Water-based coating material

A water-based coating material with epoxy and acrylic resin emulsions and a solvent improves film performance by enhancing adhesion and stability, addressing issues of conventional water-based coatings.

JP7561058B2Active Publication Date: 2024-10-03BEKKU KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021029435
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-26
Publication Date
2024-10-03
Estimated Expiration
2041-02-26

AI Technical Summary

Technical Problem

Conventional water-based coating materials face issues such as reduced adhesion and whitening due to low temperatures or high humidity, and they often have inferior coating film properties compared to solvent-based paints.

Method used

A water-based coating material comprising an epoxy resin emulsion, an amino group-containing resin, an acrylic resin emulsion, and a specific organic solvent, with controlled particle sizes and mixing ratios, to enhance film performance and stability.

Benefits of technology

The coating material suppresses adhesion and whitening issues, ensuring sufficient film properties and adhesion to various substrates, even under varying conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561058000001
    Figure 0007561058000001
  • Figure 0007561058000002
    Figure 0007561058000002
Patent Text Reader

Abstract

To provide an aqueous coating material capable of suppressing the influence of coating conditions and securing sufficient coating film performance.SOLUTION: The aqueous coating material is obtained by mixing a main agent containing an epoxy resin emulsion (A) and a curing agent containing an amino group-containing resin (B). The aqueous coating material contains an acrylic resin emulsion (C) and an organic solvent (D) having a boiling point of 200°C or higher and a solubility in water at 20°C of 10 g / 100 g H2O or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel water-based coating material. [Background technology]

[0002] Conventionally, coating materials have been applied to interior and exterior wall and floor surfaces of buildings, factories, warehouses, etc., outdoor floor surfaces such as general sidewalks, pedestrian bridges, and platforms, and steel structures such as bridges and steel towers, to impart beauty to the walls and floors, etc. In the painting of such walls and floors or steel structures, epoxy resin-based coating materials are widely used, taking into consideration the coating film properties such as coating film strength, adhesion, and corrosion resistance. However, when epoxy resin-based coating materials are applied under low temperature or high humidity conditions using amine-based curing agents such as polyamines or polyamides, problems such as reduced adhesion due to amine blushing and whitening of the coating film may occur.

[0003] Recently, water-based coating materials are being adopted in consideration of the environment, safety, and the like. For example, Patent Document 1 describes a thermosetting water-based coating composition containing an aqueous epoxy resin dispersion and a curing agent such as an amine resin. However, water-based paints may have inferior coating film properties compared to solvent-based paints. Furthermore, depending on the coating conditions, problems such as amine blushing tend to occur. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-253004 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in consideration of such problems, and has as its object to provide an aqueous coating material capable of suppressing the effects of painting conditions and ensuring sufficient coating film performance. [Means for solving the problem]

[0006] As a result of intensive research into such problems, the inventors have discovered an aqueous coating material characterized in that the aqueous coating material has a base agent containing an epoxy resin emulsion and a curing agent containing an amino group-containing resin, and further contains an acrylic resin emulsion and a specific organic solvent, thereby completing the present invention.

[0007] That is, the present invention has the following features. 1. A resin composition having a base agent containing an epoxy resin emulsion (A) and a curing agent containing an amino group-containing resin (B). It is a water-based coating material that The amino group-containing resin (B) contains a polyamine resin, The aqueous coating material contains an acrylic resin emulsion (C) and an organic solvent (D) having a boiling point of 200°C or higher and a solubility in water at 20°C of 10g / 100gH2O or less. fruit, The mixing weight ratio of the epoxy resin emulsion (A) to the acrylic resin emulsion (C) is 5:95 to 9.2:9.9 (48.2:51.8). 1. An aqueous coating material comprising: 2. The acrylic resin emulsion (C) is a monomer group including an epoxy group-containing monomer. 1. The aqueous coating material according to 1, which is a polymer. 3. Average particle size of the above epoxy resin emulsion (A) and the above acrylic resin emulsion (C) 3. The aqueous coating material according to 1 or 2, wherein the particle size ratio (A) / (C) is greater than 1. Effect of the Invention

[0008] The aqueous coating material of the present invention is capable of suppressing deterioration in adhesion and whitening of the coating film caused by coating conditions, and exhibiting sufficient coating film properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention relates to an aqueous coating material (hereinafter, also simply referred to as "aqueous coating material") comprising a base agent containing an epoxy resin emulsion (A) and a curing agent containing an amino group-containing resin (B).

[0010] The epoxy resin emulsion (A) of the present invention (hereinafter also simply referred to as "component (A)") is obtained by dispersing / emulsifying an epoxy resin in an aqueous medium. When dispersing an epoxy resin in an aqueous medium, an emulsifier or the like can be used as necessary. The aqueous medium is a medium that mainly contains water, and may contain water-soluble solvents such as lower alcohols, polyhydric alcohols, ether compounds, ester compounds, and alkylene oxide-containing compounds as necessary.

