less than 0.25% W: 0% to less than 0.25%, Ag: 0% to less than 0.25% P: 0% to less than 0.25%, Ni: 0% to less than 0.25% Co: 0% to less than 0.25% V: 0% to less than 0.25%, Nb: 0% to less than 0.25% Cu: 0% to less than 0.25% Mn: 0% to less than 0.25% Li: 0% to less than 0.25%, Na: 0% to less than 0.25% K: 0% to less than 0.25%, Fe: 0%~5.0%, Sr: 0% to less than 0.5%, Sb: 0% to less than 0.5% Pb: 0% to less than 0.5%, B: 0% to less than 0.5%, and It has a chemical composition consisting of impurities.
[0027] In the chemical composition of the plating layer, Sn, Bi, In, Ca, Y, La, Ce, Si, Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, K, Fe, Sr, Sb, Pb, and B are optional components. In other words, these elements do not have to be included in the plating layer. When these optional components are included, the content of each of the optional elements is preferably within the range described below.
[0028] Here, the chemical composition of the plating layer refers to the average chemical composition of the entire plating layer (if the plating layer has a single-layer structure of Zn-Al-Mg alloy layer, the average chemical composition of the Zn-Al-Mg alloy layer; if the plating layer has a laminated structure of Al-Fe alloy layer and Zn-Al-Mg alloy layer, the average chemical composition of the combined Al-Fe alloy layer and Zn-Al-Mg alloy layer).
[0029] In the hot-dip galvanizing method, the chemical composition of the Zn-Al-Mg alloy layer is usually almost the same as that of the plating bath, because the reaction of forming the plating layer is almost completed in the plating bath. In addition, in the hot-dip galvanizing method, the Al-Fe alloy layer is formed and grows instantly immediately after immersion in the plating bath. The reaction of forming the Al-Fe alloy layer is completed in the plating bath, and the thickness of the layer is often sufficiently smaller than that of the Zn-Al-Mg alloy layer. Therefore, unless special heat treatment such as alloying treatment is performed after plating, the average chemical composition of the entire plating layer is substantially equal to the chemical composition of the Zn-Al-Mg alloy layer, and the components of the Al-Fe alloy layer can be ignored.
[0030] Each element in the plating layer will be described below.
[0031] Zn: over 65.0% Zn is an element necessary for obtaining corrosion resistance. When considering the Zn concentration in terms of atomic composition ratio, it is necessary for Zn to be the main component in terms of atomic composition ratio, since the plating layer is composed of elements with low specific gravity such as Al and Mg. Therefore, the Zn concentration is set to more than 65.0%. The Zn concentration is preferably 70% or more. The upper limit of the Zn concentration is the concentration of the remainder other than elements other than Zn and impurities.
[0032] Al: Over 1.0% to less than 25.0% Al is an essential element for forming Al crystals and ensuring corrosion resistance. Furthermore, Al is also an essential element for improving the adhesion of the plating layer and ensuring workability. Therefore, the lower limit of the Al concentration is set to more than 1.0% (preferably more than 5.0%, and more preferably 10.0% or more). On the other hand, if the Al concentration is too high, the corrosion resistance tends to deteriorate, so the upper limit of the Al concentration is set to less than 25.0% (preferably 23.0% or less).
[0033] Mg: Over 1.0% to less than 12.5% Mg is an essential element for ensuring corrosion resistance, and therefore the lower limit of the Mg concentration is set to more than 1.0% (preferably more than 3.0%, and more preferably more than 5.0%). On the other hand, if the Mg concentration is too high, workability tends to deteriorate, so the upper limit of the Mg concentration is set to less than 12.5% (preferably 10.0% or less).
[0034] Sn: 0-5.0% Sn is an element that contributes to corrosion resistance, and therefore the lower limit of the Sn concentration is preferably more than 0% (preferably 0.1% or more, and more preferably 0.5% or more). On the other hand, if the Sn concentration is too high, the corrosion resistance tends to deteriorate, so the upper limit of the Sn concentration is set to 5.0% or less (preferably 3.0% or less).
[0035] Bi: 0% to less than 5.0% Bi is an element that contributes to corrosion resistance, and therefore the lower limit of the Bi concentration is preferably more than 0% (preferably 0.1% or more, and more preferably 3.0% or more). On the other hand, if the Bi concentration is too high, the corrosion resistance tends to deteriorate, so the upper limit of the Bi concentration is set to less than 5.0% (preferably 4.8% or less).
[0036] In: 0% to less than 2.0% In is an element that contributes to corrosion resistance, and therefore the lower limit of the In concentration is preferably more than 0% (preferably 0.1% or more, and more preferably 1.0% or more). On the other hand, if the In concentration is too high, the corrosion resistance tends to deteriorate, so the upper limit of the In concentration is set to less than 2.0% (preferably 1.8% or less).
[0037] Ca: 0% to 3.0% Ca is an element that can adjust the amount of Mg elution that is optimal for imparting corrosion resistance, and therefore the lower limit of the Ca concentration is preferably more than 0% (preferably 0.05% or more). On the other hand, if the Ca concentration is too high, the corrosion resistance and workability tend to deteriorate, so the upper limit of the Ca concentration is set to 3.0% or less (preferably 1.0% or less).
[0038] Y: 0%~0.5% Y is an element that contributes to corrosion resistance, and therefore the lower limit of the Y concentration is preferably more than 0% (preferably 0.1% or more). On the other hand, if the Y concentration is too high, the corrosion resistance tends to deteriorate, so the upper limit of the Y concentration is set to 0.5% or less (preferably 0.3% or less).