[0011] The epoxy resin of the component (A) may be any epoxy resin that can be dispersed in an aqueous medium, and may be either a solid epoxy resin and / or a liquid epoxy resin. As such an epoxy resin, for example, a resin containing one or more, preferably two or more, epoxy groups in the molecule can be used, and examples thereof include aromatic epoxy resins, aliphatic epoxy resins, alicyclic epoxy resins, polybutadiene resins having epoxy groups, and polyurethane resins having epoxy groups. In the present invention, aromatic epoxy resins are preferred, and examples thereof include bisphenol A type epoxy resins, bisphenol AD ​​type epoxy resins, bisphenol F type epoxy resins, and novolac type epoxy resins. Among these, particularly, one or more selected from bisphenol A type epoxy resins, bisphenol AD ​​type epoxy resins, and bisphenol F type epoxy resins are preferred. Furthermore, the epoxy resin may be one whose molecular weight has been increased as necessary, a fatty acid-modified epoxy resin obtained by reacting a fatty acid, or one obtained by making an amine-added epoxy resin (amine-modified epoxy resin) obtained by addition reaction of an amino group-containing compound water-soluble. These may be used alone or in combination of two or more. In addition, a solid epoxy resin refers to one that is solid at room temperature (23°C), and a liquid epoxy resin refers to one that is liquid at room temperature (23°C).

[0012] In the present invention, a specific example of the component (A) is an embodiment containing a solid epoxy resin (a1) as an essential component. Such an embodiment includes an embodiment containing only the solid epoxy resin (a1) and an embodiment containing the solid epoxy resin (a1) and the liquid epoxy resin (a2). This allows the effects of the present invention to be fully achieved. When the solid epoxy resin (a1) and the liquid epoxy resin (a2) are mixed, the mixing ratio (solid content weight ratio) is preferably 100:0 to 5:95 (more preferably 100:0 to 10:90), depending on the epoxy equivalent of each epoxy resin. In the present invention, "α to β" is synonymous with "α or more and β or less".

[0013] The method for preparing the component (A) is not particularly limited, but may be, for example, a method in which a solid epoxy resin and / or a liquid epoxy resin is mixed with an emulsifier as necessary to prepare a resin solution, and then the solution is mixed with an aqueous medium (containing an emulsifier as necessary) to emulsify the solution. In addition, the above preparation may be heated as necessary. In the present invention, when a solid epoxy resin and a liquid epoxy resin are used in combination, it is preferable to prepare aqueous dispersions of the solid epoxy resin and the liquid epoxy resin, and then mix them together for use. The resin solid content of the epoxy resin aqueous dispersion is not particularly limited, but is preferably 10 to 80% by weight (more preferably 20 to 70% by weight).

[0014] As the emulsifier, for example, anionic surfactants and nonionic surfactants can be used either alone or in combination. Examples of the anionic surfactant include alkali metal sulfonates such as sodium dodecylbenzenesulfonate, sodium laurylnaphthalenesulfonate, and sodium stearyl diphenyl ether disulfonate; and alkali metal sulfates such as sodium lauryl sulfate, polyoxyethylene lauryl ether sodium sulfate, and polyoxyethylene octylphenyl ether sodium sulfate. Examples of nonionic surfactants include polyoxyethylene lauryl ether, polyoxyethylene oleyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, and oxyethylene-oxypropylene block copolymers. The amount of the emulsifier to be added is preferably within the range of 0.1 to 15% by weight (more preferably 0.1 to 10% by weight, and even more preferably 0.5 to 5% by weight) based on the resin solid content.

[0015] The average particle size of the component (A) of the present invention is not particularly limited, but is preferably 100 to 1000 nm (more preferably 150 to 900 nm, even more preferably 200 to 800 nm, and particularly preferably 300 to 600 nm). If the average particle size is within such a range, advantageous effects can be obtained in terms of sealing properties, efflorescence resistance, whitening resistance, and the like. The average particle size referred to here is a value measured by dynamic light scattering.

[0016] The component (A) of the present invention has an epoxy equivalent x a However, the epoxy equivalent x is preferably 100 to 3000 (more preferably 110 to 2000, and further preferably 120 to 1500). a " is the number of grams of resin solids containing 1 gram equivalent of epoxy groups [g / eq], and is the value obtained by dividing the weight average molecular weight of the epoxy resin by the number of epoxy groups per molecule.

[0017] In addition, the above component (A) has an epoxy equivalent x a It is also possible to use a mixture of particles having different sizes and average particle sizes.

[0018] The amino group-containing resin (B) of the present invention (hereinafter, simply referred to as "component (B)") reacts with the epoxy resin emulsion (A) to form a coating film. As the component (B), for example, a polyamine resin containing two or more amino groups in one molecule can be used, and examples thereof include aliphatic polyamines, alicyclic polyamines, aromatic polyamines, heterocyclic amines, and modified polyamine resins obtained by modifying the amino groups of these polyamine resins. In addition, known methods can be used to modify the polyamine resin, and examples thereof include amidation of amino groups, Mannich reaction of amino groups with carbonyl compounds, addition reaction of amino groups with epoxy groups, and addition reaction of amino groups with styrene. In addition, as the component (B), aliphatic polyamides, alicyclic polyamides, aromatic polyamides, aliphatic polyamidoamines, alicyclic polyamidoamines, aromatic polyamidoamines, etc. can also be used. These can be used alone or in combination of two or more.

[0019] In the present invention, it is preferable that the (B) component contains at least one selected from, for example, aliphatic polyamines and modified aliphatic polyamines. This improves adhesion and adhesion to substrates and coatings when mixed with a base material containing an epoxy resin emulsion. Examples of aliphatic polyamines include chain aliphatic polyamines such as diethylenetriamine, triethylenetetraamine, tetraethylenepentamine, dipropylenediamine, diethylaminopropylamine, and hexamethylenediamine; cyclic aliphatic polyamines such as N-aminoethylpiperazine, bis(4-amino-3-methylcyclohexyl)methane, menthenediamine, isophoronediamine, 4,4'-diaminodicyclohexylmethane, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro[5.5]undecane (spiroacetaldiamine), norbornanediamine, tricyclodecanediamine, and 1,3-bisaminomethylcyclohexane; and aliphatic aromatic amines such as metaxylenediamine. In the present invention, it is particularly preferable that the monomer contains at least one selected from meta-xylylenediamine and a styrene addition reaction product of meta-xylylenediamine.

[0020] The embodiment of the (B) component is not particularly limited, but a water-soluble resin that can be dissolved in an aqueous medium, or a water-dispersed resin that can be dispersed in an aqueous medium, can be used. In the present invention, it is preferable that the (B) component contains a water-soluble resin. In this case, the storage stability is excellent, and when mixed with the main agent, the compatibility and reactivity with the epoxy resin emulsion (A) are increased, and the adhesion and adhesion to the substrate and the coating film are further improved, and a coating film excellent in water resistance and coating film appearance can be formed. The (B) component may be a solvent-free type (solid content 100% by weight) or may be a type in which the (B) component is dissolved or dispersed in an aqueous medium in advance. The solid content of the (B) component is preferably 50% by weight or more (more preferably 55% by weight or more, and even more preferably 60% by weight or more). The upper limit of the solid content of the (B) component is 100% by weight or less. When this range is satisfied, the effects of the present invention can be fully exhibited. The aqueous medium is a medium that mainly contains water, and may contain water-soluble solvents such as lower alcohols, polyhydric alcohols, ether compounds, ester compounds, and alkylene oxide-containing compounds, as necessary.

[0021] In addition, the active hydrogen equivalent y of the component (B) is b is preferably 10 to 1000 (more preferably 50 to 800, and further preferably 80 to 600). b " is the number of grams of resin solids containing 1 gram equivalent of active hydrogen groups [g / eq], and is the value obtained by dividing the weight average molecular weight of the amino group-containing resin by the number of hydrogen atoms of the amino group per molecule.

[0022] The aqueous coating material of the present invention is a mixture of the base agent and the curing agent in an amount of 100% by weight of the epoxy equivalent ([X A ]: solid content equivalent) and the active hydrogen equivalent of component (B) in the hardener ([Y B ] (solid content equivalent) ratio [X A / (Y BIt is preferable to mix so that the ratio of (R) to (C) is preferably 0.1 to 3 (more preferably 0.0.5 to 2, and even more preferably 0.7 to 1.5). In such a case, the adhesion and adhesion of the aqueous coating material to the substrate and the coating film are improved. Furthermore, the stability and usable life of the aqueous coating material can be increased.

[0023] In addition, the above X A , the above Y B is determined from the blending parts at the time of mixing, and specifically, the above [X A ] is the amount of component (A) contained in the base resin (solid weight parts) multiplied by the epoxy equivalent of component (A) x a In addition, the above [Y B is the amount of component (B) contained in the curing agent (parts by weight of solid content) expressed as the active hydrogen equivalent y b This is the value divided by .

[0024] The aqueous coating material of the present invention is characterized in that it contains, in addition to the above-mentioned (A) and (B) components, an acrylic resin emulsion (C) (hereinafter also simply referred to as "(C) component"), and an organic solvent (D) (hereinafter also simply referred to as "(D) component") having a boiling point of 200°C or higher and a solubility in water at 20°C of 10g / 100gH2O or less. By containing the (C) component and the (D) component in combination, the compatibility and reactivity of the (A) component and the (B) component are improved, and excellent film-forming properties can be obtained. As a result, a dense coating film can be formed, the effects of coating conditions can be efficiently suppressed, and amine blushing and the like are less likely to occur.