[0039] La and Ce: 0% to less than 0.5% La and Ce are elements that contribute to corrosion resistance, and therefore the lower limit of each of the La concentration and the Ce concentration is preferably more than 0% (preferably 0.1% or more). On the other hand, if the La concentration and Ce concentration are too high, the corrosion resistance tends to deteriorate, so the upper limit of each of the La concentration and Ce concentration is set to less than 0.5% (preferably 0.4% or less).
[0040] Si: 0% to less than 2.5% Si is an element that suppresses the growth of the Al-Fe alloy layer and contributes to improving corrosion resistance. Therefore, the Si concentration is preferably more than 0% (preferably 0.05% or more, more preferably 0.1% or more). In particular, when Sn is not included (i.e., when the Sn concentration is 0%), the Si concentration is preferably 0.1% or more (preferably 0.2% or more) from the viewpoint of ensuring corrosion resistance. On the other hand, if the Si concentration is too high, the corrosion resistance and workability tend to deteriorate. Therefore, the upper limit of the Si concentration is set to less than 2.5%. In particular, from the viewpoint of corrosion resistance, the Si concentration is preferably 2.4% or less, more preferably 1.8% or less, and further preferably 1.2% or less.
[0041] Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K: 0% to less than 0.25% Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K are elements that contribute to corrosion resistance. Therefore, the lower limit of the concentration of each of Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K is preferably more than 0% (preferably 0.05% or more, more preferably 0.1% or more). On the other hand, if the concentrations of Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K are too high, the corrosion resistance tends to deteriorate. Therefore, the upper limits of the concentrations of Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K are each set to less than 0.25%. The upper limits of the concentrations of Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K are preferably set to 0.22% or less.
[0042] Fe: 0% to 5.0% When the plating layer is formed by hot dip plating, the Zn-Al-Mg alloy layer and the Al-Fe alloy layer contain a certain concentration of Fe. It has been confirmed that Fe does not adversely affect performance even if it is contained in the plating layer (especially the Zn-Al-Mg alloy layer) with a concentration of up to 5.0%. Since most Fe is contained in the Al-Fe alloy layer, the thicker this layer is, the higher the Fe concentration will generally be.
[0043] Sr, Sb, Pb and B: 0% to less than 0.5% Sr, Sb, Pb and B are elements that contribute to corrosion resistance. Therefore, the lower limit of each of the concentrations of Sr, Sb, Pb and B is preferably more than 0% (preferably 0.05% or more, more preferably 0.1% or more). On the other hand, corrosion resistance tends to deteriorate if the concentrations of Sr, Sb, Pb, and B are too high. Therefore, the upper limits of the concentrations of Sr, Sb, Pb, and B are each set to less than 0.5%.
[0044] impurities Impurities are components contained in raw materials or components mixed in during the manufacturing process, but not intentionally added. For example, trace amounts of components other than Fe may be mixed into the plating layer as impurities due to atomic diffusion between the base checkered steel sheet and the plating bath.
[0045] The chemical composition of the plating layer is measured by the following method. First, the plating layer is peeled off and dissolved with an acid containing an inhibitor that suppresses the corrosion of the base checkered steel sheet to obtain an acid solution. Next, the obtained acid solution is measured by ICP analysis to obtain the chemical composition of the plating layer (when the plating layer has a single-layer structure of Zn-Al-Mg alloy layer, the chemical composition of the Zn-Al-Mg alloy layer; when the plating layer has a laminated structure of Al-Fe alloy layer and Zn-Al-Mg alloy layer, the total chemical composition of the Al-Fe alloy layer and the Zn-Al-Mg alloy layer). There are no particular restrictions on the type of acid as long as it can dissolve the plating layer. The chemical composition is measured as an average chemical composition. In ICP analysis, the Zn concentration is calculated using the formula (a): Zn concentration = 100% - other element concentration (%).