[0025] The above-mentioned (C) component and (D) component can be mixed with either the base agent or the curing agent, or with both. In the present invention, it is preferable to mix the above-mentioned (C) component and the above-mentioned (D) component with the base agent. This further enhances the above-mentioned effects, and makes it possible to form a coating film with excellent aesthetics in which amine blushing and the like are suppressed.

[0026] The (C) component is a (meth)acrylic acid alkyl ester that is the main component of the resin skeleton, and is copolymerized with other monomers and other polymerizable monomers as necessary. In the present invention, the acrylic acid alkyl ester and the methacrylic acid alkyl ester are collectively referred to as the (meth)acrylic acid alkyl ester. The monomer is a general term for a compound having a polymerizable unsaturated double bond.

[0027] In the present invention, it is preferable that the monomer group constituting component (C) contains a hydrophobic monomer, for example, a long-chain alkyl (meth)acrylate, an aromatic group-containing monomer, or the like.

[0028] As the long-chain alkyl (meth)acrylate, an alkyl (meth)acrylate having an alkyl group having 4 or more carbon atoms can be used, for example, n-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, octadecyl (meth)acrylate, cyclohexyl (meth)acrylate, etc. These can be used alone or in combination of two or more.

[0029] Examples of aromatic group-containing monomers include styrene-based monomers such as styrene, 2-methylstyrene, vinyltoluene, ethylvinylbenzene, vinylnaphthalene, and chlorostyrene, and aromatic group-containing (meth)acrylates such as phenyl(meth)acrylate, benzyl(meth)acrylate, and phenoxyethyl(meth)acrylate, etc. These may be used alone or in combination of two or more.

[0030] The content of the hydrophobic monomer in the monomer group is preferably 10% by weight or more, more preferably 30% by weight or more, and even more preferably 40% by weight or more, in terms of weight ratio. The upper limit is not particularly limited, but is preferably 99.5% by weight or less. In such a case, the compatibility with the (D) component is improved, and the effect of the present invention can be enhanced.

[0031] Specific examples of the other monomers include amide group-containing monomers, carbonyl group-containing monomers, carboxyl group-containing monomers, amino group-containing monomers, epoxy group-containing monomers, hydroxyl group-containing monomers, vinylidene halide monomers, alkoxysilyl group-containing monomers, ethylene, propylene, isoprene, butadiene, vinyl ether, vinyl ketone, etc. These can be used alone or in combination of two or more.

[0032] In the present invention, it is preferable to include an epoxy group-containing monomer. Examples of the epoxy group-containing monomer include glycidyl (meth)acrylate, diglycidyl fumarate, 3,4-epoxycyclohexyl (meth)acrylate, 3,4-epoxyvinylcyclohexane, allyl glycidyl ether, ε-caprolactone-modified glycidyl (meth)acrylate, and β-methylglycidyl (meth)acrylate. These can be used alone or in combination of two or more.

[0033] In the present invention, the monomers constituting component (C) may contain an epoxy group-containing monomer in an amount of preferably 0.5 to 50% by weight (more preferably 1 to 30% by weight), which can suppress deterioration of adhesion and whitening of the coating film due to amine blushing, etc., and provide sufficient coating film properties.

[0034] Other specific examples of monomers include: Examples of nitrile group-containing monomers include (meth)acrylonitrile, vinylidene cyanide, and α-cyanoethyl (meth)acrylate. Examples of the amide group-containing monomer include maleic acid amide, (meth)acrylamide, N-monoalkyl (meth)acrylamide, N,N-dialkyl (meth)acrylamide, 2-(dimethylamino)ethyl (methacrylate), N-[3-(dimethylamino)propyl] (meth)acrylamide, and vinylamide. Examples of the carbonyl group-containing monomer include acrolein, diacetone (meth)acrylamide, vinyl methyl ketone, vinyl ethyl ketone, and vinyl butyl ketone. Examples of the carboxyl group-containing monomer include (meth)acrylic acid, crotonic acid, maleic acid, itaconic acid, fumaric acid, isocrotonic acid, and salicylic acid. Examples of amino group-containing monomers include aminomethyl acrylate, aminoethyl acrylate, aminopropyl (meth)acrylate, amino-n-butyl (meth)acrylate, butylvinylbenzylamine, vinylphenylamine, p-aminostyrene, N-methylaminoethyl (meth)acrylate, and Nt-butylaminoethyl (meth)acrylate. Examples of hydroxyl group-containing monomers include hydroxypropyl (meth)acrylate, ethylene glycol mono(meth)acrylate, and glycerol mono(meth)acrylate. Examples of vinylidene halide monomers include vinylidene fluoride, etc. Examples of the alkoxysilyl group-containing monomer include vinyltrimethoxysilane, vinyltriethoxysilane, γ-(meth)acryloyloxypropyltrimethoxysilane, γ-(meth)acryloyloxypropyltriethoxysilane, γ-(meth)acryloyloxypropylmethyldimethoxysilane, etc. These can be used alone or in combination of two or more.