[0046] Here, when a pre-plated checkered steel sheet is used as the base checkered steel sheet, the components of the pre-plating are also detected. For example, when a pre-Ni plated checkered steel sheet is used, ICP analysis detects not only Ni in the plated layer but also Ni in the pre-Ni plating. 2 ~3g / m 2 When a pre-plated checkered steel sheet (thickness: about 0.1-0.3 μm) is used as a base checkered steel sheet, even if the Ni concentration in the plating layer is 0%, the Ni concentration is detected as 0.1-15%. Therefore, the Ni concentration in the plating layer may be unknown in the ICP analysis results. Therefore, the Ni concentration in the plating layer when a pre-Ni plated checkered steel sheet is used as a base steel sheet is measured by glow discharge optical emission spectrometry (quantitative GDS). Specifically, a calibration curve is created for the relationship between Ni concentration and Ni emission intensity using three or more types of standard samples with different Ni concentrations using a high-frequency glow discharge optical emission surface analyzer (manufactured by Horiba, Ltd., model number: GD-Profiler2). The standard samples used are Zn alloy standard samples IMN ZH1, ZH2, and ZH4 manufactured by BAS. The measurement conditions for GDS are as follows. HV: Fe is 785V, Ni is 630V, Co is 720V Anode diameter: φ4mm Gas: Ar Gas pressure: 600Pa Output: 35W Next, the Ni emission intensity at the 1 / 2 position of the film thickness of the plating layer of the plated steel material to be measured is obtained using GDS under the above conditions. The Ni concentration at the 1 / 2 position of the plating layer is obtained from the obtained Ni emission intensity and the created calibration curve. The 1 / 2 position of the plating layer is the position at the time when the Fe intensity is saturated, i.e., 1 / 2 the time when it reaches the base steel, in the GDS analysis under the above conditions. The obtained Ni concentration at the 1 / 2 position of the plating layer is the Ni concentration in the plating layer. In this case, the "other element concentration (%)" in the above-mentioned formula (1) for calculating the Zn concentration is the sum of the concentration (%) of elements other than Ni in the ICP analysis and the Ni concentration (%) in the GDS analysis. In other words, when a pre-Ni plated steel material is used as the base steel material, the Zn concentration of the plating layer is calculated by "Formula (a'): Zn concentration = 100 - (concentration (%) of elements other than Ni in the ICP analysis + Ni concentration (%) in the GDS analysis)". When pre-Ni plated checkered steel sheet is used as the base checkered steel sheet, a small amount of Ni in the pre-Ni plated layer dissolves in the plating bath when the base checkered steel sheet is immersed in the plating bath. Therefore, the Ni concentration in the plating bath is 0.02 to 0.03% higher than the Ni concentration in the prepared plating bath. Therefore, when pre-Ni plated checkered steel sheet is used, the Ni concentration in the plating layer is up to 0.03% higher. Here, the method for determining whether the base checkered steel sheet is a pre-plated checkered steel sheet or not is as follows. A sample is taken from the target checkered steel plate, with the cross section cut along the plate thickness direction of the checkered steel plate serving as the measurement surface. The measurement surface of the sample is subjected to line analysis near the interface between the plating layer of the checkered steel sheet and the base checkered steel sheet using an electron probe microanalyser (FE-EPMA) to measure the Ni concentration. The measurement conditions are an acceleration voltage of 15 kV, a beam diameter of approximately 100 nm, an irradiation time per point of 1000 ms, and a measurement pitch of 60 nm. The measurement distance may be any distance that allows confirmation of whether or not the Ni concentration is enriched at the interface between the plating layer of the checkered steel sheet and the base checkered steel sheet. If the Ni concentration is enriched at the interface between the plating layer and the base checkered steel sheet in the checkered steel sheet, the base checkered steel sheet is determined to be a pre-plated checkered steel sheet.
[0047] Next, the Al-Fe alloy layer will be described. The Al-Fe alloy layer may be formed on the surface of the checkered steel plate (specifically, between the checkered steel plate and the Zn-Al-Mg alloy layer), and the structure of the Al-Fe alloy layer may be 5 The Fe phase is the main phase of the layer. The Al-Fe alloy layer is formed by mutual atomic diffusion between the base checkered steel sheet and the coating bath. In the checkered steel sheet of the present disclosure, the coating layer is formed by a hot-dip coating method, so that the Al-Fe alloy layer is easily formed in the coating layer containing the Al element. Since the coating bath contains a certain concentration or more of Al, 5 The Fe phase is formed most frequently. However, atomic diffusion takes time, and there are also areas where the Fe concentration is high near the base checkered steel sheet. Therefore, the Al-Fe alloy layer is partially composed of AlFe phase, Al 3 Fe phase, Al phase 5 Fe 2 In some cases, the Al-Fe alloy layer may contain small amounts of Zn, because the plating bath contains a certain concentration of Zn.
[0048] Al 5 Fe phase, Al phase 3 Fe phase, AlFe phase, and Al 5 Fe 2 The corrosion resistance of each phase is not significantly different. The corrosion resistance here refers to the corrosion resistance in the parts that are not affected by welding.
[0049] Here, when the plating layer contains Si, Si is particularly likely to be incorporated into the Al-Fe alloy layer, and may become an Al-Fe-Si intermetallic compound phase. The intermetallic compound phase identified is the AlFeSi phase, and isomers include α, β, q1, q2-AlFeSi phases. Therefore, these AlFeSi phases may be detected in the Al-Fe alloy layer. An Al-Fe alloy layer containing these AlFeSi phases is also called an Al-Fe-Si alloy layer. In addition, since the Al-Fe-Si alloy layer is thinner than the Zn-Al-Mg alloy layer, the effect of the Al-Fe-Si alloy layer on the corrosion resistance of the entire plating layer is small.
[0050] In addition, when various pre-plated checkered steel sheets are used as the base checkered steel sheet, the structure of the Al-Fe alloy layer may change depending on the amount of pre-plating applied. Specifically, if the pure metal layer used in the pre-plating remains around the Al-Fe alloy layer, an intermetallic compound phase (e.g., Al 3 In some cases, an alloy layer is formed in which an Al phase (Ni phase, etc.) is substituted with Al atoms and some of the Fe atoms, an Al-Fe alloy layer is formed in which some of the Al atoms, Fe atoms, and Si atoms are substituted, or an Al-Fe-Si alloy layer is formed in which some of the Al atoms, Fe atoms, and Si atoms are substituted.
[0051] In other words, the Al-Fe alloy layer is 5 In addition to the alloy layer mainly composed of an Fe phase, the layer includes the alloy layers of the various modes described above.
[0052] Among various types of pre-plated checkered steel sheets, when a plating layer is formed on a pre-Ni plated checkered steel sheet, an Al-Ni-Fe alloy layer is formed as the Al-Fe alloy layer.
[0053] The thickness of the Al—Fe alloy layer is, for example, not less than 0 μm and not more than 7 μm. The thickness of the Al-Fe alloy layer is preferably 0.05 μm or more and 5 μm or less from the viewpoints of improving the adhesion of the plating layer (specifically, the Zn-Al-Mg alloy layer) and ensuring corrosion resistance and workability.
[0054] Normally, the Zn-Al-Mg alloy layer is thicker than the Al-Fe alloy layer, so the contribution of the Al-Fe alloy layer to the corrosion resistance of the plated checkered steel sheet is smaller than that of the Zn-Al-Mg alloy layer. However, as inferred from the results of the composition analysis, the Al-Fe alloy layer contains a certain concentration of Al and Zn, which are corrosion-resistant elements. Therefore, the Al-Fe alloy layer has a certain degree of corrosion resistance against the base checkered steel sheet.
[0055] Furthermore, when a plating layer having the chemical composition specified in the present disclosure is formed by hot-dip plating, an Al-Fe alloy layer having a thickness of 100 nm or more is often formed between the base checkered steel sheet and the Zn-Al-Mg alloy layer.
[0056] From the viewpoint of corrosion resistance, the thicker the Al-Fe alloy layer, the better. Therefore, the thickness of the Al-Fe alloy layer is preferably 0.05 μm or more. However, a thick Al-Fe alloy layer causes a significant deterioration in plating workability, so a certain thickness or less is preferable. From the viewpoint of workability, the thickness of the Al-Fe alloy layer is preferably 7 μm or less. When the thickness of the Al-Fe alloy layer is 7 μm or less, the amount of cracks and powdering that occur starting from the Al-Fe alloy layer is reduced, improving workability. The thickness of the Al-Fe alloy layer is more preferably 5 μm or less, and even more preferably 2 μm or less.
[0057] The thickness of the Al-Fe alloy layer is measured as follows. After embedding the sample in resin, polish it and measure the thickness at any five points of the identified Al-Fe alloy layer in the backscattered electron image (magnification 10,000 times, field of view size: vertical 50 μm × horizontal 200 μm, field of view in which the Al-Fe alloy layer is visible) of the cross section of the plating layer (cut surface along the plate thickness direction of the plating layer). The arithmetic average of the five points is regarded as the thickness of the Al-Fe alloy layer.
[0058] (Characteristics of galvanized checkered steel sheet) -Thickness ratio of plating layer on flat area- In the plated checkered steel sheet of the present disclosure, when the plated layer is locally thin or thick in a flat portion, the corrosion resistance is deteriorated and the workability is also deteriorated. Therefore, the layer thickness ratio of the plating layer in the flat portion on the left and right of the convex portion (layer thickness of the left plating layer / layer thickness of the right plating layer) is set to 0.2 or more and 5.0 or less. The thickness ratio of the plating layer in the flat portion (thickness of the plating layer on the left side / thickness of the plating layer on the right side) is preferably 0.25 or more and 4.00 or less, more preferably 0.33 or more and 3.00 or less, from the viewpoint of improving corrosion resistance and workability.
[0059] From the viewpoints of corrosion resistance and workability, the thickness of the plating layer in the flat portion is preferably 1.0 to 300.0 μm, and more preferably 2.0 to 200.0 μm.
[0060] The layer thickness ratio of the plating layer in the flat portion is measured as follows. First, a sample is taken from the center of the sheet surface of the plated checkered steel sheet to be measured, at the longitudinal center of the protrusion, perpendicular to the longitudinal direction of the protrusion and along the sheet thickness direction, so that the observation surface is a cut surface (specifically, a cut surface corresponding to the FF cross section in Figure 3A). Next, the sample is embedded in resin, and the observation surface of the sample is observed at a magnification of 500x or 2000x using a scanning electron microscope (SEM) (see Figs. 1A and 1B). Next, the thicknesses of the plating layers on the left and right flat portions are measured, and the ratio of the thickness of the plating layer on the left side to the thickness of the plating layer on the right side is calculated. Here, the thickness of the plating layer of the left and right flat portions (see FT in Fig. 1B) is measured at a point 3 mm away (see FP in Fig. 1) from the boundary between the convex portion and the flat portion (specifically, the end of the flat portion where a pair of plate surfaces facing each other in the plate thickness direction are parallel (see EG in Fig. 1A)). In FIG. 1, B indicates the base checkered steel sheet, C indicates the plating layer, Q indicates the convex portion, and P indicates the flat portion.
[0061] This operation is then performed on three samples taken at locations at least 100 mm apart from each other, and the calculated average value of the obtained "ratio of left side plating layer thickness / right side plating layer thickness" is regarded as the "plating layer thickness ratio of flat portion."
[0062] -Formula 1 and Formula 2- In the plated checkered steel sheet of the present disclosure, if the stripe height Tt, which is the difference between the thickness T of the base checkered steel sheet at the convex parts and the thickness t of the base checkered steel sheet at the flat parts, is too large, the difference in the amount of thermal expansion between the convex parts and the flat parts becomes too large. As a result, the plated checkered steel sheet is deformed by heating and cooling before immersion in the plating bath, and the flatness deteriorates. Therefore, the stripe height Tt is set to be equal to or less than the thickness of the base checkered steel sheet at the flat parts. On the other hand, the lower limit of the stripe height Tt is set to more than 0.5 mm in order to ensure the functionality (eg, slip resistance) of the plated checkered steel sheet.