[0035] The above-mentioned (C) component can be produced by emulsion polymerization of a monomer group obtained by appropriately mixing the above-mentioned monomers. A known method can be adopted as the polymerization method, and in addition to normal emulsion polymerization, soap-free emulsion polymerization, feed emulsion polymerization, seed emulsion polymerization, multi-stage emulsion polymerization, etc. can also be adopted. During polymerization, for example, an emulsifier, an initiator, a dispersant, a polymerization inhibitor, a polymerization retarder, a buffer, a chain transfer agent, a pH adjuster, etc. can be used.

[0036] As the emulsifier, various surfactants that can be used in emulsion polymerization can be used, and these may be reactive types (reactive surfactants) having polymerizable unsaturated double bonds. As the emulsifier, for example, anionic surfactants and nonionic surfactants can be used alone or in combination. Specifically, for example, they can be appropriately selected from those described in the above component (A).

[0037] The glass transition temperature (hereinafter simply referred to as "Tg") of the component (C) can be adjusted by selecting the type and mixing ratio of the monomers. This Tg may be set appropriately taking into consideration the final required performance, etc., but it is preferable that the Tg is -5 to 80°C (more preferably -3 to 60°C). Two or more types of components with different Tgs can also be used as the component (C). In this case, it is preferable that the total Tg falls within the above range. The glass transition temperature can be calculated using Fox's formula.

[0038] The average particle size of the component (C) is not particularly limited, but is preferably 300 nm or less (more preferably 10 to 250 nm, even more preferably 20 to 200 nm, and particularly preferably 30 to 180 nm). If the average particle size is within such a range, advantageous effects can be obtained in terms of impregnation reinforcement, sealing properties, efflorescence resistance, whitening resistance, and the like. In addition, two or more types of component (C) having different average particle sizes can also be used. The average particle size referred to here is a value measured by dynamic light scattering.

[0039] In the present invention, it is preferable that the ratio of the average particle size of the (A) component to the (C) component is (A) / (C)>1 (more preferably >1.2). This tends to result in a high concentration of the (A) component near the substrate of the formed coating film, while the concentration of the (C) component near the surface of the formed coating film, thereby suppressing the influence of the coating conditions and enabling sufficient coating film properties to be exhibited. Note that, when the (A) component and the (C) component contain two or more types with different average particle sizes, it is preferable that the average value of the average particle size of the (A) component and the average value of the average particle size of the (C) component satisfy the above condition.

[0040] The mixing ratio of the (C) component is preferably such that the solids weight ratio with the (A) component is (A):(C)=5:95 to 95:5 (more preferably 10:90 to 90:10, and even more preferably 20:80 to 80:20). In such a case, the influence of coating conditions can be suppressed, and excellent adhesion to various substrates and coating films can be exhibited. Furthermore, a coating film excellent in water resistance and coating appearance can be formed.

[0041] The (D) component is not particularly limited as long as it is an organic solvent having a boiling point of 200° C. or higher and a solubility in water of 10 g / 100 gH2O or lower at 20° C., but examples thereof include ethylene glycol ether compounds such as ethylene glycol monohexyl ether, ethylene glycol dibutyl ether, and ethylene glycol phenyl ether; diethylene glycol ether compounds such as diethylene glycol monohexyl ether, diethylene glycol monobutyl ether acetate, and diethylene glycol dibutyl ether; propylene glycol ether compounds such as propylene glycol phenyl ether, dipropylene glycol-n-butyl ether, dipropylene glycol-tert-butyl ether, dipropylene glycol-n-propyl ether, and tripropylene glycol-n-butyl ether; 2-ethyl-1,3-hexanediol, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, 2,2,4-trimethyl-1,3-pentanediol diisobutyrate, and benzyl alcohol. These can be used alone or in combination of two or more. The boiling point of component (D) is 200° C. or higher, with the upper limit being preferably 350° C. or lower (more preferably 300° C. or lower). The solubility of component (D) in water at 20° C. is 10 g / 100 g H2O or lower, preferably 8 g / 100 g H2O or lower, with the lower limit being preferably 0 g / 100 g H2O or higher (more preferably 0.1 g / 100 g H2O or higher).

[0042] In the present invention, it is particularly preferable to contain at least one propylene glycol ether compound such as propylene glycol phenyl ether, dipropylene glycol-n-butyl ether, dipropylene glycol-tert-butyl ether, dipropylene glycol-n-propyl ether, and tripropylene glycol-n-butyl ether.