[0063] In the plated checkered steel sheet of the present disclosure, if the gap height x between the plated checkered steel sheet and the surface on which it is placed is too large, the flatness deteriorates. Therefore, the gap height x is set to be equal to or less than the stripe height Tt × 1.5.
[0064] Furthermore, if the flatness of the plated checkered steel sheet of the present disclosure deteriorates, the layer thickness ratio of the plated layer in the flat portion on the left and right of the convex portion increases, and the corrosion resistance and workability also deteriorate.
[0065] Therefore, when the thickness of the plain checkered steel plate at the convex portions is T and the thickness of the plain checkered steel plate at the flat portions is t, the stripe height Tt and, when the plated checkered steel plate is placed stationary, the gap height x between the resting surface and the plate surface of the plated checkered steel plate facing the resting surface should satisfy the following formulas 1 and 2. Formula 1: x / (Tt)≦1.5 Formula 2:0.5 <T-t≦t In formulas 1 and 2, the units of the plate thickness T, t, and gap height x of the plain checkered steel plate are "mm."
[0066] In the formula 1, from the viewpoints of improving flatness, corrosion resistance, and workability, the value of "x / (Tt)" is preferably 1.2 or less, and more preferably 1.0 or less. From the same viewpoints, the value of "x / (Tt)" is preferably close to 0. In formula 2, from the viewpoints of improving flatness, corrosion resistance, and workability, the "Tt" value is preferably 0.8t or less, and more preferably 0.7t or less. The lower limit of the stripe height Tt is set in consideration of improving the functions (e.g., slip resistance) of the plated checkered steel sheet.
[0067] Here, the plate thickness t of the base checkered steel plate at the flat portion is preferably 1.6 to 6.0 mm. From the viewpoints of flatness, corrosion resistance and processability, the gap height x is preferably 3.0 mm or less, and more preferably 2.0 mm or less. In addition, when the functionality (for example, slip resistance) of the plated checkered steel sheet is taken into consideration, the area occupancy rate of the convex portions (that is, the checkered portions) is preferably 15 to 60%.
[0068] The thickness T of the plain checkered steel plate at the convex portion, the thickness t of the plain checkered steel plate at the flat portion, the stripe height Tt, and the gap height x are measured as follows.
[0069] First, a 300 mm square sample is taken from the center of the surface of the plated checkered steel sheet to be measured. Next, the collected sample is placed on a horizontal surface (resting surface). However, the sheet surface of the sample facing the resting surface corresponds to the sheet surface of the plated checkered steel sheet that does not have any convex portions or flat portions. The placed sample is observed from a direction horizontal to the surface on which it is placed, and the gap height between the surface and the surface of the sample facing the surface is measured (see Figure 2). This operation is carried out in the directions of the four sides of the sample, and the maximum gap height is defined as the gap height x. In FIG. 2, CS denotes the plated checkered steel sheet sample, and Su denotes the stationary surface.
[0070] On the other hand, a sample measuring 300 mm square is taken from the center of the longitudinal direction of the convex portion, with the cross section perpendicular to the longitudinal direction of the convex portion and cut along the plate thickness direction (specifically, the cross section corresponding to the FF cross section in Figure 3A) as the observation surface. Next, the sample is embedded in resin, and the observation surface of the sample is observed under an optical microscope at a magnification of 25 times (see Figure 1). Next, the thickness of the bare checkered steel plate at the widthwise center of the convex portions and the thickness of the bare checkered steel plate at the widthwise center of the flat portions are each measured.
[0071] This operation was then performed on three samples, and the maximum values obtained for "the thickness of the plain checkered steel plate at the widthwise center of the convex portions" and "the thickness of the plain checkered steel plate at the widthwise center of the flat portions" were designated as the thickness T of the plain checkered steel plate at the convex portions and the thickness t of the plain checkered steel plate at the flat portions, respectively, and the difference between them was designated as the stripe height Tt.
[0072] (Method of manufacturing plated checkered steel sheet) Hereinafter, an example of a method for producing a plated checkered steel sheet according to the present disclosure will be described.
[0073] The method for producing plated checkered steel sheet of the present disclosure, for example, involves heating a bare checkered steel sheet to a temperature 20°C higher than the coating bath temperature and 850°C or lower at a heating rate of 5 to 20°C / s and holding the sheet thereat, then cooling the bare checkered steel sheet to a temperature higher than the coating bath and 10°C higher than the coating bath temperature at a cooling rate of 5 to 20°C / s, immersing the cooled bare checkered steel sheet in a coating bath, removing the sheet from the coating bath, and then, if the coating bath temperature is higher than 500°C, cooling the sheet to 500°C at a cooling rate of 5 to 20°C / s to produce a plated checkered steel sheet. Here, the plating is carried out by a continuous hot-dip metal plating method such as the Sendzimir method.
[0074] A specific example of the manufacturing method is as follows. First, a plain checkered steel sheet whose stripe height Tt satisfies Equation 1 is prepared. Next, the raw checkered steel sheet is pickled, and then heated and held at the heating temperature. Here, after pickling and before heating, the base checkered steel sheet may be subjected to pre-plating (for example, pre-Ni plating).
[0075] The heating temperature is between 20°C above the plating bath temperature and 850°C below. By keeping the heating temperature below 850°C, deformation of the base checkered steel sheet is suppressed and flatness is improved. The heating rate is 5 to 20°C / s. By slowly heating at a heating rate of 20°C / s or less, the temperature of the convex and flat parts of the base checkered steel sheet is raised uniformly, suppressing deformation due to the difference in thermal expansion between the convex and flat parts. As a result, further deterioration of the flatness is suppressed. On the other hand, if the heating rate is too slow, it becomes difficult for the convex and flat parts of the base checkered steel sheet to rise in temperature uniformly, and deformation due to the difference in thermal expansion between the convex and flat parts becomes likely to occur. Therefore, the heating rate is set to 5°C / s. When pre-plating is not performed, the heating and holding time is set to 10 to 120 seconds. By setting the heating and holding time to 10 to 120 seconds, the oxide film on the surface can be reduced, improving plating properties.
[0076] The base checkered steel sheet is heated by, for example, electrical heating, non-oxidizing direct flame heating, or radiant heating.
[0077] Next, the bare checkered steel sheet is cooled to a temperature in the range of not less than the temperature of the plating bath but not more than 10° C. above the temperature of the plating bath. The cooling rate is 5 to 20°C / s. By slowly cooling at a cooling rate of 20°C / s or less, the convex and flat parts of the base checkered steel sheet are cooled uniformly, suppressing deformation due to the difference in thermal contraction between the convex and flat parts. As a result, further deterioration of flatness is suppressed. On the other hand, if the cooling rate is too slow, it becomes difficult to uniformly cool the convex and flat parts of the checkered steel plate, and deformation due to the difference in thermal contraction between the convex and flat parts becomes likely to occur. Therefore, the cooling rate is set to 5°C / s.
[0078] The green checkered steel plate is cooled, for example, by nitrogen gas cooling.
[0079] As described above, by performing heating and cooling on the bare checkered steel sheet before plating, deterioration of flatness is suppressed, and a plated checkered steel sheet in which the gap height x satisfies Equation 2 is obtained.
[0080] Next, the cooled bare checkered steel sheet is immersed in a plating bath having a chemical composition equivalent to that of the plating layer in the plated checkered steel sheet of the present disclosure.
[0081] Next, the base checkered steel sheet is pulled out of the plating bath, the plating coverage is adjusted by wiping, and then it is cooled. When the temperature of the plating bath is 500°C or less, there are no particular restrictions on the cooling conditions after plating. On the other hand, when the temperature of the plating bath is more than 500°C, the cooling rate to 500°C after plating is set to 5 to 20°C / s. By slowly cooling at a cooling rate of 20°C / s or less, the convex and flat portions of the base checkered steel sheet are cooled uniformly, suppressing deformation due to the difference in thermal expansion between the convex and flat portions. As a result, further deterioration of flatness is suppressed. On the other hand, if the cooling rate is too slow, it becomes difficult to uniformly cool the convex and flat parts of the checkered steel plate, and deformation due to the difference in thermal expansion between the convex and flat parts becomes likely to occur. Therefore, the cooling rate is set to 5°C / s. There are no particular limitations on the cooling conditions below 500°C. The cooling after plating is carried out, for example, by air cooling or nitrogen gas cooling.
[0082] Here, if the flatness of the base checkered steel sheet is poor, the distance between the wiping nozzle and the base checkered steel sheet will vary depending on the location during wiping after plating, resulting in locally thin and thick areas of the plating layer and variation in the thickness of the plating layer between flat areas. Furthermore, when gas cooling is used, the distance between the cooling nozzle and the base checkered steel sheet varies depending on the location, resulting in locally thin and thick areas of the plating layer, and in variations in the thickness of the plating layer between flat portions. In particular, since a Zn-Al-Mg-based plating bath has a lower viscosity than a Zn-based plating bath, the thickness of the plating layer is likely to vary.
[0083] However, as described above, further deterioration of the flatness of the base checkered steel sheet is suppressed during heating and cooling before immersion in the coating bath, so even if the Zn-Al-Mg-based coating is applied, variation in the thickness of the coating layer is unlikely to occur between the flat portions, and a Zn-Al-Mg-based coated checkered steel sheet can be obtained in which the thickness ratio of the coating layer in the flat portions on the left and right of the convex portion (thickness of the left-side coating layer / thickness of the right-side coating layer) satisfies the above-mentioned range.
[0084] Hereinafter, post-treatments that can be applied to the plated checkered steel sheet of the present disclosure will be described.
[0085] In the plated checkered steel sheet of the present disclosure, a coating may be formed on the plating layer. The coating may be formed in one layer or in two or more layers. Examples of the type of coating directly on the plating layer include a chromate coating, a phosphate coating, and a chromate-free coating. The chromate treatment, phosphate treatment, and chromate-free treatment for forming these coatings can be performed by known methods.
[0086] Chromate treatment includes electrolytic chromate treatment, which forms a chromate film by electrolysis, reactive chromate treatment, which forms a film by utilizing a reaction with the material and then washes away excess treatment liquid, and coating chromate treatment, which applies a treatment liquid to the substrate and then dries it without rinsing with water to form a film. Any of these treatments may be used.
[0087] Examples of electrolytic chromate treatments include electrolytic chromate treatments using chromic acid, silica sol, resin (acrylic resin, vinyl ester resin, vinyl acetate acrylic emulsion, carboxylated styrene butadiene latex, diisopropanolamine modified epoxy resin, etc.), and hard silica.
[0088] Examples of the phosphate treatment include zinc phosphate treatment, zinc calcium phosphate treatment, and manganese phosphate treatment.