[0043] The amount of component (D) mixed is preferably 1 to 80 parts by weight (more preferably 2 to 60 parts by weight) per 100 parts by weight of component (A) (solid content). Within this range, the above effects can be fully exhibited.

[0044] In addition to the above-mentioned components, the aqueous coating material of the present invention may contain color pigments, extender pigments, rust-preventive pigments, silane coupling agents, pH adjusters, plasticizers, preservatives, antifungal agents, antialgae agents, defoamers, leveling agents, dispersants, antisettling agents, antisagging agents, thickeners (thixotropic adjusters), film-forming assistants, matting agents, crosslinking agents, catalysts (curing accelerators), adhesion agents, ultraviolet absorbers, light stabilizers, etc., as necessary, in the range in which the effects of the present invention are not significantly impaired. The pH of the aqueous coating material of the present invention is preferably 3 to 12 (more preferably 4 to 11). In the present invention, it is preferable that the pH of the aqueous coating material satisfies the above.

[0045] Examples of the color pigment include titanium oxide, zinc oxide, carbon black, lamp black, bone black, graphite, black iron oxide, cobalt black, copper manganese iron black, red iron oxide, molybdate orange, permanent red, permanent carmine, anthraquinone red, perylene red, quinacridone red, yellow iron oxide, titanium yellow, fast yellow, benzimidazolone yellow, cobalt green, phthalocyanine green, ultramarine blue, Prussian blue, cobalt blue, phthalocyanine blue, quinacridone violet, dioxazine violet, aluminum pigments, and pearl pigments. These pigments may be used alone or in combination of two or more.

[0046] Examples of the extender pigment include heavy calcium carbonate, kansuiite, light calcium carbonate, white carbon, talc, kaolin, clay, china clay, diatomaceous earth, barite powder, barium sulfate, precipitated barium sulfate, silica sand, silica powder, quartz powder, resin beads, glass beads, hollow balloons, and the like. One or more of these can be used.

[0047] As the rust-preventive pigment, commercially available or known materials can be used, but pigments that do not contain either chromium or lead (also referred to as "non-chromium rust-preventive pigments") are preferred. Specifically, for example, phosphate compounds such as zinc phosphate, iron phosphate, aluminum phosphate, calcium phosphate, and magnesium phosphate; phosphate compounds such as zinc phosphite, iron phosphite, aluminum phosphite, calcium phosphite, and magnesium phosphite; polyphosphate compounds such as zinc polyphosphate, iron polyphosphate, and aluminum polyphosphate; molybdic acid compounds such as zinc molybdate, aluminum molybdate, calcium molybdate, barium molybdate, and aluminum phosphomolybdate; vanadium compounds such as vanadium oxide; boric acid compounds such as barium borate, barium metaborate, and calcium borate; cyanamide compounds such as zinc cyanamide and zinc calcium cyanamide, and one or more of these can be used. In addition, the above pigments can also be used after various surface treatments.

[0048] The aqueous coating material of the present invention preferably contains a catalyst (curing accelerator). Examples of the catalyst (curing accelerator) include various aromatic carboxylic acids such as benzoic acid, salicylic acid, trihydroxybenzoic acid, phthalic acid, cinnamic acid, and benzenehexacarboxylic acid; tertiary amines such as trimethylamine, ethyldimethylamine, propyldimethylamine, N,N'-dimethylpiperazine, pyridine, picoline, 1,8-diazabiscyclo(5,4,0)undecene-1 (DBU), benzyldimethylamine, 2-(dimethylaminomethyl)phenol (DMP-10), and 2,4,6-tris(dimethylaminomethyl)phenol (DMP-30); hydroxylamine, phenoxyamine, and other hydroxyamines. Examples of the imidazoles include the above-mentioned (B) component, such as dimethylamines, imidazole, 1-methylimidazole, 2-methylimidazole, 4(5)-methylimidazole, 2-ethyl-4-methylimidazole, 2-ethylimidazole, and 2-phenylimidazole, and amines other than the above-mentioned (M) component; phenols such as phenol novolac, o-cresol novolac, p-cresol novolac, t-butylphenol novolac, and dicyclopentadiene cresol; and organometallic compounds such as tin octylate, dibutyltin dilaurate, dibutyltin diacetate, organotitanate, and sodium acetate. These can be used alone or in combination of two or more.

[0049] The aqueous coating material of the present invention preferably has a solids content of 5 to 60% by weight (more preferably 6 to 50% by weight, and even more preferably 7 to 45% by weight). The solids content can be adjusted by mixing the above-mentioned aqueous medium. When the solids content is within this range, the coating workability is excellent and adhesion to various substrates and coating films can be further improved.