[0089] Chromate-free treatments are particularly suitable because they do not place a burden on the environment. Chromate-free treatments include electrolytic chromate-free treatments that form a chromate-free film by electrolysis, reactive chromate-free treatments that form a film by utilizing a reaction with the material and then wash away excess treatment liquid, and coating-type chromate-free treatments that apply a treatment liquid to the substrate and dry it without rinsing with water to form a film. Any of these treatments may be used.
[0090] Furthermore, one or more organic resin films may be provided on the film directly on the plating layer. The organic resin is not limited to a specific type, and examples thereof include polyester resin, polyurethane resin, epoxy resin, acrylic resin, polyolefin resin, and modified products of these resins. The modified product here refers to a resin obtained by reacting a reactive functional group contained in the structure of these resins with another compound (monomer, crosslinking agent, etc.) containing a functional group capable of reacting with the functional group in the structure.
[0091] As such an organic resin, one or more organic resins (unmodified) may be mixed and used, or one or more organic resins obtained by modifying at least one other organic resin in the presence of at least one organic resin may be mixed and used. In addition, any coloring pigment or rust-preventive pigment may be contained in the organic resin film. Aqueous resins that have been dissolved or dispersed in water may also be used. EXAMPLES
[0092] An example of the present disclosure will be described, but the conditions in the example are one example of conditions adopted to confirm the feasibility and effects of the present disclosure, and the present disclosure is not limited to this one example of conditions. The present disclosure may adopt various conditions as long as they do not deviate from the gist of the present disclosure and the object of the present disclosure is achieved.
[0093] (Example) A predetermined amount of pure metal ingot was used and melted to prepare a plating bath in the atmosphere so as to obtain a plating layer having the chemical composition shown in Tables 1 and 2. A batch-type hot-dip plating apparatus was used to prepare the plated checkered steel sheet.
[0094] Then, plated checkered steel sheets were produced under the conditions shown in Tables 1 and 2. Specifically, the conditions are as follows. The base checkered steel plate is 2 -H 2 (5%) (dew point -40°C or less, oxygen concentration less than 25 ppm) environment, the temperature was raised from room temperature by electrical heating, and the temperature was maintained for 60 seconds. 2 The plate was cooled to a temperature of 10°C above the plating bath temperature by gas blowing, and immediately immersed in the plating bath. 2 The gas wiping pressure was adjusted to achieve a plating coating weight of 250 g / m2 on the plate surface with the convex and flat parts. 2 A plated checkered steel sheet was produced so that the thickness was approximately equal to that of the plated checkered steel sheet.
[0095] As the base checkered steel sheets, various hot-rolled checkered steel sheets having different sheet thicknesses T of the convex portions and sheet thicknesses t of the flat portions were used. The shape of the raw checkered steel plate used was the same as that shown in Figures 3A to 3C. In the figures, A, B, C, D, E, and H respectively represent the following: A: The angle of the projections relative to the rolling direction. B: The length of one protrusion. C: The maximum width of one convex part. D: The minimum width of one convex part. E: The arrangement pitch of the protrusions. H: Height of the convex part (i.e., fringe height). This checkered steel plate was a hot-rolled Al-killed steel, with an angle A of 45°, a length B of 25.3 mm, a maximum width C of 5.1 mm, a minimum width D of 2.5 mm, and a pitch E of 28.6 mm. The area occupancy rate of the protruding portion was 40%. However, the height H of the protrusions (that is, the stripe height Tt) was as shown in Table 1.
[0096] In some examples, the base checkered steel sheet was a pre-Ni plated checkered steel sheet obtained by pre-plating the above-mentioned hot-rolled checkered steel sheet. The Ni coating weight was 1 g / m 2 ~3g / m 2 In addition, examples in which pre-Ni plated checkered steel sheet was used as the base checkered steel sheet are indicated as "Pre-Ni" in the "Base checkered steel sheet" column in the table.
[0097] -Various measurements- The obtained plated checkered steel sheet was measured for the following items according to the methods described above. - Ratio of plating layer thickness on the flat part on the left and right of the convex part (Left side plating layer thickness / Right side plating layer thickness) - Thickness T of the base checkered steel plate at the convex part (in the table, this is indicated as "Convex part thickness T") - Thickness t of the plain checkered steel plate at the flat part (in the table, this is indicated as "flat part thickness T") Gap height x
[0098] -Flatness- To compare the flatness, the sample was placed on a flat table and pressed down on to evaluate the degree of wobble. If there was no wobble, it was rated "A+", if there was some wobble, it was rated "A", and if there was a lot of wobble, it was rated "NG".
[0099] -Corrosion resistance- To compare corrosion resistance, manufactured samples were subjected to 30 cycles of accelerated corrosion testing (JASO M609-91) and the average area ratio of red rust was evaluated. An area ratio of red rust of 3.0% or less was rated "A+", 5.0% or less was rated "A", 7.0% or less was rated "B", and over 7.0% was rated "NG".
[0100] -Workability- To evaluate the workability of the plating layer, the plated checkered steel sheet was bent 90° in a V shape with the surface with the convex and flat parts facing the crest, and a 24 mm wide cellophane tape was pressed against the crest of the V-bend and then pulled away. If the area ratio of the plating layer that was separated from the plated checkered steel sheet and adhered to the cellophane tape relative to the area of the pressed cellophane tape was 3.0% or less, it was evaluated as "A+", 5.0% or less as "A", 10.0% or less as "B", and more than 10.0% as "NG".