[0050] The aqueous coating material of the present invention is preferably used as a coating material (particularly a primer) for painting interior and exterior wall surfaces and floor surfaces, or outdoor floor surfaces such as general sidewalks, pedestrian bridges, and platforms, and even steel structures such as bridges and steel towers. For example, it is preferably used as a primer material applied to substrates such as mortar, concrete, ceramic siding boards, ceramic siding boards, metal siding boards, extrusion molding boards, slate boards, calcium silicate boards, ALC boards, metals, steel materials, wood, glass, ceramics, synthetic resins, etc., or substrates such as a wide variety of existing coating films formed on such substrates (substrate surfaces). In addition, the shape of such substrates (substrates and existing coating films) can be smooth (flat), or have various uneven patterns (for example, stone-like, brick / tile-like, wood-grain-like, border-like, plaster-like, spray-on, etc.). Furthermore, it can also be applied to substrates including sealing joints.

[0051] In the application of the aqueous coating material of the present invention, various methods can be used, such as brush application, roller application, spray application, etc. Furthermore, when applying in a factory, in addition to the above, a roll coater, a flow coater, etc. can also be used for application.

[0052] The amount of the aqueous coating material applied is preferably 0.05 to 0.5 kg / m 2 (More preferably 0.07 to 0.3 kg / m 2 ) The number of coats of the aqueous coating material may be appropriately determined depending on the condition of the substrate, but is preferably 1 to 2 coats. The drying time of the aqueous coating material is preferably 1 hour or more and 1 week or less. The drying temperature is preferably -10°C or more and 50°C or less, more preferably -5°C or more and 40°C or less. The aqueous coating material of the present invention is preferably a room temperature curing type.

[0053] The coating film formed by the aqueous coating material of the present invention has excellent adhesion to a wide variety of topcoat materials. The topcoat material is not particularly limited as long as it is generally used for painting buildings, and the binder may be, for example, an organic binder such as acrylic resin, polyurethane resin, epoxy resin, fluororesin, alkyd resin, or polyester resin, or an inorganic binder such as silicon resin, alkoxysilane, colloidal silica, or silicate, or an organic-inorganic composite binder such as acrylic silicon resin. In particular, in the present invention, the adhesiveness with the topcoat material containing one or more selected from the organic binder and the organic-inorganic composite binder can be fully exhibited.

[0054] Specific topcoat materials include, for example, weather-resistant topcoat paint for architecture (JIS K5658:2010), weather-resistant paint for steel structures (JIS K5659:2008), glossy synthetic resin emulsion paint (JIS K5660:2008), fireproof paint for architecture (JIS K5661:1970), synthetic resin emulsion paint (JIS K5663:2008), paint for road markings (JIS K5665:2011), multicolored pattern paint (JIS K5667:2003), synthetic resin emulsion pattern paint (JIS K5668:2010), acrylic resin-based non-aqueous dispersion paint (JIS K5670:2008), lead- and chromium-free rust-preventive paint (JIS K5674:2008), high solar reflectance paint for roofs (JIS K5675:2011), floor paint for buildings (JIS K5970:2008), architectural coating waterproofing materials (JIS A6021:2011), architectural finishing coating materials (JIS A6909:2014), etc.

[0055] The method of applying the topcoat material is not particularly limited and can be applied by a known method, for example, brush coating, trowel coating, spray coating, roller coating, roll coater, flow coater, etc. In other words, each topcoat material can be applied based on the normal process with the optimal coating specifications for each topcoat material. EXAMPLES

[0056] The following examples and comparative examples will clarify the features of the present invention.

[0057] <Production of main agents 1 to 11> The epoxy resin emulsion (A), the acrylic resin emulsion (C), the organic solvent (D), the catalyst (P), the additives, and water were mixed in the mixing ratios shown in Table 1 to obtain main components 1 to 11.

[0058] <Preparation of hardener 1> The amino group-containing resin (B1) was used as a curing agent 1.