[0101] The examples are listed in Tables 1 and 2.
[0102] [Table 1-1]
[0103] [Table 1-2]
[0104] [Table 1-3]
[0105] [Table 1-4]
[0106] [Table 2-1]
[0107] [Table 2-2]
[0108] [Table 2-3]
[0109] [Table 2-4]
[0110] From the above results, it can be seen that the Examples corresponding to the plated checkered steel sheets of the present disclosure are superior in flatness, corrosion resistance, and workability to the Comparative Examples.
[0111] Moreover, Test No. 97 (Comparative Example) is an example in which the heating temperature before plating was high, at 850° C. or higher. Test No. 98 (comparative example) is an example in which the heating rate before plating was high at 30° C. / s. Test No. 99 (comparative example) is an example in which the cooling rate after heating before plating was high at 30° C. / s. Test No. 100 (comparative example) is an example in which the heating rate before plating and the cooling rate after heating before plating were high, at 30° C. / s. Test No. 101 (comparative example) is an example in which the cooling rate after plating was high at 30° C. / s. Test No. 102 (comparative example) is an example in which Tt is large, equal to or greater than the plate thickness t. Test Examples No. 103 (Comparative Example) to No. 105 (Comparative Example) are examples in which the heating rate before plating, the cooling rate after heating before plating, and the cooling rate after plating were slow. All of these Test Nos. 97 to 103 satisfied the composition of the plating layer of the present disclosure, but the layer thickness ratio and "x / (Tt)" value of the plating layer in the flat portion were large, and the flatness, corrosion resistance, and workability were deteriorated.
[0112] Although the preferred embodiments and examples of the present disclosure have been described in detail above with reference to the accompanying drawings, the present disclosure is not limited to such examples. It is clear that a person having ordinary knowledge in the technical field to which the present disclosure belongs can conceive of various modified or amended examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present disclosure.
[0113] The disclosure of Japanese Patent Application No. 2021-064721 is incorporated herein by reference in its entirety. All publications, patent applications, and standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A Zn-Al-Mg-based plated checkered steel sheet having a base checkered steel sheet having a convex portion and a flat portion on one sheet surface, and a plating layer including a Zn-Al-Mg alloy layer arranged on the sheet surface of the base checkered steel sheet having the convex portion and the flat portion, The plating layer comprises, in mass %, Zn: more than 65.0%, Al: more than 1.0% to less than 25.0%; Mg: more than 1.0% to less than 12.5%; Sn: 0% to 5.0%, Bi: 0% to less than 5.0% In: 0% to less than 2.0% Ca: 0% to 3.00%, Y: 0% to 0.5%, La: 0% to less than 0.5%, Ce: 0% to less than 0.5% Si: 0% to less than 2.5%; Cr: 0% to less than 0.25% Ti: 0% to less than 0.25% Zr: 0% to less than 0.25% Mo: 0% to less than 0.25% W: 0% to less than 0.25%, Ag: 0% to less than 0.25% P: 0% to less than 0.25%; Ni: 0% to less than 0.25% Co: 0% to less than 0.25% V: 0% to less than 0.25%, Nb: 0% to less than 0.25% Cu: 0% to less than 0.25% Mn: 0% to less than 0.25%; Li: 0% to less than 0.25% Na: 0% to less than 0.25% K: 0% to less than 0.25%, Fe: 0% to 5.0%, Sr: 0% to less than 0.5% Sb: 0% to less than 0.5% Pb: 0% to less than 0.5% B: 0% to less than 0.5%, and It has a chemical composition made up of impurities, when observing a cross section cut at a longitudinal center of the protrusion perpendicular to the longitudinal direction of the protrusion and along the plate thickness direction, a layer thickness ratio of the plating layer of the flat portion on the left and right of the protrusion (layer thickness of the left side plating layer / layer thickness of the right side plating layer) is 0.2 or more and 5.0 or less, A Zn-Al-Mg-based plated checkered steel sheet, in which a stripe height T-t, where T is the thickness of the base checkered steel sheet at the convex portion and t is the thickness of the base checkered steel sheet at the flat portion, and a gap height x between a resting surface and a sheet surface of the plated checkered steel sheet facing the resting surface when the plated checkered steel sheet is placed at rest, satisfy the following formulas 1 and 2. Formula 1: x / (T-t)≦1.5 Formula 2: 0.5<T-t≦t In Equation 1 and Equation 2, the units of the plate thickness T, t, and gap height x of the base checkered steel plate are "mm."
2. The Zn-Al-Mg plated checkered steel sheet according to claim 1, wherein the Al concentration is more than 5.0% and less than 25.0%, and the Mg concentration is more than 3.0% and less than 12.5%.
3. The Zn-Al-Mg plated checkered steel sheet according to claim 1 or 2, wherein the plating layer includes an Al-Fe alloy layer between the base checkered steel sheet and the Zn-Al-Mg alloy layer.
Citation Information
Patent Citations
Galvanized banded steel plate excellent in resistances to flawing, wearing and corrosion
JP1999279732A
Hot dip galvanized checkered steel plate having excellent scratch resistance, wear resistance, and corrosion resistance
JP2005273019A
Convex bar-attached type melting galvanized steel plate and production method for the same, and hot stamp molded body
JP2018053288A
Continuous hot-dip metal plating method for band-shaped striped steel plate
JP2743774B2
Hot-dip plated checkered plate and manufacturing method thereof
WO2019054483A1