[0059] The following raw materials were used: Epoxy resin emulsion (A) (A1) Epoxy resin emulsion [bisphenol A type epoxy resin (solid type) water dispersion, solid content 46% by weight, average particle size: 390 nm, epoxy equivalent x a 508] Amino group-containing resin (B) (B1) Polyamine resin [water-soluble, styrene addition reaction product of meta-xylenediamine, solid content 100% by weight, active hydrogen equivalent y b :103] Acrylic resin emulsion (C) (C1) Acrylic resin emulsion [styrene / 2-ethylhexyl acrylate / glycidyl methacrylate copolymer, glass transition temperature: 20°C, solid content: 33% by weight, glycidyl methacrylate content: 9% by weight, average particle size: 75 nm] (C2) Acrylic resin emulsion [styrene / 2-ethylhexyl acrylate / glycidyl methacrylate copolymer, glass transition temperature: -3°C, solid content: 33% by weight, glycidyl methacrylate content: 9% by weight, average particle size: 160 nm] (C3) Acrylic silicone resin emulsion [methyl methacrylate / n-butyl acrylate / glycidyl methacrylate / 3-methacryloyloxypropyltrimethoxysilane / acrylic acid copolymer, glass transition temperature: 20°C, solid content: 33% by weight, alkoxysilyl group-containing monomer content: 1% by weight, glycidyl methacrylate content: 2% by weight, average particle size: 120 nm] (C4) Acrylic resin emulsion [styrene / 2-ethylhexyl acrylate / methacrylate copolymer, glass transition temperature: 20°C, solid content: 33% by weight, average particle size: 75 nm] Organic solvents (D) (D1) Dipropylene glycol-n-butyl ether [boiling point 229°C, solubility in water at 20°C 5g / 100gH2O] (D2) Propylene glycol phenyl ether [boiling point 243°C, solubility in water at 20°C 1g / 100gH2O] (D3) Tripropylene glycol-n-butyl ether [boiling point 274°C, solubility in water at 20°C 3g / 100gH2O] (D4) 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate [boiling point 255°C, solubility in water at 20°C 0.09g / 100gH2O] (D5) Propylene glycol-n-butyl ether [boiling point 170°C, solubility in water at 20°C 6g / 100gH2O] (D6) Propylene glycol [boiling point 187°C, solubility in water at 20°C is ∞] (P1) Organotin compound dispersion [solid content: 10% by weight] Additives: Antifoaming agents, thickeners, etc.

[0060] [Table 1]

[0061] (Examples 1 to 8, Comparative Examples 1 to 3) Base agents 1 to 11 and curing agent 1 shown in Table 1 were mixed together, and the epoxy equivalent of component (A) in the base agent ([X A]: solid content equivalent) and the active hydrogen equivalent of component (B) in the hardener ([Y B ] (solid content equivalent) ratio [X A / (Y B )]=1.0 was obtained as an aqueous coating material (clear aqueous coating material), and the following evaluations were carried out.

[0062] <Evaluation 1> The existing coating was prepared by mixing the base agent and hardener on a black acrylic plate (150mm x 200mm x 3mm) and applying the water-based coating material to a thickness of 0.15mm immediately after mixing, and then drying for one day under standard conditions (air temperature 23°C, relative humidity 50%) to prepare test specimen [I]. Each test specimen was immersed in water at 20°C for 48 hours, then removed and dried (23°C, 3 hours), and the condition of the coating was visually observed and evaluated for swelling, peeling, whitening, etc. The evaluation criteria were a six-level scale (AA>A>AB>B>C>D), with "A" being almost no abnormality and "D" being abnormality. The results are shown in Table 2.

[0063] <Evaluation 2> A water-based coating material is applied to a steel plate (150mm x 200mm x 1mm) at a rate of 0.1kg / m 2 Immediately after mixing, the mixture was applied and dried for 3 days at 10°C and 80% humidity. Then, a water-based topcoat (acrylic silicone resin emulsion paint) was applied at a rate of 0.1 kg / m. 2 The coating was applied as shown in the figure and dried for one day under standard conditions to prepare test specimen [II]. The adhesion of the prepared specimen [II] was evaluated by the cross-cut tape method according to JIS K 5600-5-6. The results are shown in Table 2. The evaluation criteria are as follows: AA: Defect area is less than 5% A: The area of ​​the defect is 5% or more but less than 10% AB: Defect area is 10% or more but less than 25% B: Defect area is 25% or more but less than 40% C: Defect area is 40% or more but less than 55% D: Defective area is 55% or more

[0064]

Table 2

Claims

1. The composition has a base agent containing an epoxy resin emulsion (A) and a curing agent containing an amino group-containing resin (B). It is a water-based coating material that The amino group-containing resin (B) contains a polyamine resin, The aqueous coating material includes an acrylic resin emulsion (C) and a water-soluble polymer having a boiling point of 200° C. or higher and a solubility in water at 20° C. of 10 g / 100 gH 2 Contains an organic solvent (D) of O or less, The aqueous coating material is characterized in that the mixing weight ratio of the epoxy resin emulsion (A) to the acrylic resin emulsion (C) is 5:95 to 9.2:9.9 (48.2:51.8).

2. The acrylic resin emulsion (C) is a monomer group including an epoxy group-containing monomer.

2. The water-based coating material of claim 1, which is a polymer.

3. The average particle size of the epoxy resin emulsion (A) and the acrylic resin emulsion (C) 3. The aqueous coating material according to claim 1, wherein the particle size ratio (A) / (C) is greater than 1.

Citation Information

Patent Citations

  • Epoxy resin emulsion composition

    JP1998046008A

  • Normal temperature-curable two-component aqueous epoxy resin coating composition

    JP1999166153A

  • Aqueous epoxy resin dispersion

    JP2003253004A

  • Aqueous coating material

    JP2010065098A

  • Coating method

    JP2010247070A